Substrate processing method and plasma processing apparatus
The method alternates precursor adsorption and chemical species application in plasma etching to control film thickness, preventing recess opening blockage and ensuring precise film deposition within the substrate recesses.
Patent Information
- Application Number
- JP2021006624
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-08-28
- Filing Date
- 2021-01-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2041-01-19
AI Technical Summary
Existing plasma etching techniques struggle to prevent the lateral expansion of recesses in substrates, often leading to the blocking of openings by films formed on the sidewalls.
A method involving alternating steps of adsorbing a precursor and supplying chemical species to form a film on the sidewall surface, where a second chemical species suppresses the film thickness, particularly at the recess opening, using a plasma processing apparatus with controlled electrical bias to adjust film formation depth.
Effectively prevents the blocking of recess openings by managing film thickness, allowing precise control over film deposition within the recess, thereby maintaining the integrity of the substrate features.
Smart Images

Figure 0007577546000001 
Figure 0007577546000002 
Figure 0007577546000003
Abstract
Description
[Technical field]
[0001] SUMMARY Exemplary embodiments of the present disclosure relate to a substrate processing method and a plasma processing apparatus. [Background technology]
[0002] Plasma etching is used to form a recess in a substrate. In plasma etching, it is required to suppress the recess from expanding laterally. For this reason, a technique is used to form a film on the sidewall surface that defines the recess. Such a technique is described in Patent Documents 1 and 2. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] US Patent Application Publication No. 2016 / 0343580 [Patent Document 2] US Patent Application Publication No. 2018 / 0174858 Summary of the Invention [Problem to be solved by the invention]
[0004] The present disclosure provides a technique for suppressing blocking of an opening of a recess by a film formed on a substrate. [Means for solving the problem]
[0005] In one exemplary embodiment, a method for processing a substrate is provided. The method for processing a substrate includes a step (a) of adsorbing a precursor on a sidewall surface of the substrate. The sidewall surface defines a recess in the substrate. The method for processing a substrate further includes a step (b) of providing a first chemical species and a second chemical species to the substrate. The first chemical species forms a film from the precursor on the sidewall surface, and the second chemical species inhibits an increase in thickness of the film. Steps (a) and (b) are alternately repeated. Effect of the Invention
[0006] According to one exemplary embodiment, blocking of the opening of the recess by a film formed on a substrate is suppressed. [Brief description of the drawings]
[0007] [Figure 1] 1 is a flow diagram of a substrate processing method according to an exemplary embodiment. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of a portion of an example substrate. [Diagram 3] 1 is a schematic diagram illustrating a plasma processing apparatus according to an exemplary embodiment; [Figure 4] 2 is a partially enlarged cross-sectional view of the example substrate after step ST2 of the substrate processing method shown in FIG. 1 has been applied; FIG. [Diagram 5] 2 is a timing chart of an example related to the substrate processing method shown in FIG. [Figure 6] 13 is a timing chart of another example related to the substrate processing method shown in FIG. [Figure 7] 2 is a partially enlarged cross-sectional view of an example of a substrate with a film formed on a side wall surface in the substrate processing method shown in FIG. 1. FIG. [Figure 8] 2 is a partially enlarged cross-sectional view of an example of a substrate after the substrate processing method shown in FIG. 1 has been applied; FIG. [Figure 9] 2 is a partially enlarged cross-sectional view of an example of a substrate before alternate repetition of steps STa and STb is applied in the substrate processing method shown in FIG. 1. FIG. [Figure 10] 1 illustrates a schematic diagram of a substrate processing system according to an exemplary embodiment; [Figure 11] FIGS. 11(a), 11(b), 11(c), and 11(d) are graphs showing the distribution of ΔCD in the depth direction obtained in the first to fourth experiments, respectively. [Figure 12] FIG. 12(a), FIG. 12(b), and FIG. 12(c) are graphs showing the distribution of ΔCD in the depth direction obtained in the fifth to seventh experiments, respectively. [Figure 13]FIG. 13(a), FIG. 13(b), and FIG. 13(c) are graphs showing the distribution of ΔCD in the depth direction obtained in the eighth to tenth experiments, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Various exemplary embodiments are described below.
[0009] In one exemplary embodiment, a method for processing a substrate is provided. The method for processing a substrate includes a step (a) of adsorbing a precursor on a sidewall surface of the substrate. The sidewall surface defines a recess in the substrate. The method for processing a substrate further includes a step (b) of providing a first chemical species and a second chemical species to the substrate. The first chemical species forms a film from the precursor on the sidewall surface, and the second chemical species inhibits an increase in thickness of the film. Steps (a) and (b) are alternately repeated.
[0010] In the above embodiment, a film is formed on the sidewall surface by reaction between the precursor and the first chemical species. The second chemical species inhibits an increase in the thickness of the film, particularly at the opening of the recess. Thus, according to the above embodiment, blocking of the opening of the recess by the film formed on the substrate is inhibited.
[0011] In one exemplary embodiment, the second species may be a halogen species. The second species may be a fluorine species.
[0012] In one exemplary embodiment, the second chemical species may be generated from at least one of a fluorocarbon, a hydrofluorocarbon, nitrogen trifluoride, and sulfur hexafluoride.
