Hierarchical and nanoporous metal composites in porous polymer matrices

A composite material with a porous polymeric substrate and nanoporous metal addresses mechanical and manufacturing limitations of traditional nanoporous metals, enhancing durability and electrochemical performance for biosensors.

JP7576188B2Active Publication Date: 2024-10-30WL GORE & ASSOC INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023564162
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-04-01
Filing Date
2022-04-14
Publication Date
2024-10-30
Estimated Expiration
2042-04-14

AI Technical Summary

Technical Problem

Nanoporous metals face limitations in mechanical properties, manufacturing processes, and pore size that hinder large-scale commercialization, including brittleness, cumbersome manufacturing methods using hazardous chemicals, and restricted mass transfer and tissue ingrowth.

Method used

A composite material comprising a porous polymeric substrate with a nanoporous metal within, featuring a hierarchical structure and a unimodal, right-skewed nanopore size distribution, which enhances mechanical strength, supports tissue integration, and allows for additive manufacturing without a carrier film.

Benefits of technology

The composite material improves mechanical durability, supports tissue ingrowth, and maintains electrochemical performance across varying biological fluids, enabling broader applications such as electrochemical analyte biosensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576188000015
    Figure 0007576188000015
  • Figure 0007576188000016
    Figure 0007576188000016
  • Figure 0007576188000017
    Figure 0007576188000017
Patent Text Reader

Abstract

A composite material is disclosed that includes a porous polymer substrate and a nanoporous metal present within the porous polymer substrate. The nanoporous metal may have a hierarchical structure. The nanoporous metal may have a unimodal and right-skewed number-based nanopore size distribution. The porous polymer substrate may support tissue integration and / or tissue ingrowth in certain applications. The composite material may be used in electrochemical analyte biosensors and other applications.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of Provisional Application No. 63 / 176,669, filed April 19, 2021, and the benefit of Provisional Application No. 63 / 326,593, filed April 1, 2022, which are incorporated by reference in their entireties for all purposes.

[0002] The present disclosure relates generally to composite materials comprising hierarchical and nanoporous metallic phases within porous polymeric substrates (matrix or base materials), and related methods of making and using such materials. [Background technology]

[0003] Nanoporous metals have been widely investigated for a wide range of applications, including enzyme-based biosensors and biofuel cells. Such interest is driven by a combination of properties including electrical conductivity, high metal surface area, and nanoscale pores. Taken together, these properties could make nanoporous metals superior when converted into electrodes in laboratory-scale bench-top or in vivo studies. These electrodes exhibit very high electrochemical surface areas compared to metal foils, and also higher signal responses (e.g., for sensors) or higher current densities normalized to geometric area (e.g., for biofuel cells). They have also shown greater retention of electrochemical signals in the presence of biofouling agents, such as albumin and fibrinogen. This phenomenon is commonly referred to as "biofouling resistance" and is attributed to the size exclusion of biofouling materials by nanoscale pores. However, despite intense interest and over a decade of development, nanoporous metals still exhibit limitations that prevent large-scale commercialization.

[0004] The first limitation of traditional nanoporous metals is their relatively poor mechanical properties. Nanoporous metals are brittle and prone to tearing, which makes them difficult to handle and process. These brittleness also raises concerns about the long-term durability of the target application. These mechanical properties can limit how thin these materials can be made (typically around 100 μm) before they must be placed on a carrier film, such as polyethylene terephthalate (PET). The use of these carrier films is often undesirable because they block mass transfer to and from one side of the nanoporous metal. The carrier film can also cause stability issues in the target application, particularly in vivo applications or applications that require exposure to high temperatures or difficult chemical environments.

[0005] A second limitation of traditional nanoporous metals is the cumbersome and wasteful process by which they are typically manufactured. The standard process involves dealloying the metal foil, which typically involves the use of hazardous chemicals, such as strong mineral acids. This is essentially a subtractive process and therefore wasteful. Dealloying also results in significant volumetric shrinkage of the foil. Volumetric shrinkage makes it difficult to use the foil with multilayer composites, as this increases interfacial stresses that can lead to delamination and / or bowing. Furthermore, cutting the foil to produce the complex shapes often desired in applications such as sensors is also a subtractive process and therefore wasteful.

[0006] A final limitation of traditional nanoporous metals is the pore size of the nanopores themselves, which, while advantageous in some contexts, can be quite limiting in others. For example, mass transport into the nanoscale pores can be significantly restricted, making it difficult to access the internal surface area for active sites for electrochemical reactions. As another example, nanoscale pores are typically too small to allow tissue ingrowth and vascularization, which can be desirable in some in vivo applications. Summary of the Invention [Means for solving the problem]

[0007] The present disclosure provides a composite material including a porous polymer substrate and a nanoporous metal present within the porous polymer substrate. The nanoporous metal may have a hierarchical structure. The nanoporous metal may have a number-based nanopore size distribution that is unimodal and right-skewed. The porous polymer substrate may support tissue integration and / or tissue ingrowth in certain applications. The composite material may be used in electrochemical analyte biosensors and other applications. The present disclosure addresses one or more of the limitations of traditional nanoporous metals using porous polymer substrates.

[0008] According to an exemplary embodiment of the present disclosure, a composite material is disclosed that includes a porous polymeric substrate and a nanoporous metal present within the porous polymeric substrate and comprising a number-based nanopore size distribution and a volume-based nanopore size distribution, wherein an average of the volume-based pore size distribution is at least 200% greater than an average of the number-based nanopore size distribution.

[0009] According to another exemplary embodiment of the present disclosure, a composite material is disclosed that includes a microporous polymer substrate comprising a plurality of interconnected micropores, and a nanoporous metal at least partially contained within the micropores of the microporous polymer substrate and separated from the microporous polymer substrate so as to define a gap.

[0010] According to yet another exemplary embodiment of the present disclosure, a composite material is disclosed that includes a first continuous network comprising a microporous polymer having a plurality of interconnected micropores and a second substantially continuous network comprising a nanoporous metal, the second substantially continuous network interpenetrating the first continuous network, the composite material having a porosity of at least 30 vol.%. [Brief description of the drawings]

[0011] The accompanying drawings are included to provide a further understanding of the disclosure, and are incorporated in and constitute a part of this specification, illustrating embodiments and, together with the description, serving to explain the principles of the disclosure.

[0012] [Figure 1] FIG. 1 is a cross-sectional view showing a composite material of the present disclosure.

[0013] [Diagram 2] FIG. 2 is a schematic diagram showing the apparatus used to measure the sheet resistance of the samples.

[0014] [Figure 3A] FIG. 3A is a scanning electron micrograph (SEM) image showing the microarchitecture of the nanoporous gold (NPG) / expanded polytetrafluoroethylene (ePTFE) composite of Example 1. [Figure 3B] FIG. 3B is a scanning electron micrograph (SEM) image showing the microarchitecture of the nanoporous gold (NPG) / expanded polytetrafluoroethylene (ePTFE) composite of Example 1. [Figure 3C] FIG. 3C is a scanning electron micrograph (SEM) image showing the microarchitecture of the nanoporous gold (NPG) / expanded polytetrafluoroethylene (ePTFE) composite of Example 1.

[0015] [Figure 4A]FIG. 4A is another cross-sectional SEM image showing the NPG / ePTFE composite of Example 1. [Figure 4B] FIG. 4B is the same image processed for nanopore size analysis. [Figure 4C] FIG. 4C is the same image once the nanopores have been separated.

[0016] [Diagram 5] FIG. 5 is a histogram showing the nanopore size distribution within the metal phase of the NPG / ePTFE composite of Example 1.

[0017] [Figure 6] FIG. 6 is a histogram showing the ratio of minor axis to minimum Feret of pores within the metal phase of the NPG / ePTFE composite of Example 1.

[0018] [Figure 7] FIG. 7 is a histogram showing the ratio of the long axis to maximum Feret of pores within the metal phase of the NPG / ePTFE composite of Example 1.

[0019] [Figure 8A] FIG. 8A is a SEM image showing the microarchitecture of the conformal gold (CG) / ePTFE composite of Example 3. [Figure 8B] FIG. 8B is a SEM image showing the microarchitecture of the conformal gold (CG) / ePTFE composite of Example 3. [Figure 8C] FIG. 8C is an SEM image showing the microarchitecture of the conformal gold (CG) / ePTFE composite of Example 3. [Figure 8D] FIG. 8D is an SEM image showing the microarchitecture of the conformal gold (CG) / ePTFE composite of Example 3.

[0020] [Figure 9] FIG. 9 is a graph showing the cyclic voltammogram of the NPG / ePTFE working electrode / silver-imbibing-treated pseudo reference electrode of Example 6.

[0021] [Figure 10] 10A and 10B are graphs showing the glucose response of a GOx-based glucose sensor including the NPG / ePTFE material of Example 9.

[0022] [Figure 11] 11A and 11B are graphs showing the glucose response of a GOx-based glucose sensor including the CG / ePTFE material of Example 9.

[0023] [Figure 12] FIG. 12 is a graph showing the dependence of electrochemical surface area on electrolyte solvent surface tension for Example 10.

