Non-magnetic member, its manufacturing method, and electric device and its field element
A titanium-based composite material with TiCy reinforcing particles addresses the challenge of eddy current loss and mechanical integrity in electromagnetic members by providing high specific resistance and rigidity, ensuring stability under high rotational speeds.
Patent Information
- Application Number
- JP2018172004
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2018-09-14
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2038-09-14
AI Technical Summary
Existing electromagnetic members used in alternating magnetic fields face challenges in reducing eddy current loss and maintaining mechanical integrity under high rotational speeds, particularly when constructed from materials like carbon fiber reinforced plastic (CFRP), which lack sufficient mechanical properties.
Employing a titanium-based composite material with TiCy reinforcing particles dispersed in a titanium alloy matrix, which provides high specific resistance, rigidity, and strength, thereby reducing eddy current loss and preventing deformation or damage from centrifugal forces.
The titanium-based composite material effectively suppresses eddy current loss and maintains structural integrity even at high rotational speeds, ensuring the mechanical stability of permanent magnets and reducing the risk of damage.
Smart Images

Figure 0007576387000002 
Figure 0007576387000003 
Figure 0007576387000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-magnetic member or the like used in an alternating magnetic field. [Background technology]
[0002] There are various types of equipment that utilize electromagnetism (simply referred to as "electromagnetic equipment"), such as electric motors (including generators as well as motors) and actuators, and many of these equipment utilize alternating magnetic fields. In order to save energy, such electromagnetic equipment is required to reduce high-frequency losses when used in an alternating magnetic field. In particular, in electric motors that rotate at (ultra-) high speeds, there is a strong demand to reduce eddy current losses, which increase in proportion to the square of the rotation speed (frequency of the alternating magnetic field). For this reason, for example, the rotor cores and stator cores of motors are often constructed by laminating electromagnetic steel sheets coated with an insulating layer that suppresses eddy currents that occur in the direction perpendicular to the alternating magnetic field.
[0003] However, for some components (simply referred to as "electromagnetic components") that are used in alternating magnetic fields, it is difficult to adopt such a configuration. In such cases, it is necessary to construct the electromagnetic components from a material with high electrical resistivity (simply referred to as "resistivity") to reduce eddy current loss.
[0004] The electromagnetic components disposed in the magnetic circuit are not limited to magnetic materials, and may be non-magnetic materials. Furthermore, the electromagnetic components may be required to satisfy not only electrical characteristics (e.g., resistivity) and magnetic characteristics (e.g., magnetic permeability), but also certain mechanical characteristics (rigidity, strength, ductility, etc.). The following patent documents contain descriptions related to such electromagnetic components: [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-339886 A [Patent Document 2] JP 2008-29153 A Summary of the Invention
Problems to be Solved by the Invention
[0006] In the above patent document, as an example of an electromagnetic member made of a non-magnetic material (simply referred to as a "non-magnetic member"), there is a description of a protective tube (sleeve) made of carbon fiber reinforced plastic (CFRP). The protective tube is fitted on the outer peripheral side of a cylindrical permanent magnet provided on the outer peripheral side of the rotor shaft (rotating shaft) of a motor. The protective tube prevents damage to the permanent magnet on which a large centrifugal force acts during high-speed rotation. However, when the rotational speed is further increased, the mechanical properties of the protective tube made of CFRP are not always sufficient.
[0007] The present invention has been made in view of such circumstances, and an object thereof is to provide a new non-magnetic member and the like different from the conventional ones.
Means for Solving the Problems
[0008] As a result of intensive research by the present inventor to solve this problem, it has been newly found that a titanium-based composite material having TiCy (0 < y < 1) as reinforcing particles exhibits not only high strength and high rigidity but also high specific resistance, which is an unknown attribute. With the idea of using this titanium-based composite material as a non-magnetic member and embodying and developing it, the present invention described below has been completed.
[0009] 《Non-Magnetic Member》 (1) The present invention is a non-magnetic member used in an alternating magnetic field, which is made of a titanium-based composite material in which reinforcing particles are dispersed in a matrix made of a titanium alloy, and the reinforcing particles are a non-magnetic member made of TiCy (0 < y < 1).