[0013] In one exemplary embodiment, the precursor may contain silicon.
[0014] In one exemplary embodiment, an electric bias may be applied to a lower electrode of a substrate support that supports the substrate in step (b), and according to this embodiment, the depth position within the recess where the film is formed may be set by the magnitude of the electric bias.
[0015] In one exemplary embodiment, the magnitude of the electric bias may be changed in the alternating repetition of steps (a) and (b). According to this embodiment, it is possible to change the depth position in the recess where the film is formed in the alternating repetition of steps (a) and (b).
[0016] In one exemplary embodiment, the substrate processing method may further include, after the alternating repetition of steps (a) and (b), a step (c) of etching the substrate to increase the depth of the recess.
[0017] In one exemplary embodiment, a first cycle and a second cycle, each including alternating repetitions of steps (a) and (b) and step (c), may be performed in sequence, and the magnitude of the electrical bias applied to a lower electrode of a substrate support supporting a substrate in step (b) in the first cycle may be different from the magnitude of the electrical bias applied to the lower electrode in step (b) in the second cycle.
[0018] In one exemplary embodiment, the magnitude of the electrical bias used in step (b) in the second cycle may be greater than the magnitude of the electrical bias used in step (b) in the first cycle, which allows the film to be formed deeper within the feature depending on the depth of the feature.
[0019] In one exemplary embodiment, a plasma processing apparatus is provided. The plasma processing apparatus includes a chamber, a gas supply unit, a plasma generation unit, and a control unit. The gas supply unit is configured to supply a precursor gas, a first gas, and a second gas into the chamber. The plasma generation unit is configured to generate plasma from the first gas and the second gas. The control unit (a) controls the gas supply unit to supply the precursor gas into the chamber. By controlling (a), a precursor contained in the precursor gas is adsorbed on the sidewall surface of the substrate. The control unit (b) controls the gas supply unit and the plasma generation unit to generate plasma from the first gas and the second gas in the chamber. By controlling (b), a first chemical species that forms a film from the precursor on the sidewall surface is generated from the first gas, and a second chemical species that suppresses an increase in the thickness of the film is generated from the second gas. The control unit is configured to alternately repeat the control of (a) and the control of (b).
[0020] Various exemplary embodiments will now be described in detail with reference to the drawings, in which the same or corresponding parts are designated by the same reference numerals.
[0021] Fig. 1 is a flow diagram of a substrate processing method according to an example embodiment. The substrate processing method shown in Fig. 1 (hereinafter referred to as "method MT") is performed to form a film on a sidewall surface that defines a recess in a substrate. Method MT may further include etching the substrate after the formation of the film.
[0022] Fig. 2 is a partially enlarged cross-sectional view of an example substrate. The method MT may be applied to the substrate W shown in Fig. 2. The substrate W has a film EF and a mask MK. The substrate W may further have an underlayer region UR. The film EF may be provided on the underlayer region UR.
[0023] The film EF is an etch film (Etch Film) and is etched in the method MT. The film EF is, for example, a silicon-containing film. The silicon-containing film may be a single-layer film or a multi-layer film. The single-layer film is, for example, a silicon oxide film, a silicon nitride film, a polycrystalline silicon film, or a silicon-containing low dielectric constant film. The multi-layer film is formed of two or more of a silicon oxide film, a silicon nitride film, and a polycrystalline silicon film. The film EF may be formed of other materials.
[0024] The mask MK is provided on the film EF. The mask MK can be made of any material as long as the film EF can be selectively etched with respect to the mask MK. The mask MK is made of, for example, a photoresist film, an organic film such as an amorphous carbon film or a spin-on carbon film, a silicon-containing film, or a metal-containing film. The mask MK has a pattern to be transferred to the film EF. That is, the mask MK provides recesses OP.
[0025] In one embodiment, the method MT is performed using a plasma processing apparatus. FIG. 3 is a schematic diagram of a plasma processing apparatus according to an exemplary embodiment. The method MT can be performed using the plasma processing apparatus 1 shown in FIG. 3. The plasma processing apparatus 1 is a capacitively coupled plasma processing apparatus. The plasma processing apparatus 1 includes a chamber 10. The chamber 10 provides an internal space 10s therein.
[0026] In one embodiment, the chamber 10 may include a chamber body 12. The chamber body 12 has a substantially cylindrical shape. An internal space 10s is provided inside the chamber body 12. The chamber body 12 is made of a conductor such as aluminum. The chamber body 12 is grounded. A corrosion-resistant film is provided on the inner wall surface of the chamber body 12. The corrosion-resistant film may be a film made of a ceramic such as aluminum oxide or yttrium oxide.
[0027] The sidewall of the chamber body 12 provides a passage 12p. The substrate W passes through the passage 12p when being transferred between the internal space 10s and the outside of the chamber 10. The passage 12p can be opened and closed by a gate valve 12g. The gate valve 12g is provided along the sidewall of the chamber body 12.
