Manufacturing method for Li-ion-containing cathode material

Coating LiMn0.5Ni0.5O4 cathode materials with a SiO2 layer formed from polysilazane addresses the issue of electrolyte decomposition, enhancing discharge capacity and cycle stability in lithium ion batteries.

JP7576769B2Active Publication Date: 2024-11-01NIIGATA UNIVERSITY +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020180351
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-28
Publication Date
2024-11-01
Estimated Expiration
2040-10-28

AI Technical Summary

Technical Problem

Conventional LiMn0.5Ni0.5O4 (LNMO) cathode materials suffer from poor discharge capacity at high temperatures and rates due to electrolyte oxidation and decomposition, and surface coatings to prevent this hinder lithium ion conduction, leading to poor charge and discharge performance.

Method used

A SiO2 layer is formed on the surface of LiMn0.5Ni0.5O4 particles by adding polysilazane to the precursor, which enhances lithium ion conduction and improves cycle characteristics without compromising discharge capacity.

Benefits of technology

The SiO2-coated LiMn0.5Ni0.5O4 exhibits improved discharge capacity and cycle stability at medium to high rates, maintaining excellent charge/discharge performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576769000002
    Figure 0007576769000002
  • Figure 0007576769000003
    Figure 0007576769000003
  • Figure 0007576769000004
    Figure 0007576769000004
Patent Text Reader

Abstract

To provide a positive electrode material that indicates a high discharge capacity, and has an excellent cycle stability, and a lithium ion secondary battery containing the positive electrode material.SOLUTION: A manufacturing method of a positive electrode material, contains at least first to third steps. In the first step, a Li ion inclusion oxide is prepared as a precursor. In the second step, a polysilazane is applied to the precursor. In the third step, the precursor and the polysilazane are mixed and reacted under a temperature range of 0°C to 50°C, and a SiO2 layer having a Si component in the polysilazane is coated to an outer peripheral surface of a crystal grain of the Li ion inclusion oxide. The Li ion inclusion oxide is preferably at least one of LiNi0.5Mn1.5O4, LiCoO2, and LiFePO4. In the second step, it is preferable polysilazane be added so that SiO2 derived from the polysilazane becomes 0.1wt% to 10wt% of the precursor.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode material that can be used in lithium ion secondary batteries and the like, and a method for producing the same. [Background technology]

[0002] Lithium-ion secondary batteries are widely used as power sources for small electronic devices such as mobile phones, laptops, and digital cameras. In recent years, lithium-ion secondary batteries with increased energy density have been attracting attention as a power source for electric vehicles.

[0003] (LMNO) LiNi was synthesized by replacing part of the Mn in LiMn2O4 with Ni as a solid solution, which has a spinel structure. 0.5 Mn 1.5 The O4 (hereinafter, also referred to as "LNMO") positive electrode is known to operate at a high voltage of about 5 V (4.7 V). The energy density of LNMO is 686 Wh / kg, which is higher than other positive electrode materials, and it is expected to be used as a positive electrode for lithium-ion secondary batteries for electric vehicles (for example, see Patent Document 1 and Non-Patent Document 1).

[0004] (Issues with conventional cathode materials, including LMNO) However, as mentioned above, LNMO operates at high voltages, and the electrolyte is oxidized and decomposed on the positive electrode, resulting in poor discharge capacity at high temperatures and high rates.

[0005] To prevent this phenomenon, a measure has been proposed in the past in which the particle surfaces are coated with insulating oxides such as magnesium oxide (see, for example, Non-Patent Documents 2-3). Although this measure can improve cycle characteristics by suppressing decomposition of the electrolyte, it has the problem of being inferior in terms of charge / discharge performance because it inhibits the conduction of lithium ions. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2015 / 083481 Brochure [Non-patent literature]