[0010] (2) The non-magnetic member of the present invention is made of a titanium-based composite material that satisfies the desired high strength, high rigidity, and high resistivity at a high level. As a result, the non-magnetic member of the present invention reduces eddy current loss generated in the non-magnetic member itself even when used in an alternating magnetic field in the high frequency (e.g., high rotation speed) range. In addition, since the non-magnetic member of the present invention has high rigidity and high strength, it is unlikely to deform or break even in a situation where a large centrifugal force or inertial force is applied, for example, due to high-speed rotation or reciprocation. The non-magnetic member of the present invention is basically made of a titanium-based composite material (non-magnetic material) with low magnetic permeability. Its "non-magnetic" (magnetic permeability) may be such that it does not short-circuit the magnetic circuit of the electromagnetic device.
[0011] 《Electromagnetic equipment / Electric equipment》 (1) The present invention can also be understood as various electromagnetic devices equipped with the above-mentioned non-magnetic member. One example is an electric device equipped with a field element and an armature, in which the field element has a rotating shaft, a cylindrical permanent magnet provided on the outer periphery of the rotating shaft, and a cylindrical protective member fitted over the outer periphery of the permanent magnet, and the protective member is the above-mentioned non-magnetic member.
[0012] (2) In such an electric device, when a field element having a cylindrical permanent magnet as a field source rotates at high speed, a large centrifugal force acts on the permanent magnet in the radial direction. In the electric device of the present invention, a protective member (non-magnetic member) made of the above-mentioned titanium-based composite material is fitted on the outer periphery of the permanent magnet. The protective member has high rigidity and strength, and therefore suppresses deformation of the permanent magnet when subjected to large centrifugal forces, preventing damage to the permanent magnet.
[0013] In light of this, the present invention can also be understood as a field element (electromagnetic component) of an electric device or electric motor having a rotating shaft, a cylindrical permanent magnet provided on the outer periphery of the rotating shaft, and a cylindrical protective member fitted over the outer periphery of the permanent magnet.
[0014] <<Method for manufacturing non-magnetic member>> The present invention can also be understood as a manufacturing method for obtaining the above-described non-magnetic member. For example, the present invention may be a manufacturing method for a non-magnetic member including a sintering step of heating and sintering a molded body of a mixed powder containing TiC powder.
[0015] TiC particles (y = 1) themselves are conductive particles with a specific resistance of about 0.52 μΩm. However, according to the manufacturing method of the present invention, during the sintering step, the TiC particles react in-situ with the particles of the raw material powder constituting the matrix. As a result, a part of the C constituting the TiC particles diffuses (and further dissolves) into the matrix made of a titanium alloy, and a titanium-based composite material in which strengthening particles composed of TiCy (0 < y < 1) with a part of C missing are dispersed substantially uniformly in the matrix is generated. In this way, a non-magnetic member made of a titanium-based composite material with a high specific resistance and high mechanical properties is obtained.
[0016] 《Others》 Unless otherwise specified, "x to y" as used in this specification includes the lower limit value x and the upper limit value y. A range such as "a to b" can be newly established with any numerical value included in various numerical values or numerical ranges described in this specification as a new lower limit value or upper limit value.
Brief Description of the Drawings
[0017] [Figure 1] It is a scatter diagram showing the relationship between the Young's modulus and the specific resistance of the titanium-based composite material for each sample. [Diagram 2] It is an X-ray diffraction pattern of the titanium-based composite material for each sample. [Diagram 3] It is an optical microscope image of the titanium-based composite material for Sample 1 before the tensile test. [Figure 4] It is a scanning electron microscope (SEM) image of the titanium-based composite material for Sample 1 after the tensile test (fracture surface). [Diagram 5] It is a cross-sectional view of a motor which is an example of an electric device. [Figure 6] It is an explanatory diagram showing a method for measuring the specific resistance.
Embodiments for Carrying Out the Invention
[0018] One or more components arbitrarily selected from this specification can be added to the components of the present invention described above. The content described in this specification applies not only to non-magnetic members, electric devices, etc. of the present invention, but also to manufacturing methods of non-magnetic members, and can be either a methodological component or a component related to an object. Whether any embodiment is the best depends on the object, required performance, etc.
[0019] 《Titanium-based composite material》 (1) Reinforcing particles The reinforcing particle TiCy (0 < y < 1) may have y values of 0.4 to 0.9, 0.45 to 0.6, or even 0.5 to 0.55. If y is too small, the improvement in the mechanical properties of the titanium-based composite material will be less. If y is too large, the increase in the specific resistance of the titanium-based composite material will be less. Note that y is calculated based on the X-ray diffraction pattern of the titanium-based composite material. The details will be described later.
