Magnetic coated conductor and method for producing the same
By coating a conductive wire with a tape-like magnetic material and insulator, the method achieves uniform thickness and stable magnetic properties, reducing AC resistance and enhancing magnetic material stability.
Patent Information
- Application Number
- JP2023212191
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-01-17
AI Technical Summary
Existing methods for applying magnetic materials to conductive wires face challenges in achieving uniform thickness and stability due to issues with adhesion and fluidity of magnetic powder, leading to uneven distribution and variations in magnetic properties.
A method involving coating a conductive wire with a tape-like magnetic material containing a binder and magnetic powder, followed by a tape-like insulator, and applying heat treatment to solidify the magnetic material uniformly around the wire.
The method ensures a uniform thickness of the magnetic material, enhancing magnetic properties stability and reducing AC resistance by uniformly distributing the magnetic material, even under bending conditions.
Smart Images

Figure 0007577285000005 
Figure 0007577285000006 
Figure 0007577285000007
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a magnetic coated conductor that can be realized at low cost and a method for manufacturing the magnetic coated conductor. [Background technology]
[0002] In coils, inductors, etc., as a method for reducing the AC resistance caused by the proximity effect experienced by any conductor, providing a magnetic body on the outer surface of the conductor has been considered. For example, a manufacturing method of applying magnetic plating to the surface of a conductor (Patent Document 1) has been used for a long time. By covering the outer surface of the conductor with a magnetic material, the magnetic field generated by the current flowing through the adjacent conductor is bypassed by the magnetic body, suppressing the magnetic field from penetrating into the conductor, and as a result, the eddy current generated in the conductor is reduced, and the AC resistance value can be lowered.
[0003] However, the method using magnetic plating has problems such as the need for large and expensive equipment, the difficulty of thickening the magnetic body to increase the relative magnetic permeability, and the time required for the process.In recent years, therefore, a method of bonding magnetic powder (Patent Document 1) and a method of mixing magnetic powder with silicone varnish and spraying it (Patent Document 2) have been proposed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Publication No. 151594 / 1983 [Patent Document 2] JP 2018-018585 A [Patent Document 3] JP 2018-137120 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the techniques of Patent Documents 2 and 3 are both premised on adhering the magnetic powder to the conductor part, and when the magnetic body is provided over the entire coil having a relatively wide wall surface, such as a tightly wound helical coil, there is no problem with adhesion. However, when attempting to provide the magnetic body to the thin single wire that constitutes the coil using the above method, it is difficult to form the magnetic body with a uniform thickness. In particular, it is difficult to mix the magnetic powder and the binder, and increasing the binder ratio increases the fluidity, and the magnetic body will have uneven thickness due to the influence of gravity and the like from adhering to the conductor until it is mostly solidified. Conversely, if the ratio of magnetic powder is high, the fluidity decreases and it becomes difficult to spray continuously from the spray. If the magnetic body is not provided evenly in this way, there is a problem that the characteristics will vary as a result. [Means for solving the problem]
[0006] A magnetic coated conductor according to one embodiment of the present disclosure is a magnetic coated conductor in which the surface of a conductor is coated with a tape- or sheet-like magnetic material containing a binder and magnetic powder, and a tape-like insulator is wound spirally around the surface of the magnetic material at a pitch narrower than the width of the magnetic material, wherein the binder is thermosetting and the insulator is heat-shrinkable, and the magnetic material is evenly fastened, compressed, and solidified by the insulator toward the center of the conductor.
[0007] The magnetic powder in the magnetic-material-coated conductor may be spherical, and the magnetic material may contain magnetic powder whose maximum spherical diameter is 0.05 to 1.0 times the thickness of the magnetic material.
[0008] The magnetic body may be a tape-shaped magnetic body having a width narrower than that of the insulator, and wound in a spiral shape.
[0009] The magnetic body may have a relative magnetic permeability of 9-30.
[0010] The insulator may include polyethylene terephthalate resin.
