High energy barrier dysprosium single ion magnet, its manufacture and use

A stable dysprosium single ion magnet with a triclinic crystal structure and eight-coordinated triangular dodecahedral arrangement is synthesized, addressing synthesis challenges and instability issues, enabling high-density information storage applications with a high energy barrier and blocking temperature.

JP7577286B2Active Publication Date: 2024-11-05JIANGSU UNIV OF SCI & TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023548926
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-04
Filing Date
2022-11-08
Publication Date
2024-11-05
Estimated Expiration
2042-11-08

AI Technical Summary

Technical Problem

Existing dysprosium-based single ion magnets are difficult to synthesize under controlled conditions, have poor reproducibility, and are unstable at room temperature or in air, limiting their application in high-density information storage and quantum computing.

Method used

A dysprosium single ion magnet with a triclinic crystal structure and eight-coordinated triangular dodecahedral arrangement, synthesized using a method involving refluxing DyCl3 in methanol with sodium trimethylsilyloxy and sodium tetraphenylborate, followed by two-phase diffusion, to produce a stable and reproducible magnet with an energy barrier of over 1600K.

Benefits of technology

The synthesized dysprosium single ion magnet exhibits slow relaxation behavior, stable in air, and has a high energy barrier and blocking temperature, suitable for high-density information storage devices like optical and hard disks, with a simple and controllable synthesis process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577286000005
    Figure 0007577286000005
  • Figure 0007577286000006
    Figure 0007577286000006
  • Figure 0007577286000007
    Figure 0007577286000007
Patent Text Reader

Abstract

The present invention discloses a high energy barrier dysprosium single ion magnet, its manufacturing method and use. The single ion magnet has the structural formula [Dy(BPA-TPA)(CH3O)](BPh4)2·CH2Cl2, where BPA-TPA is 2,6-bis(bis(2-pyridylmethyl)amino)methylpyridine. Compared with the prior art, the present invention has the following advantages. (1) The dysprosium single ion magnet of the present invention exhibits typical slow relaxation behavior in zero magnetic field, has the characteristics of a single molecule magnet, has an energy barrier exceeding 1600K, and can be used as a molecular magnetic material in novel high-density information storage devices (e.g., optical disks, hard disks, etc.). (2) The dysprosium single ion magnet does not weather in air and has excellent stability. (3) The method has a safe and simple process, high controllability, and excellent reproducibility.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention belongs to the technical field of magnetic materials, and relates to single-molecule magnet materials, in particular high-energy barrier dysprosium single-ion magnets, their manufacturing methods and uses. [Background technology]

[0002] With the development of information technology, the number of electronic devices integrated is increasing exponentially, while the size of the devices is constantly required to decrease. This progress in integration and miniaturization is limited by processing and cost, which results in intractable problems in the integration technology of modern electronic devices. Therefore, the research and development of molecular-based magnetic materials has become the focus of scientists' attention. Single-molecule magnets (SMMs) are an important field in the research of molecular-based magnetic materials. They also have promising applications in the fields of high-density information storage, quantum computing, and molecular spinology.

[0003] Lanthanide ions are suitable for designing single-ion magnets because they have a large number of single electrons and stronger spin-orbit coupling. Dy(III) has a Kramer electron layer structure (f-layers have an odd number of electrons), so the ground state of dysprosium-based single-ion magnets is a bistable state and does not depend on the equilibrium of the coordination field. Therefore, dysprosium-based single-ion magnets have attracted the attention of many researchers and have already become the optimal single-ion magnet system in terms of performance, with an effective energy barrier and blocking temperature of 1540 cm. -1 The temperature range of the magnets is 80K and the temperature range of the magnets is 80K. However, the synthesis of these high-performance dysprosium-based single-ion magnets requires extreme conditions without water and oxygen, which makes the synthesis process difficult to control, resulting in poor reproducibility and low yield. In addition, some of these materials are unstable at room temperature and in air, and are prone to decomposition and weathering. Summary of the Invention [Problem to be solved by the invention]

[0004] In order to overcome the shortcomings of the prior art, obtain a stable dysprosium complex with excellent single-molecule magnetic properties, and provide a synthesis method with mild, controllable, and highly reproducible synthesis conditions, the present invention provides a high-energy barrier dysprosium single ion magnet, its manufacturing method, and use. [Means for solving the problem]

[0005] A high energy barrier dysprosium single ion magnet, The structural formula of the single ion magnet is [Dy(BPA-TPA)(CH3O)](BPh4)2·CH2Cl2, where BPA-TPA is 2,6-bis(bis(2-pyridylmethyl)amino)methylpyridine, and the chemical structural formula of the single ion magnet is as follows: [ka]

[0006] Preferably, the structural unit of the dysprosium single ion magnet has a crystal of the triclinic system, belongs to the P-1 space group, and has cell parameters of a = 12.7371(3) angstroms, b = 14.2679(4) angstroms, c = 22.1844(6) angstroms, and α = 101.261(2). o , β=93.525(2) o , γ=116.025(2) o It is.