[0020] The reinforcing particles may be contained in an amount of 1 to 15% by volume, and more preferably 6 to 12% by volume, based on the entire titanium-based composite material. If the amount of reinforcing particles is too small, the improvement in the rigidity of the titanium-based composite material will be less. If the amount of reinforcing particles is too large, the ductility (elongation) of the titanium-based composite material will decrease and the workability will also deteriorate. The volume ratio of the reinforcing particles is expressed as the volume ratio (% by volume) with respect to the entire titanium-based composite material (100% by volume), unless otherwise specified. The volume ratio of the reinforcing particles dispersed in the titanium-based composite material is the volume fraction of the reinforcing particles calculated by a composition analysis software: ImageJ (open source program) from a two-dimensional optical microscope photograph (image).
[0021] In addition, the titanium-based composite material according to the present invention may further contain reinforcing particles other than TiCy (for example, TiC, TiB, etc.). Even in this case, the total amount of the reinforcing particles is preferably 15% by volume or less.
[0022] (2) Matrix The matrix may be any titanium alloy, and may be, for example, mainly composed of α-phase, β-phase, α2-phase, etc. If the matrix is an α-type titanium alloy or (α+β)-type titanium alloy, it is easier to achieve a higher level of both rigidity and resistivity in the titanium-based composite. Note that since the α2-phase is a Ti3Al phase, the matrix is a titanium alloy containing Al.
[0023] Titanium alloys may have various compositions, but it is preferable that the titanium alloy contains at least 4-10%, 5-9%, or even 5.5-8.5% of Al, which is an α-phase stabilizing element, relative to the entire titanium alloy (100 mass%). This makes it easier for the titanium-based composite to exhibit high resistivity and stable strength up to high temperatures. Unless otherwise specified, the matrix composition in this specification is the mass ratio relative to the entire matrix (titanium alloy) and is expressed in mass% (simply referred to as "%").
[0024] The amount of Al may be understood as Al equivalent. For example, when the titanium alloy contains α-phase stabilizing elements such as Al, Sn, and Zr, the Al equivalent calculated by [Al]eq=[Al]+[Sn] / 2+[Zr] / 6 ([]: mass%) should be within the above-mentioned range. In other words, the Al equivalent is preferably 4 to 10%, 5 to 9%, or even 5.5 to 8.5%.
[0025] The titanium alloy may contain β-phase stabilizing elements such as Mo and Cr in addition to α-phase stabilizing elements such as Al. Mo is preferably contained in an amount of, for example, 0.5 to 5%, or more preferably 1.5 to 4%. Cr is preferably contained in an amount of, for example, 0.5 to 4%, or more preferably 1 to 3%. A titanium-based composite material containing an appropriate amount of Mo and Cr in the matrix has excellent plastic deformability (ductility).
[0026] The titanium alloy may contain neutral elements such as V, Sn, and Zr. These elements can also contribute to improving the strength and ductility of the matrix (titanium alloy). The total amount of V, Sn, and Zr is preferably, for example, 0.5 to 10%, or more preferably 1 to 9%. In particular, V is preferably contained at 0.5 to 8%, or more preferably 3 to 6%.
[0027] The titanium alloy may further contain 1 mass % or less, or even 0.5 mass % or less in total, of O or N (α-phase stabilizing elements). O and N are interstitial elements, and, like C, can improve the resistivity and other properties of the titanium-based composite material if they are within the range of solid solubility in Ti.
[0028] (3)Characteristics The titanium-based composite material according to the present invention exhibits excellent electrical or mechanical properties. For example, it exhibits a resistivity of 2μΩm to 5μΩm, 2.5μΩm to 4μΩm, or even 2.8μΩm to 3.5μΩm. Incidentally, the resistivity of pure Ti is about 0.43μΩm, that of TiC is about 0.52μΩm, and that of TiB2 is about 0.07μΩm, all of which are small. In other words, the resistivity of the titanium-based composite material according to the present invention is far greater than that of Ti, which is a metal, or TiB2, TiC, which are compounds (ceramics). The resistivity value in this specification means a measured value measured by a direct current four-terminal method on a sample (bulk material) of a given size, unless otherwise specified.
