Wave absorber film and its manufacturing method
A thin radio wave absorber film with an aromatic ester-urethane copolymer binder resin and magnetic material provides superior absorption in high frequency bands, addressing the need for thinner and more effective absorbers.
Patent Information
- Application Number
- JP2021540702
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-19
- Filing Date
- 2020-07-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-07-30
AI Technical Summary
Existing radio wave absorbers are not thin enough and do not provide superior absorption performance, especially in high frequency bands such as the 76 GHz band and higher.
A radio wave absorber film is developed with a magnetic material and a binder resin containing an aromatic ester-urethane copolymer, applied as a coating on a base layer and dried to form a thin, effective absorption layer.
The film achieves excellent radio wave absorption performance, even in high frequency bands, with minimal thickness and improved crack resistance during bending or cutting.
Smart Images

Figure 0007576800000002 
Figure 0007576800000003 
Figure 0007576800000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a radio wave absorber film having excellent radio wave absorbing performance, and a manufacturing method thereof. [Background technology]
[0002] The use of radio waves in the high frequency band is becoming widespread in various information and communication systems such as mobile phones, wireless LAN, ETC systems, intelligent road transport systems, driving assistance systems, and satellite broadcasting. However, the expansion of the use of radio waves in the high frequency band raises concerns that interference between electronic components may lead to breakdowns and malfunctions of electronic devices. To address this issue, a method has been adopted in which unnecessary radio waves are absorbed by radio wave absorbers.
[0003] For this reason, even in radars and the like that use radio waves in the high frequency band, radio wave absorbers are used to reduce the effects of unnecessary radio waves that should not be received. In order to meet such demands, various radio wave absorbers capable of effectively absorbing radio waves in the high frequency band have been proposed, such as a radio wave absorbing sheet containing carbon nanocoils and resin (for example, Patent Document 1).
[0004] Among the applications of radio waves in the high frequency band, research has been progressing on driving assistance systems for automobiles. In such driving assistance systems, radio waves in the 76 GHz band are used in on-board radars for detecting the distance between vehicles, etc. It is predicted that the use of radio waves in high frequency bands, for example, 100 GHz or higher, will spread to various applications, not limited to driving assistance systems for automobiles. For this reason, there is a demand for radio wave absorbers that can effectively absorb radio waves in the 76 GHz band and higher frequency bands.
[0005] In order to meet such demands, as a radio wave absorber capable of absorbing radio waves well over a wide range in the high frequency band, for example, a radio wave absorber having a radio wave absorbing layer containing magnetic crystals made of ε-Fe2O3-based iron oxide has been proposed (for example, Patent Document 2, Non-Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2009-060060 A [Patent Document 2] JP 2008-277726 A [Non-patent literature]
[0007] [Non-Patent Document 1] A. Namai, S. Sakurai, M. Nakajima, T. Suemoto, K. Matsumoto, M. Goto, S. Sasaki, and S. Ohkoshi, J. Am. Chem. Soc., 131, 1170-1173 (2009). [Non-Patent Document 2] A. Namai, M. Yoshikiyo, K. Yamada, S. Sakurai, T. Goto, T. Yoshida, T Miyazaki, M. Nakajima, T. Suemoto, H. Tokoro, and S. Ohkoshi, Nature Communications, 3, 1035 / 1-6 (2012). [Non-Patent Document 3] S. Ohkoshi, S. Kuroki, S. Sakurai, K. Matsumoto, K. Sato, and S. Sasaki, Angew. Chem. Int. Ed., 46, 8392-8395 (2007). Summary of the Invention [Problem to be solved by the invention]
[0008] However, for the radio wave absorbing sheet described in Patent Document 1, there is a strong demand for a thinner sheet and better radio wave absorbing performance at the same time.
[0009] The present invention has been made in consideration of the above-mentioned problems of the conventional techniques, and has an object to provide a thin wave absorber film having excellent wave absorbing performance, and a method for manufacturing the wave absorber film. [Means for solving the problem]
[0010] The present inventors have found that the above problems can be solved by making the radio wave absorbing layer contain a magnetic material and a binder resin in a radio wave absorber film formed on a base material layer and by using an aromatic ester-urethane copolymer as the binder resin, thereby completing the present invention.
[0011] A first aspect of the present invention is a radio wave absorber comprising a radio wave absorbing layer formed on a base layer, the electromagnetic wave absorbing layer includes a magnetic material and a binder resin; The radio wave absorber film contains a binder resin that includes an aromatic ester-urethane copolymer.
[0012] A second aspect of the present invention includes a radio wave absorbing layer forming step of applying a paste containing a magnetic material and a binder resin onto a base layer to form a coating film, and then drying the coating film to form a radio wave absorbing layer; The method for producing a radio wave absorber film includes a binder resin containing an aromatic ester-urethane copolymer. Effect of the Invention
[0013] According to the present invention, it is possible to provide a thin wave absorber film having excellent wave absorbing performance, and a method for producing the wave absorber film. [Brief description of the drawings]
[0014] [Figure 1] FIG. 3 is a graph showing the return loss of the wave absorber film of Example 1. [Diagram 2] FIG. 11 is a diagram showing the return loss of the wave absorber film of Example 2. [Diagram 3] FIG. 11 is a diagram showing the return loss of the radio wave absorber film of Example 3. [Figure 4] FIG. 11 is a diagram showing the return loss of the radio wave absorber film of Example 4. [Diagram 5] FIG. 10 is a diagram showing the return loss of the wave absorber film of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The following describes in detail the embodiments of the present invention. However, the present invention is not limited to the following embodiments and can be implemented with appropriate modifications within the scope of the object of the present invention. In addition, in this specification, "~" means from above to below unless otherwise specified.
[0016] <Radio wave absorber film> The radio wave absorber film includes a radio wave absorbing layer formed on a base layer. The radio wave absorbing layer includes a magnetic material and a binder resin. The binder resin includes an aromatic ester-urethane copolymer. By incorporating a magnetic material and an aromatic ester-urethane copolymer as a binder resin in the radio wave absorbing layer, a radio wave absorber film having excellent radio wave absorbing properties can be produced even in the form of a thin film.
[0017] From the viewpoint of more reliably absorbing high-frequency radio waves in the millimeter wave band or higher, the wave absorber film preferably has a frequency band of 30 gigahertz (GHz) or higher, preferably 30 GHz to 300 GHz, more preferably 40 GHz to 200 GHz. It is preferable that the reflection loss measured from the surface having the radio wave absorbing layer has a peak with an absolute value of 30 dB or higher. Unless otherwise specified, the value of the transmission attenuation is a value measured under the conditions described in the examples below.
