Water-in-oil emulsion ink
The water-in-oil emulsion ink with separate aqueous phases and specific components addresses pigment aggregation and adhesion issues, providing stable and high-quality prints on absorbent media.
Patent Information
- Application Number
- JP2020217986
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-25
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2040-12-25
AI Technical Summary
Water-in-oil emulsion inks face issues with pigment aggregation in the aqueous phase, leading to poor storage stability and inadequate adhesion to highly absorbent print media, which are critical for high-speed printing in commercial and industrial applications.
A water-in-oil emulsion ink formulation with a first aqueous phase containing a pigment and polymer dispersant, and a second aqueous phase with pigment-free polymer particles, along with a water-insoluble organic solvent and emulsifier, is developed to enhance storage stability and fixing properties.
The formulation achieves excellent storage stability and improved adhesion to highly absorbent printing media, ensuring high-quality printed matter with enhanced fixing properties.
Smart Images

Figure 0007575942000001 
Figure 0007575942000002 
Figure 0007575942000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a water-in-oil emulsion ink and a method for producing the water-in-oil emulsion ink. [Background technology]
[0002] Inkjet recording is a method of directly ejecting ink droplets from minute nozzles and depositing them on a printing medium to obtain a printed matter on which characters and images are recorded. This method has the advantages of being easy to produce full color, being inexpensive, and not contacting the printed matter, so it is no longer limited to consumer printing, and in recent years it has begun to be applied to commercial and industrial printing fields. Conventionally, water-based inks using pigments or dyes as colorants have been used as inks for inkjet recording. However, when printing on plain paper using water-based inks, although the print density is high due to the high water absorption of plain paper, there is a problem that the water contained in the water-based ink causes the plain paper fibers to expand, resulting in curling and deformation of the printed matter. In addition, in the fields of commercial and industrial printing, high-speed printing is required, and in order to meet this demand, printers that employ a line-head type inkjet recording method have been developed and oil-based pigment inks are used. When printing on plain paper using oil-based pigment inks, deformation of the printed matter can be reduced, but there is a problem that the ink penetrates into the interior of the printed matter, resulting in a low print density. Therefore, the use of water-in-oil (W / O) emulsion inks has been investigated. For example, Patent Document 1 discloses an inkjet emulsion ink that is a water-in-oil type emulsion ink consisting of an oil phase and an aqueous phase, with the aim of providing an inkjet emulsion ink that is excellent in properties such as high-speed fixing ability and abrasion resistance, and the aqueous phase contains water and a colorant, and the colorant is a modified pigment containing a polymer. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-189859 A Summary of the Invention [Problem to be solved by the invention]
[0004] Water-in-oil emulsion inks are composed of an oil phase as a continuous phase and an aqueous phase emulsified in the oil phase. When a pigment is contained as a colorant in the aqueous phase, the aqueous phase tends to aggregate, and therefore, improvement in storage stability is required. In addition, it was found that when water-in-oil emulsion ink is used to print on a highly water-absorbent print medium such as plain paper, the pigment remains on the surface of the print medium, and sufficient adhesion to the highly water-absorbent print medium cannot be obtained. An object of the present invention is to provide a water-in-oil emulsion ink which has excellent storage stability and is capable of producing printed matter with excellent fixation even when printed on a highly water-absorbent printing medium, and a method for producing the water-in-oil emulsion ink. [Means for solving the problem]
[0005] The present inventors have found that the above-mentioned problems can be solved by providing a water-in-oil emulsion ink containing a first aqueous phase and a second aqueous phase in an oil phase, in which the first aqueous phase contains a pigment and a polymer dispersant and the second aqueous phase contains polymer particles that do not contain a pigment, thereby improving fixability while maintaining excellent storage stability. That is, the present invention provides the following [1] and [2]. [1] A water-in-oil emulsion ink containing a first aqueous phase and a second aqueous phase in an oil phase, a first aqueous phase containing a pigment and a polymeric dispersant A; a second aqueous phase containing non-pigmented polymer particles B; A water-in-oil emulsion ink in which the oil phase contains a non-water-soluble organic solvent and an emulsifier. [2] A method for producing the water-in-oil emulsion ink according to item [1] above, comprising the following steps I and II: Step I: A step of mixing and emulsifying a first aqueous phase component containing an aqueous pigment dispersion in which a pigment is dispersed in an aqueous medium with a polymer dispersant A with an oil phase component containing a water-insoluble organic solvent and an emulsifier to obtain a preparation. Step II: A step of adding a second aqueous phase component containing an aqueous dispersion of polymer particles B that does not contain a pigment to the preparation obtained in step I, mixing and emulsifying the mixture to obtain a water-in-oil emulsion ink. Effect of the Invention
[0006] The present invention can provide a water-in-oil emulsion ink which has excellent storage stability and is capable of producing printed matter with excellent fixation even when printed on a highly water-absorbent printing medium, and a method for producing the water-in-oil emulsion ink. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] [Water-in-oil emulsion ink] The water-in-oil emulsion ink of the present invention (hereinafter also referred to as "emulsion ink") is a water-in-oil emulsion ink containing a first aqueous phase and a second aqueous phase in an oil phase, wherein the first aqueous phase contains a pigment and a polymer dispersant A, the second aqueous phase contains polymer particles B that do not contain a pigment, and the oil phase contains a water-insoluble organic solvent and an emulsifier. In the present invention, of the aqueous phases dispersed in the oil phase, the aqueous phase containing the pigment and polymer dispersant A is referred to as the "first aqueous phase", and the aqueous phase containing polymer particles B that do not contain a pigment is referred to as the "second aqueous phase". In the present invention, the first aqueous phase and the second aqueous phase exist separately in the oil phase, and the existence forms of the first aqueous phase and the second aqueous phase can be confirmed, for example, by observation with an optical microscope.
[0008] The water-in-oil emulsion ink of the present invention has the special effect of exhibiting excellent storage stability and excellent fixability even when printed on a highly water-absorbent printing medium. The reason for this is not clear, but is thought to be as follows. In the present invention, the pigment is dispersed in the first aqueous phase by the polymer dispersant, and furthermore, the second aqueous phase contains polymer particles that do not contain a pigment, which improves the dispersion stability of the aqueous phase, which is the dispersed phase, and is believed to be able to stabilize the entire emulsion ink system, possibly because coalescence of the aqueous phase is suppressed. As a result, it is believed that the function of the polymer particles that do not contain a pigment contained in the second aqueous phase as a fixing aid can be exerted, improving the fixing property, while maintaining excellent storage stability when the emulsion ink is stored for a long period of time at high temperatures.
[0009] <First aqueous phase> The first aqueous phase contains a pigment and a polymer dispersant A from the viewpoint of improving storage stability and fixing property.
[0010] (Pigments) The pigment according to the present invention may be either an inorganic pigment or an organic pigment, and may be a lake pigment or a fluorescent pigment. If necessary, these pigments may be used in combination with an extender pigment. Specific examples of inorganic pigments include carbon black, metal oxides such as titanium oxide, iron oxide, red iron oxide, and chromium oxide, pearlescent pigments, etc. In particular, carbon black is preferred for black ink. The type of carbon black is not particularly limited, and examples thereof include furnace black, lamp black, acetylene black, and channel black. The DBP oil absorption of the carbon black is preferably 20 mL / 100 g or more and 200 mL / 100 g or less, from the viewpoints of improving the dispersion stability of the pigment in the aqueous phase and improving the storage stability. The DBP oil absorption refers to the oil absorption measured by the DBP method, specifically, a value based on ASTM D2414-65T.
[0011] Specific examples of organic pigments include azo pigments such as azo lake pigments, insoluble monoazo pigments, insoluble disazo pigments, and chelate azo pigments; and polycyclic pigments such as phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, thioindigo pigments, isoindolinone pigments, quinophthalone pigments, diketopyrrolopyrrole pigments, benzimidazolone pigments, and threne pigments. The hue is not particularly limited, and any chromatic pigment such as yellow, magenta, cyan, blue, red, orange, green, etc. can be used. Specific examples of preferred organic pigments include one or more product numbers selected from CI Pigment Yellow, CI Pigment Red, CI Pigment Orange, CI Pigment Violet, CI Pigment Blue, and CI Pigment Green. Examples of the extender pigment include silica, calcium carbonate, and talc. The pigments can be used alone or in combination of two or more kinds.
[0012] (Polymer Dispersant A) The pigment in the emulsion ink of the present invention is dispersed in the first aqueous phase using polymer dispersant A from the viewpoints of improving the dispersion stability of the pigment in the aqueous phase, thereby improving storage stability, and improving fixability.
[0013] The polymer dispersant A according to the present invention is not particularly limited as long as it has at least pigment dispersibility. From the viewpoint of improving the dispersion stability of the pigment in the aqueous phase, improving storage stability, and improving fixability, it preferably contains an acid group. The acid group of the polymer dispersant A is a group that exhibits acidity by dissociating and releasing a hydrogen ion, such as a carboxyl group (-COOM), a sulfonic acid group (-SO3M), or a phosphoric acid group (-OPO3M2), or a group in the dissociated ionic form (-COO - , -SO3 - , -OPO3 2- , -OPO3 -In the above chemical formula, M represents a hydrogen atom, an alkali metal, ammonium or an organic ammonium. Among these, a carboxy group (-COOM) is preferred from the same viewpoint as above.
[0014] At least a portion of the acid groups of the polymer dispersant A is preferably neutralized from the viewpoints of improving the dispersion stability of the pigment in the aqueous phase, improving the storage stability, and improving the fixability. Examples of the neutralizing agent used for neutralizing the polymer dispersant A include alkali metal hydroxides, ammonia, etc. Among them, from the viewpoints of improving the dispersion stability of the pigment in the aqueous phase, improving the storage stability, and improving the fixing property, preferred are alkali metal hydroxides, and more preferred are one or more selected from sodium hydroxide and potassium hydroxide. From the same viewpoint as above, the degree of neutralization is preferably 20 mol% or more, more preferably 30 mol% or more, even more preferably 40 mol% or more, still more preferably 45 mol% or more, and is preferably 80 mol% or less, more preferably 70 mol% or less, and even more preferably 60 mol% or less. Specifically, the degree of neutralization (mol %) can be determined by the following formula. Degree of neutralization (mol%) = [{weight of neutralizing agent added (g) / equivalent weight of neutralizing agent} / [{acid value of polymer dispersant A (mg KOH / g) × weight of polymer dispersant A (g)} / (56.1 × 1,000)]] × 100
[0015] [Polymer (a)] The polymer dispersant A according to the present invention may be a non-crosslinked polymer (hereinafter also referred to as "non-crosslinked polymer (a)" or "polymer (a)") from the viewpoint of improving the dispersion stability of the pigment in the aqueous phase, improving storage stability, and improving fixability. From the same viewpoint as above, the polymer (a) preferably contains an acid group.
[0016] From the viewpoint of improving the dispersion stability of the pigment in the aqueous phase and improving the storage stability, the acid value of the polymer (a) is preferably 70 mgKOH / g or more, more preferably 100 mgKOH / g or more, even more preferably 150 mgKOH / g or more, even more preferably 200 mgKOH / g or more, even more preferably 220 mgKOH / g or more, and preferably 320 mgKOH / g or less, more preferably 300 mgKOH / g or less, even more preferably 280 mgKOH / g or less, even more preferably 260 mgKOH / g or less. If the acid value is in the above range, the amount of acid groups can be sufficient to ensure the dispersion stability of the pigment. It is also preferable from the viewpoint of the balance between the affinity of the polymer (a) with water and the interaction between the polymer (a) with the pigment. The acid value of the polymer (a) can be measured by the method described in the Examples. The acid value of the polymer (a) can be calculated from the mass ratio of the constituent monomers.
[0017] Examples of the polymer (a) include polyester resins, polyurethane resins, vinyl resins, etc. Among them, vinyl resins are preferred, and vinyl resins containing a carboxyl group-containing monomer-derived structural unit and a hydrophobic monomer-derived structural unit are more preferred. The vinyl resin may further contain a nonionic monomer-derived structural unit.
