The method constructs an ecological desert stone breakwater by using cement-based paints and concrete substrates to attract oysters, addressing the destruction of marine ecosystems and enhancing the durability and ecological restoration of coastal areas.

JP7575808B2Active Publication Date: 2024-10-30HARBIN ENG UNIV
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022533424
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-02
Filing Date
2020-12-01
Publication Date
2024-10-30
Estimated Expiration
2040-12-01

AI Technical Summary

Technical Problem

The rapid development of coastal regions in China has led to the destruction of marine ecosystems due to the construction of breakwaters, which are fragile and have short service lives, necessitating the need for ecologically effective breakwaters that can dissipate waves, have a long service life, and improve the environmental efficiency.

Method used

A method for constructing an ecological desert stone breakwater by attracting oyster larvae using cement-based paints and concrete substrates with specific formulations that include dark pigments, biocalcium powder, and trace elements to promote oyster attachment, metamorphosis, and growth, while maintaining the durability and ecological integrity of marine structures.

Benefits of technology

The method effectively attracts oysters to attach to concrete surfaces, enhancing the durability of marine structures, purifying water bodies, and restoring the marine ecosystem by promoting the growth of oysters, which can purify water and improve the ecological environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575808000001
    Figure 0007575808000001
  • Figure 0007575808000002
    Figure 0007575808000002
  • Figure 0007575808000003
    Figure 0007575808000003
Patent Text Reader

Abstract

This paper presents cement paint and application technology for attracting marine sessile organisms to attach, particularly a construction method for an ecological rubble breakwater, and an attractive cement-based paint and its manufacturing method. The cement paint for attracting marine sessile organisms is applied to the stone surface, and a rational spatial layout is used to ensure that each stone pile (stone block) effectively dissipates waves and allows smooth exchange of water between both sides. After the oysters attached to each stone pile (stone block) multiply in large numbers, they can purify the water body and improve the ecological environment of the surrounding sea area.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority from Chinese Patent Application No. 201911210502.6, filed on December 2, 2019, for "Construction Method of Ecological Rubble Breakwater," and claims the benefit of priority from Chinese Patent Application No. 201911210521.9, filed on December 2, 2019, for "Cement-based Paint for Attracting Sessile Organisms on Marine Project Surface and Manufacturing Method Thereof," the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to ecological breakwater technology, in particular to a construction method for an ecological riprap breakwater, an attractive cement-based paint and its manufacturing method, which belong to the field of marine ecological engineering. [Background technology]

[0003] In recent decades, the rapid development of the economy in China's coastal areas, but the lack of attention to environmental protection, has caused large-scale destruction of the ecosystem in China's coastal areas, which has serious impacts on the ecosystem and economy of China's coastal areas. At present, with the implementation of a series of relevant national policies, China's marine project construction is also entering a peak period, and at the same time, the large-scale construction of marine projects and breakwaters to ensure the stabilization of the surrounding sea areas will further damage the already fragile marine ecosystem. If proper protection of the ecological environment is not taken, it will more seriously damage the ecosystem in China's coastal areas. At the same time, most of the infrastructure in China's coastal areas cannot be dismantled and the ecosystem of the sea area needs to be restored, so people gradually realize that by applying ecological technologies to many infrastructures, the ecosystem of the sea area can be effectively improved or restored. Therefore, building breakwaters with high ecological effect or ecologicalizing existing breakwaters is very important and urgent for the improvement of the ecological environment of China's coastal areas. Summary of the Invention

[0004] The objective of the present invention is to provide a method for constructing a durable and ecological rubble breakwater, so as to solve the problem that the expansion and repair of current breakwaters destroys the ecosystem in coastal areas and the service life of existing breakwaters is short, so that the breakwater also has good wave-dissipating function, long service life and environmental efficiency.

[0005] Based on the fact that oysters prefer to attach to dark substrates and the surface of the same kind of shells, and higher alkalinity affects the attachment and transformation of oysters, and considering the effect of simultaneously mixed external additives on the performance of cement-based paint and concrete, the present invention determines the design, molding and curing method of paint and concrete to attract oysters to attach. The specific technical solutions are as follows:

[0006] (1) Investigating the marine area in which the ecological project will be constructed, investigating the dominant species of oysters in said marine area and whether oysters are attached, and also investigating the air temperature, seawater temperature, dissolved oxygen, planktonic organisms, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca in said marine area in different seasons. 2+ , Zn 2+ , K + We will also investigate the number of typhoons that have occurred in the past and their intensity.

[0007] (2) Regarding the manufacture of a concrete bond base, one of the following bond bases is manufactured: a plate-shaped bond base, a corrugated bond base, or a cylindrical bond base.

[0008] (3) To quantitatively harvest and cultivate oyster larvae, during the period when the floating oyster larvae in the local sea area are concentrated and attach to the sea and metamorphose, the attachment substrate is placed in the seeding area of ​​the nearby sea area, and the attachment amount of oyster larvae is 15 to 25 oysters / 100 cm 2 In this case, seedling collection is stopped and the attached substrate is then moved to an area of ​​sea where food is abundant for floating culture.

[0009] (4) Treat the rock surface by washing the rock surface and, when the saturated surface has dried, spray or paint a cement-based paint to attract sessile organisms to the marine project surface.

[0010] (5) Regarding the placement of rock blocks, in the second year, during the period when the floating oyster larvae are concentrated in the local waters to attach and metamorphose, the rock blocks with a volume of more than 1 cubic meter are placed individually, and each rock block is covered with a rope basket. In addition, the rope basket is used to cover multiple rock blocks with a volume of less than 1 cubic meter, thereby forming a rock pile with a volume of 1 to 5 cubic meters, the internal porosity of which is 40% to 60%, and the rocks or rock piles are connected with ropes, etc.

[0011] (6) Regarding the placement of oyster attachment substrates at the site, the substrates carrying oysters at the mature stage of gonad development in (2) shall be transported to the sea area where the breakwater is to be constructed, and a rough-surfaced lightweight concrete oyster attachment substrate shall be placed on each stone block or pile of stones, and the stone blocks or piles of stones shall be secured with ropes. In addition, feeding or feeding nutrients shall be added as necessary based on the planktonic organism conditions in the local sea area.

[0012] (7) Monitoring and management of oyster larvae attachment: Monitor the attachment status of oyster larvae on the concrete surface, and keep the number at 30-40 per 100 cm. 2 In this case, the oyster attachment substrate will be removed and the ecological condition of the breakwater will be monitored over the long term, with improvement measures being taken according to the actual situation.

[0013] Regarding the lightweight concrete oyster-attached base with a rough surface described in the specific measures in (2), the components of the material are cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water, dark color pigment, bio-calcium powder, calcium carbonate powder, trace elements, short fiber, and superplasticizer, and the weight percentages thereof are 21.8% to 34.5%, 24.6% to 37.5%, 15.8% to 29.6%, 8.4% to 16.4%, 0.6% to 3.0%, 0.4% to 2.0%, 0.4% to 2.0%, 0.2% to 1.8%, 0.15% to 1.5%, and 0.03% to 0.18%, respectively.

[0014] Preferably, the deep color pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red.

[0015] Preferably, the dark pigments are modified with one of the following materials depending on their impact on concrete performance: transparent resin, organosilicon, dimethylsiloxane, and superhydrophobic material.

[0016] Preferably, the biocalcium powder is bovine bone powder. or It contains one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, and the fineness of the powder is 100 mesh to 1000 mesh. Here, oyster shell powder, fish bone powder, eggshell powder, and coral powder are referred to as bio-calcium carbonate powder. )

[0017] Preferably, the biocalcium powder is prepared by treating eggshell powder, coral powder, oyster shell powder and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid and sulfurous acid, and treating cow bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.

[0018] Preferably, the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, and processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultra-fine precipitated calcium carbonate, and has a fineness of greater than 200 mesh.

[0019] Preferably, the trace elements zinc, iron, potassium and phosphorus are modified by selecting natural minerals, industrial products or chemical reagents including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to realize sustained release of corresponding ions and reduce or eliminate the adverse effects on concrete performance. However, in the case of eutrophication areas, materials containing nitrogen or phosphorus elements are not selected.

[0020] Preferably, the cementitious material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, where the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material includes one of alkali-activated slag and alkali-activated slag + fly ash.

[0021] Preferably, the short fibers are inorganic fibers (length 12 to 20 mm) including one or more of basalt fibers, alkali-resistant glass fibers, and carbon fibers.

[0022] Preferably, the lightweight coarse aggregate is one or two of crushed lightweight porous basalt, lightweight ceramsite having a maximum particle size of less than 20mm.

[0023] Preferably, the lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, and has a particle size of 0.2 mm to 5 mm.

[0024] The method for manufacturing a rough surface cement concrete oyster adhesion base is as follows: Step S1 of designing different roughness according to the preferred characteristics of oyster larvae to attach to rough surfaces, and then manufacturing molding forms with different roughness; Step S2 of measuring the cementitious material, the lightweight coarse aggregate, the lightweight fine aggregate, the water, the dark color pigment, the bio-calcium powder, the calcium carbonate powder, the trace elements, the short fibers and the superplasticizer; First, put the lightweight coarse aggregate and the lightweight fine aggregate into the concrete mixer and mix for 0.5-1 minute, then add the cementitious material, dark color pigment, bio-calcium powder, calcium carbonate powder and trace elements and mix for another 1-2 minutes, then add short fiber, water and superplasticizer and mix for 2-6 minutes, and then mix evenly, then pour and vibrate; step S3; The method includes step S4 of placing the molded concrete specimen in a curing box with high concentration of CO2 according to the circumstances and curing it for 0.5 to 5 hours to reduce the alkalinity of the cement specimen, and then curing it for 28 days as standard or according to the actual circumstances.

[0025] This makes it possible to produce a cement concrete oyster attachment base having a rough surface and excellent attracting effect.

