Ultra-long nano silver wire material and its manufacturing method
An aqueous-based method for producing ultralong nanosilver wires addresses the limitations of existing technologies by ensuring easy cleaning and scalability, facilitating their industrial application in flexible electronics.
Patent Information
- Application Number
- JP2023544218
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-11-08
- Filing Date
- 2022-11-03
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-11-03
AI Technical Summary
Current methods for producing ultralong nanosilver wire materials face challenges such as high viscosity of reaction solutions, difficulty in cleaning, environmental pollution, and limitations in scalability, which hinder their industrial application in flexible electronic devices.
A manufacturing method using an aqueous solution system with reducing sugar and polyvinylpyrrolidone, avoiding organic solvents, and employing controlled hydrothermal conditions to produce ultralong nanosilver wires with a high aspect ratio, utilizing a sedimentation washing process to ensure purity and ease of cleaning.
The method enables the production of ultralong nanosilver wires that are easy to clean, environmentally friendly, and suitable for large-scale industrial production, with improved reproducibility and reduced energy consumption, enhancing their performance in flexible electronic applications.
Smart Images

Figure 0007576709000001 
Figure 0007576709000002 
Figure 0007576709000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of noble metal nano-materials, and in particular to ultra-long nano silver wire materials and methods for producing the same.
[0002] This application claims priority from Chinese patent application No. 202111311087.3, filed on November 8, 2021. This application incorporates the entire text of the above Chinese patent application by reference. [Background technology]
[0003] As nanomaterial manufacturing technology develops and the demand for flexible electronic products increases, research at home and abroad is turning to new nanomaterials to replace metal oxide thin films, such as graphene, carbon nanotubes, composite nanomaterials, metal meshes and metal nanowires. Due to the high DC conductivity of these materials, the ultra-thin films produced have good electrical conductivity, which overcomes the mechanical brittleness and poor flexibility of traditional electrodes and enables the production of transparent electrodes with excellent performance. Among them, nano silver wires, as one-dimensional metal nanomaterials, have a high aspect ratio and can form an irregular mesh structure on the substrate, which can reduce the bending radius of the electrode and reduce the resistance change rate when bending. In addition, transparent electrodes made of ultra-long nano silver wire materials have lower haze and better light transmittance compared to some other new materials.
[0004] At present, the manufacturing methods of nano silver wires can be divided into two types: physical and chemical. Physical methods include magnetron sputtering, ultrasonic grinding, mechanical grinding, etc. Chemical methods include hydrothermal synthesis, photochemical reduction, electrochemical, template, ultrasonic reduction, polyhydric alcohol, etc. Physical methods have complex processes, high energy consumption, high technical requirements, and the morphology of the obtained products is poor, which severely limits the specifications of nano silver wires manufactured by physical methods. Compared with physical methods, the chemical liquid phase method is the most commonly used method for controllably synthesizing nano materials, which has a simple process, low cost, and can control the morphology and dimensions of nano materials in a simple liquid phase reaction process, and is the most promising method for industrialized production of ultra-long nano silver wire materials. Among them, the manufacturing method of ultra-long nano silver wire materials by polyhydric alcohol proposed by Xia Younan is a widely accepted and universally applied technical method. The most commonly used method is to use ethylene glycol as a solvent and PVP as a surfactant to suppress adhesion between nano silver wires, and add a control agent to prevent adhesion between Ag + and form a colloid, Ag +The aim is to control the reduction rate and the growth rate of the nano silver wires, and finally obtain ultra-long nano silver wire materials. Based on this, many explorations have been made. By examining the mechanism and various influencing parameters, nano silver wires of various specifications have been produced. However, this method still requires a complicated manufacturing process, the material input process needs to be precisely controlled, and there are many influencing factors, and the currently reported manufacturing scale is mostly at the milligram and gram level, which is very disadvantageous for mass production of nano silver wires. In addition, all polyhydric alcohol methods require the use of organic reagents (ethylene glycol, propylene triol, etc.) as solvents and reducing agents, and the viscosity of the reaction solution is high, making the subsequent cleaning process of the product difficult and causing environmental pollution. In addition, the aspect ratio of the ultra-long nano silver wire material has a great influence on the performance of flexible transparent electrodes. With the same sheet resistance and diameter, the transmittance of nano wires is inversely proportional to the number of nano wires, the transmittance of transparent electrodes made of long nano silver wires is higher than that of short nano silver wires, and the photoelectric performance of transparent electrodes made of long nano silver wires is better than that of short nano wires. However, the nanosilver wire materials produced by the polyhydric alcohol method are generally short, and there have been few reports on ultra-long nanosilver wire materials with lengths of 70 μm or more. Moreover, the scale is extremely small and the reproducibility is poor, which severely limits the industrial application of ultra-long nanosilver wire materials in the field of flexible electrodes.
