Perovskite-type complex oxide and method for producing same
The BaZr1-x-yCe x M y O 3 composition allows for the production of a dense sintered body at low temperatures in air, addressing the limitations of existing methods by achieving a dense structure suitable for solid oxide fuel cells.
Patent Information
- Application Number
- JP2019128535
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-07-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-07-10
AI Technical Summary
Existing methods for producing perovskite-type composite oxides for solid oxide fuel cells require vacuum heat treatment and low-temperature baking in air, failing to achieve a dense sintered body.
A method involving the composition formula BaZr1-x-yCe x M y O 3 (M = Y, Yb, Sc, Tm) is used, where the solid material is neutralized with an acidic solution and alkali, then fired at 1000 to 1370°C in an air atmosphere, producing a dense sintered body.
The method enables the production of a dense sintered body at relatively low temperatures in air, with a BET specific surface area of 4-14 m 2 /g and crystallite diameter of 15-26 nm, suitable for electrolyte materials in solid oxide fuel cells.
Smart Images

Figure 0007577433000001 
Figure 0007577433000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a perovskite complex oxide and a method for producing the same, and more particularly to a proton-conductive perovskite complex oxide suitable for use as an electrolyte material in solid oxide fuel cells and a method for producing the same. [Background technology]
[0002] A solid oxide fuel cell generally has a stack structure in which unit cells each made of an air electrode made of an oxide, a solid electrolyte, and a fuel electrode are connected by an interconnector. As a method for producing a proton-conductive perovskite-type composite oxide suitable as an electrolyte material for such solid oxide fuel cells, a method has been proposed in which a precursor of a carbon-containing perovskite consisting of perovskite ABO3 (A is Ba or Sr, B is Ce) is heat-treated in a vacuum at 500 to 1200°C to produce a proton-conductive perovskite-type composite oxide (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2007-137697 A (paragraph number 0012) Summary of the Invention [Problem to be solved by the invention]
[0004] However, the method for producing a perovskite complex oxide in Patent Document 1 requires heat treatment in a vacuum, and it is not possible to obtain a dense sintered body (required for electrolyte materials for solid oxide fuel cells, etc.) by firing at a relatively low temperature in an air atmosphere.
[0005] Accordingly, in view of such conventional problems, an object of the present invention is to provide a perovskite-type composite oxide and a method for producing the same, which can obtain a dense sintered body even when fired at a relatively low temperature in an air atmosphere.
Means for Solving the Problems
[0006] As a result of intensive studies to solve the above problems, the present inventors have found that by firing a solid obtained by adding and neutralizing an alkali to an acidic solution containing a starting material of a perovskite-type composite oxide represented by the composition formula BaZr 1-x-y Ce x M y O3 (M is one or more elements selected from the group consisting of Y, Yb, Sc, and Tm, 0 ≦ x ≦ 0.7, 0 < y ≦ 0.2), a perovskite-type composite oxide capable of obtaining a dense sintered body even when fired at a relatively low temperature in an air atmosphere can be produced, and the present invention has been completed.
[0007] That is, the method for producing a perovskite-type composite oxide according to the present invention is characterized by firing a solid obtained by adding and neutralizing an alkali to an acidic solution containing a starting material of a perovskite-type composite oxide represented by the composition formula BaZr 1-x-y Ce x M y O3 (M is one or more elements selected from the group consisting of Y, Yb, Sc, and Tm, 0 ≦ x ≦ 0.7, 0 < y ≦ 0.2).
[0008] In this method for producing a perovskite-type composite oxide, the acidic solution is preferably an aqueous nitric acid solution, the alkali is preferably an ammonium salt, and the firing temperature is preferably 1000 to 1370 °C.
[0009] Further, the perovskite-type composite oxide according to the present invention has the composition formula BaZr 1-x-y Ce x M yA perovskite-type composite oxide represented by O3 (M is one or more elements selected from the group consisting of Y, Yb, Sc, and Tm, 0 ≦ x ≦ 0.7, 0 < y ≦ 0.2), characterized by containing 0.15 to 1.0% by mass of carbon.
