Ziegler-Natta catalyst system having treated magnesium chloride component

A procatalyst system with a high surface area magnesium chloride support, titanium component, and high oxidation state transition metal compound addresses the limitation of Ziegler-Natta catalysts, enhancing ethylene-based polymer HDF and molecular weight for improved polymer performance.

JP7576466B2Active Publication Date: 2024-10-31DOW GLOBAL TECHNOLOGIES LLC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020564642
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-06-01
Filing Date
2019-05-29
Publication Date
2024-10-31
Estimated Expiration
2039-05-29

AI Technical Summary

Technical Problem

Ziegler-Natta catalysts are limited in their ability to produce ethylene-based polymers with differentiated densities, particularly high density fractions, necessitating the development of procatalysts and catalysts that can enhance the high density fraction (HDF) of such polymers.

Method used

A procatalyst system comprising a preformed magnesium chloride catalyst support with a high surface area, a titanium-containing component, a chlorinating agent, and a hydrocarbon-soluble transition metal compound in a high oxidation state (excluding vanadium) is used to produce ethylene-based polymers with increased HDF.

Benefits of technology

The procatalyst system significantly enhances the molecular weight and HDF of ethylene-based polymers, achieving higher catalyst efficiency and polymer properties suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576466000001
    Figure 0007576466000001
  • Figure 0007576466000002
    Figure 0007576466000002
  • Figure 0007576466000003
    Figure 0007576466000003
Patent Text Reader

Abstract

Pro catalyst is 100m 2 The catalyst includes a preformed magnesium chloride catalyst support having a surface area of ​​1 / g or greater, a titanium-containing component, a chlorinating agent, and a hydrocarbon-soluble transition metal compound having an oxidation state of 5+ or greater, wherein the hydrocarbon-soluble transition metal compound having an oxidation state of 5+ or greater is not vanadium. [Selection diagram] None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Application No. 62 / 679,279, filed June 1, 2018, which is incorporated by reference in its entirety.

[0002] FIELD OF THE DISCLOSURE Embodiments of the present disclosure relate generally to procatalysts comprising high oxidation state transition metal compounds that can be used to produce ethylene-based polymers. More specifically, embodiments of the present disclosure relate to procatalysts comprising high oxidation state transition metal compounds that, excluding vanadium, can be used to produce ethylene-based polymers with increased density fractions. [Background technology]

[0003] Ethylene-based polymers are commonly used in a variety of applications, depending on the structure of the polymer. For example, high density polyethylene (HDPE) can be used as bottles, piping, geomembranes, plastic lumber, etc. It is estimated that about 30 million metric tons of HDPE are produced each year.

[0004] HDPE has a high strength-to-density ratio. Although its density is only slightly higher than that of low-density polyethylene (LDPE), HDPE has very little branching, which gives it greater intermolecular forces and tensile strength than LDPE. The difference in strength outweighs the difference in density, giving HDPE a higher strength-to-weight ratio. It is also harder, more opaque, and can withstand somewhat higher temperatures (e.g., 120°C / 248°F for short periods). The lack of branching can be ensured by proper choice of catalyst and reaction conditions.

[0005] Ziegler-Natta catalysts have been used for many years in the production of various polyethylenes, including HDPE. These catalysts generally comprise a magnesium halide support and at least one catalytic compound. Summary of the Invention

[0006] Although Ziegler-Natta catalysts are effective, they are generally limited in their ability to produce differentiated polymers, such as making ethylene-based polymers with very high or very low polymer density under normal polymerization conditions. Thus, there is a continuing need for procatalysts, catalysts, and processes for producing new, differentiated HDPE polymers. In particular, there is a continuing need for procatalysts, catalysts, and processes for producing ethylene-based polymers with increased high density fraction (HDF). The present disclosure relates to procatalysts, catalysts, and processes utilizing these procatalysts and catalysts to produce ethylene-based polymers with increased HDF.

[0007] According to at least one embodiment, the procatalyst is 100 m 2 / g or greater, a titanium-containing component, a chlorinating agent, and a hydrocarbon-soluble transition metal compound having an oxidation state of 5+ or greater, wherein the hydrocarbon-soluble transition metal compound having an oxidation state of 5+ or greater is free of vanadium.

[0008] According to another embodiment, the catalyst is 2 / g or greater, a titanium-containing component, a chlorinating agent, a hydrocarbon-soluble transition metal compound having an oxidation state of 5+ or greater, and an alkylaluminum cocatalyst, wherein the hydrocarbon-soluble transition metal compound having an oxidation state of 5+ or greater is free of vanadium.

[0009] According to another embodiment, the method for preparing the procatalyst comprises the steps of: 2(A) a titanium-containing component, (B) a chlorinating agent, and (C) a hydrocarbon-soluble transition metal compound having an oxidation state of 5+ or greater, added to a magnesium chloride catalyst support having a surface area of ​​1000 nm / g or greater, wherein at least one of (A), (B), or (C) is added to the magnesium chloride catalyst support separated in time from at least one other of (A), (B), or (C), and wherein the hydrocarbon-soluble transition metal compound having an oxidation state of 5+ or greater does not contain vanadium.

[0010] Additional features and advantages are set forth in the following Detailed Description, and in part will be readily apparent to those skilled in the art from that description or will be recognized by practicing the embodiments described herein, including the following Detailed Description, and the claims. It is to be understood that both the foregoing general description and the following detailed description are intended to provide an overview or framework for describing the various embodiments and for understanding the nature and characteristics of the claimed subject matter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The term "polymer" refers to a polymeric compound prepared by polymerizing monomers, whether of the same or different types. Thus, the generic term polymer encompasses the term "homopolymer," which is commonly used to refer to a polymer prepared from only one type of monomer, as well as "copolymer," which refers to a polymer prepared from two or more different monomers.

[0012] "Ethylene-based polymer" means a polymer containing more than 50% by weight of units derived from ethylene monomers. This includes polyethylene homopolymers or copolymers (meaning units derived from two or more comonomers). Common forms of ethylene-based polymers known in the art include low density polyethylene (LDPE), linear low density polyethylene (LLDPE), ultra low density polyethylene (ULDPE), very low density polyethylene (VLDPE), single-site catalyzed linear low density polyethylene (m-LLDPE) containing both linear and substantially linear low density resins, medium density polyethylene (MDPE), and high density polyethylene (HDPE).

[0013] As used herein, a "solution polymerization reactor" is a vessel in which solution polymerization is carried out, where ethylene monomer is dissolved in a non-reactive solvent containing, optionally, a comonomer and a catalyst, and then polymerized or copolymerized. Heat can be removed from or added to a solution polymerization reactor by coupling the reactor to a heat exchanger. Hydrogen can be utilized in solution polymerization processes, but is not required in all solution polymerization processes.

[0014] Ziegler-Natta catalysts are commonly used to produce ethylene-based polymers in processes that polymerize ethylene, and optionally produce one or more alpha-olefin comonomers. In these polymerization processes involving typical Ziegler-Natta catalysts, the average molecular weight of the polymer decreases rapidly as the polymerization temperature increases. However, higher polymerization temperatures in solution polymerization processes can increase production throughput and produce ethylene-based polymers with desirable properties such as excellent optics and dart / tear balance. Increasing the molecular weight capabilities of Ziegler-Natta catalysts can expand the ability to make new products and allow operation at higher polymerization temperatures.