[0011] A method for manufacturing a magnetically coated conductor according to one embodiment of the present disclosure includes the steps of preparing a conductor, a tape- or sheet-shaped magnetic material containing a thermosetting binder and magnetic powder, and a tape-shaped insulator having heat shrinkability, covering the conductor with the magnetic material, winding the insulator in a spiral shape at a pitch narrower than its width together with the magnetic material coating, and performing a heat treatment, wherein the heat treatment process is divided into a process of heating the magnetic material until it is solidified to an extent that the thickness can be maintained, and a process of heating the insulator together with the insulator after it has been wound around the conductor.
[0012] The process for covering the conductor may be a process for winding a tape-shaped magnetic material in a spiral shape around the conductor.
[0013] The magnetic body may be attached to the insulator in advance, and then wound helically around the conductor wire.
[0014] The process of covering the conductor may be a process of wrapping the tape-shaped magnetic material in parallel with the conductor. Effect of the Invention
[0015] According to one aspect of the present disclosure, the thickness of the magnetic body around the conductor can be easily made uniform, and further, since the heat-shrinkable tape-shaped insulator uniformly tightens the magnetic body provided on the conductor from the outside, the magnetic body can be maintained regardless of the slight bending of the conductor. In particular, when a tape-shaped magnetic body is used, the thickness can be easily controlled with precision during the process of creating the tape, and as a result, the precision of the magnetic properties can be improved. [Brief description of the drawings]
[0016] [Figure 1] 1A and 1B are an external view and a partial cross-sectional view of an embodiment (first embodiment) of the present disclosure. [Diagram 2] 1A to 1C are an external view of a second embodiment of the present disclosure and a cross-sectional view of a magnetic body in the same embodiment. [Diagram 3] 13A and 13B are an external view and a partial cross-sectional view of a third embodiment of the present disclosure. [Figure 4] FIG. 2 is a cross-sectional view of a magnetic body containing magnetic powder with a maximum diameter. [Diagram 5] 1A to 1C are three-view diagrams showing the shape and dimensions of the coil used in the embodiment of the present disclosure. [Figure 6] 1 is a graph showing magnetic field-magnetic flux characteristics of a magnetic material used in an embodiment of the present disclosure. [Figure 7] 1 is a graph showing frequency-complex relative permeability characteristics of a magnetic body used in an embodiment of the present disclosure. [Figure 8] FIG. 11 is an explanatory diagram showing the effect of an embodiment of the present disclosure compared to a comparative example. [Figure 9] 1 is a diagram showing magnetic flux and current distribution obtained by two-dimensional AC magnetic field analysis. [Figure 10] 1 is a graph showing frequency characteristics of coils according to an embodiment of the present disclosure and a comparative example. [Figure 11] FIG. 1 is a block diagram illustrating an experimental environment for an embodiment of the present disclosure. [Figure 12] 1 is a graph showing time-temperature changes in examples and comparative examples of the present disclosure. [Figure 13] 1 is a photograph showing the measurement of heat generation in an example and a comparative example of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] An embodiment according to one aspect of the present disclosure (hereinafter, the present embodiment) will be described in detail below with reference to the drawings. FIG. 1(a) shows an external view of a magnetic coated conductor wire 1 in the present embodiment, and FIG. 1(b) shows a partial cross-sectional view. In FIG. 1(a), a conductor wire 2 is a wire having a circular cross section made of a conductive material such as copper, aluminum, or other metal. The diameter is preferably 0.1 mm to 3.0 mm. Furthermore, the length of the conductor wire 2 may range from several hundred meters to several kilometers when used as a wire for manufacturing motor coils or transformers.
[0018] A magnetic body 3 is provided on the surface of the conductor 2, and an insulator 4 is provided on the outer side thereof. As shown in the enlarged view on the right side of FIG. 1(b), the magnetic body 3 is mainly composed of a composite material in which a binder 3a is mixed with magnetic powder 3b. The mixing ratio of the two is adjusted so that the relative permeability of the magnetic body 3 is 9 to 30. The magnetic body 3 has an adhesive layer 3c, and is bonded to the conductor 2 via this adhesive layer. In this embodiment, the insulator 4 is tape-shaped and has heat shrinkability. Also, the binder 3a is thermosetting, and the magnetic body 3 is tape-shaped.