[0024] [Figure 13] FIG. 13 is a diagram showing a wet bending particulate durability test method. [Figure 14] FIG. 14 is a diagram showing a wet bending particulate durability test method. [Figure 15] FIG. 15 is a diagram showing a wet bending particulate durability test method.

[0025] [Figure 16] FIG. 16 is a graph showing the capillary flow polimetry data of Example 11.

[0026] [Figure 17] FIG. 17 is a schematic diagram showing the electrochemical cell configuration for electrochemical surface area (ECSA) testing.

[0027] [Figure 18] FIG. 18 includes cross-sectional SEM images showing the NPG / ePTFE composite of Example 1 compared to the dense silver / ePTFE (CPS / ePTFE) composite of Example 14 at 2000x magnification.

[0028] [Figure 19]FIG. 19 includes cross-sectional SEM images showing the NPG / ePTFE composite of Example 1 compared to the CPS / ePTFE composite of Example 14 at 20,000x magnification, and also shows the nanopore phase isolated from the corresponding images for nanopore size analysis.

[0029] [Figure 20] FIG. 20 includes histograms comparing the number-based and volume-based nanopore size distributions within the metal phase of the NPG / ePTFE composite of Example 1 and the CPS / ePTFE composite of Example 14. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] definition This disclosure is not intended to be read in a restrictive manner, for example, the terms used in this application should be read broadly in light of the meaning that one of ordinary skill in the art would ascribe to such terms.

[0031] With respect to terms expressing imprecision, the terms "about" and "approximately" may be used interchangeably to mean a measurement that includes the stated measurement and also includes any measurement that is substantially close to the stated measurement. A measurement that is substantially close to the stated measurement deviates from the stated measurement by a substantially small amount that can be understood and easily ascertained by one of ordinary skill in the art. Such deviations can be attributed, for example, to measurement errors, differences in measurement and / or manufacturing equipment calibration, human error in reading and / or setting measurements, performance and / or construction parameters that take into account differences in measurements relative to other components, fine-tuning made to optimize a particular implementation scenario, imprecise adjustment and / or manipulation of objects by humans or machines, and / or the like. In cases where it is determined that such substantially small differences are not readily ascertainable by one of ordinary skill in the art, the terms "about" and "approximately" may be understood to mean plus or minus 10% of the stated value.

[0032] "Tissue integration," as used herein, means exposing the device to the surrounding tissue while minimizing adverse reactions, such as inflammation and encapsulation, of the surrounding tissue that may impair the intended performance of the device over its intended period of use. Essentially, and without wishing to be bound by theory, the device reaches a biocompatible quiescent state within the surrounding tissue.

[0033] As used herein, the term "tissue ingrowth" refers to the growth of tissue, cells, capillaries, and / or other body components into the full or partial thickness of a porous material.

[0034] The term "microporous" as used herein means a material containing pores having a single pore size or a distribution of pore sizes. The average pore size may be from about 0.1 μm to about 50 μm. Of course, microporous materials may contain individual pores outside this average size range, including some macropores. Microporous materials may have a characteristic or nominal pore size, as characterized by bubble point analysis or another suitable test, as described below. The average pore size of a membrane may be characterized, for example, by the mean flow pore size determined by capillary flow porometry.

[0035] The term "nanoporous" as used herein refers to a material that contains pores having a single pore size or a distribution of pore sizes. The number-based average pore size may be from about 1 nm to about 500 nm. The distribution may include a plurality of pore clusters having different sizes ranging from about 1 nm diameter to about 10 nm, from about 10 nm to about 100 nm, or from about 100 nm to about 500 nm. Of course, nanoporous materials may contain individual pores outside these ranges, including some micropores. Pore size may be characterized by quantitative image analysis, as described below.

[0036] As used herein, the term "conformal" refers to a coating layer that coats the interior surface of an underlying porous substrate. In embodiments in which the coating layer comprises an electrically conductive material, the conformal coating can achieve electrical conductivity through and along the surface of the coating layer.

[0037] As used herein, the term "imbibed" refers to a material that is deposited within the pores of a porous substrate using a fluid carrier, but the material is not substantially incorporated into the matrix of the porous substrate, leaving the porous substrate substantially intact.

[0038] As used herein, the term "conductive" refers to a material that transports electrons with low resistance such that the electrical resistance of the material does not render it unsuitable for use in its intended application. In practice, this term typically refers to a material that transports electrons with low resistance such that the electrical resistance of the material does not render it unsuitable for use in its intended application. -3 It means resistivity in ohms x cm.

[0039] As used herein, "electrically non-conductive material" and "electrically insulating material" refer to materials that have a high resistivity such that the electrical conductivity of the material does not render it unsuitable for use in its intended application. In practice, this expression typically refers to a material that has a resistivity of about 1×10 8 It means a resistivity of over ohms x cm.

[0040] Detailed Description composite material Referring initially to Figure 1, an embodiment of a composite material 200 is shown that includes a porous polymer substrate 210 having a metal region 220. The metal region 220 may span a partial thickness of the porous polymer substrate 210, as shown in Figure 1, or may span the entire thickness of the porous polymer substrate 210. The metal region 220 may extend beyond the thickness of the porous polymer substrate 210 and into other layers. The metal region 220 includes a nanoporous metal 224 that is present within the porous polymer substrate 210. As discussed further below, the metal region 220 may provide electrical conductivity through the composite material 200.

[0041] The composite material 200 may be used for a wide range of applications, including, as an example, an electrochemical analyte biosensor. As described herein and demonstrated in the examples, the composite material 200 may have certain advantages over traditional nanoporous metals. First, the porous polymer substrate 210 may support or reinforce the nanoporous metal 224, thereby improving its mechanical properties without a traditional carrier film. Also, the porous polymer substrate 210 may facilitate additive manufacturing by serving as a scaffold. Furthermore, the porous polymer substrate 210 may have a controllable and larger average pore size than the nanoporous metal 224, such that the nanopores of the nanoporous metal 224 are substantially contained within the pores of the polymer substrate 210. These advantages may also aid in the broader application of the composite material 200.

[0042] The composite material 200 may include one or more hierarchical features. For example, the composite material 200 may have an interface region 217 distinct from the metal region 220 to protect the metal region 220 and allow for conditioning of the biological interface. In certain embodiments, the interface region 217 may be a unitary, integral, non-laminated portion of the porous polymer substrate 210. As another example, the composite material 200 may have a gap 226 between the nanoporous metal 224 and the porous polymer substrate 210 to promote tissue ingrowth and / or mass transport while maintaining electrical conductivity of the metal region 220. As yet another example, the metal region 220 of the composite material 200 may have a pore size distribution that includes small and large nanopores. Without wishing to be bound by theory, this mix of pore sizes may balance the surface area and mass transport of the composite material 200. These hierarchical features are described below.

[0043] The porosity of the composite material 200 may be at least 30 vol%, 40 vol%, 50 vol%, 60 vol%, 70 vol%, 80 vol%, or more. The polymer of the polymer substrate 210 may comprise less than 30 vol%, less than 20 vol%, or less than 10 vol% of the composite material 200. The metal of the metal regions 220 may comprise less than 40 vol%, less than 30 vol%, less than 20 vol%, or less than 10 vol% of the composite material 200. Despite its high porosity and low metal content, the composite material 200 may have good electrical conductivity.

[0044] Each element of composite material 200 is further described below.

[0045] Porous Polymer Substrate The porous polymer substrate 210 of the composite material 200 may be a biocompatible, flexible, chemically inert material. In certain embodiments, the porous polymer substrate 210 may comprise a fluoropolymer, such as expanded polytetrafluoroethylene (ePTFE), a polyolefin, such as expanded polyethylene (ePE), or another suitable polymer. The flexibility (or bending stiffness) of the porous polymer substrate 210 may be measured, for example, using a Kawabata Pure Bending Tester.

[0046] As shown in FIG. 1, the porous polymer substrate 210 has a first (i.e., upper in FIG. 1 ) surface 212, a second (i.e., lower in FIG. 1 ) surface 214, and a plurality of interconnected pores 216 between the first surface 212 and the second surface 214. The porous polymer substrate 210 may include one or more interface regions 217 at the first surface 212 and / or the second surface 214. The interface regions 217 may be different from the metal regions 220 and may not contain a conductive material (e.g., may not be metallized or may be bare). In certain applications where the composite material 200 is associated with a living organism, the interface regions 217 may serve as tissue interface regions. The tissue interface regions aid in the integration and / or ingrowth of tissue T (illustratively capillaries) through the first and / or second surfaces 212, 214 and into the pores 216. Such integration and / or ingrowth of tissue T may enhance the biocompatibility of the composite material 200 and minimize adverse reactions in the surrounding tissue, such as fibrous encapsulation or chronic inflammation. It is within the scope of the present disclosure for interface region 217 to include one or more bioactive agents to promote such integration and / or ingrowth of tissue T. The therapeutic agents may be physically bonded, covalently bonded, physisorbed, or chemisorbed to interface region 217 by means known to those skilled in the art. In other applications, interface region 217 may serve as a protective layer. The protective layer protects metal region 220 from damage (e.g., abrasion) or fouling. Interface region 217 may be an integral, non-laminated portion of porous polymer substrate 210.

