Wire rod that can omit softening heat treatment and its manufacturing method
A wire rod with controlled alloying and microstructure achieves high strength and spheroidization without softening heat treatment, enhancing productivity and cold working capabilities for automotive and construction applications.
Patent Information
- Application Number
- JP2021534917
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-18
- Filing Date
- 2019-12-13
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2039-12-13
AI Technical Summary
Existing wire rod manufacturing processes require lengthy and costly softening heat treatments at high temperatures, which decrease productivity due to slow cooling rates and necessitate specialized equipment, hindering efficient production for applications in automobiles and construction parts.
A wire rod composition comprising specific alloying elements (C, Si, Mn, Cr, Al, Mo, N) with controlled microstructures (pro-eutectoid ferrite, recycled pearlite, bainite, and martensite fractions) and cooling rates, allowing omission of softening heat treatment by refining ferrite and cementite structures through controlled rolling and cooling processes.
The solution enables the production of a wire rod with enhanced strength and spheroidization capabilities, eliminating the need for softening heat treatment and improving productivity by ensuring fine grain sizes and phase distributions, facilitating cold working processes.
Smart Images

Figure 0007576033000005 
Figure 0007576033000006 
Figure 0007576033000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a wire rod for which softening heat treatment can be omitted and a manufacturing method thereof, and more particularly to a wire rod for machine structures applicable to automobiles, construction parts, etc. for which softening heat treatment can be omitted and a manufacturing method thereof. [Background technology]
[0002] Conventionally, softening materials for cold working required long heat treatment at high temperatures of 600 to 800°C for 10 to 20 hours or more, and many technologies have been developed to shorten or eliminate this process.
[0003] A representative technique is described in Patent Document 1. This technique aims to omit the subsequent softening heat treatment step by controlling the ferrite grain size to 11 or more to refine the grains and controlling the hard plate-like cementite phase in the pearlite structure to have about 3 to 15% in a segmented form. However, the production of this material is ensured only by a very slow cooling rate of 0.02 to 0.3°C / s during cooling after hot rolling, but such a slow cooling rate reduces productivity and requires separate slow cooling equipment and a slow cooling yard depending on the environment. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2000-336456 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a wire rod which makes it possible to omit the softening heat treatment required during cold working of automobile, construction parts, etc., and a method for producing the same. [Means for solving the problem]
[0006] The wire rod of the present invention, which can be provided without a softening heat treatment, is characterized in that it comprises, by weight%, 0.2-0.45% C, 0.02-0.4% Si, 0.3-1.5% Mn, 0.3-1.5% Cr, 0.02-0.05% Al, 0.01-0.5% Mo, 0.01% or less N, with the balance being Fe and other unavoidable impurities, has a microstructure in which, by area%, the pro-eutectoid ferrite fraction is 40% or more of the equilibrium phase, the regenerated pearlite and bainite fractions are 40% or more, and the martensite fraction is 20% or less, and the average size of pearlite colonies in a region from the surface to 2 / 5 to 3 / 5 of the diameter is 5 μm or less.