[0018] The shape of the wave absorber film may have a curved surface or may be composed of only flat surfaces, and is preferably a flat plate shape. From the viewpoint of making the film thinner and smaller without impairing the effects of the present invention, the thickness of the radio wave absorber film is preferably 1000 μm or less, more preferably 900 μm or less, even more preferably 450 μm or less, and particularly preferably 200 μm or less. The thickness of the wave absorber film may be uniform or non-uniform.
[0019] <Radio wave absorbing layer> As described above, the electromagnetic wave absorbing layer contains a magnetic material and a binder resin. The binder resin contains an aromatic ester-urethane copolymer.
[0020] The thickness of the radio wave absorbing layer is not particularly limited as long as it does not impair the object of the present invention. From the viewpoint of the balance between the thinning of the radio wave absorber film and the radio wave absorbing performance, the thickness of the radio wave absorbing layer is preferably 100 μm or less, and more preferably 50 μm or less. The lower limit of the thickness of the radio wave absorbing layer is not particularly limited as long as it does not impair the effects of the present invention, and examples thereof include 1 μm or more, 10 μm or more, and the like. The thickness of the electromagnetic wave absorbing layer may be uniform or non-uniform.
[0021] The essential and optional components of the electromagnetic wave absorbing layer will be described below.
[0022] [Binder resin] The radio wave absorbing layer contains a binder resin together with a magnetic material. The binder resin contains an aromatic ester-urethane copolymer. By using an aromatic ester-urethane copolymer as the binder resin, it is possible to produce a radio wave absorber film that exhibits excellent radio wave absorbing properties even if it is thin, while dispersing the magnetic material well in the binder resin.
[0023] Furthermore, when an aromatic ester-urethane copolymer is used as the binder resin, it is possible to impart to the radio wave absorbing layer resistance to cracking when bending or cutting, and low warpage. From the viewpoint of obtaining good crack resistance and low warpage of the radio wave absorbing layer, the glass transition temperature of the binder resin is preferably 100° C. or lower, and more preferably 0° C. or lower. For this reason, the glass transition temperature of the aromatic ester-urethane copolymer is also preferably 100° C. or lower, and more preferably 0° C. or lower.
[0024] The aromatic ester-urethane copolymer is a copolymer containing an ester bond (--CO--O--) and a urethane bond (--NH--CO--O--) and containing an aromatic group in the main chain skeleton. The aromatic group in the main chain skeleton may be an aromatic hydrocarbon group or a heterocyclic aromatic group, and is preferably an aromatic hydrocarbon group. The aromatic ester-urethane copolymer may be a random copolymer in which ester bonds and urethane bonds are randomly introduced into the molecular chain, or may be a block copolymer consisting of one or more ester blocks and one or more urethane blocks.
[0025] The method for producing the aromatic ester-urethane copolymer is not particularly limited. The aromatic ester-urethane copolymer can typically be produced by polymerizing one or more monomers selected from the group consisting of a diol component (a1), a dicarboxylic acid (a2), a hydroxycarboxylic acid component (a3), and a diisocyanate component (a4) in one stage or multiple stages.
[0026] The dicarboxylic acid component (a2) and the hydroxycarboxylic acid component (a3) may be used as ester derivatives such as methyl esters and ethyl esters, carboxylic acid halides such as carboxylic acid chlorides, or urethane-forming derivatives.
[0027] The above-mentioned monomer used in the production of the aromatic ester-urethane copolymer is preferably a compound in which two functional groups selected from the group consisting of a hydroxyl group, a carboxyl group, and an isocyanate group are bonded to a divalent hydrocarbon group having an unbranched structure. The divalent hydrocarbon group having an unbranched structure may be an alkylene group, an alkenylene group, an alkynylene group, an arylene group, or a combination of these groups. The alkylene group, the alkenylene group, and the alkynylene group are preferably linear.
[0028] When the unbranched divalent hydrocarbon group is an alkylene group, an alkenylene group, or an alkynylene group, these groups preferably have 1 to 8 carbon atoms, more preferably 2 to 6 carbon atoms, and even more preferably 2 to 4 carbon atoms.
[0029] When the unbranched divalent hydrocarbon group is an arylene group, the arylene group is preferably a phenylene group or a naphthylene group, more preferably a phenylene group, and even more preferably a p-phenylene group.
[0030] Of the divalent hydrocarbon groups having an unbranched structure described above, alkylene groups, arylene groups, and combinations of alkylene groups and arylene groups are preferred.
[0031] Specific preferred examples of the diol component (a1) include ethylene glycol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, and 1,5-pentanediol. Specific preferred examples of the dicarboxylic acid (a2) include terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, succinic acid, glutaric acid, adipic acid, oxalic acid, and malonic acid. Specific preferred examples of the hydroxycarboxylic acid component (a3) include 4-hydroxybenzoic acid, 3-hydroxybenzoic acid, 6-hydroxynaphthalene-2-carboxylic acid, glycolic acid, lactic acid, and γ-hydroxybutyric acid. Specific examples of suitable diisocyanate components (a4) include ethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, m-xylylene diisocyanate, p-phenylene diisocyanate, tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and 1,5-naphthalene diisocyanate.
[0032] The weight average molecular weight (Mw) of the aromatic ester-urethane copolymer is preferably from 5,000 to 500,000, and more preferably from 10,000 to 200,000. In the specification of the present application, the weight average molecular weight (Mw) is the weight average molecular weight measured by GPC and calculated as polystyrene.
[0033] Commercially available aromatic ester-urethane copolymers include the Vylon series (product name) (manufactured by Toyobo Co., Ltd.). More specifically, Vylon UR-1400, Vylon UR-1410, Vylon UR-1700, Vylon UR-2300, Vylon UR-3200, Vylon UR-3210, Vylon UR-3500, Vylon UR-6100, Vylon UR-8300, and Vylon UR-8700 can be preferably used.
[0034] The binder resin may contain other resins other than the aromatic ester-urethane copolymer as long as the object of the present invention is not hindered. The type of other resin is not particularly limited as long as the object of the present invention is not hindered. The other resin may be an elastic material such as an elastomer or rubber. The other resin may be a thermoplastic resin or a curable resin. When the other resin is a curable resin, the curable resin may be a photocurable resin or a thermosetting resin.
[0035] Suitable examples of the other resin that is a thermoplastic resin include polyacetal resin, polyamide resin, polycarbonate resin, polyester resin (polybutylene terephthalate, polyethylene terephthalate, polyarylate, etc.), FR-AS resin, FR-ABS resin, AS resin, ABS resin, polyphenylene oxide resin, polyphenylene sulfide resin, polysulfone resin, polyethersulfone resin, polyetheretherketone resin, fluorine-based resin, polyimide resin, polyamideimide resin, polyamide bismaleimide resin, polyetherimide resin, polybenzoxazole resin, polybenzothiazole resin, polybenzimidazole resin, BT resin, polymethylpentene, ultra-high molecular weight polyethylene, FR-polypropylene, cellulose resin (e.g., methyl cellulose, ethyl cellulose), (meth)acrylic resin (polymethyl methacrylate, etc.), and polystyrene.