[0047] The porous polymer substrate 210 may have a microstructure of nodes 218 with interconnected fibrils 219 that cooperate to define pores 216. The pores may include micropores as defined above. It is also within the scope of the present disclosure for the porous polymer substrate 210 to have a "nodeless" microstructure of interconnected fibrils 219 that cooperate to define pores 216. The fibrils 219 may vary in length from about 0.1 μm to about 1000 μm and in diameter from about 0.002 μm to about 100 μm, although these dimensions may vary widely. The porous polymer substrate 210 may have a characteristic or nominal pore size as measured using techniques known to those skilled in the art, such as the bubble point test method described below. Such techniques are based on the ability of the porous polymer substrate 210 to filter particles of a particular size or resist fluid flow, and not necessarily on the size or shape of the pores 216 themselves.

[0048] In certain embodiments, the porous polymeric substrate 210 may include a combination of both smaller pores 216 and larger pores 216. The larger pores 216 may be positioned outwardly near the first and / or second surfaces 212, 214 to encourage integration and / or ingrowth of tissue T, while the smaller pores 216 may be positioned inwardly near the center of the porous polymeric substrate 210, which may be adjacent to the metal region 220.

[0049] The porous polymeric substrate 210 itself may be hydrophobic or hydrophilic. In hydrophilic embodiments, the porous polymeric substrate 210 may tend to mix with or be wetted by water or other polar liquids, including polar biological fluids such as blood.

[0050] The porous polymer substrate 210 may be shaped and sized to reach the desired shape and dimensions of the composite material 200. For example, the porous polymer substrate 210 may be shaped as a membrane, film, fiber, tube, or another desired shape to produce a similarly shaped composite material 200. The porous polymer substrate 210 may also be bent, microwrinkled, stretched, rolled, folded, cut, or otherwise physically manipulated to reach the desired shape and compliance of the composite material 200 based on the surrounding environment. In certain embodiments, it may be desirable for the compliance of the porous polymer substrate 210 to match or approximate the compliance of the surrounding tissue.

[0051] metal area The metal region 220 includes a nanoporous metal 224 that is at least partially contained within the interconnected pores 216 of the porous polymer substrate 210 without being substantially incorporated into the matrix of the porous polymer substrate 210. In this arrangement, the nodes 218 and fibrils 219 of the porous polymer substrate 210 may define a first continuous network, and the metal region 220 may define a second, substantially continuous, conductive metal network that penetrates the polymer network. In this manner, the polymer network of the porous polymer substrate 210 and the metal network of the metal region 220 may be substantially co-continuous and interpenetrating at least within the metal region 220. In one example, the nanoporous metal 224 may be nanoporous gold (NPG). In other non-limiting examples, the nanoporous metal 224 is platinum, iridium, palladium, silver, copper, nickel, or combinations or alloys thereof.

[0052] The metal network may include hierarchical features. For example, unlike a conformal coating, the nanoporous metal 224 may be spaced from the porous polymer substrate 210 and may avoid significant contact with the porous polymer substrate 210, particularly the nodes 218 of the porous polymer substrate 210. These gaps 226 between the nanoporous metal 224 and the nodes 218 may be micropores. The micropores facilitate tissue ingrowth and / or mass transport through the porous polymer substrate 210 without disrupting the metal network of the metal regions 220 and while also maintaining mechanical reinforcement from the porous polymer substrate 210. Exposing these gaps 226 at the surface of the composite 200 (e.g., in the thickness or z-direction of FIG. 3B) may allow such tissue ingrowth while maintaining electrical conductivity (e.g., at least in the plane or xy-direction of FIG. 3B).

[0053] In another example of hierarchical features, the nanoporous metal 224 of the present disclosure may include a unimodal and right-skewed number-based nanopore size distribution in certain embodiments. In some typical preparations of nanoporous metals known to those skilled in the art, the number-based nanopore size distribution is unimodal and monodisperse, or in other words, the average nanopore size is approximately the modal nanopore size (e.g., A Pastre, "Porous Gold Films Fabricated by Wet-Chemistry Processes", J Nanomater, vol 2016, article ID 3536153, 2016). In other typical preparations of nanoporous metals known to those skilled in the art, the nanopore size distribution is multimodal and complex, i.e., there is more than one modal nanopore size (e.g., Y. Ding, “Nanoporous Metals with Controlled Multimodal Pore Size Distribution”, J Am Chem Soc, vol 125, p 7772, 2003). However, in embodiments of the present invention, the number-based nanopore size distribution of the nanoporous metal 224 is unimodal and right-skewed, i.e., the average number-based nanopore size is significantly larger (e.g., at least 75%, 100%, 125%, 150%, 175%, 200%, 225%, or 250% larger) than the unimodal number-based nanopore size, suggesting that a large number of nanopores are larger than a single mode and only a small number of nanopores are smaller than a single mode (see FIG. 5 and Examples 1 and 14 below). The unimodal and right-skewed number-based nanopore size distribution of the nanoporous metal 224 may provide benefits for performance in challenging environments, such as high surface tension liquid environments, biofouling environments, or tissue integration environments. For example, the nanopore size distribution may balance surface area and mass transport throughout the composite material 200.

[0054] A right-skewed number-based nanopore size distribution may be characterized by an average pore size significantly larger (eg, at least 10%, 20%, 30%, 40%, 50%, 60%, or 70% larger) than the median pore size.

[0055] The nanoporous metal 224 of the present invention may include a volume-based pore size distribution whose mode is significantly larger (e.g., at least 200%, 500%, 1000%, 1500%, 2000%, 2500%, 3000%, 3500%, or 4000% larger) than the mode of the number-based pore size distribution.

[0056] The nanoporous metal 224 of the present invention may include a volume-based pore size distribution whose average is significantly greater (e.g., at least 150%, 200%, 250%, 300%, 350%, 400%, 450%, 500%, 550%, or 600% greater) than the average of the number-based pore size distribution.

[0057] To load the porous polymer substrate 210 with the nanoporous metal 224, an imbibing process may be performed. This process may involve (1) preparing a non-aqueous wetting solution containing a metal precursor (e.g., a salt) in a non-aqueous solvent, (2) imbibing the porous polymer substrate 210 with the non-aqueous wetting solution, and (3) heating the imbibed structure to remove elements of the non-aqueous wetting solution, reduce the metal precursor to the metallic state, sinter the metal, and leave the nanoporous metal 224. The non-aqueous wetting solution may be tailored to sufficiently wet the porous polymer substrate 210. In the case of a hydrophobic ePTFE porous polymer substrate 210, for example, the non-aqueous wetting solution may include a wetting package consisting of a substantially water-insoluble alcohol and a surfactant, based on the teachings of U.S. Pat. No. 9,018,264. The heating step may involve heating the structure at one or more temperatures up to about 300° C. or higher for a suitable period of time up to several hours. In certain embodiments, the immersing process may be controlled such that the nanoporous metal 224 is deposited in a desired pattern within the porous polymer substrate 210. This desired pattern may be achieved by controlling the delivery of the metal precursor into the porous polymer substrate 210, by masking certain areas of the porous polymer substrate 210, as with inkjet printing or other printing means known to those skilled in the art or lithography, or by other suitable techniques.

[0058] Use as a working electrode in electrochemical analyte biosensors One potential application of the composite material 200 is as a working electrode in an electrochemical analyte biosensor. An electrochemical analyte biosensor converts an interaction between a bioreceptor (e.g., enzymes, aptamers, exomes, catalytic antibodies, catalytic ribonucleic acids, catalytic polysaccharides, and the like) and an analyte (e.g., glucose, lactate, pyruvate, glycerol, glutamate, glutamine, peptides, hormones, cardiac specific enzymes, opioids / anesthetics, and chemotherapeutic drugs) into an electrical signal, at least in part, via an electrochemical process, to generate a signal containing information about the analyte, e.g., its concentration. The composite material 200 may further include one or more diffusion barrier regions and one or more immobilized bioreceptor regions. In use, the nanoporous metal 224 of the metal region 220 may provide electrical conductivity through and along its surface. Thus, the metal region 220 may detect the target analyte and transmit a corresponding electrical signal to an electronic processor (not shown). Further details regarding the use of the composite material 200 in electrochemical analyte biosensor applications are disclosed in co-pending U.S. Patent No. 63 / 176,653 (applicant reference number 1862US01), filed on even date herewith.

