Surface conditioner for adding to coating film forming liquid

A copolymer-based surface conditioner addresses the challenges of achieving long-term hydrophilicity and durability in coatings by using polysiloxane and ammonium cation groups to reduce receding contact angles, enhancing self-cleaning and antifouling properties.

JP7576292B2Active Publication Date: 2024-10-31KYOEISHA CHEM CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2019212584
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-11-25
Publication Date
2024-10-31
Estimated Expiration
2039-11-25

AI Technical Summary

Technical Problem

Existing coating technologies face challenges in achieving long-term hydrophilicity without compromising durability, adhesion, and resistance to fouling, particularly when exposed to outdoor conditions, due to limitations in resin components and stability issues with current surface conditioning agents.

Method used

A surface conditioner is formulated with a specific copolymer composition containing polysiloxane and ammonium cation groups, which imparts hydrophilicity by reducing the receding contact angle upon water exposure, enhancing self-cleaning and antifouling properties while maintaining film integrity.

Benefits of technology

The copolymer-based surface conditioner provides long-term stain resistance and improved adhesion, ensuring the coating remains hydrophilic only when water is present, reducing dirt adhesion and maintaining a smooth, durable surface even under outdoor exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576292000001
    Figure 0007576292000001
  • Figure 0007576292000002
    Figure 0007576292000002
  • Figure 0007576292000003
    Figure 0007576292000003
Patent Text Reader

Abstract

To provide a surface conditioning agent for the addition to a coating film-forming liquid agent that is blended in a small amount into a coating film-forming liquid agent for forming a coating film to impart long-term anti-fouling property resulting from performing self-cleaning of the coating film in outdoor exposure by giving hydrophilicity only when water adheres to the coating film.SOLUTION: The surface conditioning agent for the addition to a coating film-forming liquid agent contains a copolymer which includes (a) a copolymerization repeating unit of a (meth)acrylic acid ester having a polysiloxane structure in an alcohol component of the ester and (b) a copolymerization repeating unit of a (meth)acrylic acid ester having an ammonium cation structure in an alcohol component of the ester and has a weight average molecular weight of 1,500 to 100,000, and has mass ratios of the copolymerization repeating unit (a) and the copolymerization repeating unit (b) each to the total amount thereof in the copolymer of 0.1 to 20.0 and 99.9 to 80.0, respectively.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface conditioner for addition to a coating film-forming liquid agent, which is added in small amounts to a coating film-forming liquid agent such as a paint or coating agent, and which imparts leveling properties to the exposed surface of the paint coating film formed thereby, and imparts hydrophilicity by lowering the receding contact angle in the expansion and contraction method, which is a type of water contact angle measurement method. [Background technology]

[0002] In recent years, with the trend of adding high value to painted surfaces, there is a demand for improving the antifouling properties of a paint coating film formed with a coating film-forming liquid agent such as a paint or coating agent to be applied to an object to be coated by making the exposed surface hydrophilic. Hereinafter, a paint coating film is also simply referred to as a film.

[0003] Generally, the method of imparting hydrophilicity to the above-mentioned coating is to make the exposed surface of the formed coating hydrophilic by making the resin itself contained in the coating agent that forms the coating or the crosslinking component itself that forms the coating hydrophilic. However, in this case, the resin and crosslinking component that can be used are limited because the curable resin component needs to be hydrophilic. In addition, if the entire coating becomes hydrophilic, moisture will easily penetrate into the coating, and water will penetrate or swell at the interface between the coating and the coated object, which will cause concerns about the durability of the coating itself.

[0004] In addition, when imparting hydrophilicity to existing coating agents, etc., improvements are required from the curable resin component, and a major review is required. In some cases, hydrophilicity is imparted by overcoating a coating formed by a non-hydrophilic coating agent, etc. with a hydrophilic coating agent, etc. In this case, however, since the coating formed by the non-hydrophilic coating agent, etc. and the coating formed by the hydrophilic coating agent, etc. are in a laminated state, the coating is likely to come off due to interlayer peeling, and there is a problem that it is difficult to obtain weather resistance. In addition, the gradual peeling causes changes in the surface shape of the coating, resulting in poor appearance such as a decrease in gloss.

[0005] In recent years, there has been a strong demand for hydrophilic agents in baking coatings, and examples of applications include outdoor storage sheds and pre-coated metal roofs, etc. These require long-term weather resistance of the coating.

[0006] On the other hand, when a surface conditioner is used to impart hydrophilicity, adding a small amount to an existing coating agent can make the exposed surface of the coating hydrophilic without changing the physical properties required for the coating, such as the durability and hardness of the formed coating.

[0007] As a surface conditioner that imparts hydrophilicity to the coating, silicates, such as ethyl silicate, which exhibit hydrophilicity through hydrolysis, are often used. In this case, hydrolysis takes about 2 to 3 months. After hydrophilicity is exhibited, it is possible to maintain the hydrophilicity for a long period of time, but long-term hydrophilicity may reduce the durability of the coating itself because moisture gradually penetrates into the coating.