[0018] [Carboxy Group-Containing Monomer] The carboxyl group-containing monomer is preferably used as a monomer component of the vinyl resin from the viewpoints of improving the dispersion stability of the pigment in the aqueous phase, improving the storage stability, and improving the fixability. Examples of the carboxy group-containing monomer include (meth)acrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid, citraconic acid, and 2-methacryloyloxymethylsuccinic acid, with (meth)acrylic acid being preferred, and acrylic acid being more preferred. In this specification, "(meth)acrylic acid" means at least one selected from acrylic acid and methacrylic acid. The carboxyl group-containing monomers can be used alone or in combination of two or more kinds.
[0019] [Hydrophobic Monomer] The hydrophobic monomer is preferably used as a monomer component of the vinyl resin from the viewpoints of improving the adsorption of the polymer to the pigment, improving the dispersion stability of the pigment in the aqueous phase, improving the storage stability, and improving the fixability. In this specification, "hydrophobic" means that when a monomer is dissolved to saturation in 100 g of ion-exchanged water at 25° C., the amount of the dissolved hydrophobic monomer is preferably 5 g or less, more preferably 1 g or less, from the viewpoint of the adsorption of the polymer to the pigment. Examples of the hydrophobic monomer include aromatic group-containing monomers and (meth)acrylates having a hydrocarbon group derived from an aliphatic alcohol. In this specification, the term "(meth)acrylate" refers to at least one selected from acrylate and methacrylate. The hydrophobic monomers can be used alone or in combination of two or more.
[0020] The aromatic group-containing monomer is preferably a vinyl monomer having an aromatic group with 6 to 22 carbon atoms, which may have a substituent containing a hetero atom, and more preferably at least one selected from a styrene-based monomer and an aromatic group-containing (meth)acrylate. The molecular weight of the aromatic group-containing monomer is preferably less than 500. The styrene-based monomer is preferably at least one selected from styrene, α-methylstyrene, 2-methylstyrene, vinyltoluene, and divinylbenzene, and more preferably at least one selected from styrene and α-methylstyrene. The aromatic group-containing (meth)acrylate is preferably at least one selected from phenyl (meth)acrylate, benzyl (meth)acrylate, and phenoxyethyl (meth)acrylate, and more preferably benzyl (meth)acrylate.
[0021] The (meth)acrylate having a hydrocarbon group derived from an aliphatic alcohol preferably has a hydrocarbon group derived from an aliphatic alcohol having 1 to 22 carbon atoms. Examples of such acrylates include (meth)acrylates having a straight chain alkyl group such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, and stearyl (meth)acrylate; (meth)acrylates having a branched chain alkyl group such as isopropyl (meth)acrylate, isobutyl (meth)acrylate, tertiary butyl (meth)acrylate, isopentyl (meth)acrylate, isooctyl (meth)acrylate, isodecyl (meth)acrylate, isododecyl (meth)acrylate, isostearyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; and (meth)acrylates having an alicyclic alkyl group such as cyclohexyl (meth)acrylate.
[0022] In the present invention, a hydrophobic macromonomer may be used as the hydrophobic monomer constituting the vinyl resin. The macromonomer is a compound having a number average molecular weight of 500 to 100,000 and having a polymerizable functional group at one end, and can be used as a monomer component of a vinyl resin from the viewpoint of improving the dispersion stability of a pigment in an aqueous phase. The polymerizable functional group present at one end is preferably an acryloyloxy group or a methacryloyloxy group, and more preferably a methacryloyloxy group. The number average molecular weight of the macromonomer is preferably from 1,000 to 10,000. The number average molecular weight is measured by gel permeation chromatography using chloroform containing 1 mmol / L dodecyldimethylamine as a solvent and polystyrene as a standard substance. As the macromonomer, from the viewpoint of dispersion stability of the pigment in the aqueous phase, aromatic group-containing monomer-based macromonomers and silicone-based macromonomers are preferred, and aromatic group-containing monomer-based macromonomers are more preferred. Examples of the aromatic group-containing monomer constituting the aromatic group-containing monomer-based macromonomer include the aromatic group-containing monomers described above in relation to the hydrophobic monomer, and styrene and benzyl (meth)acrylate are preferred, with styrene being more preferred. The macromonomers can be used alone or in combination of two or more kinds. Specific examples of commercially available styrene-based macromonomers include AS-6(S), AN-6(S), and HS-6(S) (product names of Toagosei Co., Ltd.). The silicone macromonomer may be, for example, an organopolysiloxane having a polymerizable functional group at one end.
[0023] From the viewpoints of improving the adsorption of the polymer to the pigment, improving the dispersion stability of the pigment in the aqueous phase, improving storage stability, and improving fixability, the hydrophobic monomer is preferably one or more types selected from aromatic group-containing monomers, (meth)acrylates having a hydrocarbon group derived from an aliphatic alcohol, and aromatic group-containing monomer-based macromonomers, more preferably one or more types selected from aromatic group-containing monomers and (meth)acrylates having a hydrocarbon group derived from an aliphatic alcohol, even more preferably an aromatic group-containing monomer, and still more preferably one or more types selected from styrene-based monomers and aromatic group-containing (meth)acrylates.
[0024] [Nonionic Monomer] From the viewpoint of dispersion stability of the pigment in the aqueous phase, a nonionic monomer can be used as a monomer component of the vinyl resin. Examples of nonionic monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 3-hydroxypropyl (meth)acrylate; polyalkylene glycol (meth)acrylates such as polypropylene glycol (n=2-30, n indicates the average number of moles of oxypropylene groups added. The following n indicates the average number of moles of oxyalkylene groups added.) (meth)acrylate and polyethylene glycol (n=2-30) (meth)acrylate; alkoxypolyalkylene glycol (meth)acrylates such as methoxypolyethylene glycol (n=1-30) (meth)acrylate; and phenoxy (ethylene glycol-propylene glycol copolymer) (n=1-30, ethylene glycol: n=1-29) (meth)acrylate. Among them, polypropylene glycol (n=2-30) (meth)acrylate, alkoxypolyalkylene glycol (meth)acrylate, and phenoxy (ethylene glycol / propylene glycol copolymer) (meth)acrylate are preferred. The nonionic monomers can be used alone or in combination of two or more kinds. Specific examples of commercially available nonionic monomers include NK Ester M-20G, 40G, 90G, 230G, and the like manufactured by Shin-Nakamura Chemical Co., Ltd.; Blenmer PE-90, 200, 350, and the like, Blenmer PME-100, 200, 400, and the like, Blenmer PP-500, 800, 1000, and the like, Blenmer AP-150, 400, 550, and the like, Blenmer 50PEP-300, 50POEP-800B, 43PAPE-600B, and the like manufactured by NOF Corporation.
[0025] As described above, the polymer (a) according to the present invention is preferably a vinyl resin containing one or more structural units derived from a carboxyl group-containing monomer selected from acrylic acid and methacrylic acid, and one or more structural units derived from a hydrophobic monomer selected from an aromatic group-containing monomer, a (meth)acrylate having a hydrocarbon group derived from an aliphatic alcohol, and an aromatic group-containing monomer-based macromonomer, and may further be a vinyl resin containing a structural unit derived from a nonionic monomer. However, from the viewpoint of improving the dispersion stability of the pigment in the aqueous phase, improving the storage stability, and improving the fixability, it is more preferably a vinyl resin containing one or more structural units derived from a carboxyl group-containing monomer selected from acrylic acid and methacrylic acid, and one or more structural units derived from a hydrophobic monomer selected from an aromatic group-containing monomer and a (meth)acrylate having a hydrocarbon group derived from an aliphatic alcohol, and even more preferably a vinyl resin containing one or more structural units derived from a carboxyl group-containing monomer selected from acrylic acid and methacrylic acid, and one or more structural units derived from a hydrophobic monomer selected from a styrene-based monomer and an aromatic group-containing (meth)acrylate.
[0026] (Content of structural units derived from each monomer in vinyl resin) The content of the constituent units derived from each monomer in the vinyl resin is as follows, from the viewpoints of improving the dispersion stability of the pigment in the aqueous phase, improving the storage stability, and improving the fixability. The content of structural units derived from carboxy group-containing monomers in the vinyl resin is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, still more preferably 20% by mass or more, and is preferably 70% by mass or less, more preferably 60% by mass or less, even more preferably 50% by mass or less, and still more preferably 40% by mass or less. The content of structural units derived from hydrophobic monomers in the vinyl resin is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, still more preferably 60% by mass or more, and is preferably 95% by mass or less, more preferably 90% by mass or less, even more preferably 85% by mass or less. When the vinyl resin contains a structural unit derived from a macromonomer, the content of the structural unit derived from the macromonomer in the vinyl resin is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and preferably 35% by mass or less, more preferably 30% by mass or less, even more preferably 25% by mass or less. When the vinyl resin contains a structural unit derived from a nonionic monomer, the content of the structural unit derived from the nonionic monomer in the vinyl resin is preferably 3 mass% or more, more preferably 5 mass% or more, even more preferably 7 mass% or more, and preferably 30 mass% or less, more preferably 20 mass% or less, even more preferably 15 mass% or less. The content of the constituent units derived from each monomer in the vinyl resin can be measured by analysis such as NMR. The preferred range of the content of each monomer in the raw material monomers during the production of the vinyl resin (content as unneutralized amount) can be considered to be the same as the preferred range of the content of the constituent units derived from each monomer in the vinyl resin.
[0027] The total content of the constituent units derived from the carboxy group-containing monomer and the constituent units derived from the hydrophobic monomer in the vinyl resin is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, still more preferably 90% by mass or more, and is preferably 100% by mass or less, still more preferably substantially 100% by mass, and still more preferably 100% by mass. The mass ratio of the content of constituent units derived from carboxyl group-containing monomers to the content of constituent units derived from hydrophobic monomers in the vinyl resin [content of constituent units derived from carboxyl group-containing monomers / content of constituent units derived from hydrophobic monomers] is preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.3 or more, still more preferably 0.4 or more, and is preferably 2 or less, more preferably 1.5 or less, even more preferably 1.0 or less, still more preferably 0.9 or less, still more preferably 0.8 or less, still more preferably 0.7 or less, and still more preferably 0.5 or less.
[0028] Vinyl resins are produced by copolymerizing raw material monomers by known polymerization methods such as bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization. Among these polymerization methods, solution polymerization is preferred. There is no limitation on the chain form of the polymerized monomers, and any of the polymerization forms such as random, block, and graft may be used.
[0029] The weight average molecular weight of the vinyl resin is preferably 2,000 or more, more preferably 5,000 or more, and even more preferably 7,000 or more, and is preferably 100,000 or less, more preferably 50,000 or less, even more preferably 30,000 or less, and even more preferably 20,000 or less. If the weight average molecular weight of the vinyl resin is within the above range, the adhesive power to the pigment is sufficient and dispersion stability can be exhibited. The weight average molecular weight of the vinyl resin is measured by the method described in the Examples.
[0030] [Crosslinked polymer (a')] In the present invention, from the viewpoint of improving the dispersion stability of the pigment in the aqueous phase, thereby improving storage stability, and from the viewpoint of improving fixability, it is preferable that the pigment is dispersed using a polymer dispersant A, and that the polymer dispersant A contains a crosslinked structure. From the viewpoint of improving the dispersion stability of the pigment in the aqueous phase, improving storage stability, and improving fixability, the polymer dispersant A is preferably a polymer containing a crosslinked structure crosslinked with a crosslinking agent or a polymer having a self-crosslinked structure into which a crosslinkable group has been introduced, more preferably a polymer containing a crosslinked structure crosslinked with a crosslinking agent, and even more preferably a crosslinked polymer (a') obtained by crosslinking the aforementioned non-crosslinked polymer (a) with a crosslinking agent. That is, the crosslinked polymer (a') has a structure derived from the crosslinking agent in addition to the constituent units derived from the monomers constituting the polymer (a). In the present invention, the crosslinked polymer (a') used as the polymer dispersant A is firmly adsorbed or fixed onto the pigment surface, suppressing pigment aggregation, particularly depletion aggregation, in the aqueous phase, improving the dispersion stability of the pigment in the aqueous phase, and further suppressing swelling of the polymer, thereby stabilizing the entire emulsion ink system. Therefore, it is believed that storage stability can be improved even in the case of a second aqueous phase.