[0007] [Non-Patent Document 1] Yo Kobayashi et al., “5V Class All-Solid-State Composite Lithium Battery with Li3PO4 Coated LiNi0.5Mn1.5O4”, Journal of The Electrochemical Society, 150(12) A1577-A1582(2003) [Non-Patent Document 2] D. Arumugam et al., “Synthesis and electrochemical characterizations of Nano-SiO2-coated LiMn2O4 cathode materials for rechargeable lithium batteries”, Journal of Electroanalytical Chemistry 624(1-2), 197-204 (2008) [Non-Patent Document 3] Y. Iriyama et al., “Effects of surface modification by MgO on interfacial reactions of lithium cobalt oxide thin film electrode”, Journal of Power Sources, 137, 1, 111-116 (2004) [Non-Patent Document 4] J. Huang et al., “Enhancing the Ion Transport in LiMn1.5Ni0.5O4 by Altering the Particle Wulff Shape via Anisotropic Surface Segregation”, ACS Applied Materials & Interfaces, 9, 36745-36754 (2017) Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, the present invention aims to provide a positive electrode material with improved charge / discharge performance by adding polysilazane to a raw material (precursor) such as LNMO and coating the periphery of the precursor crystal with SiO2. [Means for solving the problem]

[0009] The inventors discovered that by coating a raw material (precursor) such as LNMO with SiO2, it is possible to produce a positive electrode material such as LNMO that exhibits good discharge capacity at a relatively high charging rate and has excellent cycle characteristics, and thus completed the present invention.

[0010] The present invention has, for example, the following configurations and features. (Aspect 1) A first step of preparing a Li-ion-containing oxide as a precursor; A second step of adding polysilazane to the precursor; a third step of mixing and reacting the precursor with the polysilazane in a temperature range of 0° C. to 50° C. to coat an SiO2 layer containing the Si component in the polysilazane on the outer peripheral surfaces of the crystal particles of the Li-ion-containing oxide; Including See, and The Li-ion-containing oxide is LiNi 0.5 Mn 1.5 O 4 , LiCoO 2 or LiFePO 4 At least one of , In the second step, the precursor is treated with the polysilazane-derived SiO 2 The polysilazane is added so that the content is 0.1 wt% to 5 wt%. A method for producing a Li-ion-containing positive electrode material, comprising: Effect of the Invention

[0011] The Li-ion-containing positive electrode material of the present invention produced by the above-mentioned method exhibits good discharge capacity at medium or high charge / discharge rates and exhibits excellent cycle characteristics. [Brief description of the drawings]

[0012] [Figure 1] 1 is a flowchart showing the manufacturing process of Example 1 (SiO 2 layer-coated LNMO). [Diagram 2] FIG. 1 shows powder XRD patterns of samples of Example 1 and Comparative Example 1. [Diagram 3] 1 is a SEM image showing the crystal structures of samples of Example 1 and Comparative Example 1. [Figure 4] 1 shows the charge / discharge characteristics (capacity retention rate) of electrochemical cells produced using the samples of Example 1 and Comparative Example 1. [Diagram 5] 1 is a flowchart showing the manufacturing process of Example 2 (SiO 2 layer-coated LCO). [Figure 6] FIG. 2 shows powder XRD patterns of samples of Example 2 and Comparative Example 2. [Figure 7] 1 is a SEM image showing the crystal structures of the samples of Example 2 and Comparative Example 2. [Figure 8] 1 shows the capacity retention rates of electrochemical cells made using the samples of Example 2 and Comparative Example 2. [Figure 9] 1 is a flow chart showing the manufacturing process of Example 3 (SiO 2 layer-coated LFP). [Figure 10] FIG. 2 shows powder XRD patterns of samples of Example 3 and Comparative Example 3. [Figure 11] 1 is a SEM image showing the crystal structures of the samples of Example 3 and Comparative Example 3. [Figure 12]1 shows the capacity retention rates of electrochemical cells made using the samples of Example 3 and Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments.

[0014] (Raw material (precursor) for Li-ion-containing cathode materials) The Li-ion-containing positive electrode material of the present invention is composed of crystal particles of a Li-ion-containing oxide. Here, the "Li-ion-containing oxide" defined in the present invention is LiNi 0.5 Mn 1.5 It is particularly preferable that the oxide containing Li ions is at least one of Li(Co,Ni,Mn)O4 (hereinafter also referred to as LNMO), LiCoO2 (hereinafter also referred to as LCO), or LiFePO4 (hereinafter also referred to as LFP), but is not necessarily limited to these. The Li-ion-containing oxide also includes, for example, Li(Co,Ni,Mn)O2 in which a part of the Co element is replaced with Ni and / or Mn.

[0015] (SiO2 layer) In addition, the present invention is characterized in that the outer peripheral surface of the crystal particle made of the Li-ion-containing oxide is coated with a SiO2 layer. This SiO2 layer is preferably formed of a Si component derived from polysilazane. The SiO2 layer is preferably contained in an amount of 0.1 wt% to 10 wt% relative to the Li-ion-containing oxide.