[0059] The nanoporous metal 224 of the present disclosure may exhibit a consistent electrochemical surface area regardless of the surface tension of the surrounding biological fluid. For adequate functioning of an implanted biosensor, it is known to those skilled in the art that the entire surface of the electrode and the microstructure must be contacted and wetted by the biological fluid so that the entire electrode surface area can be active for analyte sensing. Since the ability of a liquid to wet a microstructure is related to its surface tension, fluids with high surface tension (greater than about 50 mN / m), such as saline (about 72 mN / m) and blood (about 50 mN / m), have a lower tendency to wet hydrophobic substrates. Conversely, fluids with low surface tension (less than about 30 mN / m), such as isopropanol (about 23 mN / m) and a 50:50 saline:isopropanol mixture (about 25 mN / m), have a higher tendency to wet hydrophobic substrates. Since the composite material 200 of the present disclosure may include a hydrophobic porous polymer substrate 210, such as ePTFE, contact or wetting by high surface tension biological fluids is expected to be reduced. This will also reduce the electrochemical surface area and / or analyte sensing activity of the metal regions 220. The presence of the imbibed nanoporous metal 224 within the pores 216 of the hydrophobic porous polymer substrate 210 is not expected to change the hydrophobicity of the composite material 200 because the hydrophobic porous polymer substrate 210 is present in excess, including along the first and second surfaces 212, 214. In other words, the composite material 200 including the imbibed hydrophobic porous polymer substrate 210 with the nanoporous metal 224 is expected to be hydrophobic itself, which will in turn reduce contact or wetting by high surface tension biological fluids. However, the inventors have surprisingly discovered that the electrochemical surface area of ​​the composite 200 having the immersed nanoporous metal 224 is not strongly dependent on wetting due to the surface tension of the liquid, thus enabling the composite 200 to function in low or high surface tension biological fluids. For example, the percent change in the electrochemical surface area of ​​the composite 200 having the immersed nanoporous metal 224 between low and high surface tension biological fluids may be about 50% or less, about 25% or less, or about 10% or less (see FIG. 12 and Example 10 below).This unexpected wetting behavior can be exploited to take advantage of the high surface area of ​​the imbibing nanoporous metal 224 .

[0060] As will be apparent to one of ordinary skill in the art, the various aspects of the disclosure may be implemented by any number of methods and devices configured to perform the intended functions. It should be noted that the accompanying drawings referred to herein are not necessarily drawn to scale and may be exaggerated to illustrate the various aspects of the disclosure. In that regard, the drawings should not be construed as limiting.

[0061] Test Method It will be appreciated that although certain particular methods and equipment are described below, other methods or equipment may alternatively be utilized as deemed suitable by those skilled in the art.

[0062] Non-contact thickness Non-contact thickness was measured using a laser micrometer (Keyence Model No. LS-7010, Mechelen, Belgium) using the following technique: A metal cylinder was aligned between the laser micrometer source and the laser micrometer receiver so that a first shadow of the top of the cylinder was projected onto the receiver. The location of the first shadow was then set as the "zero" reading on the laser micrometer. A single layer of the test article was then draped onto the surface of the metal cylinder with no overlap and no wrinkles. This projected a second shadow onto the receiver. The laser micrometer then indicated the change in position between the first and second shadows as the thickness of the sample. Each thickness was measured three times and averaged for each sample.

[0063] Mass per area The mass per area of ​​the samples was measured according to standard ASTM D 3776 (Standard Test Methods for Mass Per Unit Area (Weight) of Fabric, Test Method Option C).

[0064] Bubble point Bubble point pressure was measured using a Capillary Flow Porometer (Model 3Gzh, Quantachrome Instruments, Boynton Beach, Fla.) according to ASTM F31 6-03 and using Silwick silicone fluid (20.1 dynes / cm, Porous Materials Inc.) The value shown for bubble point pressure is the average of two measurements.

[0065] Sheet resistance A 2.125" x 0.5" specimen was die cut from the sheet of material under test. The specimen was laid flat on a closed cell silicone sponge sheet (1 / 2" thick, Bellofoam #7704). Resistance was measured with a Keithley 2750 Digital Multimeter utilizing the four-point probe shown in Figure 2. The four-point probe was connected to the multimeter in the standard four-point probe configuration (i.e., with the voltage sense leads on the innermost two terminals and the input leads on the outermost two terminals). After gently placing the four-point probe on the sample under test, a 330 gram weight was placed on top of the probe to ensure reliable and uniform contact of the probe with the sample. Care was taken to ensure adequate contact of the probe with the conductive phases of the sample. Insulating the weight with a plastic sheet ensured that it did not short out the probe. The Keithley multimeter was operated in the four-point probe mode with "OCOMP" 4-wire offset compensation enabled. For each measurement, the system was allowed to stabilize for approximately 10 seconds before the resistance value was recorded. Data was reported in units of ohms per square area.

[0066] Quantitative image analysis for measuring pore size inside metallic phases To collect images for pore size analysis, cross sections of each sample were prepared by a broad beam ion mill (Gatan, Illon 2, USA) to preserve their structure. A thin conductive platinum coating was deposited using a sputter coater (Cressington, 208HR, UK) to improve sample stability under the electron beam during SEM imaging. Cross-sectional images of the structures were taken at a magnification of 50,000X by scanning electron microscopy (Hitachi, Japan, SEM: SU8200) with a resolution of at least 2560 pixels x 1920 pixels (horizontal field width of 2.5 μm).

[0067] Analysis of pore size within the metallic phase was performed via quantitative analysis of cross-sectional SEM images using “Fiji” ImageJ 1.53 software. An automated macro, shown in Table 1 below, was used to minimize subjectivity and maximize reproducibility of data analysis. [Table 1-1] [Table 1-2] [Table 1-3] [Table 1-4] [Table 1-5] [Table 1-6] [Table 1-7]

[0068] First, the cross-sectional SEM images were preprocessed using the “Macro1_PreProcess” macro in Table 1 above to remove the grayscale variations caused by the conductive Pt coating.

[0069] The pre-processed images were then manually censored to eliminate all areas except those constituting the metallic phase and its embedded pores within the plane of the cross section. Manual censoring involved identifying visual cues such as surface texture and perspective. Manual censoring was performed with the assistance of the macros "Macro2_After_Segmenting_Support" and "Macro3_After_Segmenting_Void" in Table 1 above.

[0070] Finally, the pre-processed and manually censored images were analyzed using the “Macro4_Analysis” macro in Table 1 above. This macro identified individual pores by parsing the images. This involved further segmenting the complex pore space into individual pores separated by throats. This macro also performed the following analysis as of June 29, 2020: https: / / imagej.nih.gov / ij / docs / menus / analyze.html#set A data file was generated tabulating the various measurements for each individual pore according to the ImageJ documentation available at: http: / / imagej.stackexchange.com / articles / 20130233 / 11047. Specifically, the data file contained the pore size measurements shown in Table 2 below. [Table 2]

[0071] The pore size of an individual pore was defined as the average of the major and minor axes of the best-fit ellipse. To show the pore size distribution, the pore sizes of all pores in the data table were plotted as a histogram. A quality check was also performed to ensure that the pores were correctly analyzed. This quality check ensures that the pores were not underanalyzed (meaning that multiple connected pores were defined as a single pore) or overanalyzed (meaning that a single pore was further divided into multiple pores). The ratios of "major axis to Feret diameter" and "minor axis to minimum Feret diameter" were checked to ensure that these were within the range of 0.5 to 1.2. Such a range is close to 1 and confirms that the data has been quality checked. In this way, a processed image was generated for pore size analysis.

[0072] To determine the pore size distribution by number, a histogram was generated by the following procedure: The pores were bucketed into 3 nm wide groups between 0 nm and 1500 nm (i.e., group 1 included all pores >0 nm and <=3 nm, group 2 included all pores >3 nm and <=6 nm, and so on until the final group included all pores >1497 nm and <=1500 nm). The "pore size" of each group was the average of the pore size range rounded down to the nearest micron (i.e., group 1 was 1 nm, group 2 pores were 4 nm, and so on until the final group was 1498 nm in diameter). The frequency of pores in each group was determined by dividing the number of pores in that group by the total number of pores. To plot the pore size distribution by number, the frequency of pores in each group was assigned to the y-axis and the pore size of that group to the x-axis.

[0073] The number-based pore size distribution was then used to calculate the volume-based pore size distribution. To calculate the unit pore volume of each group, the number-based frequency of pores in each group was multiplied by the cubed "pore size" of that group. To calculate the pore volume percent of each group, the unit pore volume of each group was divided by the sum of the unit pore volumes across all groups. To plot the volume-based pore size distribution, the pore volume percent of each group was assigned to the y-axis and the pore size of that group to the x-axis.

[0074] The number-weighted mean pore size was calculated by weighting the pore sizes in each group by number frequency. The volume-weighted mean pore size was calculated by weighting the pore sizes in each group by volume %. The mode of each distribution was determined by finding the maximum of the peaks in the distribution.

[0075] To further elaborate the quantitative image analysis test method, the principles behind the design of this test method are described in more general terms. To satisfy this test method, a cross-sectional SEM image representative of the pore phase is taken, the image portion showing the nanoporous metal in the cross-sectional plane is isolated, and the size of the pores is quantified. The visual cues required to remove image artifacts and isolate the image portion suitable for analysis, including texture and perspective, referred to above as "censoring", will be readily apparent to those skilled in the art. The pore phase analyzed for analysis should demonstrate excellent fidelity to the SEM image when the two are compared visually (see, for example, Figures 7A-7C). The minimum feature size that can be resolved corresponds to approximately 5 pixels. The diameter-to-Ferret ratio allows a practical check to ensure that the analysis of the pores to determine their individual diameters is performed correctly.