[0036] Suitable examples of the other resin that is a thermosetting resin include phenol resin, melamine resin, epoxy resin, alkyd resin, etc. As the photocurable resin, a resin obtained by photocuring a monomer having an unsaturated bond, such as various vinyl monomers or various (meth)acrylic acid esters, can be used.
[0037] When the other resin is an elastic material, suitable examples include olefin-based elastomers, styrene-based elastomers, polyamide-based elastomers, polyester-based elastomers, and polyurethane-based elastomers.
[0038] The ratio of the mass of the other resin to the total mass of the binder resin is not particularly limited as long as it does not impair the object of the present invention. The ratio of the mass of the other resin to the total mass of the binder resin is, for example, preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, even more preferably 1% by mass or less, and most preferably 0% by mass, because it is easy to obtain a radio wave absorber film with desired performance.
[0039] The content of the binder resin in the radio wave absorbing layer is not particularly limited as long as it does not impair the object of the present invention. The content of the binder resin is preferably from 5% by mass to 30% by mass, more preferably from 10% by mass to 25% by mass, based on the solid content mass of the radio wave absorbing layer.
[0040] [Magnetic material] The type of magnetic material is not particularly limited as long as the radio wave absorber film exhibits the desired radio wave absorbing characteristics. From the viewpoint of being able to absorb high-frequency radio waves in the millimeter wave band or higher, the magnetic material is preferably a magnetic material that magnetically resonates in a frequency band of 30 GHz or higher, and more preferably a magnetic material that magnetically resonates in a frequency band of 30 GHz or higher and 300 GHz or lower.
[0041] The magnetic resonance may be based on the precession motion of electrons in atoms undergoing spin motion in a frequency band equal to or higher than the millimeter wave band. Natural magnetic resonance due to the gyromagnetic effect based on the precession motion in a frequency band equal to or higher than the millimeter wave band is preferred.
[0042] The magnetic material is not particularly limited as long as it can absorb high-frequency radio waves in the millimeter wave band or higher. Preferred magnetic materials include magnetic materials containing at least one selected from the group consisting of epsilon-type iron oxide, barium ferrite magnetic material, and strontium ferrite magnetic material. The epsilon type iron oxide will be described below.
[0043] (epsilon iron oxide) Epsilon-type iron oxide includes ε-Fe2O3 crystals and ε-Fe2O3 crystals with the same crystal structure and space group as ε-Fe2O3, but with part of the Fe site of the ε-Fe2O3 crystal substituted with an element M other than Fe, and has the formula ε-M x Fe 2-x O3, where x is 0 or more and 2 or less (preferably 0 or more and less than 2). Since such epsilon-type iron oxide crystals are magnetic crystals, the crystals may be referred to as "magnetic crystals" in the present specification.
[0044] Any ε-Fe2O3 crystal can be used. It has the same crystal structure and space group as ε-Fe2O3, and some of the Fe sites of the ε-Fe2O3 crystal are replaced with an element M other than Fe, and has the formula ε-M x Fe 2-x The crystal represented by O3, in which x is 0 or more and 2 or less (preferably 0 or more and less than 2), will be described later. In this specification, ε-Fe2O3 crystals in which part of the Fe site is replaced with a substitution element M are referred to as ε-M x Fe 2-x O3 is also called "M-substituted ε-Fe2O3".
[0045] The particle size of the particles having ε-Fe2O3 crystals and / or M-substituted ε-Fe2O3 crystals in the magnetic phase is not particularly limited as long as it does not impair the object of the present invention. For example, the particles having magnetic crystals of epsilon-type iron oxide in the magnetic phase, which are produced by the method described below, have an average particle size measured from a TEM (transmission electron microscope) photograph in the range of 5 nm to 200 nm. In addition, the coefficient of variation (standard deviation of particle size / average particle size) of particles having epsilon-type iron oxide magnetic crystals in their magnetic layer, which are manufactured by the method described below, is in the range of less than 80%, and the particles are relatively fine and have a uniform particle size.
[0046] In a suitable electromagnetic wave absorbing layer, a powder of such epsilon-type iron oxide magnetic particles (i.e., particles having ε-Fe2O3 crystals and / or M-substituted ε-Fe2O3 crystals in the magnetic phase) is used as a magnetic substance, which is an electromagnetic wave absorbing material in the electromagnetic wave absorbing layer. The "magnetic phase" here is the part that is responsible for the magnetism of the powder. "Having ε-Fe2O3 crystals and / or M-substituted ε-Fe2O3 crystals in the magnetic phase" means that the magnetic phase is composed of ε-Fe2O3 crystals and / or M-substituted ε-Fe2O3 crystals, and includes cases where the magnetic phase contains impurity magnetic crystals that are unavoidable during production.
[0047] The magnetic crystals of epsilon-type iron oxide may contain impurity crystals of iron oxides having a different space group or oxidation state from the ε-Fe2O3 crystals (specifically, α-Fe2O3, γ-Fe2O3, FeO, and Fe3O4, as well as crystals in which part of the Fe in these crystals has been replaced with other elements). When the magnetic crystals of epsilon-type iron oxide contain impurity crystals, it is preferable that the magnetic crystals of ε-Fe2O3 and / or M-substituted ε-Fe2O3 are the main phase. In other words, it is preferable that the ratio of the magnetic crystals of ε-Fe2O3 and / or M-substituted ε-Fe2O3 in the magnetic crystals of epsilon-type iron oxide constituting the radio wave absorbing material is 50 mol % or more in terms of molar ratio as a compound.
[0048] The abundance ratio of crystals can be determined by analysis using the Rietveld method based on the X-ray diffraction pattern. Non-magnetic compounds such as silica (SiO2) formed during the sol-gel process may be attached to the periphery of the magnetic phase.
[0049] (M-substituted ε-Fe2O3) The type of element M in M-substituted ε-Fe2O3 is not particularly limited as long as it satisfies the conditions that the crystal and space group are the same as those of ε-Fe2O3 and a part of the Fe site of the ε-Fe2O3 crystal is substituted with an element M other than Fe. The M-substituted ε-Fe2O3 may contain multiple types of elements M other than Fe.