[0016] (Method of manufacturing the cathode material of the present invention) The method for producing a cathode material of the present invention includes a first step of preparing a Li-ion-containing oxide as a precursor. As described above, the Li-ion-containing oxide is preferably LNMO, LCO, or LFP. These precursors may be commercially available products, or may be produced prior to the present method.

[0017] (LNMO precursor) The LNMO precursor can be synthesized by, for example, a solid-phase reaction of Li2CO3, NiO, and MnO2. During this reaction, the mixture of raw materials is preferably fired at a temperature in the range of 500°C to 1,000°C. The firing time is preferably about 1 to 12 hours. Here, the LNMO precursor is usually LiNi 0.5 Mn 1.5 The target composition is O4, but due to the manufacturing process, Χ Mn 2-Χ O4 (however, 0.3≦X≦0.7), and the composition of Ni and Mn may vary within the range of 0.3≦X≦0.7.

[0018] (LCO precursor) The LCO precursor can be synthesized by, for example, a solid-phase reaction of Li2CO3 and Co3O4. During this reaction, the mixture of raw materials is preferably fired at a temperature in the range of 500°C to 1,000°C. The firing time is preferably about 1 to 12 hours.

[0019] (LFP precursor) For example, a precursor made of LFP can be synthesized by a solid-state reaction of Li2CO3, Fe(II)C2O4·H2O, and (NH4)2HPO4. During this reaction, the mixture of raw materials is preferably fired at a temperature in the range of 300°C to 1,000°C. The firing time is preferably 1 to 36 hours (more preferably about 6 to 12 hours).

[0020] The LNMO precursor, LCO precursor, or LFP precursor can be synthesized, for example, by mixing a number of other inexpensive raw materials, but commercially available LNMO, LCO, or LFP itself may also be prepared.

[0021] (Polysilazane) The polysilazane added to the LNMO precursor is a compound represented by the following chemical formula (1).

[0022] [ka]

[0023] In chemical formula (1), R 1 R are hydrogen atoms or groups selected from aliphatic hydrocarbon groups having 1 to 12 carbon atoms, aromatic hydrocarbon groups having 6 to 12 carbon atoms, alkoxy groups having 1 to 6 carbon atoms, and monovalent organic groups having 2 to 12 carbon atoms and one carbon-carbon unsaturated bond per molecule, and may be the same or different. 2 is a group selected from an aliphatic hydrocarbon group having 1 to 12 carbon atoms, an aromatic hydrocarbon group having 6 to 12 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, and a monovalent organic group having 2 to 12 carbon atoms and one carbon-carbon unsaturated bond per molecule. a is a positive number of 5 or more, b, c, and d are each 0 or a positive number, b / (a+b+c+d)=0 to 0.9, and a+b+c+d=a positive number of 5 to 22,200.

[0024] Here, R 1 and R 2 Examples of the aliphatic hydrocarbon group having 1 to 12 carbon atoms include a methyl group, an ethyl group, an n-propyl group, a hexyl group, an octyl group, a decyl group, a trifluoropropyl group, etc. Examples of the aromatic hydrocarbon group having 6 to 12 carbon atoms include a phenyl group, a methylphenyl group, a dimethylphenyl group, a trimethylphenyl group, etc. Examples of the alkoxy group having 1 to 6 carbon atoms include a methoxy group, an ethoxy group, etc.

[0025] Examples of monovalent organic groups having 2 to 12 carbon atoms and one carbon-carbon unsaturated bond per molecule include alkenyl groups such as a vinyl group, an allyl group, a 4-vinylbutyl group, and an 8-vinyloctyl group; alicyclic unsaturated hydrocarbon groups such as a 3-cyclohexenyl group and a norbornenyl group; alkynyl groups such as an ethynyl group and a 2-propynyl group; aromatic unsaturated hydrocarbon groups such as a styryl group; unsaturated ester groups such as an acryl group and a methacryl group; and unsaturated cyclic imides such as an N-propylmaleimide group.