[0031] [Crosslinking Agent] From the viewpoint of reactivity with the polymer (a), the water solubility (mass ratio) of the crosslinking agent is preferably 50% or less, more preferably 40% or less, and even more preferably 35% or less. The water solubility (mass ratio) refers to the solubility (%) when 10 parts by mass of the crosslinking agent is dissolved in 90 parts by mass of water at room temperature (25° C.).
[0032] The crosslinking agent is preferably a polyfunctional compound, and when the polymer (a) contains an acid group, the crosslinkable functional group of the polyfunctional compound is preferably capable of reacting with the acid group of the polymer (a) to form a covalent bond. The covalent bond is preferably one or more selected from ester bond, thioester bond, amide bond, amino bond, ether bond, thioether bond, carbonyl bond, thiocarbonyl bond and sulfonyl bond, more preferably one or more selected from ester bond, thioester bond and amide bond. The crosslinkable functional group of the polyfunctional compound is not particularly limited as long as it can form the above-mentioned covalent bond. The molecular weight of the crosslinking agent is preferably 120 or more, more preferably 150 or more, and even more preferably 200 or more, from the viewpoints of ease of reaction, improving the dispersion stability of the pigment in the aqueous phase, improving storage stability, and improving fixability, and is preferably 2,000 or less, more preferably 1,500 or less, and even more preferably 1,000 or less.
[0033] The crosslinkable functional group is preferably one or more selected from epoxy group, isocyanate group, aziridino group, amino group and oxazoline group, more preferably epoxy group. The concept of epoxy group includes glycidyl group. That is, the crosslinking agent is preferably a multifunctional epoxy compound, and from the viewpoint of crosslinking efficiency, more preferably a compound having two or more epoxy groups in the molecule, even more preferably a compound having two or more glycidyl ether groups, and even more preferably a polyglycidyl ether compound of a polyhydric alcohol having a hydrocarbon group with 3 to 8 carbon atoms. When the crosslinking agent is a polyfunctional epoxy compound, the epoxy equivalent of the crosslinking agent is preferably 90 or more, more preferably 100 or more, even more preferably 110 or more, and preferably 300 or less, more preferably 200 or less, even more preferably 150 or less. When the crosslinking agent is a polyfunctional epoxy compound, the number of epoxy groups in the crosslinking agent is 2 or more per molecule from the viewpoints of efficiently carrying out a crosslinking reaction to improve the dispersion stability of the pigment in the aqueous phase, improving the storage stability, and improving the fixability, and is preferably 6 or less per molecule, and from the viewpoint of market availability, is more preferably 4 or less, and even more preferably 3 or less.
[0034] Specific examples of the crosslinking agent include polyglycidyl ethers such as polypropylene glycol diglycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, sorbitol polyglycidyl ether, pentaerythritol polyglycidyl ether, resorcinol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether, cyclohexanedimethanol diglycidyl ether, diethylene glycol diglycidyl ether, and hydrogenated bisphenol A diglycidyl ether. Among these, preferred is one or more selected from trimethylolpropane polyglycidyl ether, pentaerythritol polyglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,4-butanediol diglycidyl ether, cyclohexanedimethanol diglycidyl ether, and diethylene glycol diglycidyl ether, and more preferred is trimethylolpropane polyglycidyl ether.
[0035] From the viewpoint of improving the dispersion stability of the pigment in the aqueous phase and thereby improving storage stability, and from the viewpoint of improving fixability, the degree of crosslinking of the crosslinked polymer (a') is preferably 20 mol % or more, more preferably 30 mol % or more, even more preferably 40 mol % or more, still more preferably 45 mol % or more, and is preferably 80 mol % or less, more preferably 70 mol % or less, even more preferably 60 mol % or less, and still more preferably 55 mol % or less. As described above, the degree of crosslinking of the crosslinked polymer (a') is obtained by crosslinking the polymer (a) with a crosslinking agent, and when the polymer (a) contains an acid group, the degree of crosslinking is calculated from the equivalent of the acid group of the polymer (a) and the equivalent of the crosslinkable functional group of the crosslinking agent, and is expressed as "the number of molar equivalents of the crosslinkable functional group of the crosslinking agent / the number of molar equivalents of the acid group of the polymer (a)". As described above, when some of the acid groups of the polymer (a) are neutralized, the neutralized acid groups can also become crosslinking points. Therefore, when the sum of the neutralization degree and the crosslinking degree exceeds 100 mol%, the crosslinking degree is expressed as "the molar equivalent number of the crosslinkable functional group of the crosslinking agent / the molar equivalent number of the acid group of the polymer (a)" as described above, and the neutralization degree of the crosslinked polymer (a') is the value obtained by subtracting the crosslinking degree from 100 mol%.
[0036] The acid value of the crosslinked polymer (a') is preferably 40 mgKOH / g or more, more preferably 60 mgKOH / g or more, even more preferably 80 mgKOH / g or more, even more preferably 100 mgKOH / g or more, even more preferably 110 mgKOH / g or more, and is preferably 200 mgKOH / g or less, more preferably 180 mgKOH / g or less, even more preferably 160 mgKOH / g or less, even more preferably 140 mgKOH / g or less, and even more preferably 130 mgKOH / g or less, from the viewpoint of improving the dispersion stability of the pigment in the aqueous phase and improving the storage stability. If the acid value is in the above range, the amount of acid groups can be sufficient to ensure the dispersion stability of the pigment. It is also preferable from the viewpoint of the balance between the affinity of the crosslinked polymer (a') with water and the interaction between the crosslinked polymer (a') and the pigment. The acid value of the crosslinked polymer (a') can be measured by the method described in the Examples. The acid value of the crosslinked polymer (a') can also be calculated by the following formula. Acid value of crosslinked polymer (a') (mg KOH / g) = [Acid value of polymer (a) (mg KOH / g)] × [100 - degree of crosslinking (mol%)] / 100 Here, the acid value of the polymer (a) is as described above. Also, the degree of crosslinking is expressed as "the molar equivalent number of the crosslinkable functional group of the crosslinking agent / the molar equivalent number of the acid group of the polymer (a)" as described above.
[0037] At least a part of the acid groups of the crosslinked polymer (a') is preferably neutralized from the viewpoint of improving the dispersion stability of the pigment in the aqueous phase, thereby improving storage stability, and from the viewpoint of improving fixability. Examples of the neutralizing agent used for neutralizing the crosslinked polymer (a') include the same ones as those exemplified above. The counter ion of the neutralized acid group of the crosslinked polymer (a') is preferably an alkali metal cation, more preferably a sodium ion (Na + ) and potassium ion (K + ) is one or more selected from the following. Regarding the degree of neutralization of the crosslinked polymer (a'), a part of the acid groups of the crosslinked polymer (a') may be neutralized, or all of the acid groups may be neutralized.
[0038] The form of the polymer (a) or crosslinked polymer (a') as the polymer dispersant A in the aqueous phase of the emulsion ink of the present invention may be in a state where it is adsorbed to the pigment, a state where it contains the pigment (including a particle form in which the pigment is encapsulated and a particle form in which the pigment is uniformly dispersed), or a form in which the pigment is not adsorbed. From the viewpoint of improving the dispersion stability of the pigment and improving the storage stability, in the present invention, the form of particles in which the polymer (a) contains the pigment (hereinafter also referred to as "pigment-containing polymer particles") or particles in which the crosslinked polymer (a') contains the pigment (hereinafter also referred to as "pigment-containing crosslinked polymer particles") is preferred, the form of pigment-containing crosslinked polymer particles is more preferred, and the form of particles in which the crosslinked polymer (a') encapsulates the pigment is even more preferred.
[0039] (Surfactant) In the emulsion ink of the present invention, a surfactant may be contained in the first aqueous phase. It is considered that the surfactant can improve the dispersion stability of the pigment in the aqueous phase, reduce the energy of the interface between the aqueous phase and the oil phase, contribute to the formation of a stable dispersed phase, and improve storage stability. From this viewpoint, the surfactant is preferably a nonionic surfactant, more preferably one or more selected from acetylene glycol surfactants, polyoxyalkylene alkyl ether surfactants, polyether-modified silicone surfactants, and fluorine-based surfactants, even more preferably one selected from acetylene glycol surfactants and polyether-modified silicone surfactants, and even more preferably an acetylene glycol surfactant. The HLB (hydrophilic-lipophilic balance) value of the nonionic surfactant is preferably 6 or more, more preferably 8 or more, even more preferably 10 or more, still more preferably 12 or more, and is preferably 20 or less, more preferably 18 or less. The HLB value indicates the affinity of a surfactant to water and oil, and can be calculated by the Griffin method using the following formula: In the following formula, examples of the "hydrophilic group contained in the surfactant" include a hydroxyl group and an ethyleneoxy group. HLB = 20 × [(total formula weight of hydrophilic groups contained in surfactant) / (molecular weight of surfactant)]
[0040] The acetylene glycol surfactant is preferably an ethylene oxide (hereinafter also referred to as "EO") adduct of 2,4,7,9-tetramethyl-5-decyne-4,7-diol, an EO adduct of 3,6-dimethyl-4-octyne-3,6-diol, an EO adduct of 2,5-dimethyl-3-hexyne-2,5-diol, an EO adduct of 2,5,8,11-tetramethyl-6-dodecyne-5,8-diol, and an EO adduct of 3,5-dimethyl-1-hexyne-2,5-diol. The EO adduct of 2,4,7,9-tetramethyl-5-decyne-4,7-diol is more preferably at least one selected from the EO adduct of 3,6-dimethyl-4-octyne-3,6-diol and the EO adduct of 2,5-dimethyl-3-hexyne-2,5-diol, and even more preferably the EO adduct of 2,4,7,9-tetramethyl-5-decyne-4,7-diol. The average EO addition mole number of the above-mentioned EO adduct used as the acetylene glycol surfactant is preferably 5 or more, more preferably 6 or more, even more preferably 7 or more, and still more preferably 8 or more, and is preferably 40 or less, more preferably 36 or less, and even more preferably 32 or less. Commercially available acetylene glycol surfactants include the Surfynol series manufactured by Nissin Chemical Industry Co., Ltd.; the Acetylenol series manufactured by Kawaken Fine Chemical Co., Ltd.; and the like.
[0041] The polyether-modified silicone surfactant is preferably one having a structure in which the side chain and / or terminal hydrocarbon group of silicone oil is replaced with a polyether group.As the polyether group, a polyethyleneoxy group, a polypropyleneoxy group, an ethyleneoxy group (EO) and a propyleneoxy group (trimethyleneoxy group or propane-1,2-diyloxy group; PO) are preferably added in a block or random manner to a polyalkyleneoxy group, and a compound in which a polyether group is grafted to a silicone main chain, a compound in which silicone and a polyether group are bonded in a block form, etc. can be used. Commercially available polyether-modified silicone surfactants include KF-353, KF-355A, KF-642, etc. manufactured by Shin-Etsu Chemical Co., Ltd.; Silface SAG005, etc. manufactured by Nissin Chemical Industry Co., Ltd.; FZ-2191, etc. manufactured by NUC Corporation; and BYK-348, etc. manufactured by BYK-Chemie Japan K.K.
[0042] (Water-soluble organic solvent) In the emulsion ink of the present invention, from the viewpoint of improving the dispersion stability of the pigment in the aqueous phase, thereby improving storage stability, and from the viewpoint of improving fixability, the first aqueous phase may further contain a water-soluble organic solvent. A water-soluble organic solvent is an organic solvent that dissolves in 100 mL of water at 25°C in an amount of 10 mL or more. The water-soluble organic solvent is preferably one that is normally used in the aqueous phase of water-in-oil emulsion inks and is miscible with water in any ratio, and examples of such solvents include alkanols having 1 to 4 carbon atoms, polyhydric alcohols, polyhydric alcohol alkyl ethers, ketones, cyclic ethers, nitrogen-containing heterocyclic compounds, amides, amines, sulfur-containing compounds, etc. Of these, one or more selected from polyhydric alcohols and polyhydric alcohol alkyl ethers are more preferred. The boiling point of the water-soluble organic solvent is preferably 60°C or higher, more preferably 90°C or higher, even more preferably 150°C or higher, and preferably 350°C or lower, more preferably 330°C or lower, even more preferably 310°C or lower. The water-soluble organic solvent may be used alone or in combination of two or more kinds, so long as it is miscible with water in any ratio.