[0050] Suitable examples of the element M include In, Ga, Al, Sc, Cr, Sm, Yb, Ce, Ru, Rh, Ti, Co, Ni, Mn, Zn, Zr, and Y. Among these, In, Ga, Al, Ti, Co, and Rh are preferred. When M is Al, ε-M x Fe 2-xIn the composition represented by O3, x is preferably, for example, in the range of 0 or more and less than 0.8. When M is Ga, x is preferably, for example, in the range of 0 or more and less than 0.8. When M is In, x is preferably, for example, in the range of 0 or more and less than 0.3. When M is Rh, x is preferably, for example, in the range of 0 or more and less than 0.3. When M is Ti and Co, x is preferably, for example, in the range of 0 or more and less than 1.
[0051] The frequency at which the amount of electromagnetic wave absorption is maximum can be adjusted by adjusting at least one of the type and the amount of substitution of element M in M-substituted ε-Fe2O3.
[0052] Such M-substituted ε-Fe2O3 magnetic crystals can be synthesized, for example, by a process combining a reverse micelle method and a sol-gel method, and a firing process, as described below. Also, as disclosed in JP 2008-174405 A, M-substituted ε-Fe2O3 magnetic crystals can be synthesized by a process combining a direct synthesis method and a sol-gel method, and a firing process.
[0053] in particular, Jian Jin, Shin-ichi Ohkoshi and Kazuhito Hashimoto, ADVANCED MATERIALS 2004,16,No.1, January 5,p.48-51, Shin-ichi Ohkoshi, Shunsuke Sakurai, Jian Jin, Kazuhito Hashimoto, JOURNAL OF APPLIED PHYSICS, 97, 10K312 (2005), Shunsuke Sakurai, Jian Jin, Kazuhito Hashimoto and Shin-ichi Ohkoshi, JOURNAL OF THE PHYSICAL SOCIETY OF JAPAN, Vol.74, No.7, July, 2005, p.1946-1949, As described in, for example, Asuka Namai, Shunsuke Sakurai, Makoto Nakajima, Tohru Suemoto, Kazuyuki Matsumoto, Masahiro Goto, Shinya Sasaki, and Shin-ichi Ohkoshi, Journal of the American Chemical Society, Vol. 131, p. 1170-1173, 2009, M-substituted ε-Fe2O3 magnetic crystals can be obtained by a process combining the reverse micelle method and the sol-gel method and a firing process.
[0054] In the reverse micelle method, two types of micellar solutions containing surfactants, namely micellar solution I (raw micelle) and micelle solution II (neutralizer micelle), are mixed together to allow the precipitation reaction of iron hydroxide to proceed within the micelles. Next, a silica coating is applied to the surface of the iron hydroxide fine particles generated within the micelles by the sol-gel method. The iron hydroxide fine particles with the silica coating layer are separated from the liquid and then subjected to heat treatment in air at a specified temperature (within the range of 700 to 1300°C). This heat treatment results in fine particles of ε-Fe2O3 crystals.
[0055] More specifically, for example, M-substituted ε-Fe2O3 magnetic crystals are produced as follows.
[0056] First, iron (III) nitrate as an iron source, M nitrate as an M element source to substitute for part of the iron (aluminum (III) nitrate nonahydrate in the case of Al, gallium (III) nitrate hydrate in the case of Ga, indium (III) nitrate trihydrate in the case of In, titanium (IV) sulfate hydrate and cobalt (II) nitrate hexahydrate in the cases of Ti and Co) and a surfactant (e.g., cetyltrimethylammonium bromide) are dissolved in the aqueous phase of micellar solution I, which has n-octane as the oil phase.
[0057] An appropriate amount of nitrate of an alkaline earth metal (Ba, Sr, Ca, etc.) can be dissolved in the aqueous phase of micellar solution I. This nitrate acts as a shape control agent. When an alkaline earth metal is present in the solution, rod-shaped particles of M-substituted ε-Fe2O3 magnetic crystals are ultimately obtained. In the absence of a shape control agent, particles of M-substituted ε-Fe2O3 magnetic crystals that are nearly spherical are obtained.
[0058] The alkaline earth metal added as a shape control agent may remain in the surface layer of the resulting M-substituted ε-Fe2O3 magnetic crystal. The mass of the alkaline earth metal in the M-substituted ε-Fe2O3 magnetic crystal is preferably 20 mass% or less, more preferably 10 mass% or less, based on the total mass of the substitution element M and the mass of Fe in the M-substituted ε-Fe2O3 magnetic crystal.
[0059] Aqueous ammonia solution is used as the aqueous phase of micellar solution II in which n-octane is the oil phase.
[0060] After mixing micellar solutions I and II, the sol-gel method is applied. That is, silane (e.g., tetraethylorthosilane) is added dropwise to the mixture of micellar solutions while stirring is continued, and the reaction of producing iron hydroxide or iron hydroxide containing element M in the micelles proceeds. As a result, the particle surfaces of the fine iron hydroxide precipitate produced in the micelles are coated with silica produced by hydrolysis of the silane.
[0061] Next, the silica-coated M element-containing iron hydroxide particles are separated from the liquid, washed and dried to obtain a particle powder, which is then charged into a furnace and heat-treated (fired) in air at a temperature range of 700°C or higher and 1300°C or lower, preferably 900°C or higher and 1200°C or lower, and more preferably 950°C or higher and 1150°C or lower. This heat treatment causes an oxidation reaction to proceed within the silica coating, and the fine particles of M element-containing iron hydroxide are transformed into fine particles of M-substituted ε-Fe2O3.
[0062] During this oxidation reaction, the presence of the silica coat contributes to the formation of M-substituted ε-Fe2O3 crystals, which have the same space group as ε-Fe2O3, rather than α-Fe2O3 or γ-Fe2O3 crystals, and also acts to prevent sintering of particles. In addition, when an appropriate amount of alkaline earth metal is present, the particles tend to grow into rod-like shapes.
[0063] In addition, as described above, as disclosed in JP 2008-174405 A, the M-substituted ε-Fe2O3 magnetic crystals can be synthesized more economically and advantageously by a process that combines a direct synthesis method and a sol-gel method, and a firing process.
[0064] To put it simply, a precursor consisting of iron hydroxide (which may be partially substituted with another element) is formed by first adding a neutralizing agent such as aqueous ammonia to an aqueous solvent in which a trivalent iron salt and a salt of the substituting element M (Ga, Al, etc.) are dissolved, while stirring.
[0065] The sol-gel method is then applied to form a silica coating layer on the surface of the precursor particles. After separating the silica-coated particles from the liquid, they are heat-treated (calcined) at a specified temperature to obtain fine particles of M-substituted ε-Fe2O3 magnetic crystals.
[0066] In the synthesis of M-substituted ε-Fe2O3 as described above, iron oxide crystals (impurity crystals) with different space groups and oxidation states from ε-Fe2O3 crystals may be generated. The most common polymorphisms with different crystal structures that have the composition of Fe2O3 are α-Fe2O3 and γ-Fe2O3. Other iron oxides include FeO and Fe3O4. The inclusion of such impurity crystals is not desirable in terms of bringing out the properties of the M-substituted ε-Fe2O3 crystal as highly as possible, but is permissible within a range that does not impair the effects of the present invention.