[0015] The present disclosure is directed to Ziegler-Natta type procatalysts and catalysts comprising the procatalysts that exhibit increased molecular weight capability and exhibit the ability to increase the HDF of ethylene-based polymers. As used herein, a "procatalyst" is a catalyst composition that is essentially catalytically inactive prior to contact with a cocatalyst and becomes catalytically active upon contact with the cocatalyst. The procatalysts disclosed herein, in embodiments, are capable of being used in a range of 100 to 2000 cycles. 2 / g or greater, a titanium-containing component, a chlorinating agent, and a hydrocarbon soluble transition metal compound having an oxidation state of 5+ or greater, wherein the hydrocarbon soluble transition metal compound having an oxidation state of 5+ or greater is free of vanadium. Embodiments also include catalysts comprising a procatalyst and an alkyl aluminum cocatalyst, and polymerization processes comprising the procatalyst and / or the catalyst.

[0016] The MgCl2 component may be prepared by selecting an organomagnesium compound or a complex containing an organomagnesium compound and reacting the organomagnesium compound with a chloride compound, such as a metal or nonmetal chloride, under conditions suitable to make the MgCl2 component. Examples of organomagnesium compounds and / or complexes may include, but are not limited to, C2-C8 alkyl and aryl magnesium, magnesium alkoxides and aryloxides, carboxylated magnesium alkoxides, and carboxylated magnesium aryloxides, or combinations thereof. In some embodiments, the organomagnesium compound may include C2-C8 alkyl magnesium, magnesium C1-C4 alkoxide, or combinations thereof. In some embodiments, the organomagnesium compound may be butylethyl magnesium.

[0017] In one or more embodiments, the MgCl component includes, for example, the reaction product of a chloride source and a hydrocarbon-soluble hydrocarbyl magnesium compound or mixture of compounds. Exemplary organomagnesium compounds are di(C1-C 20 ) Alkyl magnesium or di(C6-C 20) arylmagnesium compounds, particularly di(n-butyl)magnesium, di(sec-butyl)magnesium, diisopropylmagnesium, di-n-hexylmagnesium, isopropyl-n-butyl-magnesium, ethyl-n-hexylmagnesium, ethyl-n-butylmagnesium, di-n-octylmagnesium, and combinations thereof. Exemplary suitable diarylmagnesiums include diphenylmagnesium, dibenzylmagnesium, and ditolylmagnesium. The organomagnesium compounds may be optionally treated with organoaluminum compounds to improve solubility, reduce the viscosity of the solution, or improve solubility and reduce the viscosity of the solution. Stabilizers may also be present, including those derived from substituted phenolic compounds. Additional suitable organomagnesium compounds include alkylmagnesium and arylmagnesium alkoxides, aryloxides and chlorides, and mixtures of the foregoing. Highly preferred organomagnesium compounds are halogen-free organomagnesium compounds.

[0018] Among the chloride sources that may be used in the preparation of the MgCl2 component for use herein are metal chlorides and non-metal chlorides, including organic chlorides and hydrogen chloride. Suitable metal chlorides that may be used herein include MR y-a Cl a where M is a metal in Group 13, 14, or 15 of the Periodic Table of the Elements, R is a monovalent organic radical, y has a value corresponding to the valency of M, and a has a value from 1 to y.

[0019] In one or more embodiments, the metal chloride has the formula: AlR 3-a Cl a wherein each R is independently selected from alkylaluminum chlorides having the formula: 10)hydrocarbyl, preferably (C1-C6)alkyl, and a is a number from 1 to 3. The alkylaluminum chloride may include, but is not limited to, ethylaluminum sesquichloride, diethylaluminum chloride, and ethylaluminum dichloride, with ethylaluminum dichloride being particularly preferred. Alternatively, metal chlorides such as aluminum trichloride, or a combination of aluminum trichloride and alkylaluminum chlorides or trialkylaluminum compounds may be suitably used.

[0020] Suitable nonmetal chloride and organic chlorine compounds have the formula R'Cl r In the formula, R' is hydrogen or (C1-C 10 ) hydrocarbyl or a nonmetal such as Si, Ga or Ge, and the subscript r is an integer from 1 to 6. Particularly suitable chloride sources include, for example, hydrogen chloride and active organic chlorides such as t-alkyl chlorides, sec-alkyl chlorides, allyl chloride, and benzyl chloride and other active hydrocarbyl chlorides in which the hydrocarbyl is as previously described herein. By active organic chlorides is meant hydrocarbyl chlorides that are at least as active as the chloride of sec-butyl chloride, preferably as active as t-butyl chloride, i.e., contain an unstable chloride that is easily lost to another compound. In addition to organic monochlorides, it is understood that organic dichlorides, trichlorides and other polychlorides that are active as previously defined herein may also be suitably used. Examples of preferred chloride sources include hydrogen chloride, t-butyl chloride, t-amyl chloride, allyl chloride, benzyl chloride, crotyl chloride, and diphenylmethyl chloride. Most preferred are hydrogen chloride, t-butyl chloride, allyl chloride, and benzyl chloride.

[0021] The organomagnesium halide can be preformed from an organomagnesium compound and a chloride source and stored for later use, or can be preformed in situ, in which case the procatalyst is preferably prepared by combining (1) the organomagnesium component and (2) the chloride source, followed by the other procatalyst components, in a suitable solvent or reaction medium.

[0022] In embodiments, the organomagnesium compound or complex may be soluble in a hydrocarbon diluent, such as an inert hydrocarbon diluent. Examples of hydrocarbon diluents may include, but are not limited to, liquefied ethane, propane, isobutane, n-butane, n-hexane, various isomeric hexanes, isooctane, paraffinic mixtures of alkanes having 5 to 30 carbon atoms, industrial solvents composed of saturated or aromatic hydrocarbons, such as cyclohexane, methylcyclopentane, dimethylcyclohexane, dodecane, kerosene, naphtha, and combinations thereof. In some embodiments, the hydrocarbon diluent may be substantially free of any impurities, including alkynes, dienes, arenes, and any compounds containing one or more heteroatoms. As used herein, the term "substantially free" of a component means that the composition contains less than 0.1% by weight of a component (e.g., impurities, compounds, elements, etc.). In some embodiments, the hydrocarbon diluent may have a boiling point in the range of about -50°C to about 200°C. The hydrocarbon diluent may, in embodiments, include an isoparaffinic solvent. Examples of isoparaffinic solvents may include, but are not limited to, ISOPAR™ synthetic paraffinic solvents available from ExxonMobile (e.g., ISOPAR™ E paraffinic solvents), and special boiling point (SBP) solvents by Shell Chemicals (e.g., SBP 100 / 140 high purity dearomatized hydrocarbon solvents). Other examples of hydrocarbon diluents may include methylcyclopentane, ethylbenzene, cumene, decalin, and combinations thereof.