[0007] Another embodiment of the wire rod of the present invention in which the softening heat treatment can be omitted includes a step of heating a billet consisting of, by weight, 0.2-0.45% C, 0.02-0.4% Si, 0.3-1.5% Mn, 0.3-1.5% Cr, 0.02-0.05% Al, 0.01-0.5% Mo, 0.01% or less N, with the balance being Fe and other inevitable impurities, at 950-1050°C, a step of secondary hot rolling the heated billet to obtain a wire rod, a step of coiling the wire rod, and a step of cooling the coiled wire rod to 600°C at a cooling rate of 2°C / sec or less, and then cooling at a cooling rate of 3°C / sec or more, the secondary hot rolling being characterized by including a step of intermediate finish rolling the heated billet, and a step of finish rolling at 730°C to Ae3, which is equal to or greater than the critical deformation amount represented by Equation 1. [Formula 1] Critical deformation amount = -2.46Ceq 2 +3.11Ceq-0.39 (where Ceq=C+Mn / 6+Cr / 5, and C, Mn, and Cr are in weight percent) Effect of the Invention
[0008] According to the present invention, it is possible to provide a wire rod that makes it possible to omit the softening heat treatment that is necessary during cold working of automobile, construction parts, etc., and a method for producing the same. [Brief description of the drawings]
[0009] [Figure 1]1 is a photograph of the microstructure of Comparative Example 1 before finish hot rolling, observed with an optical microscope. [Diagram 2] 1 is a photograph of the microstructure of Example 1 before finish hot rolling, observed with an optical microscope. [Diagram 3] 3A and 3B are photographs of the microstructure of Comparative Example 1 after rolling and cooling, where (a) is a photograph observed with an optical microscope, and (b) is a photograph observed with an SEM. [Figure 4] 3A and 3B are photographs of the microstructure of Example 1 after rolling and cooling, where (a) is a photograph observed with an optical microscope, and (b) is a photograph observed with an SEM. [Diagram 5] 1 is a photograph of the microstructure after spheroidizing heat treatment in Comparative Example 1, observed by SEM. [Figure 6] 1 is a photograph of the microstructure of Example 1 after spheroidizing heat treatment, observed by SEM. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The wire rod according to the present invention for which the softening heat treatment can be omitted will be described below, but first, the alloy composition of the present invention will be described. The contents of the alloy compositions described below are in weight percent unless otherwise specified.
[0011] C: 0.2-0.45% C is an element added to ensure a certain level of strength. If the C content exceeds 0.45%, all the structures are made of pearlite, making it difficult to ensure the ferrite structure targeted by the present invention, and the hardenability may increase excessively, resulting in the occurrence of a large amount of light low-temperature transformation structures. On the other hand, if the C content is less than 0.2%, it is difficult to ensure sufficient strength after the heat treatments of quenching and tempering performed after the softening heat treatment and forging process due to the decrease in strength of the base metal. Therefore, the C content is preferably in the range of 0.2 to 0.45%. The lower limit of the C content is more preferably 0.22%, even more preferably 0.24%, and most preferably 0.26%. The upper limit of the C content is more preferably 0.43%, even more preferably 0.41%, and most preferably 0.39%.
[0012] Silicon: 0.02 to 0.4% Si is a typical substitutional element, and is added to ensure a certain level of strength. If the Si content is less than 0.02%, it is difficult to ensure the strength of the steel and sufficient hardenability, and if it exceeds 0.4%, there is a drawback in that the cold forgeability during forging after softening heat treatment is deteriorated. Therefore, the Si content is preferably in the range of 0.02 to 0.4%. The lower limit of the Si content is more preferably 0.022%, further preferably 0.024%, and most preferably 0.026%. The upper limit of the Si content is more preferably 0.038%, further preferably 0.036%, and most preferably 0.034%.
[0013] Mn: 0.3 to 1.5% Mn is an element that forms a substitutional solid solution in the matrix structure, lowers the A1 temperature, refines the spacing between pearlite layers, and increases the subgrains in the ferrite structure. If the Mn content exceeds 1.5%, it will have a detrimental effect due to the heterogeneity of the structure caused by manganese segregation. Although macrosegregation and microsegregation are likely to occur due to the segregation mechanism during the solidification of steel, Mn promotes the segregation zone due to its relatively low diffusion coefficient compared to other elements, and the improvement in hardening ability due to this is the main cause of the formation of a low-temperature structure such as martensite in the center. On the other hand, if the Mn content is less than 0.3%, it is difficult to ensure sufficient hardenability to ensure a martensite structure after the heat treatment for quenching and tempering performed after the softening heat treatment and the forging process. Therefore, the Mn content is preferably in the range of 0.3 to 1.5%. The lower limit of the Mn content is more preferably 0.4%, even more preferably 0.5%, and most preferably 0.6%. The upper limit of the Mn content is more preferably 1.4%, further preferably 1.3%, and most preferably 1.2%.