[0005] As the application fields of ultra-long nano silver wire materials expand, their manufacturing methods are also developing further. The trend of development is to develop environmentally friendly technologies and processes around the chemical liquid phase method, and to reduce the factors that affect the environment in the crystal growth process, and the manufacturing technology is developing toward lower cost, lower consumption, and lower pollution. The manufactured ultra-long nano silver wire materials should be easy to clean, meet the demands of industrial production, and make it possible to realize industrial production. In addition, in response to the demands of the development of the flexible electronics field, in order to meet the application requirements of the conductivity, transparency, and flexibility of flexible electronic devices, attention will be paid in particular to the manufacturing process technology of ultra-long nano silver wire materials in the future. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to provide an ultra-long nano silver wire material and a manufacturing method thereof in response to the above-mentioned shortcomings of the prior art. This manufacturing method focuses on the fact that most of the currently available manufacturing processes for ultra-long nano silver wire materials use polyhydric alcohol organic systems, which have problems such as high viscosity of the product solution, difficult cleaning, serious pollution, and strict reaction conditions, and develops a manufacturing method for ultra-long nano silver wire material that uses an aqueous solution system, does not require the use of organic solvents, does not require protection by an inert atmosphere, is low-cost, environmentally friendly, and easy to industrialize.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions: Step 1: adding reducing sugar and polyvinylpyrrolidone to deionized water and stirring uniformly to obtain a clear solution; Step 2: mixing the clear solution with a metal ion solution to obtain a mixed solution A; Step 3: mixing the mixed solution A with a halide solution to obtain a mixed solution B; Step 4: adding a solution containing silver ions dropwise to the mixed solution B and stirring to obtain a reaction solution, and then transferring the reaction solution to a hydrothermal reactor and reacting at 110°C to 130°C for 14 hours to 20 hours to obtain a flocculated product; and step 5, sequentially precipitating and washing the flocculated product with deionized water and absolute ethanol to obtain an ultralong nanosilver wire material having an aspect ratio of more than 3000.
[0008] In some preferred embodiments, the following manufacturing method is used: In step 1, glucose and polyvinylpyrrolidone are added to deionized water and stirred uniformly to obtain a clear solution; In step 2, the copper sulfate solution is added to the clear solution obtained in step 1 and stirred uniformly to obtain a mixed solution A; In step 3, the sodium chloride solution is added to the mixed solution A obtained in step 2 and stirred uniformly to obtain a mixed solution B; In step 4, the silver nitrate solution is dropped into the mixed solution B obtained in step 3 and stirred to obtain a reaction solution, which is then transferred to a hydrothermal reaction vessel and reacted at 110°C to 130°C for 14 to 20 hours to obtain a flocculated product; In step 5, the flocculated product obtained in step 4 is successively precipitated and washed with deionized water and absolute ethanol to obtain ultra-long nano silver wire material with an aspect ratio of more than 3000.
[0009] In the present invention, first, reducing sugar (e.g., glucose), polyvinylpyrrolidone and deionized water are mixed, and then a metal ion solution (e.g., copper sulfate solution), a halide solution (e.g., sodium chloride solution) are added in sequence, and a silver ion-containing solution (e.g., silver nitrate solution) is further added, and the reaction is carried out under hydrothermal conditions to obtain an ultra-long nano silver wire material. In the present invention, instead of using polyhydric alcohol as a solvent, a mild and environmentally friendly reducing sugar (e.g., glucose) is used as a reducing agent, which effectively reduces the viscosity of the reaction solution, makes it easy to wash the product, and effectively reduces the cost of the reactants. In the present invention, a very small amount of polyvinylpyrrolidone is used as a surfactant, which prevents the product from being affected by the coating of the activator, and improves the stability of use. In the present invention, water is used as a solvent, which effectively reduces environmental pollution. The reason why an aqueous solution system is used instead of an organic solution system in the present invention is that the organic solution system When using an aqueous solution of silver, it is common to introduce an inert gas into the organic solution to remove the dissolved oxygen in the organic solution. However, the presence of oxygen will consume a large amount of the five-sided twin structure obtained in the first stage of silver precipitation. The five-sided twin structure is a necessary prerequisite for nano silver crystals to grow into nanowires. The five-sided twin will grow into particles in the presence of oxygen, and even if the reaction time is increased, the obtained product will remain as particles. Thus, a large amount of nano silver particles will appear in the reaction system, which will cause great difficulties in subsequent sample processing. In contrast, the twin structure obtained in the aqueous solution system used in the present invention is not sensitive to oxygen in the solution, and can maintain the five-sided twin structure without the introduction of an inert gas. The final product is basically a nanowire structure. The present invention does not require any additional operations, only requires reaction at room temperature throughout the entire process, and does not require the introduction of an inert atmosphere for protection, which is advantageous for industrial production, has a simple process, and low energy consumption.