[0023] The organomagnesium compound may be dispersed in a hydrocarbon diluent to form a slurry. A chloride compound may be added to the slurry to contact the organomagnesium compound with the chloride compound to produce MgCl2. The chloride compound may be a metal or nonmetal chloride. For example, in some embodiments, the chloride compound may be hydrochloride gas. In embodiments, the organomagnesium compound and the chloride compound may be contacted at a temperature between -25°C and 100°C, or between 0°C and 50°C. In some embodiments, heat removal is required to control the set reaction temperature to within ±5°C, such as ±3°C. In some embodiments, the amount of chloride source is controlled to achieve a target molar ratio of Cl to Mg in the resulting MgCl2. For example, the molar ratio of Cl to Mg may be 1.8 to 2.0 for chloride-deficient MgCl2 supports and 2.0 to 2.2 for chloride-rich MgCl2 supports. In some embodiments, the slurry of the organomagnesium compound and the metal or nonmetal chloride may be contacted for a time between 1 hour and 12 hours, or between 4 hours and 6 hours. The concentration of the organomagnesium compound in the slurry (i.e., before the chloride compound is added to the slurry) can be sufficient such that when the chloride compound is added to the slurry, the resulting composition can include a magnesium concentration of from 0.005 moles per liter (mol / L) to 1.000 moles / L.

[0024] The reaction of the organomagnesium compound with the metal or nonmetal chloride produces a MgCl2 component, which may be present in a MgCl2 slurry comprising MgCl2 particles dispersed in a hydrocarbon diluent. In some embodiments, the MgCl2 slurry is prepared prior to treatment with other procatalyst components, and is referred to herein as a "preformed MgCl2 slurry." In some embodiments, the MgCl2 slurry may have a concentration of MgCl2 from 0.005 mol / L to 10.00 mol / L, or from 0.05 mol / L to 1.00 mol / L.

[0025] In embodiments, the MgCl2 component may be formed by solution precipitation of a hydrocarbon soluble alkylmagnesium precursor with a non-metal chloride. The alkylmagnesium precursor may be a C2-C8 alkylmagnesium precursor in some embodiments. The non-metal chloride may be hydrochloride gas in some embodiments. The hydrocarbon soluble alkylmagnesium precursor and the non-metal chloride are added to a hydrocarbon diluent, such as, for example, the hydrocarbon diluents described in this disclosure. The conditions for this precipitation process are the same as those previously disclosed for forming the organomagnesium compound.

[0026] In an embodiment, the MgCl component is 150 mM 2 / g or more, or 200m 2 / g or more, 300m 2 / g or more, 400m 2 / g or more, such as a surface area of ​​100 square meters per gram (m 2 / g) or more. In some embodiments, the upper limit of the surface area of ​​the MgCl component is 800 m 2 / g.

[0027] Following preparation of the MgCl2 component, the MgCl2 component can be contacted with a chlorinating agent having the structural formula A(Cl): x (R 1 ) 3-x or Si(Cl) y (R 1 ) 4-y wherein R 1 is (C1~C 30) hydrocarbyl, x is 1, 2, or 3, and y is 1, 2, 3, or 4. In some embodiments, A can be aluminum or boron. Examples of chlorinating agents include, but are not limited to, aluminum trichloride, methylaluminum dichloride, dimethylaluminum chloride, ethylaluminum dichloride, diethylaluminum chloride, ethylaluminum sesquichloride, isobutylaluminum dichloride, diisobutylaluminum chloride, boron trichloride, phenylboron dichloride, dicyclohexylboron chloride, silicon tetrachloride, methyltrichlorosilane, dimethyldichlorosilane, chlorotrimethylsilane, ethyltrichlorosilane, dichlorodiethylsilane, chlorotriethylsilane, n-propyltrichloro ... In some embodiments, the chlorinating agent may include an alkylaluminum chloride, dichlorodi(n-propyl)silane, chlorotri(n-propyl)silane, isopropyltrichlorosilane, dichlorodiisopropylsilane, chlorotriisopropylsilane, n-butyltrichlorosilane, dichlorodi(n-butyl)silane, chlorotri(n-butyl)silane, isobutyltrichlorosilane, dichlorodiisobutylsilane, chlorotriisobutylsilane, cyclopentyltrichlorosilane, dicyclopentyldichlorosilane, n-hexyltrichlorosilane, cyclohexyltrichlorosilane, dichlorodicyclohexylsilane, or combinations thereof. In some embodiments, the chlorinating agent is an alkylaluminum chloride.

[0028] The MgCl2 component may be contacted with the chlorinating agent under conditions sufficient to condition the MgCl2 component. In embodiments, the MgCl2 component may be contacted with the chlorinating agent at a temperature between 0°C and 50°C, such as between 0°C and 35°C, between 25°C and 50°C, or between 25°C and 35°C. The MgCl2 component may be contacted with the chlorinating agent for a time between 4 hours and 24 hours, such as between 4 hours and 12 hours, between 6 hours and 24 hours, or between 6 hours and 12 hours. Without intending to be bound by any theory, it is believed that conditioning the MgCl2 component by contacting the MgCl2 component with a chlorinating agent may promote or enhance the adsorption of additional metals, such as titanium species, onto the MgCl2 component. In some embodiments, the procatalyst may include a molar ratio of chlorinating agent to MgCl2 component in the heterogeneous procatalyst of 3:40 to 40:40, such as 3:40 to 20:40, or 20:40 to 40:40.

[0029] The MgCl2 component may be further contacted with a titanium-containing component. The titanium-containing component may be any titanium compound or complex. In some embodiments, the titanium-containing component may include a titanium halide, a titanium alkoxide, or a combination thereof. For example, in embodiments, the titanium-containing component may include, but is not limited to, titanium tetrachloride (TiCl4), titanium isopropoxide (TiPT), other titanium halides or titanium alkoxides, Ti(OR)4 (where R is C1-C10), titanium tetrachloride (TiCl4), titanium isopropoxide (TiPT), other titanium halides or titanium alkoxides, Ti(OR)4 (where R is C1-C10), titanium alkoxide (TiPT ... 21 ) hydrocarbyl, or combinations thereof.

[0030] The MgCl2 component may be contacted with the titanium-containing component under conditions such that at least a portion of the titanium-containing component is adsorbed onto the MgCl2 component. For example, in embodiments, the MgCl2 component may be contacted with the titanium-containing component at a temperature between 0°C and 150°C, such as between 0°C and 35°C, between 25°C and 50°C, or between 25°C and 35°C. In some embodiments, the MgCl2 component may be contacted with the titanium-containing component at such temperatures for a period between 3 hours and 24 hours, such as between 3 hours and 12 hours, between 6 hours and 24 hours, or between 6 hours and 12 hours. In some embodiments, the MgCl2 component is contacted with the titanium-containing component after the MgCl2 component is conditioned by the chlorinating agent. In other embodiments, the MgCl2 component is contacted with the titanium-containing component before the MgCl2 component is contacted with the chlorinating agent. In still other embodiments, the MgCl2 component may be contacted with the chlorinating agent and the titanium-containing component simultaneously by adding the chlorinating agent and the titanium-containing component simultaneously to the MgCl2 slurry. The chlorinating agent, in embodiments, may react with the titanium-containing component as well as the MgCl2 component. For example, the chlorinating agent may react with titanium in the titanium-containing component to form titanium chlorides, such as, for example, TiCl3, or TiCl4.