[0026] Among the above examples, methyl and phenyl groups are preferred because of ease of synthesis. 1is a hydrogen atom and R 2 More preferred is an inorganic polysilazane having a structure that does not contain

[0027] Here, R 1 Polysilazanes in which R is a hydrogen atom and do not contain a b structure are inorganic polysilazanes. 1 Polysilazanes containing an organic group other than hydrogen atom and / or a structure are used as organic polysilazanes depending on the application and purpose. In the present invention, both inorganic polysilazanes and organic polysilazanes can be used, but the use of inorganic polysilazanes is preferred because it is not only advantageous for the formation of SiO2 but also makes it easier for the precursor crystals to be coated with SiO2.

[0028] In the above chemical formula (1), a is a positive number of 5 or more, preferably 30 to 220, and b, c, and d are each 0 or a positive number, preferably b is 0 to 30, c is 1 to 30, and d is 1 to 4. In addition, b / (a+b+c+d)=0 to 0.9, and a+b+c+d=a positive number of 5 to 22,200, preferably 30 to 300.

[0029] The polysilazane in the present invention is characterized by having a weight average molecular weight of 200 to 1,000,000 measured by gel permeation chromatography (GPC) using THF (tetrahydrofuran) as an eluent from the viewpoint of solution stability and workability during application and impregnation, preferably within the range of 1,000 to 100,000, more preferably 2,000 to 20,000. If the weight average molecular weight is less than 200, it is not preferable because it is highly volatile, the amount of SiO2 coated on the precursor varies, and the improvement of the positive electrode material characteristics becomes unstable. Also, if it exceeds 1,000,000, it is not preferable because it is not sufficiently dissolved in an organic solvent, not only is the stability of the solution poor, but also the effect of SiO2 coating on the precursor is not fully exhibited. The weight average molecular weight referred to in the present invention refers to the weight average molecular weight measured by gel permeation chromatography (GPC) using polystyrene as a standard substance under the following conditions.

[0030] [Measurement conditions] Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.6mL / min Detector: UV detector Column: (The following two types, both manufactured by Tosoh Corporation) TSK Guardcolumn SuperH-L TSKgel SuperMultiporeHZ-M(4.6mmI.D.×15cm×4) Column temperature: 40℃ Sample injection volume: 20 μL (THF solution with a concentration of 0.5% by mass in terms of SiO2)

[0031] (Organic solvent) The polysilazane of the present invention is used by dissolving it in an organic solvent. The organic solvent is not particularly limited as long as it dissolves the polysilazane. For example, saturated chain aliphatic hydrocarbons such as n-pentane, i-pentane, n-hexane, i-hexane, n-heptane, i-heptane, n-octane, i-octane, 2,2,4-trimethylpentane (isooctane), n-nonane, i-nonane, n-decane, i-decane, and 2,2,4,6,6-pentamethylheptane (isododecane) are used, and saturated cyclic aliphatic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, ethylcyclohexane, p-menthane, and decahydronaphthalene are used. Benzene, toluene, xylitol, and the like are used. Examples of the aromatic ether include aromatic hydrocarbons such as benzene, ethylbenzene, diethylbenzene, trimethylbenzene, triethylbenzene, and tetrahydronaphthalene; alkyl ethers such as dipropyl ether, dibutyl ether, diethyl ether, dipentyl ether, dihexyl ether, methyl tertiary butyl ether, and butoxyethyl ether; aryl ethers such as anisole and diphenyl ether; and ester compounds such as n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, isoamyl acetate, and ethyl caproate.

[0032] Among the above examples, from the viewpoint of solubility in polysilazane, aromatic hydrocarbons, alkyl ethers, and saturated aliphatic hydrocarbons are preferred as organic solvents, and saturated aliphatic hydrocarbons having 4 to 20 carbon atoms are particularly preferred.

[0033] The mixing ratio of polysilazane to the organic solvent is in the range of 0.1 / 99.9 to 50 / 50 by mass ratio, preferably 0.5 / 99.5 to 30 / 70, more preferably 1 / 99 to 20 / 80. Within this range, not only the solubility and storage stability but also the coating operation of the SiO2 layer on the precursor is favorable, which is preferable.

[0034] (Amount of polysilazane added) The amount of polysilazane added in the present invention varies depending on the type of precursor, but is set so that SiO2 derived from polysilazane is 0.1 wt% to 10 wt% relative to the precursor. When an LNMO precursor is used, it is preferably set so that SiO2 derived from polysilazane is 1 wt% to 5 wt%. When an LCO precursor is used, it is preferably set so that SiO2 derived from polysilazane is 1 wt% to 5 wt% (more preferably 2 wt% to 4 wt%). When an LFP precursor is used, it is preferably set so that SiO2 derived from polysilazane is 1 wt% to 5 wt%.