[0043] In the present invention, the first aqueous phase may contain a viscosity modifier, an antifoaming agent, an antiseptic, an antifungal agent, an antirust agent, etc., within the range not impairing the effects of the present invention.
[0044] <Second aqueous phase> (Polymer particles B not containing pigment) The second aqueous phase contains polymer particles B (hereinafter also referred to as "polymer particles B") that do not contain a pigment, from the viewpoint of improving storage stability and fixability. In the present invention, the polymer constituting the polymer particles B may have the same composition as or different from the polymer dispersant A described above. In the present invention, the second aqueous phase preferably does not contain a colorant such as a pigment.
[0045] The polymer constituting the pigment-free polymer particles B preferably contains an acid group from the viewpoint of improving storage stability and fixability. Examples of such acid groups include the same as those exemplified for the polymer dispersant A. Among them, a carboxy group (-COOM) is preferred from the viewpoint of improving storage stability and fixability.
[0046] It is preferable that at least a portion of the acid groups of the pigment-free polymer particles B are neutralized from the viewpoints of improving the dispersion stability of the polymer particles B in the aqueous phase, improving the storage stability, and improving the fixability. Examples of the neutralizing agent used for neutralization include alkali metal hydroxides, ammonia, etc. Among them, from the viewpoints of improving the dispersion stability of the polymer particles B in the aqueous phase, improving the storage stability, and improving the fixing property, preferred are alkali metal hydroxides, and more preferred are one or more selected from sodium hydroxide and potassium hydroxide. From the same viewpoint as above, the degree of neutralization is preferably 20 mol% or more, more preferably 30 mol% or more, even more preferably 40 mol% or more, still more preferably 45 mol% or more, and is preferably 80 mol% or less, more preferably 70 mol% or less, and even more preferably 60 mol% or less. Specifically, the degree of neutralization (mol %) can be determined by the following formula. Degree of neutralization (mol%)=[{weight of neutralizing agent added (g) / equivalent weight of neutralizing agent} / [{acid value of polymer constituting polymer particle B (mg KOH / g) × weight of polymer particle B (g)} / (56.1 × 1,000)]] × 100
[0047] [Polymer (b)] The pigment-free polymer particles B according to the present invention are not particularly limited as long as they have at least a fixing aid function, but may be composed of a non-crosslinked polymer (b) from the viewpoint of improving the dispersion stability of the polymer particles B in the aqueous phase, improving storage stability, and improving fixing property. The polymer (b) preferably contains an acid group from the same viewpoint as above.
[0048] Examples of the polymer (b) include polyester resins, polyurethane resins, vinyl resins, etc. Among them, vinyl resins are preferred, and vinyl resins containing a carboxyl group-containing monomer-derived structural unit and a hydrophobic monomer-derived structural unit are more preferred. The vinyl resin may further contain a nonionic monomer-derived structural unit. Examples of the carboxyl group-containing monomer, hydrophobic monomer, and nonionic monomer include the same as those exemplified for the above-mentioned polymer (a), and the preferred embodiment and the preferred content of each monomer are also the same.
[0049] That is, the polymer (b) according to the present invention is preferably a vinyl resin containing one or more structural units derived from a carboxyl group-containing monomer selected from acrylic acid and methacrylic acid, and one or more structural units derived from a hydrophobic monomer selected from an aromatic group-containing monomer, a (meth)acrylate having a hydrocarbon group derived from an aliphatic alcohol, and an aromatic group-containing monomer-based macromonomer, and may further be a vinyl resin containing a structural unit derived from a nonionic monomer. However, from the viewpoint of improving the dispersion stability of the polymer particles B in the aqueous phase, improving the storage stability, and improving the fixability, it is more preferably a vinyl resin containing one or more structural units derived from a carboxyl group-containing monomer selected from acrylic acid and methacrylic acid, and one or more structural units derived from a hydrophobic monomer selected from an aromatic group-containing monomer and a (meth)acrylate having a hydrocarbon group derived from an aliphatic alcohol, and even more preferably a vinyl resin containing one or more structural units derived from a carboxyl group-containing monomer selected from acrylic acid and methacrylic acid, and one or more structural units derived from a hydrophobic monomer selected from a styrene-based monomer and an aromatic group-containing (meth)acrylate.
[0050] The acid value of the polymer (b) is preferably 60 mgKOH / g or more, more preferably 100 mgKOH / g or more, more preferably 140 mgKOH / g or more, more preferably 180 mgKOH / g or more, more preferably 220 mgKOH / g or more, and is preferably 320 mgKOH / g or less, more preferably 300 mgKOH / g or less, more preferably 280 mgKOH / g or less, and more preferably 260 mgKOH / g or less, from the viewpoint of improving the dispersion stability of the polymer particles B in the aqueous phase, improving the storage stability, and improving the fixability. If the acid value is in the above range, the amount of acid groups can be sufficient to ensure the dispersion stability of the polymer particles (b). The acid value of the pigment-free polymer particles B can be measured by the method described in the Examples, and can also be calculated from the mass ratio of the constituent monomers.
[0051] [Crosslinked polymer (b')] The polymer constituting the pigment-free polymer particles B according to the present invention preferably contains a crosslinked structure. That is, the pigment-free polymer particles B are preferably pigment-free crosslinked polymer particles B composed of a crosslinked polymer. The polymer constituting the pigment-free crosslinked polymer particles B is, from the viewpoint of improving the dispersion stability of the polymer particles B in the aqueous phase and thereby improving storage stability, and from the viewpoint of improving fixability, preferably a polymer containing a crosslinked structure crosslinked with a crosslinking agent or a polymer having a self-crosslinked structure into which a crosslinkable group has been introduced, more preferably a polymer containing a crosslinked structure crosslinked with a crosslinking agent, and even more preferably a polymer (b') obtained by crosslinking the aforementioned non-crosslinked polymer (b) with a crosslinking agent. That is, the crosslinked polymer (b') has a structure derived from a crosslinking agent in addition to the constituent units derived from the monomers constituting the polymer (b). The crosslinked polymer (b') has a crosslinked structure, which suppresses aggregation of the polymer particles B in the aqueous phase, particularly depletion aggregation, improves the dispersion stability of the polymer particles B in the aqueous phase, and further suppresses swelling of the polymer, thereby stabilizing the entire emulsion ink system, and is therefore considered to improve storage stability. Examples of the crosslinking agent include the same ones as those exemplified for the polymer dispersant A described above, and preferred embodiments of the crosslinking agent are also the same.
[0052] The degree of crosslinking of the crosslinked polymer (b') is, from the viewpoint of improving the dispersion stability of the polymer particles B in the aqueous phase, improving storage stability, and improving fixability, preferably 20 mol % or more, more preferably 30 mol % or more, even more preferably 40 mol % or more, still more preferably 45 mol % or more, and is preferably 80 mol % or less, more preferably 70 mol % or less, even more preferably 60 mol % or less, and still more preferably 55 mol % or less. As described above, the degree of crosslinking of the crosslinked polymer (b') is obtained by crosslinking the polymer (b) with a crosslinking agent, and when the polymer (b) contains acid groups, the degree of crosslinking is calculated from the equivalent of the acid groups of the polymer (b) and the equivalent of the crosslinkable functional groups of the crosslinking agent, and is expressed as "the number of molar equivalents of the crosslinkable functional groups of the crosslinking agent / the number of molar equivalents of the acid groups of the polymer (b)". As described above, when some of the acid groups of the polymer (b) are neutralized, the neutralized acid groups can also become crosslinking points. Therefore, when the sum of the neutralization degree and the crosslinking degree exceeds 100 mol %, the crosslinking degree is expressed as "the number of molar equivalents of the crosslinkable functional groups of the crosslinking agent / the number of molar equivalents of the acid groups of the polymer (b)" as described above, and the neutralization degree of the polymer (b') is the value obtained by subtracting the crosslinking degree from 100 mol %.
[0053] The acid value of the crosslinked polymer (b') is preferably 40 mgKOH / g or more, more preferably 60 mgKOH / g or more, more preferably 80 mgKOH / g or more, even more preferably 100 mgKOH / g or more, even more preferably 110 mgKOH / g or more, and is preferably 200 mgKOH / g or less, more preferably 180 mgKOH / g or less, even more preferably 160 mgKOH / g or less, even more preferably 140 mgKOH / g or less, and even more preferably 130 mgKOH / g or less, from the viewpoint of improving the dispersion stability of the polymer particles (B) in the aqueous phase, and improving the storage stability, and is preferably 200 mgKOH / g or less, more preferably 180 mgKOH / g or less, even more preferably 160 mgKOH / g or less, even more preferably 140 mgKOH / g or less, and even more preferably 130 mgKOH / g or less. If the acid value is in the above range, the amount of acid groups can be sufficient to ensure the dispersion stability of the polymer particles (B). The acid value of the crosslinked polymer (b') can be measured by the method described in the Examples. When the crosslinked polymer (b') is obtained by crosslinking the polymer (b) with a crosslinking agent, the acid value of the crosslinked polymer (b') can also be calculated by the following formula. Acid value of crosslinked polymer (b') (mg KOH / g) = [Acid value of polymer (b) (mg KOH / g)] × [100 - degree of crosslinking (mol%)] / 100 Here, the acid value of the polymer (b) is as described above. Also, the degree of crosslinking is expressed as "the molar equivalent number of the crosslinkable functional group of the crosslinking agent / the molar equivalent number of the acid group of the polymer (b)" as described above.
[0054] At least a part of the acid groups of the crosslinked polymer (b') is preferably neutralized from the viewpoint of improving the dispersion stability of the polymer particles B in the aqueous phase, thereby improving storage stability, and from the viewpoint of improving fixability. Examples of the neutralizing agent used for neutralizing the crosslinked polymer (b') include the same neutralizing agents as those exemplified for the above-mentioned polymer (a). The counter ion of the neutralized acid group of the crosslinked polymer (b') is preferably an alkali metal cation, more preferably a sodium ion (Na + ) and potassium ion (K + ) is one or more selected from the following. Regarding the degree of neutralization of the crosslinked polymer (b'), a part of the acid groups of the crosslinked polymer (b') may be neutralized, or all of the acid groups may be neutralized.
[0055] <Oil phase> The oil phase of the emulsion ink of the present invention contains a water-insoluble organic solvent and an emulsifier from the viewpoint of improving storage stability and fixability.
[0056] (Non-water-soluble organic solvent) A water-insoluble organic solvent is an organic solvent that dissolves in less than 10 mL of water at 25° C. when dissolved in 100 mL of water. As the non-water-soluble organic solvent, either a non-polar organic solvent or a polar organic solvent can be used. These can be used alone or in combination of two or more kinds as long as they form a single continuous phase.
[0057] Examples of non-polar organic solvents include aliphatic hydrocarbon solvents such as paraffin-based, isoparaffin-based, and naphthenic hydrocarbon solvents, alicyclic hydrocarbon solvents, and aromatic hydrocarbon solvents. The initial boiling point of the non-polar organic solvent is preferably 90° C. or higher, more preferably 150° C. or higher, and preferably 300° C. or lower, more preferably 250° C. or lower. Commercially available non-polar organic solvents include the Isopar (trade name) series and Exxor (trade name) series (both manufactured by ExxonMobil Corporation); and the AF Solvent (trade name) series (manufactured by JXTG Nippon Oil & Energy Corporation).
[0058] Examples of the polar organic solvent include ester-based solvents and higher alcohol-based solvents. The ester solvent is preferably a fatty acid ester solvent. Examples of the fatty acid ester solvent include fatty acid esters having 13 to 30 carbon atoms, such as isononyl isononanoate, isodecyl isononanoate, isotridecyl isononanoate, methyl laurate, isopropyl laurate, hexyl laurate, 2-ethylhexyl laurate, isopropyl myristate, isopropyl palmitate, isostearyl palmitate, methyl oleate, ethyl oleate, isopropyl oleate, isobutyl oleate, methyl linoleate, ethyl linoleate, isobutyl linoleate, butyl stearate, 2-ethylhexyl stearate, isopropyl isostearate, methyl soybean oil, isobutyl soybean oil, methyl tall oil, isobutyl tall oil, propylene glycol monocaprate, diisopropyl adipate, diisopropyl sebacate, diethyl sebacate, trimethylolpropane tri-2-ethylhexanoate, and glyceryl tri-2-ethylhexanoate. Examples of higher alcohol solvents include higher alcohols having 12 to 20 carbon atoms, such as isomyristyl alcohol, isopalmityl alcohol, isostearyl alcohol, and oleyl alcohol.