[0014] Cr: 0.3~1.5% Cr is mainly used as an element to improve the hardenability of steel, similar to Mn. If the Cr content is less than 0.3%, it is difficult to ensure sufficient hardenability to obtain martensite during the heat treatments of quenching and tempering performed after the softening heat treatment and forging process, and if it exceeds 1.5%, there is a high possibility that a large amount of low-temperature structure will be generated in the wire rod due to promotion of center segregation. Therefore, the Cr content is preferably in the range of 0.3 to 1.5%. The lower limit of the Cr content is more preferably 0.4%, even more preferably 0.5%, and most preferably 0.6%. The upper limit of the Cr content is more preferably 1.4%, even more preferably 1.3%, and most preferably 1.2%.
[0015] Al: 0.02 to 0.05% Al is an element that not only has a deoxidizing effect, but also precipitates Al-based carbonitrides, which helps to suppress the growth of austenite grains and ensure that the proeutectoid ferrite fraction is close to the equilibrium phase. If Al is less than 0.02%, the deoxidizing effect is insufficient, and if it exceeds 0.05%, hard inclusions such as Al2O3 may increase, and in particular, nozzle clogging due to the inclusions during continuous casting may occur. Therefore, the Al content is preferably in the range of 0.02 to 0.05%. The lower limit of the Al content is more preferably 0.022%, even more preferably 0.024%, and most preferably 0.026%. The upper limit of the Al content is more preferably 0.048%, even more preferably 0.046%, and most preferably 0.044%.
[0016] Mo: 0.01 to 0.5% Mo not only precipitates Mo-based carbonitrides, inhibits the growth of austenite grains, and helps promote the formation of proeutectoid ferrite during cooling, but also forms Mo2C precipitates during tempering, which is one of the heat treatments for quenching and tempering performed after the softening heat treatment and forging process, and is an element that is effective in inhibiting strength reduction (temper softening). If Mo is less than 0.01%, it is difficult to have a sufficient effect of inhibiting strength reduction, and if it exceeds 0.5%, a large amount of low-temperature structure may be generated in the wire rod, which may result in additional heat treatment costs for removing the low-temperature structure. Therefore, Mo is preferably in the range of 0.01 to 0.5%. The lower limit of the Mo content is more preferably 0.012%, even more preferably 0.013%, and most preferably 0.014. The upper limit of the Mo content is more preferably 0.49%, even more preferably 0.48%, and most preferably 0.47%.
[0017] N: 0.01% or less N is an impurity element, and if it exceeds 0.01%, the material toughness and ductility may be reduced due to the dissolved nitrogen that is not bound to the precipitates. Therefore, the N content is preferably in the range of 0.01% or less. stomach.
[0018] The remaining component of the present invention is iron (Fe). However, in a normal manufacturing process, unintended impurities may be inevitably mixed in from the raw materials or the surrounding environment, and it is not possible to exclude them. Since these impurities are known to anyone skilled in the normal manufacturing process, the contents of all of them are not specifically described in this specification.