[0019] The magnetic powder 3b may be made of Fe-based amorphous, pure iron, Fe-Si, nanocrystal, or sendust. The shape is preferably spherical. The larger the spherical diameter, the higher the relative magnetic permeability tends to be. When the thickness of the magnetic body 3 is used as a reference, the magnetic powder 3b may have a maximum spherical diameter of about 0.05 to 1.0 times the thickness of the magnetic body, and more preferably, about 0.2 to 1.0 times the thickness of the magnetic body.
[0020] Here, 1.0 times the thickness of the magnetic material refers to a state in which magnetic powder (magnetic spheres) 33a having approximately the same diameter as the magnetic material thickness are held by binder 3a, as shown in Fig. 4. In this case, to further increase the magnetic permeability, magnetic powder 33b having a size of 0.05 times the thickness of the magnetic material (approximately 1 / 20th the size of the magnetic spheres) may be embedded in the gaps between the magnetic spheres.
[0021] The binder 3a may be a resin or rubber-based material. If it is a resin-based material, it may be a material that has thermosetting properties such as silicone resin or epoxy resin. If it is a rubber-based material, it may be a material that becomes an elastomer when heated, and may be either synthetic rubber or natural rubber.
[0022] A method for manufacturing the magnetic coated conductor 1 will be described below. First, the conductor 2 is coated with the magnetic material 3. In this embodiment, the tape-shaped magnetic material 3 is wound spirally around the outer periphery of the conductor 2 with no gaps to coat the entire circumference. Next, the insulator 4 is wound spirally on the surface of the magnetic material 3 at the same pitch as the tape width of the magnetic material 3. If the tape width of the insulator 4 is designed to be slightly wider than the tape width of the magnetic material 3, then the entire surface of the magnetic material 3 can be coated by the wider width so as to slightly cover the top of the previously wound insulator 4, as shown in FIG. 1(b).
[0023] As described above, the surface of the conductor 2 is coated with the magnetic material 3, and the surface of that is further coated with the insulator 4, and these are then successively heated. As a result, the thermosetting magnetic material 3 solidifies, and at the same time, the insulator 4 exerts a contracting force that evenly tightens the magnetic material 3 toward the center of the conductor 2. As a result, the magnetic material 3 can be compressed and solidified with a uniform thickness. Here, solidification refers to the state of a material in which the shape is maintained when left alone, and includes both solidification and elasticity.
[0024] As a result of the above process, a magnetic-material-coated conductor 1 can be manufactured in which the thickness of the magnetic body 3 is uniform and the magnetic body is less likely to crack or warp when bent. When the insulator 4 thermally shrinks, it shrinks not only in the longitudinal direction but also in the width direction. If the tape width of the insulator 4 were made the same as the tape width of the magnetic body 3, a gap would be created between the insulator 4 of adjacent turns due to thermal shrinkage. As a result, insulation problems would occur in the magnetic-material-coated conductor 1. Therefore, the tape width of the insulator 4 is set wider than the tape width of the magnetic body 3 (i.e., the winding pitch of the magnetic body 3).
[0025] The advantage of forming the magnetic material 3 in tape or sheet form beforehand is that the thickness of the magnetic material can be made uniform. Immediately after mixing the magnetic powder and binder, the magnetic composite material still has a certain degree of fluidity, and is stretched with rollers with fixed gaps while being moderately heated to produce a sheet of uniform thickness. This can then be cut to an appropriate width to prepare the tape-like magnetic material 3. Note that the heating at this stage does not completely solidify the magnetic composite material (binder), but must be such that it retains sufficient flexibility to be wound around the conductor wire 2.
