Method for producing fluid catalytic cracking catalyst
The production method for an FCC catalyst using a specific silicon-to-aluminum ratio and silica-based matrix with controlled aluminum contact improves gasoline RON and LPG production by modifying cation sites, addressing the limitations of conventional catalysts.
Patent Information
- Application Number
- JP2020185176
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-05
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-11-05
AI Technical Summary
Conventional FCC catalysts have limitations in improving the octane number (RON) of gasoline and promoting the production of liquefied petroleum gas (LPG) in fluid catalytic cracking processes.
A method involving the production of an FCC catalyst using a specific ratio of silicon to aluminum atoms in ultra-stabilized Y-type zeolite and/or rare-earth metal-containing zeolite, combined with a silica-based matrix-forming component, and a controlled pH contact with aluminum salt, including steps of spray drying and water treatment to enhance catalyst performance.
The method results in an FCC catalyst that improves the RON of gasoline and promotes LPG production by modifying cation sites with aluminum cations, increasing acid strength and reducing non-aromatic fraction decomposition, thereby enhancing LPG selectivity and RON.
Smart Images

Figure 0007576428000001 
Figure 0007576428000002 
Figure 0007576428000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a fluid catalytic cracking catalyst. [Background technology]
[0002] Various developments have been made for catalysts (hereinafter also referred to as "FCC catalysts") used in fluid catalytic cracking of hydrocarbon oils and methods for producing the same, with the aim of increasing the yield of gasoline fraction in fluid catalytic cracking. For example, Patent Document 1 discloses a method for producing an FCC catalyst, which is obtained by mixing zeolite (ultra-stable Y-type zeolite, rare earth-exchanged ultra-stable Y-type zeolite, etc.), a binder (basic aluminum chloride), and an inorganic oxide matrix (kaolin, etc.), and spray-dries a slurry with an adjusted pH, with the aim of providing a method for producing an FCC catalyst with a high gasoline yield, a low coke yield, and high attrition resistance. It also discloses that the spherical particles obtained by spray-drying are washed with pure water, then washed with water containing ammonium sulfate, and dried to produce an FCC catalyst. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-657 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, conventional FCC catalysts have room for further improvement in terms of improving the gasoline octane number (hereinafter also referred to as "RON") and promoting the production of liquefied petroleum gas (hereinafter also referred to as "LPG") in fluid catalytic cracking. Therefore, an object of the present invention is to provide a method for producing an FCC catalyst that can improve the RON of gasoline and promote the production of LPG in fluid catalytic cracking. [Means for solving the problem]
[0005] The present invention relates to, for example, the following [1] to [6]. [1] (a) preparing a raw material slurry by mixing a zeolite, which is an ultra-stable Y-type zeolite and / or a rare earth metal-containing ultra-stable Y-type zeolite, having a ratio of silicon atoms to aluminum atoms of 5.0 to 6.0 expressed as a molar ratio of SiO to Al2O3, a silica-based matrix-forming component, water, and optionally clay minerals and optionally additives; (b) spray-drying the raw slurry to obtain particles; and (d) contacting the particles obtained in the step (b) with water containing an aluminum salt and having a pH of 3.5 to 5.0 in a ratio of (mass of aluminum salt converted into mass of aluminum oxide) / (mass of zeolite contained in the particles)≧0.04; A method for producing a fluid catalytic cracking catalyst comprising the steps of:
[0006] [2] (c) contacting the particles obtained in step (b) with water wherein in the step (d), particles obtained in the step (b) are those that have been subjected to the step (c).
[0007] [3] The method for producing a fluid catalytic cracking catalyst according to any one of [1] and [2] above, wherein a metal capture agent is mixed as the additive in the step (a).
[0008] [4] The method for producing a fluid catalytic cracking catalyst according to any one of the above [1] to [3], wherein an active matrix component is mixed as the additive in the step (a).
[0009] [5] The method for producing a fluid catalytic cracking catalyst according to any one of the above [1] to [4], wherein the silica-based matrix-forming component is a silica sol.