[0031] The procatalyst of the embodiment also includes a hydrocarbon-soluble transition metal compound having an oxidation state of 5+ or higher, the transition metal compound being free of vanadium (hereinafter referred to as "transition metal compound"). For example, the transition metal compound may be combined with the MgCl2 component and, optionally, one or both of the titanium-containing component and the chlorinating agent dispersed in the hydrocarbon diluent. In some embodiments, the transition metal compound may be a metal-ligand complex and may be represented by the structural formula (L): n M(XR 2 ) b where M is a transition metal in an oxidation state of 5+ or higher, excluding vanadium, each L is a neutral ligand or (=O), and each XR 2 is an anionic ligand, X is a heteroatom, and R 2 is (C1~C 20 ) hydrocarbyl or (C1-C 20) heterohydrocarbyl, n is 0 (zero), 1, or 2, and b is 1, 2, 3, or 4. The metal-ligand complex may be neutral in overall charge. In embodiments, the metal-ligand complex is soluble in a hydrocarbon solvent, such as the hydrocarbon diluents previously described in this disclosure. In some embodiments, one or more of L may be a neutral ligand. In some embodiments, one or more of L may include a neutral ligand, including, for example, a nitrogen- or phosphorus-containing compound, such as ammonia, a nitrile, pyridine, an amine, a phosphine, or a combination thereof. Examples of neutral ligands may include, but are not limited to, acetonitrile, pyridine, ammonia, ethylenediamine, triphenylphosphine, other neutral ligands, or a combination thereof. In some embodiments, one or more of L may be an oxo group (=O). In some embodiments, X may be oxygen.

[0032] In some embodiments, the metal-ligand complex can be a metal alkoxide, a metal oxyalkoxide, a metal halide, or a metal oxyhalide. In embodiments, the metal-ligand complex has the structure MX n-b (OR 2 ) b where M is a transition metal (not including vanadium) having an oxidation state "n" of 5+ or higher, X is a halogen, b can be 0 to n, and R 2 is (C1~C 20 ) hydrocarbyl or (C1-C 20 In another embodiment, the metal-ligand complex has the structure M(=O)X n-b (OR 2 ) b where M is a transition metal (excluding vanadium) having an oxidation state n of 5+ or greater, X is a halogen, b can be 0 to n-2, and R 2 is (C1~C 20 ) hydrocarbyl or (C1-C 20 ) heterohydrocarbyl.

[0033] In some embodiments, the transition metal compound, such as M in the aforementioned metal ligand, may be a transition metal selected from the group consisting of molybdenum (Mo), niobium (Nb), tantalum (Ta), tungsten (W), iron (Fe), zirconium (Zr), chromium (Cr), manganese (Mn), zinc (Zn), and combinations thereof, each having an oxidation state of 5+ or higher. The transition metal compound does not include vanadium.

[0034] In embodiments, the transition metal compound may be combined with a slurry containing the MgCl2 component before or after either the titanium-containing component and the chlorinating agent are dispersed in the slurry containing the MgCl2 component. In some embodiments, the transition metal compound may be combined with a slurry containing the MgCl2 component (optionally including the titanium-containing component and / or the chlorinating agent) and mixed for a period of 0.5 minutes to 24 hours, such as 30 minutes to 12 hours.

[0035] As discussed in this disclosure, the procatalyst comprises (A) a titanium-containing component; (B) a chlorinating agent; (C) a transition metal compound having an oxidation state of 5+ or higher, excluding vanadium; and (D) 100mM of a chlorinating agent. 2 and a MgCl2 component having a surface area of ​​10 ...

[0036] Components (A), (B), (C), and (D) may be present in the procatalyst in various ratios. In embodiments, the molar ratio of the transition metal present in the transition metal compound to the titanium present in the titanium-containing compound (i.e., transition metal (mol) / Ti (mol)) is from 0.1 to 10.0, such as from 0.2 to 5.0, or from 0.5 to 3.0. In embodiments, the molar ratio of the chlorinating agent to the titanium present in the titanium-containing component (i.e., chlorinating agent (mol) / Ti (mol)) is from 0.5 to 100.0, such as from 2.0 to 50.0, or from 5.0 to 20.0. In embodiments, the molar ratio of the MgCl2 component to the titanium present in the titanium-containing component (i.e., MgCl2 (mol) / Ti (mol)) is from 1.0 to 100.0, such as from 8.0 to 80.0, or from 15.0 to 50.0.

[0037] In embodiments, a cocatalyst may be combined with a procatalyst disclosed herein to produce a catalyst system. The cocatalyst may include at least one organometallic compound, such as an alkyl or haloalkyl of aluminum, an alkylaluminum halide, a Grignard reagent, an alkali metal aluminum hydride, an alkali metal borohydride, an alkali metal hydride, or an alkaline earth metal hydride. In some embodiments, the cocatalyst is an alkyl of aluminum. The formation of the catalyst system from the reaction of the procatalyst and the cocatalyst may be carried out in situ (in place) or immediately prior to entering the polymerization reactor. Thus, the combination of the procatalyst and the cocatalyst may occur under a wide variety of conditions. Such conditions may include, for example, contacting the procatalyst and the cocatalyst at a temperature between 0° C. and 250° C., such as between 0° C. and 200° C., between 15° C. and 250° C., or between 15° C. and 200° C., under an inert atmosphere, such as nitrogen, argon, or other inert gas. The preparation of the catalytic reaction product (i.e., the catalyst system) does not require separation of the hydrocarbon-soluble components from the hydrocarbon-insoluble components. In some embodiments, the procatalyst and the cocatalyst may be introduced simultaneously into the reactor and contact each other in the reactor. In some embodiments, the catalyst system may have a molar ratio of cocatalyst to titanium species in the titanium-containing component of the procatalyst of 3:1 to 20:1, such as 3:1 to 15:1, 3:1 to 10:1, 3:1 to 8:1, 5:1 to 20:1, 5:1 to 15:1, 5:1 to 10:1, 8:1 to 20:1, or 8:1 to 15:1.

[0038] Once the catalyst system comprising the procatalyst and the cocatalyst is prepared, the catalyst system may be used in a polymerization or copolymerization process to polymerize olefins. For example, in some embodiments, the catalyst system may be utilized in a polymerization or copolymerization process to make ethylene-based polymers, such as, for example, HDPE and linear low density polyethylene (LLDPE). In some embodiments, the polymerization or copolymerization process may include contacting ethylene monomer and optionally one or more α-olefin comonomers with the catalyst system comprising the procatalyst and optionally a cocatalyst to form an ethylene-based polymer. The olefin polymerization / copolymerization reaction may be carried out in a reaction medium. The reaction medium may be any of the hydrocarbon diluents, such as isoparaffins, aliphatic hydrocarbons, or other hydrocarbon diluents previously disclosed in this disclosure. The olefin polymerization / copolymerization process may include contacting an olefin or combination of olefins with the reaction medium in the presence of the catalyst system comprising the procatalyst composition and optionally a cocatalyst. The polymerization conditions may be suitable, and a molecular weight regulator, such as, for example, hydrogen, may also be present in the reaction vessel to suppress the formation of undesirable high molecular weight polymers.