[0008] Problems with coating agents using such surface conditioners include the tendency for problems with stability over time after addition, such as gelation of the surface conditioner itself and thickening of the coating agent due to crosslinking with the resin. In addition, hydrolysis due to moisture in the air can cause the surface conditioner itself to become highly polarized, resulting in loss of surface orientation and a decline in hydrophilic performance.

[0009] In some cases, a surface conditioner containing polyalkylene oxide as a hydrophilic segment is used. This surface conditioner can exhibit hydrophilicity from the initial stage of film formation, but in the case of high-temperature baking such as baking paint, the performance tends to decrease due to thermal decomposition or hydrolysis due to the low heat resistance of polyalkylene oxide.

[0010] Patent Document 1 discloses a surface conditioner containing a copolymer of a siloxy group-containing mono(meth)acrylate monomer and an acrylamide monomer as a surface conditioner that exhibits hydrophilicity from the early stage of film formation and has good heat resistance. This surface conditioner can reduce the static contact angle of water on the surface of the film from the early stage of film formation and exhibit high hydrophilicity. However, while it exhibits high hydrophilicity from the early stage of film formation, it exhibits good antifouling properties due to self-cleaning in the early stage of film formation when exposed to the film, but in order to improve the surface tension of the film, it is easy for dirt components in the atmosphere to be adsorbed, and there is a concern that if such dirt accumulates, it will become difficult to maintain hydrophilicity and antifouling properties. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Patent No. 5437523 Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention has been made to solve the above-mentioned problems, and aims to provide a surface conditioner for addition to a coating film-forming liquid agent, which, when added in a small amount to a coating film-forming liquid agent such as a paint or coating agent that forms a film, imparts leveling properties to the exposed surface of the formed paint coating film, and hydrophilicity only when water adheres to the paint coating film, such that the static contact angle of water on the paint coating film is not reduced, but only the receding contact angle is reduced in the expansion and contraction method of water contact angle measurement, thereby providing long-term antifouling properties due to self-cleaning when the paint coating film is exposed outdoors, a coating film-forming liquid agent containing the same, and a paint coating film obtained by the same. [Means for solving the problem]

[0013] In order to achieve the above object, the present invention provides a surface conditioner for adding to a coating film forming solution, which is represented by the following chemical formula (I): [ka] (In formula (I), R 1 is a hydrogen atom or a methyl group, R 2 is an alkylene group having 1 to 10 carbon atoms, R 3 represents an alkyl group having 1 to 12 carbon atoms, and m represents a number from 2 to 150. and under Chemical formula (II) [ka] (In formula (II), R 4 is a hydrogen atom or a methyl group, R 5 is an alkylene group having 2 to 10 carbon atoms, R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, and X represents a halogen atom. and A copolymer repeating unit (c) of at least any one of functional group-containing comonomers selected from a blocked isocyanate group-containing (meth)acrylate monomer, an alkoxysilane group-containing (meth)acrylate monomer, and a hydroxyl group-containing (meth)acrylate monomer; The weight average molecular weight is 1500 to 100,000. It does not contain any copolymer repeating units of (meth)acrylamide monomers and does not contain any segments that are polyalkylene oxides. Contains a copolymer, the total mass ratio of the copolymer repeating unit (a) to the copolymer repeating unit (b) in the copolymer is 0.1 to 20.0 and 99.9 to 80.0, the copolymer repeating unit (c) is at most 10 parts by mass per 100 parts by mass of the total weight of the copolymer repeating unit (a) and the copolymer repeating unit (b); It provides hydrophilicity to the exposed surface of the paint coating film.

[0014] This surface conditioner for addition to a coating film forming liquid agent contains the copolymer having copolymerization repeating units (c) of at least any functional group-containing comonomer selected from a blocked isocyanate group-containing (meth)acrylate monomer, an alkoxysilane group-containing (meth)acrylate monomer, a hydroxyl group-containing (meth)acrylate monomer, and a hydroxyl group-containing (meth)acrylamide monomer, and the amount of the copolymerization repeating units (c) may be at most 10 parts by mass per 100 parts by mass of the total weight of the copolymerization repeating units (a) and (b).

[0015] The coating film-forming solution of the present invention, which has been made to achieve the above object, contains the above-mentioned surface conditioner for addition to the coating film-forming solution, and a film-forming component.

[0016] The paint coating film of the present invention, which has been made to achieve the above object, is a coating film of the above coating film forming liquid agent, which is formed on a substrate.

[0017] It is preferable that the paint coating film has antifouling properties on the exposed surface of the paint coating film due to the hydrophilicity. Effect of the Invention

[0018] The surface conditioner for addition to a coating film-forming liquid agent of the present invention is blended in a small amount into a coating film-forming liquid agent such as a paint or coating agent that forms a film, and the small amount becomes compatible with the entire system. During the film-forming process, the surface conditioner is oriented toward the exposed surface of the painted coating film and becomes highly concentrated on the exposed surface of the painted coating film, so that even a small blend amount can exhibit a high hydrophilicity-imparting effect.