[0059] From the viewpoint of improving storage stability and fixability, the non-water-soluble organic solvent preferably contains one or more selected from hydrocarbon-based solvents and ester-based solvents, and more preferably contains a hydrocarbon-based solvent and an ester-based solvent. When the water-insoluble organic solvent contains a hydrocarbon solvent and an ester solvent, the content of the hydrocarbon solvent in the water-insoluble organic solvent is, from the viewpoint of improving storage stability and fixability, preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and preferably 90% by mass or less, even more preferably 80% by mass or less.
[0060] (emulsifier) There are no particular limitations on the emulsifier as long as it is contained in the oil phase and can emulsify the aqueous phase to form a water-in-oil emulsion, but lipophilic emulsifiers such as surfactants and polymer dispersants are preferred. As the lipophilic surfactant, a nonionic surfactant having an HLB value of 6 or less is preferred. Examples of the nonionic surfactant include sorbitan fatty acid esters such as sorbitan monooleate, sorbitan sesquioleate, and sorbitan monostearate; polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monooleate and polyoxyethylene sorbitan trioleate; glycerin fatty acid esters such as glycerol monostearate and glycerol monooleate; polyoxyethylene glycerin fatty acid esters such as polyoxyethylene sorbit fatty acid ester and polyoxyethylene glycerin vegetable oil fatty acid ester; sucrose fatty acid esters such as sucrose stearate, sucrose palmitate, sucrose oleate, sucrose erucate, and sucrose laurate; polyethylene glycol fatty acid esters; polyglycerin condensed ricinoleate; polyoxyethylene alkyl ethers; polyoxyethylene alkylphenyl ethers; polyoxyethylene alkylamines / fatty acid amides; and polyoxyethylene polyoxypropylene alkyl ethers. The lipophilic surfactants can be used alone or in combination of two or more kinds.
[0061] Examples of lipophilic polymer dispersants include polyester polyimines, polyester polyamines, polyalkylol aminoamides and their salts, polyether polyamines, hydroxyl group-containing carboxylic acid esters, salts of long-chain polyaminoamides and high molecular weight acid esters, salts of high molecular weight polycarboxylic acids, salts of long-chain polyaminoamides and polar acid esters, high molecular weight unsaturated acid esters, modified polyurethanes, modified poly(meth)acrylates, polyether ester-type anionic surfactants, naphthalene sulfonic acid formalin condensate salts, polyoxyethylene alkyl phosphate esters, polyoxyethylene nonylphenyl ether, and stearylamine acetate. Among these, polyester polyimines, polyester polyamines, polyalkylol aminoamides and their salts, and polyether polyamines are preferred, and polyester polyimines are more preferred. These may be used alone or in combination of two or more.
[0062] The polyester polyimine is preferably an amide or salt formed by reacting a polyalkyleneimine such as polyethyleneimine with a polyester having a carboxy group such as a polymer of hydroxystearic acid or a polymer of a cyclic ester, and includes a dispersant having a graft structure in which two or more polyester chains are bonded as branches to a polyalkyleneimine chain as a backbone. When the non-water-soluble organic solvent contains an ester-based solvent, it is considered that the steric repulsion of the polyester chain of the polyester polyimine in the oil phase suppresses the interaction between the dispersed phase droplet particles, and suppresses the coalescence of the dispersed phase droplet particles, thereby stabilizing the entire emulsion ink system and improving storage stability. Commercially available lipophilic polymer dispersants include, for example, the Solsperse (product name) series manufactured by Lubrizol Japan Co., Ltd.; the Efka (product name) series manufactured by Efka Chemicals; the Disparlon (product name) series manufactured by Kusumoto Chemicals Co., Ltd.; and the Ajisper (product name) series manufactured by Ajinomoto Co., Inc.
[0063] In the present invention, from the viewpoint of improving storage stability and fixability, it is preferable that the oil phase does not contain a colorant such as a pigment.
[0064] [Manufacturing method of water-in-oil emulsion ink] From the viewpoints of improving the dispersion stability of the pigment in the aqueous phase, thereby improving storage stability, and improving fixability, the water-in-oil emulsion ink of the present invention is preferably obtained by a method including the following steps I and II. Step I: A step of mixing and emulsifying a first aqueous phase component containing an aqueous pigment dispersion in which a pigment is dispersed in an aqueous medium with a polymer dispersant A with an oil phase component containing a water-insoluble organic solvent and an emulsifier to obtain a preparation. Step II: A step of adding a second aqueous phase component containing an aqueous dispersion of polymer particles B that does not contain a pigment to the preparation obtained in step I, mixing and emulsifying the mixture to obtain a water-in-oil emulsion ink. Here, the term "aqueous" in the aqueous pigment dispersion means that water accounts for the largest proportion of the medium in which the pigment is dispersed. Also, the term "aqueous" in the aqueous dispersion of polymer particles B that do not contain a pigment means that water accounts for the largest proportion of the medium in which the pigment-free polymer particles B are dispersed.
[0065] (Process I) Step I is a step of mixing and emulsifying a first aqueous phase component containing an aqueous pigment dispersion in which a pigment is dispersed in an aqueous medium with polymer dispersant A, and an oil phase component containing a water-insoluble organic solvent and an emulsifier, to obtain a preparation.
[0066] In the case where the first aqueous phase contains the above-mentioned surfactant, water-soluble organic solvent, or optional component, the aqueous pigment dispersion is mixed with the surfactant, water-soluble organic solvent, or optional component as necessary, or the water content is adjusted to prepare a first aqueous phase component, and then the first aqueous phase component and an oil phase component are mixed and emulsified, thereby obtaining a preparation in which the first aqueous phase is dispersed in the oil phase. The amount of the first aqueous phase component, per 100 parts by mass of the oil phase component, from the standpoint of productivity and of obtaining a stable emulsion, is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, even more preferably 15 parts by mass or more, even more preferably 20 parts by mass or more, and is preferably 40 parts by mass or less, more preferably 35 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 25 parts by mass or less.
[0067] The stirring means used for mixing and emulsification in step I is not particularly limited as long as it can apply shear force, but a high-speed stirring and mixing device such as a homogenizer (e.g., "Ultra Turrax" by IKA Japan Co., Ltd.), a homomixer, or a disper (e.g., "Ultra Disper" by Asada Iron Works Co., Ltd.) is preferred. For example, when using a homogenizer, when the first aqueous phase component is dropped into the oil phase component, the rotation speed of the homogenizer is preferably adjusted to 500 rpm or more, more preferably 1,000 rpm or more, even more preferably 1,500 rpm or more, and preferably 8,000 rpm or less, more preferably 7,000 rpm or less, and even more preferably 6,000 rpm or less. After the first aqueous phase component is dropped, the rotation speed of the homogenizer is preferably adjusted to 5,000 rpm or more, more preferably 7,000 rpm or more, even more preferably 10,000 rpm or more, and preferably 20,000 rpm or less, more preferably 17,000 rpm or less, and even more preferably 15,000 rpm or less.
[0068] [Preparation of Water-Based Pigment Dispersion] In the present invention, when the pigment is dispersed using a non-crosslinked polymer (a) as the polymer dispersant A, the water-based pigment dispersion is preferably produced efficiently by a method including the following step A1. Step A1: A step of dispersing a pigment mixture containing a pigment, a polymer (a) and water to obtain an aqueous pigment dispersion in which the pigment is dispersed in an aqueous medium by the polymer (a).
[0069] (Process A1) Specifically, step A1 is preferably carried out by (1) a method of dispersing a pigment mixture obtained by mixing a previously prepared aqueous dispersion of polymer (a) particles with a pigment, or (2) a method of dispersing a pigment mixture containing a pigment, polymer (a), an organic solvent, water, and, if necessary, a neutralizing agent, a surfactant, etc., to obtain a dispersion, and then removing the organic solvent from the dispersion, etc. Among these, method (1) is preferred from the viewpoint of improving storage stability and fixability.
[0070] In the case of the method (1), it is preferable to have the following step A1-1 before the step A1. Step A1-1: A step of neutralizing a portion of the acid groups of the polymer (a) with a neutralizing agent to obtain an aqueous dispersion of polymer (a) particles. The preferred neutralizing agent and the degree of neutralization of the polymer (a) used in the neutralization in step A1-1 are as described above. The neutralizing agent is preferably used in the form of an aqueous solution in order to promote sufficient and uniform neutralization.
[0071] In the dispersion treatment in step A1, the pigment can be atomized to a desired particle size only by main dispersion using shear stress. However, from the viewpoint of obtaining a uniform aqueous pigment dispersion, it is preferable to pre-disperse the pigment mixture and then further carry out main dispersion. As a dispersing machine used for preliminary dispersion, a commonly used mixing and stirring device such as an anchor blade or a dispersing blade can be used. Examples of means for applying shear stress used in the present dispersion include kneaders such as roll mills and kneaders, high-pressure homogenizers such as microfluidizers, and media-type dispersers such as paint shakers and bead mills. Among these, it is preferable to use a high-pressure homogenizer from the viewpoint of reducing the particle size of the pigment. When the dispersion treatment is performed using a high-pressure homogenizer, the pigment can be controlled to have a desired particle size by controlling the treatment pressure and the number of passes, and the cumulant average particle size of the aqueous pigment dispersion described below can also be adjusted. From the viewpoints of productivity and economy, the treatment pressure is preferably 60 MPa or more and 300 MPa or less. The number of passes is preferably 3 or more, more preferably 7 or more, from the viewpoint of reducing the particle size of the pigment, and is preferably 30 or less, more preferably 20 or less, from the viewpoint of the dispersion stability of the pigment. When the pigment mixture contains an organic solvent, the organic solvent can be removed by a known method to obtain an aqueous pigment dispersion. It is preferable that the organic solvent in the obtained aqueous pigment dispersion is substantially removed, but it may remain as long as it does not impair the object of the present invention. The amount of the residual organic solvent is preferably 0.1% by mass or less, more preferably 0.01% by mass or less.
[0072] (Process A2) In the present invention, when the pigment is dispersed using a crosslinked polymer (a') as the polymer dispersant A, the aqueous pigment dispersion is preferably obtained after step A1, preferably by a method including step A1-1 and further including the following step A2 after step A1. Step A2: A step of adding a crosslinking agent to the aqueous pigment dispersion obtained in step A1, and crosslinking the polymer (a) with the crosslinking agent to obtain an aqueous pigment dispersion in which the pigment is dispersed in the crosslinked polymer (a').
[0073] In step A2, the preferred crosslinking agent and the degree of crosslinking are as described above. The temperature of the crosslinking treatment is preferably 40°C or higher, more preferably 50°C or higher, and even more preferably 60°C or higher, and is preferably 95°C or lower, more preferably 85°C or lower, and even more preferably 75°C or lower. From the viewpoints of completion of the crosslinking reaction and economic efficiency, the time for the crosslinking treatment is preferably 0.5 hours or more, more preferably 1 hour or more, even more preferably 3 hours or more, and is preferably 12 hours or less, more preferably 10 hours or less, even more preferably 8 hours or less.
[0074] From the viewpoints of improving the dispersion stability, improving the storage stability, and facilitating the production of the ink, the non-volatile component concentration (solid content concentration) of the aqueous pigment dispersion is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and is preferably 60% by mass or less, more preferably 55% by mass or less, even more preferably 50% by mass or less. The solid content concentration of the aqueous pigment dispersion is measured by the method described in the Examples.
[0075] From the viewpoint of improving storage stability and fixability, the cumulant average particle size of the aqueous pigment dispersion is preferably 50 nm or more, more preferably 60 nm or more, even more preferably 70 nm or more, still more preferably 80 nm or more, still more preferably 90 nm or more, and is preferably 200 nm or less, more preferably 150 nm or less, even more preferably 130 nm or less, still more preferably 100 nm or less, and still more preferably less than 100 nm. The cumulant average particle size of the aqueous pigment dispersion is measured by the method described in the Examples.