[0019] The wire rod of the present invention preferably has a microstructure in which, in area %, the pro-eutectoid ferrite fraction is 40% or more of the equilibrium phase, the regenerated pearlite and bainite fraction is 40% or more, and the martensite fraction is 20% or less. As a soft phase, pro-eutectoid ferrite exerts a major effect on the strength reduction of the material. When the pro-eutectoid ferrite fraction is less than 40% of the equilibrium phase, a relatively large amount of hard phase is formed, and it may be difficult to effectively ensure spheroidizing heat treatability. On the other hand, the pro-eutectoid ferrite fraction is preferably 80% or less of the equilibrium phase, and when it exceeds 80%, a very slow cooling rate is required, which may cause a decrease in productivity. The equilibrium phase of pro-eutectoid ferrite means the maximum fraction of pro-eutectoid ferrite that can be held in a stable state on the Fe3C phase diagram. The equilibrium phase of pro-eutectoid ferrite can be easily derived by a person having ordinary knowledge in the technical field by considering the C content and the contents of other alloy elements from the Fe3C phase diagram. Regenerated pearlite and bainite are composed of ferrite and cementite phases, and regenerated pearlite means a structure having high dislocation density and segmented cementite due to rolling or wire drawing. That is, unlike the plate-like cementite generally present in pearlite structures, regenerated pearlite is discontinuous and segmented cementite is distributed, so that it has the effect of spheroidization at a high speed during spheroidization soft heat treatment. For this effect, it is preferable that the fraction of regenerated pearlite and bainite is 40% or more. On the other hand, it is preferable that the fraction of regenerated pearlite and bainite is 80% or less, and if it exceeds 80%, there is a disadvantage that the spheroidized carbides are fined and sufficient strength reduction does not occur. Martensite, as a hard phase, has the effect of forming spheroidized carbides quickly in a short time. However, if the martensite fraction exceeds 20%, there is a disadvantage that the effect of increasing strength occurs due to fine carbides. On the other hand, the martensite fraction is preferably 3% or more. If it is less than 3%, there is a drawback that the number of spheroidized carbide seeds decreases in the initial stage of heat treatment, delaying spheroidization.
[0020] In the wire rod of the present invention, the average size of pearlite colonies in the region between 2 / 5 and 3 / 5 of the diameter is preferably 5 μm or less. By finely controlling the average size of pearlite colonies in this manner, the segmentation effect of cementite can be improved, and the spheroidization rate of cementite during spheroidizing heat treatment can be increased.
[0021] The average size of the pro-eutectoid ferrite grains in the region between 2 / 5 and 3 / 5 of the diameter is preferably 7 μm or less. By finely controlling the average size of the ferrite grains in this manner, the size of the pearlite colonies can also be refined, and this can increase the spheroidization rate of cementite during spheroidizing heat treatment.
[0022] In addition, the average size of the major axis of the cementite in the pearlite colony is preferably 5 μm or less. By controlling the average size of the major axis of the cementite in the pearlite colony to be small in this manner, that is, by controlling the aspect ratio of the cementite to be small, the spheroidization rate of the cementite can be increased during the spheroidizing heat treatment.
[0023] Meanwhile, in the present invention, the average size of the pearlite colonies, the average size of the proeutectoid ferrite grains, and the average size of the major axis of the cementite in the pearlite colonies may be those in the reference center of the diameter of the wire rod, for example, in the region from 2 / 5 to 3 / 5 points from the surface based on the diameter. Usually, the surface layer of the wire rod is subjected to a strong rolling force during rolling, so that the average size of the pearlite colonies in the surface layer, the average size of the proeutectoid ferrite grains, and the average size of the major axis of the cementite in the pearlite colonies can be fine. However, in the present invention, the average size of the pearlite colonies and the average size of the ferrite grains are refined not only in the surface layer of the wire rod but also in the center, thereby effectively increasing the spheroidization rate of the cementite during spheroidization heat treatment.
[0024] For example, in the wire of the present invention, the deviation between the average size of the pro-eutectoid ferrite grains in the region from the surface to 1 / 5 of the diameter and the average size of the pro-eutectoid ferrite grains in the region from the surface to 2 / 5 to 3 / 5 of the diameter is 6 μm or less.
[0025] The wire rod of the present invention has a tensile strength (TS) of 579+864×([C]+[Si] / 8+[Mn] / 18) MPa or more. According to the present invention, the strength of the steel is increased due to fine ferrite grains, despite the high ferrite phase fraction. The tensile strength of the wire rod of the present invention has the following relationship: The fact that the wire rod has such a strength despite the ferrite fraction of the present invention means that the ferrite grains of the steel are very fine, and the refinement of the grains of the steel can be confirmed by a tensile test performed on-site without a separate observation of the microstructure. The wire rod of the present invention has such a tensile strength, which not only makes it easy to ensure the strength of the wire rod itself, but also makes it possible to omit or shorten the softening heat treatment process during the subsequent softening heat treatment.