[0028] The plasma processing apparatus 1 further includes a substrate support 14. The substrate support 14 is configured to support the substrate W in the chamber 10, i.e., in the internal space 10s. The substrate support 14 is provided in the chamber 10. The substrate support 14 may be supported by a support portion 13. The support portion 13 is made of an insulating material. The support portion 13 has a substantially cylindrical shape. The support portion 13 extends upward from the bottom of the chamber body 12 in the internal space 10s.
[0029] In one embodiment, the substrate support 14 may include a lower electrode 18 and an electrostatic chuck 20. The substrate support 14 may further include an electrode plate 16. The electrode plate 16 is made of a conductor such as aluminum and has a generally disk-like shape. The lower electrode 18 is provided on the electrode plate 16. The lower electrode 18 is made of a conductor such as aluminum and has a generally disk-like shape. The lower electrode 18 is electrically connected to the electrode plate 16.
[0030] The electrostatic chuck 20 is provided on the lower electrode 18. The substrate W is placed on the upper surface of the electrostatic chuck 20. The electrostatic chuck 20 has a body formed from a dielectric material. The body of the electrostatic chuck 20 has a substantially disk shape. The electrostatic chuck 20 further has an electrode 20e. The electrode 20e is provided in the body of the electrostatic chuck 20. The electrode 20e is a film-like electrode. The electrode 20e is connected to a DC power supply 20p via a switch 20s. When a voltage from the DC power supply 20p is applied to the electrode of the electrostatic chuck 20, an electrostatic attractive force is generated between the electrostatic chuck 20 and the substrate W. Due to the generated electrostatic attractive force, the substrate W is attracted to the electrostatic chuck 20 and held by the electrostatic chuck 20.
[0031] The substrate support 14 may support an edge ring ER disposed thereon. The edge ring ER may be made of, but is not limited to, silicon, silicon carbide, or quartz. When processing of a substrate W is performed in the chamber 10, the substrate W is disposed on the electrostatic chuck 20 and within a region surrounded by the edge ring ER.
[0032] The lower electrode 18 provides a flow path 18f therein. The flow path 18f receives a heat exchange medium (e.g., a refrigerant) supplied from a chiller unit 22 via a pipe 22a. The chiller unit 22 is provided outside the chamber 10. The heat exchange medium supplied to the flow path 18f is returned to the chiller unit 22 via a pipe 22b. In the plasma processing apparatus 1, the temperature of the substrate W placed on the electrostatic chuck 20 is adjusted by heat exchange between the heat exchange medium and the lower electrode 18.
[0033] The temperature of the substrate W may be regulated by one or more heaters provided in the substrate support 14. In the example shown in Figure 3, a plurality of heaters HT are provided in the electrostatic chuck 20. Each of the plurality of heaters HT may be a resistive heating element. The plurality of heaters HT are connected to a heater controller HC. The heater controller HC is configured to provide a regulated amount of power to each of the plurality of heaters HT.
[0034] The plasma processing apparatus 1 may further include a gas supply line 24. The gas supply line 24 supplies a heat transfer gas (e.g., He gas) to a gap between the upper surface of the electrostatic chuck 20 and the rear surface of the substrate W. The heat transfer gas is supplied to the gas supply line 24 from a heat transfer gas supply mechanism.
[0035] The plasma processing apparatus 1 further includes an upper electrode 30. The upper electrode 30 is provided above the substrate support 14. The upper electrode 30 is supported on the upper part of the chamber body 12 via a member 32. The member 32 is made of an insulating material. The upper electrode 30 and the member 32 close the upper opening of the chamber body 12.
[0036] The upper electrode 30 may include a top plate 34 and a support 36. The bottom surface of the top plate 34 is the bottom surface on the side of the internal space 10s and defines the internal space 10s. The top plate 34 may be made of a silicon-containing material. The top plate 34 is made of, for example, silicon or silicon carbide. The top plate 34 provides a plurality of gas holes 34a. The plurality of gas holes 34a penetrate the top plate 34 in the plate thickness direction.
[0037] The support 36 detachably supports the top plate 34. The support 36 is made of a conductive material such as aluminum. The support 36 provides a gas diffusion chamber 36a therein. The support 36 further provides a plurality of gas holes 36b. The plurality of gas holes 36b extend downward from the gas diffusion chamber 36a. The plurality of gas holes 36b communicate with the plurality of gas holes 34a, respectively. The support 36 further provides a gas inlet 36c. The gas inlet 36c is connected to the gas diffusion chamber 36a. A gas supply pipe 38 is connected to the gas inlet 36c.
[0038] A gas source group 40 is connected to the gas supply pipe 38 via a valve group 41, a flow rate controller group 42, and a valve group 43. The gas source group 40, the valve group 41, the flow rate controller group 42, and the valve group 43 constitute a gas supply unit GS. The gas source group 40 includes a plurality of gas sources. The gas sources of the gas source group 40 include a plurality of gas sources used in the method MT. Each of the valve group 41 and the valve group 43 includes a plurality of opening and closing valves. The flow rate controller group 42 includes a plurality of flow rate controllers. Each of the plurality of flow rate controllers of the flow rate controller group 42 is a mass flow controller or a pressure control type flow rate controller. Each of the plurality of gas sources of the gas source group 40 is connected to the gas supply pipe 38 via a corresponding opening and closing valve of the valve group 41, a corresponding flow rate controller of the flow rate controller group 42, and a corresponding opening and closing valve of the valve group 43.
