Ceramics
The ceramic structure with controlled Ca distribution at the interface between Ca and Y-stabilized zirconia layers enhances adhesion and reduces conductivity loss, addressing poor interface adhesion issues.
Patent Information
- Application Number
- JP2020045334
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-03-16
AI Technical Summary
The interface between layers of ceramics containing Y-containing stabilized zirconia or partially stabilized zirconia laminated on a first layer experiences poor adhesion, leading to potential performance issues.
A ceramic structure is designed with a first layer containing Ca-stabilized zirconia or partially stabilized zirconia, and a second layer containing Y-stabilized zirconia or partially stabilized zirconia, where Ca is present near the interface, maintaining a Ca-to-total Zr and Ca ratio of 1.6 mol% or more at 2 μm from the interface, and less than 8.3 mol% at 10 μm, enhancing the bond strength through sintering.
The improved adhesion at the interface strengthens the bond between the layers, reducing ionic conductivity loss due to Ca diffusion and maintaining optimal performance.
Smart Images

Figure 0007576918000002 
Figure 0007576918000003 
Figure 0007576918000001
Abstract
Description
[Technical field]
[0001] The present invention relates to ceramics containing zirconia. [Background technology]
[0002] Stabilized zirconia and partially stabilized zirconia having ion conductivity are a type of ceramic material having a function of diffusing gas, such as gas permeable membranes and gas separation membranes. Patent Document 1 discloses an oxygen permeable membrane made of ceramics having a first layer containing Ca-containing stabilized zirconia. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-113714 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the above technology, ceramics in which a second layer containing stabilized zirconia or partially stabilized zirconia containing Y is laminated on a first layer have a problem that the adhesion at the interface between the first layer and the second layer may be low.
[0005] The present invention has been made to solve this problem, and has an object to provide a ceramic capable of improving the adhesion at the interface between the first layer and the second layer. [Means for solving the problem]
[0006] In order to achieve this object, the ceramic of the present invention comprises a first layer and a second layer bonded to each other, the first layer comprising stabilized zirconia or partially stabilized zirconia containing Ca, the second layer comprising stabilized zirconia or partially stabilized zirconia containing Y, Ca being present near the interface between the first layer and the second layer, and a ratio R2 of the amount of Ca to the sum of the amount of Zr and the amount of Ca at a position 2 μm away from the interface towards the second layer is 1.6 mol% or more. Effect of the Invention
[0007] According to the ceramic described in claim 1, the ratio R2 of the amount of Ca at a position 2 μm away from the interface between a first layer containing stabilized zirconia or partially stabilized zirconia containing Ca and a second layer containing stabilized zirconia or partially stabilized zirconia containing Y toward the second layer is 1.6 mol% or more, so that the bonding between the particles of the first layer and the particles of the second layer is strengthened by sintering, and the adhesion at the interface between the first layer and the second layer can be improved.
[0008] S According to Lamix, the ratio R2 is 8.3 mol% or less. 、C The decrease in ionic conductivity near the interface due to the diffusion of a can be suppressed.
[0009] Claim 2 According to the described ceramics, the ratio R of Ca to the total amount of Zr and Ca at a position 10 μm away from the interface on the second layer side is 10 Since the content is 4.2 mol% or less, the claim 1 of In addition to this effect, the decrease in ionic conductivity near the interface due to Ca diffusion can be further suppressed. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a cross-sectional view of a ceramic according to an embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view of an apparatus for measuring oxygen transmission rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. Fig. 1 is a cross-sectional view including a central axis O of a ceramic 10 in one embodiment. In this embodiment, the ceramic 10 is a cylindrical tube. Fig. 1 illustrates one side of the ceramic 10 with respect to the central axis O, and the other side of the central axis O is omitted.
[0012] The ceramic 10 includes a first layer 11 and a second layer 12 bonded to each other. The ceramic 10 is manufactured through a process of forming and firing the first layer 11 and the second layer 12. In this embodiment, the second layer 12 is bonded to the outer periphery of the first layer 11. In this embodiment, the ceramic 10 has a function of allowing oxygen to permeate in the thickness direction.
[0013] The first layer 11 contains Ca-containing stabilized zirconia or partially stabilized zirconia. Ca-containing stabilized zirconia is zirconia in which CaO (stabilizer) is dissolved in ZrO2 so that cubic crystals are stable at room temperature. Ca-containing partially stabilized zirconia is zirconia in which the amount of stabilizer is reduced compared to the amount of stabilizer in stabilized zirconia, and cubic crystals and tetragonal crystals are dispersed at room temperature. Stabilized zirconia and partially stabilized zirconia function as oxygen ion conductors.