[0026] Usually, to manufacture a wire rod from a steel wire, the steps are a primary softening heat treatment, a primary wiredrawing process, a secondary softening heat treatment, and a secondary wiredrawing process. However, the wire rod of the present invention can omit the steps corresponding to the primary softening heat treatment and the primary wiredrawing process due to the sufficient softening of the material. On the other hand, the softening heat treatment referred to in the present invention includes a low-temperature annealing heat treatment performed below the Ae1 phase transformation point, a medium-temperature annealing heat treatment performed near Ae1, and a spheroidizing annealing heat treatment performed above Ae1.
[0027] In addition, the wire rod of the present invention has an average aspect ratio of cementite after one spheroidizing annealing heat treatment of 2.5 or less. It is generally known that the more times the spheroidizing annealing heat treatment is performed, the more effective it is in spheroidizing cementite. However, in the present invention, cementite can be sufficiently spheroidized by only one spheroidizing annealing heat treatment. Meanwhile, as described above, the surface layer of the wire rod is subjected to a strong rolling force during rolling, so that cementite is smoothly spheroidized. However, in the present invention, cementite can also be sufficiently spheroidized in the reference center of the diameter of the wire rod, for example, in the region from 1 / 4 point to 1 / 2 point from the surface based on the diameter, and the average aspect ratio of cementite in the center of the wire rod is 2.5 or less. Furthermore, the wire rod of the present invention has a tensile strength of 540 MPa or less after one spheroidizing heat treatment. This makes it possible to easily perform cold heading or cold forging for manufacturing the final product.
[0028] The method for producing a wire rod according to the present invention, which allows omitting the softening heat treatment, will now be described.
[0029] First, a billet having the above-mentioned alloy composition is heated at 950 to 1050° C. If the billet heating temperature is less than 950° C., rollability decreases, and if the billet heating temperature exceeds 1050° C., rapid cooling is required for rolling, making it difficult to control cooling and also difficult to ensure good product quality due to the occurrence of cracks.
[0030] The heating time is preferably 90 minutes or less. If the heating time exceeds 90 minutes, the depth of the surface decarburized layer becomes large and the decarburized layer may remain after the rolling is completed.
[0031] The heated billet is then subjected to a second hot rolling to obtain a wire rod. The second hot rolling is preferably a groove rolling to make the billet have the shape of a wire rod. The second hot rolling may include a step of intermediate finish rolling the heated billet and a step of finish rolling at 730°C to Ae3 at or above the critical deformation amount represented by Equation 1. [Formula 1] Critical deformation amount = -2.46Ceq2 +3.11Ceq-0.39 (where Ceq=C+Mn / 6+Cr / 5, and C, Mn, and Cr are in weight percent)
[0032] The wire rod rolling speed is very fast and belongs to the dynamic recrystallization region. According to the results of research to date, it has become clear that under the conditions of dynamic recrystallization, the size of the austenite grains depends only on the deformation speed and deformation temperature. Due to the characteristics of wire rod rolling, the deformation amount and deformation speed are determined when the wire diameter is determined, and the size of the austenite grains can be changed by adjusting the deformation temperature. In the present invention, the dynamic deformation organic transformation phenomenon of dynamic recrystallization is used to refine the grains. In order to secure the ferrite grains that the present invention aims to obtain by using this phenomenon, it is preferable to control the finish rolling temperature to 730 ° C to Ae3. If the finish rolling temperature exceeds Ae3, it is difficult to obtain the ferrite grains that the present invention aims to obtain, and it is difficult to obtain sufficient spheroidizing heat treatability, and if it is less than 730 ° C, the load on the equipment increases, and the life of the equipment may be rapidly reduced.
[0033] When finish rolling is performed below the critical deformation amount represented by Equation 1, the reduction amount is insufficient, making it difficult to sufficiently refine the average aspect ratio of cementite and the average size of ferrite crystal grains in the center of the wire rod, and as a result, there is a risk that the spheroidizing heat treatability of the obtained wire rod will be reduced.