[0067] In addition, the coercive force H of M-substituted ε-Fe2O3 magnetic crystals cchanges depending on the amount of substitution by the substitution element M. In other words, by adjusting the amount of substitution by the substitution element M in the M-substituted ε-Fe2O3 magnetic crystal, the coercive force H c can be adjusted. Specifically, when Al, Ga, or the like is used as the substitution element M, the coercive force H of the M-substituted ε-Fe2O3 magnetic crystal increases as the substitution amount increases. c On the other hand, when Rh or other elements are used as the substitution element M, the coercive force H of the M-substituted ε-Fe2O3 magnetic crystal increases as the substitution amount increases. c increases. The coercive force H of M-substituted ε-Fe2O3 magnetic crystals depends on the amount of substitution by the element M. c From the viewpoint of ease of adjustment, the substitution element M is preferably Ga, Al, In, Ti, Co or Rh.
[0068] And this coercive force H c As the M-element substitution amount decreases, the frequency of the peak at which the electromagnetic wave absorption of epsilon-type iron oxide is maximum also shifts to the lower or higher frequency side. In other words, the frequency of the peak electromagnetic wave absorption can be controlled by the amount of M element substitution.
[0069] In the case of commonly used radio wave absorbers, if the incident angle or frequency of the radio wave deviates from the designed values, the amount of absorption becomes almost zero. In contrast, when epsilon-type iron oxide is used, radio wave absorption is exhibited over a wide frequency range and radio wave incident angle even if the values deviate slightly. Therefore, it is possible to provide a radio wave absorbing layer that can absorb radio waves in a wide frequency band.
[0070] The particle size of the epsilon-type iron oxide can be controlled, for example, by adjusting the heat treatment (calcination) temperature in the above process. According to the above-mentioned method of combining the reverse micelle method and the sol-gel method, or the method of combining the direct synthesis method and the sol-gel method disclosed in JP 2008-174405 A, it is possible to synthesize particles of epsilon-type iron oxide having an average particle diameter of 5 nm to 200 nm as measured from a TEM (transmission electron microscope) photograph. The average particle diameter of epsilon-type iron oxide is preferably 10 nm or more, more preferably 20 nm or more. In addition, when determining the average particle diameter, which is the number average particle diameter, if the epsilon iron oxide particles are rod-shaped, the diameter in the major axis direction of the particle observed in the TEM image is used as the diameter of the particle to calculate the average particle diameter. The number of particles to be measured when determining the average particle diameter is not particularly limited as long as it is a number that is sufficiently large for calculating the average value, but it is preferably 300 or more.
[0071] In addition, the silica coating applied to the surface of iron hydroxide fine particles by the sol-gel method may be present on the surface of the M-substituted ε-Fe2O3 magnetic crystals after heat treatment (calcination). The presence of a non-magnetic compound such as silica on the surface of the crystals is preferable in terms of improving the handleability, durability, weather resistance, etc. of the magnetic crystals. Suitable examples of the non-magnetic compound include silica, as well as heat-resistant compounds such as alumina and zirconia.
[0072] However, if the amount of the non-magnetic compound attached is too large, the particles may severely aggregate with each other, which is undesirable. When the non-magnetic compound is silica, the mass of Si in the M-substituted ε-Fe2O3 magnetic crystals is preferably 100 mass % or less relative to the total mass of the substituting element M and the mass of Fe in the M-substituted ε-Fe2O3 magnetic crystals. A part or most of the silica attached to the M-substituted ε-Fe2O3 magnetic crystals can be removed by immersing them in an alkaline solution. The amount of silica attached can be adjusted to any amount by this method.
[0073] The content of the magnetic material in the radio wave absorbing layer is not particularly limited as long as it does not impair the object of the present invention. The content of the magnetic material is preferably 30% by mass or more, more preferably 40% by mass or more, particularly preferably 60% by mass or more, and most preferably 60% by mass or more and 91% by mass or less, based on the solid content mass of the radio wave absorbing layer.
[0074] (Method of adjusting dielectric constant) The relative dielectric constant of the radio wave absorbing layer is not particularly limited, but is preferably 6.5 or more and 65 or less, more preferably 10 or more and 50 or less, and even more preferably 15 or more and 30 or less. The method for adjusting the relative dielectric constant of the radio wave absorbing layer is not particularly limited. As a method for adjusting the relative dielectric constant of each radio wave absorbing layer, a method of incorporating a dielectric powder in the radio wave absorbing layer and adjusting the content of the dielectric powder can be mentioned.
[0075] Suitable examples of the dielectric material include barium titanate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, zirconium titanate, zinc titanate, and titanium dioxide. The radio wave absorbing layer may contain a combination of powders of multiple types of dielectric materials.
[0076] The particle size of the dielectric powder used to adjust the relative dielectric constant of the electromagnetic wave absorbing layer is not particularly limited as long as it does not impair the object of the present invention. The average particle size of the dielectric powder is preferably 1 nm or more and 100 nm or less, more preferably 5 nm or more and 50 nm or less. Here, the average particle size of the dielectric powder is the number average size of the primary particles of the dielectric powder observed by an electron microscope.
[0077] When adjusting the relative dielectric constant of the electromagnetic wave absorbing layer using a dielectric powder, the amount of the dielectric powder used is not particularly limited as long as the relative dielectric constant of the electromagnetic wave absorbing layer is within a predetermined range. The amount of the dielectric powder used is preferably 0% by mass or more and 20% by mass or less, more preferably 5% by mass or more and 10% by mass or less, based on the solid content mass of each electromagnetic wave absorbing layer.
[0078] The dielectric constant can be adjusted by incorporating carbon nanotubes in the radio wave absorbing layer, which may be used in combination with the above-mentioned dielectric powder.
[0079] The amount of carbon nanotubes blended into the electromagnetic wave absorbing layer is not particularly limited as long as the relative dielectric constant of the electromagnetic wave absorbing layer is within the above-mentioned range. However, since carbon nanotubes are also a conductive material, if the amount of carbon nanotubes used is excessive, the electromagnetic wave absorbing properties provided by the electromagnetic wave absorbing layer may be impaired. The amount of carbon nanotubes used is preferably from 0% by mass to 20% by mass, and more preferably from 1% by mass to 10% by mass, based on the mass of the solid content of the radio wave absorbing layer.