[0026] For the lightweight concrete scratch-attached base having a rough surface described in the specific measures in (2), the components of the material are dark color pigment, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, where the weight percentages of the dark color pigment, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.6% to 3.0%, 21.8% to 34.5%, 24.6% to 37.5%, 15.8% to 29.6%, 8.4% to 16.4% and 0.03% to 0.18%, respectively.

[0027] For the lightweight concrete oyster-attached base having a rough surface described in the specific measures in (2), the ingredients of the material are calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, where the weight percentages of calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.4% to 2.35%, 21.8% to 34.5%, 24.6% to 37.5%, 15.8% to 29.6%, 8.4% to 16.4% and 0.03% to 0.18%, respectively.

[0028] Regarding the lightweight concrete oyster-attached base having a rough surface described in the specific measures in (2), the ingredients of the material are cow bone powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, where the weight percentages of the cow bone powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.4-2.35%, 21.8%-34.5%, 24.6%-37.5%, 15.8%-29.6%, 8.4%-16.4% and 0.03%-0.18%, respectively.

[0029] For the lightweight concrete scratch-attached base having a rough surface described in the specific measures in (2), the ingredients of the material are modified dark color pigment, calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, where the weight percentages of the modified dark color pigment, calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.6-3.0%, 0.4-2.35%, 21.8%-34.5%, 24.6%-37.5%, 15.8%-29.6%, 8.4%-16.4% and 0.03%-0.18%, respectively.

[0030] In the cement-based bioadhesive base described in the specific measures in (2), circular holes with a diameter of 3 to 5 mm are created during molding.

[0031] Regarding the concentrated attachment and metamorphosis period of oyster larvae described in the specific measures in (3), it is generally from May to August in North China and from April to October in South China.

[0032] Regarding the cement-based paint for attracting sessile organisms on the marine project surface mentioned in the specific measures in (4), the specific technical solutions are as follows:

[0033] The ingredients of the material are cementitious material, sand, water, dark color pigment, bio-calcium powder, calcium carbonate powder, trace elements, wood fiber, dispersible rubber powder and superplasticizer, and the weight ratio thereof is 1:(0.35~0.7):(0.20~0.60):(0.02~0.10):(0.02~0.10):(0.02~0.10):(0.01~0.08):(0.04~0.12):(0.05~0.15):(0.001~0.010) in that order.

[0034] Preferably, the deep color pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red.

[0035] Preferably, the dark pigments are modified with one of the following materials depending on their impact on concrete performance: transparent resin, organosilicon, dimethylsiloxane, and superhydrophobic material.

[0036] Preferably, the biocalcium powder is bovine bone powder. or The powder contains one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, and has a powder size of 100 mesh to 1000 mesh.

[0037] Preferably, the biocalcium powder is prepared by treating eggshell powder, coral powder, oyster shell powder and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid and sulfurous acid, and treating cow bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.

[0038] Preferably, the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, and processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultra-fine precipitated calcium carbonate, and has a fineness of greater than 200 mesh.

[0039] Preferably, the trace elements zinc, iron, potassium and phosphorus are modified by selecting natural minerals, industrial products or chemical reagents including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to realize sustained release of corresponding ions and reduce or eliminate the adverse effects on concrete performance. However, in the case of eutrophication areas, materials containing nitrogen or phosphorus elements are not selected.

[0040] Preferably, the cementitious material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, where the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material includes one of alkali-activated slag and alkali-activated slag + fly ash.

[0041] Preferably, the sand is one or more of river sand, machine-made sand (whose parent material is limestone, basalt, or granite), and sea sand, each having a particle size of 0.16 mm to 2.36 mm.

[0042] Preferably, the superplasticizer is one of the following: carboxylic acid, naphthalene type.

[0043] A cement-based coating for attracting sessile organisms to marine project surfaces and a method for producing the same are provided. Step S1 of measuring cementitious material, sand, water, dark pigment, biocalcium powder, calcium carbonate powder, trace elements, wood fiber, dispersible rubber powder and superplasticizer; Step S2: putting the cementitious material, the dark color pigment, the biocalcium powder, the calcium carbonate powder, and the trace elements into a material mixer and uniformly mixing them for 2 to 5 minutes at a rotation speed of 1000 to 1500 revolutions per minute; Next, in step S3, sand, wood fiber, and dispersible rubber powder are put into a mixer and mixed for 5 to 10 minutes at a rotation speed of 500 to 1000 revolutions per minute; The method includes a step S4 of sufficiently dissolving a powdered superplasticizer in water, then placing the powdered superplasticizer and the mixed materials together in a high-speed mixer and mixing the mixture at a rotation speed of 1000 to 1500 revolutions per minute for 5 to 10 minutes.

[0044] This makes it possible to produce a cement paint with excellent attractant effect for attracting sessile organisms to the surface of a marine project.

[0045] The ropes mentioned in the specific measures in (5) are one of palm ropes, glass fiber ropes, and basalt fiber ropes.

[0046] The objective of the present invention is to invent a coating material that can be applied and cured directly in a humid environment, which can rapidly and densely attach sessile organisms to the concrete surface, and utilize the adhesion properties of oysters to achieve biological corrosion protection, while the large amount of sessile organisms also plays a role in purifying water bodies and restoring ecosystems. This solves the problems of limited effectiveness, short service life, high cost, and urgent need to restore marine ecosystems due to ecosystem degradation in tidal and underwater areas of marine concrete projects.

[0047] The realization method of the present invention is as follows: In the present invention, by using low-alkalinity cementitious material, wood fiber, dispersible rubber powder and superplasticizer, and adding modified dark pigment, modified bio-calcium powder, calcium carbonate powder and trace elements to the paint, the prepared cement-based paint has the function of effectively inducing the attachment and metamorphosis of oyster larvae, and achieves the effect of dense and uniform attachment of oysters, and utilizes the fastening property of oysters to improve the durability of concrete structures, and does not pollute the marine environment.

[0048] The present invention further has the following structural features.

[0049] The ingredients of the material are cementitious material, sand, water, dark color pigment, bio-calcium powder, calcium carbonate powder, trace elements, wood fiber, dispersible rubber powder and superplasticizer, and the weight ratio thereof is 1:(0.35~0.7):(0.20~0.60):(0.02~0.10):(0.02~0.10):(0.02~0.10):(0.01~0.08):(0.04~0.12):(0.05~0.15):(0.001~0.010) in that order.

[0050] Preferably, the deep color pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red.

[0051] Preferably, the dark pigments are modified with one of the following materials depending on their impact on concrete performance: transparent resin, organosilicon, dimethylsiloxane, and superhydrophobic material.

[0052] Preferably, the biocalcium powder is bovine bone powder. or The powder contains one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, and has a powder size of 100 mesh to 1000 mesh.

[0053] Preferably, the biocalcium powder is prepared by treating eggshell powder, coral powder, oyster shell powder and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid and sulfurous acid, and treating cow bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid.

[0054] Preferably, the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, and processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultra-fine precipitated calcium carbonate, and has a fineness of greater than 200 mesh.

[0055] Preferably, the trace elements zinc, iron, potassium and phosphorus are modified by selecting natural minerals, industrial products or chemical reagents including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to realize sustained release of corresponding ions and reduce or eliminate the adverse effects on concrete performance. However, in the case of eutrophication areas, materials containing nitrogen or phosphorus elements are not selected.

[0056] Preferably, the cementitious material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, where the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material includes one of alkali-activated slag and alkali-activated slag + fly ash.

[0057] Preferably, the sand is one or more of river sand, machine-made sand (whose parent material is limestone, basalt, or granite), and sea sand, each having a particle size of 0.16 mm to 2.36 mm.

[0058] Preferably, the superplasticizer is one of the following: carboxylic acid, naphthalene type.

[0059] A cement-based coating for attracting sessile organisms to marine project surfaces and a method for producing the same are provided. Step S1 of accurately measuring cementitious material, sand, water, dark pigment, biocalcium powder, calcium carbonate powder, trace elements, wood fiber, dispersible rubber powder and superplasticizer; Step S2: putting the cementitious material, the dark color pigment, the biocalcium powder, the calcium carbonate powder, and the trace elements into a material mixer and uniformly mixing them for 2 to 5 minutes at a rotation speed of 1000 to 1500 revolutions per minute; Next, in step S3, sand, wood fiber, and dispersible rubber powder are put into a mixer and mixed for 5 to 10 minutes at a rotation speed of 500 to 1000 revolutions per minute; The method is characterized by including a step S4 of thoroughly dissolving a powdered superplasticizer in water, then placing the powdered superplasticizer and the mixed materials together in a high-speed mixer and mixing them at a rotation speed of 200 to 500 revolutions per minute for 5 to 10 minutes.

[0060] This makes it possible to produce a cement-based paint with excellent attractant effect for attracting sessile organisms to marine project surfaces.

[0061] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0062] In the present invention, a cement-based paint for attracting sessile organisms on the marine project surface is applied to the surface of natural stone blocks, and a rough-surfaced concrete oyster attachment base is placed on the stone pile, so that oyster larvae can attach to the stone blocks quickly and densely, and oysters can obtain sufficient nutrients during the process of attachment, metamorphosis and development. And a reasonable spatial layout is used, and when the ocean current load is large, each stone pile (stone block) can effectively dissipate waves, and the water bodies on both sides of the breakwater can be smoothly exchanged under normal conditions. After the oysters attached to each stone pile (stone block) reproduce in large numbers, the ecological breakwater can also purify the water body and improve the ecological environment of the surrounding sea area. In this way, the problem of the traditional breakwater hindering the exchange of water bodies on both sides, changing the pH value of the local sea area, and further destroying the ecological environment is completely solved, and it can be used to restore the ecological environment of the sea area.