[0034] At this time, the average surface temperature of the wire before finish rolling (T pf ) and the average surface temperature of the wire after finish rolling (T f ) preferably satisfies formula 2. The average surface temperature of the wire rod before finish rolling (T pf ) and the average surface temperature of the wire after finish rolling (T f ) does not satisfy formula 2, the deviation of the microstructure becomes very large, and the surface supercooling becomes large, which may result in the formation of a large amount of hard phase. [Formula 2]T pf -T f ≦50℃
[0035] On the other hand, the average size of the austenite grains of the wire rod after the intermediate finish rolling is preferably 5 to 20 μm. It is known that ferrite grows by nucleating from the austenite grain boundaries. If the austenite grains of the parent phase are fine, the ferrite nucleated from the grain boundaries can also start to form finely, so that the effect of ferrite grain refinement can be obtained by controlling the average size of the austenite grains of the wire rod after the intermediate finish rolling. If the average size of the austenite grains exceeds 20 μm, it is difficult to obtain the effect of ferrite grain refinement, and there is a disadvantage that in order to obtain an average size of the austenite grains of less than 5 μm, a separate facility that further applies a high deformation amount such as under heavy pressure is required.
[0036] Thereafter, the wound wire is cooled to 600°C at a cooling rate of 2°C / sec or less, and then cooled at a cooling rate of 3°C / sec or more. If the cooling rate to 600°C exceeds 2°C / sec, a large amount of hard phase such as martensite may be generated. Therefore, the cooling rate to 600°C is more preferably 0.5 to 2°C / sec from the viewpoint of fine ferrite grains. In the temperature range below 600°C, it is preferable to perform quenching at a cooling rate of 3°C / sec or more. In this way, by quenching, the regenerated pearlite and bainite, which are semi-hard phases, and the martensite structure, which is a hard phase, can be secured in the appropriate fraction that the present invention aims to obtain, and the growth of plate-shaped cementite, which is disadvantageous to spheroidizing heat treatment, can be suppressed.
[0037] Next, the wire is wound to produce a wire.
[0038] The average surface temperature of the wire after finish rolling (T f ) and coiling temperature (T l ) preferably satisfies formula 3. The average surface temperature of the wire rod after finish rolling (T f ) and coiling temperature (T l ) does not satisfy formula 3, the deviation of the microstructure becomes very large, and the surface becomes supercooled, which may result in the formation of a large amount of hard phase. [Formula 3]T f -Tl ≦30℃
[0039] In the present invention, after winding, the wire rod is heated to Ae1 to Ae1+40°C, maintained for 10 to 15 hours, and then cooled to 660°C at 20°C / hr or less for spheroidizing heat treatment. If the heating temperature is less than Ae1, the spheroidizing heat treatment time may be long, and if it exceeds Ae1+40°C, the seeds of spheroidized carbide may be reduced, and the effect of the spheroidizing heat treatment may be insufficient. If the maintenance time is less than 10 hours, the spheroidizing heat treatment may not be sufficient, and the aspect ratio of cementite may be large, and if it exceeds 15 hours, the cost may be increased. If the cooling rate exceeds 20°C / hr, there may be a drawback that pearlite is formed again due to the high cooling rate. Meanwhile, as described above, in the present invention, sufficient spheroidizing heat treatability can be ensured even if only the spheroidizing heat treatment is performed without the first softening heat treatment and the first wire drawing. EXAMPLES
[0040] The present invention will be described in more detail below with reference to examples. However, it should be noted that the following examples are merely intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention, since the scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.
[0041] (Example) A billet having the alloy composition of Table 1 was prepared, and then a wire having a diameter of 10 mm was manufactured using the conditions shown in Tables 2 and 3. The microstructure, average size of pro-eutectoid ferrite grains, average size of pearlite colonies, average size of cementite major axis in pearlite colonies, deviation of average size of pro-eutectoid ferrite grains between the surface layer and the center, and tensile strength of the thus manufactured wire were measured, and the results are shown in Table 3. In addition, the wire was subjected to a single spheroidizing heat treatment under the conditions of Table 4, and then the average aspect ratio of cementite and tensile strength were measured, and the results are shown in Table 4. The spheroidizing heat treatment was performed on the manufactured wire test piece without performing a first softening treatment and a first wiredrawing process.