[0010] [6] A fluid catalytic cracking catalyst produced by any one of the methods [1] to [5] above. Effect of the Invention
[0011] According to the present invention, it is possible to produce an FCC catalyst capable of improving the RON of gasoline and promoting the production of LPG in fluid catalytic cracking. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will now be described in further detail. The method for producing a fluid catalytic cracking catalyst (FCC catalyst) according to the present invention includes the steps of: (a) a step of preparing a raw material slurry by mixing a zeolite having a ratio of silicon atoms to aluminum atoms of 5.0 to 6.0 expressed as a molar ratio of SiO to Al2O3, which is ultra-stable Y-type zeolite (hereinafter also referred to as "USY") and / or rare earth-containing USY (hereinafter also referred to as "REUSY"), a silica-based matrix-forming component, and water; (b) spray-drying the raw slurry to obtain particles; and (d) contacting the particles obtained in step (b) with water containing an aluminum salt. The present invention is characterized in that it includes:
[0013] "Engineering (a)" In the step (a), zeolite, a silica-based matrix-forming component, water, and optionally clay minerals and optionally additives are mixed to prepare a raw material slurry.
[0014] (Zeolite) The zeolite is a specific ultra-stable Y-type zeolite (USY) and / or rare earth-containing USY (REUSY), i.e., USY, REUSY, or a mixture of USY and REUSY. From the viewpoint of ease of preparation of raw materials, it is preferable to use USY alone or REUSY alone.
[0015] "Ultra-Stable Y-Type Zeolite (USY)" The ratio of silicon atoms to aluminum atoms contained in the USY is 5.0 to 6.0, preferably 5.0 to 5.5, expressed as a molar ratio of SiO2 to Al2O3 (hereinafter also referred to as [SiO2 / Al2O3 molar ratio]). (The molar ratio of silicon atoms to aluminum atoms (Si / Al) is 2.5 to 3.0, preferably 2.5 to 2.75.) When the molar ratio is in this range, many acid sites based on the framework aluminum of the zeolite are expressed.
[0016] The lattice constant of the USY, measured by the method employed in the examples described below, is preferably 2.457±0.010 nm, and more preferably 2.450 to 2.465 nm. The lattice constant is determined by the interplanar spacing of the diffraction planes (553) and (642) of the zeolite by X-ray diffraction using anatase-type TiO2 as a standard substance.
[0017] When the lattice constant is within this range, the amount of aluminum in the zeolite framework is large, and there are many cracking active sites. When the lattice constant is equal to or less than the upper limit, the zeolite has high hydrothermal resistance and therefore has high cracking activity as a fluid catalytic cracking catalyst, whereas when the lattice constant is equal to or more than the lower limit, the zeolite has many acid sites and therefore has high cracking activity as a fluid catalytic cracking catalyst.
[0018] The USY can be produced by a conventional method, for example, the method described in JP 2020-19694 A. For example, the USY can be produced by preparing NH4-Y type zeolite (Y type zeolite having ammonium ions) and calcining the NH4-Y type zeolite with steam.
[0019] "Rare Earth Metal-Containing Ultra-Stable Y-Type Zeolite (REUSY)" The ratio of silicon atoms to aluminum atoms contained in the REUSY is 5.0 to 6.0, preferably 5.0 to 5.5, expressed as the molar ratio of SiO2 to Al2O3 (hereinafter also referred to as [SiO2 / Al2O3 molar ratio]). (The molar ratio of silicon atoms to aluminum atoms (Si / Al) is 2.5 to 3.0, preferably 2.5 to 2.75.) When the molar ratio is in this range, many acid sites based on the framework aluminum of the zeolite are expressed.
[0020] The rare earth metal content of the REUSY is 10 to 40 mass%, preferably 10 to 20 mass%, calculated as rare earth metal oxide (RE2O3 is an oxide of rare earth metal (RE)). When the content is within this range, the zeolite framework is stabilized by the rare earth metal cations.
[0021] Examples of the rare earth metal include lanthanum, cerium, praseodymium, neodymium, yttrium, samarium, and europium, and among these, lanthanum and cerium are preferred. These may be used alone or in combination of two or more.
[0022] The lattice constant of the REUSY, measured by the method employed in the examples described below, is preferably 2.465±0.010 nm, and more preferably 2.460 to 2.470 nm. The lattice constant is determined by the interplanar spacing of the diffraction planes (553) and (642) of the zeolite by X-ray diffraction using anatase-type TiO2 as a standard substance.
[0023] When the lattice constant is within this range, the amount of aluminum in the zeolite framework is large, and there are many cracking active sites.
[0024] The REUSY can be produced by a conventional method, for example, the method described in JP-A-2004-337758 or JP-A-2009-22842. As an example, the REUSY can be produced by preparing NaUSY-type zeolite and exchanging the sodium ions in the NaUSY-type zeolite with rare earth metal ions.
