Energy control coating structures, devices, and methods for producing the same
Hydrogenated metal nitride dielectric layers in multilayer coatings address the challenges of transparency, thermal insulation, and conductivity in window coatings, enhancing performance and stability while reducing costs.
Patent Information
- Application Number
- JP2023112995
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-04-17
- Filing Date
- 2023-07-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2038-04-17
AI Technical Summary
Existing multilayer coatings for windows face challenges in simultaneously achieving high transparency, thermal insulation, and electrical conductivity while maintaining economic viability and stability against oxidation and corrosion.
Incorporation of hydrogenated metal nitride dielectric layers into multilayer metal-dielectric coatings, with controlled hydrogen concentration and spatial profile, to enhance adhesion, reduce percolation thresholds, and improve optical and electrical properties.
The coatings exhibit high transparency, enhanced infrared reflectance, and improved electrical conductivity, offering efficient energy control and resistance to oxidation, while maintaining optical performance and reducing material costs.
Smart Images

Figure 0007577369000001 
Figure 0007577369000002 
Figure 0007577369000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to optical coatings. More particularly, the present disclosure relates to optical coatings for low emissivity or solar control windows. This application claims priority to U.S. Provisional Application No. 62 / 486,351, filed April 17, 2017, entitled "," the entire contents of which are incorporated herein by reference. [Background technology]
[0002] Efficient, reliable and economical devices that can effectively control the flow of light, heat and electrical energy are important to achieve energy efficiency and desired passive and active functions in a variety of applications. Perhaps one of the earliest energy control devices is the Dewar flask, invented by James Dewar. In the Dewar flask, a partially evacuated gap between two flasks (one metal flask enclosing the other, the two connected only at the neck) acts to significantly reduce heat transfer by conduction and convection. This design evolved into the double-walled glass thermos, in which the gap is partially evacuated and the glass walls are coated with a low-emissivity metal film.
[0003] Later, Osram applied a thin film of gold, about 50 nm thick, with an anti-reflective surface coating onto sodium glass lamps, which achieved remarkable visible transparency and reflected thermal radiation back into the lamp, thereby increasing the lamp's energy efficiency. Shortly thereafter, this coating was replaced by a more transparent semiconducting tin oxide film, about 320 nm thick, implemented by Philips. Kostlin then reported the application of a tin oxide coating to the inner surface of double-glazed windows, which significantly reduced radiative heat loss through the window.
[0004] Subsequently, Fan and Bachner reported the synthesis of tin-doped indium oxide and titanium oxide / silver / titanium oxide multilayer metal-dielectric coatings as effective heat mirrors and proposed the application of these and similar coatings for various applications including "solar-to-thermal-to-electrical conversion, solar thermal, photovoltaic conversion, and window insulation." Since the work of Fan and Bachner, the field of metal-dielectric-based spectrally selective coatings has been extensively developed. This has led to the design of a variety of multilayer coatings, including a range of dielectrics and metals, with the aim of achieving modulation across the visible, near-infrared, and mid-infrared portions of the optical electromagnetic spectrum.
[0005] The dielectric layer ranges from metal oxides, metal nitrides, metal oxynitrides, silicon oxide, silicon oxynitride, silicon nitride, silicon carbide, amorphous silicon, and amorphous carbon. With regard to metals, silver is a strong choice when considering optical properties. Other metals are used in a functional manner, such as seed layers to promote adhesion of silver or buffer / blocking layers to protect the silver layer from diffusion of impurities and oxidation.
[0006] Additionally, metal and metal alloy layers are also used as tuning layers to meet, for example, the requirements of transmission and / or reflection color and the requirement of optical performance stability with respect to the need for tempering (heat treatment). Dielectrics are used for purposes other than light modulation, for example, oxygen and moisture protection, and improving adhesion of metals to the underlying substrate. These structures have evolved into numerous multi-layer coatings with the inevitable use of many different materials and different deposition steps. The increasing complexity of design and fabrication poses challenges to effectively and simultaneously address multiple functional requirements while facing the demands of coating economy. Summary of the Invention
[0007] In various exemplary embodiments of the present disclosure, a multilayer metal-dielectric energy control coating is disclosed in which one or more layers are formed from a transparent metal-nitride dielectric. The metal-nitride dielectric can be hydrogenated during or after dielectric deposition. One or more properties of the multilayer coating can be improved or configured by appropriately adjusting the hydrogen concentration (and / or its spatial profile) in one or more of the metal-nitride dielectric layers. One or more metal layers of the multilayer coating may be formed on top of the hydrogenated nitride dielectric layer to facilitate metal adhesion and enable the formation of a thin metal layer that exhibits substantial transparency in the visible spectrum.
[0008] In some exemplary embodiments, hydrogenation of the dielectric layer or post-deposition multilayer coating can be carried out using pure hydrogen gas or multiple gases containing molecular hydrogen (e.g., inert gases (e.g., Ar), or nitrogen, or other gases) at various temperatures and durations. Post-deposition hydrogenation can also be carried out using atomic hydrogen.
[0009] These post-deposition treatments at elevated temperatures can also be used to improve or maintain multilayer coating properties during simultaneous shaping of the substrate (eg, bending of glass, etc.). Additionally, other transparent dielectric layer(s) may also be incorporated as encapsulation layers and / or to improve multilayer coating properties. Furthermore, the optical properties can be tuned through plasmon resonance by engineering nanostructures in the metal film or by incorporating metal nanostructures in the transparent dielectric film. Electrical busbars may be integrated with one or more metal layers to provide functions such as de-icing and defogging.
[0010] Micro / nano thick metal grid lines, invisible to the human eye, can be connected to bus bars without substantial change in optical performance, allowing increased power density levels while operating within the voltage rating of available power sources. Thus, in a first aspect, a metal-dielectric solar control structure is provided, comprising a transparent substrate and a multi-layer metal-dielectric coating formed on the transparent substrate. The multi-layer metal-dielectric coating includes, as a series of layers, a first transparent dielectric layer formed on the transparent substrate, a metal layer formed on the first transparent dielectric layer, and a second transparent dielectric layer formed on the metal layer. At least one of the first transparent dielectric layer and the second transparent dielectric layer is a hydrogenated metal nitride dielectric layer, the metal layer being sufficiently thin and each of the hydrogenated metal nitride dielectric layers comprising an effective hydrogen concentration such that the structure exhibits at least 70% transparency in at least a portion of the visible spectrum.
[0011] In another aspect, a method for producing a metal dielectric coating on a transparent substrate is provided, comprising depositing a first transparent dielectric layer on the transparent substrate, depositing a metal layer on the first transparent dielectric layer such that the metal layer forms a continuous film without the presence of isolated islands, and depositing a second transparent dielectric layer on the metal layer, wherein at least one of the first transparent dielectric layer and the second transparent dielectric layer is a metal nitride dielectric layer, and performing post-deposition hydrogenation such that at least one metal nitride dielectric layer becomes a hydrogenated metal nitride dielectric layer. The thickness of the metal layer and the hydrogen concentration of each of the hydrogenated metal nitride dielectric layers are selected such that the metal dielectric coating exhibits at least 70% transparency in at least a portion of the visible spectrum.
[0012] In another aspect, a method for producing a metal-dielectric coating on a transparent substrate is provided. The method includes depositing a first transparent dielectric layer on the transparent substrate, depositing a metal layer on the first transparent dielectric layer such that the metal layer forms a continuous film without the presence of isolated islands, and depositing a second transparent dielectric layer on the metal layer. At least one of the first transparent dielectric layer and the second transparent dielectric layer is a metal nitride dielectric layer. The method includes performing a post-deposition hydrogenation such that at least one metal nitride dielectric layer becomes a hydrogenated metal nitride dielectric layer. The thickness of the metal layer and the hydrogen concentration of each of the hydrogenated metal nitride dielectric layers are selected such that the metal-dielectric coating exhibits at least 70% transparency in at least a portion of the visible spectrum.