[0076] The aqueous pigment dispersion is preferably a dispersion in which pigment-containing polymer particles are dispersed in an aqueous medium. The form of the pigment-containing polymer particles is not particularly limited as long as the particles are formed by at least the pigment and the non-crosslinked polymer (a) or the crosslinked polymer (a'), but as described above, the form of the particles is preferably a form in which the pigment is encapsulated in the non-crosslinked polymer (a) or the crosslinked polymer (a'). The aqueous pigment dispersion may contain 1% by mass or more and 10% by mass or less of glycerin, polyethylene glycol, or the like as a moisturizing agent to prevent drying, and may also contain additives such as antifungal agents. The above additives may be added when the pigment is dispersed in the polymer (a), or may be added after the pigment is dispersed or crosslinked.
[0077] (Process II) Step II is a step of adding a second aqueous phase component containing an aqueous dispersion of polymer particles B that does not contain a pigment to the preparation obtained in Step I, mixing and emulsifying the mixture to obtain a water-in-oil emulsion ink.
[0078] In the case where the second aqueous phase contains the above-mentioned surfactant, water-soluble organic solvent, or optional component, the aqueous dispersion of polymer particles B is mixed with the surfactant, water-soluble organic solvent, or optional component as necessary, or the water content is adjusted to prepare a second aqueous phase component, and then the second aqueous phase component is added to the preparation obtained in step I, followed by mixing and emulsification, to obtain a water-in-oil emulsion ink in which the second aqueous phase is dispersed in the oil phase. The amount of the second aqueous phase component, from the standpoint of productivity and obtaining a stable emulsion, is preferably 1 part by mass or more, more preferably 3 parts by mass or more, even more preferably 5 parts by mass or more, still more preferably 8 parts by mass or more, and is preferably 25 parts by mass or less, more preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 13 parts by mass or less, per 100 parts by mass of the oil phase component.
[0079] The stirring means used for mixing and emulsification in step II may be the same as those exemplified in step I. For example, when using a homogenizer, it is preferable to adjust the rotation speed of the homogenizer to preferably 500 rpm or more, more preferably 1,000 rpm or more, even more preferably 1,500 rpm or more, and preferably 8,000 rpm or less, more preferably 7,000 rpm or less, and even more preferably 6,000 rpm or less when dropping the second aqueous phase component into the preparation obtained in step I. Then, after the completion of dropping the second aqueous phase component, it is preferable to adjust the rotation speed of the homogenizer to preferably 5,000 rpm or more, more preferably 7,000 rpm or more, even more preferably 10,000 rpm or more, and preferably 20,000 rpm or less, more preferably 17,000 rpm or less, and even more preferably 15,000 rpm or less.
[0080] [Preparation of aqueous dispersion of pigment-free polymer particles B] The polymer particles B not containing a pigment (polymer particles B) may be appropriately synthesized or may be a commercially available product, but is preferably used as an aqueous dispersion. The aqueous dispersion of polymer particles B can be produced by a method in which a polymer constituting the polymer particles B is obtained by a known polymerization method, and then a mixture containing the polymer, water, and optionally a neutralizing agent is stirred while being heated, and then the temperature is lowered; a method in which a mixture containing the polymer, an organic solvent, a neutralizing agent, and water is dispersed to obtain a dispersion, and then the organic solvent is removed from the dispersion, etc. Among these, from the viewpoint of ease of operation, the method in which a mixture containing the polymer, water, and a neutralizing agent is stirred while being heated, and then the temperature is lowered is preferred.
[0081] The temperature when the mixture is stirred is preferably 60° C. or more, more preferably 70° C. or more, even more preferably 80° C. or more, and preferably 100° C. or less, more preferably 95° C. or less. The stirring time is preferably 0.5 hours or more, more preferably 1 hour or more, even more preferably 3 hours or more, and preferably 30 hours or less, more preferably 15 hours or less, even more preferably 10 hours or less.
[0082] In the case where the polymer constituting the polymer particles B is a non-crosslinked polymer (b), the aqueous dispersion of the polymer particles B is preferably prepared by neutralizing the polymer (b) with a neutralizing agent. In this case, the aqueous dispersion of the polymer particles B preferably includes the following step B1-1. Step B1-1: A step of neutralizing a portion of the acid groups of the polymer (b) with a neutralizing agent to obtain an aqueous dispersion of polymer (b) particles. The preferred neutralizing agent and the degree of neutralization of the polymer (b) used in the neutralization in step B1-1 are as described above. The neutralizing agent is preferably used in the form of an aqueous solution in order to promote sufficient and uniform neutralization.
[0083] (Process B1) When the polymer particles B are composed of a crosslinked polymer (b') obtained by crosslinking a non-crosslinked polymer (b) with a crosslinking agent, it is preferable that the aqueous dispersion of the polymer particles B is obtained by a method that further includes the following step B1 after step B1-1. Step B1: A step of adding a crosslinking agent to the aqueous dispersion of polymer (b) particles obtained in step B1-1, crosslinking the polymer (b) with the crosslinking agent, and obtaining an aqueous dispersion of polymer particles B that does not contain a pigment and is composed of a crosslinked polymer (b').
[0084] In step B1, the preferred crosslinking agent and the degree of crosslinking are as described above. The temperature of the crosslinking treatment is preferably 40°C or higher, more preferably 50°C or higher, and even more preferably 60°C or higher, and is preferably 95°C or lower, more preferably 85°C or lower, and even more preferably 75°C or lower. From the viewpoints of completion of the crosslinking reaction and economic efficiency, the time for the crosslinking treatment is preferably 0.5 hours or more, more preferably 1 hour or more, even more preferably 3 hours or more, and is preferably 12 hours or less, more preferably 10 hours or less, even more preferably 8 hours or less.
[0085] The non-volatile component concentration (solid content concentration) of the aqueous dispersion of polymer particles B is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 35% by mass or more, and is preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 45% by mass or less, from the viewpoints of improving the dispersion stability of polymer particles B, improving storage stability, improving fixability, and facilitating production of ink. The solid content concentration of the aqueous dispersion of polymer particles B is measured by the method described in the Examples.
[0086] From the viewpoint of improving storage stability and fixability, the cumulant average particle size of the aqueous dispersion of polymer particles B is preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 10 nm or more, and is preferably 200 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less. The average particle size is measured by the method described in the Examples.
[0087] The total amount of the first aqueous phase component and the second aqueous phase component is, from the viewpoint of productivity and of obtaining a stable emulsion, preferably 20 parts by mass or more, more preferably 25 parts by mass or more, even more preferably 30 parts by mass or more, and is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and more preferably 40 parts by mass or less, per 100 parts by mass of the oil phase component, from the viewpoint of productivity and of obtaining a stable emulsion.
[0088] If necessary, the emulsion ink of the present invention may further contain various additives commonly used in water-in-oil emulsion inks, such as a humectant, wetting agent, penetrating agent, dispersant, surfactant, viscosity modifier, defoamer, preservative, antifungal agent and rust inhibitor, and may further be subjected to filtration treatment using a filter or the like. The contents and physical properties of each component in the emulsion ink of the present invention are as follows.
[0089] From the viewpoint of improving print density, the content of the pigment in the emulsion ink is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and even more preferably 5% by mass or more, and from the viewpoint of reducing the ink viscosity when the solvent evaporates and improving storage stability, the content of the pigment in the emulsion ink is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 7% by mass or less.
[0090] The total content of the pigment and polymer dispersant A in the emulsion ink is preferably 3% by mass or more, more preferably 4% by mass or more, even more preferably 5% by mass or more, and is preferably 15% by mass or less, more preferably 10% by mass or less, even more preferably 7% by mass or less.
[0091] The mass ratio of the pigment content to the polymer dispersant A content in the emulsion ink of the present invention [pigment / polymer dispersant A] is preferably 1 or more, more preferably 3 or more, even more preferably 5 or more, and still more preferably 6 or more, from the viewpoint of improving the print density, and is preferably 10 or less, more preferably 9 or less, and even more preferably 8 or less, from the viewpoint of improving the dispersion stability of the pigment and improving the storage stability. Here, when the polymer dispersant A is a non-crosslinked polymer (a), the mass ratio [pigment / polymer dispersant A] is the mass ratio between the pigment and the non-crosslinked polymer (a) in the aqueous phase [pigment / non-crosslinked polymer (a)], and when the polymer dispersant is a crosslinked polymer (a'), the mass ratio [pigment / polymer dispersant A] is the mass ratio between the pigment and the crosslinked polymer (a') in the aqueous phase [pigment / crosslinked polymer (a')].
[0092] The mass ratio of the content of the pigment-free polymer particles B to the content of the pigment in the emulsion ink of the present invention [pigment-free polymer particles B / pigment] is, from the viewpoint of improving print density, preferably 0.03 or more, more preferably 0.05 or more, even more preferably 0.1 or more, still more preferably 0.3 or more, and still more preferably 0.5 or more, and from the viewpoint of obtaining a stable emulsion and improving storage stability, is preferably 1.5 or less, more preferably 1.3 or less, even more preferably 1 or less, and still more preferably 0.8 or less.
[0093] From the viewpoint of improving storage stability and fixability, the water content in the emulsion ink of the present invention is preferably 5% by mass or more, more preferably 7% by mass or more, even more preferably 9% by mass or more, still more preferably 10% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, even more preferably 20% by mass or less, and still more preferably 18% by mass or less.
[0094] From the viewpoints of improving the storage stability and fixability, and of adjusting the viscosity of the emulsion ink, the content of the water-insoluble organic solvent in the emulsion ink is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 65% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, even more preferably 75% by mass or less, and still more preferably 70% by mass or less.
[0095] From the viewpoint of stabilizing the emulsion and improving storage stability, the content of the emulsifier in the emulsion ink is preferably 0.5% by mass or more, more preferably 1% by mass or more, even more preferably 3% by mass or more, and is preferably 15% by mass or less, more preferably 10% by mass or less, even more preferably 7% by mass or less.
[0096] In the present invention, from the viewpoint of improving the dispersion stability of the pigment and improving the storage stability, it is preferable that the pigment-containing polymer particles or pigment-containing crosslinked polymer particles in the first aqueous phase do not swell, shrink, or aggregate between the particles, and when the emulsion ink of the present invention is produced using the above-mentioned aqueous pigment dispersion, it is preferable that the average particle size of the pigment-containing polymer particles or pigment-containing crosslinked polymer particles is the same as the cumulant average particle size of the above-mentioned aqueous pigment dispersion. That is, the cumulant average particle size of the pigment-containing polymer particles or pigment-containing crosslinked polymer particles in the first aqueous phase is preferably 50 nm or more, more preferably 60 nm or more, even more preferably 70 nm or more, still more preferably 80 nm or more, still more preferably 90 nm or more, and preferably 200 nm or less, more preferably 150 nm or less, even more preferably 130 nm or less, still more preferably 100 nm or less, and still more preferably less than 100 nm. In addition, when measuring the average particle size of the pigment-containing polymer particles or pigment-containing crosslinked polymer particles in the first aqueous phase of the emulsion ink, the average particle size of the pigment-containing polymer particles or pigment-containing crosslinked polymer particles can be measured, for example, by recovering the aqueous phase component from the emulsion ink and observing the average particle size of the pigment-containing polymer particles or pigment-containing crosslinked polymer particles with an electron microscope.
[0097] In the present invention, from the viewpoint of improving storage stability and fixability, it is preferable that the pigment-free polymer particles B in the second aqueous phase do not swell or shrink or aggregate between the particles, and when the emulsion ink of the present invention is produced using the above-mentioned aqueous dispersion of pigment-free polymer particles B, it is preferable that the average particle size of the pigment-free polymer particles B is the same as the cumulant average particle size of the aqueous dispersion of pigment-free polymer particles B. That is, the cumulant average particle size of the pigment-free polymer particles in the second phase is preferably 1 nm or more, more preferably 5 nm or more, even more preferably 10 nm or more, and preferably 200 nm or less, more preferably 150 nm or less, even more preferably 100 nm or less. In addition, when measuring the average particle size of the pigment-free polymer particles B in the second aqueous phase of the emulsion ink, the average particle size of the pigment-free polymer particles B can be measured, for example, by recovering the aqueous phase component from the emulsion ink and observing the average particle size of the pigment-free polymer particles B with an electron microscope.