[0029] The titanium-based composite material according to the present invention has high rigidity and strength. For example, it exhibits a Young's modulus of 120 to 150 GPa, or even 130 to 140 GPa. It also exhibits a tensile strength (breaking strength) of 1000 to 1300 MPa, or even 1100 to 1250 MPa.
[0030] Furthermore, the titanium matrix composite material according to the present invention can exhibit an elongation of about 0.5 to 4%, or even 1.2 to 3.5%, depending on the matrix composition and the amount of dispersed reinforcing particles (volume %). Thus, the titanium matrix composite material having a suitable degree of plastic deformability can be plastically processed into various types of non-magnetic members.
[0031] 《Manufacturing method》 There are various methods for manufacturing non-magnetic members made of titanium-based composite materials. For example, they may be manufactured by sintering, melting, (powder) additive manufacturing (so-called 3D printer), etc. Here, as an example, we will explain the reactive sintering method (simply called the "sintering method"), which is excellent in the dispersibility of TiCy and the controllability of the atomic ratio (C / Ti) (i.e., the controllability of y).
[0032] The sintering method is a method in which a powder compact is heated to obtain a sintered body. If the compact or sintered body is close to the shape of a non-magnetic member (i.e., if it is near-net shape), post-processing can be reduced. Of course, the sintered body may be subjected to plastic processing such as forging or pressing in a cold or hot state.
[0033] (1) Powder It is preferable to use a mixed powder obtained by mixing a powder that will mainly become the matrix with a powder that will mainly become the reinforcing particles. The powder that will mainly become the matrix may be a single type of powder, but by combining a Ti source powder (e.g., pure Ti powder) with one or more alloy element source powders (alloy powders or compound powders), it becomes easier to control the composition of the matrix. It is preferable that each powder (especially the Ti source powder) is classified, for example, by sieving to 50 μm or less, or even 40 μm or less, so that the titanium-based composite material can be made uniform.
[0034] The powders that mainly become reinforcing particles may be multiple types of powders, or may be a single type of powder (for example, TiC powder). If the average particle size of each powder is 1 to 20 μm, or even 3 to 15 μm, the reinforcing particles are likely to be uniformly dispersed in the matrix.
[0035] The mixed powder is preferably prepared by uniformly mixing a plurality of types of powder using a V-type mixer, a ball mill, a vibration mill, or the like (mixing step).
[0036] (2) Molding process The mixed powder is molded, CIP (Cold Isostatic Pressing), RIP (Rubber Isostatic Pressing), or the like to form a molded body of a desired shape. The shape of the molded body may be close to the shape of the final member (non-magnetic member), or may be a billet shape (intermediate material shape) when processing is performed after the sintering process. The molding pressure can be appropriately adjusted, but is preferably, for example, 200 to 1200 MPa, or further preferably 300 to 800 MPa.
[0037] (3) Sintering process The compact is heated in a vacuum or in an inert gas to become a sintered body. The sintering temperature is, for example, 1150°C to 1400°C, or preferably 1200 to 1350°C. The sintering time is, for example, 3 to 25 hours, or preferably 10 to 20 hours. By using an appropriate sintering temperature and sintering time, a titanium-based composite material with high properties can be efficiently obtained. The above-mentioned molding step and sintering step may be performed simultaneously by HIP (Hot Isostatic Pressing) molding.
[0038] (4) Cooling process After the sintering step, the material may be cooled at a rate of, for example, 0.1 to 10° C. / s by furnace cooling or forced cooling (by introducing an inert gas, etc.). By controlling the cooling rate, it may be possible to adjust the structure of the matrix and the composition and volume fraction of the reinforcing particles.
[0039] <Non-magnetic parts / electric devices> The non-magnetic member of the present invention can be used in any application as long as it is used in an alternating magnetic field and requires high resistivity, high rigidity, high strength, and low magnetic permeability (non-magnetic material). An example of the application of the non-magnetic member is a protective member used in the field magnet of an electric motor (electromagnetic device, electric device). A specific example of this application will be described in detail below with reference to FIG. 5.