[0025] The raw slurry contains the zeolite (i.e., the USY or the REUSY) in an amount of, for example, 10 to 50 mass %, and preferably 20 to 40 mass % (where the amount of solids in the raw slurry (components other than the dispersion medium in the raw slurry) is taken as 100 mass %) on a dry basis (mass after heat treatment at 800°C for 1 hour; the same applies below) of the zeolite. When the content is equal to or more than the lower limit, the obtained FCC catalyst exhibits sufficient activity. On the other hand, when the content is equal to or less than the upper limit, over-cracking and reduced selectivity due to excessive activity in the obtained FCC catalyst can be prevented.
[0026] (Silica-Based Matrix-Forming Component) The silica-based matrix forming component is a component for forming a silica-based matrix that functions as a binder in the FCC catalyst, and examples thereof include silica, silica gel (including silica hydrogel), silica sol (including silica hydrosol), water glass (sodium silicate), and silicic acid liquid. When fluid catalytic cracking is performed using the FCC catalyst, the formation of coke is suppressed because the matrix is a silica-based matrix.
[0027] The raw material slurry contains the silica-based matrix-forming component in an amount of, for example, 10 to 90 mass %, preferably 10 to 40 mass %, and more preferably 15 to 25 mass % on a dry basis (where the solid content of the raw material slurry is taken as 100 mass %).
[0028] In the prior art, basic aluminum chloride (e.g., [Al(OH) n Cl 6-n ] m(However, 0 < n < 6, 1 ≤ m ≤ 10, preferably 4.8 ≤ n ≤ 5.3, 3 ≤ m ≤ 7. Note that m represents a natural number.) is represented. ) may be used. However, when washing the matrix formed from basic aluminum chloride with water (corresponding to steps (c) and (d) in the present invention), it is necessary to control the pH of the water within a narrow range in order to prevent dissolution of the matrix. On the other hand, when the matrix-forming component of the FCC catalyst is a silica-based matrix-forming component, from the viewpoint that the allowable pH range for preventing dissolution during washing is wider than that of basic aluminum chloride, the working efficiency of FCC catalyst production is excellent. Therefore, the raw material slurry preferably does not contain basic aluminum chloride, or if it contains it, the amount is small (for example, 1% by mass or less of the silica-based matrix-forming component), and more preferably does not contain it.
[0029] (Clay Minerals) The clay minerals are clay and / or clay minerals, examples of which include kaolin, bentonite, kaolinite, halloysite, montmorillonite, etc., and among these, kaolin is preferred.
[0030] The raw material slurry contains the clay minerals, for example, 60% by mass or less, preferably 10 - 60% by mass, more preferably 15 - 30% by mass on a dry basis (assuming the solid content of the raw material slurry is 100% by mass). When the content is at least the lower limit value, the pore structure of the FCC catalyst, the catalyst shape, abrasion resistance, fluidity, etc. are good. On the other hand, when the content is at most the upper limit value, since the ratio of the zeolite in the FCC catalyst is high, the activity of the FCC catalyst is good.
[0031] (Additives) Examples of the additive that may be optionally added include additives that are usually contained in FCC catalysts, such as active matrix components and metal scavengers. Examples of the active matrix component include substances having solid acids such as activated alumina, silica-alumina, silica-magnesia, alumina-magnesia, and silica-magnesia-alumina.
[0032] The raw slurry contains the active matrix component in an amount of, for example, 40% by mass or less, preferably 5 to 40% by mass, and more preferably 10 to 30% by mass (where the solid content of the raw slurry is taken as 100% by mass) on a dry basis.
[0033] Examples of the metal scavenger include manganese oxide, magnesium oxide, calcium oxide, and lanthanum oxide. The raw material slurry contains the metal capture agent in an amount of, for example, 10% by mass or less, preferably 1 to 10% by mass, and preferably 2 to 5% by mass (where the solid content of the raw material slurry is taken as 100% by mass) on a dry basis.
[0034] <Preparation of Raw Material Slurry> The raw material slurry can be prepared by mixing the above-mentioned zeolite (USY or REUSY), and a silica-based matrix-forming component, as well as a clay mineral and, if necessary, additives such as the activated alumina and the metal capture agent, with water.
[0035] The raw material slurry may contain a small amount of a component other than water as a dispersion medium, such as methanol, ethanol, or acetone. As the mixing method, a conventionally known mixing method can be adopted.