[0039] Any ethylene polymerization or copolymerization reaction process may be used with the catalysts disclosed herein to produce an ethylene-based polymer. Such ethylene polymerization or copolymerization reaction processes may include, but are not limited to, slurry phase polymerization processes, solution phase polymerization processes, gas phase processes, and combinations thereof. The polymerization or copolymerization process may be carried out in one or more conventional reactors, examples of which may include, but are not limited to, loop reactors, stirred tank reactors, batch reactors in parallel or series, and / or any combination thereof. In some embodiments, the polymerization process may be carried out in two or more reactors in series, parallel, or combinations thereof. In other embodiments, the polymerization process may be carried out in a single reactor. The polymerization process may be a batch polymerization process or a continuous polymerization process. For example, in some embodiments, the polymerization process may be a batch polymerization process that may be carried out in a stirred tank reactor. In some embodiments, the polymerization process may be continuous, such as a polymerization reaction carried out in a continuous solution polymerization reactor. In other embodiments, the polymerization process may include two or more polymerization steps. In these embodiments, the catalyst system including the procatalysts disclosed herein may be used in any one or more polymerization steps.

[0040] The polymers produced from the polymerization / copolymerization processes utilizing the procatalysts and / or catalysts disclosed herein may be C2-C olefins such as ethylene, propylene, or 4-methyl-1-pentene. 20 In some embodiments, the polymers formed in the presence of the procatalysts and / or catalysts disclosed herein can be homopolymers of ethylene or propylene and at least one or more α-olefin comonomers, C2-C4 20 Acetylenic unsaturated comonomers, and / or C4-C 18 In some embodiments, the polymer may include interpolymers of ethylene and the above C3-C6 copolymers in combination with other unsaturated comonomers. 20The ethylene-based polymer may be an α-olefin comonomer, such as an interpolymer with at least one of an α-olefin, a diolefin, and / or an acetylenically unsaturated comonomer. In some embodiments, the comonomer may be an α-olefin comonomer having 20 or fewer carbon atoms. For example, in some embodiments, the α-olefin comonomer may have 3 to 20 carbon atoms, 3 to 10 carbon atoms, or 3 to 8 carbon atoms. Exemplary α-olefin comonomers may include, but are not limited to, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, and 4-methyl-1-pentene. In some embodiments, the ethylene-based polymer may include an α-olefin comonomer selected from the group consisting of 1-butene, 1-hexene, and 1-octene. In some embodiments, the ethylene-based polymers produced in the presence of the procatalysts and / or catalyst systems disclosed herein can be interpolymers of ethylene monomer units and comonomer units selected from 1-butene, 1-hexene, 1-octene, or combinations thereof.

[0041] In some embodiments, a solution polymerization / copolymerization process is used. Polymerization is carried out by adding a catalytic amount of the procatalyst and / or catalyst to a polymerization reactor containing the selected α-olefin monomer (e.g., ethylene and / or one or more α-olefin comonomers), or vice versa. The polymerization reactor may be maintained at a temperature of 60°C to 300°C. For example, in some embodiments, the polymerization reactor may be maintained at a temperature of 150°C to 230°C, such as 150°C to 200°C, 180°C to 300°C, 180°C to 230°C, 180°C to 200°C, etc. In some embodiments, the reactants, the catalyst system, or both, may have a residence time of 5 minutes to 20 minutes in the polymerization reactor. In some embodiments, the residence time may be 30 minutes to 4 hours. Alternatively, longer or shorter residence times may be used alternatively.

[0042] In some embodiments, the polymerization / copolymerization process may be carried out at relatively low pressures, such as pressures of 150 to 3,000 psig (1.0 to 20.7 MPa), e.g., 250 to 1,000 psig (1.7 to 6.9 MPa), or 450 to 800 psig (3.1 to 5.5 MPa). However, polymerization / copolymerization in the presence of the procatalysts and / or catalysts disclosed herein may be carried out at pressures from atmospheric pressure up to pressures determined by the capabilities (e.g., pressure rating) of the polymerization equipment.

[0043] In some embodiments, the polymerization / copolymerization process may include a support, which may be an inert organic diluent, excess monomer, or both. Oversaturation of the support with polymer may generally be avoided during the polymerization / copolymerization process. If such saturation of the support with polymer occurs before the catalyst system is exhausted, the full efficiency of the catalyst system may not be realized. In some embodiments, the polymerization / copolymerization process may be operated at conditions sufficient to maintain the amount of polymer in the support / diluent at a concentration lower than the supersaturated concentration of polymer. For example, in some embodiments, the polymerization / copolymerization process may be operated at conditions sufficient to maintain the amount of polymer in the support / diluent at less than 30 weight percent (wt%) based on the total weight of the reaction mixture. In some embodiments, the polymerization / copolymerization process may include mixing or stirring the reaction mixture to maintain temperature control and to enhance uniformity of the polymerization reaction throughout the polymerization zone. In some embodiments, such as for more rapid reaction with a relatively active catalyst, the polymerization / copolymerization process may include refluxing monomer and diluent, if a diluent is included, thereby removing at least a portion of the heat of reaction. In some embodiments, a heat transfer device (eg, a heat exchanger, cooling jacket, or other heat transfer means) may be provided to remove at least a portion of the exothermic heat of polymerization.

[0044] In some embodiments, the reaction mixture added to the polymerization / copolymerization process may include a sufficient amount of ethylene monomer to maintain reactor stability and enhance catalyst efficiency. In some embodiments, the reaction mixture may have a molar ratio of diluent to ethylene monomer of 1:2 to 1:8, such as 1:2 to 1:5, 1:3 to 1:8, or 1.3 to 1.5. In some embodiments, a portion of the excess ethylene monomer may be vented from the polymerization process to maintain the concentration of ethylene monomer in the reactor.

[0045] In some embodiments, the polymerization / copolymerization process may include contacting hydrogen gas with the reaction mixture during the reaction. The hydrogen gas may be operable to reduce the formation of ultra-high molecular weight molecules of the ethylene-based polymer. In some embodiments, the concentration of hydrogen gas in the reaction mixture may be maintained at 0.001 to 1.000 moles of hydrogen per mole of monomer, where the monomers include ethylene monomer and any optional α-olefin comonomer. Hydrogen may be added to the polymerization reactor along with the monomer stream, as a separate hydrogen feed stream, or both. Hydrogen may be added to the polymerization reactor before, during, and / or after the addition of the monomers to the polymerization reactor. In some embodiments, hydrogen may be added before or during the addition of the catalyst system.

[0046] The resulting ethylene-based polymer may be recovered from the polymerization mixture by stripping off unreacted monomer, comonomer, diluent, or combinations thereof. In some embodiments, further removal of impurities may not be required. The resulting ethylene-based polymer may contain small amounts of catalyst residues. The resulting ethylene-based polymer may be further melt screened. For example, the ethylene-based polymer may be melted in an extruder and then passed through one or more active screens arranged in series, each active screen having a micron retention size of 2 micrometers (μm) to about 400 μm, such as 2 μm to about 300 μm, or 2 μm to about 70 μm. During melt screening, the mass flow rate of the ethylene-based polymer may be from 5 to about 100 pounds per hour per square inch. 2(1.0~approx. 20.0kg / sec / m 2 ).