[0063] At present, there is no environmentally friendly and economical method for the durability of marine concrete or the ecologicalization of marine concrete projects. Oysters, as marine "ecological engineers", have the function of densifying the surface of concrete structures and improving the ecological environment. The cement-based paint for attracting sessile organisms provided by the present invention not only has the characteristics of quickly attracting sessile organisms to attach, transform, and promote long-term growth, but also has the characteristics of easy construction and application. It can be applied to new marine projects, especially marine projects with a large amount of in-use. It can not only improve the durability of reinforced concrete structures, but also easily and economically realize the restoration of the marine ecological environment. It can not only greatly expand the application of corrosion prevention of marine sessile organisms to in-use reinforced concrete structures, but also be widely used in marine ecological environment restoration projects. [Brief description of the drawings]

[0064] [Figure 1]Mold grows on the surface of concrete that has a different mix ratio, that is, 10% cow bone powder mixed in. [Diagram 2] The powder size is 200 mesh, and the mixing ratio is different when 10% modified cow bone powder is mixed. [Diagram 3] FIG. 1 is a schematic diagram of a 210-day actual marine adhesion experiment. [Figure 4] This is a schematic diagram of a 300-day actual marine adhesion experiment. [Diagram 5] FIG. 1 is a schematic diagram of a concrete oyster attachment base. [Figure 6] FIG. 1 is a schematic diagram of a concrete oyster attachment base. [Figure 7] FIG. 1 is a schematic diagram of a concrete oyster attachment base. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0065] The present invention will now be described in detail with reference to examples, which are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0066] The specific technical solutions of the project plan are as follows:

[0067] Example 1 (1) In the survey of the sea area where the breakwater will be constructed, the dominant species of oysters in the sea area and the presence or absence of oysters will be surveyed, and tests will be conducted 15 times every quarter to measure the air temperature, seawater temperature, dissolved oxygen, planktonic organisms, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca in the sea area. 2+ , Zn 2+ , K + record the occurrence of tropical cyclones, investigate the number of tropical cyclones and their intensity in the past, examine meteorological and hydrological data of the sea area over the years, and analyze feasible methods and solutions for the construction of ecological riprap breakwaters;

[0068] (2) In the manufacture of the concrete adhesion base, eco-concrete is used to manufacture a lightweight concrete oyster adhesion base with a rough surface. The size of the adhesion base is 10 cm x 10 cm x 2 cm. After being demolded, it is immediately subjected to CO2 curing at 10 atmospheres for 1 hour, and then to standard curing for 28 days.

[0069] (3) To ensure the timely and quantitative harvesting and cultivation of oyster larvae, a rough lightweight concrete oyster attachment base was placed in a nearby sea area in July, and the attachment rate of oyster larvae was set at 20 oysters / 100 cm. 2 In this case, seedling collection is stopped and the attached substrate is then moved to an area of ​​sea where food is abundant for floating culture.

[0070] (4) Treating the rock surface: inspecting the rock surface, cleaning the rock surface of impurities and chemical contaminants, and applying a cement-based paint to the marine project surface to attract sessile organisms when the saturated surface dries;

[0071] (5) Regarding the placement of the stones, in June of the second year, they will be placed in a dispersed manner, and stones with a volume of more than 1 cubic meter will be placed individually, and each stone will be covered with a rope basket. The rope basket will then cover multiple stone blocks with a volume of less than 1 cubic meter, forming a stone pile with a volume of 1 to 5 cubic meters, with an internal porosity of 50%. The rocks or stone piles will be connected with ropes, etc., and the distance between each stone block (stone pile) will be maintained at 4 meters.

[0072] (6) Regarding the placement of oyster attachment substrates at the site, substrates with a good adhesion of oysters (at the mature stage of gland development) to the concrete surface are transported to the sea area where the breakwater is to be constructed, and oyster attachment substrates are placed on each stone block (stone pile), and the stone blocks or stone piles are secured with ropes;

[0073] (7) Regarding the management and monitoring of oyster larvae attachment, the attachment density of oyster larvae on the concrete surface is 35 pieces / 100 cm 2 When the number of oysters reaches 100, the oyster attachment substrate is removed, and at the same time, it is decided whether or not to feed the oysters based on the type and number of planktonic organisms in the sea area.

[0074] Example 2 (1) Regarding the survey of the marine area in which the breakwater will be constructed, the dominant species of oysters in the said marine area and the presence or absence of oysters will be surveyed, and tests will be conducted 15 times every quarter to measure the air temperature, seawater temperature, dissolved oxygen, planktonic organisms, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca in the said marine area. 2+ , Zn 2+ , K + record the occurrence of tropical cyclones, investigate the number of tropical cyclones and their intensity in the past, examine meteorological and hydrological data of the sea area over the years, and analyze feasible methods and solutions for the construction of ecological riprap breakwaters;

[0075] (2) In the manufacture of the concrete adhesion base, eco-concrete is used to manufacture a lightweight concrete oyster adhesion base with a rough surface. The size of the adhesion base is 10 cm x 10 cm x 3 cm. After being demolded, it is immediately subjected to CO2 curing at 10 atmospheres for 1.5 hours, and then to standard curing for 28 days.

[0076] (3) To ensure the timely and quantitative harvesting and cultivation of oyster larvae, a rough lightweight concrete oyster attachment base was placed in a nearby sea area in August, and the attachment rate of oyster larvae was set at 25 oysters / 100 cm. 2 In this case, seedling collection is stopped and the attached substrate is then moved to an area of ​​sea where food is abundant for floating culture.

[0077] (4) Treating the rock surface: inspecting the rock surface, cleaning the rock surface of impurities and chemical contaminants, and applying a cement-based paint to the marine project surface to attract sessile organisms when the saturated surface dries;

[0078] (5) Regarding the placement of the stones, in July of the second year, they will be placed in a dispersed manner, and stones with a volume of more than 1 cubic meter will be placed individually, and each stone will be covered with a rope basket. The rope basket will then cover multiple stone stones with a volume of less than 1 cubic meter, forming a stone pile with a volume of 1 to 5 cubic meters, with an internal porosity of 60%. The rocks or stone piles will be connected with ropes, etc., and the distance between each stone block (stone pile) will be maintained at 5 meters.

[0079] (6) Regarding the placement of oyster attachment substrate at the site, substrate with a concrete surface to which oysters (at the mature stage of gland development) can attach well will be transported to the sea area where the breakwater will be constructed, and an oyster attachment substrate will be placed on each stone block (stone pile), and the stone block or stone pile will be secured with ropes.

[0080] (7) Regarding the management and monitoring of oyster larvae attachment, the attachment density of oyster larvae on the concrete surface is 40 pieces / 100 cm 2 When the number of oysters reaches 100, the oyster attachment substrate is removed, and at the same time, it is decided whether or not to feed the oysters based on the type and number of planktonic organisms in the sea area.

[0081] The mixing ratio of the oyster adhesion base and the cement-based paint described in Example 1 and Example 2 is as follows. The shape design of the concrete oyster adhesion base is specifically shown in Figures 5 to 7.

[0082] The concrete mix ratio for the rough surface lightweight concrete oyster attachment base (1-25) and the mix ratio for the cement-based paint (26-35) for attracting sessile organisms to the marine project surface are as follows:

[0083] 1. Regarding the concrete mix ratio of ordinary Portland cement, the weight percentages of ordinary Portland cement, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water-reducing agent powder are 29.37%, 33.53%, 24.48%, 12.59% and 0.03%, respectively.

[0084] The lightweight coarse aggregate is one or two of crushed lightweight porous basalt and lightweight ceramsite, the maximum particle size of which is less than 20 mm. The lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, the particle size of which is 0.2 mm to 5 mm and has a high grade. The water must meet the quality standard for water for concrete (JGJ63-2006) and must be free of Cl. - The content is <1000mg / L, the pH value is >4.5, and there is little effect on the initial setting time difference, final setting time, strength, and permeability of cement. In addition, the above materials selected in 1 to 25 are the same.

[0085] 2. Regarding the mix ratio of the standard concrete, the weight percentages of ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 17.62%, 1.47%, 10.28%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0086] 3. The weight percentages of unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.57%, 24.48%, 12.59% and 0.03%, respectively.

[0087] 4. The weight percentages of unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.28%, 8.99%, 33.57%, 24.48%, 12.59% and 0.03%, respectively.

[0088] 5. The weight percentages of unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.18%, 8.23%, 33.57%, 24.48%, 12.59% and 0.03%, respectively.

[0089] 6. The weight percentages of modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0090] 7. The weight percentages of modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.28%, 8.99%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0091] 8. The weight percentages of modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.18%, 8.23%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0092] The modified dark pigment is 196 transparent resin, mixed with 3% hardener and 1.5% accelerator, and the volume ratio of pigment to resin is 1:0.2. It is cured at room temperature for 4 hours, then cured at 60℃ for 4 hours, and then crushed by beating and ground by vibration mill until the powder size exceeds 400 mesh.

[0093] 9. The weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0094] 10. The weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.28%, 8.99%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0095] 11. The weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.18%, 8.23%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0096] 12. The weight percentages of modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 0.87%, 17.62%, 1.18%, 8.23%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0097] 13. The weight percentages of modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 1.47%, 17.62%, 1.10%, 7.71%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0098] 14. The weight percentages of modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 2.35%, 17.62%, 0.99%, 6.94%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0099] 15. The weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0100] 16. The weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.28%, 8.99%, 33.57%, 24.48%, 12.59% and 0.03%, respectively.

[0101] 17. The weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.18%, 8.23%, 33.57%, 24.48%, 12.59% and 0.03%, respectively.

[0102] 18. The weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.57%, 24.48%, 12.59% and 0.03%, respectively.

[0103] 19. The weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.28%, 8.99%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0104] 20. The weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.18%, 8.23%, 33.57%, 24.48%, 12.59% and 0.03%, respectively.