[0026] As described above, the magnetic coated conductor wire 1 of the present embodiment has the following features. (1) Since the magnetic body 3 is formed with a uniform thickness, the magnetic properties are uniform and stable. (2) The thickness of the magnetic body 3 is maintained by the pressure of the insulating layer 4, so the initial rigidity and elasticity of the magnetic body 3 are not particularly important. In other words, the ratio of magnetic powder to binder can be increased to increase the relative permeability. (3) Since the magnetic body 3 is pressurized by the insulating layer 4, the magnetic body 3 is less likely to bend or crack even when slightly bent. (4) Since the insulating layer 4 is wound with some overlapping, the magnetic body 3 is not exposed when bent, and the insulating layer 4 has excellent insulation properties. (5) Since the insulating layer 4 has high insulating properties, short circuits with adjacent conductors are unlikely to occur even if the density or spherical diameter of the magnetic powder 3b is increased. In particular, the features (3), (4), and (5) are extremely important when winding the magnetic coated conductor wire 1 of this embodiment to fabricate a coil or a transformer.
[0027] A second embodiment of the present disclosure will be described below. FIG. 2(a) shows an external view of this embodiment, and FIG. 2(b) shows a cross-sectional view of the magnetic body 3. In this embodiment, in order to simplify the manufacturing process of the magnetic body covered conductor 1, a synthetic magnetic tape 30 is used in which the magnetic body 3 and a wider insulator 4 are bonded together in advance. By spirally winding this tape around the conductor 2, it is possible to obtain the magnetic body covered conductor 1 in which the insulators overlap and are covered as in FIG. 1(a). In this embodiment, the characteristics and detailed configurations of the conductor 2, the magnetic body 3, and the magnetic body 4 are the same as those of the first embodiment.
[0028] A third embodiment of the present disclosure will be described below. Fig. 3(a) shows an external view of this embodiment, and Fig. 3(b) shows a cross-sectional view. In this embodiment, the magnetic body 3 is not wound in a spiral shape, but is wrapped and wound in parallel with the conductor wire 2 as shown in Fig. 3(a). A tape-shaped insulator 4 is wound in a spiral shape on top of it. As a result, as shown in Fig. 3(b), a magnetic-body-coated conductor wire 1 can be produced in which there is no joint of the magnetic body 3 in the longitudinal direction of the conductor wire 2.
[0029] The advantage of this embodiment is that the magnetic material 3 can be provided on the surface of the conductor 2 using relatively simple equipment or method. On the other hand, there is a structural weakness in that the joint is continuous in the longitudinal direction of the conductor 2, but since it is held in place from all sides by the spirally wound insulator 4, there is little possibility of peeling or wrinkling. EXAMPLES
[0030] Examples of the present disclosure will be described below. In the examples, an experiment for confirming the homogeneity of the magnetic coated conductor wire 1 of the present disclosure and the results thereof will be described.
[0031] (Structure of magnetic coated conductor and coil used in the experiment) The structure of the magnetic coated conductor and coil is shown in Figure 5. (b) in the figure is a cross-sectional view of the conductor of the comparative example (hereafter, COW), and (c) in the figure is a cross-sectional view of the magnetic coated conductor of this embodiment (hereafter, MCW). Both the comparative example (COW) and this embodiment (MCW) have the number of turns N=9 and are wound around a coil bobbin (Figure 5(a)) made of Teflon (registered trademark) that has grooves cut into it with a pitch of 2.2 mm. The comparative example (COW) has only an insulating layer of 18 μm thick on the outer circumference of a copper conductor with a diameter of 1.45 mm.
[0032] The magnetic coated conductor 1 of this embodiment (MCW) is a copper conductor 2 (Conductor) having the same diameter as the comparative example (COW) with a tape-like magnetic material 3 (Magnetic tape) having a thickness of 0.125 mm wound around it. The total diameter of the magnetic coated conductor 1 is 1.74 mm. The coil pitch is set to 2.2 mm to prevent the magnetic coated conductors from contacting each other. In the comparative example (COW), a Teflon (registered trademark) tape of the same thickness is wound to match the coil pitch with this embodiment (MCW). Note that the present embodiment does not use an insulator 4 because the purpose is to confirm the homogeneity of the magnetic properties by using a tape-like magnetic material 3 with a uniform thickness, and a coil bobbin with a groove cut in advance is used to prevent short circuits between the conductors.