[0010] In the present invention, the solvent of the solution is entirely water.
[0011] In the present invention, the reducing sugar may be one or more of glucose, maltose, fructose, sucrose, and galactose, but is preferably glucose.
[0012] In the present invention, the metal ion solution may be one or more of a nickel nitrate solution, a nickel sulfate solution, a ferrous nitrate solution, a ferrous sulfate solution, a copper sulfate solution, a copper nitrate solution, and a manganese sulfate solution, but is preferably a copper sulfate solution.
[0013] In the present invention, the halide solution may be a potassium chloride solution and / or a sodium chloride solution.
[0014] In the present invention, the silver ion-containing solution may be a silver nitrate solution.
[0015] In the present invention, the molecular weight Mw of the polyvinylpyrrolidone may be 4,000 to 1,300,000 daltons, but preferably 8,000 to 100,000 daltons, for example, 24,000 or 58,000 daltons.
[0016] In step 1 of the present invention, the molar ratio of the reducing sugar, the polyvinylpyrrolidone, and the deionized water may be 1:(0.05-0.1):(280-560), preferably 1:(0.05-0.1):(350-550), for example, 1:0.05:400, 1:0.06:430, 1:0.08:350, 1:0.07:550, 1:0.06:450, or 1:0.1:500. In some specific embodiments, in step 1, the molar ratio of the glucose, the polyvinylpyrrolidone, and the deionized water is 1:(0.05-0.1):(280-560).
[0017] In the present invention, reducing sugar (e.g., glucose) is a reducing agent, and polyvinylpyrrolidone is a structure-directing agent. By controlling the molar ratio of reducing sugar (e.g., glucose), polyvinylpyrrolidone, and deionized water, the final product is ensured to have an ultra-long nanowire structure and the production of nanoparticles is avoided. Also, in the present invention, the amount of surfactant used is extremely small, and the use of a small amount of surfactant makes processes such as washing the product easier.
[0018] In step 2 of the present invention, the molar ratio of the reducing sugar to the metal ion in the mixed solution A may be 1:(480 to 600), but is preferably 1:(500 to 580), for example, 1:550, 1:560, or 1:567.
[0019] In some specific embodiments, in step 2, the molar ratio of glucose to copper sulfate in the mixed solution A is 1:(480 to 600).
[0020] In the present invention, the molar ratio of reducing sugar (eg, glucose) to metal ion (eg, copper sulfate) is controlled to ensure that the final product has a nanowire structure and prevents the formation of nanoparticles.
[0021] In the present invention, in step 3, the molar ratio of the halide to the metal ion in the mixed solution B may be 1:(2.5 to 4.8), but is preferably 1:(3 to 4.5), for example, 1:3.67, 1:4, or 1:4.17.
[0022] In some specific embodiments, in step 3, the molar ratio of sodium chloride to copper sulfate in the mixed solution B is 1:(3 to 4.8).
[0023] In the present invention, the molar ratio of halide (e.g., sodium chloride solution) to metal ion (e.g., copper sulfate) is controlled to ensure that the final product has a nanowire structure and prevents the formation of nanoparticles.
[0024] In step 4 of the present invention, the molar ratio of the reducing sugar to the silver ions in the reaction solution may be 1:(300 to 500), but is preferably 1:(350 to 480), for example, 1:400, 1:440, or 1:450.
[0025] In some specific embodiments, in step 4, the molar ratio of glucose to silver nitrate in the reaction solution is 1:(300 to 500).