[0047] The resulting ethylene-based polymers produced with the procatalysts and / or catalysts disclosed herein may exhibit increased HDF compared to ethylene-based polymers not prepared in the presence of the procatalysts and / or catalysts disclosed herein. HDF content may be determined according to the test methods disclosed in this disclosure. As used herein, the term "comparative polymer" refers to a polymer prepared by a comparative polymerization process in which an ethylene-based polymer is polymerized in the presence of a comparative catalyst system. The comparative catalyst system includes a comparative procatalyst composition, except that it does not contain a hydrocarbon-soluble transition metal compound having an oxidation state of 5+ or higher in place of the procatalysts disclosed herein.

[0048] In some embodiments, ethylene-based polymers produced in the presence of the procatalysts and / or catalysts disclosed herein may have a HDF determined according to the test methods disclosed herein that is at least 25% greater than the HDF of the comparative polymer (HFD change). In some embodiments, ethylene-based polymers produced by processes including the catalyst systems disclosed herein may have a HDF at least 30% greater than the HDF of the comparative polymer (HFD change), such as at least 35% greater than the HDF of the comparative polymer.

[0049] The efficiency of the catalyst in producing ethylene-based polymers is, in embodiments, from 100 kg polymer / gTi to 1500 kg polymer / gTi, such as from 175 kg polymer / gTi to 425 kg polymer / gTi, from 200 kg polymer / gTi to 400 kg polymer / gTi, from 225 kg polymer / gTi to 375 kg polymer / gTi, or from 250 kg polymer / gTi to 350 kg polymer / gTi.

[0050] Molecular weights of ethylene-based polymers produced according to embodiments are measured by gel permeation chromatography (GPC). In some embodiments, ethylene-based polymers produced in the presence of the procatalysts and / or catalysts disclosed herein can have a Mw that is at least 2%, or at least 5%, or at least 7% greater than the Mw (Mw change) of a comparative polymer, determined according to the test methods disclosed herein.

[0051] The ethylene-based polymers produced in the presence of the procatalysts and / or catalysts disclosed herein may further comprise additional components such as other polymers and / or additives. Examples of additives may include, but are not limited to, antistatic agents, color enhancers, dyes, lubricants, fillers, pigments, primary antioxidants, secondary antioxidants, processing aids, UV stabilizers, and combinations thereof. In some embodiments, antioxidants such as IRGAFOS™ 168 and IRGANOX™ 1010 available from Ciba Geigy may be used to protect the ethylene-based polymer composition from thermal and / or oxidative degradation. The ethylene-based polymers may include any amount of additives. For example, in some embodiments, the ethylene-based polymer can include 0.0 wt.% to 10.0 wt.%, such as 0.0 wt.% to 7.0 wt.%, 0.0 wt.% to 5.0 wt.%, 0.0 wt.% to 3.0 wt.%, 0.0 wt.% to 2.0 wt.%, 0.0 wt.% to 1.0 wt.%, or 0.0 wt.% to 0.5 wt.%, based on the total weight of the ethylene-based polymer composition including such additives.

[0052] The ethylene-based polymers produced in the presence of the catalyst system disclosed herein may be included in a wide variety of products, including, in embodiments, LLDPE, as well as high density polyethylene (HDPE), plastomers, medium density polyethylene, and polypropylene copolymers. For these and other applications, articles may be prepared that exhibit improved overall quality due to the increase in average molecular weight and high density fraction of the ethylene-based polymer. Useful forming operations of the polymers may include, but are not limited to, extrusion and coextrusion of films, sheets, tubes, and fibers, as well as blow molding, injection molding, and rotational molding may be performed. Films may include blown or cast films formed by coextrusion or lamination, and may be useful as shrink films, cling films, stretch films, sealing films, oriented films, snack packaging, heavy duty bags, grocery bags, baked and frozen food packaging, medical packaging, industrial liners, agricultural film applications, and membranes in food contact and non-food contact applications, for example. Fibers may include melt-spun, solution-spun, and melt-blown fiber operations for use in woven and nonwoven fabric forms to make filters, diaper fabrics, medical garments, and geotextiles. Extruded articles may include medical tubing, wire and cable coatings, geomembranes, and pond liners. Molded articles may include single and multi-layer structures in the form of bottles, tanks, large hollow articles, rigid food containers, and toys.

[0053] Test Method density Density is measured according to ASTM D792 and is expressed in grams per cubic centimeter (g / cc or g / cm 3 ) will be reported.

[0054] Melt Index Melt index (I2) is measured according to ASTM D1238 under conditions of 190°C and 2.16 kg load. Melt flow index (I2) was obtained using a CEAST 7026 or Instron MF20 instrument. The instrument followed ASTM D1238, methods E and N. Melt index (I2) is reported in grams dissolved per 10 minutes (g / 10 min). Melt index I2 was used for polymer characterization. Higher I2 values ​​can generally be correlated with lower Mw.

[0055] Gel Permeation Chromatography (GPC) The weight average molecular weight (Mw) of ethylene-based polymers is measured by GPC. The polymer samples are dissolved by adding them to 1,2,4-trichlorobenzene (TCB) at a concentration of 10 mg / mL and heating the mixture at 160 °C for 120 min. The solution contains 300 parts per million by weight (ppmw) of butylated hydroxytoluene (BHT) to stabilize the solution. Each sample was then diluted to 1 milligram per milliliter (mg / mL) immediately before injecting a 250 microliter (μL) aliquot of the sample. The chromatograph is equipped with two Polymer Labs PLgel 10 μm MIXED-B columns (300 millimeters (mm) × 10 mm) and is operated at a flow rate of 2.0 mL / min and a temperature of 160 °C. Sample detection is performed using a PolymerChar IR4 detector in concentration mode. At this temperature, conventional calibration of polystyrene (PS) and homopolyethylene (PE) narrow standard reference materials was utilized, with apparent units adjusted to PE, using the known Mark-Houwink coefficients for PS and homopolyethylene (PE) in TCB.

[0056] High Density Fraction (HDF) Improved comonomer content distribution (iCCD) analysis was performed using a Crystallization Elution Fractionation (CEF) instrument (PolymerChar, Spain) equipped with an IR-5 detector (PolymerChar, Spain) and a two-angle light scattering detector (e.g., Precision Detectors, currently a Model 2040 detector from Agilent Technologies). Just before the IR-5 detector in the detector oven, a guard column is installed, containing 20-27 micron glass (MoSci Corporation, USA) packed in a 10 centimeter (cm) (length) × 1 / 4 inch (6.35 mm) inner diameter (ID) stainless steel column. Orthodichlorobenzene (oDCB, 99% anhydrous grade or technical grade) is distilled before use. Silica gel 40 (Aldrich, high purity grade, 35-70 mesh) is used for further drying of the oDCB. The silica gel is dried in a vacuum oven at 160 °C for approximately 2 h before use. Silica gel 40 is packed into three 300 mm x 7.5 mm GPC sized stainless steel columns. The silica gel 40 columns are attached to the pump inlet of the CEF instrument. The CEF instrument is equipped with an autosampler with N2 purging capability. The oDBC is continuously sparged with dry nitrogen (N2) for at least 1 hour prior to use.