[0014] In addition to stabilized zirconia or partially stabilized zirconia, the first layer 11 may contain other oxygen ion conductors, electronic conductors, or oxides that have both oxygen ion conductivity and electronic conductivity (hereinafter referred to as "mixed conductive oxides").
[0015] Other oxygen ion conductors include, for example, ceria-based solid solutions, such as cerium-based composite oxides, such as gadolinium-doped ceria and samarium-doped ceria.
[0016] The electron conductor may be selected from oxides having a perovskite structure, oxides having a spinel crystal structure, and metal materials such as precious metals. Examples of oxides having a perovskite structure include oxides in which Sr is added to the La site in a LaMnO3 compound, composite oxides such as CaTiO3 and BaTiO3, and La 1-X M X CrO 3-Z (wherein M is an alkaline earth metal excluding Mg, 0≦X≦0.4, and Z is a value indicating that the ratio of metal elements or the amount of oxygen atoms varies.)
[0017] Examples of mixed conductive oxides include oxides having a perovskite structure in which Sr is added to the La site and Fe is added to the Ga site in a LaGaO3 compound, oxides having a perovskite structure in which Ba is added to the Sr site and Fe is added to the Co site in a SrCoO3 compound, oxides having a layered perovskite structure, oxides having a fluorite structure, oxides having an oxyapatite structure, and oxides having a melilite structure.
[0018] The first layer 11 may contain a catalyst. Examples of the catalyst include metals such as Ni, Co, and Cu, and precious metals such as Rh and Pt. The first layer 11 may contain other oxides such as tantalum oxide and niobium oxide. The first layer 11 may be porous. When the first layer 11 is porous, the porosity of the first layer 11 is, for example, 20 to 60%. The porosity of the first layer 11 can be obtained from an image of a cross section of the ceramic 10 taken by a scanning electron microscope (SEM). The porosity is a percentage obtained by dividing the sum of the area of pores surrounded by the first layer 11 that appears in the field of view of the SEM by the sum of the area of the first layer 11 and the area of the pores in the field of view.
[0019] The second layer 12 contains Y-containing stabilized zirconia or partially stabilized zirconia. Y-containing stabilized zirconia is zirconia in which Y2O3 (stabilizer) is dissolved in ZrO2 so that cubic crystals are stable at room temperature. Y-containing partially stabilized zirconia is zirconia in which the amount of stabilizer is reduced compared to the amount of stabilizer in stabilized zirconia, and cubic crystals and tetragonal crystals are dispersed at room temperature. Stabilized zirconia and partially stabilized zirconia function as oxygen ion conductors.
[0020] The second layer 12 may contain other oxides in addition to Y-containing stabilized zirconia and partially stabilized zirconia. Examples of other oxides include LaCrO3-based oxides having a perovskite structure. 1-X Sr X CrO 3-Z (0≦X≦0.2, Z is a value indicating that the ratio of metal elements and the amount of oxygen atoms vary.) In addition, the second layer 12 can contain, as other oxides, one or more selected from the oxygen ion conductors, electron conductors, and mixed conductive oxides exemplified for the first layer 11.
[0021] A catalyst can be supported on the second layer 12. Examples of the catalyst include metals such as Ni, Co, and Cu, and noble metals such as Rh and Pt.
[0022] The element constituting the compound contained in the second layer 12 is preferably an element other than Ca. This is to suppress a decrease in the ionic conductivity of the second layer 12. The element constituting the compound contained in the first layer 11 is preferably an element other than Y. This is to specify the position of the interface 13 between the first layer 11 and the second layer 12 by the concentration of Y contained in the second layer 12.
[0023] The ceramic 10 is manufactured, for example, as follows. First, a compact for the first layer 11 is prepared. The compact for the first layer 11 is made by mixing a pore-forming agent, such as synthetic resin beads or carbon powder, and a binder with a powder of a specific oxide, and then extrusion molding, press molding, or the like. The porosity of the first layer 11 is set by the particle size and amount of the pore-forming agent, etc.
[0024] Next, the paste constituting the second layer 12 is applied to the surface of the compact of the first layer 11 and dried to form the compact of the second layer 12. The paste constituting the second layer 12 is a mixture of a powder of a specific oxide and a vehicle. The application of the paste is carried out by a printing method, a spraying method, a dip coating method, a doctor blade method, or the like. In this way, the compacts of the first layer 11 and the second layer 12 are integrated.