[0039] The plasma processing apparatus 1 may further include a shield 46. The shield 46 is detachably provided along the inner wall surface of the chamber body 12. The shield 46 is also provided on the outer periphery of the support portion 13. The shield 46 prevents by-products of the plasma processing from adhering to the chamber body 12. The shield 46 is formed, for example, by forming a corrosion-resistant film on the surface of a member made of aluminum. The corrosion-resistant film may be a film made of a ceramic such as yttrium oxide.
[0040] The plasma processing apparatus 1 may further include a baffle member 48. The baffle member 48 is provided between the support 13 and the side wall of the chamber body 12. The baffle member 48 is formed by forming a corrosion-resistant film on the surface of a plate-like member made of aluminum, for example. The corrosion-resistant film may be a film made of ceramic, such as yttrium oxide. The baffle member 48 provides a plurality of through holes. An exhaust port 12e is provided below the baffle member 48 and at the bottom of the chamber body 12. An exhaust device 50 is connected to the exhaust port 12e via an exhaust pipe 52. The exhaust device 50 has a pressure adjustment valve and a vacuum pump, such as a turbo molecular pump.
[0041] The plasma processing apparatus 1 further includes a high-frequency power supply 62 and a bias power supply 64. The high-frequency power supply 62 is configured to generate high-frequency power (hereinafter, referred to as "high-frequency power HF"). The high-frequency power HF has a frequency suitable for generating plasma. The frequency of the high-frequency power HF is, for example, 27 MHz or more and 100 MHz or less. The high-frequency power supply 62 is connected to the upper electrode 30 via a matching device 66. The matching device 66 has a circuit for matching the impedance of the load side (upper electrode 30 side) of the high-frequency power supply 62 to the output impedance of the high-frequency power supply 62. In one embodiment, the high-frequency power supply 62 can constitute a plasma generating unit. The high-frequency power supply 62 may be connected to the lower electrode 18 via the matching device 66.
[0042] The bias power supply 64 is configured to apply an electric bias EB to the lower electrode 18. The electric bias EB has a frequency suitable for attracting ions to the substrate W. The frequency of the electric bias EB is, for example, 100 kHz or more and 40.68 MHz or less. When the electric bias EB is used together with the high frequency power HF, the electric bias EB has a frequency lower than the frequency of the high frequency power HF.
[0043] In one embodiment, the electric bias EB may be a radio frequency bias power (hereinafter referred to as "radio frequency power LF"). In this embodiment, the bias power supply 64 is connected to the lower electrode 18 via a matching box 68 and the electrode plate 16. The matching box 68 has a circuit for matching the impedance of the load side (lower electrode 18 side) of the bias power supply 64 to the output impedance of the bias power supply 64. The plasma processing apparatus 1 may be configured to generate plasma using only the radio frequency power LF. In this case, the bias power supply 64 constitutes a plasma generating unit of one embodiment. In this case, the plasma processing apparatus 1 may not include the radio frequency power supply 62 and the matching box 66.
[0044] In one embodiment, the electrical bias EB may be a pulse of negative DC voltage, which is periodically applied to the bottom electrode 18.
[0045] The plasma processing apparatus 1 further includes a control unit 80. The control unit 80 may be a computer including a processor, a storage unit such as a memory, an input device, a display device, a signal input / output interface, and the like. The control unit 80 controls each unit of the plasma processing apparatus 1. In the control unit 80, an operator can use the input device to input commands and the like to manage the plasma processing apparatus 1. In addition, the control unit 80 can visualize and display the operating status of the plasma processing apparatus 1 using the display device. Furthermore, a control program and recipe data are stored in the storage unit of the control unit 80. The control program is executed by the processor of the control unit 80 to execute various processes in the plasma processing apparatus 1. The processor of the control unit 80 executes the control program and controls each unit of the plasma processing apparatus 1 according to the recipe data, whereby at least some or all of the steps of the method MT are executed in the plasma processing apparatus 1.
[0046] Referring again to FIG. 1, the method MT will be described in detail. Hereinafter, the method MT will be described by taking as an example a case where the method MT is applied to the substrate W shown in FIG. 2 using the plasma processing apparatus 1. The control of the control unit 80 for each part of the plasma processing apparatus 1 will also be described. In addition to FIG. 1, the following description will refer to FIG. 4, FIG. 5, FIG. 6, FIG. 7, and FIG. 8. FIG. 4 is a partially enlarged cross-sectional view of an example of a substrate in a state after step ST2 of the substrate processing method shown in FIG. 1 is applied. FIG. 5 is an example of a timing chart related to the substrate processing method shown in FIG. 1. FIG. 6 is another example of a timing chart related to the substrate processing method shown in FIG. 1. FIG. 7 is a partially enlarged cross-sectional view of an example of a substrate in a state where a film is formed on a sidewall surface in the substrate processing method shown in FIG. 1. FIG. 8 is a partially enlarged cross-sectional view of an example of a substrate in a state after the substrate processing method shown in FIG. 1 is applied.