[0010] The BET specific surface area of this perovskite-type composite oxide is preferably 4 m 2 / g or more, and the crystallite size is preferably 30 nm or less.
[0011] Also, the perovskite-type composite oxide according to the present invention has a composition formula BaZr 1-x-y Ce x M y O3 (M is one or more elements selected from the group consisting of Y, Yb, Sc, and Tm, 0 ≦ x ≦ 0.7, 0 < y ≦ 0.2), and is characterized by having a BET specific surface area of 4 to 14 m 2 / g.
[0012] Furthermore, the solid oxide fuel cell according to the present invention is characterized by using the above perovskite-type composite oxide as a material for the electrolyte.
Advantages of the Invention
[0013] According to the present invention, a perovskite-type composite oxide capable of obtaining a dense sintered body even when fired at a relatively low temperature in an air atmosphere can be produced.
Embodiments for Carrying Out the Invention
[0014] In an embodiment of the method for producing a perovskite-type composite oxide according to the present invention, the composition formula is BaZr 1-x-y Ce x M yA nitrate (such as a nitrate solution like an aqueous nitric acid solution) or an acidic solution containing nitric acid, which contains a starting material of a perovskite-type composite oxide represented by O3 (M is one or more elements selected from the group consisting of Y, Yb, Sc, and Tm, 0 ≦ x ≦ 0.7, 0 < y ≦ 0.2), is neutralized by adding an alkali (such as a mixture of carbonic acid and ammonia or an ammonium salt like ammonium carbonate). The obtained solid (neutralization product) is dried and then fired at 1000 to 1370 °C (preferably 1100 to 1350 °C) in an air atmosphere. Note that pellets (preferably with a density of 2.7 g / cm 3 or more) obtained by pressing and molding the perovskite-type composite oxide produced in this way are fired (preferably at a temperature of about 1450 °C) to obtain a dense fired body (required for materials such as the electrolyte of a solid oxide fuel cell).
[0015] In addition, an embodiment of the perovskite-type composite oxide according to the present invention has a composition formula BaZr 1-x-y Ce x M y O3 (M is one or more elements selected from the group consisting of Y, Yb, Sc, and Tm, 0 ≦ x ≦ 0.7, 0 < y ≦ 0.2), and contains 0.15 to 1.0 mass% of carbon. The BET specific surface area of this perovskite-type composite oxide is preferably 4 m 2 / g or more, and more preferably 4 to 14 m 2 / g. Further, the crystallite size of this perovskite-type composite oxide is preferably 30 nm or less, and preferably 15 to 26 nm.
[0016] In addition, an embodiment of the perovskite-type composite oxide according to the present invention has a composition formula BaZr 1-x-y Ce x M y O3 (M is one or more elements selected from the group consisting of Y, Yb, Sc, and Tm, 0 ≦ x ≦ 0.7, 0 < y ≦ 0.2), and has a BET specific surface area of 4 to 14 m 2 / g. The crystallite size of this perovskite-type composite oxide is preferably 15 to 26 nm.
[0017] Furthermore, an embodiment of the perovskite-type composite oxide according to the present invention has a composition formula BaZr 1-x-y Ce x M y O3 (M is one or more elements selected from the group consisting of Y, Yb, Sc, and Tm, 0 ≦ x ≦ 0.7, 0 < y ≦ 0.2), and is a perovskite-type composite oxide having a crystallite size of 15 to 26 nm.
[0018] Note that the composition formula of the above perovskite-type composite oxide can also be expressed as BaZr 1-x-y Ce x M y O 3-σ (M is one or more elements selected from the group consisting of Y, Yb, Sc, and Tm, 0 ≦ x ≦ 0.7, 0 < y ≦ 0.2, σ is an oxygen deficiency (natural number)).
Example
[0019] Hereinafter, examples of the perovskite-type composite oxide according to the present invention and a method for producing the same will be described in detail.
[0020] [Example 1] 112.6 g of barium nitrate, 222 g of an aqueous zirconium nitrate solution containing 20% by mass of zirconium in terms of ZrO2, and 33.4 g of ytterbium nitrate trihydrate were dissolved in 1 L of pure water so that the composition ratio of barium (Ba), zirconium (Zr), and ytterbium (Yb) was Ba:Zr:Yb = 1.0:0.8:0.2 to obtain an aqueous nitric acid solution of Ba, Zr, and Yb.