[0013] In another aspect, a metal-dielectric solar control structure is provided that includes a transparent substrate and a multi-layer metal-dielectric coating formed on the transparent substrate, the multi-layer metal-dielectric coating comprising, in order, a first transparent dielectric layer formed on the transparent substrate, a metal layer formed on the first transparent dielectric layer, and a second transparent dielectric layer formed on the metal layer, wherein at least one of the first transparent dielectric layer and the second transparent dielectric layer is a hydrogenated metal nitride dielectric layer. [Brief description of the drawings]
[0014] [Figure 1] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate having a metal layer disposed between uniform dielectric layers. [Diagram 2] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate having an underlying hydrogenated metal nitride dielectric layer. [Diagram 3] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate having an underlying hydrogenated metal nitride dielectric layer having a continuous or quasi-continuously graded hydrogen concentration. [Figure 4] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate having an overlying hydrogenated metal nitride dielectric layer. [Diagram 5] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate having an overlying hydrogenated metal nitride dielectric layer having a continuously or quasi-continuously varying hydrogen concentration. [Figure 6] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate having a metal layer and hydrogenated metal nitride dielectric layers above and below the metal layer. [Figure 7] An exemplary embodiment of a metal-dielectric multilayer coating on a substrate is shown in which hydrogenated metal nitride dielectric layers are provided above and below a metal layer, with each of the hydrogenated metal nitride dielectric layers provided above and below the metal layer having a continuously or quasi-continuously varying hydrogen concentration. [Figure 8] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate that includes two metal layers and a first underlying hydrogenated metal nitride dielectric layer. [Figure 9] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate including two metal layers, a first underlying hydrogenated metal nitride dielectric layer, and a second overlying hydrogenated metal nitride dielectric layer. [Figure 10] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate that includes two thin metal layers and three hydrogenated metal nitride dielectric layers. [Figure 11] An exemplary embodiment of a metal-dielectric multilayer coating on a substrate is shown, comprising two metal layers and three hydrogenated metal nitride dielectric layers, where the intermediate hydrogenated metal nitride dielectric layer has a continuously or quasi-continuously varying hydrogen concentration. [Figure 12] An exemplary embodiment of a metal-dielectric multilayer coating on a substrate is shown, comprising two metal layers and three hydrogenated metal nitride dielectric layers, where the top and middle hydrogenated metal nitride dielectric layers have continuously or quasi-continuously varying hydrogen concentrations. [Figure 13] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate that includes two metal layers and three hydrogenated metal nitride dielectric layers, each of which has a continuously or quasi-continuously varying hydrogen concentration. [Figure 14]1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate including three metal layers, a first underlying hydrogenated metal nitride dielectric layer, and a second overlying hydrogenated metal nitride dielectric layer. [Figure 15] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate that includes three metal layers and four hydrogenated metal nitride dielectric layers. [Figure 16] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate that includes three metal layers and four hydrogenated metal nitride dielectric layers, each of which has a continuously or quasi-continuously varying hydrogen concentration. [Figure 17A] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate in which electrical busbar contacts are integrated onto the metal layer. [Figure 17B] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate in which electrical busbar contacts are integrated onto the metal layer. [Figure 17C] 1 illustrates an exemplary defogging or de-icing system. [Figure 18A] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate comprising two metal layers, with electrical busbar contacts integrated onto each of the metal layers. [Figure 18B] 1 illustrates an exemplary embodiment of a metal-dielectric multilayer coating on a substrate comprising two metal layers, with electrical busbar contacts integrated onto each of the metal layers. [Figure 19] 13 is a plot of measured refractive index versus wavelength dependence for a set of AlN:H films prepared with hydrogen concentrations ranging from approximately 0% to 10% volume fraction. [Figure 20] 13 is a plot of measured absorption coefficient dependence on wavelength for a set of AlN:H films prepared with hydrogen concentrations ranging from approximately 0% to 10% volume fraction. [Figure 21]Shown are scanning electron microscope (SEM) images for AlN films prepared without (A) and with (B) hydrogenation, atomic force microscope (AFM) observation graphs for AlN films prepared without (C) and with (D) hydrogenation, and AFM distribution plots of surface protrusions in the z direction (i.e., vertical direction) for exemplary films (E and F). [Figure 22] 1 shows grazing angle x-ray diffraction profiles of exemplary AlN and AlN:H films. [Diagram 23] 1 is a plot of the transmittance of an exemplary AlN film before and after hydrogenation. [Figure 24] 1 shows plots of optical transmittance and reflectance profiles for an exemplary metal dielectric coating on a 50 μm thick polyethylene terephthalate (PET) film, as well as the optical transmittance and reflectance profiles for an uncoated PET film. [Diagram 25] 1 is a plot of optical transmittance and reflectance profiles for an exemplary metal-dielectric coating on 1.1 mm thick glass. [Figure 26] 1 plots the optical transmittance and reflectance profiles for an exemplary metal-dielectric coating on a 3 mm thick polycarbonate sheet, as well as the profiles for an uncoated polycarbonate sheet. [Figure 27] 1 is a plot of the temperature-time profile of an exemplary metal-dielectric coating on glass exposed to different voltage (and therefore power) levels. [Figure 28] 28A and 28B show the simulated defogging performance of an exemplary metal-dielectric coating on glass, where Fig. 28A plots the dependence of ice sliding time on power density on a slightly inclined glass, and Fig. 28B plots the dependence of energy consumed on power density. [Figure 29A]29A-29C illustrate the simulated fog elimination performance of an example metal-dielectric coating on glass, with FIG. 29A plotting the time dependence of the foggy area as current is applied to the stack. [Figure 29B] 1 shows the simulated spatial dependence of the cloudy area at three different times. [Figure 29C] 1 shows the simulated spatial dependence of the cloudy area at three different times. [Figure 29D] 1 shows the simulated spatial dependence of the cloudy area at three different times. [Figure 30A] At several points (D), optical transmittance curves (A-C) on an exemplary metal-dielectric film are shown, measured at different times after a series of thermal heating and cooling cycles. [Figure 30B] At several points (D), optical transmittance curves (A-C) on an exemplary metal-dielectric film are shown, measured at different times after a series of thermal heating and cooling cycles. [Figure 30C] At several points (D), optical transmittance curves (A-C) on an exemplary metal-dielectric film are shown, measured at different times after a series of thermal heating and cooling cycles. [Figure 30D] At several points (D), optical transmittance curves (A-C) on an exemplary metal-dielectric film are shown, measured at different times after a series of thermal heating and cooling cycles. [Diagram 31] 1 shows a cross-sectional SEM image of an exemplary metal-dielectric coating. [Diagram 32] 1 shows a depth profile from ToF-SIMS of an exemplary metal-dielectric coating. [Diagram 33] 1 shows optical absorption curves of three exemplary metal-dielectric coatings with different silver layer thicknesses. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Various embodiments and aspects of the present disclosure are described with reference to the details discussed below. The following description and drawings are illustrative of the present disclosure and should not be construed as limiting the present disclosure. Numerous specific details are described in order to provide a thorough understanding of various embodiments of the present disclosure. However, in some cases, well-known or conventional details are not described in order to provide a concise discussion of the embodiments of the present disclosure.
[0016] As used herein, the terms "comprises" and "comprising" should be interpreted as inclusive and not limiting. Specifically, as used in this specification and claims, the terms "comprises" and "comprises," and variations thereof, mean that the specified features, steps, or components are included. These terms should not be interpreted to exclude the presence of other features, steps, or components. As used herein, the term "exemplary" means "serving as an example, instance, or illustration," and should not be interpreted as preferred or advantageous over other configurations disclosed herein.
[0017] The terms "about" and "approximately" as used herein are meant to encompass variations that may exist at the upper and lower limits of a range of values, such as variations in properties, parameters, and dimensions. Unless otherwise specified, the terms "about" and "approximately" mean ±25% or less. Unless otherwise stated, any particular range or group is to be understood as a possible way of referring to each and every member of the range or group individually, as well as to any sub-ranges or subgroups contained therein. Unless otherwise stated, the present disclosure relates to and expressly incorporates each and every specific member and combination of subranges or subgroups. As used herein, the term "about," when used in conjunction with a quantity or parameter, refers to a range ranging from about one-tenth to ten times the stated quantity or parameter.
[0018] Referring to FIG. 1, an example of a conventional metal-dielectric multilayer solar control structure is shown. The multilayer structure includes a transparent substrate 10 and a multilayer metal-dielectric coating formed thereon. The multilayer metal-dielectric includes a first (lower) dielectric layer 20, a metal layer 30, and a second (upper) dielectric layer 40. The metal layer 30 is thin enough to allow transmission within the visible spectrum (400-700 nm) while at the same time exhibiting substantial reflectance in the infrared.
[0019] The inventors have discovered that the properties and performance of such metal-dielectric structures may be improved if one or more of the dielectric layers are provided as hydrogenated metal nitride dielectric layers. In various exemplary embodiments of the present disclosure, multi-layer metal-dielectric energy control coatings are disclosed in which one or more layers are formed from a hydrogenated metal nitride dielectric. As described in more detail below, the properties of such multi-layer coatings can be improved or selected by appropriately adjusting the hydrogen concentration (and / or its spatial profile) in one or more hydrogenated metal nitride dielectric layers.
[0020] In some exemplary embodiments, at least one metal layer of a multi-layer coating may be formed on each hydrogenated metal nitride dielectric layer. As described below, hydrogenated metal nitride dielectric layers provide a substrate that facilitates metal adhesion and a low percolation threshold that allows for the formation of thin metal layers that exhibit substantial transparency in the visible spectrum.
[0021] 2, an exemplary embodiment of a multi-layer metal dielectric stack is shown in which one of the dielectric layers is a metal hydride nitride dielectric layer. In the illustrated embodiment, a lower dielectric layer (below metal layer 30) formed on a transparent substrate 10 is provided as a metal hydride nitride dielectric layer 21. A middle metal layer 30 is formed on the metal hydride nitride dielectric layer 21. Above the metal layer 30 is provided an upper dielectric layer 40, which may be a metal hydride nitride dielectric layer.
[0022] The hydrogenated metal nitride dielectric layer may be amorphous, crystalline, or both amorphous and crystalline. Non-limiting examples of hydrogenated metal nitride dielectrics include hydrogenated aluminum nitride, hydrogenated titanium nitride, and hydrogenated titanium aluminum nitride.
[0023] The overlying dielectric layer 40 may be, for example, a metal nitride such as aluminum nitride or titanium nitride or titanium aluminum nitride. The hydrogenated metal nitride dielectric layer may be uniformly hydrogenated, as shown in FIG. 2, or may be hydrogenated to produce a spatially dependent hydrogen concentration, as described in more detail below.
[0024] As described in more detail below, it has been discovered that by controlling the hydrogen content in the metal nitride dielectric layer, it is possible to control, select, and / or optimize the optical, physical and chemical properties of the layer and the overall metal dielectric structure.
[0025] The intermediate metal layer 30 is a metal such as silver. Other suitable metals include, but are not limited to, copper, aluminum, gold, and metal alloys (as used herein, "metal" refers to both elemental metals and metal alloys).
[0026] The substrate 10 can be any suitable transparent dielectric, including, but not limited to, flexible films / foils / sheets, such as polymeric films / foils / sheets formed from materials including polyethylene terephthalate, polycarbonate, polyimide, and polyvinyl butyral (e.g., processed in a roll-to-roll sputter deposition system), and rigid substrates such as polycarbonate and glass sheets (glazing) (e.g., processed in an in-line or shuttle sputter deposition system).