[0076] Glucose Amperometric Benchtop Test Amperometric benchtop testing was performed using the following system. The completed electrode (with 4 mm diameter) was immersed in a 20 mL beaker containing phosphate buffered saline (PBS) and a magnetic stir bar, side-by-side with a Ag / AgCl reference electrode (Gamry) and side-by-side with a 0.25 mm platinum wire counter electrode (Alfa Aesar). The electrodes were connected to a potentiostat system (Digi-Ivy #DY211, or Gamry Reference 600) with a set potential of 0.6-0.7 V and an oversampling rate of 5 Hz. The working electrode voltage is reported relative to the reference (or pseudo reference) electrode. The system was allowed to equilibrate for 60 minutes with magnetic stirring at 300 rpm. The concentration of glucose was successively increased by pipetting varying microliter volumes of test solution (D-(+)-glucose, 0.4 g / mL in deionized water) into PBS every 50-500 seconds, and the current was measured as a function of time.

[0077] Pseudo-reference electrode test A potentiostat (Gamry Reference 600) was used in conjunction with Gamry Instruments Echem Analyst Software and Gamry Instruments Framework® Data Acquisition Software to perform the tests. Two variations of the three-electrode electrochemical cell were assembled. The electrolyte solution contained 1 M potassium chloride (Sigma Aldrich) with 1 mM potassium ferricyanide (Sigma Aldrich) in deionized water (>18 M-ohm).

[0078] The first variant (meaning the variant traditionally used in the art) consisted of a liquid junction Ag / AgCl reference electrode (Gamry), a platinum wire (99.9%) as counter electrode, a 3 mm diameter flat gold electrode (Alfa Aesar) as working electrode, and an electrolyte solution. The working and reference electrodes were physically separated by a distance of about 1 cm.

[0079] The second variation consisted of an ePTFE silver invibrated film as a pseudo reference electrode, a platinum wire (99.9%) as a counter electrode, an NPG / ePTFE membrane (housed in a PTFE electrochemical cell with a 3 mm diameter opening) as a working electrode, and an electrolyte solution. The pseudo reference electrode and the working electrode were physically separated by a distance of about 1 cm.

[0080] Cyclic voltammograms were generated in the modified form using an initial electrode of 0.5 V versus a reference (or pseudo-reference) electrode and scanned to 0.1 V, followed by a back scan to 0.5 V at a scan rate of 50 mV / s.

[0081] Biofouling resistance test A biofouling test was developed to evaluate the electrochemical performance of sample electrodes in the presence of a common biofouling medium, such as bovine serum albumin (BSA). Solutions are aqueous unless otherwise stated.

[0082] A potassium ferricyanide stock solution (2 mM in 0.1 M KCl solution) was employed as a small molecule redox generator to characterize the electrochemical performance. A set of BSA biofouling test solutions was prepared by dissolving BSA in the potassium ferricyanide stock solution at 2 mg / mL, 6 mg / mL, 10 mg / mL, 15 mg / mL, and 25 mg / mL.

[0083] The surface of the sample electrode was rinsed with 70% isopropanol for 3-5 seconds, then the sample electrode was placed in a 20 mL beaker filled with 0.05 M sulfuric acid solution, side-by-side with an Ag / AgCl reference electrode and a 0.25 mm platinum wire counter electrode. The electrode was connected to a potentiostat system (Digi-Ivy #DY211). The working electrode voltage is reported relative to the reference (or pseudo reference) electrode. The working electrode was cleaned by performing a cleaning CV scan (10 cycles, scan range: 0-1.5 V, scan rate: 50 mV / s). After cleaning, the electrode was removed from the sulfuric acid test cell and rinsed with DI water, then Kimwipes® tissue was used to absorb the residual water.

[0084] The sample electrode, Ag / AgCl reference electrode, and platinum wire counter electrode were immersed in a 20 mL beaker filled with potassium ferricyanide. Baseline CV data were obtained by conducting continuous CV scans (10–20 cycles, scan range: -0.2–0.6 V, scan rate: 100 mV / s). The electrode was then transferred to another 20 mL beaker filled with BSA biofouling test solution, followed by continuous CV scans (100 cycles, scan range: -0.2–0.6 V, scan rate: 100 mV / s) to obtain biofouling CV data. The electrochemical performance of the sample electrode in the presence of biofouling media was evaluated by comparing the peak current from the potassium ferricyanide stock solution with the peak current from the BSA biofouling test solution.

[0085] Capillary Flow Polymetry (CFP) Test Measurements were performed using a Quantachrome Porometer 3G zH. The wetting fluid was silicone oil with a nominal surface tension of 19.78 dynes / cm. The pressure range was 0.255 psig to 394 psig. Sample size was 10 mm diameter. The ramp rate setting was "2x," resulting in a run time of approximately 28 minutes. Only "wet" curve data was generated (i.e., no "dry" curve data was collected). The maximum measurable flow rate was 10 liters / min.

[0086] Wet Flex Particulation Test This durability test was developed to evaluate the tendency of composite materials to shed particles. For the test to be valid, the specimen must have a bending stiffness low enough to allow full bending motion under the test conditions. To perform the test, a 2.125” x 0.5” specimen was cut from the composite. The specimen was loaded into the test fixture by sandwiching it between pieces of engineering plastic cut to the shape shown in Figure 13. The specimen was loaded with a controlled amount of slack and held in place by an O-ring shown in Figure 14. For scale, the size of the window that allows the specimen to bend is 24.5mm long x 14.1mm wide x 2.7mm thick. The test fixture containing the specimen was then loaded into a standard 50mL centrifuge tube. The tube was then filled with isopropanol to the 40mL line. The tube was then closed with a cap and tape to prevent leakage. The tube was then loaded into an Intelli-Mixer (#RM-2L) with the plane of the test fixture parallel to the axis of rotation as shown in Figure 15. This orientation allows for flexing of the sample. The Intelli-Mixer was set to rock the sample + / - 99 degrees at 20 rpm for the desired time (typically 1-7 days). Each time the sample was rocked, it also flexed based on the fluid dynamics within the tube. Flexing refers to the slack in the sample being switched from one side of the test fixture to the other. After rocking for the desired time, the liquid within the tube was withdrawn using a pipette and analyzed using ICP-MS to check for the presence of metal that may have been shed from the composite.

[0087] Electrochemical Surface Area (ECSA) Test Electrochemical tests were carried out in a WonATech CCK05 corrosion cell kit (500 mL) as shown in Figure 17. The working electrode sample was fitted with an 11.28 mm electrode diameter (1 cm 2 The counter electrode was a WonATech PFL5 platinum flat plate electrode (active area 5 cm 2) or 10 cm platinum wire (Sigma Aldrich 1.5 mm diameter, ≥99.9% trace metals basis, 349399-3.8G). The reference electrode was Gamry 932-00018, Ag / AgCl, which was filled with and stored in a saturated KCl solution. The cell utilized a Luggin capillary to bring the reference electrode into close proximity to the working electrode surface. The cell was filled with 500 mL of sulfuric acid (LabChem LC256801, 0.05M). The reference sample for the working electrode was gold foil (Sigma Aldrich 326496-1.5G 0.127 mm thick, 99.99% trace metals basis or equivalent). Dissolved oxygen was removed from the electrolyte by bubbling nitrogen gas through a glass frit for at least 10 min (stirring of the electrolyte was avoided by turning off the nitrogen purge during cyclic voltammetry measurements).

[0088] The samples were cut or punched into circular disks with diameters between 15.5 mm and 22 mm, which were then loaded into flat specimen holders. Care was taken during insertion of the sample holder to ensure that all O-rings and internal parts were dry to ensure there were no ionically conductive paths around the sample. Complete wetting was ensured by wetting the sample with isopropanol and then submerging it in the electrolyte. Cyclic voltammetry (CV) was used to ensure that the working electrode was clean, as will be understood by those skilled in the art.

[0089] The electrochemical surface area was determined by measuring the double layer capacitance since ECSA is proportional to the double layer capacitance. To determine the double layer capacitance, representative cyclic voltammetry curves were collected by scanning the potential (vs. the reference electrode) from 0 mV to 100 mV at the following scan rates: 100 mV / s, 50 mV / s, 20 mV / s, and 10 mV / s. The height of the curve (amps (h)) at 50 mV was determined and plotted versus the sweep rate (V / s). The double layer capacitance was determined from the slope of the best fit line. To determine the roughness factor, which is the ratio of the electrochemical surface area to the geometric surface area, the double layer capacitance of the sample was normalized by the double layer capacitance of a smooth gold foil. A smooth gold foil was assumed to have a roughness factor of 1. To calculate the metal specific surface area, the roughness factor of the sample was divided by the mass per metal area of ​​the sample. EXAMPLES

[0090] Example 1: Preparation of NPG / ePTFE Composite In this example, a nanoporous gold-incorporated ePTFE membrane ("NPG / ePTFE" composite) is described.