[0021] In addition, 344 g of ammonium carbonate was dissolved in 2.2 L of pure water to obtain an aqueous ammonium carbonate solution.
[0022] Next, while stirring the ammonium carbonate aqueous solution, the nitric acid aqueous solution was added to the ammonium carbonate aqueous solution (so that the pH after neutralization was about 8) to generate a neutralized precipitate, and then the solid matter obtained by solid-liquid separation was recovered. After drying the solid matter, it was fired at 1350°C in an air atmosphere to obtain a perovskite-type composite oxide.
[0023] The composition of Ba, Zr, and Yb of the perovskite-type composite oxide thus obtained was analyzed by ICP emission spectrometry, and the results showed that Ba:Zr:Yb=1:0.8:0.2. The composition of the perovskite-type composite oxide thus obtained was BaZr 1-x-y Ce x M y O3(M=Yb, x=0, y=0.2)(BaZr 0.8 Yb 0.2 The carbon content in the perovskite-type complex oxide was measured using a carbon / sulfur analyzer (EMIA-920V2, manufactured by Horiba, Ltd.) and found to be 0.30% by mass.
[0024] The obtained perovskite-type composite oxide was ground in an agate mortar, and the BET specific surface area of the perovskite-type composite oxide was measured by the BET single-point method using a BET specific surface area measuring device (4Sorb US manufactured by Yuasa Ionics Co., Ltd.). The BET specific surface area of the perovskite-type composite oxide was 6.9 m 2 / g.
[0025] In addition, the obtained perovskite complex oxide was subjected to X-ray diffraction (XRD) measurement using an X-ray diffraction (XRD) device (Ultima IV, a multipurpose aqueous sample X-ray diffractometer manufactured by Rigaku Corporation) with a CuKα tube as the X-ray tube and an X-ray tube output of 40 kV / 40 mA to obtain an X-ray diffraction pattern. Based on this X-ray diffraction pattern, the crystal phase of the obtained perovskite complex oxide was identified, and it was confirmed that it had a single-phase perovskite structure. In addition, the crystallite diameter (Dx) was calculated from Scherrer's formula D=(K·λ) / (β·cosθ) using the half-width β of the (110) plane of the perovskite phase obtained from the X-ray diffraction pattern, and the crystallite diameter (Dx) was found to be 25.1 nm. In the Scherrer formula, D is the crystallite diameter (nm), λ is the measurement X-ray wavelength (nm), β is the diffraction width caused by the crystallites, θ is the Bragg angle of the diffraction angle, and K is the Scherrer constant. In this formula, the measurement X-ray wavelength λ is the Cu-Kα ray wavelength, and the Scherrer constant K is 0.9.
[0026] Next, 0.25 g of the obtained perovskite complex oxide was weighed and filled into a φ5 mm molding machine, and a load of 1623 N was applied to the pellet using a hydraulic manual press and held for 10 seconds to form a pellet. The pellet was heated from room temperature to 1450°C while applying a load of 98 mN to obtain a sintered body. The mass, diameter, and height of the sintered body were measured to calculate the density of the sintered body, which was 2.93 g / cm. 2 It was.
[0027] The open porosity of this sintered body was measured according to JIS R1634 (1998) (Method of measuring density and open efficiency of sintered body of fine ceramics). Specifically, the mass of this sintered body was measured as the dry mass W1, and then the sintered body was placed in a container and sucked by a vacuum pump at 2.0 kPa or less for 15 minutes to fully remove the air in the pores of the sintered body. Next, water was poured until the sintered body was completely immersed, and the cock on the container was gradually opened to return the inside of the container to atmospheric pressure, and then the container was left for 30 minutes. The vacuum pump was operated during the water injection and stopped after the injection. The sintered body immersed in water was suspended by a wire, and the mass of the sintered body in water was measured in this state, and the mass corrected for the part suspended by the wire was taken as the submerged mass W2. Next, the sintered body was taken out of the water, and its surface was quickly wiped with a wet gauze to remove water droplets, and its mass was measured and taken as the saturated mass W3. The gauze was soaked in water and then squeezed out just enough to wipe off the water droplets on the surface of the sintered body taken out of the water. Using the masses W1 to W3 thus obtained, the open porosity P0 of the sintered body was calculated from P0 = (W3 - W1) x 100 / (W3 - W2). As a result, the open porosity of the sintered body was 51%.