[0026] In the present invention, reducing sugar (e.g., glucose) is used as a reducing agent to reduce silver ions (e.g., silver nitrate) to nanosilver, so the ratio must be controlled; otherwise, if the amount of reducing agent is insufficient, silver nitrate cannot be reduced to silver, and if the amount of reducing agent is too much, the reaction will be too fast, which is detrimental to the growth of nanowire structures.
[0027] In step 5 of the present invention, the sedimentation washing process is as follows: the flocculated product is added to deionized water, shaken and left to stand; when the flocculated product and deionized water are separated, the supernatant is discarded, and deionized water is further added; this process is repeated 3-5 times; the flocculated product is added to absolute ethanol, shaken and left to stand; when the flocculated product and absolute ethanol are separated, the supernatant is discarded, and absolute ethanol is further added; this process is repeated 3-5 times. Normally, all nano materials require centrifugal washing, but the product obtained in the present invention is ultra-long nano silver wires. When centrifugal washing is performed, if the rotation speed is not properly controlled, irreversible aggregation phenomenon occurs in the ultra-long nano silver wires, which affects the subsequent use of the nano wires. Therefore, a sedimentation washing method that does not cause aggregation of nano wires is used, and by washing with deionized water and absolute ethanol, respectively, both inorganic and organic impurities can be effectively washed, and the washing effect is good.
[0028] In the present invention, in any of steps 1, 2, and 3, the mixed solution is stirred at room temperature.
[0029] In the present invention, the stirring times in steps 2 and 3 are each 0.5 to 2 hours.
[0030] The present invention further provides an ultra-long nanosilver wire material produced by the method as described above.
[0031] Compared with the prior art, the present invention has the following advantages:
[0032] 1. In the present invention, the reaction is carried out in an aqueous solution system, which differs from the conventional manufacturing process of ultra-long nanosilver wire materials using polyhydric alcohol organic systems, and does not require the use of any organic solvent. This eliminates the technical limitations of the difficulty of cleaning the ultra-long nanosilver wire materials, the strict reaction conditions, and the serious pollution, and develops a new manufacturing method for ultra-long nanosilver wire materials in an aqueous solution system, does not require protection by an inert atmosphere, is low-cost, environmentally friendly, and easy to industrialize.
[0033] 2. In addition, the present invention adopts reducing sugar (such as glucose) instead of polyhydric alcohol as a reducing agent, which eliminates environmental pollution caused by polyhydric alcohol, and reducing sugar (such as glucose) is easy to obtain and inexpensive, which can meet the requirements of low-carbon production currently advocated. The obtained product is easy to wash, and can meet the needs of use by only settling and washing, and reduces the irreversible aggregation of the product caused by centrifugation.
[0034] 3. In the present invention, the amount of the surfactant polyvinylpyrrolidone used is small. Under the condition of small usage amount, the dispersibility of the ultralong nano silver wire material is well maintained and no obvious aggregation phenomenon is observed.
[0035] 4. The present invention has the advantages of simple equipment, low cost, controllable process parameters, high reproducibility and easy large-scale production. The ultra-long nano silver wire material produced by the present invention is expected to be useful in antibacterial, printed circuit boards, transparent conductive films, wireless RF electronic tags, catalysts, electrochemical sensing, radio wave absorption, electromagnetic shielding and other fields. [Brief description of the drawings]
[0036] [Figure 1] 1 is a SEM image of the ultra-long nano silver wire material produced in Example 1 of the present invention. [Diagram 2] 1 shows SEM images (a is low magnification, b is high magnification) of the ultra-long nano silver wire material produced in Example 1 of the present invention. [Diagram 3]1 shows SEM images (a is low magnification, b is high magnification) of the ultra-long nanosilver wire material produced in Example 2 of the present invention. [Figure 4] 1 is a SEM image of the ultra-long nano silver wire material produced in Example 3 of the present invention. [Diagram 5] 1 is a SEM image of the ultra-long nano silver wire material produced in Example 4 of the present invention. [Figure 6] 1 is a SEM image of the ultra-long nano silver wire material produced in Example 5 of the present invention. [Figure 7] 1 is a SEM image of the ultra-long nano silver wire material produced in Example 6 of the present invention. [Figure 8] 1 is a SEM image of the ultra-long nano silver wire material produced in Example 8 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS EXAMPLES