[0047] In each of FIG. 5 and FIG. 6, "ON" of the precursor gas indicates that the precursor gas is supplied into the chamber 10, and "OFF" of the precursor gas indicates that the precursor gas is not supplied into the chamber 10. In addition, "ON" of the first gas indicates that the first gas is supplied into the chamber 10, and "OFF" of the first gas indicates that the first gas is not supplied into the chamber 10. In addition, "ON" of the second gas indicates that the second gas is supplied into the chamber 10, and "OFF" of the second gas indicates that the second gas is not supplied into the chamber 10. In addition, "ON" of the high frequency power HF indicates that the high frequency power HF is supplied, and "OFF" of the high frequency power HF indicates that the high frequency power HF is not supplied. In addition, "ON" of the electric bias EB indicates that the electric bias EB is applied to the lower electrode 18, and "OFF" of the electric bias EB indicates that the electric bias EB is not applied to the lower electrode 18.
[0048] 1, the method MT begins with step ST1. In step ST1, a substrate W is prepared. The substrate W is placed on a substrate support 14 in a chamber 10 and held by an electrostatic chuck 20.
[0049] The method MT may further include step ST2. In step ST2, the film EF of the substrate W is etched as shown in Fig. 4. That is, the film EF is partially etched in the film thickness direction to a position between its upper surface and lower surface.
[0050] In step ST2, an etching gas is supplied into the chamber 10. The etching gas is selected according to the type of the film EF. When the film EF is a silicon-containing film, the etching gas contains one or more of a fluorocarbon gas, a hydrofluorocarbon gas, a halogen-containing gas, and the like. The halogen-containing gas is, for example, HBr, Cl, or the like. 2etc. The etching gas may further include a rare gas. In step ST2, plasma is generated from the etching gas in the chamber 10. The film EF is etched by chemical species from the plasma. The etching in step ST2 increases the depth of the recess OP to a position inside the film EF. Also, the etching in step ST2 provides the film EF, together with the mask MK, with a sidewall surface SS that defines the recess OP.
[0051] For step ST2, the control unit 80 controls the gas supply unit GS to supply an etching gas into the chamber 10. The control unit 80 also controls the exhaust unit 50 to set the pressure of the gas in the chamber 10 to a designated pressure. The control unit 80 also controls the plasma generation unit to generate plasma from the etching gas. In the plasma processing apparatus 1, the control unit 80 controls the high frequency power supply 62 and / or the bias power supply 64 to supply high frequency power HF and / or an electric bias EB.
[0052] The method MT does not necessarily include step ST2. In this case, the substrate W shown in FIG. 4 is placed on the substrate support 14 in the chamber 10 and held by the electrostatic chuck 20 in step ST1.
[0053] As shown in Figures 1, 5, and 6, the method MT further includes a step STa and a step STb. The steps STa and STb are alternately repeated. That is, a cycle CYA including the steps STa and STb is performed multiple times. The alternate repetition of the steps STa and STb is performed to form a film PF on the side wall surface SS, as shown in Figure 7. The film PF can function as a protective film that protects the side wall surface SS in the etching of the step STc described below.
[0054] In step STa, a precursor gas is supplied into the chamber 10. The precursor gas includes a precursor from which a film PF is formed. In step ST2, the precursor is adsorbed on the surface of the substrate W. The surface of the substrate W includes a sidewall surface SS. The precursor gas is selected according to the material of the film PF. The precursor gas is, for example, a silicon-containing gas such as an aminosilane gas.
[0055] In step STa, the precursor may be adsorbed on the entire surface of the substrate W. Alternatively, the amount of the precursor adsorbed on the surface of the substrate W in step STa may vary depending on the position on the surface of the substrate W. For example, the amount of the precursor adsorbed on the surface of the substrate W may have a distribution such that the amount of the precursor adsorbed on the surface of the substrate W decreases with increasing depth position in the substrate W. In the latter case, in step STa, at least one of the conditions (1) to (5) is satisfied. In the condition (1), the gas pressure in the chamber 10 during the execution of step STa is set to a pressure lower than the pressure at which the precursor is adsorbed on the entire surface of the substrate W when other processing conditions are the same. In the condition (2), the processing time of step STa is set to a time shorter than the processing time at which the precursor is adsorbed on the entire surface of the substrate W when other processing conditions are the same. In the condition (3), the dilution degree of the precursor gas is set to a value higher than the dilution degree at which the precursor is adsorbed on the entire surface of the substrate W when other processing conditions are the same. Under condition (4), the temperature of the substrate support 14 during step STa is set to a temperature lower than the temperature at which the precursors are adsorbed to the entire surface of the substrate W when other processing conditions are the same. Condition (5) may be applied when plasma is generated in step STa. Under condition (5), the absolute value of the high frequency power (high frequency power HF and / or electric bias EB) is set to a value smaller than the absolute value at which the precursors are adsorbed to the entire surface of the substrate W when other processing conditions are the same.
[0056] For the process STa, the control unit 80 controls the gas supply unit GS to supply a precursor gas into the chamber 10. The control unit 80 also controls the exhaust unit 50 to set the pressure of the gas in the chamber 10 to a designated pressure. In the process STa, the control unit 80 may control the plasma generation unit to generate plasma from the precursor gas. In the plasma processing apparatus 1, the control unit 80 may control the high frequency power supply 62 and / or the bias power supply 64 to supply high frequency power HF and / or an electric bias EB.