[0028] [Example 2] An aqueous solution of nitric acid of Ba, Zr, and Y was obtained by dissolving 112.6 g of barium nitrate, 222 g of an aqueous zirconium nitrate solution containing 20 mass % zirconium calculated as ZrO2, and 31.0 g of yttrium nitrate hexahydrate in 1 L of pure water so that the composition ratio of barium (Ba), zirconium (Zr), and yttrium (Y) was Ba:Zr:Y = 1.0:0.8:0.2.
[0029] Next, while stirring the same ammonium carbonate aqueous solution as in Example 1, the above nitric acid aqueous solution was added to the ammonium carbonate aqueous solution (so that the pH after neutralization was about 8) to generate a neutralized precipitate, and then the solid matter obtained by solid-liquid separation was recovered. After drying this solid matter, it was fired at 1350°C in an air atmosphere to obtain a perovskite-type composite oxide.
[0030] The composition of Ba, Zr, and Y of the perovskite-type composite oxide thus obtained was analyzed by ICP emission spectrometry, and the results showed that Ba:Zr:Y=1:0.8:0.2. The composition of the perovskite-type composite oxide thus obtained was BaZr 1-x-y Ce x M y O3(M=Y, x=0, y=0.2)(BaZr 0.8 Y 0.2 O3).
[0031] The carbon content and BET specific surface area of the perovskite-type composite oxide thus obtained were measured in the same manner as in Example 1. The carbon content was 0.19 mass% and the BET specific surface area was 5.2 m. 2 / g. When the crystal phase of the perovskite complex oxide was identified by the same method as in Example 1, it was confirmed that it had a single-phase perovskite structure. When the crystallite diameter of the perovskite complex oxide was calculated by the same method as in Example 1, the crystallite diameter was 20.8 nm. When the obtained perovskite complex oxide was used to produce a sintered body by the same method as in Example 1, the density of the sintered body was calculated and the open porosity was measured, and the density of the sintered body was found to be 2.76 g / cm. 2 The open porosity was 47%.
[0032] [Example 3] An aqueous solution of nitrates of Ba, Zr, Ce, Y, and Yb was obtained by dissolving 50.3 g of barium nitrate, 14.3 g of an aqueous zirconium nitrate solution containing 20 mass% zirconium calculated as ZrO2, 62.2 g of cerium sulfate hexahydrate, 13.4 g of an aqueous yttrium nitrate solution containing 13.5 mass% yttrium, and 8.4 g of ytterbium nitrate trihydrate in 1 L of pure water so that the composition ratio of barium (Ba), zirconium (Zr), cerium (Ce), yttrium (Y), and ytterbium (Yb) was Ba:Zr:Ce:Y:Yb=1:0.1:0.7:0.1:0.1.
[0033] Next, while stirring the same ammonium carbonate aqueous solution as in Example 1, the above nitric acid aqueous solution was added to the ammonium carbonate aqueous solution (so that the pH after neutralization was about 8) to generate a neutralized precipitate, and then the solid matter obtained by solid-liquid separation was recovered. After drying this solid matter, it was fired at 1100°C in an air atmosphere to obtain a perovskite-type composite oxide.
[0034] The composition of the perovskite-type composite oxide thus obtained was analyzed by ICP emission spectrometry to determine the composition of Ba, Zr, Ce, Y, and Yb. The composition was found to be Ba:Zr:Ce:Y:Yb=1:0.1:0.7:0.1:0.1. The composition of the perovskite-type composite oxide thus obtained was BaZr 1-x-y Ce x M y O3(M=Y+Yb, x=0.7, y=0.2)(BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O3).