[0019] According to the surface conditioner for adding to a coating film-forming liquid agent of the present invention, by adding a small amount to a coating film-forming liquid agent, for example, a paint or coating agent for baking that is cured at high temperature, it is possible to impart leveling properties and hydrophilicity that reduces the receding contact angle in the expansion and contraction method, which is a type of water contact angle measurement method, to the exposed surface of the formed film. As a result, it is possible to impart long-term antifouling properties to the exposed surface of the film by self-cleaning when the film is exposed outdoors.

[0020] In addition, by imparting hydrophilicity only when water adheres to the coating film, such as by reducing only the receding contact angle in water contact angle measurement without reducing the static contact angle of water on the paint coating film, adhesion of dirt components to the exposed surface of the film when dried is reduced, and anti-fouling properties can be achieved by improving the washability with water such as rainwater and the self-cleaning function.

[0021] The coating film forming solution of the present invention contains a surface conditioner for addition to the coating film forming solution that has a high orientation to the interface, and exerts leveling properties due to the effect of uniforming the surface tension, thereby minimizing defects on the exposed coating surface such as uneven coating and citrus peel.

[0022] The coating film of the present invention, which is a coating film of the above-mentioned coating film-forming liquid agent, can exhibit hydrophilicity on its exposed surface only when water is present on the exposed surface of the film, and is less susceptible to adsorption of fouling substances to the film when it dries, thereby exhibiting long-term antifouling properties.

[0023] Furthermore, this paint coating film does not cause uneven painting when a top coat is applied, and the paint coating film and the top coat layer can be firmly adhered to each other without reducing the adhesion between them. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, embodiments for carrying out the present invention will be described in detail, but the scope of the present invention is not limited to these embodiments.

[0025] The surface conditioner for addition to a coating film forming solution of the present invention contains a copolymer having a copolymer repeating unit (a) having a polysiloxane skeleton represented by the above chemical formula (I) and a copolymer repeating unit (b) having an ammonium cation group represented by the above chemical formula (II). This copolymer has a weight average molecular weight of 1500 to 100000, and the total mass ratio of the copolymer repeating unit (a) to the copolymer repeating unit (b) in the copolymer is 0.1 to 20.0 and 99.9 to 80.0.

[0026] The weight-average molecular weight of this copolymer is more preferably 3000 to 50000. If the weight-average molecular weight is less than 1500, bubbles are likely to occur when the copolymer is added to a paint or coating agent and then applied, whereas if it exceeds 100000, the orientation to the coating film surface decreases, making it impossible to obtain sufficient hydrophilicity.

[0027] The copolymer repeating unit (a) having a polysiloxane skeleton is preferably 0.1 to 20.0 parts by mass, and more preferably 1 to 10 parts by mass, in a total of 100 parts by mass of the copolymer repeating unit (a) and the copolymer repeating unit (b).

[0028] The copolymer repeating unit (b) having an ammonium cationic group is preferably 99.9 to 80.0 parts by mass, more preferably 99 to 90 parts by mass, in the total of 100 parts by mass of the copolymer repeating unit (a) and the copolymer repeating unit (b). If the copolymer repeating unit (b) is less than 80 parts by mass, sufficient hydrophilicity cannot be exhibited. In addition, when added to a paint or coating agent, compatibility with other components therein becomes extremely poor, causing repelling during application or dents on the coating surface, and worsening the leveling property of the topcoat, making it impossible to obtain sufficient topcoat adhesion.

[0029] The copolymer repeating unit (a) having a polysiloxane skeleton in the copolymer can be obtained by using a mono(meth)acrylate monomer having one terminal (meth)acryl-modified, represented by the following chemical formula (III).

[0030] [ka] (In formula (III), R 7 is a hydrogen atom or a methyl group, R 8 is an alkylene group having 1 to 10 carbon atoms, R 9 represents an alkyl group having 1 to 12 carbon atoms, and n is a number from 2 to 150.

[0031] For example, one-terminated (meth)acrylic monomers such as Silaplane FM-0711, Silaplane FM-0721, Silaplane FM-0725 (all product names of JNC Corporation; Silaplane is a registered trademark of JNC Corporation), KF-2012, X-22-2426, and X-22-2475 (all product names of Shin-Etsu Chemical Co., Ltd.) can be used.

[0032] The repeating unit (b) having an ammonium cationic group in the copolymer is preferably a repeating unit (b) having a quaternary ammonium cationic group. The repeating unit (b) having a quaternary ammonium cationic group in the copolymer can be obtained by using, for example, DMAPAA-Q (product name of KJ Chemicals Co., Ltd.), Acrylate DMC (product name of Mitsubishi Chemical Co., Ltd.), or Light Ester DQ-100 (product name of Kyoeisha Chemical Co., Ltd.).

[0033] Also usable is a (meth)acrylate monomer having a tertiary amine structure represented by the following chemical formula (IV).

[0034] [ka] (In formula (IV), R 10 is a hydrogen atom or a methyl group, R 11 is an alkylene group having 2 to 10 carbon atoms, R 12 each independently represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms.