[0105] The method for modifying the bone powder is as follows: 100 mesh bone powder is added to a 2% phosphoric acid solution, the weight ratio of the two is 1:3, the temperature is 20-30°C, the mixer is stirred at 200-500 revolutions / min for 30 minutes, the centrifuge is centrifuged at 3000-5000 revolutions / min for 3 minutes, the supernatant is discarded, and the centrifuged solid is washed with water 2-3 times, the washing water is not acidic, the centrifuged solid is vacuum dried at 40°C, the dried bone powder and slag powder are mixed in a ratio of 1:4, and the powder is ground in a vibration mill until the powder size exceeds 200 mesh, and then it is prepared for use.

[0106] 21, the weight percentages of calcium carbonate powder, zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), ordinary Portland cement, blast furnace slag powder, silica fume, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 0.5%, 1.47%, 17.62%, 0.93%, 6.50%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0107] 22, the weight percentages of calcium carbonate powder, zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), ordinary Portland cement, blast furnace slag powder, silica fume, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 1.2%, 1.47%, 17.62%, 0.84%, 5.89%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0108] 23, the weight percentages of zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder in a ratio of 2:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.5%, 1.47%, 1.47%, 0.87%, 17.62%, 0.93%, 6.50%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0109] 24, the weight percentages of zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder in a ratio of 2:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.6%, 1.47%, 1.47%, 0.87%, 17.62%, 0.84%, 5.89%, 33.57%, 24.48%, 12.59%, and 0.03%, respectively.

[0110] The method of modifying zinc sulfate is as follows: select diatomaceous earth with SiO2 content >90% and fineness of 600 mesh, add 150g water in a mixer at 60°C, then add 100g zinc sulfate, stir until completely dissolved, and prepare for use; then heat 150g of the above diatomaceous earth to 60°C, add it to the solution, stir for 10 minutes in a mixer with a rotation speed of 200-500 revolutions / min, and then dry in a drying oven with a drying temperature of 100°C to obtain the modified zinc sulfate.

[0111] 25, the weight percentages of zinc sulfate, modified dark pigment, modified bio-calcium powder (modified cow bone powder: oyster shell powder = 2:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water, short fiber and polycarboxylate water reducer powder are 0.5%, 1.47%, 1.47%, 0.87%, 17.62%, 0.93%, 6.50%, 33.07%, 24.18%, 12.59%, 0.8%, and 0.03%, respectively.

[0112] 26. The weight ratio of cementitious material, sand, water, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder=2:1), calcium carbonate powder, zinc sulfate, wood fiber, dispersible rubber powder and superplasticizer is 1:0.5:0.4:0.03:0.03:0.03:0.02:0.06:0.06:0.005.

[0113] 27. The weight ratio of cementitious material, sand, water, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder=2:1), calcium carbonate powder, zinc sulfate, wood fiber, dispersible rubber powder and superplasticizer is 1:0.5:0.4:0.05:0.05:0.05:0.02:0.06:0.06:0.005, respectively.

[0114] 28. The weight ratio of cementitious material, sand, water, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder=2:1), calcium carbonate powder, zinc sulfate, wood fiber, dispersible rubber powder and superplasticizer is 1:0.5:0.4:0.05:0.05:0.05:0.04:0.08:0.09:0.005, respectively.

[0115] 29. The weight ratio of cementitious material, sand, water, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder=2:1), calcium carbonate powder, zinc sulfate, wood fiber, dispersible rubber powder and superplasticizer is 1:0.5:0.4:0.08:0.08:0.08:0.04:0.08:0.09:0.005, respectively.

[0116] 30, the weight ratio of cementitious material, sand, water, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder=2:1), calcium carbonate powder, zinc sulfate, wood fiber, dispersible rubber powder and superplasticizer is 1:0.5:0.4:0.08:0.08:0.08:0.06:0.10:0.12:0.005, respectively.

[0117] 31. The weight ratio of cementitious material, sand, water, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder=2:1), calcium carbonate powder, zinc sulfate, wood fiber, dispersible rubber powder and superplasticizer is 1:0.5:0.4:0.03:0.03:0.03:0.04:0.06:0.06:0.005.

[0118] 32. The weight ratio of cementitious material, sand, water, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder=2:1), calcium carbonate powder, zinc sulfate, wood fiber, dispersible rubber powder and superplasticizer is 1:0.5:0.4:0.05:0.05:0.05:0.04:0.06:0.06:0.005, respectively.

[0119] 33. The weight ratio of cementitious material, sand, water, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder=2:1), calcium carbonate powder, zinc sulfate, wood fiber, dispersible rubber powder and superplasticizer is 1:0.5:0.4:0.05:0.05:0.05:0.02:0.08:0.09:0.005, respectively.

[0120] 34. The weight ratio of cementitious material, sand, water, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder=2:1), calcium carbonate powder, zinc sulfate, wood fiber, dispersible rubber powder and superplasticizer is 1:0.5:0.4:0.08:0.08:0.08:0.06:0.08:0.09:0.005, respectively.

[0121] 35, the weight ratio of cementitious material, sand, water, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), modified bio-calcium powder (modified cow bone powder:oyster shell powder=2:1), calcium carbonate powder, zinc sulfate, wood fiber, dispersible rubber powder and superplasticizer is 1:0.5:0.4:0.03:0.03:0.03:0.06:0.10:0.12:0.005, respectively.

[0122] The modification method of the modified dark pigment is as follows: Use 196 transparent resin, mix 3% hardener and 1.5% accelerator, mix with pigment, and the volume ratio of pigment to resin is 1:0.2, cure at room temperature for 4 hours, cure at 60℃ for 4 hours, then crush by beating, and grind by vibration mill until the powder size exceeds 400 mesh.

[0123] The method for modifying the bone powder is as follows: 100 mesh bone powder is added to a 2% phosphoric acid solution, the weight ratio of the two is 1:3, the temperature is 20-30°C, the mixer is stirred at 200-500 revolutions / min for 30 minutes, the centrifuge is centrifuged at 3000-5000 revolutions / min for 3 minutes, the supernatant is discarded, and the centrifuged solid is washed with water 2-3 times, the washing water is not acidic, the centrifuged solid is vacuum dried at 40°C, the dried bone powder and slag powder are mixed in a ratio of 1:4, and the powder is ground in a vibration mill until the powder size exceeds 200 mesh, and then it is prepared for use.

[0124] The method of modifying zinc sulfate is as follows: select diatomaceous earth with SiO2 content >90% and fineness of 600 mesh, add 150g water in a mixer at 60°C, then add 100g zinc sulfate, stir until completely dissolved, and prepare for use; then heat 150g of the above diatomaceous earth to 60°C, add it to the solution, stir for 10 minutes in a mixer with a rotation speed of 200-500 revolutions / min, and then dry in a drying oven with a drying temperature of 100°C to obtain the modified zinc sulfate.

[0125] Reference 1, Living Breakwaters - Green Infrastructure for the New York Coast - Mago Ichiro

[0126] In Reference 1, a "living" breakwater is constructed, and the number of marine organisms is increased by macro design, surface texture, and concrete components made with low-alkali cement. The increased marine organisms are marine plants and marine sessile organisms, mainly marine plants. In the present invention, in addition to reducing the alkalinity of cement, dark color pigments, biocalcium powder, calcium carbonate powder, and trace elements are mixed into the concrete to attract oyster larvae, which are characterized by rapid and dense attraction, and are highly effective, greatly improving the ecological environment of the marine area.

[0127] Compared with Reference 2, Biomimetic Concrete Artificial Reef and Its Manufacturing Method 2015 CN104938384 A, the differences are as follows:

[0128] (1) The object of the present invention is different from that of Reference 2, in which a cement mortar mixed with crushed oyster shells is applied to the concrete surface, but the object is to improve the aquatic environment by attracting fish, microorganisms and algae through biomimetic surface and increasing the number of microorganisms, and oysters are not mentioned. The object of the cement-based paint of the present invention is to attract oysters to attach.

[0129] (2) According to Reference 2, in cement mortar, biocalcium carbonate powder (150-200 mesh) less than 10% of the cement dosage is ineffective against adhesion by attraction. However, in the research process of the present invention, by using a cement-based paint (fineness of 100-1000 mesh) mixed with modified cow bone powder and biocalcium carbonate powder, it is found that the optimal dosage of cow bone powder and biocalcium carbonate powder is less than 10% of the cementitious material.

[0130] (3) The modification of beef bone powder and biocalcium carbonate powder specifically involves treating eggshell powder, coral powder, oyster shell powder, and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid, sulfurous acid, etc., and treating beef bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid, and nitric acid.

[0131] (4) In the references, it is difficult to embed oyster shells on the concrete surface, and not all project surfaces use this method, which is not feasible. The present invention can achieve the excellent effect of attracting sessile organisms by applying a layer of cement-based paint to the concrete surface, which does not require embedding oyster shells, is not only easy to apply, but also greatly improves the amount of oyster adhesion.

[0132] (5) In recent years, serious corrosion of artificial reefs has been observed in marine environments. The serious corrosion is mainly caused by the combined action of biological sulfuric acid secreted by anaerobic microorganisms such as Thiobacillus subtilis and acidic substances secreted by other bacteria. However, calcium carbonate has very poor resistance to acid corrosion. If the content of calcium carbonate with large fineness is too high, it can cause serious acid corrosion.

[0133] Compared to Reference 3 (Fan Ruiliang: The effects of substrate type on oyster attachment, growth, population establishment and reef development [D]), the differences are as follows:

[0134] (1) In Reference 3, 80 mesh cow bone powder, calcium powder, and gypsum powder are taken and mixed into concrete separately. The fineness of all calcium materials in this invention is more than 100 mesh, which is larger than the fineness of the materials in Reference 3. Similarly, cow bone powder is modified for mixing, taking into account the grading of paint and concrete particles and their attracting ability.