[0027] The thicknesses of the dielectric layers 21 and 40 and the metal layer 30 may be selected to exhibit suitable optical and electrical properties, including, for example, optical properties such as transmittance in the visible, reflectance in the near infrared, and emissivity in the mid infrared, and electrical properties such as, but not limited to, electrical conductivity and sheet resistance. Exemplary thickness ranges for the metal hydride nitride dielectric layers include, but are not limited to, 10 nm to 100 nm. Exemplary thickness ranges for the metal layers include, but are not limited to, 3 nm to 30 nm. In some exemplary embodiments, the layers may be formed by sputter deposition. Such methods may be performed at ambient, near ambient, or low temperatures (e.g., 50° C. to 200° C.). The dielectric layers, including the metal hydride nitride layers, may be deposited by reactive sputtering. For example, an aluminum nitride film may be deposited using reactive sputtering of aluminum with argon and nitrogen sputter gases. Aluminum nitride films with various grain sizes are typically obtained by varying the substrate temperature.
[0028] As described in detail below, various properties of the metal hydride nitride dielectric (e.g., but not limited to, refractive index and extinction coefficient), as well as various aspects of the metal hydride nitrate dielectric's interaction with other layers, such as metal layers and / or transparent substrates (e.g., adhesion, passivation, barrier protection against moisture and / or oxygen), can be controlled, tuned, modulated, selected, or otherwise varied by controlling the addition of hydrogen, such as by controlling the addition of hydrogen gas during reactive sputter deposition, in addition to the usual deposition parameters of power, precursor gas flow rates (typically argon and nitrogen), chamber pressure, and substrate temperature. Additionally or alternatively, the properties of the hydrogenated metal nitride dielectric can be tailored by adding an atomic and / or ionic hydrogen source to the growth surface during the sputter deposition process.
[0029] In yet another embodiment, the properties of the hydrogenated metal nitride dielectric can be tuned after sputter deposition by exposing the layer to an atomic and / or ionic hydrogen source. In an exemplary embodiment including multiple hydrogenated metal nitride dielectric layers, any one or more of the layers can be tailored to perform one or more functions, collectively providing an intentional multi-layer coating.
[0030] In one embodiment, hydrogen is incorporated into the metal nitride dielectric layer during growth by sputtering by supplying hydrogen gas having a concentration in the range of 0.25 vol.% to 2.5 vol.%, or 0.5 vol.% to 5 vol.%, or 0.5 vol.% to 10 vol.%, or 1 vol.% to 10 vol.%, or 0.5 vol.% to 20 vol.%.
[0031] In one embodiment, hydrogen is incorporated into the metal nitride dielectric layer either during or after growth at a concentration ranging from 1 ppm to 1000 ppm, or 1 ppm to 10,000 ppm, or 10 ppm to 10,000 ppm, or 100 ppm to 100,000 ppm by weight.
[0032] As described in the examples provided below, the addition of elemental hydrogen gas having a range of concentrations in a low temperature sputter deposition process has been found to produce a range of hydrogenated aluminum nitride (AlN:H) films exhibiting a corresponding range of physical, chemical and optical properties. In another approach, the addition of atomic and / or ionic hydrogen flux at various levels at the film growth surface equivalently gives rise to a series of hydrogenated aluminum nitride films exhibiting a corresponding range of physical, chemical, and optical properties.
[0033] In yet another approach, exposing aluminum nitride films after deposition to varying levels and ranges of atomic or ionic hydrogen fluxes and varying exposure times produces a series of hydrogenated aluminum nitride films with equivalent and corresponding ranges of physical, chemical, and optical properties.
[0034] In some exemplary embodiments, hydrogenation of the dielectric layer or multilayer coating post-deposition can be carried out at various temperatures and durations using pure hydrogen gas or a gas containing molecular hydrogen (e.g., an inert gas (e.g., Ar), or nitrogen, or other gases). Post-deposition hydrogenation can also be performed with atomic hydrogen. These post-deposition treatments at high temperatures can also be used to improve or maintain multilayer coating properties while simultaneously shaping the substrate (e.g., bending glass).
[0035] Additionally, other transparent dielectric layer(s) may also be incorporated as encapsulation layers and / or to improve multilayer coating properties. In some exemplary embodiments, the hydrogen concentration (in-process concentration, such as the concentration of hydrogen gas, or the post-deposition concentration of hydrogen in the hydrogenated metal nitride dielectric layer) is selected or controlled such that the refractive index of the hydrogenated metal nitride dielectric layer is between about 1.5 and 1.7, or between about 1.6 and 1.8, or between about 1.5 and 1.8, or between about 1.7 and 2.1, or between about 1.6 and 2.1, or between about 1.5 and 2.1 in the visible spectrum.
[0036] In some exemplary embodiments, the hydrogen concentration (either in-process concentration, such as the concentration of hydrogen gas, or the post-deposition concentration of hydrogen in the metal nitride dielectric layer) and the thickness of the metal layer (and optionally the number of metal-dielectric bilayers) deposited on the metal nitride dielectric layer are selected or controlled such that the metal-dielectric structure exhibits a transparency of at least 70%, or at least 75%, or at least 80%, or at least 85% in at least a portion of the visible spectrum.
[0037] In one embodiment, the hydrogen concentration (either an in-process concentration, such as the concentration of hydrogen gas, or a post-deposition concentration of hydrogen in the metal hydride nitride dielectric layer) and the thickness of the metal layer (and optionally the number of metal-dielectric bilayers) deposited on the metal hydride nitride dielectric layer are selected or controlled such that the metal-dielectric structure exhibits at least 70% transparency in at least a portion of the visible spectrum and at least 70% reflectivity in at least a portion of the infrared spectrum.
[0038] In some exemplary embodiments, the hydrogen concentration (either an in-process concentration, such as the concentration of hydrogen gas, or a post-deposition concentration of hydrogen in the hydrogenated metal nitride dielectric layer) is selected or controlled such that the extinction coefficient of the hydrogenated metal nitride dielectric layer is (i) between 0 to 0.15 or 0 to 0.07 for wavelengths between 200 nm and 400 nm, and (ii) between 0 to 0.02 or 0 to 0.05 for wavelengths in the visible spectrum between 400 nm and 700 nm.
[0039] In some exemplary embodiments, the hydrogen concentration (in-process concentration, such as the concentration of hydrogen gas, or the post-deposition concentration of hydrogen in the hydrogenated metal nitride dielectric layer) and the thickness of the metal layer deposited on the hydrogenated metal nitride dielectric layer are selected or controlled such that the resistivity (at room temperature) of the metal layer is between about 2 μΩcm and 6 μΩcm, or between 6 μΩcm and 10 μΩcm, or between 10 μΩcm and 20 μΩcm, or between 2 μΩcm and 20 μΩcm, or between 2 μΩcm and 10 μΩcm.
[0040] In some exemplary embodiments, the hydrogen concentration (either an in-process concentration, such as the concentration of hydrogen gas, or a post-deposition concentration of hydrogen in the hydrogenated metal nitride dielectric layer) is selected or controlled such that the average grain size of the hydrogenated metal nitride dielectric layer is between 30 nm and 100 nm, or between 5 nm and 30 nm, or between 5 nm and 100 nm, or less than 100 nm, less than 30 nm, or 5 nm.
[0041] Furthermore, in certain embodiments, a sufficient process concentration of hydrogen gas is used to produce an amorphous hydrogenated aluminum nitride network that is free of nanocrystallites. In some exemplary embodiments, the hydrogen concentration of the hydrogenated metal nitride dielectric layer (either a process concentration such as the concentration of hydrogen gas or a post-deposition concentration of hydrogen in the hydrogenated metal nitride dielectric layer) is selected or controlled such that the full width at half maximum of the distribution of surface feature / grain protrusion size in the growth direction (i.e., vertical / z direction) is between 3 nm and 5 nm, or between 2 nm and 3 nm, or between 1 nm and 2 nm, or less than 5 nm, less than 4 nm, less than 3 nm, less than 2.5 nm, less than 2 nm, or less than 1 nm.
[0042] The hydrogen concentration of the hydrogenated metal nitride dielectric layer 21 can be selected to promote the growth of a smooth (continuous) metal film such that the metal layer 30 is sufficiently thin to exhibit transmittance in the visible spectrum (e.g., at least 70%, or at least 75%, or at least 80%, or at least 85% transmittance in at least a portion of the visible spectrum) and enhanced electrical conductivity, while being free of isolated islands.
[0043] Thus, in one embodiment, for a given selected metal layer and a given selected metal nitride, the hydrogen concentration can be varied (e.g., indirectly by varying the amount of hydrogen present during the hydrogenation step, such as by varying the volume fraction of hydrogen gas) to identify suitable conditions for the growth of a thin but island-free metal layer. Without intending to be limited by theory, it is believed that the presence of hydrogen in the hydrogenated metal nitride layer is also beneficial in enhancing adhesion between the metal nitride dielectric layer and the transparent substrate 10. Thus, in one embodiment, for a given selected transparent substrate and a given selected metal nitride, the hydrogen concentration can be varied (e.g., indirectly by varying the amount of hydrogen present during the hydrogenation step, e.g., by varying the volume fraction of hydrogen gas) to identify appropriate conditions that achieve sufficient adhesion of the hydrogenated metal nitride dielectric layer to the transparent substrate. Without intending to be limited by theory, it is believed that the hydrogenated metal nitride dielectric can also provide a dense and intimate network with appropriate formation of hydroxides and oxides at the underlying interface between the hydrogenated metal nitride dielectric and the transparent substrate.
[0044] This dense, dense network can therefore act as an effective and robust barrier to the transmission of moisture and oxygen from the underlying transparent substrate, especially in the case of permeable polymeric materials.