[0036] Furthermore, when preparing the raw material slurry, the raw materials may be subjected to a pulverization / dispersion treatment. By carrying out the pulverization / dispersion treatment, the raw materials are uniformly dispersed. As the pulverization / dispersion treatment, a conventionally known method can be adopted. The solid content concentration of the raw slurry is, for example, 10 to 50% by mass, and preferably 20 to 40% by mass, from the viewpoint of easily carrying out spray drying of the raw slurry.
[0037] "Engineering (b)" In the step (b), the raw material slurry is spray-dried to obtain particles. For example, the raw slurry is filled into a slurry storage tank of a spray dryer, and the raw slurry is sprayed into a drying chamber through which an air current (e.g., an air current) adjusted to a temperature in the range of, for example, 120 to 450° C. flows, thereby obtaining particles (hereinafter also referred to as “spray-dried particles”). Although the temperature of the air current decreases due to the spray drying of the raw slurry, the temperature at the outlet of the drying chamber is maintained in the range of, for example, 50 to 300° C. using a heater or the like. The particle size of the spray-dried particles can be adjusted by adjusting the concentration, viscosity, spray amount, spray pressure, nozzle diameter of the spray dryer, hot air temperature, and the like of the raw material slurry.
[0038] "Engineering (c)" The method for producing a fluid catalytic cracking catalyst (FCC catalyst) according to the present invention may include a step (c) of contacting the particles obtained in the step (b) (i.e., the spray-dried particles) with water. It is believed that the step (c) removes impurities such as alkali metals and sulfate ions that may be contained in the spray-dried particles.
[0039] The embodiment of the step (c) is, for example, (c1) dispersing the spray-dried particles in water and separating the particles from the resulting slurry; and Step (c2) of pouring water over the spray-dried particles. Examples include:
[0040] In step (c1), the operation of dispersing the spray-dried particles in water and separating the particles from the resulting slurry (hereinafter also referred to as "contact operation (C)") may be carried out only once or may be repeated multiple times (i.e., the operation of dispersing the spray-dried particles in water, separating the particles from the resulting slurry, then dispersing the particles separated from the slurry again in water, and separating the particles from the resulting slurry may be carried out once or multiple times).
[0041] The step (c) may be a combination of the steps (c1) and (c2), for example a step (c3) of dispersing the spray-dried particles in water, separating the particles from the resulting slurry, and pouring water over the separated particles. From the viewpoint of removing impurities, the step (c) is preferably the step (c3).
[0042] When preparing a slurry during the step (c1) or the step (c3), the slurry is preferably stirred. The stirring time is, for example, 5 to 30 minutes. In the step (c1), the particles can be separated from the slurry by a conventional method, such as filtration or centrifugation.
[0043] In the step (c2), the particles can be separated from the water by pouring water over the particles placed on a filter paper. The temperature of the water used in the step (c) is preferably 50 to 90° C. from the viewpoint of the solubility of impurities. The pH of the slurry obtained in the step (c1) is preferably 3 to 10 from the viewpoint of suppressing the elution of silica and alumina. The pH is adjusted by adding, for example, hydrochloric acid or aqueous ammonia. In addition, from the viewpoint of removing alkali metals, it is preferable to use water containing an ammonium salt.
[0044] "Engineering (d)" In the step (d), the particles obtained in the step (b) (if the step (c) is carried out, the particles obtained in the step (c) are hereinafter collectively referred to as "raw material particles for FCC catalyst") are contacted with water containing an aluminum salt (usually an aqueous solution of an aluminum salt). The pH of the water containing the aluminum salt is 3.5 to 5.0, preferably 3.5 to 4.0, because when the pH is in this range, aluminum ions do not precipitate as hydroxides and aluminum contained in the raw material particles for FCC catalyst is not eluted. The amount of water containing the aluminum salt used is such that the mass of the aluminum salt, when converted to the mass of aluminum oxide (Al2O3) containing the same amount of aluminum, is 0.04 (Al2O3 [g-aluminum salt] / zeolite [g-FCC catalyst raw material particle]) or more relative to the mass of the zeolite contained in the FCC catalyst raw material particle. This is because the cations contained in the zeolite (USY or REUSY) contained in the FCC catalyst raw material particle can be sufficiently ion-exchanged with the aluminum ions. Therefore, if this value is less than 0.04, the aluminum ions cannot be sufficiently ion-exchanged, and if it exceeds 0.10, the amount of unnecessary aluminum salt increases, which is not economically preferable. Therefore, the amount of water containing the aluminum salt used is more preferably an amount such that Al2O3 [g-aluminum salt] / zeolite [g-FCC catalyst raw material particle] is 0.04 to 0.10, and even more preferably an amount such that 0.05 to 0.10.