[0135] (2) At room temperature, when the cow bone powder is crushed by a vibrating mill and the fineness exceeds 80 mesh, the cow bone powder contains a large amount of collagen, so it becomes lumpy and cannot be crushed further. In the present invention, by using the dilute acid modification technology and crushing with other substances, cow bone powder with small particle size and modified bio-calcium powder with fineness > 200 mesh can be obtained. The obtained bio-calcium powder retains the original substance of bio-calcium, improves the release rate of the substance for attracting oyster larvae to attach, and reduces the dosage of bio-calcium powder, thereby reducing the impact on paint and concrete performance.

[0136] (3) Bone powder contains a large amount of organic substances such as collagen. Mixing a large amount of these substances will reduce the strength and permeation resistance of paint and concrete. Especially when the dosage exceeds 5%, the strength of paint and concrete will rapidly decrease, the permeation resistance will be significantly reduced, and mold will grow on the paint and concrete surface under standard curing conditions. Figure 1 shows the mold growing on the concrete surface. Figure 2 shows the surface of the modified concrete.

[0137] As can be seen from Figure 1, the mold on the concrete surface is white and cotton-like, covering almost the entire concrete surface, while when the cow bone powder, age and curing conditions are the same, there is no mold on the concrete surface in Figure 2.

[0138] The present invention uses dilute acid modification and composite crushing technology to fully utilize the attractant ability of cow bone powder, greatly reduce the dosage of cow bone powder, and perform anti-corrosion treatment and modification to produce a composite attractant mainly made of cow bone powder, which is low in dosage and has little effect on the strength and permeability of paint and concrete. At the same time, it has high oyster larvae adhesion ability and solves the problem of mold growth on paint and concrete. In addition, compared with concrete without attractant, the number of oyster larvae attached to concrete mixed with attractant is greatly increased. Specifically, see Figure 3.

[0139] As can be seen from the references and the materials examined, calcium content is essential for the attachment of oyster larvae, and some current test results also prove that mixing an appropriate amount of calcium carbonate material into cement-based materials can promote the attachment and growth of oyster larvae. However, cement paint and cement concrete contain a large amount of calcium ions, and the pH value of the pore solution is generally above 12.5, and at room temperature, the pH value of saturated calcium hydroxide solution is about 12, so the calcium ion concentration in the concrete pore solution is about 5 mmol / L, and the solubility of calcium carbonate is very low, at 25°C, it is 9.5×10 -5 mol / L(9.5×10 -2 Currently, the optimal range of calcium ion concentration for attracting oysters to attach is thought to be 10-25 mmol / L, and even when oyster larvae are placed in a saturated calcium carbonate solution, there is not enough Ca to provide the ion concentration suitable for oyster attachment. 2+ Furthermore, while Ca(OH)2 in cement paint and concrete can be released quickly, it takes time for calcium carbonate to dissolve. Therefore, when calcium carbonate materials are mixed into paint and concrete to promote the attachment of oyster larvae, Ca 2+ It can be determined that HCO3 does not play a dominant role. - In the case of transformation, Ca 2+ Together with the calcium carbonate, a secondary shell of calcium carbonate is formed. After calcium carbonate is mixed in, it reacts with CO2 and water to generate Ca(HCO3)2, which is involved in adhesion and is the basic mechanism that promotes the adhesion of oyster larvae.

[0140] There is an optimal amount of calcium carbonate for cement-based materials, which can be explained by the following three aspects:

[0141] 1) With the same amount of substitute cement, as the dosage of calcium carbonate increases, the alkali in the paint and concrete is diluted, and the total alkalinity decreases. However, as the dosage of calcium carbonate increases, the probability of dissolving calcium carbonate in the paint and concrete increases, and the HCO3 in the solution increases.- The content is improved, which promotes the adhesion and transformation of oysters. However, if the dosage is too large, the permeability of the paint and concrete will increase rapidly, and the alkali and carbonate in the paint and concrete will rapidly leach out, the adverse effect of the alkali will become obvious, and the critical effect or adverse effect of the carbonate will begin to appear, resulting in a decrease in the adhesion amount;

[0142] 2) With the same amount of substitute aggregate, the permeability of paint and concrete decreased with increasing dosage, and calcium ions and OH - The leaching of calcium ions decreased, but the permeability of carbonate ions gradually improved and reached a certain value, and the attachment of oysters reached its maximum value. As the dosage continued to increase, the calcium ions decreased significantly, and carbonates may also decrease. The calcium ion concentration limited the attachment of oyster larvae, which was manifested as a decrease in the attachment amount.

[0143] 3) With the same amount of alternative mineral admixture, the permeability improved with increasing dosage, and the increase in calcium carbonate reduced the amount of HCO3 required for oyster attachment. - As the concentration reaches the appropriate range, which is manifested as improved oyster larval attachment, and the mineral admixture dosage continues to increase, the mineral admixture dosage decreases, and the amount of leached alkali and carbonate increases, but the alkali and HCO3 - Too many ions inhibit the attachment of oyster larvae.

[0144] Compared to Reference 4 (Li Zhenzhen, Gong Pihai, Guan Changtao, et al. Bioadhesion effect of concrete artificial reefs with different cement types [J]. Progress in Fisheries Science, 2017, 38(5):57-63.), the differences are as follows:

[0145] In Reference 4, composite Portland cement, slag Portland cement, pozzolanic Portland cement, fly ash Portland cement and alumina cement are used, and in the present invention, ordinary Portland cement is mixed with mineral admixtures to realize low alkalinity segments, where silica fume is one of the mineral admixtures, which has high activity and appropriate dosage has obvious effect on improving the durability of reinforced concrete in marine environment, and low alkalinity cement with excellent strength and durability can be obtained through optimization design and testing. At the same time, due to the high penetration prevention characteristics of silica fume concrete, even if the alkalinity inside the concrete is high, a large number of oyster larvae can attach, transform and grow. In addition, the low alkalinity sulfoaluminate cement is mixed to adjust the alkalinity of cement concrete and provide a suitable pH value for the attachment of oyster larvae. In addition, marine plants and sessile organisms such as oysters and barnacles have different alkali tolerances, and the environments required during the attachment and later stages are different. For example, the attachment, metamorphosis and later growth of barnacles and oysters require large amounts of calcium ions.

[0146] In Reference 4, concrete is used to attract marine organisms, which mainly starts from the size and diversity of the attached organisms, the main attached organisms being various algae. In the present invention, the research objective is to attract oysters to attach, but the alkali resistance of oysters and barnacles is higher than that of algae, and the attachment and transformation of oysters requires a large amount of calcium ions, so although the two types of concrete look similar, they are actually quite different. Figures 4 and 5 respectively show a comparison of the biofouling situation after about 210 days of actual sea attachment experiment in Reference 3 and the biofouling situation after 300 days of actual sea attachment experiment in the present invention.

[0147] In Reference 4, concrete is used to attract marine organisms, mainly due to the size and diversity of the attached organisms, the main of which are various algae. In this invention, the research objective is to attract oysters to attach, but the alkali resistance of oysters and barnacles is higher than that of algae, and the attachment and transformation of oysters requires a large amount of calcium ions, so although the two types of concrete look the same, they are actually quite different.

[0148] Thus, similarly, this piece of knowledge relates to the interdisciplinary fusion of marine sessile organisms, marine plants and marine concrete engineering, and neither a person skilled in the field of concrete engineering nor a person skilled in the field of marine biology can obtain, according to Reference 3, the technical features in the present invention in which the reduction in alkalinity of concrete and the balance of calcium ion concentration are closely related to the attachment of marine sessile organisms.

[0149] The unique features and beneficial effects of the present invention are as follows:

[0150] Deep color pigment

[0151] Taking advantage of the phototaxis of oyster eyespot larvae, dark color pigments (one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red) are mixed into the concrete to change the color of the concrete, making the concrete darker and making the oyster larvae think that it is a dark environment, attracting the oyster larvae to reach the dark colored concrete surface by themselves, increasing the probability of contact between the oyster larvae and the concrete surface, and increasing the probability of attracting the oyster larvae to attach. Specifically, it is as follows.

[0152] (Researchers in marine biology have considered research into the attachment of marine sessile organisms using substrates of different colors to cultivate and grow or eliminate undesirable populations, which belongs to the field of marine biology. It is quite different from marine concrete engineering and concrete materials science, which are two major fields entirely. Through the interdisciplinary fusion of marine sessile organisms and concrete materials science, dark colored paints and concrete are used to attract oyster larvae to attach. The present invention adds dark color pigments to darken the color of the paints and concrete, promoting the attachment of oyster larvae. Other materials are mixed into the paints and concrete, thus affecting their performance. The present invention considers that concretes of different cements have different surface colors. Thus, the concretes of different cements have different surface colors. The dosage of the dark color material is determined based on the type and dosage of the cement. The dark color pigment also affects the paint and concrete performance. The most important thing is that if the penetration rate of alkali and Ca2+ in the paint and concrete is not controlled while mixing the dark color pigment, the released alkali will affect the attachment, metamorphosis and growth of the sessile organism larvae, and if the dosage exceeds a certain value, the attachment amount of the larvae will decrease. In the present invention, the penetration prevention property of the concrete is designed and controlled, and the main measures are the selection of the type of dark color pigment, the control of the dosage and modification. With the increase in the dosage of the dark color material, the attachment amount of the larvae will be higher, and when the dosage is 0.5%-6% of the cementitious material, the attachment amount of the larvae is the highest, but then increases slightly or does not change.

[0153] trace elements

[0154] The oyster body contains a large amount of zinc, much higher than the seawater in which it lives, and at the same time, the oyster body contains a lot of Fe, P, and K elements. At the same time, adequate Zn in the solution 2+ and K + The concentration of zinc phosphate, potassium phosphate, ammonium phosphate, zinc sulfate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, iron phosphate, and calcium phosphate were used as trace elements and mixed into concrete.