[0045] Thus, in one embodiment, for a given selected transparent substrate and a given selected metal nitride, the hydrogen concentration can be varied (e.g., indirectly by varying the amount of hydrogen present during the hydrogenation process, such as by varying the volume fraction of hydrogen gas) to identify appropriate conditions that achieve sufficient barrier protection against moisture and / or oxygen permeation from the transparent substrate.
[0046] It is further noted that the presence of hydrogen at various concentrations during the growth of the metal nitride dielectric layer can provide a variety of potentially beneficial effects. For example, and without intending to be limited by theory, it is believed that the presence of hydrogen during layer formation can provide passivation of atomic scale defects, alteration of grain size, change of physical structure from crystalline to amorphous, alteration of surface properties, and tuning of the chemical environment.
[0047] Some of the implications of these changes include increased optical transmission and reduced extinction coefficients, which can enhance performance in a given optical device design through improved visible transmission, increased infrared reflectance, as well as better transparency neutrality and optical-solar gain.
[0048] The inclusion of hydrogen also leads to a more electrically resistive network, likely the result of passivation of dangling bonds, and a corresponding mitigation of defect-induced charge hopping. For example, this in turn can serve to mitigate Ag island formation and lower the percolation threshold, thereby promoting smoother metal films (e.g., silver).
[0049] In addition, an appropriate level of hydrogenation can also result in enhanced adhesion between the metal layer (e.g., silver) and the dielectric film, as well as between the dielectric film and the underlying substrate. In addition, an appropriate level of hydrogen can also lead to film stress relaxation. Hydrogenation also allows for adjustment of film hardness.
[0050] Yet another example use of the aforementioned exemplary embodiment involves the use of hydrogenated metal nitrides, which provide in-process or post-deposition spectrally selective coatings that offer inherent resistance and stability to oxidation or corrosion of metals (e.g., Ag) after exposure to air through the spontaneous formation of oxynitrides and hydroxides.
[0051] Yet another variation of the aforementioned exemplary embodiment includes a spectrally selective coating in which another transparent dielectric is deposited over the metal dielectric coating to provide additional / secondary encapsulation. Potential transparent dielectrics include, but are not limited to, alkali halides (e.g., MgF2) and other large bandgap ceramics (e.g., nitrides, metal oxynitrides, or hydride metal oxynitrides).
[0052] Yet another variation of the aforementioned exemplary embodiment includes the deposition of transparent dielectric layer(s) or thin (e.g., 0.05 nm to 3 nm) metal layer(s) above and / or below the metal layer to act as encapsulation layer(s) and / or layer(s) that enhance the properties of the multilayer coating. In another exemplary embodiment, the top dielectric layer, if provided as a suitably hydrogenated metal nitride layer, may readily result in the formation of hydroxides and oxides upon exposure to ambient oxygen and moisture.
[0053] Aluminum hydroxide forms readily at active grain boundary sites and, given its larger lattice constant, tends to fill voids in the structure. Aluminum also readily forms native oxides. Thus, the combination of both aluminum oxide and aluminum hydroxide can provide a robust permeation barrier to oxygen and moisture permeation.
[0054] Without intending to be limited by theory, it is believed that hydrogenated metal films can be modified by hydrogen concentration (either during processing, such as the concentration of hydrogen gas, or the post-deposition concentration of hydrogen in the hydrogenated metal layer) resulting in modulation of metal film properties. It is believed that hydrogen can help to passivate active electronic sites, thus improving the conductivity of the network. It is further believed that hydrogen can affect the growth of the metal film, affecting the grain structure and thus its properties.
[0055] Thus, in one embodiment, for a given selected metal layer and a given selected metal nitride, the hydrogen concentration can be varied (e.g., indirectly by varying the amount of hydrogen present during the hydrogenation process, such as by varying the volume fraction of hydrogen gas) to identify suitable conditions for enhanced properties (e.g., optical transmittance, electrical conductivity, etc.) of a thin but island-free metal layer.
[0056] Various embodiments of metal-dielectric multilayer stacks, including those described herein, can be manufactured, for example, in roll-to-roll or in-line / shuttle manufacturing systems. Roll-to-roll systems are typically used to deposit multilayer coatings onto flexible films / foils, while in-line / shuttle systems are typically used to deposit multilayer coatings onto rigid sheets.
[0057] In a roll-to-roll system, the flexible film / substrate is typically of a width, for example the film width is 1.6 m or 2.1 m, the film is on a roll, and the film is of a length, the web length (for example, 1 kilometer or more).
[0058] In an exemplary roll-to-roll manufacturing system, deposition of a metal-dielectric multilayer stack, such as a hydrogenated aluminum nitride-silver-hydrogenated aluminum nitride device, can include three successive deposition zones.
[0059] In the dielectric film deposition zone, RF, DC, pulsed RF, or DC magnetron reactive sputter deposition of hydrogenated aluminum nitride can be performed using various standard techniques of reactive sputter deposition of aluminum nitride, along with introduction / injection of hydrogen in the deposition zone. Alternatively, DC sputtering or low to medium frequency sputtering can be used. In one exemplary configuration, molecular hydrogen gas is introduced / injected at or near the film growth surface where the plasma extending from the aluminum target optimally interacts with the molecular hydrogen, allowing it to dissociate into hydrogen atoms and ions, which then chemically integrate in the growth of the hydrogenated aluminum nitride dielectric film.
[0060] In another exemplary configuration, hydrogen gas is added at an appropriate volume concentration into a sputter gas, such as an argon-nitrogen mixture, to result in reactive sputter deposition of a hydrogenated aluminum nitride film.
[0061] In yet another exemplary configuration, hydrogen is introduced / injected at the film growth surface and added to the sputter gas at an appropriate level to produce a hydrogenated aluminum nitride film.
[0062] In yet another configuration, an atomizer / ionizer is used to introduce / inject atomic and / or ionic hydrogen at or near the growth surface, thereby causing the growth of a hydrogenated aluminum nitride film.
[0063] In the latter configuration, the atomizer / ionizer consists of a hydrogen glow discharge that appropriately supplies / injects atomic and / or ionic hydrogen at or near the film growth surface. The hydrogen glow discharge can be generated using a suitable RF, DC, pulsed or microwave plasma configuration. Similar hydrogen introduction means can be integrated to the metal film deposition zone.
[0064] In one example, within a given deposition zone in a roll-to-roll manufacturing system, hydrogen injectors can be uniformly distributed laterally, i.e., along the web width, to ensure uniformity of the gas / plasma chemistry along the width, thereby contributing to achieving uniformity of the resulting film properties along the entire width of the film.
[0065] Furthermore, in the simplest configuration, an appropriate density of hydrogen injectors can be distributed longitudinally, i.e. along the direction of web movement, to ensure uniform deposition of the hydrogenated aluminum nitride film relative to the deposition zone.
[0066] In an alternative configuration, the hydrogen injector may be longitudinally subdivided into two banks, allowing injection of hydrogen (molecular, or atomic, and / or ionic) at two different concentrations longitudinally, resulting in two quasi-continuous regions of the hydrogenated aluminum nitride film with respect to hydrogen concentration.
[0067] In yet another configuration, the hydrogen injector may be appropriately subdivided to achieve a gradient of hydrogen concentration in the longitudinal direction, thus resulting in a hydrogenated aluminum nitride film having an essentially continuously graded hydrogen concentration. Similar techniques can be used to control the hydrogen concentration in the deposition zone of the metal film and modulate the metal film properties accordingly. In an in-line / shuttle manufacturing system, hydrogen can be introduced using methods similar to those described above to produce the desired modulation in film properties. Furthermore, in an in-line / shuttle manufacturing system, hydrogenation can be performed after deposition.
[0068] For example, a three-layer stack can include depositing aluminum nitride, silver, and aluminum nitride sequentially in a deposition zone, after which the multi-layer stack is treated with a hydrogen-containing gas (e.g., Ar, N2, etc.). Additionally, post-deposition treatments can be performed at elevated temperatures to improve the properties of the multi-layer coating. Additionally, the temperature can be increased to a sufficiently high level to achieve substrate shaping (e.g., bending of glass) while maintaining or improving the coating properties.
[0069] An exemplary gas is a forming gas containing primarily nitrogen with a small concentration of hydrogen, where the presence of nitrogen can also serve to "heal" or "repair" any defects in the aluminum nitride film, while the hydrogen can serve to passivate dangling bonds during the entire process as well as provide a reducing environment to reduce or eliminate any oxidation of the metal and dielectric films.
[0070] In some exemplary embodiments described below, the metal film deposited on the hydrogenated metal nitride dielectric layer may be patterned. In one example to facilitate such patterning, a laser ablation subsystem is integrated within the roll-to-roll manufacturing system, for example, after the Ag deposition zone but before the subsequent dielectric film deposition zone, i.e., in the vacuum curtain wall separating the two deposition zones.
[0071] Additionally, the laser system can output ultrashort picosecond or femtosecond laser pulses such that interaction between the laser optical field and the metal layer (e.g., Ag) results in the emission of an atomic / ion plasma plume without substantial heating of the underlying layer. These processes, along with a laser beam output control system such as a computer-controlled galvo scanner, allow for the creation of patterned silver such as nanometer, micrometer, or millimeter scale apertures to produce specific electromagnetic transmission / reflection properties (such as providing transmission over a specific band of microwave frequencies) or to generate specific radio frequency transceiver functionality.
[0072] In some exemplary embodiments described below, the fabrication process can be adapted such that the multilayer metal-dielectric device exhibits one or more plasmonic absorption peaks (e.g., one or more peaks in its optical absorption spectrum). Such plasmonic absorption features can be used, for example, to modify the optical properties of the metal-dielectric multilayer device for purposes including, but not limited to, visible color change and UV protection. Plasmonic features can be introduced by incorporating metal nanostructures into the multilayer metal-dielectric device. For example, plasmonic absorption can be introduced by creating nanoscale roughness (0.1 nm to 30 nm RMS roughness) in the metal film, which results in the creation of metal nanostructures.