[0045] By carrying out the step (d), an FCC catalyst is obtained. Although it is not necessarily certain, the USY and REUSY between each process 27 From the change in the peaks around 60 ppm and 0 ppm in the Al MAS NMR spectrum, it is speculated that in step (d), Al ions are exchanged with cations contained in the USY and REUSY. Examples of the cations include ammonium ions, rare earth metal ions, sodium ions, and protons, depending on the method for producing the USY and REUSY.
[0046] Examples of the aluminum salt include aluminum chloride, aluminum nitrate, aluminum sulfate, aluminum oxalate, and aluminum acetate, and among these, aluminum chloride is preferred.
[0047] The embodiment of the step (d) is, for example, (d1) dispersing the raw material particles for FCC catalyst in water containing an aluminum salt and separating the particles from the resulting slurry; and The process includes a step (d2) of pouring water containing an aluminum salt onto the raw material particles for the FCC catalyst.
[0048] In the step (d1), the operation of dispersing the FCC catalyst raw material particles in water containing an aluminum salt and separating the particles from the obtained slurry (hereinafter also referred to as "contact operation (D1)") may be performed only once or may be repeated multiple times (i.e., the operation of dispersing the FCC catalyst raw material particles in water containing an aluminum salt, separating the particles from the obtained slurry, then dispersing the particles separated from the slurry again in water containing an aluminum salt, and separating the particles from the obtained slurry may be performed once or multiple times).
[0049] When preparing a slurry in the step (d1), the obtained slurry is preferably stirred. The stirring time for each contact step (D1) is, for example, 5 to 30 minutes, and preferably 15 to 30 minutes.
[0050] In the step (d1), the particles can be separated from the slurry by a conventional method, such as filtration or centrifugation. In the step (d2), for example, water containing an aluminum salt is poured over the particles placed on a filter paper, so that the particles and the poured water (water containing an aluminum salt) can be separated. The time for pouring the water containing an aluminum salt in the step (d2) is, for example, 3 to 30 minutes.
[0051] Moreover, both the step (d1) and the step (d2) may be carried out. The particles that have been subjected to step (d1) or step (d2) may be contacted with water in the same manner as step (c). The temperature of the water is preferably 50 to 90° C. After contact with water, step (d1) or step (d2) may be repeated.
[0052] "Engineering (e)" The method for producing an FCC catalyst according to the present invention may include a step of drying the particles obtained through the step (d) because carrying out the step (e) reduces the moisture content of the particles, allowing the particles to be handled as dry particles.
[0053] The step (e) can be carried out by a conventionally known method, for example, by subjecting the particles obtained through the step (d) to a heat treatment at 100 to 180° C. for 6 to 24 hours.
[0054] <FCC Catalyst> The specific surface area of the FCC catalyst produced by the production method according to the present invention, as measured by the method employed in the examples described below, is preferably 200 to 400 m. 2 / g, more preferably 250 to 350 m 2 / g.
[0055] The method for producing an FCC catalyst according to the present invention makes it possible to produce an FCC catalyst that, when used in fluid catalytic cracking, improves the RON of gasoline and promotes the production of LPG, compared with an FCC catalyst produced using the same spray-dried particles but without going through step (d). The reason for this is presumably that the cationic sites of USY or REUSY are modified with aluminum cations, which increases the acid strength of USY or REUSY, causing over-cracking of fractions other than aromatics in gasoline (particularly isoparaffins and olefins), promoting the production of LPG, and increasing the proportion of aromatics in the gasoline fraction, thereby increasing LPG selectivity and RON. EXAMPLES
[0056] The present invention will now be described in more detail with reference to examples. [Measurement or Evaluation Method of Catalyst, etc.] (Loss on Ignition (LOI)) The ignition loss of the zeolites obtained in the Production Examples and the catalysts obtained in the Examples was calculated by heat treating the samples in air at 1000° C. for 1 hour and calculating the ignition loss according to the following formula. Ignition loss (mass%) = mass loss due to heat treatment / mass of sample before heat treatment × 100
[0057] (Composition) The content of each element contained in the zeolite obtained in the Production Examples and the catalyst obtained in the Examples was measured using a fluorescent X-ray analyzer (Rigaku Corporation, RIX 3000).
[0058] (Lattice Constant of Zeolite) The lattice constant of the zeolite was determined from the spacing between the diffraction planes (553) and (642) of the zeolite by X-ray diffraction method under the following conditions using anatase type TiO2 as a standard substance.