[0057] As shown in Fig. 1 and Fig. 5, the method MT may further include a step STP1. The step STP1 is performed between the step STa and the step STb. In the step STP1, the internal space 10s of the chamber 10 is purged. In the step STP1, the exhaust device 50 is controlled by the control unit 80 to exhaust the gas in the chamber 10. In the step STP1, the excess precursor on the surface of the substrate W and the precursor in the gas phase that is not adsorbed on the substrate W may be removed. In the step STP1, the method MT may not include the step STP1, as shown in Fig. 6.
[0058] In step STb, a first chemical species and a second chemical species are supplied to the substrate W. The first chemical species forms a film PF from a precursor on the side wall surface SS. The first chemical species is generated by generating plasma from a first gas. The first gas is, for example, O 2 The first gas is an oxygen-containing gas such as a gas. When the first gas is an oxygen-containing gas, oxygen ions and / or radicals are formed as the first chemical species. When the first gas is an oxygen-containing gas and the precursor contains silicon, a silicon oxide film is formed as the film PF.
[0059] In step STb, the second chemical species suppresses an increase in the thickness of the film PF. The second chemical species suppresses an increase in the thickness of the film PF by etching the film PF and / or the precursor or by inhibiting the formation of the film PF on the surface of the substrate W. The second chemical species is generated by generating a plasma from a second gas. The second chemical species may be a halogen chemical species. The second chemical species is, for example, a fluorine chemical species. When the second chemical species is a fluorine chemical species, the second gas is CF 4 Such as fluorocarbons, hydrofluorocarbons, nitrogen trifluoride (NF 3 ), and sulfur hexafluoride (SF 6 ) includes at least one of the following:
[0060] In the step STb, the reaction between the precursor and the first chemical species may occur uniformly on the surface of the substrate W. Alternatively, in the step STb, at least one of the conditions (1) to (5) may be satisfied. In the condition (1), the pressure of the gas in the chamber 10 during the step STb is set to a pressure lower than the pressure at which the reaction between the first chemical species and all the precursors on the surface of the substrate W is completed when other processing conditions are the same. In the condition (2), the processing time of the step STb is set to a time shorter than the processing time at which the reaction between the first chemical species and all the precursors on the surface of the substrate W is completed when other processing conditions are the same. In the condition (3), the dilution degree of the first gas is set to a value higher than the dilution degree at which the reaction between the first chemical species and all the precursors on the surface of the substrate W is completed when other processing conditions are the same. In the condition (4), the temperature of the substrate support 14 during the step STb is set to a temperature lower than the temperature at which the reaction between the first chemical species and all the precursors on the surface of the substrate W is completed when other processing conditions are the same. Under condition (5), the absolute value of the high frequency power (high frequency power HF and / or high frequency power LF) is set to a value smaller than the absolute value at which the reaction between the first chemical species and all of the precursors on the surface of the substrate W is completed when other processing conditions are the same.
[0061] For the process STb, the control unit 80 controls the gas supply unit GS to supply the first gas and the second gas into the chamber 10. The ratio of the flow rate of the second gas to the sum of the flow rates of the first gas and the second gas may be 10% or more and 90% or less. The control unit 80 also controls the exhaust device 50 to set the pressure of the gas in the chamber 10 to a designated pressure. The control unit 80 also controls the plasma generation unit to generate plasma from the first gas and the second gas. In the plasma processing device 1, the control unit 80 controls the high frequency power supply 62 and / or the bias power supply 64 to supply the high frequency power HF and / or the electric bias EB. When the high frequency power HF is used, the power level may be 100 W or more. When the high frequency power LF is used, the power level may be greater than 0 W and less than 1000 W. When the electric bias EB is used, the pulsed electric bias EB may be supplied intermittently or periodically in the process STb.
[0062] As shown in Figures 1 and 5, the method MT may further include a step STP2. The step STP2 is performed between the step STb and the step STa. The step STP2 is the same step as the step STP1. Note that, as shown in Figure 6, the method MT may not include the step STP2.
[0063] In step STJ1, it is determined whether or not a stop condition is satisfied. The stop condition is satisfied, for example, when the number of times that steps STa and STb are alternately repeated (the number of cycles CYA) reaches a predetermined number. If it is determined in step STJ1 that the stop condition is not satisfied, the process is executed again from step STa. On the other hand, if it is determined in step STJ1 that the stop condition is satisfied, the process may transition to step STc.
[0064] In step STc, the film EF is further etched to increase the depth of the recess OP. In step STc, an etching gas is supplied into the chamber 10. The etching gas may be the same gas as the etching gas described above in connection with step ST2. In step STc, a plasma is generated from the etching gas in the chamber 10. The film EF is etched by chemical species from the plasma.
[0065] For the process STc, the control unit 80 controls the gas supply unit GS to supply an etching gas into the chamber 10. The control unit 80 also controls the exhaust unit 50 to set the pressure of the gas in the chamber 10 to a designated pressure. The control unit 80 also controls the plasma generation unit to generate plasma from the etching gas. In the plasma processing apparatus 1, the control unit 80 controls the high frequency power supply 62 and / or the bias power supply 64 to supply high frequency power HF and / or an electric bias EB.