[0037] This embodiment includes the following steps: Step 1: Glucose and polyvinylpyrrolidone with a molecular weight Mw of 58000 Daltons are added to deionized water and stirred uniformly to obtain a clear solution, the molar ratio of glucose, polyvinylpyrrolidone and water is 1:0.1:280, and the molar mass of glucose is 0.01 mmol; Step 2: Add copper sulfate solution to the clear solution obtained in step 1 and stir evenly for 0.5 h to obtain mixed solution A, in which the molar mass of copper sulfate is 4.8 mmol; Step 3: Add sodium chloride solution to the mixed solution A obtained in step 2 and stir uniformly for 2 hours to obtain mixed solution B, in which the molar mass of sodium chloride is 1 mmol; Step 4: Drop the silver nitrate solution into the mixed solution B of step 3 and stir to obtain a reaction solution. Then, transfer the reaction solution to a hydrothermal reactor and react at 110°C for 16 hours to obtain a flocculated product. In the silver nitrate solution, the molar mass of silver nitrate is 3 mmol; Step 5: The flocculated product obtained in step 4 is successively precipitated and washed using deionized water and absolute ethanol to obtain an ultralong nano silver wire material. In the precipitation washing process, the flocculated product is added to deionized water, shaken and allowed to stand. When the flocculated product and deionized water are separated, the supernatant is discarded and more deionized water is added. This process is repeated three times, and then the flocculated product is added to absolute ethanol, shaken and allowed to stand. When the flocculated product and absolute ethanol are separated, the supernatant is discarded and more absolute ethanol is added. This process is repeated five times.
[0038] Figure 1 is an SEM image of the ultralong nanosilver wire material produced in this embodiment, and in Figure 2, a and b are low-magnification SEM images and high-magnification SEM images of the ultralong nanosilver wire material produced in this embodiment. As can be seen from Figure 1, the obtained product has a nanowire structure with a diameter of about 130 nm, and no other forms or impurity products other than the one-dimensional nanowire structure were observed in the product, which indicates that the purity of the obtained product is high, and it was found that at this magnification, the length of all single nanowires exceeded 100 μm. As can be seen from Figure 2, in order to further understand the length of the obtained nanowires, this embodiment also conducted tests at low magnification. However, since the nanowires produced are indeed long, due to the influence of the magnification of the instrument, it is difficult to capture the entire nanowire from beginning to end in the field of view, and in most cases only one end is within the field of view, while the other end is beyond the visible range of the field of view. In this embodiment, a single ultra-long nanosilver wire material that is shorter and measurable within the field of view is found, and this nanowire is bow-shaped, with a straight length between both ends of 318 μm, and the actual length is greater than 318 μm. Therefore, the aspect ratio of the ultra-long nanosilver wire material produced in this embodiment is much greater than 3000. EXAMPLES
[0039] This embodiment includes the following steps: Step 1: Glucose and polyvinylpyrrolidone with a molecular weight Mw of 24000 Daltons are added to deionized water and stirred uniformly to obtain a clear solution, the molar ratio of glucose, polyvinylpyrrolidone and water is 1:0.05:400, and the molar mass of glucose is 0.01 mmol; Step 2: Add copper sulfate solution to the clear solution obtained in step 1 and stir evenly for 1 h to obtain mixed solution A, in which the molar mass of copper sulfate is 6 mmol; Step 3: Add sodium chloride solution to the mixed solution A obtained in step 2 and stir uniformly for 0.5 h to obtain mixed solution B, in which the molar mass of sodium chloride is 2 mmol; Step 4: Drop the silver nitrate solution into the mixed solution B of step 3 and stir to obtain a reaction solution. Then, transfer the reaction solution to a hydrothermal reactor and react at 130°C for 20 hours to obtain a flocculated product. In the silver nitrate solution, the molar mass of silver nitrate is 4.8 mmol; Step 5: The flocculated product obtained in step 4 is successively precipitated and washed using deionized water and absolute ethanol to obtain an ultralong nano silver wire material. In the precipitation washing process, the flocculated product is added to deionized water, shaken and allowed to stand. When the flocculated product and deionized water are separated, the supernatant is discarded and more deionized water is added. This process is repeated three times, and then the flocculated product is added to absolute ethanol, shaken and allowed to stand. When the flocculated product and absolute ethanol are separated, the supernatant is discarded and more absolute ethanol is added. This process is repeated three times.