[0098] In the present invention, from the viewpoint of ease of production and of improving storage stability and fixability, the average particle size of the emulsion is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.5 μm or more, and is preferably 2.0 μm or less, more preferably 1.7 μm or less, even more preferably 1.5 μm or less. The average particle size of the emulsion is measured by the method described in the Examples.
[0099] The viscosity of the emulsion ink of the present invention at 25°C is preferably 2 mPa·s or more, more preferably 5 mPa·s or more, even more preferably 7 mPa·s or more, and still more preferably 9 mPa·s or more, and from the viewpoint of using the emulsion ink for inkjet recording, preferably 20 mPa·s or less, more preferably 17 mPa·s or less, even more preferably 15 mPa·s or less, and still more preferably 13 mPa·s or less. The viscosity of the emulsion ink can be measured using an E-type viscometer (model: TV-25, manufactured by Toki Sangyo Co., Ltd., using a standard cone rotor 1°34′×R24, rotation speed 50 rpm).
[0100] From the viewpoint of ejection properties, the emulsion ink of the present invention is preferably used for inkjet recording. The emulsion ink can be loaded into a known inkjet recording device and ejected as ink droplets onto a printing medium to record an image or the like. The printing medium used may be plain paper with high water absorption, coated paper with low water absorption, or resin film with no water absorption. The coated paper may be general-purpose glossy paper or multicolor foam gloss paper. The resin film may be at least one selected from polyester film, polyvinyl chloride film, polypropylene film, and polyethylene film. The resin film may be a corona-treated substrate. Among these, plain paper is preferred from the viewpoint of fixation. EXAMPLES
[0101] In the following Preparation Examples, Production Examples, Examples and Comparative Examples, "parts" and "%" are "parts by mass" and "% by mass" unless otherwise specified. Various physical properties were measured by the following methods.
[0102] (1) Acid value measurement The measurements were performed according to JIS K0070, except that the measurement solvent was changed from a mixed solvent of ethanol and ether to a mixed solvent of ethanol and toluene [ethanol:toluene=1:1 (volume ratio)].
[0103] (2) Measurement of weight average molecular weight of vinyl resin The measurement was performed by gel permeation chromatography (GPC apparatus (model: HLC-8320GPC, manufactured by Tosoh Corporation), columns (TSKgel SuperAWM-H, TSKgel SuperAW3000, TSKgel guardcolumn Super AW-H, all of which are product names of Tosoh Corporation), flow rate: 0.5 mL / min) using a solution of phosphoric acid and lithium bromide dissolved in N,N-dimethylformamide to a concentration of 60 mmol / L and 50 mmol / L, respectively, as an eluent, and using a monodisperse polystyrene kit with known molecular weights (PStQuick B (F-550, F-80, F-10, F-1, A-1000), PStQuick C (F-288, F-40, F-4, A-5000, A-500), all of which are product names of Tosoh Corporation) as a standard substance. The measurement sample was prepared by mixing 0.1 g of vinyl resin with 10 mL of the eluent in a glass vial, stirring with a magnetic stirrer at 25°C for 10 hours, and filtering with a syringe filter (product name: DISMIC-13HP, membrane filter material: hydrophilic PTFE, pore size 0.2 μm, manufactured by Advantec Co., Ltd.).
[0104] (3) Measurement of solids concentration 10.0 g of sodium sulfate, which had been kept constant in a desiccator, was weighed out into a 30 mL polypropylene container (φ=40 mm, height=30 mm), and about 1.0 g of the sample was added thereto and mixed, then accurately weighed, and maintained at 105°C for 2 hours to remove volatile matter, and then left in the desiccator at room temperature (25°C) for 15 minutes, after which the mass was measured. The mass of the sample after removing the volatile matter was taken as the solid content, and was divided by the mass of the sample added to obtain the solid content concentration.
[0105] (4) Measurement of cumulant average particle size Cumulant analysis was performed using a laser particle analysis system (model: ELS-8000, manufactured by Otsuka Electronics Co., Ltd.) to measure the cumulant average particle size. The measurement conditions were a temperature of 25°C, an angle between the incident light and the detector of 90°, and 100 integrations. The refractive index of water (1.333) was input as the refractive index of the dispersion medium. The concentration of the measurement sample was 5×10-3 % (solids concentration equivalent).
[0106] (5) Average particle size of emulsion The volume median particle size (D) was measured using a laser diffraction / scattering particle size analyzer "Mastersizer 3000" (Malvern Panalytical). 50 ) was taken as the average particle size of the emulsion. The measurement sample was prepared by adding hexyl laurate (product name: Exepar HL, manufactured by Kao Corporation, viscosity at 20°C 6.8 mPa s) to the emulsion ink and adjusting the concentration so that the scattering intensity was 5 to 15%. The particle refractive index was 1.59 (absorption coefficient 0.1, density 1 g / cm 3 ) and the refractive index of the dispersion medium was 1.44.
[0107] <Preparation of vinyl resin> Preparation Example 1 19.2 parts of acrylic acid, 70.8 parts of styrene, and 10.0 parts of α-methylstyrene were mixed to prepare raw material monomers. 10 parts of methyl ethyl ketone (hereinafter referred to as "MEK"), 0.3 parts of 2-mercaptoethanol (polymerization chain transfer agent), and 10% of the raw material monomers were mixed in a reaction vessel, and the atmosphere was thoroughly replaced with nitrogen gas. Meanwhile, a mixture of the remaining raw monomer (90%), 0.27 parts of the polymerization chain transfer agent, 40 parts of MEK, and 1.1 parts of an azo radical polymerization initiator (trade name: V-65, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., 2,2'-azobis(2,4-dimethylvaleronitrile)) (hereinafter referred to as "V-65") was placed in a dropping funnel, and the raw monomer in the reaction vessel was heated to 65°C while stirring under a nitrogen atmosphere, and the mixture in the dropping funnel was dropped over 3 hours. After stirring for 2 hours from the end of the dropping while maintaining the contents in the reaction vessel at 65°C, a solution in which 0.15 parts of the polymerization initiator was dissolved in 2.5 parts of MEK was added, and the mixture was further aged at 65°C for 2 hours and 70°C for 2 hours to obtain a solution of a vinyl resin (P1) having a carboxy group. The weight average molecular weight and acid value are shown in Table 1.
[0108] Preparation Example 2 and Preparation Example 4 Solutions of vinyl resins (P2) and (P4) having a carboxy group were obtained in the same manner as in Preparation Example 1, except that the compositions of the raw material monomers were changed as shown in Table 1. The weight average molecular weights and acid values are shown in Table 1.
[0109] Preparation Example 3 37.0 parts of methacrylic acid, 33.0 parts of benzyl acrylate, 40.0 parts of styrene macromer (manufactured by Toagosei Co., Ltd., trade name: AS-6S, number average molecular weight: 6,000, solid content concentration 50%) (hereinafter referred to as "styrene macromer") (20.0 parts as solid content), and 10.0 parts of polypropylene glycol monomethacrylate (manufactured by NOF Corporation, trade name: Blenmer PP-800, average number of propylene oxide added moles: 13, terminal: hydroxyl group) (hereinafter referred to as "PP-800") were mixed to prepare a raw material monomer. In a reaction vessel, 10 parts of MEK, 0.3 parts of 2-mercaptoethanol (polymerization chain transfer agent), and 10% of the raw material monomer were added and mixed, and nitrogen gas replacement was performed sufficiently. Meanwhile, a mixture of the remaining raw material monomers (90%), 0.27 parts of the polymerization chain transfer agent, 40 parts of MEK, and 1.1 parts of the azo radical polymerization initiator (V-65) was placed in a dropping funnel, and the rest of the procedure was the same as in Preparation Example 1 to obtain a solution of a vinyl resin (P3) having a carboxy group. The weight average molecular weight and acid value are shown in Table 1.
[0110] [Table 1]
[0111] <Production of Aqueous Dispersion of Polymer Particles (Step A1-1 and Step B1-1)> Manufacturing Example 1-1 The vinyl resin solution obtained in Preparation Example 1 was dried under reduced pressure, and then 80.0 parts of the vinyl resin (P1) obtained by pulverization was added with 316.0 parts of ion-exchanged water and 25.3 parts of a 5N aqueous sodium hydroxide solution so that the ratio of the number of moles of sodium hydroxide to the number of moles of carboxyl groups in the vinyl resin (P1) became 50 mol% (neutralization degree: 50 mol%). The mixture was neutralized and dispersed by heating at 90°C for 5 hours while stirring at 150 rpm, to obtain an aqueous dispersion (D1) of polymer particles (solid concentration: 20%, cumulant average particle size: 56 nm).
[0112] Manufacturing Examples 1-2 to 1-4 In Production Example 1-1, the type of vinyl resin, the amount of sodium hydroxide aqueous solution, and the amount of ion-exchanged water were changed as shown in Table 2, but in the same manner, aqueous dispersions (D2) to (D4) of polymer particles (all having a solid content concentration of 20% and a degree of neutralization of 50 mol%) were obtained.
[0113] [Table 2]
[0114] <Production of Water-Based Pigment Dispersion (i) (Step A1)> Manufacturing Example 2-1 400.0 parts of ion-exchanged water and 100.0 parts of black pigment (carbon black, trade name: MONARCH717, manufactured by Cabot Corporation, DBP oil absorption amount 53mL / 100g) were added to 55.5 parts of the aqueous dispersion (D1) of polymer particles obtained in Production Example 1-1, and the mixture was stirred for 60 minutes using a Disper (manufactured by Asada Iron Works Co., Ltd., trade name: Ultra Disper) at 20°C with a Disper blade rotating at 7,000 rpm. The resulting mixture was subjected to 10-pass dispersion treatment at a pressure of 200 MPa using a Microfluidizer (manufactured by Microfluidics, trade name) to obtain a dispersion treatment product. The obtained dispersion was filtered using a 25 mL needleless syringe (manufactured by Terumo Corporation) equipped with a 5 μm filter (acetyl cellulose membrane, outer diameter: 2.5 cm, manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) to remove coarse particles, and then an aqueous pigment dispersion (i-1) with a solid content of 20% was obtained.
[0115] Manufacturing Examples 2-2 to 2-4 Water-based pigment dispersions (i-2) to (i-4) were obtained in the same manner as in Production Example 2-1, except that the type of water-based dispersion of polymer particles was changed as shown in Table 3.
[0116] [Table 3]
[0117] <Production of Water-Based Pigment Dispersion (Step A2)> Manufacturing Example 3-1 100.0 parts (solids concentration 20%) of the water-based pigment dispersion (i-1) obtained in Production Example 2-1 was placed in a screw-capped glass bottle, and 0.37 parts of trimethylolpropane polyglycidyl ether (product name: Denacol EX-321, manufactured by Nagase ChemteX Corporation, epoxy equivalent: 139, water solubility: 27%) (hereinafter referred to as "EX-321") was added as a crosslinking agent so that 50 mol % of the total carboxy groups in the vinyl resin (P1) as the polymer (a) were crosslinked (crosslinking degree 50 mol %). The bottle was then sealed and heated at 70°C for 5 hours while stirring with a stirrer. After 5 hours, the temperature was lowered to room temperature, and the solution was filtered using a 25 mL needleless syringe (Terumo Corporation) equipped with a 5 μm filter (acetyl cellulose membrane, outer diameter: 2.5 cm, Fujifilm Wako Pure Chemical Industries, Ltd.), and then concentrated under reduced pressure so that the pigment content in the resulting aqueous pigment dispersion was 40.0 mass%, to obtain an aqueous black pigment dispersion (hereinafter also referred to as "black pigment dispersion") Bk-I (mass ratio [pigment / crosslinked polymer (a')] = 7.9, pigment content 40.0%, cumulant average particle size: 95 nm).
[0118] Manufacturing Examples 3-2 to 3-4 Black pigment dispersions Bk-II to Bk-IV were obtained in the same manner as in Production Example 3-1, except that the type of water-based pigment dispersion (i) and the amount of crosslinking agent were changed as shown in Table 4.