[0035] The carbon content and BET specific surface area of the perovskite-type composite oxide thus obtained were measured in the same manner as in Example 1. The carbon content was 0.21 mass % and the BET specific surface area was 6.1 m 2 / g. When the crystal phase of the perovskite complex oxide was identified by the same method as in Example 1, it was confirmed that it had a single-phase perovskite structure. When the crystallite diameter of the perovskite complex oxide was calculated by the same method as in Example 1, the crystallite diameter was 20.1 nm. When the obtained perovskite complex oxide was used to produce a sintered body by the same method as in Example 1, the density of the sintered body was calculated and the open porosity was measured, and the density of the sintered body was found to be 3.26 g / cm. 2 The open porosity was 45%.
[0036] [Comparative Example 1] 29.4g of barium carbonate, 14.7g of zirconium oxide, and 5.9g of ytterbium oxide were added to 50g of pure water so that the composition ratio of barium (Ba), zirconium (Zr), and ytterbium (Yb) was Ba:Zr:Yb=1.0:0.8:0.2, and the mixture was pulverized by a bead mill so that the center diameter of the pulverized slurry was 1μm or less. The pulverized slurry was dried and then fired at 1400℃ in the air to obtain a perovskite-type composite oxide.
[0037] The composition of Ba, Zr, and Yb of the perovskite-type composite oxide thus obtained was analyzed by ICP emission spectrometry, and the results showed that Ba:Zr:Yb=1:0.8:0.2. The composition of the perovskite-type composite oxide thus obtained was BaZr 1-x-y Ce x M y O3(M=Yb, x=0, y=0.2)(BaZr 0.8 Yb 0.2 O3).
[0038] The carbon content and BET specific surface area of the perovskite-type composite oxide thus obtained were measured in the same manner as in Example 1. The carbon content was 0.09 mass% and the BET specific surface area was 2.8 m. 2 / g. When the crystal phase of the perovskite complex oxide was identified by the same method as in Example 1, it was confirmed that it had a single-phase perovskite structure. When the crystallite diameter of the perovskite complex oxide was calculated by the same method as in Example 1, the crystallite diameter was 35.7 nm. When a sintered body was produced by the same method as in Example 1 using the obtained perovskite complex oxide, and the density of the sintered body was calculated, the density of the sintered body was 2.27 g / cm 2 In addition, an attempt was made to measure the open porosity of the sintered body by the same method as in Example 1, but the sintered body collapsed in water, making it impossible to measure (ND).
[0039] [Comparative Example 2] 31.0g of barium carbonate, 15.5g of zirconium oxide, and 3.55g of yttrium oxide were added to 50g of pure water so that the composition ratio of barium (Ba), zirconium (Zr), and yttrium (Y) was Ba:Zr:Y = 1.0:0.8:0.2, and the mixture was pulverized by a bead mill so that the center diameter of the pulverized slurry was 1 μm or less. The pulverized slurry was dried and then fired at 1400 ° C. in an air atmosphere to obtain a perovskite-type composite oxide.
[0040] The composition of Ba, Zr, and Y of the perovskite-type composite oxide thus obtained was analyzed by ICP emission spectrometry, and the results showed that Ba:Zr:Y=1:0.8:0.2. The composition of the perovskite-type composite oxide thus obtained was BaZr 1-x-y Ce x M y O3(M=Y, x=0, y=0.2)(BaZr 0.8 Y 0.2 O3).
[0041] The carbon content and BET specific surface area of the perovskite-type composite oxide thus obtained were measured in the same manner as in Example 1. The carbon content was 0.11% by mass and the BET specific surface area was 2.3 m. 2 / g. When the crystal phase of the perovskite complex oxide was identified by the same method as in Example 1, it was confirmed that it had a single-phase perovskite structure. When the crystallite diameter of the perovskite complex oxide was calculated by the same method as in Example 1, the crystallite diameter was 26.6 nm. When a sintered body was produced by the same method as in Example 1 using the obtained perovskite complex oxide and the density of the sintered body was calculated, the density of the sintered body was 2.24 g / cm 2 In addition, an attempt was made to measure the open porosity of the sintered body by the same method as in Example 1, but the sintered body collapsed in water, making it impossible to measure (ND).