[0059] Measurement conditions The samples (USY or REUSY obtained in Production Examples 1 and 2, and catalysts obtained in Examples, etc.) were crushed and molded, and then set in an X-ray diffractometer (X-RAY DIFFRACT METER (RINT 1400) manufactured by Rigaku Corporation) and measured under the following conditions: tube voltage 30.0 kV, tube current 130.0 mA, anticathode Cu, measurement range: start angle to end angle (2θ) 10.000° to 70.000°, scan speed 2.000° / min, divergence slit 1 deg, scattering slit 1 deg, receiving slit 0.15 mm.
[0060] (Specific Surface Area) The specific surface area of the catalysts in the examples was measured using a BELSORP-mini Ver2.5.6 manufactured by Microtrack-Bell Corporation. Specifically, the catalyst was heat-treated at 500°C for 1 hour while being evacuated to a vacuum, and nitrogen gas was adsorbed onto the catalyst, and the specific surface area (m 2 / g) was calculated.
[0061] (Catalytic Activity) The catalysts in the examples were subjected to a performance evaluation test using ACE-MAT (Advanced Cracking Evaluation-Micro Activity Test). As a pretreatment, the catalyst was calcined at 600°C for 2 hours, and then heat-treated at 780°C for 13 hours in a 100% steam atmosphere. The reaction conditions in the catalyst performance evaluation test were as follows: Feedstock: 100% desulfurized vacuum gas oil (DSVGO) Reaction temperature: 520℃ Catalyst mass space velocity (WHSV): 8h -1 Catalyst / oil ratio: 3.75, 5.0 (mass% / mass%) Conversion rate: 100-(yield of LCO and HCO) Cutting temperature of produced oil Dry gas: H2+C1-C2 LPG:C3-C4 Gasoline: C5 ~ boiling point 216℃ Light cycle oil (LCO): boiling point range 216-343℃ Heavy cycle oil (HCO): boiling point range above 343°C Measurements were performed at catalyst / oil ratios of 3.75 and 5.0, and the respective yields at the same conversion were calculated by interpolation. Furthermore, the gasoline fraction of the product liquid was analyzed by gas chromatography (GC System HP6890A) manufactured by Agilent, and the octane number (RNO) was calculated.
[0062] [Production Example 1] (Preparation of Ultra-Stable Y-Type Zeolite (USY1)) The SiO2 / Al2O3 molar ratio is 5.2, the lattice constant is 2.466 nm, and the specific surface area is 720 m 2 / g, and the Na content is 13.0 mass% calculated as Na2O. The Na-Y type zeolite was subjected to ammonium salt ion exchange to obtain a SiO2 / Al2O3 molar ratio of 5.2, a lattice constant of 2.471 nm, and a specific surface area of 740 m 2NH4-Y type zeolite with a SiO2 / Al2O3 molar ratio of 5.2, a lattice constant of 2.457 nm, a specific surface area of 670 m2, and a lattice constant of 2.457 nm were obtained. 2 / g.
[0063] [Production Example 2] (Preparation of Rare Earth Metal-Containing Ultra-Stable Y-Type Zeolite (REUSY1)) The SiO2 / Al2O3 molar ratio is 5.2, the lattice constant is 2.466 nm, and the specific surface area is 720 m 2 / g, and the Na content is 13.0 mass% calculated as Na2O. The Na-Y type zeolite was obtained by ion-exchanging with ammonium salt. The SiO2 / Al2O3 molar ratio is 5.2, the lattice constant is 2.471 nm, and the specific surface area is 740 m 2 NH4-Y type zeolite having a Na content of 1.0 mass% in terms of Na2O was prepared. 50.0 kg of this NH4-Y type zeolite was suspended in 500 L of pure water at 60°C, and 62.7 kg of a rare earth metal chloride aqueous solution (containing La and Ce in a mass ratio of La:Ce=10:2, and containing 20 mass% of each rare earth metal in terms of oxide) was added, and these were stirred for 20 minutes. This dispersion was filtered, and 1000 L of pure water at 60°C was poured over the filtered solid. The obtained solid was left overnight in an oven at 120°C to dry, and REY type zeolite was obtained.