[0033] Fig. 6 shows the DC magnetic characteristics of the magnetic body 3 in this embodiment. A vibration-type magnetometer (Riken Denshi) was used for the measurement. The saturation magnetic flux density was 0.72 T. Fig. 7 shows the complex relative permeability, which was measured using a BH analyzer (IWATSU SY-8218). As a result of the measurement, μ' was constant at approximately 9.3 over all frequencies.
[0034] Figure 8 visually shows the skin effect and proximity effect that occur in each conductor of a coil. There are two types of AC resistance: resistance Rs due to the skin effect and resistance Rp due to the proximity effect. Resistance Rs due to the skin effect is the resistance that occurs when high-frequency current flows through a conductor, as the current is biased toward the surface of the conductor due to the time change in the magnetic field caused by the current flowing through the conductor. Resistance Rp due to the proximity effect is the resistance caused by the magnetic field created by the current in the current-carrying conductor itself linking with the surrounding conductors, generating eddy currents. The AC resistance R of a coil is the sum of the AC resistance mentioned above and the DC resistance of the copper wire.
number
[0035] (Simulation analysis) Next, a simulation analysis was performed to confirm that winding the magnetic material 3 induces the flow of magnetic flux and reduces AC copper loss. ANSYS Maxwell Ver.18 was used for the analysis. The model used for the analysis had the same configuration as the cross-sectional view of the single-wire coil in Figure 5(a). Table 1 shows the analysis conditions for this coil. [Table 1] The reason for setting the current value at 5A is that the rated current density of normal copper wire is 3A / mm 2 This was applied to the conductor (diameter 1.45 mm) of this embodiment and the comparative example. In the analysis of this embodiment, in order to calculate the frequency characteristics of the coil over a wider range, calculations were performed at frequencies of 50 kHz, 85 kHz, 300 kHz, 500 kHz, and 1 MHz. For the complex relative permeability μ', μ" of the magnetic body 3 (magnetic tape), the actual measured values at each frequency (Figure 7) were used.
[0036] 9(a) and (b) show the magnetic flux distribution obtained by two-dimensional AC magnetic field analysis (simulation). On the right side of each figure, an enlarged view of the coil end area where the influence of the magnetic body 3 is particularly large is shown. At the coil end, the magnetic flux passing between the copper wires of the coil in the comparative example of FIG. 9(a) is induced to the magnetic body 3 in this embodiment. That is, the magnetic flux that interlinked the copper wires is induced to the magnetic body 3, so that the resistance caused by the proximity effect can be reduced. Numerically, at 50 kHz, the AC resistance was reduced by 18.7%, from 40.5 mΩ to 32.9 mΩ. It was also confirmed that the AC resistance at 85 kHz, 300 kHz, 500 kHz, and 1 MHz was reduced by 19.9%, 19.0%, 16.8%, and 11.6%, respectively.
[0037] (Measurement of prototype coil and its results) Coils of the comparative example (COW) and this embodiment (MCW) were actually fabricated to evaluate the effect of reducing AC resistance. The current value during measurement was 20 mA. Figures 10(a) to (c) show the results (measured) of the AC characteristics of coils using the prototype conductor of the comparative example (COW) and the magnetic coated conductor of this embodiment (MCW) measured with an impedance analyzer (Agilent, 4294A). The analytical results (calculated) from the simulation are also overlaid.
[0038] The magnetic body 3 used in this embodiment is in the form of a tape with a thickness of 0.125 mm and a width of 1 cm, and is made of a composite material made by mixing a silicone resin binder with iron-based magnetic powder with a diameter of about 2 μm. The measured values of the relative permeability are shown in Figure 7. The magnetic body 3 is wound in a spiral shape so as to completely cover the surface of the conductor 2. As mentioned above, the insulator 4 is not used in this embodiment.