[0025] Next, the compact is fired. Through the firing process, the ceramic 10 is obtained in which the first layer 11 and the second layer 12 are bonded to each other. When the second layer 12 is to support a catalyst, a paste in which a powder of a specific catalyst is mixed with a vehicle is applied to the surface of the second layer 12 of the ceramic 10, and then fired.
[0026] The production of the molded body is not limited to extrusion molding and paste coating. It is of course possible to produce the molded body by other known methods. Examples of other methods include sheet molding, sheet lamination, press molding, etc.
[0027] In the ceramic 10, Ca is present near the interface 13 between the first layer 11 and the second layer 12. The position of the interface 13 is identified from the cross section of the ceramic 10 using a wavelength dispersive spectrometer (WDS) of an electron probe microanalyzer (EPMA). The conditions for the WDS analysis are an acceleration voltage of 15 kV, an irradiation current of 80 nA, and an irradiation time of 15 ms, and the smallest beam diameter that can be set under these conditions is used.
[0028] First, by WDS analysis, Zr, Ca, and Y within a square field of view 14 measuring 50 μm in length and 50 μm in width near the boundary between the first layer 11 and the second layer 12 in the cross section of the ceramic 10 are quantitatively analyzed (area analysis) at 62,500 measurement points evenly allocated throughout the field of view 14. The measurement points are arranged in 250 columns at 0.2 μm intervals in the direction in which the boundary between the first layer 11 and the second layer 12 extends, and in 250 rows at 0.2 μm intervals in the direction approximately perpendicular to the boundary.
[0029] In the firing process, Ca contained in the compact of the first layer 11 diffuses toward the second layer 12, and Y contained in the compact of the second layer 12 diffuses toward the first layer 11. However, since Ca diffuses more easily than Y in ZrO2, Y, which is less diffusive, is used as an index, and a map is created in which the measured values (counts) of Y correspond to the positions of 62,500 measurement points. The map is compared with the structure of the ceramic 10 based on the backscattered electron image, and one measurement point that is the interface 13 between the first layer 11 and the second layer 12 is determined for every 250 rows of measurement points.
[0030] Next, for each row of measurement points, the measured value (count) of Zr and the measured value (count) of Ca are obtained at the measurement point at the position 15 located 2 μm away from the interface 13 toward the second layer 12 side from the interface 13, and the average value of each measured value is obtained. When the corresponding measurement point overlaps with a pore appearing in the cross section of the ceramic 10, the measurement value at that measurement point is excluded from the average value.
[0031] The Zr concentration (wt%) and Ca concentration (wt%) are calculated from the average values of Zr and Ca thus calculated, and then the amount of Zr and the amount of Ca are calculated. The amount of Zr is the value obtained by dividing the Zr concentration (wt%) obtained from the WDS analysis by the molar mass of Zr, 91 (g / mol). The amount of Ca is the value obtained by dividing the Ca concentration (wt%) obtained from the WDS analysis by the molar mass of Ca, 40 (g / mol). Next, the ratio R2 (mol%) of the amount of Ca to the total amount of Zr and Ca is calculated.
[0032] As in the case of finding the ratio R2 (mol%), the measured values (counts) of Zr and Ca are found for each row of measurement points at the measurement point at the position 16 located 10 μm away from the interface 13 toward the second layer 12 side from the interface 13, and then the amount of Zr and the amount of Ca are found. Next, the ratio R 10 Calculate (mol%).
[0033] In ceramic 10, the proportion R2 (average value) of the amount of Ca at a position 2 μm away from interface 13 toward second layer 12 is 1.6 mol% or more. This means that Ca contained in the compact of first layer 11 diffuses toward second layer 12 during the firing process. Since the bonds between the particles of first layer 11 and the particles of second layer 12 are strengthened by sintering, the adhesion of interface 13 between first layer 11 and second layer 12 can be improved.
[0034] The ceramic 10 has a ratio R2 (average value) of 8.3 mol% or less. This means that the diffusion of Ca contained in the compact of the first layer 11 is not excessive during the firing process. Therefore, the decrease in ion conductivity near the interface 13 due to Ca diffused into the second layer 12 can be suppressed.
[0035] The ceramic 10 has a Ca ratio R at a position 10 μm away from the interface 13 toward the second layer 12. 10 (average value) is 4.2 mol% or less. This also means that the diffusion of Ca contained in the compact of the first layer 11 is not excessive during the firing process. Therefore, the decrease in ion conductivity near the interface 13 due to the diffusion of Ca can be further suppressed. EXAMPLES
[0036] The present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples.