[0035] Examples of (meth)acrylate monomers having a tertiary amine structure include DMAPAA (product name of KJ Chemicals Co., Ltd.), Acryester DM, Acryester DE (product name of Mitsubishi Chemical Corporation), Aron DA (product name of Toagosei Co., Ltd.), and Light Ester DM (product name of Kyoeisha Chemical Co., Ltd.).

[0036] The amines of these tertiary amine-containing (meth)acrylate monomers are converted into quaternary salts using an alkyl halide represented by the following chemical formula (V).

[0037] [ka] (In formula (V), X is an iodine atom, a bromine atom, or a chlorine molecule; R 13 represents an alkylene group having 4 to 16 carbon atoms.

[0038] The alkyl halide may be, for example, 1-chlorobutane, 1-chloropentane, 1-chlorohexane, 1-chloroheptane, 1-chlorooctane, 1-chlorononane, 1-chlorodecane, 1-chloroundecane, 1-chlorododecane, 1-chlorotridecane, 1-chlorotetradecane, 1-chloropentadecane, 1-chlorohexadecane, 1-bromobutane, 1-bromopentane, 1-bromohexane, 1-bromoheptane, 1-bromooctane, 1-bromononane, 1-bromo Examples of the iodoalkyl include decane, 1-bromoundecane, 1-bromododecane, 1-bromotridecane, 1-bromotetradecane, 1-bromopentadecane, 1-bromohexadecane, 1-iodobutane, 1-iodopentane, 1-iodohexane, 1-iodoheptane, 1-iodooctane, 1-iodononane, 1-iododecane, 1-iodoundecane, 1-iodododecane, 1-iodotridecane, 1-iodotetradecane, 1-iodopentadecane, and 1-iodohexadecane.

[0039] The copolymer in the surface conditioner for adding to the coating film forming liquid agent may have not only the copolymer repeating unit (a) and the copolymer repeating unit (b) as the repeating unit constituting the copolymer, but also other copolymer repeating units. For example, the copolymer may be a copolymer containing the copolymer repeating unit (a) and the copolymer repeating unit (b), and may further contain a copolymer repeating unit (c) of at least any functional group-containing comonomer selected from a blocked isocyanate group-containing (meth)acrylate monomer, an alkoxysilane group-containing (meth)acrylate monomer, a hydroxyl group-containing (meth)acrylate monomer, and a hydroxyl group-containing (meth)acrylamide monomer.

[0040] The copolymer repeating unit (c) is preferably 10 parts by mass or less relative to 100 parts by mass of the total weight of the copolymer repeating unit (a) and the copolymer repeating unit (b). This makes it more difficult for the surface conditioner for adding to the coating film forming liquid agent to be dissolved by rainwater, which is advantageous for antifouling properties, when added to a coating film forming liquid agent such as a paint or a coating agent and used, to react with the resin, which is a film forming component in the coating film forming liquid agent, on the exposed surface of the paint coating film formed thereby. If it exceeds 10 parts by mass, there is a risk of impairing the original performance. These functional group-containing comonomers may be used alone or in combination as long as the total weight is equal to or less than the specified blending amount.

[0041] The blocked isocyanate group-containing (meth)acrylate monomer is a blocked isocyanate group-containing (meth)acrylate, and examples thereof include a monomer obtained by reacting a (meth)acrylate monomer having an isocyanate group with a blocking agent selected from ethyl alcohol, isopropyl alcohol, caprolactam, methyl ethyl ketone-oxime, dimethylpyrazole, and diethyl malonate.

[0042] Examples of alkoxysilane group-containing (meth)acrylate monomers include 3-methacryloxypropyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyldimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyldiethoxysilane, and 3-acryloxypropyltriethoxysilane.

[0043] The hydroxyl group-containing (meth)acrylate monomer is a hydroxyl group-containing (meth)acrylate, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and the like.

[0044] The hydroxyl group-containing (meth)acrylamide monomer is a hydroxyl group-containing (meth)acrylamide, such as N-hydroxyethylacrylamide, N-hydroxymethylacrylamide, or the like.

[0045] Furthermore, the surface conditioner for addition to the coating film forming solution of the present invention may contain at least one repeating copolymer unit (d) of a comonomer selected from alkyl (meth)acrylates, (meth)acrylamides, and vinyl group-containing compounds in the copolymer, so long as it does not impair the hydrophilicity imparting performance of the agent. This can improve the leveling property of the coating film and suppress popping during baking and curing of the coating film.

[0046] The copolymer repeating unit (d) is preferably at most 10 parts by mass per 100 parts by mass of the total weight of the copolymer repeating unit (a) and the copolymer repeating unit (b), or the copolymer repeating unit (a), the copolymer repeating unit (b), and the copolymer repeating unit (c). If the amount exceeds 10 parts by mass, the inherent performance may be impaired. The above comonomers may be used alone or in combination as long as the total weight is equal to or less than the prescribed blending amount.