[0080] (Relative permeability adjustment method) The relative magnetic permeability of the electromagnetic wave absorbing layer is not particularly limited, but is preferably 1.0 or more and 1.5 or less. The method for adjusting the relative magnetic permeability of the electromagnetic wave absorbing layer is not particularly limited. As described above, examples of the method for adjusting the relative magnetic permeability of each electromagnetic wave absorbing layer include a method for adjusting the amount of substitution by the substitution element M in the epsilon-type iron oxide and a method for adjusting the content of the magnetic material in the electromagnetic wave absorbing layer.
[0081] (Dispersant) The radio wave absorbing layer may contain a dispersant for the purpose of dispersing well the magnetic material and the substance added to adjust the relative dielectric constant and relative magnetic permeability in the radio wave absorbing layer. The dispersant may be mixed uniformly with the magnetic material, polymer, etc. The dispersant may be blended in the binder resin. In addition, the magnetic material and the substance added to adjust the relative dielectric constant and relative magnetic permeability, which have been previously treated with a dispersant, may be blended in the material constituting the radio wave absorbing layer.
[0082] The type of dispersant is not particularly limited as long as it does not impair the object of the present invention. The dispersant can be selected from various dispersants that have been used in the past for dispersing various inorganic and organic fine particles.
[0083] Suitable examples of the dispersant include a silane coupling agent (eg, phenyltrimethoxysilane), a titanate coupling agent, a zirconate coupling agent, and an aluminate coupling agent.
[0084] The content of the dispersant is not particularly limited as long as it does not impair the object of the present invention. The content of the dispersant is preferably from 0.1% by mass to 30% by mass, more preferably from 1% by mass to 15% by mass, and particularly preferably from 1% by mass to 10% by mass, based on the solid content mass of the radio wave absorbing layer.
[0085] [Other ingredients] The radio wave absorbing layer may contain various additives other than the above components, so long as the object of the present invention is not impaired. Examples of additives that the radio wave absorbing layer may contain include colorants, antioxidants, ultraviolet absorbers, flame retardants, flame retardant assistants, plasticizers, and surfactants. These additives are used in the range that does not impair the object of the present invention, taking into consideration the amounts in which they are conventionally used.
[0086] <Paste for forming electromagnetic wave absorbing layer> As a method for forming the radio wave absorbing layer, a method using a paste for forming the radio wave absorbing layer is preferred, since the radio wave absorbing layer can be formed with high efficiency without any particular thickness restriction and the radio wave absorbing layer can be formed directly on the base layer. The electromagnetic wave absorbing layer forming paste preferably contains the binder resin and the magnetic material. The electromagnetic wave absorbing layer forming paste may contain the substances added for adjusting the relative dielectric constant, relative magnetic permeability, etc., as described above for the electromagnetic wave absorbing layer, and other components. When the binder resin contains a curable resin, the electromagnetic wave absorbing layer forming paste contains a compound that is a precursor of the curable resin. In this case, the electromagnetic wave absorbing layer forming paste contains a curing agent, a curing accelerator, a polymerization initiator, etc., as necessary.
[0087] Furthermore, when the paste for forming an electromagnetic wave absorbing layer contains a photopolymerizable or thermally polymerizable compound, the coating film may be exposed to light or heated as necessary to form an electromagnetic wave absorbing layer.
[0088] The paste for forming the electromagnetic wave absorbing layer preferably further contains a dispersion medium. As the dispersion medium, water, an organic solvent, and an aqueous solution of an organic solvent can be used. As the dispersion medium, an organic solvent is preferable because it is easy to dissolve organic components, has a low latent heat of vaporization, and is easy to remove by drying.
[0089] Suitable examples of organic solvents used as dispersion media include nitrogen-containing polar solvents such as N,N,N',N'-tetramethylurea (TMU), N-methyl-2-pyrrolidone (NMP), N,N-dimethylacetamide (DMAc), N,N-dimethylisobutylamide, N,N-diethylacetamide, N,N-dimethylformamide (DMF), N,N-diethylformamide, N-methylcaprolactam, 1,3-dimethyl-2-imidazolidinone (DMI), and pyridine; ketones such as diethyl ketone, methyl butyl ketone, dipropyl ketone, and cyclohexanone; alcohols such as n-pentanol, 4-methyl-2-pentanol, cyclohexanol, and diacetone alcohol; ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monoethyl ether. Ether alcohols such as ethylene glycol dimethyl ether and diethylene glycol diethyl ether; saturated aliphatic monocarboxylic acid alkyl esters such as n-butyl acetate and amyl acetate; lactate esters such as ethyl lactate and n-butyl lactate; ketones such as acetone, methyl ethyl ketone, cyclohexanone, acetophenone, and benzophenone; methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol monomethyl ether acetate, and propylene glycol Examples of the ether esters include monoethyl ether acetate, ethyl 3-ethoxypropionate, 2-methoxybutyl acetate, 3-methoxybutyl acetate, 4-methoxybutyl acetate, 2-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-ethyl-3-methoxybutyl acetate, 2-ethoxybutyl acetate, 4-ethoxybutyl acetate, 4-propoxybutyl acetate, and 2-methoxypentyl acetate. These can be used alone or in combination of two or more.
[0090] The solid content concentration of the electromagnetic wave absorbing layer forming paste is appropriately adjusted depending on the method of applying the electromagnetic wave absorbing layer forming paste, the thickness of the electromagnetic wave absorbing layer, etc. Typically, the solid content concentration of the electromagnetic wave absorbing layer forming paste is preferably 3% by mass or more and 60% by mass or less, and more preferably 10% by mass or more and 50% by mass or less. The solid content concentration of the paste is a value calculated by taking the total mass of the solid content as the mass of the components not dissolved in the dispersion medium and the mass of the components dissolved in the dispersion medium.
[0091] <Base material layer> The radio wave absorbing layer is laminated on a substrate layer. The substrate layer may be a layer containing any substrate as long as it does not impair the effects of the present invention, and examples of the substrate layer include a layer containing a resin. Examples of the resin include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), acrylic (PMMA), polycarbonate (PC), cycloolefin polymer (COP), polyethersulfone, polyimide, polyamideimide, etc. Among these, PET is preferred because of its excellent heat resistance and good balance between dimensional stability and cost.
[0092] The shape of the substrate layer may have a curved surface or may be composed of only flat surfaces, and is preferably a flat plate shape. From the viewpoint of making the film thinner and smaller without impairing the effects of the present invention, the thickness of the base layer is preferably 800 μm or less, more preferably 500 μm or less, even more preferably 300 μm or less, and particularly preferably 150 μm or less. The lower limit of the thickness of the base layer is not particularly limited as long as it does not impair the effects of the present invention, and examples thereof include 1 μm or more, 10 μm or more, and 50 μm or more.