[0040] The motor M is a synchronous machine including a rotor 1 (field element / rotor), a stator 2 (armature / stator), and a housing 3 that houses them. The rotor 1 has a shaft 11 (rotating shaft), a ring magnet 12 fitted onto the outer circumferential surface side of the rotor 1, and a sleeve 13 (protective member) fitted onto the outer circumferential surface side of the ring magnet 12. The shaft 11 is pivotally supported by a bearing 4 provided in the housing 3. The stator 2 has a yoke and a coil attached to the yoke. When a high-frequency current is applied to the coil from an external control device, a rotating magnetic field is generated in the stator 2.
[0041] The ring magnet 12 is composed of a cylindrical permanent magnet with a constant wall thickness, and has a desired number of magnetic poles with S and N poles in the radial direction magnetized alternately. The ring magnet 12 is fixed to the shaft 11, and the two rotate integrally.
[0042] The permanent magnet may be a sintered magnet or a bonded magnet (plastic magnet). The permanent magnet is preferably a rare earth magnet with high magnetic properties. Examples of rare earth magnets include Nd-Fe-B based magnets (permanent magnets containing Nd2Fe 14 B), Sm-Fe-N based magnets (permanent magnets containing Sm2Fe 17 N3 or SmFe9N 1.5 ), Sm-Co based magnets (permanent magnets containing SmCo5 or Sm2Co 17 ), etc. When the motor M is used in a high-temperature range, it is preferable to use a Sm-Co based magnet with excellent temperature characteristics.
[0043] The sleeve 13 is made of a titanium-based composite material in which TiCy particles (0 < y < 1) are dispersed in a titanium alloy matrix. The fitting of the sleeve 13 onto the ring magnet 12 may be performed by shrink fitting by heating the sleeve 13, or press fitting by cooling the ring magnet 12, etc. Thereby, the ring magnet 12 is in a state where a preload in the compression direction (diameter-reducing direction) is applied by the sleeve 13.
[0044] When the motor M rotates at high speed (for example, 50,000 to 150,000 rpm), a large centrifugal force acts on the ring magnet 12. Here, since the sleeve 13 has high rigidity and high strength, it suppresses the deformation of the low-strength ring magnet 12 and prevents its damage.
[0045] Also, an alternating magnetic field corresponding to the rotation speed of the motor M penetrates the sleeve 13, and eddy currents are also generated in the sleeve 13. Here, since the sleeve 13 has a high resistivity, even when the motor M rotates at high speed, the eddy current loss generated in the sleeve 13 is suppressed.
[0046] The motor M can be used in various electric devices. One example of an electric device is a centrifugal compressor that requires high speed rotation. Such a compressor is used, for example, in an engine supercharger or an air compressor for a fuel cell. EXAMPLES
[0047] Various samples (titanium matrix composites) with different matrices or reinforcing particles were produced and their electrical properties (resistivity) and mechanical properties (Young's modulus, tensile strength, elongation) were evaluated. The present invention will be described in more detail below with reference to such specific examples.
[0048] <Sample Preparation> (1) Raw material powder Pure Ti powder and various alloy source powders, which mainly constitute the matrix, and various compound powders, which mainly constitute the reinforcing particles, were prepared.
[0049] The Ti powder used was a commercially available hydrogenated / dehydrogenated powder (manufactured by Toho Tech Co., Ltd.) that had been classified using a sieve (#350, average particle size 75 μm). One or more of the following powders were used as the alloy source powder. (a) Al-40% V powder (average particle size: 9 μm / Kinsei Matec Co., Ltd.) (b) Ti-36%Al powder (average particle size: 9 μm / manufactured by Daido Steel Co., Ltd.) (c) Mo2C powder (average particle size: 3 μm / manufactured by Japan New Metals Co., Ltd.) (d) Cr2C powder (average particle size: 3 μm / manufactured by Japan New Metals Co., Ltd.)
[0050] As the compound powder, any one of the following powders was used. (a) TiC powder (average particle size: 3 μm / manufactured by Japan New Metals Co., Ltd.) (b) TiB2 powder (average particle size: 3 μm / manufactured by Japan New Metals Co., Ltd.) (c) SiC powder (average particle size: 3 μm / manufactured by Shinano Electric Smelting Co., Ltd.) (d) AlN filler (average particle size: 3 μm / manufactured by Furukawa Electronics Co., Ltd.)