[0040] Figures 3a and 3b are SEM images of the ultra-long nanosilver wire material produced in this embodiment. As can be seen from Figure 3, the obtained product has a nanowire structure, and no other forms or impurity products other than the one-dimensional nanowire structure are found in the product, which indicates that the purity of the obtained product is high, the diameter distribution of the obtained nanowires is uniform, and the aspect ratio of the ultra-long nanosilver wire material is much greater than 3000. EXAMPLES
[0041] This embodiment includes the following steps: Step 1: Glucose and polyvinylpyrrolidone with a molecular weight of 1,300,000 Daltons are added to deionized water and stirred uniformly to obtain a clear solution, the molar ratio of glucose, polyvinylpyrrolidone and water is 1:0.06:430, and the molar mass of glucose is 0.05 mmol; Step 2: Add the iron nitrate solution to the clear solution obtained in step 1 and stir evenly for 2 hours to obtain mixed solution A, in which the molar mass of iron nitrate is 28 mmol; Step 3: Add sodium chloride solution to the mixed solution A obtained in step 2 and stir uniformly for 0.5 h to obtain mixed solution B, in which the molar mass of sodium chloride is 7 mmol; Step 4: Drop the silver nitrate solution into the mixed solution B of step 3 and stir to obtain a reaction solution. Then, transfer the reaction solution to a hydrothermal reactor and react at 115°C for 15 hours to obtain a flocculated product. In the silver nitrate solution, the molar mass of silver nitrate is 22 mmol; Step 5: The flocculated product obtained in step 4 is successively precipitated and washed using deionized water and absolute ethanol to obtain an ultralong nano silver wire material. In the precipitation washing process, the flocculated product is added to deionized water, shaken and allowed to stand. When the flocculated product and deionized water are separated, the supernatant is discarded and more deionized water is added. This process is repeated three times, and then the flocculated product is added to absolute ethanol, shaken and allowed to stand. When the flocculated product and absolute ethanol are separated, the supernatant is discarded and more absolute ethanol is added. This process is repeated three times.
[0042] 4 is a SEM image of the ultra-long nano silver wire material prepared in Example 3 of the present invention. As can be seen, the obtained product has a one-dimensional nano wire structure, with good nano wire dispersion and uniform diameter. EXAMPLES
[0043] This embodiment includes the following steps: Step 1: Fructose and polyvinylpyrrolidone with a molecular weight of 58,000 Daltons are added to deionized water and stirred uniformly to obtain a clear solution, the molar ratio of fructose, polyvinylpyrrolidone and water is 1:0.08:350, and the molar mass of fructose is 0.02 mmol; Step 2: Add iron (II) sulfate solution to the clear solution obtained in step 1 and stir evenly for 1 h to obtain mixed solution A, the molar mass of the iron (II) sulfate is 10 mmol; Step 3: Add sodium chloride solution to the mixed solution A obtained in step 2 and stir uniformly for 1.5 hours to obtain mixed solution B, in which the molar mass of sodium chloride is 4 mmol; Step 4: Drop the silver nitrate solution into the mixed solution B of step 3 and stir to obtain a reaction solution. Then, transfer the reaction solution to a hydrothermal reactor and react at 120°C for 18 hours to obtain a flocculated product. In the silver nitrate solution, the molar mass of silver nitrate is 8 mmol; Step 5: The flocculated product obtained in step 4 is successively precipitated and washed using deionized water and absolute ethanol to obtain an ultralong nano silver wire material. In the precipitation washing process, the flocculated product is added to deionized water, shaken and allowed to stand. When the flocculated product and deionized water are separated, the supernatant is discarded and more deionized water is added. This process is repeated three times, and then the flocculated product is added to absolute ethanol, shaken and allowed to stand. When the flocculated product and absolute ethanol are separated, the supernatant is discarded and more absolute ethanol is added. This process is repeated three times.