[0042] [Comparative Example 3] 27.3g of barium carbonate, 1.7g of zirconium oxide, 16.7g of cerium oxide, 1.6g of yttrium oxide, and 2.7g of ytterbium oxide were added to 50g of pure water so that the composition ratio of barium (Ba), zirconium (Zr), cerium (Ce), yttrium (Y), and ytterbium (Yb) was Ba:Zr:Ce:Y:Yb=1:0.1:0.7:0.1:0.1, and the mixture was pulverized by a bead mill so that the center diameter of the pulverized slurry was 1μm or less. The pulverized slurry was dried and then fired at 1400°C in an air atmosphere to obtain a perovskite-type composite oxide.
[0043] The composition of the perovskite-type composite oxide thus obtained was analyzed by ICP emission spectrometry to determine the composition of Ba, Zr, Ce, Y, and Yb. The composition was found to be Ba:Zr:Ce:Y:Yb=1:0.1:0.7:0.1:0.1. The composition of the perovskite-type composite oxide thus obtained was BaZr 1-x-y Ce x M y O3(M=Y+Yb, x=0.7, y=0.2)(BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O3).
[0044] The carbon content and BET specific surface area of the perovskite-type composite oxide thus obtained were measured in the same manner as in Example 1. The carbon content was 0.11 mass % and the BET specific surface area was 1.9 m. 2 / g. When the crystal phase of the perovskite complex oxide was identified by the same method as in Example 1, it was confirmed that it had a single-phase perovskite structure. When the crystallite diameter of the perovskite complex oxide was calculated by the same method as in Example 1, the crystallite diameter was 26.7 nm. When the obtained perovskite complex oxide was used to produce a sintered body by the same method as in Example 1, the density of the sintered body was calculated and the open porosity was measured, and the density of the sintered body was found to be 2.68 g / cm. 2 The open porosity was 56%.
[0045] Tables 1 and 2 show the production conditions and properties of the perovskite complex oxides of these examples and comparative examples.
[0046] [Table 1]
[0047] [Table 2]
[0048] From Tables 1 and 2, it can be seen that the sintered bodies made from the perovskite-type complex oxides of Examples 1 to 3 have higher density and lower open porosity than the sintered bodies made from the perovskite-type complex oxides of Comparative Examples 1 to 3, and are therefore denser sintered bodies. [Industrial Applicability]
[0049] The perovskite complex oxide according to the present invention can be used as a dense sintered body and as an electrolyte material for solid oxide fuel cells.
Claims
1. Composition formula BaZr 1-x-y C.E. x M y O 3 (M is one or more elements selected from the group consisting of Y, Yb, Sc and Tm, 0≦x≦0.7, 0<y≦0.2) to neutralize an acidic solution containing a starting material for the perovskite complex oxide, and the resulting solid is fired at 1000 to 1370° C. in an air atmosphere.
2. 2. The method for producing a perovskite complex oxide according to claim 1, wherein the acidic solution is an aqueous solution of nitric acid.
3. Composition formula BaZr 1-x-y C.E. x M y O 3 (M is one or more elements selected from the group consisting of Y, Yb, Sc and Tm, 0≦x≦0.7, 0<y≦0.2), characterized in that the perovskite complex oxide contains 0.15 to 0.3 mass % of carbon and has a BET specific surface area of 4 m 2 / g or more.
4. 4. The perovskite complex oxide according to claim 3, wherein the crystallite size of the perovskite complex oxide is 30 nm or less.
5. Composition formula BaZr 1-x-y C.E. x M y O 3 (M is one or more elements selected from the group consisting of Y, Yb, Sc and Tm, 0≦x≦0.7, 0<y≦0.2), and has a BET specific surface area of 5.2 to 6.9 m. 2 / g.
6. 6. A solid oxide fuel cell comprising the perovskite complex oxide according to claim 3 as an electrolyte material.
Citation Information
Patent Citations
Method for producing proton conductive perovskite fine particle and the fine particle
JP2007137697A
Fuel electrode material, cell for solid oxide fuel battery, catalyst for hydrogen production, and method for producing hydrogen
JP2017050180A