[0051] The composition of each powder shown in this example is a mass percentage (mass%) unless otherwise specified. The average particle size of each powder is a value determined by a laser diffraction / scattering type particle size distribution analyzer (MT3300EX / manufactured by Nikkiso Co., Ltd.). Incidentally, a small amount of oxygen is adsorbed or bonded to the particle surface of each powder. Pure Ti powder may contain 0.1 to 0.5 mass% of oxygen relative to the entire powder, and alloy source powder may contain about 0.1 mass% of oxygen relative to the entire powder.
[0052] (2)Mixing process First, Ti powder and each alloy source powder were weighed and mixed to obtain the matrix composition (mass ratio when the entire matrix is taken as 100 mass%) shown in Table 1. In this case, alloy source powder (a) was used in samples 1, 2, 6, C1, C2, and C3. Alloy source powders (b) and (c) were used in samples 3 and 4. Alloy source powders (b), (c), and (d) were used in sample 5.
[0053] To the matrix powder thus obtained, 10% by volume (volume ratio when the total mixed powder is 100% by volume) of each compound powder, which is a source of reinforcing particles, was added. In other words, the volume ratio of the matrix powder to the compound powder was set to 9:1. The matrix powder and compound powder mixed in the desired ratio were mixed for 1 hour in a V-type mixer. In this way, the mixed powder for each sample was obtained.
[0054] (3) Molding process Each mixed powder was placed in a polyvinyl chloride tube (PVC) and CIP molded to obtain a round rod-shaped molded body (approximately φ16mm × 150mm). The molding pressure at this time was 4t / cm 2 (392 MPa).
[0055] (4) Sintering process Each compact was placed in a vacuum (1×10 -5 The samples were sintered by heating at 1300°C for 16 hours at a pressure of 100 torr. However, the sintering time was set to 4 hours for sample 6 only. In all cases, the heating rate up to the sintering temperature was about 5°C / min, and the cooling rate after the sintering time had elapsed was 10°C / s.
[0056] (5) Processing process Furthermore, the sintered bodies of each sample were hot forged in an air atmosphere. The heating temperature was 1000-1200°C, and the processing rate was 50%. The processing rate was calculated as the reduction in area (Aw / Ao). Aw is the cross-sectional area after processing, and Ao is the cross-sectional area before processing. Various measurements and observations were performed using each test material (billet) obtained in this way.
[0057] "measurement" (1) Electrical properties (resistivity) The resistivity of each sample was determined as shown in FIG. 6. Specifically, first, electrodes were formed on a prism (3.014 mm (t) × 3.014 mm (w) × 20 mm) made from each test material as follows. The center part of each prism (voltage electrode interval (L): 10 mm) was masked with masking tape. Terminal wires (silver wire: φ0.20 mm) were wound around the masked end parts and the two outer parts, which are four places (see FIG. 6). Silver paste (Dotite D-550, manufactured by Fujikura Kasei Co., Ltd.) was applied to the parts where the terminal wires were wound and to both end faces of the prism. After application, the prism was heated in the air at 100°C for 12 hours to dry. In this way, a test piece equipped with a current electrode and a voltage electrode was prepared.
[0058] The resistivity (electrical resistivity) of each sample was calculated from the voltage (V) and current (I) values measured for each test piece by the DC four-terminal method at room temperature and the cross-sectional shape (S = t × w) of the test piece (rectangular column) (see formula (1) in Figure 6). The resistivity (measured value) of each sample thus obtained is also shown in Table 1.
[0059] The resistivity of sample C1 was 1.51 μΩm. Table 1 also shows the ratio of the resistivity of each sample (resistivity ratio) to the resistivity of sample C1 (reference).
[0060] (2) Mechanical properties (Young's modulus, tensile strength, elongation) A tensile test was performed using a round bar tensile test piece (parallel part diameter: φ2.4 mm, gauge length: 14 mm) made from the test material, using an autograph (AUTOGRAPH AG-1 50 kN, manufactured by Shimadzu Corporation). The tensile test was performed in air at room temperature, with a strain rate of 5 × 10 -4 The tensile tests were carried out in units of tensile strain per second (s). The mechanical properties of each sample were determined based on the stress-strain relationship calculated from the load-stroke diagram obtained in the tensile tests. The results are also shown in Table 1. The tensile strength was calculated based on the load at break and the initial shape of the test piece. The elongation is the strain of the test piece at break.