[0037] (Preparation of test specimens) Powders of calcia-stabilized zirconia or calcia-partially-stabilized zirconia, an acrylic pore former, and a catalyst (Pt) were mixed with a binder and extrusion-molded to produce a molded body. This molded body was cut to obtain a plate-shaped molded body (first layer molded body) with a length of 20 mm, width of 20 mm, and thickness of 1.5 mm.
[0038] In addition, 8mol% yttria-stabilized zirconia, LaCrO3-based oxide (La 0.8 Sr 0.2 Each powder of CrO3 and a vehicle was mixed to obtain a paste for the second layer. This paste was printed on the entire surface of the compact of the first layer to a thickness of 100 μm to obtain a compact in which the compact of the second layer was laminated on the compact of the first layer. This compact was fired in air to obtain test pieces of various ceramics in which the first layer and the second layer were bonded together.
[0039] Next, a paste made by mixing catalyst (Pt) powder and a vehicle was applied to the surface of the second layer of the test piece, and then fired at 1000° C. This caused the catalyst to adhere to the surface of the second layer.
[0040] The zirconia constituting the first layer was various stabilized zirconia or partially stabilized zirconia with different amounts of calcia dissolved therein in the range of 10 to 19 mol%. The firing conditions for the molded bodies used to obtain the test pieces were a heating rate of 1 to 10°C / min, a maximum temperature of 1000 to 1500°C, and a holding time at the maximum temperature of 0 to 20 hours, which were all varied. The other factors used to prepare the test pieces were kept the same, and various test pieces were obtained.
[0041] (R2 and R 10 (Calculation of Using EPMA WDS analysis (accelerating voltage 15 kV, irradiation current 80 nA, irradiation time 15 ms), Zr, Ca, and Y were quantitatively analyzed at 62,500 measurement points evenly distributed within a square field of view of 50 μm length and 50 μm width on the cross section (polished surface) of the test piece. If a measurement point was located at the position of a pore appearing on the cross section of the test piece, the result of that measurement point was excluded. Within the field of view, one measurement point was determined for every 250 rows of measurement points, which was the interface between the second layer where Zr and Y were detected and the first layer where Y was below the detection limit. The position of the field of view was set so that two opposing sides of the field of view intersected the interface almost perpendicularly and another two opposing sides of the field of view were almost parallel to the interface.
[0042] Next, for each row of measurement points, the measured values of Zr and Ca were obtained at a position 2 μm away from the interface on the second layer side. The concentrations (wt%) of Zr and Ca were obtained from the average values, and then the amounts of Zr and Ca were obtained, and the ratio R2 (mol%) of the amount of Ca to the total amount of Zr and Ca was calculated.
[0043] Similarly, for each row of measurement points, the measured values of Zr and Ca were obtained at a position 10 μm away from the interface on the second layer side. The concentrations (wt%) of Zr and Ca were calculated from the average values, and the amounts of Zr and Ca were then calculated. The ratio R of the amount of Ca to the total amount of Zr and Ca was calculated. 10 (mol%) was calculated.
[0044] (Interface adhesion) The interface state of five test pieces for each preparation condition was observed using a scanning electron microscope (SEM).
[0045] (Oxygen transmission rate) The oxygen transmission rate of the test piece 20 was measured using an apparatus 30 shown in FIG. 2. FIG. 2 is a schematic cross-sectional view of the apparatus 30 for measuring the oxygen transmission rate. The apparatus 30 has the test piece 20 placed between two tubes 31 and 33. The tube 31 forms an air chamber 32, and the tube 32 forms a hydrogen chamber 34. The first layer 11 formed on the test piece 20 faces the hydrogen chamber 34, and the second layer 12 faces the air chamber 32. Air is supplied to the air chamber 32 from a tube 35, and hydrogen gas is supplied to the hydrogen chamber 34 from a tube 36. A ring 37 made of borosilicate glass is interposed between the test piece 20 and the tube 33. The ring 37 melts and solidifies to seal the hydrogen chamber 34, and the test piece 20 isolates the air chamber 32 and the hydrogen chamber 34. A heater 38 heats the test piece 20 when the oxygen transmission rate is measured. The ring 37 is melted and solidified prior to the measurement, and during the measurement, the ring 37 functions as a seal to seal the hydrogen chamber 34 .