[0073] Such roughness may be generated, for example, by (i) varying the roughness of the underlying dielectric layer, which can be altered by sputter deposition rate and sputter gas chemistry, (ii) by altering the growth characteristics of the metal film by varying the sputter deposition rate and sputter gas chemistry, or (iii) by atomic / ion bombardment of the dielectric or metal layer.
[0074] In another exemplary embodiment, the metal nanoparticles are, for example, (i) Varying the thickness of the metal film (ii) changing the dielectric chemistry, for example by hydrogenation, thereby promoting diffusion and aggregation of metal atoms; (iii) performing nanoparticle deposition simultaneously with the dielectric film deposition, for example by spraying metal nanoparticles or using a sputter-based process where the metal atoms can condense into nanoparticles before impacting the growth surface; It can be incorporated into a transparent dielectric layer by
[0075] In some exemplary embodiments, the range of wavelengths and / or the strength of the plasmonic absorption can be controlled. For example, in examples where one or more plasmonic features are provided via roughness in a metal film, the wavelength and / or strength of the plasmonic features may be varied by controlling the amount of roughness introduced.
[0076] Alternatively, in an exemplary embodiment in which one or more plasmonic features are provided through the incorporation of metal nanoparticles into a transparent dielectric layer, the wavelength and / or intensity of the plasmonic feature may be varied by controlling the dispersion of the metal nanoparticles.
[0077] The various exemplary embodiments disclosed herein may be used in a wide range of applications and may be used, for example, as passive or active devices. Various metal-dielectric structures and variations thereof disclosed herein include, but are not limited to, A spectrally selective coating including a transparent heat mirror and a transparent solar control coating. A spectrally selective resistive heater including a transparent heat mirror and a transparent solar control coating that simultaneously provides a transparent heat mirror and a transparent solar control coating. Spectrally selective resistive heaters that act as transparent heat mirrors and transparent solar control coatings and are used as highly efficient defrosters and defoggers in automotive, aerospace, marine and related applications. Spectrally selective radiative cooling coatings; transparent conductors; nearly invisible radio transceivers and transmitters Near-invisible radio frequency energy harvester It may also be used for other purposes.
[0078] The following description discloses a set of exemplary embodiments of different structural configurations of metal-dielectric structures, including different layer configurations and combinations that use one or more hydrogenated metal nitride dielectric layers.
[0079] 3, another exemplary embodiment of a metal-dielectric stack is shown in which the underlying dielectric layer 22 is quasi-continuously or continuously graded in hydrogen concentration to locally enhance film properties in response to interface and bulk requirements. As shown, the concentration is graded in a direction parallel to the surface normal associated with the transparent substrate 10. Specifically, at the underlying dielectric film-substrate interface, the hydrogen concentration is selected for adhesion and permeation barrier, while at the underlying dielectric film-metal film interface, the hydrogen concentration is selected for adhesion and smoothness of the metal film, as well as suitable electrical and optical properties.
[0080] In another embodiment of the metal dielectric stack shown in Figure 4, the lower dielectric 20 is a metal nitride dielectric film and the upper dielectric layer 41 is a hydrogenated metal nitride film, while the intermediate layer 30 is a metal film. Layer 41 is suitably hydrogenated to support the formation of hydroxides and oxides upon exposure to air to achieve a dense network that acts as an effective and robust barrier to oxygen and moisture penetration.
[0081] Additionally, the film may be appropriately hydrogenated to enhance or tailor the optical properties to provide desired optical performance, including clear-neutrality and optical-solar gain. The overlying dielectric film 41 also provides a dense and robust hydrogenated network over the underlying metal film.
[0082] In an alternative embodiment of the metal-dielectric stack shown in FIG. 5, the top dielectric 42 is quasi-continuously or continuously graded in hydrogen concentration to locally enhance film properties in response to appropriate interface and bulk requirements. Specifically, at the top dielectric film-metal film interface, the hydrogen concentration is selected for adhesion of the top dielectric film to the metal film, while at the top dielectric film-air interface, the hydrogen concentration is selected to promote a dense and robust network and chemical composition for the formation of a robust native hydroxide and oxide barrier layer. The film may also be appropriately hydrogenated to enhance or tune optical properties, thereby providing desired optical performance, including transparency neutral and optical-solar gain.
[0083] In another embodiment of the metal-dielectric stack shown in Figure 6, the underlying dielectric 21 and the overlying dielectric layer 41 are hydrogenated metal nitride dielectric films, while the intermediate layer 30 is a metal film. Layer 21 may be appropriately hydrogenated to support enhanced adhesion with the underlying substrate and to promote overtop non-island smooth Ag film growth. The underlying layer also provides a dense and robust network with appropriate formation of hydroxides and oxides at the dielectric-substrate interface, which acts as an effective and robust barrier against moisture and oxygen permeation from the underlying substrate, especially in the case of permeable polymeric materials.
[0084] Layer 41 may be suitably hydrogenated to favor the formation of hydroxides and oxides upon exposure to air to achieve a dense, strong network that acts as an effective and strong barrier to oxygen and moisture penetration. Additionally, the film may be suitably hydrogenated to enhance or adjust the optical properties to provide desired optical performance, including transparency neutral and optical-solar gain. The film also provides a dense, strong hydrogenated network in contact with the underlying metal film.
[0085] In an alternative embodiment of the metal-dielectric stack shown in Figure 7, the lower dielectric 22 and upper dielectric 42 are quasi-continuously or continuously graded in hydrogen concentration to locally enhance film properties in response to interfacial as well as bulk requirements. Specifically, at the upper dielectric film-metal film interface, the hydrogen concentration is selected for adhesion of the upper dielectric film to the metal film, while at the upper dielectric film-air interface, the hydrogen concentration is selected to promote a dense and robust network and chemical composition for the formation of robust native hydroxide and oxide barrier layers.
[0086] In contrast, at the underlying dielectric film-substrate interface, the hydrogen concentration is selected for adhesion and permeation barrier, while at the underlying dielectric film-metal film interface, the hydrogen concentration is selected for metal film adhesion and smoothness as well as suitable electrical and optical properties. Additionally, the two dielectric films may also be appropriately hydrogenated to enhance or modulate the optical properties, thereby providing desired optical performance, including transparent neutral and optical-solar gain.
[0087] Another exemplary embodiment of a metal-dielectric multilayer stack is shown in Figure 8, where 21 is a first lower dielectric layer, 30 is a first metal layer, 40 is a first upper dielectric layer and a second lower dielectric layer, 50 is a second metal layer, and 60 is a second upper dielectric layer. The multilayer structure is provided on a substrate 10.
[0088] The first underlying dielectric layer 21 is a metal nitride hydride such as hydrogenated aluminum nitride or hydrogenated titanium nitride or hydrogenated titanium aluminum nitride, and the dielectric layer 20 is a metal nitride dielectric layer such as aluminum nitride or titanium nitride or titanium aluminum nitride, while the intermediate metal layer 30 is a metal film such as silver. The thicknesses of the dielectric layers 21, 40 and 60 and the silver layers 30 and 50 are selected (suitably selected) to achieve the desired optical and electrical properties, including but not limited to optical properties such as transmittance in the visible, reflectance in the near infrared, and emissivity in the mid infrared, and electrical properties such as electrical conductivity and sheet resistance.
[0089] In an alternative embodiment of a metal dielectric stack shown in Figure 9, 21 is a first lower dielectric layer, 30 is a first metal layer, 40 are a first upper dielectric layer and a second lower dielectric layer, 50 is a second metal layer, and 61 is a second upper dielectric layer. The multi-layer structure is overlying a substrate 10. The first lower dielectric layer 21 and the second upper dielectric layer 61 are hydrogenated.
[0090] In another alternative embodiment of the metal-dielectric stack shown in Fig. 10, 21 is a first lower dielectric layer, 30 is a first metal layer, 41 are a first upper and second lower dielectric layer, 50 is a second metal layer, and 61 is a second upper dielectric layer. The multi-layer structure is provided on a substrate 10. The first lower dielectric layer 21, the first upper and second lower dielectric layers 41, and the second upper dielectric layer 61 are hydrogenated.
[0091] In another alternative embodiment of the metal-dielectric stack shown in Fig. 11, 21 is a first lower dielectric layer, 30 is a first metal layer, 42 is a first upper dielectric layer and a second lower dielectric layer, 50 is a second metal layer, and 61 is a second upper dielectric layer. The multilayer structure is provided on a substrate 10. The first lower dielectric layer 21 and the second upper dielectric layer 61 are hydrogenated, while the first upper dielectric layer and the second lower dielectric layer 42 are quasi-continuously or continuously graded in hydrogen concentration, thereby locally enhancing the film properties in response to interface as well as bulk requirements.
[0092] In another alternative embodiment of a metal dielectric stack shown in Figure 12, 21 is a first lower dielectric layer, 30 is a first metal layer, 42 is a first upper dielectric layer and a second lower dielectric layer, 50 is a second metal layer, and 62 is a second upper dielectric layer. The multi-layer structure is provided on a substrate 10.
[0093] The first underlying dielectric layer 21 is hydrogenated, while the first underlying dielectric layer and the second underlying dielectric layer 42 and the second underlying dielectric layer 62 are quasi-continuously or continuously graded in hydrogen concentration to locally enhance film properties in response to interface as well as bulk requirements.
[0094] In another alternative embodiment of a metal dielectric stack shown in Figure 13, 22 is a first lower dielectric layer, 30 is a first metal layer, 42 is a first upper dielectric layer and a second lower dielectric layer, 50 is a second metal layer, and 62 is a second upper dielectric layer. The multi-layer structure is provided on a substrate 10.