[0007] Preferably, the Dy(III) is coordinated to seven nitrogen atoms and one methoxy group of one BPA-TPA ligand to form an eight-coordinate trigonal dodecahedral arrangement.

[0008] Preferably, the dysprosium single ion magnet is a colorless bulk crystal, exhibits typical slow relaxation behavior at zero magnetic field, and has the characteristics of a single molecule magnet, with an energy barrier exceeding 1600K and a blocking temperature reaching 8K.

[0009] A method for producing the high-energy barrier dysprosium single ion magnet described above, comprising the steps of: The method includes dissolving 2,6-bis(bis(2-pyridylmethyl)amino)methylpyridine (BPA-TPA) and DyCl3·6H2O in methanol, heating and refluxing for 2 hours until a clear yellow solution is obtained, adding sodium trimethylsilyloxy, continuing reflux for 2 hours until a trace amount of yellow precipitate is formed, cooling to room temperature, filtering out traces of insoluble matter, adding sodium tetraphenylborate (NaBPh4) to the solution, stirring for 30 minutes until a large amount of pale yellow precipitate is formed, filtering the precipitate, dissolving it in dichloromethane, transferring it to a test tube, slowly adding n-hexane, allowing it to stand, and allowing it to undergo two-phase diffusion to obtain the dysprosium single ion magnet. Here, the molar ratio of DyCl3·6H2O to BPA-TPA is 1:1-1.5, and 1 mmol of DyCl3·6H2O corresponds to 15-20 mL of methanol, 1-2 mmol of sodium trimethylsilyloxy, 3-5 mmol of sodium tetraphenylborate, and 5-10 mL of dichloromethane.

[0010] Preferably, the volume of the n-hexane is 3 to 4 times that of the dichloromethane.

[0011] Preferably, the standing time is 2 to 4 days to obtain colorless massive crystals.

[0012] 2. Use of the high energy barrier dysprosium single ion magnet according to any one of the preceding claims in the manufacture of molecular-based magnetic materials. Effect of the Invention

[0013] The beneficial effects are as follows: The dysprosium single ion magnet of the present invention exhibits typical slow relaxation behavior in zero magnetic field, has the characteristics of a single molecule magnet, has an energy barrier exceeding 1600K, and can be used as a molecular magnetic material in new high-density information storage devices (e.g., optical disks, hard disks, etc.). (2) The dysprosium single ion magnet does not weather in air and has excellent stability. (3) The method has a safe and simple process, high controllability, and excellent reproducibility. [Brief description of the drawings]

[0014] [Figure 1] Crystal structure of the high-energy barrier dysprosium single ion magnet, [Dy(BPA-TPA)(CH3O)](BPh4)2·CH2Cl2. [Diagram 2] Powder X-ray diffraction pattern of high-energy barrier dysprosium single ion magnet, [Dy(BPA-TPA)(CH3O)](BPh4)2·CH2Cl2. [Diagram 3] This is a DC magnetic susceptibility test diagram for the high-energy barrier dysprosium single ion magnet [Dy(BPA-TPA)(CH3O)](BPh4)2·CH2Cl2. [Figure 4] Hysteresis loop diagram of high-energy barrier dysprosium single ion magnet [Dy(BPA-TPA)(CH3O)](BPh4)2·CH2Cl2. [Diagram 5] This is a graph of the imaginary AC magnetic susceptibility of the high-energy barrier dysprosium single ion magnet, [Dy(BPA-TPA)(CH3O)](BPh4)2·CH2Cl2. [Figure 6] This figure shows the relationship between relaxation time and temperature for the high-energy barrier dysprosium single ion magnet [Dy(BPA-TPA)(CH3O)](BPh4)2·CH2Cl2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The following examples further illustrate the contents of the present invention, but should not be understood as limiting the present invention. Any modifications and substitutions of the methods, steps or conditions of the present invention without departing from the spirit and scope of the present invention are within the scope of the present invention. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art.