[0057] Sample preparation is performed using an autosampler at 3.6 mg / ml (unless otherwise specified) with shaking at 160 °C for 2 h. Injection volume is 300 μL. The temperature profile of the iCCD is: stabilization at 105 °C, crystallization from 105 °C to 30 °C with a cooling rate of 3 °C / min, thermal equilibration at 30 °C for 3 min (with the soluble fraction elution time set at 2 min), elution from 30 °C to 140 °C with a heating rate of 3 °C / min. The flow rate during crystallization is 0.0 mL / min. The flow rate during elution is 0.50 mL / min. Data is collected at one data point / sec. The iCCD column is packed with Bright 7GNM8-NiS (Bright 7GNM8-NiS) in a 15 cm (length) x 1 / 4 inch (6.35 mm) ID stainless steel tube according to reference (Cong et al., US78203, 2015). Calibration of the column temperature is performed by a mixture of standards linear homopolymer polyethylene 38-4 (1.0 mg / ml) and eicosane (2 mg / ml) in oDCB. The molecular weight of the polymer and the molecular weight of the polymer fraction were determined directly from the LS detector (90 degree angle) and the concentration detector (IR-5) assuming a form factor of 1 and all virial coefficients equal to zero according to the Rayleigh-Gans-Debye approximation (Striegel and Yau, Modern Size Exclusion Liquid Chromatogram, Page 242 and Page 263). The baseline is subtracted from the LS and concentration detector chromatograms. For the whole resin, the integration window is set to integrate all chromatograms with elution temperatures ranging from 23.0 °C to 120 °C (temperature calibration specified above). The weight percent of the high density fraction (HDF) of the resin is defined by the following Equation 1 (EQU.1):

number

[0058] Catalyst efficiency is calculated based on the amount of ethylene consumed during polymerization per gram of Ti used in the procatalyst composition (g / gTi). EXAMPLES

[0059] The embodiments of the present disclosure are further clarified by the following examples.

[0060] Preparation of procatalyst The MgCl2 slurry is prepared as described in the "Magnesium Halide Support" section of WO2018 / 005821A1.

[0061] All procatalyst preparations were carried out in a nitrogen-purged glove box. The preparations involved the sequential room temperature addition (with stirring) of stock solutions of the procatalyst components in hexane (0.25 M) to a MgCl2 slurry (0.2 M in Isopar-E). The procatalyst components were added to the MgCl2 in the following order: Et2AlCl, transition metal component reagent X (if present), and Ti compound (TiCl4 or TiPt). The reaction time for each reaction step is about 12 hours. For example, the procatalyst (12Al; 1Ti; 2Zn) of Example 2 was prepared by adding EtAlCl2 to the MgCl2 slurry. After stirring at room temperature for 12 hours, a hexane solution of zinc 2-ethylhexanoate (Zn(EHA)2; about 80% in mineral spirits) obtained from STREM Chemical, Inc. was added. The reaction was allowed to proceed with stirring for an additional 12 hours at room temperature, after which a TiCl4 solution was introduced to the mixture and the contents were stirred at room temperature overnight to obtain the procatalyst. The molar ratios of the individual reagents (relative to 40 equivalents of Mg) are given in the following table:

[0062] Batch polymerization of ethylene / octene. Solution batch ethylene / 1-octene polymerizations were carried out in a stirred 1-gallon reactor charged with 250 g 1-octene (C8) and 1330 g Isopar-E. The reactor was heated to 190 °C and then saturated with ethylene (450 psig) in the presence of hydrogen (40 mmol). The catalyst premix and cocatalyst (triethylaluminum, TEA, TEA / Ti=15 in Table 1 and TEA / Ti=10 in Table 2) were mixed briefly (1–5 min) in an overhead shot tank before being injected into the reactor. The polymerization was allowed to proceed for 10 min during which ethylene pressure was maintained via an on-demand ethylene supply. The bottom valve was then opened and the contents transferred to a glass kettle and mixed with antioxidant solution (1 mL containing 0.1 g IRGAFOS 168 (BASF Corporation) and 0.05 g IRGANOX 1010 (BASF Corporation)). The contents were poured into a Mylar-lined pan, cooled, and left in a hood overnight. The resin was then dried in a vacuum oven at 60 °C for 48 h. Catalyst loadings typically ranged from 1 to 3 micromoles of Ti. [Table 1]

[0063] As shown in Table 1 above, many transition metal compounds with oxidation states of 4+ or lower reduced the molecular weight and HDF content of the polymer (see Comparative Example 1 vs. Comparative Examples 2-7). In contrast, compounds with oxidation states of 5 or higher, i.e., Mo(OEt)5, Nb(O n Bu)5 and Ta(O n Bu)5 increased the molecular weight and HDF content of the polymer (see Examples 1 to 3 and Comparative Example 1). [Table 2]

[0064] As shown in Table 2, WCl6 increased the molecular weight and HDF of the polymer, and the effect of high oxidation state transition metal compounds was also demonstrated in procatalyst formulations using Ti(OiPr)4 as the Ti source instead of TiCl4 as shown in Examples 1-3.