[0061] (3) X-ray diffraction (determining y) The test materials for each sample were subjected to X-ray diffraction analysis (XRD / Cu-Kα). The diffraction patterns obtained for some of the samples are summarized in Figure 2. Figure 2 also shows the diffraction pattern of a representative titanium alloy (Ti-6%Al-4%V).
[0062] "observation" (1) The structure of the test material before the tensile test was observed by a SEM (Scanning Electron Microscope). As an example, an observation image (SEM image) of Sample 1 is shown in Figure 3. In addition, an SEM image of the fracture surface of Sample 1 after the tensile test is shown in Figure 4.
[0063] (2) The volume fraction of the reinforcing particles dispersed in the test material (titanium matrix composite) was determined by image analysis of the SEM images of each sample using ImageJ. The volume fraction thus obtained was almost the same as the predicted volume fraction at the time of compounding (when the powders were mixed).
[0064] "evaluation" (1) Electrical properties (resistivity) As is clear from Table 1, the titanium-based composites of samples 1 to 6, which used TiC powder as the reinforcing particle source, had resistivities approximately twice (1.7 to 2.1 times) higher than those of titanium-based composites such as sample C1.
[0065] (2) Mechanical properties As is clear from Table 1, it was also found that the titanium-based composite materials of Samples 1 to 6 had high Young's modulus, tensile strength, or elongation comparable to that of the titanium-based composite materials such as Sample C1.
[0066] The relationship between Young's modulus and resistivity for each sample shown in Table 1 is shown in Figure 1. As is clear from Figure 1, titanium matrix composites using TiC powder as the reinforcing particle source have high resistivity and high Young's modulus. The titanium matrix composite of sample C2 also has high resistivity and high Young's modulus, but its tensile strength and elongation are extremely low and it is not suitable for structural components. For reference, Figure 1 also plots a typical ingot titanium alloy (Ti-6%Al-4%V / Young's modulus: 110GPa, resistivity: 1.5-1.8μΩm) that constitutes the matrix.
[0067] (3) XRD As is clear from FIG. 2, first, the peak position of (211)β, which indicates the β phase and is located near 2θ=71°, showed almost no difference between the samples.
[0068] Next, when observing the peak position of (112)α, which indicates the α phase near 2θ=76.8°, the peak position of sample C1 was almost the same as that of Ti-6%Al-4%V, but the peak position of sample 1 was shifted to the lower angle side. This tendency was also observed for the peak position of (201)α, which indicates the α phase near 2θ=78°. From these, it was found that the lattice spacing of the α phase related to sample 1 was expanded. It was also confirmed that samples 2 to 6 showed the same tendency as sample 1.
[0069] (4) Atomic ratio of TiCy (C / Ti) As shown in Figure 2, in sample 1, which uses TiC powder, a peak of TiCy was observed near 2θ = 73°. From the diffraction pattern, the Bragg equation and the assumption that TiCy has an fcc structure were used to determine the lattice constant (a) of TiCy. Specifically, in the case of a cubic crystal, the lattice constant (a) is 1 / d between the interplanar spacing d and the diffraction peaks (h, k, l). 2 =h 2 +k 2 +l 2 / a 2Applying Bragg's law (λ = 2dsinθ), the lattice constant is: a = λ / 2sinθ √(h 2 +k 2 +l 2 ) Furthermore, the atomic ratio (i.e., y) can be calculated from the lattice constant using the Ramqvist relationship. As a result, it was confirmed that the average value was y = 0.53. The atomic ratios of samples 2 to 6 were calculated in the same manner as for sample 1, and the results were y = 0.53 for samples 2 and 6, and y = 0.81 for samples 3 to 5.
[0070] The relationship between the lattice constant and the atomic ratio is described in detail in L. Ramqvist et al., Journal of Physics and Chemistry of Solids, vol. 30.7 (1969), pp. 1849-1860. In this embodiment, the atomic ratio (y) was specified according to the description in the reference.
[0071] (5) Organization As is clear from Figure 3, the grain boundaries of the raw powder were not discernible in the matrix, and the crystal grains of each phase were about 20 μm, smaller than the grains of the raw powder. TiCy particles of about 5 to 30 μm were dispersed almost uniformly in this matrix.
[0072] As is clear from Figure 4, ridges and fine dimples were observed in the SEM image of the fracture surface. The ridges are thought to be the grain boundaries of the matrix. TiCy particles with cracks of about 10 to 30 μm were observed inside the ridges. A small number of nano-sized TiCy particles were also observed inside the dimples. It is presumed that the precipitated nano-sized TiCy particles exerted a pinning effect and contributed to controlling the morphology of the structure.