[0044] 5 is a SEM image of the ultra-long nano silver wire material prepared in Example 4 of the present invention. As can be seen from the figure, the obtained product has a one-dimensional nano wire structure and good nano wire dispersion. EXAMPLES
[0045] This embodiment includes the following steps: Step 1: Sucrose and polyvinylpyrrolidone with a molecular weight of 58000 Daltons are added to deionized water and stirred uniformly to obtain a clear solution, the molar ratio of fructose, polyvinylpyrrolidone and water is 1:0.07:550, and the molar mass of sucrose is 0.03 mmol; Step 2: Add nickel nitrate solution to the clear solution obtained in step 1 and stir evenly for 1 h to obtain mixed solution A, in which the molar mass of nickel nitrate is 17 mmol; Step 3: Add sodium chloride solution to the mixed solution A obtained in step 2 and stir uniformly for 0.5 h to obtain mixed solution B, in which the molar mass of sodium chloride is 4 mmol; Step 4: Drop the silver nitrate solution into the mixed solution B of step 3 and stir to obtain a reaction solution. Then, transfer the reaction solution to a hydrothermal reactor and react at 115°C for 15 hours to obtain a flocculated product. In the silver nitrate solution, the molar mass of silver nitrate is 12 mmol; Step 5: The flocculated product obtained in step 4 is successively precipitated and washed using deionized water and absolute ethanol to obtain an ultralong nano silver wire material. In the precipitation washing process, the flocculated product is added to deionized water, shaken and allowed to stand. When the flocculated product and deionized water are separated, the supernatant is discarded and more deionized water is added. This process is repeated three times, and then the flocculated product is added to absolute ethanol, shaken and allowed to stand. When the flocculated product and absolute ethanol are separated, the supernatant is discarded and more absolute ethanol is added. This process is repeated three times.
[0046] 6 is a SEM image of the ultra-long nano silver wire material produced in Example 5 of the present invention. As can be seen, the product obtained has a one-dimensional nano wire structure, with good dispersion of the nano wires, and the length of the nano wires is large, exceeding the length characterized by this magnification. EXAMPLES
[0047] This embodiment includes the following steps: Step 1: Glucose and polyvinylpyrrolidone with a molecular weight of 58000 Daltons are added to deionized water and stirred uniformly to obtain a clear solution, the molar ratio of glucose, polyvinylpyrrolidone and water is 1:0.06:450, and the molar mass of glucose is 0.01 mmol; Step 2: Add copper nitrate solution to the clear solution obtained in step 1 and stir evenly for 0.5 h to obtain mixed solution A, in which the molar mass of copper nitrate is 5 mmol; Step 3: Add sodium chloride solution to the mixed solution A obtained in step 2 and stir uniformly for 1 h to obtain mixed solution B, in which the molar mass of sodium chloride is 1.2 mmol; Step 4: Drop the silver nitrate solution into the mixed solution B of step 3 and stir to obtain a reaction solution. Then, transfer the reaction solution to a hydrothermal reactor and react at 120°C for 16 hours to obtain a flocculated product. In the silver nitrate solution, the molar mass of silver nitrate is 4.5 mmol; Step 5: The flocculated product obtained in step 4 is successively precipitated and washed using deionized water and absolute ethanol to obtain an ultralong nano silver wire material. In the precipitation washing process, the flocculated product is added to deionized water, shaken and allowed to stand. When the flocculated product and deionized water are separated, the supernatant is discarded and more deionized water is added. This process is repeated three times, and then the flocculated product is added to absolute ethanol, shaken and allowed to stand. When the flocculated product and absolute ethanol are separated, the supernatant is discarded and more absolute ethanol is added. This process is repeated three times.
[0048] 7 is a SEM image of the ultra-long nano silver wire material prepared in Example 6 of the present invention. As can be seen, the obtained product has a one-dimensional nano wire structure, with good nano wire dispersion and uniform diameter. EXAMPLES
[0049] This embodiment includes the following steps: Step 1: Maltose and polyvinylpyrrolidone with a molecular weight of 8000 Daltons are added to deionized water and stirred uniformly to obtain a clear solution, the molar ratio of the maltose, polyvinylpyrrolidone and water is 1:0.1:500, and the molar mass of the maltose is 0.01 mmol; Step 2: Add iron(II) sulfate solution to the clear solution obtained in step 1 and stir evenly for 1 h to obtain mixed solution A, in which the molar mass of iron(II) sulfate in the iron(II) sulfate solution is 5.5 mmol; Step 3: Add sodium chloride solution to the mixed solution A obtained in step 2 and stir uniformly for 1 h to obtain mixed solution B, in which the molar mass of sodium chloride is 1.2 mmol; Step 4: Drop the silver nitrate solution into the mixed solution B of step 3 and stir to obtain a reaction solution. Then, transfer the reaction solution to a hydrothermal reactor and react at 130°C for 18 hours to obtain a flocculated product. In the silver nitrate solution, the molar mass of silver nitrate is 4 mmol; Step 5: The flocculated product obtained in step 4 is successively precipitated and washed using deionized water and absolute ethanol to obtain an ultralong nano silver wire material. In the precipitation washing process, the flocculated product is added to deionized water, shaken and allowed to stand. When the flocculated product and deionized water are separated, the supernatant is discarded and more deionized water is added. This process is repeated three times, and then the flocculated product is added to absolute ethanol, shaken and allowed to stand. When the flocculated product and absolute ethanol are separated, the supernatant is discarded and more absolute ethanol is added. This process is repeated three times. EXAMPLES