[0095] The first underlying dielectric layer 22, the first underlying dielectric layer 42, and the second underlying dielectric layer 62 have a quasi-continuous or continuous gradient in hydrogen concentration to locally enhance film properties in response to interface as well as bulk requirements.
[0096] Another exemplary embodiment of a metal-dielectric multilayer stack is shown in Figure 14. In Figure 14, 21 is a first lower dielectric layer, 30 is a first metal layer, 40 is a first upper dielectric layer and a second lower dielectric layer, 50 is a second metal layer, 60 is a second upper dielectric layer, a third lower dielectric layer, 70 is a third metal layer, and 81 is a third upper dielectric layer. The multilayer structure is provided on a substrate 10.
[0097] The first lower dielectric layer 21 and the third upper dielectric layer 81 are metal hydride nitrides such as hydrogenated aluminum nitride or hydrogenated titanium nitride or hydrogenated titanium aluminum nitride, while the dielectric layers 40 and 60 are metal nitrides such as aluminum nitride or titanium nitride or titanium aluminum nitride, while the intermediate metal layers 30, 50 and 70 are metal films such as silver. The thicknesses of the dielectric layers 21, 40, 60 and 81 and the metal layers 30, 50 and 70 can be selected (suitably adjusted) to achieve desired optical and electrical properties. The optical and electrical properties include, but are not limited to, optical properties such as transmittance in the visible, reflectance in the near infrared, and emissivity in the mid infrared, among others, and electrical properties such as electrical conductivity and sheet resistance.
[0098] In an alternative embodiment of a metal dielectric multilayer stack shown in Figure 15, 21 is a first lower dielectric layer, 30 is a first metal layer, 41 is a first upper dielectric layer and a second lower dielectric layer, 50 is a second metal layer, 61 is a second upper dielectric layer and a third lower dielectric layer, 70 is a third metal layer, and 81 is a third upper dielectric layer. The multilayer structure is provided on a substrate 10.
[0099] The dielectric layers 21, 41, 61, 81 are hydrided metal nitrides and the intermediate metal layers 30, 50, 70 are metal films such as silver. The thicknesses of the dielectric layers 21, 40, 60 and 81 and the metal layers 30, 50 and 70 are appropriately adjusted to achieve desired optical and electrical properties, including but not limited to optical properties such as transmittance in the visible, reflectance in the near infrared, and emissivity in the mid infrared, and electrical properties such as electrical conductivity and sheet resistance.
[0100] In another alternative embodiment of a metal dielectric multilayer stack shown in Figure 16, 22 is a first lower dielectric layer, 30 is a first metal layer, 42 is a first upper dielectric layer and a second lower dielectric layer, 50 is a second metal layer, 62 is a second upper dielectric layer and a third lower dielectric layer, 70 is a third metal layer, and 82 is a third upper dielectric layer. The multilayer structure is provided on a substrate 10.
[0101] The dielectric layers 22, 42, 62 and 82 are quasi-continuously or continuously graded in hydrogen concentration to locally enhance film properties for interface and bulk requirements. The thicknesses of the dielectric layers 22, 42, 62 and 82 and the metal layers 30, 50 and 70 can be selected (suitably adjusted) to achieve desired optical and electrical properties, particularly optical properties such as transmittance in the visible, reflectance in the near infrared, and emissivity in the mid infrared, and electrical properties such as, but not limited to, electrical conductivity and sheet resistance.
[0102] Another exemplary embodiment of a metal-dielectric multilayer stack is shown in Figures 17A and 17B. In Figures 17A and 17B, the stack includes an underlying dielectric layer 21, a metal layer 30, and a dielectric layer 41. The multilayer structure is provided on a substrate 10. The dielectric layers 21 and 41 are hydrogenated metal nitrides such as AlN:H, and layer 30 is a metal such as silver.
[0103] Electrical busbar contacts 100 and 110 make ohmic contact with metal layer 30, the busbars being spaced apart to facilitate the output of power to metal-dielectric device 90 (plan view AA'), with arrows pointing from right to left indicating the direction of current flow (i.e., positive charge flow). Electrical busbars 100 and 110 of appropriate thickness can be integrated into the metal-dielectric device by depositing the metal contacts using a variety of methods, including, but not limited to, electron beam evaporation of metals and metal alloys, sputter deposition of metals and metal alloys, and printing of metal inks and pastes with associated etching and firing steps.
[0104] FIG. 17C shows an example of a demisting or de-icing system including a windshield having a solar control structure 90 having at least one hydrogenated metal nitride dielectric layer according to the above-described embodiments, and electrical bus bars 100, 110 in electrical communication with at least one metal layer formed within the structure.
[0105] The system also includes a power source 430 and a control circuit 400 for controlling the current provided to the solar control structure. The control circuit 400 may be programmed with instructions stored in memory 415 and executable by the processor 410 to provide a time-dependent current to the solar control structure (as shown diagrammatically by the demisting / de-icing module 450). For example, the control circuit may provide a current continuously or intermittently for a duration suitable for demisting and / or de-icing, optionally according to a predetermined time dependency. The control circuit may further be connected to one or more sensors 420 for sensing the presence of ice or fog.
[0106] As shown in the exemplary embodiment depicted in FIG. 17C, the control circuitry 400 may include a processor 410, a memory 415, a system bus 405, and one or more optional additional devices. It should be understood that the exemplary system depicted in the figure is not intended to be limited to the components that may be used in a given implementation. For example, the system may include one or more additional processors. Additionally, one or more components of the control and processing hardware 400 may be provided as external components interfaced to a processing device. Another exemplary embodiment of a metal-dielectric multilayer stack is shown in Figures 18A and 18B, in which the stack includes a dielectric layer 21, a metal layer 30, a dielectric layer 41, a metal layer 50, and a dielectric layer 61. The multilayer structure is provided on a substrate 10.
[0107] Dielectric layers 21, 41 and 61 are hydrogenated metal nitrides such as AlN:H, and layers 30 and 50 are metals such as silver. Electrical busbar contacts 130 and 140 make ohmic contact with metal layers 30 and 50, the busbars being spaced apart to facilitate the output of power to metal-dielectric device 120 (plan view BB', arrows pointing from right to left indicate the direction of current flow (i.e., flow of positive charge).
[0108] Electrical bus bars 130 and 140 of appropriate thickness can be integrated into metal dielectric devices by depositing metal contacts using a variety of methods, including but not limited to electron beam evaporation of metals and metal alloys, sputter deposition of metals and metal alloys, and printing of metal inks and pastes with associated etching and firing steps.
[0109] In another embodiment, electrical bus bars are deposited, printed or fixed directly onto the dielectric (e.g., onto dielectric layer 40 in FIG. 1 or onto dielectric layer 41 in FIG. 4). Metal bus bars may be e-beam or sputter deposited directly onto the dielectric, the bus bars may be printed using a metallic ink (e.g., silver ink), or metal ribbons may be fixed with a suitable conductive adhesive-epoxy. These contacts may also be appropriately heat treated-sintered to achieve good ohmic contact.
[0110] Alternatively, the resistive properties of the dielectric can be reduced by using plasma discharge to locally strip the dielectric during ink printing. Additionally, laser processing can be utilized, for example, a laser ablation process can be used to achieve selective release of the dielectric, and various methods of laser printing of metals can be used, for example, laser induced forward transfer.
[0111] In yet another embodiment, silver migration into the dielectric, Ag nanoparticles diffusing from an underlying Ag layer into the overlying dielectric as shown in FIG. 31, can be utilized in conjunction with silver diffusion from a deposited / printed silver grid on the dielectric, resulting in high quality ohmic contact. Localized thermal / optical treatments can be used simultaneously to achieve optimal silver migration and therefore low contact resistance. In addition to the use of electrical bus bars, suitable micro-nano thin electrical grids can also be utilized, where the grid connected to the bus bar facilitates the required power density while allowing lower voltage operation. The grid can be applied in a similar manner to the bus bar described in the previous paragraph, but with dimensions that are not detectable by the human eye. For example, multiple micro-nanometer thin conductive wires can be utilized.
[0112] It will be understood that the above exemplary embodiments are provided to illustrate a non-limiting set of exemplary embodiments and applications of multi-layer metal-dielectric structures with one or more hydrogenated metal nitride dielectric layers, and that multiple other potential embodiments are possible. For example, in some implementations, the spectrally selective metal-dielectric multi-layer stack can be appropriately patterned, thereby integrating other functions. For example, these can include appropriate aperture patterning of metal layers (on nanometer, micrometer, and millimeter length scales) by providing selective reflectivity and transmittance properties in the RF frequency range, and these patterns can be on single or multiple metal layers.
[0113] Yet another example includes the integration of RF electromagnetic radiation harvesting by suitable antenna patterning and subsequent rectification, which can power a suitable sensor, thus resulting in a self-powered sensor. Various exemplary embodiments, in addition to the mentioned functionality, can result in the formation of an ultra-smart window for a given enclosure / system.
[0114] Another exemplary use of the aforementioned exemplary embodiment includes the use of tunable hydrogenated metal nitrides such as AlN:H in the design of a spectrally selective radiative cooling coating device, in which the visible and near infrared portions of the electromagnetic spectrum are almost completely reflected while a mid-infrared transparency window spanning, for example, the 8-13 μm range is provided, allowing radiative heat energy to be emitted from a given volume towards a cooler outside space, thus producing radiative cooling. As an example, a photonic crystal cooling device can be constructed from various photonic crystal layers, and a broadband solar reflector comprising a bilayer of low and high refractive index large band gap materials on a silver substrate utilizes hydrogenated nitrides.
[0115] [Example] The following examples are presented to enable those skilled in the art to understand and practice embodiments of the present disclosure, but should not be considered as limiting the scope of the disclosure, but merely as being illustrative and representative thereof.