[0073] Incidentally, the AlN used in sample C3 was in a non-equilibrium state in the titanium matrix, so TiAl-based compounds precipitated at the grain boundaries with the matrix. Although AlN itself has a high resistivity, the titanium matrix composite material with AlN reinforcing particles showed numerous cracks after sintering, and could not be used as a sintered body.
[0074] 《Consideration》 The reason why the resistivity of the titanium matrix composites containing TiCy reinforcing particles, such as samples 1 to 6, is high is considered to be as follows. As mentioned above, the reinforcing particles dispersed in the titanium alloy matrix are TiCy (0 <y<1)となっている。 In such TiCy, lattice mismatch occurs due to carbon deficiency, and the mean free path of electrons becomes smaller than that of TiC, which makes electron scattering more likely to occur. It is presumed that this is why the resistivity of TiCy is significantly higher than that of TiC.
[0075] It is also assumed that the resistivity of the matrix increased due to the C (missing C) generated from TiC dissolving in the matrix (titanium alloy) as an interstitial element. In other words, it is considered that the dissolution of C causes non-uniform lattice distortion in the matrix, and the disturbance of the periodicity of the lattice makes it easier for electrons to scatter, which increases the resistivity of the matrix. In particular, the effect of the expansion of the lattice spacing of the α phase, which occupies most of the matrix (for example, more than 80% of sample 1 is α phase), is thought to be large. The same is true for the α2 phase (for example, sample 3).
[0076] In this way, it is presumed that the resistivities of TiCy and the matrix increase additively or even synergistically, and the titanium-based composite materials of samples 1 to 6 exhibit high resistivity while maintaining excellent mechanical properties.
[0077] [Table 1]
Claims
1. A non-magnetic member that is used with rotation in an alternating magnetic field, The titanium matrix composite material has reinforcing particles dispersed in a matrix of titanium alloy. The reinforcing particles are made of TiCy (0.4≦y≦0.9), The titanium-based composite material has a resistivity of 2 μΩm to 5 μΩm.
2. 2. The non-magnetic member according to claim 1, wherein y is 0.5 to 0.
6.
3. 3. The non-magnetic member according to claim 1, wherein the resistivity is 2.5 μΩm to 4 μΩm.
4. 4. The non-magnetic member according to claim 1, having a tensile strength of 1000 to 1300 MPa.
5. 5. The non-magnetic member according to claim 1, wherein the Young's modulus is 120 to 150 GPa.
6. 6. The non-magnetic member according to claim 1, wherein the reinforcing particles are contained in an amount of 1 to 15% by volume based on the total volume of the titanium-based composite material.
7. The matrix may be in the α phase, β phase or α 2 7. The non-magnetic member according to claim 1, which is made of a titanium alloy having any one of the above phases.
8. 8. The non-magnetic member according to claim 7, wherein the matrix has an Al equivalent of 4 to 10 mass % relative to the entire titanium alloy.
9. An electric device having a field element and an armature, the field element includes a rotating shaft, a cylindrical permanent magnet provided on an outer periphery of the rotating shaft, and a cylindrical protective member fitted over the outer periphery of the permanent magnet, The protective member is a non-magnetic member according to any one of claims 1 to 8.
10. A field element of an electric device having a rotating shaft, a cylindrical permanent magnet provided on an outer periphery of the rotating shaft, and a cylindrical protective member fitted over the outer periphery of the permanent magnet, The protective member is a field element of an electric device which is a non-magnetic member according to any one of claims 1 to 8.
11. A method for producing the non-magnetic member according to any one of claims 1 to 8, comprising the steps of: A method for manufacturing a non-magnetic member, comprising a sintering step of heating and sintering a compact of a mixed powder containing TiC powder.
Citation Information
Patent Citations
Titanium alloy composite material
JP1993005138A
Rotor and manufacturing method thereof, and rotating machine
JP2001339886A
Titanium based hard sintering material, production method therefor, and plain bearing obtained by using the titanium based hard sintering material
JP2004190097A
Rotor for high-speed rotation motor
JP2008029153A
Rotor member of permanent magnet electric motor, rotor and manufacturing meted of rotor