[0035] (Synthesis of polysilazane and precursor at room temperature) In addition, the present invention is characterized in that the environmental temperature when polysilazane and any of the above-mentioned precursors are mixed and synthesized is within the range of room temperature (specifically, 0°C to 50°C, more preferably 10°C to 40°C, and even more preferably 10°C to 30°C). According to conventional knowledge in the technical field, a baking step is generally required for the synthesis of polysilazane and a precursor. However, the present inventors have found that the above synthesis proceeds sufficiently without placing the mixture in a high-temperature environment due to baking (i.e., even in a room temperature environment).

[0036] The present invention will be described below based on examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and they are not excluded from the scope of the present invention. EXAMPLES

[0037] (Synthesis of LNMO precursor, addition of polysilazane, and coating with SiO2 layer) FIG. 1 shows a flow chart showing the manufacturing process of the Li-ion-containing positive electrode material (specifically, SiO2-layer-coated LNMO) of the present invention. As shown in FIG. 1, the LNMO precursor was synthesized by a solid-phase reaction. Specifically, Li2CO3 (purity 99.0%, manufactured by Kanto Chemical Co., Ltd.), NiO (purity 99.0%, manufactured by Fujifilm Wako Pure Chemical Co., Ltd.), and MnO2 (purity 99.0%, manufactured by Kojundo Chemical Laboratory Co., Ltd.) were weighed based on the stoichiometric ratio. Toluene (purity 99.5%, manufactured by Kanto Chemical Co., Ltd.) was added as a dispersion medium to these raw materials, and the above raw materials were mixed at a speed of 200 rpm for 2 hours using a ball mill. The obtained mixture was placed in an alumina boat, and the mixture was fired in air with a flow rate of 50 ml / min under the conditions of 900 °C / 6 hours, and then cooled to room temperature to obtain LNMO (precursor). The obtained LNMO (precursor) was pulverized in an agate mortar.

[0038] (Synthesis of Polysilazane) 0.19 mol of dichlorosilane with a purity of 99% or more was blown into 300 ml of dehydrated pyridine at -10°C while stirring with nitrogen. Then, 0.57 mol of ammonia with a purity of 99% or more was blown in, and the salt formed was removed by pressure filtration to synthesize polysilazane. This pyridine solution of polysilazane was heated to 150°C, and 150 ml of pyridine was distilled off. Next, 300 ml of dibutyl ether was added, and pyridine was removed by azeotropic distillation. Dibutyl ether was added so that polysilazane was 5 parts by mass per 100 parts by mass of the entire solution to prepare a polysilazane solution. The weight average molecular weight of polysilazane contained in this polysilazane solution was 3,800.

[0039] (Preparation of LNMO / SiO2 (Example 1: SiO2 layer-coated LNMO)) Polysilazane was added to 1 g of LNMO (precursor) synthesized in the above process, mixed, and the mixture was reacted at room temperature (10 to 30°C) to produce SiO2 layer-coated LNMO (LNMO / SiO2 in Figures 1 and 2). In detail, the polysilazane solution prepared above was added to LNMO (precursor) so that the SiO2 derived from polysilazane was 1 wt%, 2 wt%, 5 wt%, and 10 wt% relative to LNMO (precursor), respectively, and these were dispersed in a dibutyl ether solution. After that, these composites were filtered, washed, and dried to obtain "LNMO / SiO2", which is the positive electrode material of Example 1. The obtained sample was used to evaluate the characteristics described below. For reference, the LMNO precursor in a state where the above polysilazane solution was not added (i.e., 0 wt%) was also evaluated (Comparative Example 1).

[0040] (Evaluation by powder X-ray diffraction measurement (XRD)) The crystal phases of the powder samples obtained in Example 1 and Comparative Example 1 were identified using powder X-ray diffraction measurement (MX-Labo, manufactured by Mac Science). For the identification, the LNMO pattern stored in the Inorganic Crystal Structure Database (ICSD) was used as a comparison.