[0116] (Example 1: Dependence of refractive index and extinction coefficient on hydrogen concentration of hydrogenated AlN film) Figure 19 shows an exemplary data set of optical indices as a function of wavelength for AlN:H films deposited using RF reactive sputtering on glass substrates with hydrogen concentrations ranging from approximately 0% to 10% volume fraction during sputtering. The primary sputter gases consist of argon and nitrogen. These films deposited using reactive RF sputtering are prepared in a cryogenically pumped multi-target sputtering chamber with a nominal total gas flow rate of 20 sccm. Here, the argon flow rate is 15 sccm, the nitrogen flow rate is 5 sccm, and the hydrogen flow rate is 0-10 sccm.
[0117] Argon was introduced near the aluminum target, and nitrogen and hydrogen were introduced near the growth surface. The chamber pressure during deposition was nominally 5 mTorr. RF power ranged from 150 to 350 W. The substrate was initially at ambient temperature and was not actively heated or cooled. Figure 20 shows the corresponding data set for the extinction coefficient of the AlN:H film.
[0118] The change in precursor hydrogen content apparently serves to tune the optical index of refraction. Furthermore, it is observed that the introduction of hydrogen causes a decrease in the extinction coefficient of the dielectric film over a range of optical wavelengths. The decrease in the extinction coefficient is due to hydrogen bonding at atomic-scale defect sites. The change in optical index is a function of hydrogen bonding and also a function of the modulation of the film's physical structure-grain size.
[0119] (Example 2: Morphology and grain size of hydrogenated AlN film) Figure 21 (A-F) shows the scanning electron microscope (SEM) and atomic force microscope (AFM) observation graphs of examples of AlN and AlN:H films deposited on glass, as well as the distribution of surface features / grain protrusions / heights in the Z (vertical) direction. Hydrogenation of aluminum nitride obviously reduces the grain size (see Figures 21A and 21B showing the SEM observation graphs of AlN and AlN:H films), resulting in smoother films. The average grain size and standard deviation of the AlN film is 48.6±9 nm, and that of the AlN:H film is 25.4±9 nm. The surface roughness of the films is observed by AFM scans (see Figures 21C and 21D showing the AFM scans of the AlN and AlN:H film surfaces, respectively).
[0120] Additionally, the distribution of surface feature / particle protrusion / height in the Z direction is shown in Figures 21E and 21F. In Figure 21E, the AlN:H film has a narrow distribution with a full width at half maximum (FWHM) of about 2.2 nm. The AlN film has a FWHM of about 3.6 nm. In Figure 21F, the distributions for another example of AlN and a set of AlN:H films show FWHMs of about 2.5 nm and about 1.4 nm, respectively.
[0121] (Example 3: Small angle X-ray diffraction (XRD) test of hydrogenated AlN film) FIG. 22 shows three small angle X-ray diffraction (XRD) patterns, one for AlN and two for AlN:H films, deposited using RF reactive sputtering on Si(100). The AlN:H films were grown with 1.25% and 2.5% volume fractions of hydrogen in the precursor gas flow. The top XRD scan shows the diffraction pattern for AlN, while the second and third XRD scans show the diffraction patterns for AlN:H grown using 1.25% and 2.5% hydrogen, respectively. It is observed that the characteristic crystalline peaks / line intensities decrease as hydrogen is increased and the films exhibit increasingly amorphous character.
[0122] Example 4: Hydrogenation during and after film deposition Figure 23 shows that the optical transmittance of AlN can be similarly enhanced by post-deposition hydrogenation. Specifically, an example AlN film deposited on glass is exposed to an RF hydrogen plasma. The optical transmittance of the AlN film before and after hydrogenation (referred to as HAlN) shows that the optical transmittance of the film is improved over a range of optical wavelengths.
[0123] Example 5: Measurement of optical properties of metal-dielectric stacks with and without hydrogenation The optical properties of an exemplary metal-dielectric multilayer stack, including a bottom dielectric layer, a middle metal layer, and a top dielectric layer, are shown in FIG. 24. The metal-dielectric stack is deposited using sputter deposition. The dielectric layers are hydrogenated aluminum nitride and the metal layers are silver. The substrate is a polyethylene terephthalate (PET) film. The transmission and reflection curves of bare and coated PET films are shown in the figure. The peak transmission in the visible is 86%, the photopic weighted visible transmission is 85%, and the total solar energy rejection is 35%. The discontinuity in the transmission curve around 900 nm is the detector shift.
[0124] The optical properties of another exemplary metal-dielectric multilayer stack, including a first lower dielectric layer, a first metal layer, a first upper and second lower dielectric layers, a second metal layer, and a second upper dielectric layer, are shown in FIG. 25. The metal-dielectric stack is deposited using sputter deposition. The dielectric layers are hydrogenated aluminum nitride, the metal layers are silver, and the substrate is glass. The transmission and reflection curves of the coated glass are shown in the figure. The peak transmittance in the visible light is 77%, the photopic weighted visible transmittance is 76%, and the total solar energy rejection is 47%. The color parameters of the coated glass are L*=90.10, a*==-0.55, and b*=0.63. The discontinuity in the transmittance curve around 900 nm is the detector shift.
[0125] The optical properties of another exemplary metal-dielectric multilayer stack, including a first lower dielectric layer, a first metal layer, a first upper and second lower dielectric layers, a second metal layer, and a second upper dielectric layer, are shown in FIG. 26. The metal-dielectric stack is deposited using sputter deposition. The dielectric layers are hydrogenated aluminum nitride and the metal layers are silver. The substrate is a polycarbonate sheet. The transmission and reflection curves of the polycarbonate sheet are shown in the figure. The peak transmittance in visible light is 71%, the photopic weighted visible transmittance is 70%, and the total solar energy rejection is 49%. The color parameters of the coated polycarbonate are L*=87.04, a*=-1.48, and b*=1.42, and the color parameters of the uncoated polycarbonate are L*=90.9, a*=-0.52, and b*=0.50.
[0126] Example 6: Experimental study of the performance of metal-dielectric devices with hydrogenated AlN layers for de-icing and defogging applications The heating performance of an exemplary metal-dielectric multilayer stack is shown in Figure 27. The multilayer stack is deposited on a glass substrate. Electrical bus bars in contact with the metal layers are connected to a variable power supply. Profiles of temperature change as a function of time are shown for various power levels. Temperature is measured at the opposite glass surface.
[0127] The defrosting performance of an exemplary metal-dielectric multilayer stack is shown in Figure 28(A,B). The multilayer stack is deposited on a glass substrate, and electrical bus bars in contact with the metal layers in the stack are connected to a variable power source. A sheet of ice approximately 1 mm thick is frozen directly onto the uncoated side of the glass substrate.
[0128] At a typical room temperature of about -10°C, power is applied to the stack and the time required to remove ice from the glass surface is recorded for various power levels. Upon sufficiently uniform power output to the glass-ice interface, a thin molten layer of water develops at the interface (i.e., the entire surface of the interface), leading to sliding of the ice sheet. Here, the "time to slide" is defined as the length of time between power application and the final sliding of the ice sheet.
[0129] FIG. 28A shows the sliding time as a function of power density. Direct and uniform application of high power density over the entire ice-covered area results in rapid freeing of the sample surface from the ice (as de-icing is very fast) without requiring complete melting of the ice and without losing heat to the surroundings. This leads to significant energy savings. FIG. 28B shows that there is a minimum energy required to free the ice surface. This figure also includes the voltage and current required for equivalent defrosting on a full-scale standard vehicle windshield of approximately 0.7 m by 1.4 m.
[0130] The projected defogging performance of an exemplary metal-dielectric coating is shown in Figure 29 (A-D). The device structure is similar to that described above. Using a benchmarked full-convection COMSOL Multiphysics model, the percentage of an exemplary coated glass surface covered with fog as a function of time is shown in Figure 29A. Power to the coating is turned on at time zero. Figures 29B-D show two-dimensional maps of the defogging pattern at different times (times 0, 2 seconds, and 2.5 seconds, respectively).
[0131] Example 7: Thermal stability of metal-dielectric devices with hydrogenated AlN layers The stability of an exemplary metal-dielectric multilayer stack is shown in Figure 30 (A-D). The metal-dielectric stack is on glass and the temperature is measured on the opposite glass surface. The light transmittance is measured at three different locations (as shown in the schematic diagram of Figure 30D) at different times, first at time zero and then at different times following a series of thermal heating and cooling cycles. Each thermal cycle includes a 10 second power on followed by a 15 minute power off cooling period. The typical initial temperature is room temperature while the maximum temperature following the heat generation portion of the thermal cycle is around 100°C.
[0132] Example 8: Plasmon absorption in metal-dielectric devices with AlN layers A cross-sectional SEM image of an exemplary metal-dielectric multilayer stack is shown in Figure 31. The image shows that in backscattering mode, silver (500), seen as white particles (520), is present in the top hydrogenated AlN layer (510), seen as a dark grey layer. The silver nanoparticles give rise to localized surface plasmon resonance.
[0133] The depth profile obtained by time-of-flight secondary ion mass spectrometry (ToF-SIMS) of an exemplary metal-dielectric multilayer stack is plotted in FIG. 32. The sputter time on the horizontal axis is a proxy for distance from the stack surface. Labels at the top identify different regions of the plot as the top hydrogenated AlN layer, the middle silver layer, the bottom hydrogenated AlN layer, and the silicon substrate. The plot shows the presence of silver inside the top hydrogenated AlN layer, confirming the observation in the SEM image shown in FIG. 31.