[0065] It will be apparent to those skilled in the art that various modifications and variations can be made to the embodiments described herein without departing from the spirit and scope of the subject matter described in the claims. Accordingly, it is intended that the present specification cover modifications and variations of the various embodiments described herein, provided that such modifications and variations come within the scope of the appended claims and their equivalents. The present invention includes the following aspects. Section 1. A procatalyst comprising: 100m 2 a preformed magnesium chloride catalyst support having a surface area of ​​at least 1 / g; A titanium-containing component; A chlorinating agent; a hydrocarbon soluble transition metal compound having an oxidation state of 5+ or greater, wherein the hydrocarbon soluble transition metal compound having an oxidation state of 5+ or greater does not contain vanadium. Section 2. 2. The procatalyst of claim 1, wherein the hydrocarbon soluble transition metal compound having an oxidation state of 5+ or greater is an aliphatic hydrocarbon soluble transition metal compound having an oxidation state of 5+ or greater. Section 3. The preformed magnesium chloride catalyst support is 150 m 2 3. The procatalyst of any one of claims 1 and 2, having a surface area of ​​1.0 nm to 1.0 nm / g or more. Section 4. 4. The procatalyst of any one of items 1 to 3, wherein the preformed magnesium chloride catalyst support is a MgCl2 slurry in a hydrocarbon solvent. Section 5. 5. The procatalyst of claim 4, wherein the MgCl slurry is the reaction product of a solution of an alkyl magnesium compound in a hydrocarbon solvent and a chloride source without separating the hydrocarbon solvent. Section 6. 6. The procatalyst according to any one of items 1 to 5, wherein the titanium-containing component is titanium chloride. Section 7. The titanium-containing component is TiCl4(OR) x-4 In the formula, R is C1 to C 21 7. The procatalyst of any one of paragraphs 1 to 6, wherein x=0, 1, 2, 3, or 4. Section 8. 8. The procatalyst according to any one of items 1 to 7, wherein the chlorinating agent is an alkylaluminum chloride. Section 9. 9. The procatalyst of any one of paragraphs 1 to 8, wherein the hydrocarbon soluble transition metal compound having an oxidation state of 5+ or higher comprises a member selected from the group consisting of molybdenum, niobium, tantalum, tungsten, and combinations thereof. Section 10. 10. The procatalyst according to any one of items 1 to 9, wherein the molar ratio of the transition metal present in the hydrocarbon soluble transition metal compound having an oxidation state of 5+ or higher to the titanium present in the titanium-containing compound is from 0.1 to 10.0. Section 11. 11. The procatalyst according to any one of items 1 to 10, wherein the molar ratio of the chlorinating agent to the titanium present in the titanium-containing component is from 0.5 to 100.0. Section 12. 100m 2 12. The procatalyst of any one of claims 1 to 11, wherein the molar ratio of the preformed magnesium chloride catalyst support having a surface area of ​​1.0 to 100.0 Mg / g or more to the titanium present in the titanium-containing component is 1.0 to 100.0. Section 13. A catalyst comprising: A procatalyst according to any one of items 1 to 12, and an alkylaluminum cocatalyst. Section 14. Item 14. A process for polymerizing an ethylene-based polymer, comprising contacting ethylene, and optionally one or more α-olefins, in the presence of the catalyst of item 13. Section 15. Item 15. The process for polymerizing an ethylene-based polymer according to item 14, wherein the polymerization process is a solution polymerization process. Section 16. Item 1. A method for preparing the procatalyst according to item 1, comprising: 2 (A) said titanium-containing component; (B) said chlorinating agent; and (C) said hydrocarbon soluble transition metal compound having an oxidation state of 5+ or greater, The method, wherein said hydrocarbon soluble transition metal compound having an oxidation state of 5+ or higher does not contain vanadium. Section 17. 17. The method of claim 16, wherein at least one of (A), (B), or (C) is added to the preformed magnesium chloride catalyst support temporally separated from at least one other of (A), (B), or (C). Section 18. Item 13. An ethylene-based polymer prepared in the presence of the procatalyst of any one of items 1 to 12, wherein the ethylene-based polymer has a high density fraction that is at least 5% greater than the high density fraction of a comparison polymer. Section 19. 20. The ethylene-based polymer of claim 18, wherein the ethylene-based polymer has a high density fraction that is at least 10% greater than the high density fraction of a comparison polymer. Section 20. 20. The ethylene-based polymer of claim 18 or 19, wherein the ethylene-based polymer has a Mw at least 5% greater than the Mw of a comparison polymer.

Claims

1. A procatalyst comprising: a preformed magnesium chloride catalyst support having a surface area of ​​100 m 2 / g to 800 m 2 / g; A titanium-containing component; A chlorinating agent; a hydrocarbon soluble transition metal compound having an oxidation state of 5+ or greater, said hydrocarbon soluble transition metal compound having an oxidation state of 5+ or greater being free of vanadium; A procatalyst wherein said hydrocarbon soluble transition metal compound having an oxidation state of 5+ or greater comprises a member selected from the group consisting of molybdenum, niobium, tantalum, tungsten, and combinations thereof.

2. 2. The procatalyst of claim 1, wherein said hydrocarbon soluble transition metal compound having an oxidation state of 5+ or higher is an aliphatic hydrocarbon soluble transition metal compound having an oxidation state of 5+ or higher.

3. 3. The procatalyst of any one of claims 1 and 2, wherein the preformed magnesium chloride catalyst support has a surface area of ​​from 150 m 2 / g to 800 m 2 / g.

4. The preformed magnesium chloride catalyst support is prepared by mixing MgCl in a hydrocarbon solvent. 2 The procatalyst of any one of claims 1 to 3, which is a slurry.

5. The MgCl 2 5. The procatalyst of claim 4, wherein the slurry is the reaction product of a solution of an alkylmagnesium compound in a hydrocarbon solvent and a chloride source without separating said hydrocarbon solvent.

6. The procatalyst of any one of claims 1 to 5, wherein the titanium-containing component is titanium chloride.

7. The titanium-containing component is TiCl 4 (OR) 4-x where R is C 1 ~C 21 7. The procatalyst of any one of claims 1 to 6, wherein x=0, 1, 2, 3, or 4, and x is a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl ...

8. The procatalyst of any one of claims 1 to 7, wherein the chlorinating agent is an alkylaluminum chloride.

9. 9. The procatalyst of any one of claims 1 to 8, wherein the molar ratio of transition metal present in the hydrocarbon soluble transition metal compound having an oxidation state of 5+ or greater to titanium present in the titanium-containing component is from 0.1 to 10.

0.

10. The procatalyst of any one of claims 1 to 9, wherein the molar ratio of the chlorinating agent to the titanium present in the titanium-containing component is from 0.5 to 100.

0.

11. The procatalyst of any one of claims 1 to 10, wherein the molar ratio of the preformed magnesium chloride catalyst support to the titanium present in the titanium-containing component is from 1.0 to 100.

0.

12. A catalyst comprising: A procatalyst according to any one of claims 1 to 11; and an alkylaluminum cocatalyst.

13. 13. A process for polymerizing an ethylene-based polymer comprising contacting ethylene, and optionally one or more α-olefins, in the presence of the catalyst of claim 12.

14. 14. The process for polymerizing an ethylene-based polymer according to claim 13, wherein the polymerization process is a solution polymerization process.

15. 2. A method for preparing the procatalyst of claim 1, comprising mixing with said preformed magnesium chloride catalyst support having a surface area of ​​100 m 2 / g to 800 m 2 / g (A) said titanium-containing component, (B) said chlorinating agent, and (C) said hydrocarbon-soluble transition metal compound having an oxidation state of 5+ or higher; The method, wherein said hydrocarbon soluble transition metal compound having an oxidation state of 5+ or higher is free of vanadium.

16. 16. The method of claim 15, wherein at least one of (A), (B), or (C) is added to the preformed magnesium chloride catalyst support separated in time from at least one other of (A), (B), or (C).

17. 12. An ethylene-based polymer prepared in the presence of the procatalyst of any one of claims 1-11, wherein the ethylene-based polymer has a high density fraction that is at least 5% greater than the high density fraction of a comparison polymer.

18. 20. The ethylene-based polymer of claim 17, wherein the ethylene-based polymer has a high density fraction that is at least 10% greater than the high density fraction of a comparative polymer.

19. 19. The ethylene-based polymer of claims 17 or 18, wherein the ethylene-based polymer has a Mw at least 5% greater than the Mw of the comparative polymer.

Citation Information

Patent Citations

  • Synthesis of spherical magnesium alcoholate having narrow particle size distribution

    JP1991074341A

  • Catalyst for polymerization of alpha-olefin

    JP1992020510A

  • Olefin polymerization catalyst

    JP1992234408A