[0047] The alkyl (meth)acrylates are alkyl (meth)acrylate monomers, for example, alkyl acrylates or alkyl methacrylates, specifically methyl (meth)acrylate, ethyl (meth)acrylate, normal propyl (meth)acrylate, isopropyl (meth)acrylate, normal butyl (meth)acrylate, isobutyl (meth)acrylate, tertiary butyl (meth)acrylate, normal octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate. Examples of the acrylates include acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, dodecyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, 2-acryloyloxyethyl succinic acid, and 2-acryloyloxyethyl phthalic acid.

[0048] Examples of (meth)acrylamides include dimethyl(meth)acrylamide, dimethylaminopropyl(meth)acrylamide, isopropyl(meth)acrylamide, hydroxyethylacrylamide, (meth)acryloylmorpholine, (meth)acrylamide-tert-butylsulfonic acid, (meth)acrylamide-tert-butylsulfonic acid organic salts, and (meth)acrylamide-tert-butylsulfonic acid inorganic salts.

[0049] Incidentally, (meth)acrylic means acrylic or methacrylic.

[0050] Examples of the vinyl group-containing compound include linear, branched, or cyclic alkyl vinyl ether monomers having 1 to 12 carbon atoms, such as normal butyl vinyl ether, isobutyl vinyl ether, tertiary butyl vinyl ether, cyclohexyl vinyl ether, and lauryl vinyl ether; and vinyl ester monomers, such as vinyl acetate, vinyl propionate, and vinyl laurate.

[0051] The surface conditioner for addition to a coating film-forming solution of the present invention may consist of only the copolymer, or may be a mixture of an inert solvent, the copolymer, and, if necessary, additives, dissolved or suspended therein.

[0052] The inert solvent is preferably one that can dissolve or suspend the copolymer and can be mixed with the coating agent.Specific examples include hydrocarbon solvents such as xylene, toluene, and cyclohexane, ketone solvents such as cyclohexanone and methyl isobutyl ketone, ether solvents such as methyl cellosolve, cellosolve, butyl cellosolve, methyl carbitol, carbitol, butyl carbitol, diethyl carbitol, and propylene glycol monomethyl ether, ester solvents such as n-butyl acetate, isobutyl acetate, n-amyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate, and alcohol solvents such as n-butyl alcohol, sec-butyl alcohol, isobutyl alcohol, cyclohexanol, 2-ethylhexanol, and 3-methyl-3-methoxybutanol.These solvents may be used alone or in combination.

[0053] This surface conditioner for addition to a coating film-forming solution is prepared as follows.

[0054] A siloxy group-containing (meth)acrylate monomer as the comonomer (A) forming the copolymer repeat unit (a) and a (meth)acrylate monomer having a tertiary amine structure as the comonomer (B) forming the copolymer repeat unit (b) are randomly copolymerized in a suitable solvent in the presence of a radical polymerization initiator and, if necessary, a chain transfer agent to synthesize a copolymer. The polymerization method for this copolymer is not limited to radical polymerization. This copolymer may be a block copolymer or a graft copolymer. Next, an alkyl halide is appropriately dropped into the obtained copolymer to form a quaternary ammonium cation in the copolymer, thereby preparing a surface conditioner for addition to a coating film forming liquid agent. Furthermore, the surface conditioner for addition to a coating film forming liquid agent may be prepared by mixing the obtained copolymer with an inert solvent.

[0055] Furthermore, when the copolymer contained in the surface conditioner for addition to the coating film forming liquid agent contains copolymerization repeating unit (c) or copolymerization repeating unit (b) in addition to the copolymerization repeating unit (a) and the copolymerization repeating unit (b), the copolymer can be obtained by copolymerizing a functional group-containing comonomer (C) which forms copolymerization repeating unit (c) together with the comonomer (A) and the comonomer (B) or a comonomer (D) which forms copolymerization repeating unit (d).

[0056] The coating film forming solution of the present invention contains a surface conditioner for addition to the coating film forming solution and a film forming component, and is prepared by mixing the coating film forming solution in advance, adding the surface conditioner for addition to the coating film forming solution, and kneading the mixture. They may be mixed simultaneously or in any order.

[0057] The coating film forming solution preferably contains the above-mentioned surface conditioner for addition to the coating film forming solution in an amount of 0.1 to 10 mass %, preferably 0.5 to 5.0 mass %, calculated as solid content based on the total amount of the coating film forming solution.

[0058] Examples of the resin that is a film-forming component include acrylic resins, polyester resins, urethane resins, alkyd resins, epoxy resins, amino resins, etc. This resin may be one that cures with a chemical reaction in the presence or absence of a catalyst, such as heat-curing type, ultraviolet-curing type, electron beam-curing type, oxidation-curing type, photocation-curing type, peroxide-curing type, and acid / epoxy-curing type, or it may be a resin with a high glass transition point that cures without a chemical reaction by simply volatilizing the solvent.

[0059] The coating film-forming solution may consist of only the surface conditioner for addition to the coating film-forming solution and the film-forming component, or may contain other components.

[0060] The components contained in the coating film forming solution are not particularly limited, and examples thereof include colorants such as pigments and dyes, resins, diluting solvents, catalysts, and surfactants. In addition, sensitizers, antistatic agents, defoamers, dispersants, and viscosity modifiers may also be contained as necessary.