[0066] The method MT may end after performing step STc once. Alternatively, a cycle CYB including a plurality of cycles CYA and step STc may be performed a plurality of times. In the latter case, the method MT includes step STJ2. In step STJ2, it is determined whether or not a stop condition is satisfied. The stop condition is satisfied, for example, when the number of cycles CYB reaches a predetermined number. If it is determined in step STJ2 that the stop condition is not satisfied, the cycle CYB is performed again. On the other hand, if it is determined in step STJ2 that the stop condition is satisfied, the method MT ends. At the end of the method MT, the film EF may be in a state where it has been etched until the underlying region UR is exposed, as shown in FIG. 8.
[0067] In the method MT, the side wall surface SS is protected by the film PF when the etching in step STc is performed, and therefore the recess OP is prevented from spreading laterally due to the etching in step STc.
[0068] In the method MT, a film PF is formed on the sidewall surface SS by the reaction between the precursor and the first chemical species. The second chemical species suppresses an increase in the thickness of the film PF, particularly at the opening (i.e., the opening edge) of the recess OP. Therefore, the method MT suppresses blocking of the opening of the recess OP by the film PF.
[0069] In the method MT, the depth position MP in the recess OP where the film PF is formed can be adjusted by adjusting one or both of the flow rate of the second gas and the magnitude of the electric bias. The position MP can be defined as the position where the film PF has the maximum film thickness on the side wall surface SS. Specifically, in the method MT, the depth position MP in the recess OP where the film PF is formed can be adjusted to a deeper position in the depth direction of the recess OP according to an increase in the flow rate of the second gas used in the step STb. In addition, when the flow rate of the second gas used in the step STb is relatively large, the first chemical species is used to react with the second chemical species, and as a result, the formation of the film PF at a deep portion of the recess OP is suppressed.
[0070] In the method MT, the position MP in the depth direction in the recess OP where the film PF is formed can be adjusted to a deeper position in the depth direction of the recess OP according to an increase in the magnitude of the electric bias EB used in the step STb. Furthermore, the adjustment of the magnitude of the electric bias EB makes it possible to adjust the position MP in a range including a deeper position, compared to the adjustment of the flow rate of the second gas. When the magnitude of the electric bias EB increases, etching of the film PF occurs near the opening of the recess OP, and the first chemical species reaches a deep region of the recess OP to modify the precursor. The magnitude of the electric bias EB is the absolute value of the power level of the high frequency power LF or the voltage level of the pulse of the negative DC voltage.
[0071] In one embodiment, the magnitude of the electric bias EB may be changed during the alternating repetition of steps STa and STb, i.e., during multiple cycles CYA. According to this embodiment, during the alternating repetition of steps STa and STb, it is possible to change the position MP in the depth direction in the recess OP where the film PF is formed.
[0072] In one embodiment, the multiple cycles CYB include a first cycle and a second cycle. The first cycle and the second cycle are performed in sequence. The magnitude of the electric bias EB applied to the lower electrode 18 in the step STb in the first cycle may be different from the magnitude of the electric bias EB applied to the lower electrode 18 in the step STb in the second cycle.
[0073] In one embodiment, the magnitude of the electric bias EB used in the step STb in the second cycle may be greater than the magnitude of the electric bias EB used in the first cycle. For example, the magnitude of the electric bias EB used in the step STb may be increased as the number of times the cycle CYB is performed increases. According to this embodiment, it is possible to form the film PF at a deeper position in the recess OP according to the depth of the recess OP.
[0074] In one embodiment, as shown in Fig. 5, the first gas and the second gas may be continuously supplied into the chamber 10 while the steps STa and STb are alternately repeated. In this embodiment, the plasma of the first gas and the second gas is generated only during the period when the step STb is performed. Alternatively, as shown in Fig. 6, the first gas and the second gas may be supplied only during the period when the step STb is performed. Note that in the example shown in Fig. 6, the method MT may also include steps STP1 and STP2 as in the example shown in Fig. 5.
[0075] FIG. 9 is referred to below. FIG. 9 is a partially enlarged cross-sectional view of an example of a substrate before the alternate repetition of steps STa and STb is applied in the substrate processing method shown in FIG. 1. In one embodiment, before the alternate repetition of steps STa and STb is applied to the substrate W, as shown in FIG. 9, a deposit DP may be present on the sidewall surface SS of the substrate W. For example, the deposit DP may be present on the upper part of the mask MK and on the sidewall surface SS in the vicinity of the opening of the recess OP. The deposit DP is a by-product generated by the etching of step ST2. When the film EF is a silicon-containing film as described above, the deposit DP may contain silicon. The deposit DP may be formed on the sidewall surface SS in the vicinity of the opening of the recess OP.