[0093] <Metal layer> A metal layer may be provided on the surface of the base material layer opposite to the surface on which the radio wave absorbing layer is provided. When a metal layer is provided, radio waves reflected by the metal layer can be attenuated. Metals constituting the metal layer are preferably, for example, aluminum, titanium, SUS, copper, brass, silver, gold, platinum, and the like. The thickness of the metal layer is not particularly limited, and from the viewpoint of making the radio wave absorber film thin, it is preferably 600 μm or less, more preferably 400 μm or less, further preferably 100 μm or less, and particularly preferably 50 μm or less. The lower limit of the thickness of the metal layer is not particularly limited as long as it does not impair the effects of the present invention, and examples thereof include 0.1 μm or more, 1 μm or more, 5 μm or more, and 10 μm or more.
[0094] <Application> The above-mentioned radio wave absorber film can be preferably used as a radio wave absorbing film for use in various elements (including in-vehicle elements, high-frequency antenna elements, etc.) in various information and communication systems such as mobile phones, wireless LANs, ETC systems, intelligent road traffic systems, automobile driving assistance road systems, and satellite broadcasting.
[0095] <Production method of radio wave absorber film> The method for producing the above-mentioned radio wave absorber film is not particularly limited as long as it is possible to produce a radio wave absorber film having a predetermined structure. A preferred method includes a method including a radio wave absorbing layer forming step of applying a paste containing a magnetic material and a binder resin onto a base layer to form a coating film, and then drying the coating film to form a radio wave absorbing layer. As described above, the binder resin includes an aromatic ester-urethane copolymer.
[0096] As the paste used in the electromagnetic wave absorbing layer forming step, the above-mentioned electromagnetic wave absorbing layer forming paste can be used.
[0097] The method of applying the paste for forming an electromagnetic wave absorbing layer onto the base layer is not particularly limited as long as it is possible to form an electromagnetic wave absorbing layer of a desired thickness. Examples of the application method include spray coating, dip coating, roll coating, curtain coating, spin coating, screen printing, doctor blade, and applicator methods. The coating film formed by the above method is dried to remove the dispersion medium, thereby forming an electromagnetic wave absorbing layer. The thickness of the coating film is appropriately adjusted so that the thickness of the electromagnetic wave absorbing layer obtained after drying is a desired thickness. The drying method is not particularly limited, and examples include (1) drying on a hot plate at a temperature of 80° C. to 180° C., preferably 90° C. to 160° C., for 1 minute to 30 minutes, (2) leaving it at room temperature for several hours to several days, and (3) placing it in a hot air heater or infrared heater for several tens of minutes to several hours to remove the solvent.
[0098] The manufacturing method of the radio wave absorber film may include a cutting step of cutting the laminate including the base layer and the radio wave absorbing layer obtained in the radio wave absorbing layer forming step to obtain a radio wave absorber film of a predetermined size. As described above, the radio wave absorbing layer of the present invention contains an aromatic ester-urethane copolymer as a binder resin, and therefore has good crack resistance. Therefore, even if the radio wave absorber film is cut, cracks are unlikely to occur in the radio wave absorbing layer at the cut surface. EXAMPLES
[0099] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0100] Example 1 (Preparation of paste for forming radio wave absorbing layer) To 35 parts by mass of TMU, 40 parts by mass of the epsilon type iron oxide described below, 2 parts by mass of the carbon nanotubes (CNTs) described below, 3 parts by mass of the dispersant described below, and 20 parts by mass of the binder resin solution described below were added. The mixture was stirred with a rotation / revolution mixer to uniformly dissolve or disperse each component, thereby obtaining a paste for forming an electromagnetic wave absorbing layer.
[0101] Epsilon-type iron oxide: ε-Ga 0.45 Fe 1.55 The average particle size of epsilon-type iron oxide was 20 nm or more and 30 nm or less. As the CNTs, multi-walled carbon nanotubes (product name VGCF-H; manufactured by Showa Denko KK) with a major axis of 150 nm were used. As the dispersant, phenyltrimethoxysilane was used. As the binder resin solution, an aromatic ester-urethane copolymer (manufactured by Toyobo Co., Ltd., Vylon UR-3210, glass transition temperature -3°C, weight average molecular weight 40000, composed of 5 parts by mass of resin and 15 parts by mass of methyl ethyl ketone) was used.
[0102] (Manufacture of radio wave absorber film) The above-mentioned paste for forming an electromagnetic wave absorbing layer was applied to a PET film (thickness 125 μm) using an applicator. The applied film was then dried under conditions of 90° C. for 10 minutes and 130° C. for 10 minutes to form an electromagnetic wave absorbing layer having a thickness of 35 μm, and an electromagnetic wave absorber film was obtained. Immediately after drying, the obtained electromagnetic wave absorber film was cut into a square shape of 5 cm on each side to prepare test pieces for the following evaluations.
[0103] <Return loss> A 5 cm square sample of the radio wave absorber film was attached to an aluminum plate. Radio waves of 50 to 100 GHz were incident on the measurement sample on the aluminum plate, and the return loss was measured using a terahertz spectrometer (manufactured by Advantest Corporation). The return loss RL(f) at frequency f is calculated as RL(f) = -10Log(R(f) / 100), where R(f) is the reflectance (%). FIG. 1 shows the reflection loss (dB) of the wave absorber film of Example 1 in the frequency range of 50 to 100 GHz.
[0104] <Crack resistance (bending)> The obtained sample of the radio wave absorber film was folded 180°, and then the presence or absence of cracks on both sides of the film near the fold was confirmed. The case where no cracks were generated was judged as ◯, and the case where cracks were generated was judged as ×.
[0105] <Crack resistance (cutting)> A plurality of samples of the obtained wave absorber film were cut using a cutter, and then the presence or absence of cracks occurring near the cut surface was confirmed. A case where no cracks occurred in any of the samples was judged as ◯, a case where cracks occurred in some of the samples was judged as △, and a case where cracks occurred in all of the samples was judged as ×.
[0106] <Warpage> The obtained sample of the radio wave absorber film immediately after drying was placed on a flat table, and the angle between the radio wave absorber film and the flat surface of the table was measured to evaluate the warpage. When the angle was less than 15°, it was judged as ◯, and when the angle was 15° or more, it was judged as ×.
[0107] Example 2 Except for changing the binder resin to an aromatic ester-urethane copolymer (Vylon UR-8300, manufactured by Toyobo Co., Ltd., glass transition temperature 23° C., weight average molecular weight 30,000, consisting of 5 parts by mass of resin and 15 parts by mass of methyl ethyl ketone), a radio wave absorber film was produced and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1. Moreover, the return loss of the radio wave absorber film of Example 2 in the range of 50 to 100 GHz is shown in FIG. 2.