[0155] By modifying the concrete with these substances, the strength and permeability prevention of the concrete are basically unchanged, but the attachment attraction rate of oyster larvae is greatly improved.

[0156] Marine biology researchers have studied the effects of different ions on the attachment and metamorphosis of marine sessile organisms, which belongs to the field of marine biology, in order to clarify the attachment mechanism of oysters and the purpose of their cultivation and propagation. It is completely different from marine concrete engineering and concrete materials science, which are completely two major fields. It can be seen that the interdisciplinary fusion of marine sessile organisms and concrete materials science can add corresponding substances into paint and concrete to attract oyster larvae to attach to the cleat surface. Since soluble salts have a great impact on concrete performance such as early workability, hardening time, and later strength and anti-penetration properties, the present invention uses diatomaceous earth as a carrier to fix these inorganic salts inside diatomaceous earth, reducing the impact of soluble salts on paint and concrete performance, while utilizing the effect of diatomaceous earth to improve paint and concrete performance, and realizes that the excellent performance of paint and concrete can be maintained even if these attractants are added. In addition, since diatomaceous earth has a sustained release effect as a carrier, the release of soluble salts is relatively slow, and the release rate is kept at a very low level, especially after immersion in seawater for a certain period of time. Therefore, similarly, this part of knowledge relates to the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether a person skilled in the field of concrete engineering or a person skilled in the field of marine biology, due to the conventional background, in the present invention, by mixing trace elements into paint and concrete, changing the ion content of trace elements on the paint and concrete surface, and controlling the permeability of concrete, it is impossible to obtain technical characteristics closely related to paint and concrete with excellent ability to attract oyster larvae to attach.

[0157] Permeability of paint and concrete

[0158] The strength and permeability of paint and concrete are the two most important performances of paint and concrete. Mixing different attractants into paint and concrete will affect the performance of paint and concrete, so when mixing different substances to promote the attachment, metamorphosis and subsequent growth of oyster larvae, first, it is necessary to control as a whole so as not to have a significant effect on the strength and permeability of paint and concrete, and second, select raw materials according to the suitability of various raw materials, and if the performance of the raw materials cannot meet the actual requirements, the desired function can be achieved by modifying them before adding the raw materials. However, in fact, the above-mentioned related research considers the effect of calcium content on the attachment of oyster larvae, but does not consider the performance of the concrete itself, and does not consider the water-cement ratio, calcium content and curing, etc., and the change in the permeability of paint and concrete will change the permeability of alkali and ions inside the paint and concrete, and the lower the permeability of paint and concrete, the higher the permeability of alkali and ions inside it will be, which may increase exponentially. Therefore, these released alkalis and ions have a great impact on the larvae, changing from promoting attachment to inhibiting attachment, and this situation may become more serious, especially when the cement dosage is high. Therefore, by mixing the attractant into the paint and concrete, it is necessary to ensure that the change in the impermeability of the paint and concrete is within a controllable range, for example, the change does not exceed 10%. In this way, the attractant effects can be compared, otherwise the influence of mixing the attractant independently or mixing the attractants in combination on the attractant effect on oyster larvae cannot be evaluated.

[0159] It is necessary to grasp the optimal environment required for marine sessile organisms to attach, transform and grow later, and to design paints and concrete starting from the penetration resistance of paints and concrete, and not to ignore the fact that only considering the dosage of various raw materials will bring about changes in the penetration resistance of paints and concrete. Therefore, similarly, this part of knowledge concerns the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether a person skilled in the field of concrete engineering or a person skilled in the field of marine biology, according to the conventional background, in the present invention, the overall control of the penetration resistance of paints and concrete cannot obtain the technical characteristics that are closely related to the ability of the attractant to effectively attract oysters to attach.

[0160] Therefore, similarly, this part of knowledge is related to the interdisciplinary fusion of marine sessile organisms, marine plants, and marine concrete engineering, and neither a person skilled in the field of concrete engineering nor a person skilled in the field of marine biology can obtain the technical features closely related to the paint and concrete having the ability to effectively attract oysters to attach and high durability, by mixing dark color pigments into concrete, modifying cow bone powder, grinding technology, and controlling the permeability of paint and concrete, according to References 2-3. Also, according to Reference 4, the reduction in concrete alkalinity and the balance of calcium ion concentration cannot obtain the technical features closely related to the attachment of marine sessile organisms, according to Reference 4.

[0161] Hereinafter, the present invention will be described in detail with reference to Examples A1 to A10, and the specific implementation methods of these Examples A1 to A10 are the same as the implementation methods of the cement-based paints (26 to 35) for attracting sessile organisms to the surface of marine projects described above.

[0162] Compared with Reference 2 (Biomimetic concrete artificial reef and its manufacturing method 2015 CN104938384 A), the differences are as follows:

[0163] (1) The object of the present invention is different from that of Reference 2, in which a cement mortar mixed with crushed oyster shells is applied to the concrete surface, but the object is to improve the aquatic environment by attracting fish, microorganisms and algae through biomimetic surface and increasing the number of microorganisms, and oysters are not mentioned. The object of the cement-based paint of the present invention is to attract oysters to attach, which is mainly oysters, but the attachment of barnacles is taken into consideration when reinforced concrete in tidal areas has an anticorrosive effect.

[0164] (2) According to Reference 2, in cement mortar, biocalcium carbonate powder (150-200 mesh) less than 10% of the cement dosage is ineffective against adhesion by attraction. However, in the research process of the present invention, by using a cement-based paint (fineness of 100-1000 mesh) mixed with modified cow bone powder and biocalcium carbonate powder, it is found that the optimal dosage of cow bone powder and biocalcium carbonate powder is less than 10% of the cementitious material.

[0165] (3) The modification of beef bone powder and biocalcium carbonate powder specifically involves treating eggshell powder, coral powder, oyster shell powder, and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid, sulfurous acid, etc., and treating beef bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid, and nitric acid.

[0166] (4) In the references, it is difficult to embed oyster shells on the concrete surface, and not all project surfaces use this method, which is not feasible. The present invention can achieve the excellent effect of attracting sessile organisms by applying a layer of cement-based paint to the concrete surface, which does not require embedding oyster shells, is not only easy to apply, but also greatly improves the amount of oyster adhesion.

[0167] (5) In recent years, serious corrosion of artificial reefs has been observed in marine environments. The serious corrosion is mainly caused by the combined action of biological sulfuric acid secreted by anaerobic microorganisms such as Thiobacillus subtilis and acidic substances secreted by other bacteria. However, calcium carbonate has very poor resistance to acid corrosion. If the content of calcium carbonate with large fineness is too high, it can cause serious acid corrosion.

[0168] Compared to Reference 3 (Fan Ruiliang: The effects of substrate type on oyster attachment, growth, population establishment and reef development [D]), the differences are as follows:

[0169] (1) In Reference 3, 80 mesh cow bone powder, calcium powder, and gypsum powder are taken and mixed into concrete separately. The fineness of all calcium materials in this invention is more than 100 mesh, which is larger than the fineness of the materials in Reference 3. In addition, modified cow bone powder is mixed in, taking into account the grading of the paint particles and their attracting ability.

[0170] (2) At room temperature, when the cow bone powder is ground by a vibrating mill and the fineness exceeds 80 mesh, the cow bone powder contains a large amount of collagen, so it becomes lumpy and cannot be ground further. In the present invention, by using the dilute acid modification technology and grinding with other substances, cow bone powder with small particle size and modified bio-calcium powder with fineness > 200 mesh can be obtained. The obtained bio-calcium powder retains the original substance of bio-calcium, improves the release rate of the substance for attracting oyster larvae to attach, and reduces the dosage of bio-calcium powder, thereby reducing the impact on paint performance.

[0171] (3) Bone powder contains a large amount of organic substances such as collagen. Mixing a large amount of these substances will result in a decrease in the strength and permeation resistance of the paint. Especially when the dosage exceeds 5%, the strength of the paint will decrease rapidly, the permeation resistance will decrease significantly, and the paint will grow mold under standard curing conditions.

[0172] The present invention uses dilute acid modification and composite crushing technology to fully utilize the attracting ability of cow bone powder, greatly reducing the dosage of cow bone powder, and carrying out anti-corrosion treatment and modification to produce a composite attractant mainly made of cow bone powder, which has a low dosage, has little effect on the performance of the paint, and at the same time has a high oyster larvae attachment ability, and solves the problem of mold growth after coating. The amount of oyster larvae attached to concrete coated with paint containing an attractant is significantly higher than that of paint without the attractant.

[0173] As can be seen from the references and the materials examined, calcium content is essential for the attachment of oyster larvae, and some current test results also prove that mixing an appropriate amount of calcium carbonate material into cement-based materials can promote the attachment and growth of oyster larvae. However, cement-based paints contain a large amount of calcium ions, and the pH value of the pore solution is generally above 12.5. At room temperature, the pH value of saturated calcium hydroxide solution is about 12, so the calcium ion concentration in the pore solution is about 5 mmol / L, and the solubility of calcium carbonate is very low, at 25°C it is 9.5×10 -5 mol / L(9.5×10 -2 Currently, the optimal range of calcium ion concentration for attracting oysters to attach is thought to be 10-25 mmol / L, and even when oyster larvae are placed in a saturated calcium carbonate solution, there is not enough Ca to provide the ion concentration suitable for oyster attachment. 2+ Furthermore, while the Ca(OH)2 in the paint can be released quickly, it takes time for calcium carbonate to dissolve. Therefore, when mixing calcium carbonate material into the paint to promote the attachment of oyster larvae, Ca 2+ It can be determined that HCO3 does not play a dominant role. - In the case of transformation, Ca 2+ Together with the calcium carbonate, a secondary shell of calcium carbonate is formed. After calcium carbonate is mixed in, it reacts with CO2 and water to generate Ca(HCO3)2, which is involved in adhesion and is the basic mechanism that promotes the adhesion of oyster larvae.