[0061] The dilution solvent is not particularly limited as long as it is water or an organic solvent that is generally used, but examples of the organic solvent include hydrocarbon solvents such as xylene, toluene, and cyclohexane; ketone solvents such as cyclohexanone and methyl isobutyl ketone; ether solvents such as methyl cellosolve, cellosolve, butyl cellosolve, methyl carbitol, carbitol, butyl carbitol, diethyl carbitol, and propylene glycol monomethyl ether; ester solvents such as n-butyl acetate, isobutyl acetate, n-amyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate; and alcohol solvents such as n-butyl alcohol, sec-butyl alcohol, isobutyl alcohol, cyclohexanol, 2-ethylhexanol, and 3-methyl-3-methoxybutanol. These solvents may be used alone or in combination.

[0062] The paint coating film of the present invention is a paint film, which is formed by applying or painting a coating film-forming liquid agent on a substrate and then drying or curing the surface of the paint film.

[0063] The substrate is not particularly limited, but may be formed from a material such as plastic, rubber, paper, wood, glass, metal, stone, cement, mortar, or ceramic, and examples of the substrate include exterior materials for home appliances and automobiles, daily necessities, and building materials.

[0064] Examples of the application or coating method include spin coating, slit coating, spray coating, dip coating, bar coating, doctor blade, roll coating, and flow coating. EXAMPLES

[0065] Examples of the present invention will be described in detail below, but the scope of the present invention is not limited to these examples.

[0066] Examples of the preparation of surface conditioners for addition to coating film-forming solutions to which the present invention is applied are shown below in Examples 1 to 9, and examples of the preparation of surface conditioners for addition to coating film-forming solutions to which the present invention is not applied are shown below in Comparative Examples 1 to 6.

[0067] Example 1 100 parts by mass of n-butyl alcohol was added to a 1000 mL reaction vessel equipped with a stirrer, reflux condenser, dropping funnel, thermometer, and nitrogen gas inlet, and the temperature was raised to 110°C under a nitrogen gas atmosphere. The temperature of n-butyl alcohol was maintained at 110°C, and the dropping solution (a-1) shown in Table 1 below was dropped at a constant rate using the dropping funnel over 3 hours to prepare a monomer solution. After the drop was completed, the monomer solution was reacted at 110°C for 2 hours to synthesize a copolymer. The copolymer was eluted by molecular weight using gel permeation chromatography (column: TSKgel SuperAWM-H, manufactured by Tosoh Corporation, elution solvent: DMF, same below) capable of separating molecules of different molecular weights, and the molecular weight distribution was obtained. A calibration curve was obtained in advance from a polystyrene standard substance with a known molecular weight, and the weight average molecular weight of the copolymer was obtained by comparing it with the molecular weight distribution of the copolymer. As a result, the weight average molecular weight of the copolymer was 4000 in terms of polystyrene. The obtained copolymer was then heated to 110°C, and the additional dropping solution (a'-1) shown in Table 2 below was added dropwise at a constant rate for 1 hour. After the dropwise addition was completed, the mixture was reacted at 110°C for 2 hours to obtain a surface conditioner for addition to a coating film forming solution having a quaternary ammonium cation in the copolymer.

[0068] Example 2 A copolymer was obtained in the same manner as in Example 1, except that the dropping solution in Example 1 was changed to (a-2). The weight average molecular weight of the copolymer of the surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 12,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Example 1, except that the additional dropping solution in Example 1 was changed to (a'-2).

[0069] Example 3 A copolymer was obtained in the same manner as in Example 1, except that the dropping solution in Example 1 was changed to (a-3). The weight average molecular weight of the copolymer of the surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 45,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Example 1, except that the additional dropping solution in Example 1 was changed to (a'-3).

[0070] Example 4 A copolymer was obtained in the same manner as in Example 1, except that the dropping solution in Example 1 was changed to (a-4). The weight average molecular weight of the copolymer of the surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 13,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Example 1, except that the additional dropping solution in Example 1 was changed to (a'-4).

[0071] Example 5 A copolymer was obtained in the same manner as in Example 1, except that the dropping solution in Example 1 was changed to (a-5). The weight average molecular weight of the copolymer of the surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 11,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Example 1, except that the additional dropping solution in Example 1 was changed to (a'-5).

[0072] Example 6 A copolymer was obtained in the same manner as in Example 1, except that the dropping solution in Example 1 was changed to (a-6). The weight average molecular weight of the copolymer of the surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 10,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Example 1, except that the additional dropping solution in Example 1 was changed to (a'-6).

[0073] Example 7 A copolymer was obtained in the same manner as in Example 1, except that the dropping solution in Example 1 was changed to (a-7). The weight average molecular weight of the copolymer of the surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 10,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Example 1, except that the additional dropping solution in Example 1 was changed to (a'-7).

[0074] Example 8 A copolymer was obtained in the same manner as in Example 1, except that the dropping solution in Example 1 was changed to (a-8). The weight average molecular weight of the copolymer of the surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 11,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Example 1, except that the additional dropping solution in Example 1 was changed to (a'-8).