[0041] (Evaluation Results of Example 1 by XRD) Figure 2 shows the powder XRD patterns of the powder samples of Example 1 (see 2 wt% in the figure) and Comparative Example 1 (see 0 wt% in the figure). Here, by comparing with LNMO (#239165) cited from ICSD shown in the top row of the figure, it was determined that LNMO was obtained as the main phase in both samples.

[0042] In addition, no change or shift in the XRD pattern was observed depending on the amount of polysilazane added. The reason for this is thought to be that the amount of SiO2 in LNMO is small, at 1-10 wt% or less relative to the weight of LNMO, so no peaks derived from Si were observed. The impurity peak observed near 37° is thought to be due to remaining NiO used as a raw material.

[0043] (Evaluation by scanning electron microscope (SEM)) A scanning electron microscope (JSM-5310MVB, manufactured by JEOL Datum Co., Ltd.) was used to observe the particle shape and particle size of Example 1 and Comparative Example 1. A carbon sheet was attached onto the sample stage, and a small amount of powder sample was placed on the carbon sheet and observed at a voltage of 15 kV.

[0044] (SEM evaluation results) Fig. 3 shows SEM images showing the crystal structures of the powder samples of Example 1 and Comparative Example 1. Specifically, Fig. 3(a) shows an SEM image of Comparative Example 1 (0 wt%), and Figs. 3(b) to (d) show SEM images of Example 1 (2 wt%, 5 wt%, or 10 wt%). Both Comparative Example 1 and Example 1 exhibited a spherical particle structure, and no significant difference was observed in the particle state.

[0045] (Preparation of electrochemical cells) Next, a positive electrode material was prepared using the powder samples of Comparative Example 1 and Example 1, and a negative electrode material and an electrolyte were also prepared. These were combined to prepare an electrochemical cell.

[0046] (Cathode materials for electrochemical cells) The powder sample obtained in Example 1 or Comparative Example 1, acetylene black (manufactured by Denka Co., Ltd.) as a conductive assistant, and polyvinylidene fluoride (PVDF#9130, Kureha Co., Ltd.) as a binder were weighed to a mass ratio of 85:8:7, and added to an ointment bottle (UG type 3-52, 12 ml, manufactured by Umano Chemical Container Co., Ltd.). N-methyl-2-pyrrolidone (99.0%, manufactured by Kanto Chemical Co., Ltd.) was added as a solvent to the mixture and stirred for 20 minutes with a stirring device (AR-100, manufactured by Shinki Co., Ltd.), and then degassed for 5 minutes. After that, the mixture was stirred again for 1 minute, and the sample in a slurry state was applied onto aluminum foil. Next, the mixture was vacuum-heated at 75°C for 40 minutes using a vacuum dryer (AVO-200NS, manufactured by AS ONE Co., Ltd.), and cooled to room temperature in a vacuum state over 4 hours. Thereafter, a pressure of 20 MPa was applied to the above sample using a press, and the sample was heated in a vacuum at 130° C. for 5.5 hours, and then cooled to room temperature in a vacuum state over a period of 4 hours.

[0047] (Anode materials for electrochemical cells) The negative electrode was made of a circular piece of lithium foil cut out in a glove box (UN650F, manufactured by UNICO Corporation) filled with argon gas.

[0048] (Electrolyte for electrochemical cells) The electrolyte used was a 1 mol / L lithium hexafluorophosphate EC:DMC (1:1 v / v%) solution (Kishida Chemical Co., Ltd., EC: ethylene carbonate, DMC: dimethyl carbonate). This electrolyte was handled in a glove box filled with argon gas.

[0049] (Assembling the electrochemical cell) The cell (HS Flat Cell, manufactured by Hosen Co., Ltd.) was assembled in a glove box filled with argon gas. The negative electrode material (metallic lithium foil), a nonwoven fabric to protect it, a separator to prevent direct contact between the positive electrode material and the negative electrode material, a nonwoven fabric to protect the positive electrode material, and the positive electrode material were placed in this order in the bottom lid of the cell, and then the electrolyte was added. The top lid of the cell was then closed and sealed to assemble the electrochemical cell.