[0174] There is an optimal amount of calcium carbonate for cement-based materials, which can be explained by the following three aspects:

[0175] 1) With the same amount of substitute cement, as the dosage of calcium carbonate increases, the alkali in the cement-based material is diluted and the total alkalinity decreases. However, as the dosage of calcium carbonate increases, the probability of dissolving calcium carbonate in the cement-based material increases, and the amount of HCO3 in the solution increases. - The content is improved, which promotes the adhesion and transformation of oysters. However, if the dosage is too large, the permeability of the cement-based material will increase rapidly, and the alkali and carbonate will be rapidly leached out, the adverse effect of the alkali will become obvious, and the critical effect or adverse effect of the carbonate will begin to appear, resulting in a decrease in the adhesion amount;

[0176] 2) With the same amount of substitute aggregate, the permeability of the cement-based material decreased with increasing dosage, and the calcium ions and OH - The leaching of calcium ions decreased, but the permeability of carbonate ions gradually improved and reached a certain value, and the attachment of oysters reached its maximum value. As the dosage continued to increase, the calcium ions decreased significantly, and carbonates may also decrease. The calcium ion concentration limited the attachment of oyster larvae, which was manifested as a decrease in the attachment amount.

[0177] 3) With the same amount of alternative mineral admixture, the permeability improved with increasing dosage, and the increase in calcium carbonate reduced the amount of HCO3 required for oyster attachment. - As the concentration reaches the appropriate range, which is manifested as improved oyster larval attachment, and the mineral admixture dosage continues to increase, the mineral admixture dosage decreases, and the amount of leached alkali and carbonate increases, but the alkali and HCO3 - Too many ions inhibit the attachment of oyster larvae.

[0178] Compared to Reference 4 (Li Zhenzhen, Gong Pihai, Guan Changtao, et al. Bioadhesion effect of concrete artificial reefs with different cement types [J]. Progress in Fisheries Science, 2017, 38(5):57-63.), the differences are as follows:

[0179] In Reference 4, composite Portland cement, slag Portland cement, pozzolanic Portland cement, fly ash Portland cement and alumina cement are used, and in the present invention, ordinary Portland cement is mixed with mineral admixtures to realize low alkalinity segments, where silica fume is one of the mineral admixtures, which has high activity and appropriate dosage has obvious effect on improving the durability of reinforced concrete in marine environment, and low alkalinity cement with excellent strength and durability can be obtained through optimization design and testing. At the same time, due to the high penetration prevention characteristics of silica fume concrete, even if the alkalinity inside the concrete is high, a large number of oyster larvae can attach, transform and grow. In addition, the low alkalinity sulfoaluminate cement is mixed to adjust the alkalinity of the cement-based paint and provide a suitable pH value for the attachment of oyster larvae. In addition, marine plants and sessile organisms such as oysters and barnacles have different alkali tolerances, and the environments required during the attachment and later stages are different. For example, the attachment, metamorphosis and later growth of barnacles and oysters require large amounts of calcium ions.

[0180] In Reference 4, concrete is used to attract marine organisms, mainly due to the size and diversity of the attached organisms, the main of which are various algae. In this invention, the research objective is to attract oysters to attach, but the alkali resistance of oysters and barnacles is higher than that of algae, and the attachment and transformation of oysters requires a large amount of calcium ions, so although the two types of cement-based materials look similar, they are actually quite different.

[0181] The unique features and beneficial effects of the present invention are as follows:

[0182] Deep color pigment

[0183] Taking advantage of the phototaxis of oyster eyespot larvae, dark color pigments (one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red) are mixed into the paint to change the color of the paint, making the paint darker and making the oyster larvae think that it is a dark environment, attracting the oyster larvae to reach the dark colored concrete surface by themselves, increasing the probability of contact between the oyster larvae and the concrete surface, and increasing the probability of attracting the oyster larvae to attach. Specifically, it is as follows.

[0184] Marine biology researchers have looked into the use of different colored substrates to cultivate and grow or eliminate undesirable populations, which belongs to the field of marine biology. It is completely different from marine concrete engineering and concrete materials science, which are two major fields entirely. The interdisciplinary fusion of marine sessile organisms and concrete materials science has led to the use of dark-colored paints to attract oyster larvae to attach. The present invention adds dark-colored pigments to darken the paint color and promote the attachment of oyster larvae. Since other materials are mixed into the paint, it affects its performance. The present invention considers that paints of different cements have different surface colors. Therefore, the dosage of the dark-colored material is determined based on the cement type and dosage. The dark-colored pigment also affects the performance of the paint. Most importantly, the dark-colored pigment is mixed in while simultaneously reducing the alkali and Ca in the paint. 2+ If the penetration rate is not controlled, the released alkali will affect the attachment, metamorphosis and growth of sessile organism larvae, and if the dosage exceeds a certain value, the amount of larvae attachment will decrease. In the present invention, the penetration prevention property of the cement-based paint is designed and controlled, and the main measures are the selection of the type of dark color pigment, the control of the dosage and modification. With the increase in the dosage of the dark color substance, the amount of larvae attachment will increase, and when the dosage is 0.5% to 6% of the cementitious material, the amount of larvae attachment is the highest, and then increases slightly or remains unchanged.

[0185] trace elements

[0186] The oyster body contains a large amount of zinc, much higher than the seawater in which it lives, and at the same time, the oyster body contains a lot of Fe, P, and K elements. At the same time, adequate Zn in the solution 2+ and K + The concentration can promote the early attachment and metamorphosis of oyster larvae. Therefore, zinc sulfate, potassium sulfate, potassium nitrate, iron sulfate, zinc phosphate, ammonium nitrate, potassium phosphate, ammonium phosphate, iron phosphate, and calcium phosphate are used as trace elements and mixed into the paint, and the modification of these substances basically does not change the strength and penetration prevention of the paint, but greatly improves the attachment attraction rate of oyster larvae. The specific details are as follows:

[0187] Marine biology researchers have studied the effects of different ions on the attachment and metamorphosis of marine sessile organisms in order to clarify the attachment mechanism of oysters and the purpose of their cultivation and propagation, which belongs to the field of marine biology. It is completely different from marine concrete engineering and concrete materials science, which are completely two major fields. It can be seen that the interdisciplinary fusion of marine sessile organisms and concrete materials science can add corresponding substances in the paint to attract oyster larvae to attach to the cleat surface. Since soluble salts have a great impact on the performance of paints, such as early workability, hardening time, and later strength and anti-penetration properties, the present invention uses diatomaceous earth as a carrier to fix these inorganic salts inside the diatomaceous earth, reducing the impact of soluble salts on the performance of paints, while at the same time utilizing the effect of diatomaceous earth in improving the performance of cement-based paints, and realizing that the excellent performance of cement-based paints can be maintained even if these attractants are added. In addition, since diatomaceous earth has a sustained release effect as a carrier, the release of soluble salts is relatively slow, and the release rate is kept at a very low level, especially after immersion in seawater for a certain period of time or more. Therefore, similarly, this part of knowledge relates to the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether one is skilled in the field of concrete engineering or the field of marine biology, due to the conventional background, in the present invention, by mixing trace elements into concrete, modifying the ion content of trace elements on the paint surface, and controlling the permeability of the paint, one cannot obtain technical features closely related to a paint with excellent ability to attract oyster larvae to attach.

[0188] Permeability of concrete

[0189] The strength and permeability of the paint are of utmost importance. When different attractants are mixed into the cement-based paint, it will affect the performance of the paint, so when different substances are mixed to promote the attachment, metamorphosis and later growth of oyster larvae, first, it is necessary to control it as a whole so as not to have a significant effect on the performance of the paint, and secondly, the raw materials are selected according to the suitability of various raw materials, and if the performance of the raw materials cannot meet the actual requirements, the desired function can be achieved by modifying them before adding the raw materials. However, in fact, the above-mentioned related studies consider the effect of calcium content on the attachment of oyster larvae, but do not consider the performance of the paint itself, and do not consider the water-cement ratio, calcium content and curing, etc., and the change in the permeability of the paint will change the permeability of the alkali and ions inside it, and the lower the permeability prevention of the paint, the higher the permeability of the alkali and ions inside it will be, which may increase exponentially. Therefore, these released alkalis and ions have a great impact on the larvae, changing from promoting attachment to inhibiting attachment, and this situation may be more serious, especially when the cement dosage is high. Therefore, it is necessary to ensure that the change in the performance of the paint by mixing the attractant into the paint is within a controllable range, for example, the change does not exceed 10%, so that their attractant effects can be compared, otherwise the influence of mixing the attractant independently or mixing the attractants in combination on the attractant effect on oyster larvae cannot be evaluated.

[0190] It is necessary to grasp the optimal environment required for marine sessile organisms to attach, transform and grow later, and to design the paint starting from the penetration prevention of the paint, and not to ignore the fact that only considering the dosage of various raw materials will bring about changes in the penetration prevention of the paint. Therefore, similarly, this part of the knowledge concerns the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether a person skilled in the field of concrete engineering or a person skilled in the field of marine biology, according to the conventional background, in the present invention, the overall control of the penetration prevention of the paint cannot obtain the technical characteristics that are closely related to the ability of the attractant to effectively attract oysters to attach.

[0191] Therefore, similarly, this part of knowledge is related to the interdisciplinary fusion of marine sessile organisms, marine plants, and marine concrete engineering, and whether one is skilled in the field of concrete engineering or marine biology, according to References 2-3, the color change by mixing dark color pigments into the paint, the modification of cow bone powder, the grinding technology, and the control of the paint's permeability cannot obtain technical features closely related to the paint having the ability to effectively attract oysters to attach and high durability. Also, according to Reference 4, the reduction in the alkalinity of the paint and the balance of the calcium ion concentration cannot obtain technical features closely related to the attachment of marine sessile organisms.