[0016] Example 1 The method for producing a high-energy barrier dysprosium single ion magnet includes the steps of dissolving 2,6-bis(bis(2-pyridylmethyl)amino)methylpyridine (BPA-TPA) (1 mmol) and DyCl3·6H2O (1 mmol) in 15 mL of methanol, heating under reflux for 2 h until a clear yellow solution is obtained, adding trimethylsilyloxysodium (2 mmol), continuing reflux for 2 h until a trace amount of yellow precipitate is formed, cooling to room temperature, filtering out traces of insoluble matter, adding NaBPh4 (4 mmol) to the mixture, stirring for 30 min until a large amount of pale yellow precipitate is formed, filtering the precipitate, dissolving the precipitate in 5 mL of dichloromethane, slowly adding 15 mL of n-hexane, allowing to stand, and allowing the mixture to undergo two-phase diffusion for 2 days to obtain the dysprosium single ion magnet. The yield of the dysprosium molecular magnet produced in this example was 66.4%.

[0017] Example 2 The method for producing a high-energy barrier dysprosium single ion magnet includes the steps of dissolving 2,6-bis(bis(2-pyridylmethyl)amino)methylpyridine (BPA-TPA) (1.5 mmol) and DyCl3·6H2O (1 mmol) in 20 mL of methanol, heating under reflux for 2 h until a clear yellow solution is obtained, adding trimethylsilyloxysodium (2.5 mmol), continuing reflux for 2 h until a small amount of yellow precipitate is formed, cooling to room temperature, filtering out a small amount of insoluble matter, adding NaBPh4 (4.5 mmol) to the mixture, stirring for 30 min until a large amount of pale yellow precipitate is formed, filtering the precipitate, dissolving it in 8 mL of dichloromethane, transferring the mixture to a test tube, slowly adding 20 mL of n-hexane, allowing the mixture to stand, and allowing it to undergo two-phase diffusion for 3 days to obtain the dysprosium single ion magnet. The yield of the dysprosium molecular magnet produced in this example was 69.2%. The dysprosium ion magnets produced in this example are characterized as follows. (1) Crystal structure measurement

[0018] A single crystal of suitable size was selected under a microscope and the structure was examined at room temperature on a Bruker SMART Apex II CCD single crystal instrument using a graphite monochromated molybdenum target Mo Kα (λ=0.71073A). Data were collected and the cells were determined using the APEXII program. Normalization and absorption correction were performed on the structural data using the SAINT and SADABS programs. The structure was solved using the SHELXTL-2016 program. All non-hydrogen atom coordinates were obtained by differential Fourier synthesis, and the atomic coordinates and anisotropic temperature factors were corrected using the full matrix least squares method, and all hydrogen atoms were theoretically hydrogenated. The structure diagram is shown in Figure 1, the crystallographic data in Table 1, and the coordination bond lengths in Table 2.

[0019] [Table 1]

[0020] [Table 2]

[0021] As is apparent from the structure diagram in FIG. 1, Dy(III) coordinates to seven nitrogen atoms and one methoxy group of one BPA-TPA ligand, forming an eight-coordinate trigonal dodecahedral arrangement. (2) Measurement of phase purity by powder X-ray diffraction

[0022] The phase purity of the colorless bulk crystal product obtained in this example was characterized using a Bruker D8 Advance powder X-ray diffractometer. As shown in Figure 2, the simulation curve was obtained by simulating the single crystal structure data using Mercury software. As a result, the dysprosium single molecule magnet material has reliable phase purity and is guaranteed for use in molecular magnetic materials. (3) Characterization of magnetic properties

[0023] A superconducting quantum interference meter, Quantum Design MPMS SQUID VSM magnetic measurement system, was used for the magnetic measurements. In the DC magnetic susceptibility test, the temperature was 2.0-300K and the magnetic field was 0.1T. In the magnetization strength test, the temperature was 2-8K and the magnetic field was 0-7T. The frequency range used for the imaginary AC magnetic susceptibility and the real AC magnetic susceptibility was 1-999Hz and the temperature range was 2-60K.