[0050] (Evaluation of the discharge characteristics of electrochemical cells) The cells assembled as described above were subjected to charge / discharge measurements using a charge / discharge device (HJ-101SM6, Hokuto Denko Corporation, PFX2011, Kikusui Electronics Co., Ltd.). The current density was based on the C rate. The C rate is defined as the current density at which the theoretical capacity of the positive electrode is completely drawn out in 1 hour, and indicates the rate of discharge and charge. The charge / discharge capacity was measured at 0.1C, 0.5C, 1C, 5C, 10C, and finally at 0.1C again. Five cycles were performed at each C rate, for a total of 30 cycles. A pre-discharge time of 2 hours was set before the start of the measurement, and a rest time of 30 min was set between charge and discharge at 0.1C, 15 min at 0.5C, and 15 min at 1C. No rest time was set at 5C and 10C.

[0051] (Measurement results of discharge capacity of electrochemical cell) Fig. 4(a) shows the results of comparing the capacity retention rates of electrochemical cells using Example 1 (2 wt%) and Comparative Example 1 (0 wt%) measured by the above method. Fig. 4(a) shows that the capacity retention rate of Example 1 is higher than that of Comparative Example 1 at each rate (especially at high rates of 5C and 10C, the capacity retention rate is significantly higher).

[0052] 4(b) and (c) show the change in capacity retention rate at high rates of 5C and 10C when Example 1 with different SiO2 coating concentrations was used. From these results, it was found that Example 1 with SiO2 coating exhibited a higher capacity retention rate than Comparative Example 1. In addition, it was observed that the capacity retention rate tended to increase as the polysilazane addition rate increased, but even when 2 to 5 wt% or more was added, the increasing trend slowed down or remained almost constant. EXAMPLES

[0053] (Synthesis of LCO precursor, addition of polysilazane, and coating of SiO2 layer) Figure 5 shows a flow chart illustrating the manufacturing process of the Li-ion-containing positive electrode material (specifically, SiO2-layer-coated LCO) of the present invention. As shown in Figure 5, an LCO precursor was synthesized by a solid-phase reaction. Specifically, Li2CO3 (purity 99.0%, manufactured by Kanto Chemical Co., Ltd.) and Co3O4 (purity 99.95%, manufactured by Kanto Chemical Co., Ltd.) were weighed based on the stoichiometric ratio, and the mixture was fired and then cooled to room temperature to obtain LCO (precursor).

[0054] Then, in the same procedure as in Example 1, polysilazane was added to 1 g of LCO (precursor) synthesized in the above process, mixed, and the mixture was reacted at room temperature (10 to 30°C) to produce SiO2 layer-coated LCO (LCO / SiO2 in Figures 5 and 6). In detail, the polysilazane solution prepared above was added to LCO (precursor) so that the SiO2 derived from polysilazane was 1 wt%, 3 wt%, and 5 wt% relative to LCO (precursor), respectively, and these were dispersed in a dibutyl ether solution. Then, these composites were filtered, washed, and dried to obtain "LCO / SiO2", which is the cathode material of Example 2. Each of the obtained samples of Example 2 was evaluated in the same manner as in Example 1.

[0055] (Evaluation Results of Example 2 by XRD) 6 shows the powder XRD patterns of the powder samples of Example 2 (see 1 wt%, 3 wt%, and 5 wt% in the figure) and Comparative Example 2 (see 0 wt% in the figure). Here, by comparing with LCO (#172909) cited from ICSD shown in the top row of the figure, it was determined that LCO was obtained as the main phase in all samples.

[0056] (Evaluation results of Example 2 by SEM) Fig. 7 shows SEM images illustrating the crystal structures of the powder samples of Example 2 and Comparative Example 2. Specifically, Fig. 7(a) shows an SEM image of Comparative Example 2 (0 wt%), and Figs. 7(b) to (d) show SEM images of Example 2 (1 wt%, 3 wt%, or 5 wt%). Both Comparative Example 2 and Example 2 exhibited a spherical particle structure, and no significant difference was observed in the particle state.

[0057] (Measurement results of discharge capacity of electrochemical cell) Fig. 8(a) shows the results of comparing the capacity retention rates of electrochemical cells using Example 2 (2 wt%) and Comparative Example 1 (0 wt%) measured by the above method. Fig. 8(a) shows that the capacity retention rate of Example 2 is higher than that of Comparative Example 2 at each rate (especially at high rates of 5C and 10C, the capacity retention rate is significantly higher).