[0075] Example 9 A copolymer was obtained in the same manner as in Example 1, except that the dropping solution in Example 1 was changed to (a-9). The weight average molecular weight of the copolymer of the surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 12,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Example 1, except that the additional dropping solution in Example 1 was changed to (a'-9).

[0076] [Table 1]

[0077] [Table 2]

[0078] Comparative Example 1 100 parts by mass of n-butyl alcohol was added to a 1000 mL reaction vessel equipped with a stirrer, reflux condenser, dropping funnel, thermometer, and nitrogen gas inlet, and the temperature was raised to 110°C under a nitrogen gas atmosphere. The temperature of n-butyl alcohol was maintained at 110°C, and the dropping solution (b-1) shown in Table 3 below was dropped at a constant rate using the dropping funnel over 3 hours to prepare a monomer solution. After the dropping was completed, the monomer solution was reacted at 100°C for 2 hours to synthesize a copolymer. The copolymer was eluted by molecular weight using gel permeation chromatography (column: TSKgel SuperAWM-H, manufactured by Tosoh Corporation, elution solvent: DMF, same below) that can separate molecules of different molecular weights, and the molecular weight distribution was obtained. A calibration curve was obtained in advance from a polystyrene standard substance with a known molecular weight, and the weight average molecular weight of the copolymer was obtained by comparing it with the molecular weight distribution of the copolymer. As a result, the weight average molecular weight of the copolymer was 110,000 in polystyrene equivalent. The obtained copolymer was then heated to 110°C, and the additional dropping solution (b'-1) shown in Table 4 below was added dropwise at a constant rate for 1 hour. After the dropwise addition was completed, the mixture was reacted at 110°C for 2 hours to obtain a surface conditioner for addition to a coating film forming solution having a quaternary ammonium cation in the copolymer.

[0079] Comparative Example 2 A copolymer was obtained in the same manner as in Comparative Example 1, except that the dropping solution in Comparative Example 1 was changed to (b-2) and the reaction temperature was changed to 110°C. The weight average molecular weight of the copolymer of this surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 11,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Comparative Example 1, except that the additional dropping solution in Comparative Example 1 was changed to (b'-2).

[0080] Comparative Example 3 A copolymer was obtained in the same manner as in Comparative Example 1, except that the dropping solution in Comparative Example 2 was changed to (b-3). The weight average molecular weight of this copolymer of the surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 13,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Comparative Example 1, except that the additional dropping solution in Comparative Example 1 was changed to (b'-3).

[0081] Comparative Example 4 A copolymer was obtained in the same manner as in Comparative Example 1, except that the dropping solution in Comparative Example 2 was changed to (b-4). The weight average molecular weight of the copolymer of the surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 12,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Comparative Example 1, except that the additional dropping solution in Comparative Example 1 was changed to (b'-4).

[0082] Comparative Example 5 A copolymer was obtained in the same manner as in Comparative Example 1, except that the dropping solution in Comparative Example 2 was changed to (b-5). The weight average molecular weight of the copolymer of the surface conditioner for adding to a coating film forming solution, determined by gel permeation chromatography, was 14,000 in terms of polystyrene. In addition, a surface conditioner for adding to a coating film forming solution having a quaternary ammonium cation in the copolymer was obtained in the same manner as in Comparative Example 1, except that the additional dropping solution in Comparative Example 1 was changed to (b'-5).

[0083] Comparative Example 6 A copolymer was obtained in the same manner as in Comparative Example 1, except that the dropping solution in Comparative Example 2 was changed to (b-6). The weight average molecular weight of this copolymer of the surface conditioner for addition to a coating film forming solution, determined by gel permeation chromatography, was 12,000 in terms of polystyrene. No additional dropping was performed.

[0084] Comparative Example 7 A copolymer was obtained in the same manner as in Comparative Example 1, except that the dropping solution in Comparative Example 2 was changed to (b-7). The weight average molecular weight of this copolymer of the surface conditioner for addition to a coating film forming solution, determined by gel permeation chromatography, was 11,000 in terms of polystyrene. No additional dropping was performed.

[0085] [Table 3]

[0086] [Table 4]

[0087] (Preparation of paint for preparation) Glass beads were added to a mill base blend of 324 parts by mass of Beckolite 46-118 (polyester polyol resin, non-volatile content: 60%, manufactured by DIC Corporation) and 270 parts by mass of titanium oxide (Typake CR93, manufactured by Ishihara Sangyo Kaisha, Ltd.), and the mixture was stirred for 6 hours using a paint shaker. Further, 1000 parts by mass of letdown was added to 594 parts by mass of this mill base, which was made by adding 135 parts by mass of Beckolite 46-118 (polyester polyol resin, non-volatile content: 60%, manufactured by DIC Corporation), 22 parts by mass of Amidea L-117-60 (butylated melamine resin, NV60%, manufactured by DIC Corporation), 45 parts by mass of Amidea L-105-60 (methylated melamine resin, NV60%, manufactured by DIC Corporation), and 204 parts by mass of thinner (Solvesso 150 / cyclohexanone = 50 / 50), and the glass beads were filtered off.