[0024] As shown in Figure 3, when the temperature is 300K, the product of DC susceptibility (χ) and temperature (T) is 14.66 cm 3 Mol -1 K, and spin-only Dy(III) (S=5 / 2, L=5, 6 H 15 / 2 , g=4 / 3), which is the theoretical value of 14.17 cm 3 kmol -1 This product decreases stepwise as the temperature starts to decrease, and when the temperature becomes less than 10K, it starts to decrease rapidly, which is because the system has a significant magnetic anisotropy. From the magnetization intensity curve (Figure 4), this complex shows the properties of a hysteresis loop at 2 to 8K, confirming that this complex has single-molecule magnet properties, and also showing that the blocking temperature of this complex reaches 8K. In the case of zero magnetic field, the imaginary AC susceptibility χ'' of this complex shows significant temperature and frequency dependence in the temperature range of 2 to 60K (Figure 5), resulting in slow magnetic relaxation behavior. When the relaxation time (τ) and temperature (T) are plotted, as shown in Figure 6, the data in the high temperature region are fitted with an Arrhenius fit, and the energy barrier of this dysprosium single ion magnet is 1695K. Taking these phenomena into consideration, the dysprosium single ion magnet produced by the present invention shows typical slow relaxation behavior at zero magnetic field, has the characteristics of a single-molecule magnet, has an energy barrier exceeding 1600K, and a blocking temperature reaching 8K. As a molecular-based magnetic material, it can be used in new high-density information storage devices (eg, optical disks, hard disks, etc.).

Claims

1. A high energy barrier dysprosium single ion magnet, The structural formula of the single ion magnet is [Dy(BPA-TPA)(CH 3 O)](BPh 4 ) 2 ・CH 2 C 2 and BPA-TPA is 2,6-bis(bis(2-pyridylmethyl)amino)methylpyridine.

2. 2. The high energy barrier dysprosium single ion magnet according to claim 1, characterized in that the chemical structural formula of the single ion magnet is: [Case 2]

3. The structural unit of the dysprosium single ion magnet has a crystal of the triclinic system, belongs to the P-1 space group, and has cell parameters of a = 12.7371(3) angstroms, b = 14.2679(4) angstroms, c = 22.1844(6) angstroms, and α = 101.261(2). o , β=93.525(2) o , γ=116.025(2) o 2. The high energy barrier dysprosium single ion magnet according to claim 1, characterized in that

4. The high-energy barrier dysprosium single ion magnet according to claim 1, characterized in that the Dy(III) is coordinated to seven nitrogen atoms and one methoxy group of one BPA-TPA ligand to form an eight-coordinate trigonal dodecahedral arrangement.

5. The high energy barrier dysprosium single ion magnet of claim 1, characterized in that the dysprosium single ion magnet is a colorless bulk crystal, exhibits typical slow relaxation behavior in zero magnetic field, and has the characteristics of a single molecule magnet, with an energy barrier exceeding 1600K and a blocking temperature reaching 8K.

6. A method for producing the high-energy barrier dysprosium single ion magnet according to any one of claims 1 to 5, comprising the steps of: 2,6-Bis(bis(2-pyridylmethyl)amino)methylpyridine and DyCl 3 ・6H 2 A method for producing a high-energy barrier dysprosium single-ion magnet, comprising the steps of: dissolving O in methanol, heating and refluxing until a clear yellow solution is obtained, adding sodium trimethylsilyloxy, continuing reflux until a trace amount of yellow precipitate is formed, cooling to room temperature, filtering and removing trace amounts of insoluble matter, adding sodium tetraphenylborate to the solution, stirring to produce a large amount of pale yellow precipitate, filtering the precipitate, dissolving it in dichloromethane, transferring to a test tube, slowly adding n-hexane, allowing to stand, and allowing it to undergo two-phase diffusion to obtain a dysprosium single-ion magnet.

7. DyCl 3 ・6H 2 The molar ratio of O to BPA-TPA is 1:1 to 1.5, and the amount of DyCl per mmol is 3 ・6H 2 The method for producing a high-energy barrier dysprosium single ion magnet according to claim 6, characterized in that O corresponds to 15-20 mL of methanol, 1-2 mmol of sodium trimethylsilyloxy, 3-5 mmol of sodium tetraphenylborate, and 5-10 mL of dichloromethane.

8. The method for producing a high-energy barrier dysprosium single ion magnet according to claim 6, characterized in that the volume of the n-hexane is 3 to 4 times that of the dichloromethane.

9. The method for producing a high-energy barrier dysprosium single ion magnet according to claim 6, characterized in that the standing time is 2 to 4 days in order to obtain colorless massive crystals.

10. A method for using the high-energy barrier dysprosium single ion magnet according to any one of claims 1 to 5 as a molecular-based magnetic material in a high-density information storage device.

Citation Information

Patent Citations

  • Double-nitroxide-free-radical rare earth metal complex as well as synthetic method and application thereof

    CN103755731A

  • Fluorescence immunoassay chelating agent with pyridine-dipyridine cave-like structure and preparation method of fluorescence immunoassay chelating agent

    CN108892666A

  • Cobalt-based single-ion magnet material and preparation method and application thereof

    CN110790699A

  • Rare earth dysprosium cryptand fluorescent complex and preparation method thereof

    CN112341462A