[0039] Figure 10(a) shows the measured and simulated values of AC resistance R. In the analysis, the lengths of the prototype coil and the conductor were different, so the calculation results were multiplied by 1.06 to correct for the lengths. Both the measured values (solid and dashed lines) and the calculated values (circles and squares) in the figure confirm that the AC resistance tends to increase with increasing frequency. In the actual measurements, the coil resistance decreased by 17.7%, from a maximum of 198 mΩ to 163 mΩ, when the coil resistance was 1 MHz. Furthermore, at 50 kHz, 85 kHz, 300 kHz, and 500 kHz, the AC resistance decreased by 11.7%, 13.9%, 16.9%, and 18.0%, respectively.
[0040] Figure 10(b) shows the results of measurement and analysis of inductance. Both the actual measurement and analysis results were almost constant in the range from 10 kHz to 1 MHz, and the actual measurement value was 6.25 μH for the comparative example (COW) and 6.65 μH for this embodiment (MCW). Covering the surface with magnetic material 3 had the effect of increasing the inductance by 6%.
[0041] Figure 10(c) shows the measured and calculated Q values (equation (2) below). In both cases, it was confirmed that the higher the frequency, the higher the Q value. In addition, in the entire frequency range from 10 kHz to 1 MHz, the Q value of this embodiment (MCW) exceeded that of the comparative example (COW). In particular, at 1 MHz, the measured Q value improved from 196 to 254.
number
[0042] What is noteworthy about the results in Figures 10(a)-(c) is that the numerical values of the analysis results by simulation (shown by squares and circles in the figures) and the numerical values of the actual measurement results (shown by dashed and solid lines in the figures) are relatively consistent. In particular, the relative values (difference between COW and MCW) with and without the magnetic material 3 are almost consistent across the entire frequency range. This result suggests that the magnetic material 3 in the magnetic-material-coated conductor 1 is formed with extremely high precision.
[0043] (Measurement of heat generation frequency characteristics) In order to confirm the effect of the magnetic material 3 on the heat generation of the coil, the temperature rise-time characteristics of the coil and the resistance at thermal saturation were measured. A frequency characteristic analyzer (NF, FRA5097) was used for the measurements. In the measurements, a current of 4A was passed, which is the maximum current of a bipolar power amplifier (NF, HSA4014). The room temperature at the time of the measurements was 24°C.
[0044] Figure 11 shows the environment for measuring the temperature rise vs. frequency characteristics. The coil was placed on a brick wall to prevent the release of heat generated in the coil during measurement. The resonance capacitor was placed on polystyrene foam and cooled with air during measurement so that heat generation from the resonance capacitor could be ignored. A Thermoshot (TEST 855) was used to measure the highest temperature of the coil.
[0045] Figure 12 shows the time-temperature rise characteristics of the coil at each frequency. Figure 12(a) shows the temperature rise when the coil is excited at a frequency of 50 kHz. In the figure, squares and circles represent actual measured values for the comparative example (COW) and this embodiment (MCW), respectively, and the dotted and dashed lines are functional approximations of these. At 50 kHz, both the comparative example (COW) and this embodiment (MCW) quickly reached thermal saturation, and the temperature difference (ΔT) between the comparative example (COW) and this embodiment (MCW) at thermal saturation was 0.9°C. At this time, the AC resistance R decreased by 11.7%, from 58.91 mΩ to 52.04 mΩ.
[0046] Figure 12(b) shows the heat generation characteristics of the coil at 85 kHz. At this frequency, the temperature rose rapidly after the start of measurement and then continued to rise more gradually until it reached thermal saturation. The temperature difference (ΔT) at this point was 3.1°C. At this point, the AC resistance R decreased by 7.7%, from 64.52 mΩ to 59.53 mΩ. Figure 12(c) shows the heat generation characteristics of the coil at 300 kHz. The temperature difference at thermal saturation became even more pronounced, with the temperature difference (ΔT) being 6.7°C. At this point, the AC resistance R decreased by 23.1%, from 178.2 mΩ to 137.1 mΩ.