[0064] The resulting REY zeolite (3.0 kg) was calcined in a saturated steam atmosphere at 750°C for 2 hours to obtain about 2.7 kg of rare earth metal-containing ultra-stable Y zeolite (hereinafter referred to as "REUSY1"). This REUSY1 has a SiO2 / Al2O3 molar ratio of 5.32, a lattice constant of 2.463 nm, and a specific surface area of 598 m 2 / g, the Na content was 0.5 mass% calculated as Na2O, and the RE2O3 content was 12.2 mass%.
[0065] [Comparative Example 1] Kaolin, USY1 produced in Production Example 1, activated alumina (BK-112, manufactured by Sumitomo Chemical Co., Ltd.), and manganese oxide (Mn2O3) (manufactured by Tosoh Corporation) were prepared.
[0066] Commercially available No. 3 water glass and sulfuric acid were rapidly mixed with stirring to prepare a silica hydrosol containing 12.5 mass% silicon, calculated as a SiO2 concentration. 545 g (dry basis) of kaolin, 550 g (dry basis) of activated alumina, 875 g (dry basis) of USY1, 55 g (dry basis) of manganese oxide (Mn2O3), and water were added to 3,800 g of this silica hydrosol to prepare a slurry (a) with a solid concentration of 30 mass%.
[0067] Next, the slurry (a) was subjected to a pulverization and dispersion treatment using a colloid mill (TK150, manufactured by Tokushu Kakoh Co., Ltd.) at a discharge rate of 4 L / min to obtain a slurry (b). The slurry (b) was sprayed into a hot air current using a spray dryer under conditions of an inlet temperature of 250° C. and an outlet temperature of 150° C. to obtain spherical particles (1).
[0068] 400 g of spherical particles (1) (dry basis) was dispersed in 2 L of an aqueous solution containing 47 g of ammonium sulfate and stirred for 20 minutes. The dispersion was filtered, and 2 L of pure water at 60° C. was poured over the separated solids (particles).
[0069] The particles thus obtained (hereinafter also referred to as "particles (c1)") were left overnight in an oven at 140°C to dry, thereby obtaining FCC catalyst (c1). The evaluation results of FCC catalyst (c1) are shown in Tables 1 and 2.
[0070] [Example 1] The particles (c1) were obtained in the same manner as in Comparative Example 1. Next, an aqueous solution of 80 g of aluminum chloride (containing 9 mass% of Al as Al2O3) was added to 5 L of pure water and poured over 400 g of particles (c1) (containing 35 mass% of zeolite). The pH of this aqueous solution was 3.6. Then, 2 L of pure water at 60°C was poured over.
[0071] The particles thus obtained were dried overnight in an oven at 140° C. to obtain FCC catalyst (1). The evaluation results of FCC catalyst (1) are shown in Tables 1 and 2.
[0072] [Comparative Example 2] The particles (c1) were obtained in the same manner as in Comparative Example 1. Next, 57.5 g of a rare earth metal chloride aqueous solution (containing La and Ce in a mass ratio of La:Ce=10:2, and containing 20 mass% of each rare earth metal in terms of oxide) was added to 2.5 L of pure water and poured over 400 g of particles (c1) (containing 35 mass% of zeolite). The pH of this aqueous solution was 5.3. Next, 2 L of pure water at 60°C was poured over.
[0073] The particles thus obtained were dried overnight in an oven at 140° C. to obtain FCC catalyst (c2). The evaluation results of FCC catalyst (c2) are shown in Tables 1 and 2.
[0074] [Comparative Example 3] The particles (c1) were obtained in the same manner as in Comparative Example 1. Next, an aqueous solution of 40 g of aluminum chloride (containing 9 mass% of Al as Al2O3) was added to 2.5 L of pure water and poured over 400 g of particles (c1) (containing 35 mass% of zeolite). The pH of this aqueous solution was 3.6. Then, 2 L of pure water at 60°C was poured over.
[0075] The particles thus obtained were dried overnight in an oven at 140° C. to obtain FCC catalyst (c3). The evaluation results of FCC catalyst (c3) are shown in Tables 1 and 2.
[0076] [Comparative Example 4] Kaolin, REUSY1 produced in Production Example 2, activated alumina (BK-112, manufactured by Sumitomo Chemical Co., Ltd.), and manganese oxide (Mn2O3) (manufactured by Tosoh Corporation) were prepared.
[0077] Commercially available No. 3 water glass and sulfuric acid were rapidly mixed and stirred to prepare a silica hydrosol containing 12.5 mass% silicon, calculated as a SiO2 concentration. 545 g (dry basis) of kaolin, 550 g (dry basis) of activated alumina, 875 g (dry basis) of REUSY1, 55 g (dry basis) of manganese oxide (Mn2O3), and water were added to 3,800 g of this silica hydrosol to prepare a slurry (a') with a solid concentration of 30 mass%.