[0042] The average austenite grain size (AGS) was measured via a crop performed before finish hot rolling.
[0043] Ae1 and Ae3 are values calculated using the commonly used program JmatPro.
[0044] The mean grain size (FGS) of pro-eutectoid ferrite was measured by removing the uncooled areas after wire rolling using the ASTM E112 method, and measurements were taken at three arbitrary points in the region between 2 / 5 and 3 / 5 of the diameter of the sampled specimen, and the FGS was expressed as the average value.
[0045] The average size of pearlite colonies was determined by using the ASTM E112 method, randomly selecting 10 pearlite colonies at the same location as the FGS measurement, calculating the value of (long axis + shortening) / 2 for each colony, and then averaging the measured colony sizes.
[0046] The deviation in the average size of the pro-eutectoid ferrite grains at the surface and the center was calculated by measuring the average size of the pro-eutectoid ferrite grains in the region from the surface to 1 / 5 of the diameter and the average size of the pro-eutectoid ferrite grains in the region from 2 / 5 to 3 / 5 of the diameter using the ASTM E112 method.
[0047] The average aspect ratio of cementite after spheroidizing heat treatment was measured by photographing three fields of view at 1 / 4 to 1 / 2 points in the diameter direction of the wire rod using a SEM at 2000x (magnification), and the major axis / minus of cementite within the field of view was automatically measured using an image measurement program, and then statistical processing was performed.
[0048] [Table 1]
[0049] [Table 2]
[0050] [Table 3]
[0051] [Table 4]
[0052] As can be seen from Tables 1 to 4, in the case of Examples 1 to 5 which satisfy the alloy composition and manufacturing conditions proposed by the present invention, by securing not only the type and fraction of the microstructure of the present invention but also fine crystal grains, it is possible to obtain an average aspect ratio of cementite of 2.5 or less even with only one spheroidizing heat treatment.
[0053] However, in the case of Comparative Examples 1 to 4, which do not satisfy the alloy composition or manufacturing conditions proposed by the present invention, the type and fraction of the microstructure of the present invention are not satisfied, or fine crystal grains cannot be secured, so that the average aspect ratio of cementite after one spheroidizing heat treatment is at a high level. As a result, it can be confirmed that further spheroidizing heat treatment is necessary for application to the final product.
[0054] Fig. 1 is a photograph of the microstructure of Comparative Example 1 before finish hot rolling observed with an optical microscope, and Fig. 2 is a photograph of the microstructure of Invention Example 1 before finish hot rolling observed with an optical microscope. As can be seen from Figs. 1 and 2, Invention Example 1 has a relatively fine AGS before finish hot rolling compared to Comparative Example 1.
[0055] Fig. 3 is a photograph of the microstructure after rolling and cooling of Comparative Example 1, where (a) is a photograph observed with an optical microscope and (b) is a photograph observed with an SEM, and Fig. 4 is a photograph of the microstructure after rolling and cooling of Invention Example 1, where (a) is a photograph observed with an optical microscope and (b) is a photograph observed with an SEM. As can be seen from Figs. 3 and 4, the microstructure of Invention Example 1 after rolling and cooling is refined compared to Comparative Example 1, and it can be confirmed that the cementite is segmented.
[0056] Fig. 5 is a SEM photograph of the microstructure after spheroidizing heat treatment of Comparative Example 1, and Fig. 6 is a SEM photograph of the microstructure after spheroidizing heat treatment of Invention Example 1. As can be seen from Figs. 5 and 6, it can be confirmed that the microstructure after spheroidizing heat treatment of Invention Example 1 is more spheroidized than that of Comparative Example 1.