[0091] ePTFE membrane (3-5g / m 2A 100-μm thick, 1.5 psi bubble point, 92 μm non-contact thickness, WL Gore & Associates) was constrained in a 4.5″ diameter metal hoop and tensioned by hand to remove wrinkles. A reactive gold ink in solvent (part #LXPM-G2-1019, Liquid X, Inc.) was prepared according to the teachings of U.S. Pat. No. 9,018,264 by mixing 1.0 g of LXPM-G2-1019 and 0.05 g of Tergito® TMN-10 (Dow, The gold phase was mixed with a substrate wetting package consisting of 0.03 g of 1-hexanol and 0.03 g of NPG (Nutrition Chemicals, Inc.). The mixture was pipetted onto the surface of the membrane and spread evenly using a disposable pipette bulb until it wetted through the ePTFE (approximately 30 seconds). Excess ink was removed by wiping the surface of the ePTFE membrane with a Kimwipe® tissue. The sample was dried with a heat gun and heated in a standard convection oven at 155° C. for 20 minutes, then at 300° C. for 1 hour to reduce and sinter the gold phase and remove residual ink solvent, reducing agent, and residual substrate wetting package. The result was an NPG / ePTFE composite.

[0092] Figures 3A-3C show representative SEM images of an example of an NPG / ePTFE composite, where Figure 3A shows a cross-section of the composite, Figure 3B shows a surface image, and Figure 3C shows a close-up of a cross-section of the NPG phase.

[0093] The NPG / ePTFE composite contained a nanoporous high surface area gold matrix with a nanopore size distribution within the metal phase of about 10-200 nm. This NPG matrix was imbibed within the interior microstructure of the ePTFE membrane. The NPG can be seen in Figures 3A-3C as a light colored material within the pores between the nodes and fibrils of the ePTFE membrane. As shown in Figures 3A and 3C, the NPG matrix was shown to be spaced away from and avoiding substantial contact with the ePTFE membrane, particularly the nodes of the ePTFE membrane, forming approximately 10 μm gaps exposed along the surface of the NPG / ePTFE composite, as shown in Figure 3B. Additionally, the NPG matrix was not present on the outer surface layers (i.e., bare layers) of the ePTFE membrane where there is no need for a lamination interface. The measured sheet resistance of the NPG / ePTFE composite was about 0.3-1 ohms / square according to the four-point probe sheet resistance test described above and shown in Figure 2.

[0094] The nanopore size analysis of the NPG metal phase is summarized in Figures 4A-7. Figure 4A shows another representative cross-sectional SEM image of an example of an NPG / ePTFE composite, and Figure 4B shows the same image processed for nanopore size analysis. Figure 4C shows isolated nanopores within the metal phase of the NPG / ePTFE composite. Figure 5 shows the nanopore size distribution within the metal phase of the NPG / ePTFE composite. Figure 6 is a histogram showing the ratio of the minor axis of the best fit ellipse to the minimum Feret of the nanopores within the metal phase of the NPG / ePTFE composite. Figure 7 is a histogram showing the ratio of the major axis of the best fit ellipse to the maximum Feret of the nanopores within the metal phase of the NPG / ePTFE composite.

[0095] Example 2: Preparation of NPG / ePTFE Bare Electrodes In this example, the preparation of an NPG / ePTFE flat disk bare electrode ("NPG / ePTFE bare electrode") is described.

[0096] A PTFE hollow rod (1.5" long, 0.5" outer diameter, 0.25" inner diameter) was provided with a 0.25" proximal opening and a 3-4mm distal opening. A NPG / ePTFE bare electrode was produced by inserting the NPG / ePTFE composite of Example 1 into the hollow rod through the proximal opening, laying flat against the distal opening, and sealing with an ePTFE gasket.

[0097] Example 3: Preparation of CG / ePTFE composite In this example, the preparation of an ePTFE membrane composite incorporating a conformal gold coating ("CG / ePTFE composite") is described.

[0098] First ePTFE membrane ("target membrane") (3-5g / m 2 A second ePTFE membrane ("portal membrane") (3-5 g / m2) was placed in a 4" diameter metal hoop and tensioned by hand to remove wrinkles. 2A 0.75 mL gold nanoparticle ink (#UTDAu60X; UTDots, Mass / area, 40 psi bubble point, 18 μm non-contact thickness, WL Gore & Associates) was constrained within a 6” diameter metal hoop and tensioned by hand to remove wrinkles. The portal membrane was placed on top of the target membrane so that the two membranes were in physical contact and approximately concentric. 0.75 mL of gold nanoparticle ink (#UTDAu60X; UTDots, Mass / area, 40 psi bubble point, 18 μm non-contact thickness, WL Gore & Associates) was constrained within a 6” diameter metal hoop and tensioned by hand to remove wrinkles. The immersing solution was pipetted onto the surface of the portal membrane and spread evenly using a disposable pipette bulb until it completely wetted both the portal membrane and the target membrane (<approximately 30 seconds). Excess ink was removed by wiping the top surface of the portal membrane with a lint-free cloth. The two immersing membranes were then separated by separating their respective hoops. The portal membrane was discarded. The target membrane was then dried using a heat gun set at 200°F and then heated at 300°C for 1 hour in a standard convection oven. The result was a CG / ePTFE composite.

[0099] The mass / area of ​​the CG / ePTFE composite is 46 g / m 2 and the sheet resistance was about 0.2-0.4 ohms / square according to the four-point probe sheet resistance test described above and shown in Figure 2. The sheet resistance of the composite was nearly the same (specifically within about 15% of the lower resistive surface) whether the surface being measured was the top or bottom surface, demonstrating that the metal was conformally coated throughout the entire thickness of the target membrane.

[0100] Figures 8A-8D show representative SEM images of examples of CG / ePTFE composites. Figure 8A shows a composite cross section, Figure 8B shows a node cross section, and Figure 8C shows a fibril cross section. CG can be seen around the nodes and fibrils of the ePTFE membrane. Figure 8D shows a surface image with gaps in the conformal gold coating along the thickness or z direction. The gaps may allow tissue ingrowth while maintaining electrical conductivity in the plane or xy direction.

[0101] Example 4: Silver-imbibed ePTFE structure In this example, the preparation of a silver-imbibing ePTFE structure is described.

[0102] The portal membrane and target membrane were prepared as in Example 3 above. 5.7 g of silver nanoparticle ink (#UTDAg60x; UTDots, Inc.) was diluted with 3.3 g of xylene and pipetted onto the surface of the portal membrane, spread evenly, and allowed to completely wet the membrane as in Example 3 above. The portal membrane was removed and discarded as in Example 3 above, and the target membrane was heated as in Example 3 above. The result was a silver-imbibing ePTFE structure.

[0103] Example 5: Preparation of bare CG / ePTFE electrodes In this example, the preparation of a CG / ePTFE flat disk bare electrode ("CG / ePTFE bare electrode") is described.

[0104] A hollow PTFE rod (1.5" length, 0.5" outer diameter, 0.25" inner diameter) was provided with a 0.25" proximal opening and a 3-4mm distal opening. A bare CG / ePTFE electrode was produced by inserting the CG / ePTFE composite of Example 3 into the hollow rod through the proximal opening, laying flat against the distal opening, and sealing with an ePTFE gasket.

[0105] Example 6: Electrochemical behavior of a biosensor with an NPG / ePTFE working electrode and a silver-imbibing-treated ePTFE pseudo reference electrode In this example, the electrochemical behavior of a three-electrode electrochemical cell containing a bare NPG / ePTFE electrode as the working electrode and a silver-imbibing-treated ePTFE structure as the pseudo-reference electrode is described.

[0106] Using the pseudo reference electrode test method described above, a first electrochemical cell was constructed containing the bare NPG / ePTFE electrode of Example 2 as the working electrode and the silver imbibed ePTFE structure of Example 4 as the pseudo reference electrode ("NPG / / Ag Imbibed RE"). For comparison, a second electrochemical cell was constructed containing a flat gold electrode disk working electrode and a liquid junction Ag / AgCl reference electrode ("Gold Disk-Ag / Ag liquid junction RE").

[0107] Figure 9 shows the overlay of the cyclic voltammograms of the NPG / / Ag immersing RE electrochemical cell with the gold disk-Ag / Ag liquid junction RE electrochemical cell. As can be seen from this overlay of the data, the cyclic voltammograms are located in almost the same potential region. There is a slight shift in potential (166 mV vs. 124 mV). This shift is expected because the liquid junction reference electrode is saturated potassium chloride, whereas the pseudo reference electrode is in direct contact with the electrolyte. It is also clear that the hysteresis in the voltammogram of the NPG / / Ag immersing RE electrochemical cell is narrower and has a higher gain compared to that of the gold disk-Ag / AgCl liquid junction RE cell. This clearly demonstrates that the NPG / / Ag immersing RE cell employing the pseudo reference electrode works as expected within these defined conditions. In other words, an electrode configuration using ePTFE as a working electrode substrate with nanoporous gold and ePTFE as a pseudo reference electrode substrate with immersing treated silver, with a physical separation between them, can function as an electrochemical analyte biosensor.

[0108] Example 7: Biofouling resistance of NPG / ePTFE bare electrodes In this example, the biofouling resistance of bare NPG / ePTFE electrodes is described.