[0058] Figure 8(b) shows the change in capacity retention rate at a high rate of 10C when Example 2 with different SiO2 coating concentrations was used. From this result, it was found that Example 2 with SiO2 coating exhibited a higher capacity retention rate than Comparative Example 2. In addition, it was observed that the capacity retention rate tended to be highest when the polysilazane addition rate was about 2 to 3%. EXAMPLES

[0059] (Obtaining LFP precursor, adding polysilazane, and coating SiO2 layer) A flow chart showing the manufacturing process of the Li-ion-containing positive electrode material (specifically, the SiO2-layer-coated LFP) of the present invention is shown in Fig. 9. As shown in Fig. 9, in this embodiment, the LFP (precursor) was not synthesized in-house, but was purchased as a commercially available product (manufactured by Hosen Co., Ltd.).

[0060] Then, in the same procedure as in Example 1, polysilazane was added to 1 g of the above LFP (precursor) and mixed, and the mixture was reacted at room temperature (10 to 30°C) to prepare an SiO2 layer-coated LFP (LFP / SiO2 in Figures 9 and 10). In detail, the polysilazane solution prepared above was added to the LFP (precursor) so that the SiO2 derived from polysilazane was 1 wt%, 3 wt%, and 5 wt% relative to the LFP (precursor), respectively, and these were dispersed in a dibutyl ether solution. Then, these composites were filtered, washed, and dried to obtain "LFP / SiO2", which is the positive electrode material of Example 3. Each sample of Example 3 obtained was evaluated in the same manner as in Example 1.

[0061] (Evaluation Results of Example 3 by XRD) Figure 10 shows the powder XRD patterns of the powder samples of Example 3 (see 1wt%, 3wt%, and 5wt% in the figure) and Comparative Example 3 (see 0wt% in the figure). Here, by comparing with LFP (♯92198) cited from ICSD shown in the top row of the figure, it was determined that LFP was obtained as the main phase in both samples. Note that impurity peaks were observed in both Comparative Example 3 and Example 3, possibly because a commercially available precursor was used.

[0062] (Evaluation results of Example 3 by SEM) Fig. 11 shows SEM images illustrating the crystal structures of the powder samples of Example 3 and Comparative Example 3. Specifically, Fig. 11(a) shows an SEM image of Comparative Example 3 (0 wt%), and Figs. 11(b) to (d) show SEM images of Example 3 (1 wt%, 3 wt%, or 5 wt%). Both Comparative Example 3 and Example 3 exhibited a spherical particle structure, and no significant difference was observed in the particle state.

[0063] (Measurement results of discharge capacity of electrochemical cell) Figure 12 shows the change in capacity retention rate at a high rate of 10C when Example 3 with different SiO2 coating concentrations was used. From this result, it was found that Example 3 with SiO2 coating exhibited a higher capacity retention rate than Comparative Example 3. In addition, all samples with polysilazane addition rates exceeding 1wt% exhibited high capacity retention rates, but a tendency was observed that the sample with 3wt% had the highest capacity retention rate. [Industrial Applicability]

[0064] The Li-ion-containing oxide coated with a SiO2 layer produced by the above method exhibits good discharge capacity even at high charge / discharge rates and excellent cycle characteristics.

[0065] Therefore, the present invention has extremely high industrial applicability and applicability.

Claims

[Claim 1] A first step of preparing a Li-ion-containing oxide as a precursor; a second step of adding polysilazane to the precursor; The precursor and the polysilazane are mixed and reacted in a temperature range of 0°C to 50°C to obtain SiO having the Si component in the polysilazane. 2 a third step of coating the outer peripheral surface of the crystal particle of the Li-ion-containing oxide with a layer; and The Li-ion-containing oxide is at least one of LiNi 0.5 Mn 1.5 O 4 , LiCoO 2 , and LiFePO 4 ; In the second step, the polysilazane is added to the precursor so that the SiO 2 derived from the polysilazane is 0.1 wt % to 5 wt %. A method for producing a Li ion-containing positive electrode material, comprising:

Citation Information

Patent Citations

  • Positive electrode active material for lithium secondary battery and method of manufacturing the same

    JP2002164053A

  • Lithium secondary battery

    JP2005209469A

  • Electrode material for power storage device, power storage device, and electrical device

    JP2014096359A

  • Positive electrode for all-solid type lithium secondary batteries, and all-solid type lithium secondary battery arranged by use thereof

    JP2015185237A

  • Lithium ion secondary battery

    JP2017143049A