[0192] Although embodiments of the present invention will be shown and described, it will be understood that those skilled in the art can make various changes, modifications, substitutions and variations to these embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is limited by the claims and their equivalents.

Claims

1. A method for constructing an ecological riprap breakwater, comprising the steps of: (1) A step of investigating the marine area where the ecological project is to be constructed, which includes investigating the dominant species of oysters in the marine area and the presence or absence of oysters attached thereto, and also investigating the air temperature, seawater temperature, dissolved oxygen, planktonic organisms, total dissolved inorganic nitrogen, active phosphate, active silicate, Ca, etc. in different seasons in the marine area; 2+ , Zn 2+ , and K + and further investigating the number of typhoons that have occurred in the past and their intensity. (2) A step of producing a concrete adhesion base, the shape of which is one of a plate-shaped adhesion base, a corrugated adhesion base, and a cylindrical adhesion base, and a step of producing a lightweight concrete scratch adhesion base having a rough surface; (3) A step of quantitatively harvesting and cultivating oyster larvae, in which an attachment base is placed in a nearby sea area during the period when the oyster floating larvae in the local sea area are concentrated and attached and metamorphosed, and the attachment amount of oyster larvae is 15 to 25 pieces / 100 cm 2 The step of stopping seedling collection for the attachment base of oysters, and then transferring the attachment base with an attachment amount of 15 to 25 oyster larvae per 100 cm 2 to a sea area rich in food for floating culture; (4) preparing the rock surface by washing the rock surface and, when the saturated surface has dried, spraying or applying a cement-based paint to the marine project surface to attract sessile organisms; (5) placing rock blocks, in the second year, during the period when the floating oyster larvae are concentrated in the local sea area to attach and metamorphose, and placing rock blocks with a volume of more than 1 cubic meter individually, covering each rock block with a rope cage, and the rope cage covers a plurality of rock blocks with a volume of less than 1 cubic meter to form a rock pile with a volume of 1 to 5 cubic meters, the internal porosity of which is 40% to 60%, and connecting the rocks or rock piles with rope; (6) A step of placing an oyster attachment base on site, comprising transporting the base on which the oysters in the mature stage of gonad development in (5) are attached to the breakwater construction area, placing a rough-surfaced lightweight concrete oyster attachment base for each stone block or stone pile, and fixing the stone block or stone pile with a rope; (7) A step of monitoring and managing the attachment of oyster larvae, in which the attachment status of oyster larvae on the concrete surface is monitored, and the attachment amount of oysters is 30 to 40 pieces / 100 cm 2 and a step of long-term monitoring of the ecological condition of the breakwater.

2. The oyster adhesion base is composed of cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water, dark pigment, biocalcium powder, calcium carbonate powder, trace elements, short fibers and superplasticizer, and the weight percentages of the cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water, dark pigment, biocalcium powder, calcium carbonate powder, trace elements, short fibers and superplasticizer are 21.8% to 34.5%, 24.6% to 37.5%, 15.8% to 29.6%, 8.4% to 16.4%, 0.6% to 3.0%, 0.4% to 2.0%, 0.4% to 2.0%, 0.2% to 1.8%, 0.15% to 1.5% and 0.03% to 0.18%, The bio-calcium powder is a combination of one or more of cow bone powder, oyster shell powder, fish bone powder, eggshell powder, and coral powder; 2. The method for constructing an ecological riprap breakwater according to claim 1, characterized in that the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers and ultrafine precipitated calcium carbonate.

3. the deep color pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red; the deep color pigment is modified, and one of transparent resin, organosilicon, dimethylsiloxane, and superhydrophobic material is used for the modification treatment; The trace elements are zinc, iron, potassium and phosphorus, which can be modified by selecting natural minerals, industrial products or chemical reagents containing one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to achieve sustained release of corresponding ions and reduce or eliminate the adverse effects on concrete performance; but in the case of eutrophication areas, do not select materials containing nitrogen or phosphorus elements; The cementitious material is one of a Portland cement mixed with a mineral admixture, a sulfoaluminate cement, and an alkali-activated cementitious material, where the Portland cement mixed with a mineral admixture includes a combination of one or more of silica fume, slag powder, and fly ash; The lightweight coarse aggregate is one or two of crushed lightweight porous basalt having a maximum particle size of less than 20 mm and lightweight ceramsite; The lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, and has a particle size of 0.2 mm to 5 mm; The method for constructing an ecological riprap breakwater according to claim 2, characterized in that the short fibers are one or more of inorganic fibers including basalt fibers, alkali-resistant glass fibers, and carbon fibers.

4. The method for constructing an ecological rubble breakwater according to claim 1, characterized in that the cement-based paint is composed of cementitious material, sand, water, dark pigment, bio-calcium powder, calcium carbonate powder, trace elements, wood fiber, dispersible rubber powder and superplasticizer, and the weight ratio of the cementitious material, sand, water, dark pigment, bio-calcium powder, calcium carbonate powder, trace elements, wood fiber, dispersible rubber powder and superplasticizer is 1:(0.35-0.7):(0.20-0.60):(0.02-0.10):(0.02-0.10):(0.02-0.10):(0.01-0.08):(0.04-0.12):(0.05-0.15):(0.001-0.010) in that order.

5. The dark pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red. In addition, these pigments are modified according to the degree of influence on the concrete performance, and one of transparent resin, organic silicon, dimethylsiloxane, and superhydrophobic material is used for the modification treatment. The bio-calcium powder includes one or more combinations of cow bone powder, oyster shell powder, fish bone powder, egg shell powder, and coral powder, and has a fineness of 100 mesh to 1000 mesh; The method for modifying the bio-calcium powder is to treat eggshell powder, coral powder, oyster shell powder and fish bone powder of 100 mesh to 500 mesh with one or two of ethanoic acid, acetic acid, silicic acid and sulfurous acid, and to treat cow bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid; The calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultrafine precipitated calcium carbonate, and has a fineness of more than 200 mesh; The trace elements are zinc, iron, potassium and phosphorus, which can be modified by selecting natural minerals, industrial products or chemical reagents containing one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate to achieve sustained release of corresponding ions and reduce or eliminate the adverse effects on concrete performance; but in the case of eutrophication areas, do not select materials containing nitrogen or phosphorus elements; The sand is one or more of river sand, machine-made sand, and desalinated sea sand. The superplasticizer is one of carboxylic acid and naphthalene-based, The manufacturing method of cement-based paint is as follows: Step S1 of measuring cementitious material, sand, water, dark pigment, biocalcium powder, calcium carbonate powder, trace elements, wood fiber, dispersible rubber powder and superplasticizer; Step S2: putting the cementitious material, the dark color pigment, the bio-calcium powder, the calcium carbonate powder, and the trace elements into a material mixer and uniformly mixing them for 2 to 5 minutes at a rotation speed of 1000 to 1500 revolutions per minute; Next, in step S3, the sand, wood fiber, and dispersible rubber powder are put into a mixer and mixed for 5 to 10 minutes at a rotation speed of 500 to 1000 revolutions per minute; Step S4 of thoroughly dissolving the powdered superplasticizer in water, then putting it together with the mixed material in a high-speed mixer and mixing it at a rotation speed of 1000 to 1500 revolutions per minute for 5 to 10 minutes; The construction method of the ecological rubble breakwater according to claim 4, characterized in that it is possible to produce a cement paint having excellent attracting effect for attracting sessile organisms to the surface of the marine project.

6. The construction method of an ecological rubble breakwater according to claim 1, characterized in that the period during which the oyster larvae are concentrated, attached and metamorphosed is from May to August or from April to October.

7. The method for constructing an ecological rubble breakwater according to claim 1, characterized in that, in the oyster attachment base, a round hole having a diameter of 3 to 5 mm is created during molding.

8. 2. The method for constructing an ecological rock riprap breakwater according to claim 1, wherein the rope is one of palm rope, glass fiber rope, and basalt fiber rope.

9. The method for constructing an ecological rubble breakwater according to claim 1, characterized in that the oyster adhesion base comprises dark pigment, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, wherein the weight percentages of the dark pigment, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.6-3.0%, 21.8-34.5%, 24.6-37.5%, 15.8-29.6%, 8.4-16.4% and 0.03-0.18%, respectively.

10. The method for constructing an ecological rubble breakwater according to claim 1, wherein the oyster adhesion base comprises calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, and the weight percentages of the calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.4-2.35%, 21.8-34.5%, 24.6-37.5%, 15.8-29.6%, 8.4-16.4% and 0.03-0.18%, respectively.

11. The method for constructing an ecological rubble breakwater according to claim 1, wherein the oyster attachment base comprises cow bone powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, and the weight percentages of the cow bone powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.4-2.35%, 21.8-34.5%, 24.6-37.5%, 15.8-29.6%, 8.4-16.4% and 0.03-0.18%, respectively.

12. The method for constructing an ecological rubble breakwater according to claim 3, wherein the oyster adhesion base comprises modified dark pigment, calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, wherein the weight percentages of the modified dark pigment, calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.6-3.0%, 0.4-2.35%, 21.8-34.5%, 24.6-37.5%, 15.8-29.6%, 8.4-16.4% and 0.03-0.18%, respectively.

Citation Information

Patent Citations

  • Novel concrete artificial fish reef and preparation method thereof

    CN104529286A

  • Bionic concrete artificial fish reef and preparation method thereof

    CN104938384A

  • Seed adhering method for oysters

    CN107372242A

  • Coral-imitating porous structural material for modification of marine environment and preparation method of coral-imitating porous structural material

    CN107805037A

  • Marine environment concrete crack repair material and preparation method thereof

    CN109467354A