[0047] Figure 12(d) shows the heat generation characteristics of the coil at 500 kHz. The temperature difference (ΔT) at thermal saturation was 5.5°C. At this time, the AC resistance R reduced by 17.1%, from 328.0 mΩ to 272.0 mΩ. Figure 8(e) shows the heat generation characteristics of the coil at 1 MHz. The greatest reduction in heat generation was observed within the measurement range, with the temperature difference (ΔT) at thermal saturation being 7.8°C. At this time, the resistance R reduced by 24%, from 462.9 mΩ to 351.6 mΩ.
[0048] The above results are summarized in the heat generation characteristics of the coil in Table 2 below. It was confirmed that the magnetic body 3 suppresses heat generation and reduces AC resistance at all frequencies. In addition, the higher the frequency, the greater the effect of reducing AC resistance by the magnetic body 3. It was also confirmed that the reduction in AC resistance also suppresses heat generation. [Table 2]
[0049] Figure 13(a) shows a thermal image of the comparative example (COW) at thermal saturation at a frequency of 50 kHz, and figure 13(b) shows a thermal image of this embodiment (MCW). The coil generated the most heat near the center and near the lead wires, at 28.2°C and 27.3°C, respectively. [Industrial Applicability]
[0050] The present invention can be applied to transformers, inductors, power transmission coils, electromagnetic heating coils, power transmission lines, and any other applications requiring reduction of the skin effect and proximity effect due to AC magnetic fields. [Explanation of symbols]
[0051] 1 Magnetic coated conductor 2 conductors 3 Magnetic material 3a Binder 3b magnetic powder 3c adhesive layer 30 Synthetic Magnetic Tape 4. Insulation
Claims
1. The surface of the conductor is coated with a tape or sheet-like magnetic material containing a binder and magnetic powder, A magnetic-covered conductor in which a tape-shaped insulator is wound in a spiral shape on a surface of the magnetic body at a pitch narrower than the width of the magnetic body, The binder has a thermosetting property, and the insulator has a heat shrink property, A magnetically coated conductor, wherein the magnetic material is evenly fastened, compressed, and solidified toward the center of the conductor by the insulator.
2. The magnetic powder is spherical, and the magnetic body contains magnetic powder whose maximum spherical diameter is 0.05 to 1.0 times the thickness of the magnetic body.
3. 3. The magnetic covered conductor according to claim 1, wherein the magnetic body is a tape-shaped magnetic body having a width narrower than that of the insulator, the tape-shaped magnetic body being wound in a spiral shape.
4. The magnetic covered conductor according to any one of claims 1 to 3, characterized in that the magnetic material has a relative magnetic permeability of 9 to 30.
5. The magnetic coated conductor according to any one of claims 1 to 4, characterized in that the insulator contains a polyethylene terephthalate resin.
6. A process of preparing a conductive wire, a tape- or sheet-shaped magnetic material containing a thermosetting binder and a magnetic powder, and a tape-shaped insulator having heat shrinkability; a process of covering the conductive wire with the magnetic material; a process of spirally winding the insulating material together with the magnetic covering at a pitch smaller than the width of the insulating material; and performing a heat treatment, The manufacturing method of the magnetic coated conductor, in which the heating process is divided into a process of heating the magnetic material until it is solidified to such an extent that the thickness can be maintained, and a process of heating the conductor together with the insulator after the insulator is wound around the conductor.
7. 7. The method for producing a magnetic coated conductor according to claim 6, wherein the process for coating the conductor comprises winding a tape-shaped magnetic material in a spiral shape around the conductor.
8. The method for producing a magnetic covered conductor according to claim 7, characterized in that the magnetic material is laminated to the insulator in advance, and then wound helically around the conductor.
9. 7. The method for producing a magnetic coated conductor according to claim 6, wherein the process of coating the conductor comprises wrapping the tape-shaped magnetic material in parallel with the conductor.
Citation Information
Patent Citations
Cable with magnetic material
JP1986039319A
Production of insulated electric wire for high-frequency coil
JP1987151594A
Radiowave absorbing body
JP1989107598A
Fixing method of electromagnetic interference suppressor
JP1999068378A
Magnetic powder-coated conductor, magnetic powder-coated coil and method for producing the same