[0134] The plasmon absorption of an exemplary metal-dielectric multilayer stack is shown in Figure 33. Metal-dielectric coatings with various silver layer thicknesses are deposited on top of a glass substrate. Optical transmission and reflection are measured from the coated side of the substrate and used to determine absorption. A clear absorption peak in the violet wavelength range (380-450 nm) is prominent. The observed plasmon absorption is a signature of localized surface plasmon resonance, a phenomenon consistent with the predictions of effective medium theory, assuming the presence of silver nanoparticles in the dielectric layer. Both the peak intensity and peak wavelength decrease as the silver layer thickness decreases, demonstrating the tunability of the plasmon absorption wavelength. Further tunability can be integrated by varying the dielectric composition (e.g., by changing the hydrogenation level) and also by varying the dielectric constant of the top hydrogenated metal nitride layer, as shown in Figures 19 and 20. In maintaining the plasmon frequency dependence on the dielectric constant, varying the dielectric properties can shift the resonant wavelength of the plasmon peak, thereby enabling changes in the optical properties (e.g., designing different reflected colors).
[0135] It should be understood that the particular embodiments described above are shown by way of example, and that these embodiments may be susceptible to various modifications and alternative forms. It should also be understood that the claims are not intended to be limited to the particular forms disclosed, but rather are intended to cover all modifications, equivalents, and alternatives falling within the spirit and scope of the disclosure.
[0136] [References] 1. Soulen, Robert (March 1996). "James Dewar, His Flask and Other Achievements". Physics Today. 49 (3): 32-37. 2. https: / / en.wikipedia.org / wiki / Thermos_L.LC 3. http: / / www.lamptech.co.uk / Spec%20Sheets / D%20SLP%20GEC%20SLI175%20Gold.htm 4. http: / / www.lamptech.co.uk / Spec%20Sheets / D%20SLP%20Philips%20SOX40.htm 5. HJJ van Boort and R. Groth, “Low-pressure sodium lamps with indium oxide filter”, Philips tech. Rev. 29,17,1968. 6. H. Kostlin, “Double-glazed windows with very good thermal insulation”, Philips tech. Rev. 34, 242-243, 1974, No. 9. 7. John CC Fan and Frank J. Bachner, “Transparent heat mirrors for solar-energy applications”, Applied Optics Vol. 15, Issue 4, pp. 1012-1017 (1976). 8. Scalora, M., Bloemer, M. J., Pethel, A. S., Dowling, J. P., Bowden, C. M., & Manka, A. S., “Transparent, metallo-dielectric, one-dimensional, photonic band-gap structures”, Journal of Applied Physics, 83(5), 2377-2383 (1998). 9. Martin-Palma, R. J., Vazquez, L., & Martinez-Duart, J. M. (1998). Silver-based low-emissivity coatings for architectural windows: Optical and structural properties. Solar Energy Materials and Solar Cells, 53(1), 55-66. 10. Chiba, K., Takahashi, T., Kageyama, T., & Oda, H. (2005). Low-emissivity coating of amorphous diamond-like carbon / Ag-alloy multilayer on glass. Applied Surface Science, 246(1), 48-51. 11. Mahtani, P., Leong, K. R., Xiao, I., Chutinan, A., Kherani, N. P., & Zukotynski, S. (2011). Diamond-like carbon based low-emissive coatings. Solar Energy Materials and Solar Cells, 95(7), 1630-1637. 12. Ferrara, M., Castaldo, A., Esposito, S., D'Angelo, A., Guglielmo, A., & Antonaia, A. (2016). AlN-Ag based low-emission sputtered coatings for high visible transmittance window. Surface and Coatings Technology, 295, 2-7. 13. Hollars, Dennis R. "Method of making sputtered coatings." U.S. Patent No. 4,421,622. 20 Dec. 1983. 14. Young, P. I. & Wolfe, J. D. Solar control layered coating for glass windows US Patent 4,965,121. Oct. 1990. 15. Oyama, T., Suzuki, K. & Mizuhashi, M. Transparent laminated product US Patent 4,859,532. Aug. 1989. 16. Depauw, J.-M. & Hoyois, J.-C. Coated glazing material US Patent 5,110,662. May 1992. 17. Hartig, K. W. & Lingle, P. J. High performance, durable, low-E glass US Patent 5,344,718. Sept. 1994. 18. Tausch, P. J. & Goodman, R. D. Sputtered multi-layer color compatible solar control coating US Patent 5,332,888. July 1994. 19. Hartig, K. W., Larson, S. L. & Lingle, P. J. Low-E glass coating system and insulating glass units made therefrom US Patent 5,514,476. May 1996. 20. Veerasamy, V. S., Petrmichl, R. H. & Thomsen, S. V. Solar management coating system including protective DLC US Patent 6,764,579. July 2004. 21. Persoone, P., Vlaeminck, K. & Lievens, H. Infra-red reflecting layered structure US Patent 7,709,095. May 2010. 22. Wolfe, J. D., Belkind, A. I. & Laird, R. E. Durable low-emissivity solar control thin film coating US Patent 5,563,734. Oct. 1996. 23. Reutler, P. & Gerardin, H. Substrate provided with a stack having thermal properties US Patent App. 12 / 933,240. Mar. 2009 24. Patent, U. S. "20140177042 A1." Novel silver barrier materials for low-emissivity applications (2014).
Claims
1. 1. A method for producing a metal dielectric coating on a transparent substrate, comprising: depositing a first transparent dielectric layer onto the transparent substrate; depositing a metal layer onto the first transparent dielectric layer; depositing a second transparent dielectric layer over the metal layer; having at least one of the first transparent dielectric layer or the second transparent dielectric layer is a hydrogenated transparent metal nitride layer; the thickness of the metal layer and the hydrogen concentration of each of the hydrogenated transparent metal nitride layers are selected such that the metal-dielectric coating exhibits at least 70% transparency in at least a portion of the visible spectrum; each said hydrogenated transparent metal nitride layer being hydrogenated sufficiently to promote migration of metal atoms from said metal layer and aggregation of said metal atoms to form metal nanoparticles therein, thereby producing a plasmon resonance in the absorption spectrum of said metal dielectric coating; method.
2. The method of claim 1 , wherein each of said hydrogenated transparent metal nitride layers comprises aluminum nitride.
3. The method of claim 2 , wherein the metal layer is a silver layer and the nanoparticles are silver nanoparticles.
4. The method of claim 1 , further comprising using a localized heat treatment to facilitate migration of the metal atoms.
5. The method of claim 1 , wherein each said hydrogenated transparent metal nitride layer is hydrogenated during its deposition.
6. The method of claim 5 , wherein each said hydrogenated transparent metal nitride layer is formed via a sputtering process in the presence of hydrogen gas.
7. The method according to claim 5 or 6, wherein the hydrogen concentration during the formation of the at least one hydrogenated transparent metal nitride layer is between 1% and 10% by volume.
8. The method of claim 6, wherein the hydrogen concentration during formation of the at least one hydrogenated transparent metal nitride layer is between 0.25% and 20% by volume.
9. The method of claim 6, wherein the hydrogen concentration during formation of the at least one hydrogenated transparent metal nitride layer is between 0.25% and 2.5% by volume.
10. The method of claim 6, wherein the hydrogen concentration during formation of the at least one hydrogenated transparent metal nitride layer is between 0.25% and 5% by volume.
11. The method of claim 1 , wherein each said hydrogenated transparent metal nitride layer is hydrogenated after its deposition.
12. The method of any one of claims 1 to 11, wherein the at least one hydrogenated transparent metal nitride layer is formed having a hydrogen concentration of 1 ppm to 1000 ppm by weight.
13. The method of claim 1 , wherein the hydrogen concentration in at least one of the hydrogenated transparent metal nitride layers is spatially graded in a direction parallel to a surface normal associated with the transparent substrate.
14. 14. The method of claim 1, wherein the first transparent dielectric layer forms a first hydrogenated transparent metal nitride dielectric layer and the second transparent dielectric layer forms a second hydrogenated transparent metal nitride layer.
15. 15. The method of claim 14, wherein the metal layer and the second hydrogenated transparent metal nitride layer form a metal-dielectric bilayer, the method further comprising depositing one or more additional metal-dielectric bilayers.
16. The method of claim 15 , wherein the hydrogen concentration in at least one of the hydrogenated transparent metal nitride layers is spatially graded in a direction parallel to a surface normal associated with the transparent substrate.
17. The method according to any one of the preceding claims, wherein the refractive index of at least one of the hydrogenated transparent metal nitride layers is between 1.5 and 1.
8.
18. The method of any one of claims 1 to 17, wherein the resistivity of the metal layer is between 2 and 6 microohm cm.
19. 19. The method of claim 1, wherein the average grain size of at least one of the hydrogenated transparent metal nitride layers is less than 30 nm.
20. 20. The method of claim 1, wherein a full width at half maximum of the grain size distribution in the at least one hydrogenated transparent metal nitride layer in a growth direction of the at least one hydrogenated transparent metal nitride layer is less than 3 nm.
21. The method of any one of claims 1 to 20, wherein the metal layer has a thickness of between 3 nm and 30 nm.
22. 22. The method of any one of claims 1 to 21, wherein the metal layer is deposited in the presence of hydrogen or exposed to hydrogen after deposition.
23. 23. The method of claim 22, wherein the concentration of hydrogen used during deposition of the metal layer is controlled such that active electronic sites of an adjacent dielectric layer are passivated.
24. 23. The method of claim 22, wherein a concentration of hydrogen used during deposition of the metal layer is controlled such that one or more optical or electrical properties of the metal layer meet preselected criteria.
25. 25. The method of claim 24, wherein the optical or electrical property is selected from optical transmittance or electrical conductivity.
26. The method of claim 22 , wherein the concentration of hydrogen used during deposition of the metal layer or a given metal nitride layer is controlled such that the metal layer is devoid of islands.
Citation Information
Patent Citations
Lamination
JP1994278244A
Transparent sheet-like heater and manufacture thereof
JP1994338381A
Method of annealing photovoltaic cell
JP2008078662A
Low-emissivity coating film, method for manufacturing the same, and functional building materials for windows containing the same
JP2017500266A