Claims
1. A wire rod capable of omitting a softening heat treatment, the wire rod comprising, by weight %, 0.2-0.45% C, 0.02-0.4% Si, 0.3-1.5% Mn, 0.3-1.5% Cr, 0.02-0.05% Al, 0.01-0.5% Mo, 0.01% or less N, with the balance being Fe and other unavoidable impurities, the wire rod having a microstructure in which, by area %, the pro-eutectoid ferrite fraction is 40% or more of the equilibrium phase, the regenerated pearlite and bainite fractions are 40% or more, and the martensite fraction is 20% or less, the average size of pearlite colonies in a region from the surface to 2 / 5 points to 3 / 5 points of the diameter is 5 μm or less.
2. 2. The wire according to claim 1, wherein the wire has an average size of pro-eutectoid ferrite grains of 7 μm or less in a region from the surface to the 2 / 5 point to the 3 / 5 point of the diameter.
3. 2. The wire rod according to claim 1, wherein the average major axis size of cementite in the pearlite colonies is 5 μm or less.
4. 2. The wire according to claim 1, wherein the wire has a deviation of 6 μm or less between an average size of pro-eutectoid ferrite grains in a region from the surface to a point 1 / 5 of the diameter and an average size of pro-eutectoid ferrite grains in a region from the surface to a point 2 / 5 to 3 / 5 of the diameter.
5. 2. The wire according to claim 1, wherein the wire has a tensile strength (TS) of 579 + 864 × ([C] + [Si] / 8 + [Mn] / 18) MPa or more, and the softening heat treatment can be omitted.
6. 2. The wire rod according to claim 1, wherein when the wire rod is subjected to a single spheroidizing heat treatment at Ae1 or more, the wire rod subjected to the single spheroidizing heat treatment has an average aspect ratio of cementite of 2.5 or less.
7. 2. The wire rod according to claim 1, wherein the wire rod subjected to a single spheroidizing heat treatment at Ae1 or more has a tensile strength of 540 MPa or less.
8. heating a billet consisting of, by weight percent, 0.2-0.45% C, 0.02-0.4% Si, 0.3-1.5% Mn, 0.3-1.5% Cr, 0.02-0.05% Al, 0.01-0.5% Mo, 0.01% or less N, and the balance being Fe and other unavoidable impurities, at 950-1050°C; a second hot rolling step for obtaining a wire rod from the heated billet; winding the wire; and cooling the wound wire to 600° C. at a cooling rate of 2° C. / sec or less, and then cooling the wound wire at a cooling rate of 3° C. / sec or more; 2. The method of claim 1, wherein the second hot rolling includes the steps of intermediate finish rolling the heated billet, and finish rolling the heated billet at a temperature of 730° C. to Ae3 at a critical deformation amount or more represented by Equation 1. [Formula 1] Critical deformation amount = -2.46Ceq2 + 3.11Ceq - 0.39 (where Ceq = C + Mn / 6 + Cr / 5, and C, Mn, and Cr are in weight percent)
9. 9. The method for producing wire according to claim 8, wherein the heating time is 90 minutes or less.
10. 9. The method for producing a wire rod according to claim 8, wherein the wire rod after the intermediate finish rolling has an average austenite grain size of 5 to 20 μm.
11. The average surface temperature of the wire before the finish rolling (T pf ) and the average surface temperature of the wire rod after the finish rolling (T f 9. The method for producing a wire according to claim 8, wherein the formula 2 is satisfied. [Formula 2] T pf -T f ≦50℃
12. The average surface temperature of the wire rod after the finish rolling (T f ) and winding temperature (T l 9. The method for producing a wire according to claim 8, wherein: [Formula 3] T f -T l ≦30℃
13. The method for producing a wire according to claim 8, further comprising a spheroidizing annealing heat treatment in which the wire after cooling at the cooling rate of 3°C / sec or more is heated to Ae1 to Ae1+40°C, maintained at that temperature for 10 to 15 hours, and then cooled to 660°C at a rate of 20°C / hr or less.
Citation Information
Patent Citations
Hot rolled wire rod-bar steel for machine structure and production thereof