[0046] With the test piece 20 heated to 1000°C by the heater 38, air (flow rate 300 mL / min) was supplied to the air chamber 32, and hydrogen gas (flow rate 200 mL / min) was supplied to the hydrogen chamber 34. The concentration of water vapor contained in the gas in the hydrogen chamber 34 was measured with a mirror dew point meter, and the amount of oxygen that had permeated the test piece 20 was calculated from the concentration of water vapor in the hydrogen chamber 34. The oxygen transmission rate ((cc / min) / cm 2 ) was sought.
[0047] The R2 and R3 of the test specimens for evaluating the interfacial adhesion and oxygen transmission rate were 10 These are shown in Table 1 together with the evaluation results of adhesion and the oxygen transmission rate. No. 1-11 in Table 1 are test pieces produced under different conditions. The evaluation of the adhesion at the interface was given a B when peeling was observed at the interface of one or more of the five test pieces, and an A when no peeling was observed in any of the five test pieces.
[0048] [Table 1] As shown in Table 1, no peeling was observed at the interface in No. 3-11, where R2 was 1.6 mol% or more. However, peeling was observed at the interface in No. 1 and No. 2, where R2 was less than 1.6 mol%. It is presumed that when R2 is 1.6 mol% or more, the bond between the particles of the first layer and the particles of the second layer is strengthened by sintering, improving the adhesion at the interface.
[0049] The oxygen transmission rate was measured for test piece No. 3-11, where no peeling was observed at the interface. The oxygen transmission rate was not measured for test pieces No. 1 and No. 2, where peeling was observed at the interface. As shown in Table 1, No. 3-10, where R2 is 8.3 mol% or less, has an oxygen transmission rate of 20 (cc / min) / cm 2 However, No. 11, which has an R2 value of more than 8.3 mol%, had an oxygen permeability rate of 5 (cc / min) / cm 2 It is speculated that No. 3-10 was able to suppress the decrease in ionic conductivity near the interface due to Ca diffusion.
[0050] Also, R 10 The oxygen permeability of No. 3-10, which has a content of 4.2 mol% or less, is 20 (cc / min) / cm 2 That's all. R 10 It was revealed that the decrease in ionic conductivity near the interface due to Ca diffusion can be suppressed by keeping the Ca content at 4.2 mol% or less.
[0051] The present invention has been described above based on an embodiment, but the present invention is in no way limited to the above embodiment, and it can be easily inferred that various improvements and modifications are possible within the scope of the present invention without departing from the spirit of the present invention.
[0052] In the embodiment, the ceramic 10 is a cylindrical tube, but this is not necessarily limited to this. The ceramic 10 can be in any shape, such as a flat plate, a curved plate, or a bent tube.
[0053] In the embodiment, the ceramic 10 has a function of an oxygen permeable membrane, but the use of the ceramic 10 is not limited to this. The ceramic 10 can be used for any purpose, such as a mechanical part or an electric part. Therefore, it is possible for the first layer 11 to contain other oxides, such as alumina or mullite, instead of an ion conductor or an electron conductor.
[0054] In the embodiment, the ceramic 10 in which the second layer 12 is laminated on the first layer 11 has been described, but the present invention is not necessarily limited to this. It is of course possible to further laminate a third layer, a fourth layer, etc. on the second layer 12. Examples of the third layer and the fourth layer include various oxides exemplified as the compounds contained in the first layer 11 and the second layer 12. [Explanation of symbols]
[0055] 10. Ceramics 11 First Layer 12 Second Layer 13 Interface 15 2 μm away from the interface towards the second layer 16 10 μm away from the interface towards the second layer
Claims
1. A ceramic including a first layer and a second layer bonded together, The first layer contains stabilized zirconia or partially stabilized zirconia containing Ca, The second layer comprises stabilized zirconia or partially stabilized zirconia containing Y, Ca is present in the vicinity of an interface between the first layer and the second layer, the interface being determined by the presence or absence of Y; A ratio R of the amount of Ca to the total amount of Zr and the amount of Ca at a position 2 μm away from the interface toward the second layer 2 is 1.6 mol % or more and 8.3 mol % or less.
2. A ratio R of the amount of Ca to the total amount of Zr and the amount of Ca at a position 10 μm away from the interface toward the second layer 10 The ceramic according to claim 1, wherein the content of C is 4.2 mol % or less.
Citation Information
Patent Citations
Solid electrolyte fuel cell
JP1993151982A
Jig for firing
JP1994082166A
Solid electrolyte type electrochemical cell, and manufacture of it
JP1997139219A
Oxygen permeation membrane and production method of oxygen permeation membrane
JP2017001003A
Oxygen permeation membrane, method for manufacturing same, and reformer
JP2017113714A