[0119] [Table 4]
[0120] <Production of aqueous dispersion of polymer particles B not containing pigment (step B1)> Manufacturing Example 4-1 100.0 parts (solid content concentration 20%) of the aqueous dispersion of polymer particles obtained in Production Example 1-1 (D1) was taken into a screw-top glass bottle, and 3.71 parts of trimethylolpropane polyglycidyl ether (EX-321) was added as a crosslinking agent so that 50 mol% of the total carboxyl groups of the polymer (P1) as the polymer (b) were crosslinked (crosslinking degree 50 mol%), and the bottle was sealed and heated at 70 ° C. for 5 hours while stirring with a stirrer. After 5 hours, the temperature was lowered to room temperature, and the bottle was filtered with a 25 mL needleless syringe (Terumo Corporation) equipped with a 5 μm filter (acetyl cellulose membrane, outer diameter: 2.5 cm, Fujifilm Wako Pure Chemical Industries, Ltd.), and further concentrated under reduced pressure so that the solid content concentration of the aqueous dispersion obtained was 40.0%, to obtain an aqueous dispersion of crosslinked polymer particles B not containing a pigment (D1-CL1) (solid content concentration: 40.0%, cumulant average particle size: 56 nm).
[0121] Manufacturing Examples 4-2 and 4-3 In Production Example 4-1, the type and amount of the aqueous dispersion of polymer particles and the amount of the crosslinking agent were changed as shown in Table 5, and similar procedures were followed to obtain aqueous dispersions (D2-CL1) to (D3-CL1) of crosslinked polymer particles B not containing a pigment.
[0122] Manufacturing Example 4-4 The aqueous dispersion (D2) of polymer particles obtained in Production Example 1-2 was concentrated under reduced pressure so that the solid content of the aqueous dispersion became 40.0%, to obtain an aqueous dispersion (D2-NCL1) of non-crosslinked polymer particles B not containing a pigment.
[0123] [Table 5]
[0124] <Water-in-oil emulsion ink> Example 1 A water-in-oil emulsion ink Bk-1 was obtained by the following procedure so that the pigment content in the resulting water-in-oil emulsion ink was 5.0%. (Process I) A first aqueous phase component was prepared by mixing 12.5 parts of the pigment dispersion Bk-I obtained in Production Example 3-1 and 4.2 parts of ion-exchanged water. Separately, 51.0 parts of a hydrocarbon solvent (product name: AF Solvent No. 4 (petroleum hydrocarbon), manufactured by JXTG Nippon Oil & Energy Corporation) as a water-insoluble organic solvent, 18.5 parts of an ester solvent (product name: Exepar M-OL (methyl oleate), manufactured by Kao Corporation), and 5.0 parts of sucrose erucate ester (product name: Ryoto Sugar Ester ER-290, manufactured by Mitsubishi Chemical Foods Corporation) as an emulsifier were mixed to prepare an oil phase component. Using a homogenizer (product name: ULTLRA-TURRAX, model: T25 digital, shaft generator (model: S25N-25F), all manufactured by IKA Japan Co., Ltd.), the first aqueous phase component was added dropwise while stirring the oil phase component at 5,000 rpm. After completion of the dropwise addition, the mixture was stirred at 12,000 rpm for 3 minutes to obtain a preparation. (Process II) While stirring the preparation obtained in step I at 5,000 rpm, 8.8 parts of the water dispersion D1-CL1 of the crosslinked polymer particles B not containing a pigment obtained in Production Example 4-1 was added dropwise as the second water phase component. After the addition was completed, the mixture was stirred at 12,000 rpm for 3 minutes to obtain an oil-and-water type emulsion ink Bk-1 (average particle size of the emulsion: 1.2 μm).
[0125] Examples 2 to 11 Each water-in-oil emulsion ink was obtained in the same manner as in Example 1, except that the type or amount of each component constituting the first aqueous phase component, the second aqueous phase component, and the oil phase component was changed as shown in Table 6.
[0126] Comparative Example 1 A water-in-oil emulsion ink Bk-C1 was obtained by the following procedure so that the pigment content in the resulting water-in-oil emulsion ink was 5.0%. An aqueous phase component was prepared by mixing 12.5 parts of the water-based black pigment dispersion Bk-II obtained in Production Example 3-2 and 11.0 parts of ion-exchanged water. Separately, 51.0 parts of a hydrocarbon solvent (product name: AF Solvent No. 4 (petroleum hydrocarbon), manufactured by JXTG Nippon Oil & Energy Corporation) as a water-insoluble organic solvent, 20.5 parts of an ester solvent (product name: Exepar M-OL (methyl oleate), manufactured by Kao Corporation), and 5.0 parts of sucrose erucate ester (product name: Ryoto Sugar Ester ER-290, manufactured by Mitsubishi Chemical Foods Corporation) as an emulsifier were mixed to prepare an oil phase component. Using a homogenizer (product name: ULTLRA-TURRAX, model: T25 digital, shaft generator (model: S25N-25F), all manufactured by IKA Japan Co., Ltd.), the aqueous phase component was added dropwise while stirring the oil phase component at 5,000 rpm. After completion of the addition, the mixture was stirred at 12,000 rpm for 6 minutes to obtain water-in-oil emulsion ink Bk-C1.
[0127] <Evaluation test of water-in-oil emulsion ink> The emulsion inks obtained in the examples and comparative examples were evaluated for storage stability and fixability. The results are shown in Table 6.
[0128] [Evaluation of storage stability] The obtained emulsion ink was placed in a 100 mL screw vial and stored at 23°C and 60°C, respectively. After standing, the emulsion ink was visually observed for separation of the oil and water phases and the presence or absence of aggregated sediment, and evaluated according to the following criteria. (Evaluation Criteria) A: After one week of storage, there was no separation of the oil and water phases of the emulsion ink and no flocculation or sedimentation at either storage temperature of 23°C or 60°C. B: After storage for one week, the samples stored at 23°C showed no separation of the oil and water phases or no flocculated sediment, but the samples stored at 60°C showed separation of the oil and water phases of the emulsion ink or no flocculated sediment. C: After storage for one day, the samples stored at 23°C showed no separation of the oil and water phases or no flocculated sediment, but the samples stored at 60°C showed separation of the oil and water phases of the emulsion ink or no flocculated sediment. If the above evaluation criteria are A or B, it is suitable for practical use. If the above evaluation criteria are C, it may be difficult to use in practice.
[0129] [Evaluation of Fixation] The obtained emulsion ink was filled into an inkjet printer (product name: Business Printer PX-105, manufactured by Seiko Epson Corporation), and a 1 cm x 1 cm solid image was printed on plain paper (product name: Xerox Business 4200 copy paper, manufactured by Fuji Xerox Co., Ltd.) in an environment of room temperature 23°C and relative humidity 50%RH. Five minutes after printing, the bottom of the weight (bottom area 50 cm) was attached to a cellulose nonwoven fabric "BEMCOT (registered trademark) M3-II" (manufactured by Asahi Kasei Corporation). 2 The printed surface was rubbed back and forth five times using a 700g load. The fixation of the image was evaluated based on the degree of staining of the ink transferred to the cellulose nonwoven fabric, according to the following criteria. The evaluation results are shown in Table 1. (Evaluation Criteria) A: There was no dirt on the cellulose nonwoven fabric. B: The cellulose nonwoven fabric was almost free of stains. C: The cellulose nonwoven fabric was slightly soiled. D: The cellulose nonwoven fabric was significantly soiled. If the above evaluation criteria are A or B, the product is suitable for practical use. If the above evaluation criteria are C, the product can withstand practical use. If the above evaluation criteria are D, the product may be difficult to use in practice.
[0130] [Table 6]
[0131] It can be seen from Table 6 that Examples 1 to 11 are excellent in storage stability, and furthermore, compared to Comparative Example 1, they have improved fixability. [Industrial Applicability]
[0132] According to the emulsion ink and the method for producing the emulsion ink of the present invention, it is possible to obtain a printed matter having excellent storage stability and excellent fixation. Furthermore, the emulsion ink of the present invention is useful for inkjet recording.
Claims
1. A water-in-oil emulsion ink containing a first water phase and a second water phase in an oil phase, a first aqueous phase containing a pigment and a polymeric dispersant A; a second aqueous phase containing non-pigmented polymer particles B; the polymer dispersant A and the polymer constituting the pigment-free polymer particles B each contain an acid group, A water-in-oil emulsion ink in which the oil phase contains a non-water-soluble organic solvent and an emulsifier.
2. 2. The water-in-oil emulsion ink according to claim 1, wherein a mass ratio of a content of the polymer particles B not containing a pigment to a content of the pigment in the water-in-oil emulsion ink [pigment-free polymer particles B / pigment] is 0.03 or more and 1.5 or less.
3. 3. The water-in-oil emulsion ink according to claim 1, wherein at least a portion of the acid groups of the polymer dispersant A and the polymer constituting the pigment-free polymer particles B are neutralized with an alkali metal hydroxide.
4. 4. The water-in-oil emulsion ink according to claim 1, wherein the polymer dispersant A and the polymer constituting the pigment-free polymer particles B each contain a crosslinked structure formed by crosslinking with a crosslinking agent.
5. 5. The water-in-oil emulsion ink according to claim 4, wherein the polymer dispersant A is a crosslinked polymer (a') obtained by crosslinking a non-crosslinked polymer (a) with a crosslinking agent, and the crosslinked polymer (a') has an acid value of 40 mgKOH / g or more.
6. 6. The water-in-oil emulsion ink according to claim 1, wherein the water content in the water-in-oil emulsion ink is 5% by mass or more and 30% by mass or less.
7. 7. The water-in-oil emulsion ink according to claim 1, which is for ink-jet recording.
8. A method for producing the water-in-oil emulsion ink according to any one of claims 1 to 7, comprising the following steps I and II: Step I: A step of mixing and emulsifying a first aqueous phase component containing an aqueous pigment dispersion obtained by dispersing a pigment in an aqueous medium with a polymer dispersant A with an oil phase component containing a water-insoluble organic solvent and an emulsifier to obtain a preparation. Step II: A step of adding a second aqueous phase component containing an aqueous dispersion of polymer particles B not containing a pigment to the preparation obtained in step I, mixing and emulsifying the mixture to obtain a water-in-oil emulsion ink.
9. The polymer dispersant A is a crosslinked polymer (a') obtained by crosslinking a non-crosslinked polymer (a) with a crosslinking agent, The method for producing a water-in-oil emulsion ink according to claim 8, wherein the aqueous pigment dispersion used in step I is obtained by a method including the following steps A1-1, A1, and A2: Step A1-1: A step of neutralizing a portion of the acid groups of the polymer (a) with a neutralizing agent to obtain an aqueous dispersion of polymer (a) particles. Step A1: A step of dispersing a pigment mixture containing the aqueous dispersion of polymer (a) particles obtained in Step A1-1 and a pigment to obtain an aqueous pigment dispersion in which the pigment is dispersed in an aqueous medium by the polymer (a). Step A2: A step of adding a crosslinking agent to the aqueous pigment dispersion obtained in Step A1, and crosslinking the polymer (a) with the crosslinking agent to obtain an aqueous pigment dispersion in which the pigment is dispersed in the crosslinked polymer (a').
10. the pigment-free polymer particles B are composed of a crosslinked polymer (b') obtained by crosslinking a non-crosslinked polymer (b) with a crosslinking agent; 10. The method for producing a water-in-oil emulsion ink according to claim 8, wherein the aqueous dispersion of polymer particles B not containing a pigment used in step II is obtained by a method comprising the following steps B1-1 and B1: Step B1-1: A step of neutralizing a portion of the acid groups of the polymer (b) with a neutralizing agent to obtain an aqueous dispersion of polymer (b) particles. Step B1: A step of adding a crosslinking agent to the aqueous dispersion of polymer (b) particles obtained in step 1-1, crosslinking the polymer (b) with the crosslinking agent, and obtaining an aqueous dispersion of polymer particles B that does not contain a pigment and is composed of a crosslinked polymer (b').
Citation Information
Patent Citations
Emulsion ink for stencil printing
JP1995188598A
Production of emulsion ink for mimeographic printing and device therefor
JP1998168370A
Water-based ink for inkjet recording
JP2008063500A
Emulsion ink and method for manufacturing the same
JP2010111849A
Ink composition and inkjet recording method
JP2012251049A