[0050] This embodiment includes the following steps: Step 1: Glucose and polyvinylpyrrolidone are added to deionized water and stirred uniformly to obtain a clear solution, the molar ratio of glucose, polyvinylpyrrolidone and water is 1:0.08:560, and the molar mass of glucose is 0.01 mmol; Step 2: Add copper sulfate solution to the clear solution obtained in step 1 and stir evenly to obtain mixed solution A, in which the molar mass of copper sulfate is 5.4 mmol; Step 3: Add sodium chloride solution to the mixed solution A obtained in step 2 and stir uniformly to obtain mixed solution B, in which the molar mass of sodium chloride is 1.3 mmol; Step 4: Drop the silver nitrate solution into the mixed solution B of step 3 and stir to obtain a reaction solution. Then, transfer the reaction solution to a hydrothermal reactor and react at 120°C for 14 hours to obtain a flocculated product. In the silver nitrate solution, the molar mass of silver nitrate is 5 mmol; Step 5: The flocculated product obtained in step 4 is washed by sequential settling with deionized water and anhydrous ethanol to obtain ultra-long nano silver wire material. In the settling and washing process, the flocculated product is added to deionized water, shaken and left to stand, when the flocculated product and deionized water are separated, the supernatant is discarded, and more deionized water is added, and this process is repeated five times, and then the flocculated product is added to anhydrous ethanol, shaken and left to stand, when the flocculated product and anhydrous ethanol are separated, the supernatant is discarded, and more anhydrous ethanol is added, and this process is repeated three times. Figure 8 is an SEM image of the ultra-long nano silver wire material produced in this embodiment. As can be seen from Figure 8, the product obtained is a nanowire structure, and no other forms or other impurity products are found in the product other than the one-dimensional nanowire structure, which indicates that the purity of the product obtained is high and the diameter distribution of the obtained nanowires is uniform, and the aspect ratio of the ultra-long nano silver wire material is much greater than 3000.
[0051] Although specific embodiments of the present invention have been described above, those skilled in the art will understand that these are merely examples, and that various changes or modifications can be made to these embodiments without departing from the principles and essence of the present invention. Therefore, the patent scope of the present invention is defined by the appended claims.
Claims
1. Step 1: adding glucose and polyvinylpyrrolidone to deionized water and stirring uniformly to obtain a clear solution, the molar ratio of the glucose, the polyvinylpyrrolidone and the deionized water is 1:0.05-0.1:280-560; Step 2: adding a copper sulfate solution to the clear solution obtained in step 1 and stirring the mixture to obtain a mixed solution A, in which the molar ratio of the glucose to the copper sulfate in the mixed solution A is 1:480-600; Step 3: adding a sodium chloride solution to the mixed solution A obtained in step 2 and stirring uniformly to obtain a mixed solution B, in which the molar ratio of the sodium chloride to the copper sulfate in the mixed solution B is 1:3 to 4.8; Step 4: adding silver nitrate solution dropwise to the mixed solution B obtained in step 3 and stirring to obtain a reaction solution, and then transferring the reaction solution to a hydrothermal reaction vessel and reacting at 110°C to 130°C for 14h to 20h to obtain a flocculated product, in which the molar ratio of the glucose to the silver nitrate in the reaction solution is 1:300 to 500; and step 5, using deionized water and absolute ethanol to sequentially sediment and wash the flocculated product obtained in step 4, to obtain a nanosilver wire material having an aspect ratio of more than 1000.
2. In step 5, in the sedimentation washing process, the flocculated product is added to deionized water, shaken and left to stand, when the flocculated product and deionized water are separated, the supernatant is discarded and more deionized water is added, and this process is repeated 3 to 5 times, and then the flocculated product is added to absolute ethanol, shaken and left to stand, when the flocculated product and absolute ethanol are separated, the supernatant is discarded and more absolute ethanol is added, and this process is repeated 3 to 5 times.
Citation Information
Patent Citations
Method of manufacturing high aspect ratio silver nanowire
JP2013231231A
Method for manufacturing silver nanowire with low oxygen
JP2016135909A
Method for manufacturing silver nanowire
JP2016166402A