[0078] Next, the slurry (a') was subjected to a pulverization and dispersion treatment using a colloid mill (TK150, manufactured by Tokushu Kakoh Co., Ltd.) at a discharge rate of 4 L / min to obtain a slurry (b'). The slurry (b') was sprayed into a hot air current using a spray dryer under conditions of an inlet temperature of 250°C and an outlet temperature of 150°C to obtain spherical particles (1').
[0079] 400 g of spherical particles (1') (dry basis) was dispersed in 2 L of an aqueous solution containing 47 g of ammonium sulfate and stirred for 20 minutes. The dispersion was filtered, and 2 L of pure water at 60°C was poured over the separated solids (particles).
[0080] The particles thus obtained (hereinafter also referred to as "particles (c1')") were left overnight in an oven at 140°C to dry, thereby obtaining FCC catalyst (c4). The evaluation results of FCC catalyst (c4) are shown in Tables 3 and 4.
[0081] [Example 2] The particles (c1') were obtained in the same manner as in Comparative Example 4. Next, an aqueous solution of 80 g of aluminum chloride (containing 9 mass% of Al as Al2O3) was added to 5 L of pure water and poured over 400 g of particles (c1') (containing 35 mass% of zeolite). The pH of this aqueous solution was 3.6. Next, 2 L of pure water at 60°C was poured over.
[0082] The particles thus obtained were dried overnight in an oven at 140° C. to obtain FCC catalyst (2). The evaluation results of FCC catalyst (2) are shown in Tables 3 and 4.
[0083] [Comparative Example 5] The particles (c1') were obtained in the same manner as in Comparative Example 4. Next, 57.5 g of rare earth metal chloride aqueous solution (containing La and Ce in a mass ratio of La:Ce=10:2, and containing 20 mass% of each rare earth metal in terms of oxide) was added to 2.5 L of pure water and poured over 400 g of particles (c1') (containing 35 mass% of zeolite). The pH of this aqueous solution was 5.3. Next, 2 L of pure water at 60°C was poured over.
[0084] The particles thus obtained were dried overnight in an oven at 140° C. to obtain FCC catalyst (c5). The evaluation results of FCC catalyst (c5) are shown in Tables 3 and 4.
[0085] [Table 1]
[0086] [Table 2]
[0087] [Table 3]
[0088] [Table 4]
Claims
1. (a) The ratio of silicon atoms to aluminum atoms is Al 2 O 3 SiO 2 a step of mixing a zeolite having a lattice constant of 2.447 to 2.467 nm and / or a rare earth metal-containing ultrastable Y-type zeolite having a lattice constant of 2.455 to 2.475 nm, in which the molar ratio is 5.0 to 6.0, with at least one silica-based matrix forming component selected from silica, silica gel, silica sol, water glass, and silicic acid liquid, with water, and optionally with clay minerals, and optionally with additives, to prepare a raw material slurry; (b) spray-drying the raw slurry to obtain particles; and (d) contacting the particles obtained in the step (b) with water containing an aluminum salt and having a pH of 3.5 to 5.0 in a ratio of (mass of aluminum salt converted into mass of aluminum oxide) / (mass of zeolite contained in the particles) of 0.04 to 0.10; A method for producing a fluid catalytic cracking catalyst comprising the steps of:
2. (c) contacting the particles obtained in step (b) with water. and in the step (d), particles obtained in the step (b) are those that have been subjected to the step (c).
3. 3. The method for producing a fluid catalytic cracking catalyst according to claim 1, wherein a metal capture agent is mixed as the additive in the step (a).
4. The method for producing a fluid catalytic cracking catalyst according to any one of claims 1 to 3, wherein an active matrix component is mixed as the additive in the step (a).
5. The method for producing a fluid catalytic cracking catalyst according to any one of claims 1 to 4, wherein the silica-based matrix-forming component is a silica sol.
Citation Information
Patent Citations
fcc method with mesoporous catalyst
JP2008501522A
Manufacturing method of fluid catalytic cracking catalyst
JP2009000657A
Catalyst for fluid catalytic cracking and method for producing the same
JP2014231034A
Catalyst for residual oil decomposition active fluid catalytic cracking and manufacturing method therefor
JP2017087204A
Aluminum faujasites, catalyst containing same and process of producing same
US4224188A