[0088] (Preparation of test paints and coatings) To the obtained preparation paint, 0.5% of an antifoaming agent (Floren AC-300, manufactured by Kyoeisha Chemical Co., Ltd.) and the surface conditioner for adding to the coating film forming liquid obtained in Examples 1 to 9 and Comparative Examples 1 to 7 were added at a solid content rate of 1.5%, and the mixture was stirred in a Lab-Dyspar at 2000 rpm for 2 minutes to obtain a test paint, which is a baked polyester paint. The obtained test paint was immediately applied to a substrate with a #42 bar coater, and immediately baked and cured at 245°C for 60 seconds (PMT: 225°C) to obtain a cured coating film, which is a paint coating film.

[0089] (Measurement of water contact angle of cured coating film) The receding contact angle was measured on the coating surface immediately after curing using a contact angle meter with a 20 μL water droplet by the expansion and contraction method. The lower the value, the higher the hydrophilicity of the cured film. The measurement results are shown in Table 5 below. Measurement equipment: Contact angle measuring meter (manufactured by Kyowa Interface Science Co., Ltd.)

[0090] (Evaluation of leveling properties of cured coating film) The surface condition of the cured coating was visually observed and evaluated according to the following criteria. The results are shown in Table 5 below. Leveling performance evaluation criteria ○: No or very few bar coater paint streaks remain △: Paint streaks from the bar coater remain ×: Defective, cissing occurs

[0091] (Actual exposure evaluation of cured coating film) The cured coated panels were bent at 45° and stood vertically, facing south outdoors, and exposed for three months. The degree of staining was then visually evaluated according to the following criteria. The evaluation results are shown in Table 5 below. Contamination assessment criteria ○: Almost no contamination, good △: Slightly contaminated ×: Severely contaminated and defective

[0092] [Table 5]

[0093] As is clear from Table 5, the cured coating films of Examples 1 to 9 had lower receding water contact angle values ​​and also had good evaluations in the leveling property and field exposure test compared to the cured coating films of Comparative Examples 1 to 7. On the other hand, the cured coating films of Comparative Examples 1 to 7 did not receive a good evaluation in the field exposure test and had insufficient antifouling properties. [Industrial Applicability]

[0094] The surface conditioner for addition to a coating film-forming liquid agent of the present invention can be added to a coating film-forming liquid agent such as a paint or coating agent that is applied or painted on the surface of a coated object such as exterior materials for home appliances and automobiles, daily necessities, and building materials made of materials such as plastic, rubber, paper, wood, glass, metal, stone, cement, mortar, and ceramics.

[0095] The paint coating film formed on a substrate using this coating film forming liquid agent containing a surface conditioner for addition to the coating film forming liquid agent and a film forming component exhibits hydrophilicity on the exposed surface of the paint coating film, and is therefore provided with antifouling properties, making it useful as a coating film for various substrates.

Claims

1. The following chemical formula (I) 【Chemistry 1】 (In formula (I), R 1 is a hydrogen atom or a methyl group, R 2 is an alkylene group having 1 to 10 carbon atoms, R 3 represents an alkyl group having 1 to 12 carbon atoms, and m represents a number from 2 to 150. The following chemical formula (II) 【Chemistry 2】 (In formula (II), R 4 is a hydrogen atom or a methyl group, R 5 is an alkylene group having 2 to 10 carbon atoms, R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, and X represents a halogen atom; and (c) copolymerization repeating units of at least any functional group-containing comonomer selected from a blocked isocyanate group-containing (meth)acrylate monomer, an alkoxysilane group-containing (meth)acrylate monomer, and a hydroxyl group-containing (meth)acrylate monomer, the copolymer having a weight average molecular weight of 1,500 to 100,000, not containing copolymerization repeating units of a (meth)acrylamide monomer, and not containing a polyalkylene oxide segment; the total mass ratio of the copolymer repeating unit (a) to the copolymer repeating unit (b) in the copolymer is 0.1 to 20.0 and 99.9 to 80.0, the copolymer repeating unit (c) is at most 10 parts by mass per 100 parts by mass of the total weight of the copolymer repeating unit (a) and the copolymer repeating unit (b); A surface conditioner for addition to a coating film forming solution, characterized in that it imparts hydrophilicity to the exposed surface of a paint coating film.

2. A coating film-forming solution, comprising the surface conditioner for addition to the coating film-forming solution according to claim 1 and a film-forming component.

3. A coating film, which is a coating film of the coating film forming solution according to claim 2 and is formed on a substrate.

4. 4. The paint coating film according to claim 3, characterized in that the exposed surface of the paint coating film has antifouling properties due to the hydrophilicity.

Citation Information

Patent Citations

  • Preventive system for double recording of magnetic recordinggregenerating device

    JP1979037523A

  • Surface-modifier

    JP2001011426A

  • Surface conditioner

    JP2014224219A

  • Surface conditioning agent, coating material composition containing said surface conditioning agent, and coating film forming method

    WO2018097012A1