[0109] The NPG / ePTFE bare electrode of Example 2 was tested for biofouling resistance according to the Biofouling Resistance Test Method described above. In addition, unpolished gold foil was subjected to the same test conditions.

[0110] Table 3 shows the peak current of the NPG / ePTFE bare electrode compared to the gold foil samples, normalized to the baseline for each sample. The NPG / ePTFE samples showed only a slight reduction in peak current in the BSA biofouling test solutions, even at the highest BSA concentrations. In comparison, the gold foil samples showed a significant reduction in peak current, even at low BSA concentrations. In summary, the NPG / ePTFE samples exhibited high electrochemical performance in the presence of common biofouling media. [Table 3]

[0111] Example 8: NPG / ePTFE GOx completed electrode and CG / ePTFE GOx completed In this example, the preparation of a complete enzyme immobilized electrode containing glucose oxidase (GOx) is described. All solutions are aqueous unless otherwise noted.

[0112] The distal end of each of the NPG / ePTFE bare electrode of Example 2 and the CG / ePTFE bare electrode of Example 5 was immersed in isopropanol, immersed in deionized water, rinsed in deionized water, immersed in polyethyleneimine (PEI) solution (10 mg / mL water, 10 min, Sigma), and rinsed with deionized water. GOx (50 kU / g activity, Sigma) was dissolved in 500 U / mL phosphate buffer, and 10 μL was pipetted onto the ePTFE membrane surface through the distal opening of each electrode and air-dried. The distal end of each electrode was immersed a second time in the PEI solution, pipetted a second time with the GOx solution, and air-dried a second time. Finished NPG / ePTFE GOx or CG / ePTFE GOx electrodes were prepared by pipetting a 4 μL volume of Nafion solution (2% w / v in 92 wt% ethanol:8 wt% water, Sigma) onto the distal opening of each electrode, air drying, and storing at 4 °C, respectively.

[0113] Example 9: Electrochemical response of NPG / ePTFE GOx finished electrodes and CG / ePTFE GOx finished electrodes to glucose In this example, the electrochemical response to glucose of the finished NPG / ePTFE GOx and CG / ePTFE GOx electrodes of Example 8 is described.

[0114] As shown in Figure 10A, upon continuous addition of glucose, the measured current of the NPG / ePTFE GOx finished electrode rose rapidly and quickly stabilized. As shown in Figure 10B, the NPG / ePTFE GOx finished electrode responded to a wide range of glucose concentrations from 0 to 400 mg / dL. In comparison, the gold foil immobilized with glucose oxidase prepared according to the procedure of Example 8 showed a significantly reduced signal as a function of glucose concentration (not shown).

[0115] As shown in Figure 11A, upon continuous addition of glucose, the measured current of the CG / ePTFE GOx finished electrode rose rapidly and quickly stabilized. As shown in Figure 11B, the CG / ePTFE GOx finished electrode responded to a wide range of glucose concentrations from 0 to 400 mg / dL. In comparison, the gold foil immobilized with glucose oxidase prepared according to the procedure of Example 8 showed a significantly reduced signal as a function of glucose concentration (not shown).

[0116] Example 10: Dependence of electrochemical surface area on electrolyte solvent surface tension In this example, the dependence of electrochemical surface area on electrolyte solvent surface tension is described.

[0117] The NPG / ePTFE composite of Example 1, the CG / ePTFE composite of Example 3, and the gold foil were each immersed in a series of solutions containing various ratios of saline and isopropanol. Saline has a high surface tension of about 72 mN / m, isopropanol has a lower surface tension of about 21 mN / m, and saline:isopropanol mixtures have surface tension as a function of the ratio of solvents, such that a 50:50 saline:isopropanol mixture has a low surface tension of about 25 mN / m, and a 90:10 saline:isopropanol mixture has a high surface tension of about 50 mN / m, or the same as blood.

[0118] Electrolytes were prepared as follows: All dilutions were with DI water (>18 megohms); 0.05M sulfuric acid (H2SO4) in DI water, i.e. 2.5mL of 1M H2SO4 diluted to 50mL; 0.05M sulfuric acid in 1% isopropanol, i.e. 2.5mL of 1M H2SO4 and 0.5mL of isopropanol diluted to 50mL; 0.05M sulfuric acid in 5% isopropanol, i.e. 2.5mL of 1M H2SO4 and 2.5mL of isopropanol diluted to 50mL; 0.05M sulfuric acid in 10% isopropanol, i.e. 2.5mL of 1M H2SO4 and 5mL of isopropanol diluted to 50mL; 0.05M sulfuric acid in 20% isopropanol, i.e. 2.5mL of 1M H2SO4 and 10mL of isopropanol diluted to 50mL. 0.05M sulfuric acid in 30% isopropanol, i.e. 2.5mL of 1M H2SO4 and 15mL of isopropanol diluted to 50mL. 0.05M sulfuric acid in 50% isopropanol, i.e. 2.5mL of 1M H2SO4 and 25mL of isopropanol diluted to 50mL.

[0119] The electrochemical surface area of ​​each immersed sample was measured and the absolute change in the measured electrochemical surface area was calculated according to the following equation:

number

[0120] As shown in Figure 12, the composites showed significant differences depending on the electrolyte composition. The CG / ePTFE composites exhibited increasing surface area results with decreasing electrolyte surface tension over the range from pure saline to 50:50 saline:isopropanol. The electrochemical surface area was approximately 0.005 cm over this range.2 From about 1,000 cm 2 (or an absolute change of about 19,900%). In comparison, the NPG / ePTFE composite demonstrated that its electrochemical surface area was nearly independent of electrolyte surface tension and produced a relatively flat response over the range from pure saline to 50:50 saline:isopropanol. The electrochemical surface area was approximately 5 cm over this range. 2 From about 2.5 cm 2 to 0.25% (or an absolute change of about 50%). As noted above, such a flat response of NPG / ePTFE was not expected to be relatively constant (i.e., less than about 50%) over a wide electrolyte surface tension range, since the underlying ePTFE film was expected to be hydrophobic and thus limit wetting and result in a small observable electrochemical surface area. In contrast, the non-hydrophobic gold foil showed the expected relatively flat response over the range from pure saline to 50:50 saline:isopropanol.

[0121] Example 11: Capillary flow polimetry of NPG / ePTFE composites In this example, the capillary flow polimetry (CFP) data of the NPG / ePTFE composite of Example 1 is described according to the CFP test method described above. As explained in Example 1 and shown in Figures 3A and 3C, gaps can be seen between the NPG matrix and the ePTFE membrane, particularly between the nodes of the ePTFE membrane. The CFP data is shown in Figure 16. The extremely low bubble point (i.e., the onset of flow) is approximately 5 psig. This is consistent with the presence of these gaps between the NPG matrix and the ePTFE membrane that extend through the thickness of the composite.

[0122] Example 12: Durability of NPG / ePTFE Composites This example describes durability data for NPG / ePTFE composites formed according to the teachings of Example 1, as measured according to the Wet Flex Granulation Test described above. Upon completion of the 24 hour Wet Flex Granulation Test, the amount of gold present in the test solution was below the ICP detection limit. This result was consistent with no loss of gold from the NPG / ePTFE composite, indicating that at least 99.97 wt.% of the gold was retained in the composite.

[0123] Example 13: Fragility of thin NPG without reinforcement This example illustrates the difficulty of handling thin NPGs that are not reinforced with a polymer substrate. A piece of 12K white gold genuine gold leaf (LA Gold Leaf, 0.12 μm thick, 51% gold / 48% silver / 1% Pd) approximately 1 cm x 1 cm in size was placed in a Petri dish using tweezers. 70% HNO3(aq) was added to the Petri dish in an amount sufficient to completely cover the NPG. The gold leaf was left in the HNO3(aq) at room temperature for 15 minutes to allow for the time it takes for the silver to be etched away to produce the NPG. After etching, the sample broke easily with a light touch of the tweezers.

[0124] Example 14: Preparation of CPS / ePTFE Composite A close-packed silver / ePTFE composite (CPS / ePTFE) was formed according to the teachings of Example 1 of WO 2019 / 216885, entitled "Flexible and Durable Printed Circuits on Stretchable and Non-Stretchable Substrates," to WL Gore & Associates, Inc. The properties of this material and of an NPG / ePTFE composite prepared according to the procedure described in Example 1 were measured and compared.

[0125] Figure 18 compares low magnification (2,000x) cross-sectional SEM images of NPG / ePTFE and CPS / ePTFE, allowing the total thickness of each sample to be determined, including the bare ePTFE surface layer of NPG / ePTFE. Figure 19 compares a close-up of the metal phases of NPG / ePTFE and CPS / ePTFE, as well as their pore phases, as determined by quantitative image analysis. Figure 20 compares the pore size distributions of NPG / ePTFE and CPS / ePTFE on a count basis and on a volume basis. The modal pore size is shown on each graph, and the shift in mode from the count-based graph to the volume-based graph is indicated by a block arrow.