[0108] Example 3 Except for changing the binder resin to an aromatic ester-urethane copolymer (Vylon UR-1400, manufactured by Toyobo Co., Ltd., glass transition temperature 83° C., weight average molecular weight 40,000, consisting of 5 parts by mass of resin and 15 parts by mass of methyl ethyl ketone), a radio wave absorber film was produced and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1. Moreover, the return loss of the radio wave absorber film of Example 3 in the range of 50 to 100 GHz is shown in FIG. 3.
[0109] Example 4 Except for changing the binder resin to an aromatic ester-urethane copolymer (Vylon UR-8700, manufactured by Toyobo Co., Ltd., glass transition temperature -22°C, weight average molecular weight 32000, consisting of 5 parts by mass of resin and 15 parts by mass of methyl ethyl ketone), a radio wave absorber film was produced and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1. Moreover, the return loss of the radio wave absorber film of Example 4 in the range of 50 to 100 GHz is shown in FIG. 4.
[0110] Comparative Example 1 (Preparation of paste for forming radio wave absorbing layer) To 50.9 parts by mass of TMU, 35.1 parts by mass of the above epsilon type iron oxide, 2.2 parts by mass of the above carbon nanotubes (CNTs), 3.5 parts by mass of the below-mentioned dispersant, and 8.3 parts by mass of the below-mentioned binder resin were added. The mixture was stirred with a rotation / revolution mixer to uniformly dissolve or disperse each component, thereby obtaining a paste for forming an electromagnetic wave absorbing layer.
[0111] As the binder resin solution, ethyl cellulose (manufactured by Nisshin Seiki Co., Ltd.) was used.
[0112] (Manufacture of radio wave absorber film) The above-mentioned paste for forming an electromagnetic wave absorbing layer was applied to a PET film (thickness 125 μm) using an applicator. Thereafter, the applied film was dried under conditions of 90° C. for 10 minutes and 130° C. for 10 minutes to form an electromagnetic wave absorbing layer having a thickness of 35 μm, thereby obtaining a electromagnetic wave absorber film. The electromagnetic wave absorber film obtained immediately after drying was cut into a square shape of 5 cm on each side to prepare a test piece for evaluation. The evaluation results are shown in Table 1. Moreover, the return loss of the electromagnetic wave absorber film of Comparative Example 1 in the range of 50 to 100 GHz is shown in FIG. 5.
[0113] [Table 1]
[0114] According to Table 1, it can be seen that the radio wave absorber film of the embodiment, which has a radio wave absorbing layer formed using an aromatic ester-urethane copolymer as a binder resin, has a large amount of radio wave absorption in the frequency range of 50 to 100 GHz, despite the thin radio wave absorbing layer. On the other hand, the comparative wave absorber film having a wave absorbing layer formed using ethyl cellulose as a binder resin has a thicker wave absorbing layer than the examples, but has an inferior wave absorption amount in the frequency range of 50 to 100 GHz to the wave absorber film of the examples.
[0115] Moreover, in the wave absorber films of the Examples in which the aromatic ester-urethane copolymer was used as the binder resin, cracks were unlikely to occur when cut. In particular, in the wave absorber films of Examples 1 and 4 in which the aromatic ester-urethane copolymer exhibiting a Tg of 0°C or lower was used as the binder resin, cracks were unlikely to occur even when folded 180°. On the other hand, in the comparative wave absorber film having a wave absorbing layer formed using ethyl cellulose as a binder resin, cracks were generated both when bending and when cutting.
Claims
1. A radio wave absorber film comprising a radio wave absorbing layer formed on a base layer, the electromagnetic wave absorbing layer includes a magnetic material, a binder resin, and a dispersant; the dispersant is at least one selected from the group consisting of a silane coupling agent, a titanate coupling agent, a zirconate coupling agent, and an aluminate coupling agent; the binder resin comprises an aromatic ester-urethane copolymer, The radio wave absorber film, wherein the magnetic material includes at least one selected from the group consisting of epsilon type iron oxide, barium ferrite magnetic material, and strontium ferrite magnetic material.
2. A radio wave absorber film comprising a radio wave absorbing layer formed on a base layer, the electromagnetic wave absorbing layer includes a magnetic material and a binder resin; the binder resin comprises an aromatic ester-urethane copolymer, the magnetic material includes at least one selected from the group consisting of epsilon-type iron oxide, barium ferrite magnetic material, and strontium ferrite magnetic material; The radio wave absorber film, wherein the radio wave absorbing layer has a thickness of 50 μm or less.
3. 3. The radio wave absorber film according to claim 1, wherein the binder resin has a glass transition temperature of 100° C. or lower.
4. 4. The radio wave absorber film according to claim 3, wherein the binder resin has a glass transition temperature of 0° C. or lower.
5. The radio wave absorber film according to any one of claims 1 to 4, wherein the radio wave absorbing layer contains carbon nanotubes.
6. The radio wave absorber film according to any one of claims 1 to 5, having a thickness of 200 µm or less.
7. 2. The radio wave absorber film according to claim 1, wherein the radio wave absorbing layer has a thickness of 50 μm or less.
8. The method includes a radio wave absorbing layer forming step of applying a paste containing a magnetic material, a binder resin, and a dispersant onto a base layer to form a coating film, and then drying the coating film to form a radio wave absorbing layer; the dispersant is at least one selected from the group consisting of a silane coupling agent, a titanate coupling agent, a zirconate coupling agent, and an aluminate coupling agent; the binder resin comprises an aromatic ester-urethane copolymer, A method for producing a radio wave absorber film, wherein the magnetic material contains at least one selected from the group consisting of epsilon type iron oxide, barium ferrite magnetic material, and strontium ferrite magnetic material.
9. The method includes a radio wave absorbing layer forming step of applying a paste containing a magnetic material and a binder resin onto a base layer to form a coating film, and then drying the coating film to form a radio wave absorbing layer; the binder resin comprises an aromatic ester-urethane copolymer, the magnetic material includes at least one selected from the group consisting of epsilon-type iron oxide, barium ferrite magnetic material, and strontium ferrite magnetic material; The method for producing a radio wave absorber film, wherein the radio wave absorbing layer has a thickness of 50 μm or less.
10. 10. The method for producing a radio wave absorber film according to claim 8, further comprising a cutting step of cutting a laminate including the base material layer and the radio wave absorbing layer obtained in the radio wave absorbing layer forming step to obtain a radio wave absorber film of a predetermined size.
Citation Information
Patent Citations
Magnetic recording medium
JP1989106317A
Electromagnetic wave absorbent and its manufacturing method
JP2003229694A
Magnetic crystal for radio wave absorbing material and radio wave absorber
JP2008277726A
Electromagnetic wave absorbing sheet
JP2009060060A
High frequency antenna element and high frequency antenna module
JP2017184106A