[0126] Numerical data comparing NPG / ePTF to CPS / ePTFE are shown in Tables 4-6. To determine the volume per area and volume percent values, the following densities were assumed: gold 19.3 g / cc, silver 10.5 g / cc, and PTFE 2.2 g / cc. Some significant shifts in pore size distribution are shown in Table 7. [Table 4] [Table 5] [Table 6] [Table 7] (Aspect) (Aspect 1) 1. A composite material comprising: a porous polymer substrate; a nanoporous metal present within said porous polymeric substrate and comprising a number-based nanopore size distribution and a volume-based nanopore size distribution, wherein the mean of said volume-based nanopore size distribution is at least 200% greater than the mean of said number-based nanopore size distribution; Composite material comprising: (Aspect 2) 2. The composite material of embodiment 1, wherein the porous polymer substrate comprises a plurality of nodes and a plurality of fibrils that cooperate to define a plurality of interconnected pores, and the nanoporous metal is at least partially contained within the pores between the nodes and the fibrils. (Aspect 3) 3. The composite material of any one of the preceding claims, wherein the nanoporous metal comprises nanopores ranging from about 10 nm to about 200 nm in size. (Aspect 4) 4. The composite material of any one of the preceding claims, wherein the porous polymeric substrate comprises a fluoropolymer or a polyolefin. (Aspect 5) 5. The composite of embodiment 4, wherein the porous polymer substrate comprises expanded polytetrafluoroethylene or expanded polyethylene. (Aspect 6) 6. The composite material of any one of the preceding aspects, wherein the nanoporous metal comprises platinum, iridium, palladium, gold, silver, copper, nickel, or a combination or alloy thereof. (Aspect 7) The nanoporous metal contains nanopores having an average diameter of about 1 nm to about 500 nm, the porous polymer substrate comprises micropores which are larger than the nanopores of the nanoporous metal; 7. The composite material according to any one of embodiments 1 to 6. (Aspect 8) 8. The composite material of any one of the preceding claims, wherein the mean of the volumetric pore size distribution is at least 500% greater than the mean of the number based nanopore size distribution. (Aspect 9) 9. The composite material of embodiment 8, wherein the number-based nanopore size distribution is unimodal and right-skewed. (Aspect 10) 1. A composite material comprising: a microporous polymeric substrate comprising a plurality of interconnected micropores; a nanoporous metal at least partially contained within the micropores of the microporous polymer substrate and separated from the microporous polymer substrate so as to define gaps; Composite material comprising: (Aspect 11) 11. The composite material of embodiment 10, wherein the microporous polymer substrate is one of a membrane, a tube, and a fiber. (Aspect 12) 12. The composite material of claim 10 or 11, wherein the microporous polymeric substrate comprises a fluoropolymer or a polyolefin. (Aspect 13) 13. The composite of embodiment 12, wherein the microporous polymer substrate comprises expanded polytetrafluoroethylene or expanded polyethylene. (Aspect 14) 14. The composite material of any one of aspects 10 to 13, wherein the nanoporous metal has a number-based nanopore size distribution that is unimodal and right-skewed. (Aspect 15) 15. The composite material of any one of claims 10 to 14, wherein the nanoporous metal comprises nanopores ranging from about 10 nm to about 200 nm in size. (Aspect 16) 16. The composite material of any one of aspects 10-15, wherein the gaps are accessible in the z-direction at a surface of the composite material, and the nanoporous metal provides electrical conductivity in at least the xy directions. (Aspect 17) 1. A composite material comprising: a first continuous network comprising a microporous polymer having a plurality of interconnected micropores; a second substantially continuous network comprising nanoporous metal, said second substantially continuous network interpenetrating said first continuous network, said composite having a porosity of at least 30 vol.%; Composite material comprising: (Aspect 18) 18. The composite material of embodiment 17, wherein the first continuous network comprises an interfacial region that is not metallized and is distinct from the second substantially continuous network. (Aspect 19) 20. The composite material of embodiment 18, wherein the interfacial region is a non-laminated, integral part of the first continuous network. (Aspect 20) 20. The composite material of any one of aspects 17-19, wherein the nanoporous metal is separated from the microporous polymer in a manner that defines a gap. (Aspect 21) 21. The composite material of any one of aspects 17-20, wherein at least 99 wt. % of the nanoporous metal is retained within the composite material after 1 day of Wet Bending Granulation Test. (Aspect 22) 22. The composite material of any one of aspects 17-21, wherein at least 99.9 wt% of the nanoporous metal is retained within the composite material after 1 day of Wet Bending Granulation Test. (Aspect 23) 23. The composite material of any one of aspects 17 to 22, wherein the nanoporous metal comprises less than 40 vol.% of the composite material. (Aspect 24) An electrochemical cell comprising the composite material according to any one of embodiments 1 to 23.

Claims

1. 1. A composite material comprising: a porous polymer substrate; a nanoporous metal present within said porous polymeric substrate and comprising a number-based nanopore size distribution and a volume-based nanopore size distribution, wherein the mean of said volume-based nanopore size distribution is at least 200% greater than the mean of said number-based nanopore size distribution; Composite material comprising:

2. 2. The composite material of claim 1, wherein the porous polymer substrate comprises a plurality of nodes and a plurality of fibrils that cooperate to define a plurality of interconnected pores, and the nanoporous metal is at least partially contained within the pores between the nodes and the fibrils.

3. The composite material of claim 1 or 2, wherein the nanoporous metal comprises nanopores between 10 nm and 200 nm in size.

4. The composite material of claim 1 or 2, wherein the porous polymeric substrate comprises a fluoropolymer or a polyolefin.

5. The composite material of claim 4 , wherein the porous polymeric substrate comprises expanded polytetrafluoroethylene or expanded polyethylene.

6. 3. The composite material of claim 1 or 2, wherein the nanoporous metal comprises platinum, iridium, palladium, gold, silver, copper, nickel, or combinations or alloys thereof.

7. the nanoporous metal comprises nanopores having an average diameter of 1 nm to 500 nm; the porous polymer substrate comprises micropores which are larger than the nanopores of the nanoporous metal; 3. A composite material according to claim 1 or 2.

8. 3. The composite material of claim 1 or 2, wherein the mean of the volumetric nanopore size distribution is at least 500% greater than the mean of the number-based nanopore size distribution.

9. 9. The composite material of claim 8, wherein the number-based nanopore size distribution is unimodal and right-skewed.

10. 1. A composite material comprising: a microporous polymeric substrate comprising a plurality of interconnected micropores; a nanoporous metal at least partially contained within the micropores of the microporous polymer substrate and separated from the microporous polymer substrate so as to define gaps; Composite material comprising:

11. The composite material of claim 10 , wherein the microporous polymeric substrate is one of a membrane, a tube, and a fiber.

12. 12. The composite material of claim 10 or 11, wherein the microporous polymeric substrate comprises a fluoropolymer or a polyolefin.

13. 13. The composite material of claim 12, wherein the microporous polymeric substrate comprises expanded polytetrafluoroethylene or expanded polyethylene.

14. 12. The composite material of claim 10 or 11, wherein the nanoporous metal has a number-based nanopore size distribution that is unimodal and right-skewed.

15. The composite material of claim 10 or 11, wherein the nanoporous metal comprises nanopores between 10 nm and 200 nm in size.

16. 12. The composite material of claim 10 or 11, wherein the gaps are accessible in the z-direction at a surface of the composite material, and the nanoporous metal provides electrical conductivity in at least the xy direction.

17. 1. A composite material comprising: a first continuous network comprising a microporous polymer having a plurality of interconnected micropores; a second substantially continuous network comprising nanoporous metal, said second substantially continuous network interpenetrating said first continuous network, said composite having a porosity of at least 30 vol.%; Composite material comprising:

18. 20. The composite material of claim 17, wherein the first continuous network includes an interfacial region that is not metallized and that is distinct from the second substantially continuous network.

19. 20. The composite material of claim 18, wherein the interfacial region is a non-laminated, integral part of the first continuous network.

20. 19. The composite material of claim 17 or 18, wherein the nanoporous metal is separated from the microporous polymer so as to define a gap.

21. 19. The composite material of claim 17 or 18, wherein at least 99% by weight of the nanoporous metal is retained within the composite material after 1 day of Wet Bend Granulation Test.

22. 19. The composite material of claim 17 or 18, wherein at least 99.9 wt% of the nanoporous metal is retained within the composite material after 1 day of wet flex grain testing.

23. 19. The composite material of claim 17 or 18, wherein the nanoporous metal comprises less than 40 vol% of the composite material.

24. 20. An electrochemical cell comprising the composite material of claim 1, 2, 10, 11, 17 or 18.

Citation Information

Patent Citations

  • Metallized porous conductive polymer composite material, preparation method and application thereof

    CN112300529A

  • Composite porous membrane and its production method

    JP2008214462A

  • Micro-porous article having a three-dimensional porous network of acid-sintered interconnected silica nanoparticles and method for producing the same

    JP2017519619A

  • Porous molded body of micro or mesoporous fine particles, carrier for carrying enzyme, enzyme composite thereof and manufacturing method therefor

    JP2018090767A

  • Flexible and durable printed circuits on stretchable and non-stretchable substrates

    JP2021522092A