[0076] In step STb of one embodiment, a deposit DP present on the upper portion of the mask MK and on the side wall surface SS near the opening of the recess OP is etched (removed) while the side wall surface SS is protected by the film PF, as shown in Figures 7 and 8. Also, in step STb, the film PF is etched near the opening of the recess OP while the side wall surface SS is protected by the film PF. When the deposit DP contains silicon, the process gas used in step STb contains an oxygen-containing gas as the first gas and a fluorine-containing gas as the second gas. The oxygen-containing gas is, for example, O 2 The fluorine-containing gas is CF 4 The gas includes at least one of fluorocarbons, hydrofluorocarbons, nitrogen trifluoride, and sulfur hexafluoride. In one embodiment, the flow rate of the fluorine-containing gas in the process gas used in the step STb is greater than the flow rate of the oxygen-containing gas in the process gas. According to the method MT, it is possible to protect the side wall surface SS by the film PF while suppressing the blocking of the opening of the recess OP by the deposit DP.
[0077] Reference will now be made to Fig. 10, which illustrates a substrate processing system according to an exemplary embodiment. In the method MT, the substrate processing system PS illustrated in Fig. 10 may be used.
[0078] The substrate processing system PS includes stages 2a-2d, containers 4a-4d, a loader module LM, an aligner AN, load lock modules LL1, LL2, process modules PM1-PM6, a transfer module TF, and a controller MC. The number of stages, containers, and load lock modules in the substrate processing system PS may be any number equal to or greater than one. The number of process modules in the substrate processing system PS may be any number equal to or greater than two.
[0079] The stages 2a to 2d are arranged along one edge of the loader module LM. The containers 4a to 4d are mounted on the stages 2a to 2d, respectively. Each of the containers 4a to 4d is, for example, a container called a FOUP (Front Opening Unified Pod). Each of the containers 4a to 4d is configured to accommodate a substrate W therein.
[0080] The loader module LM has a chamber. The pressure in the chamber of the loader module LM is set to atmospheric pressure. The loader module LM has a transport device TU1. The transport device TU1 is, for example, an articulated robot, and is controlled by the controller MC. The transport device TU1 is configured to transport the substrate W through the chamber of the loader module LM. The transport device TU1 can transport the substrate W between each of the containers 4a to 4d and the aligner AN, between the aligner AN and each of the load lock modules LL1, LL2, and between each of the load lock modules LL1, LL2 and each of the containers 4a to 4d. The aligner AN is connected to the loader module LM. The aligner AN is configured to adjust the position of the substrate W (calibrate the position).
[0081] Each of the load lock modules LL1 and LL2 is provided between the loader module LM and the transfer module TF. Each of the load lock modules LL1 and LL2 provides a preliminary reduced pressure chamber.
[0082] The transfer module TF is connected to each of the load lock modules LL1 and LL2 via gate valves. The transfer module TF has a transfer chamber TC that can be depressurized. The transfer module TF has a transfer apparatus TU2. The transfer apparatus TU2 is, for example, an articulated robot, and is controlled by a controller MC. The transfer apparatus TU2 is configured to transfer the substrate W via the transfer chamber TC. The transfer apparatus TU2 can transfer the substrate W between each of the load lock modules LL1, LL2 and each of the process modules PM1 to PM6, and between any two of the process modules PM1 to PM6.
[0083] Each of the process modules PM1 to PM6 is an apparatus configured to perform a dedicated substrate processing. One of the process modules PM1 to PM6 is a plasma processing apparatus used in the process ST2 and the process STc. Another of the process modules PM1 to PM6 may be a plasma processing apparatus used in the process STc. The plasma processing apparatus used in each of the processes ST2 and STc may have the same configuration as the plasma processing apparatus 1.
[0084] Another process module among the process modules PM1 to PM6 is a plasma processing apparatus used to alternately repeat steps STa and STb. The plasma processing apparatus used to alternately repeat steps STa and STb may have the same configuration as the plasma processing apparatus 1.
[0085] In the substrate processing system PS, the control unit MC is configured to control each part of the substrate processing system PS. The control unit MC controls each part of the plasma processing apparatus so as to etch the film EF in step ST2. The control unit MC controls each part of the plasma processing apparatus so as to form a film PF on the side wall surface SS in the alternate repetition of steps STa and STb. The control unit MC controls each part of the plasma processing apparatus so as to etch the film EF in step STc. The control of the plasma processing apparatus of the substrate processing system PS in each of these steps is similar to the control of each part of the plasma processing apparatus 1 by the control unit 80 described above. This substrate processing system PS can transport the substrate W between process modules without exposing it to the atmosphere during the execution of the method MT.
[0086] Although various exemplary embodiments have been described above, the present invention is not limited to the above-described exemplary embodiments, and various additions, omissions, substitutions, and modifications may be made. In addition, elements in different embodiments can be combined to form other embodiments.
[0087] For example, the plasma processing apparatus used to perform the method MT may be a capacitively coupled plasma processing apparatus different from the plasma processing apparatus 1. The plasma processing apparatus used to perform the method MT may be a type of plasma processing apparatus different from the capacitively coupled type. Such a plasma processing apparatus is, for example, an inductively coupled plasma processing apparatus, an electron cyclotron resonance (ECR) plasma processing apparatus, or a plasma processing apparatus that generates plasma from a gas by surface waves such as microwaves.
[0088] Alternatively, after partially etching the film EF as in step ST2, a system for optically measuring a pattern shape may be used to measure the width of the recess OP before the formation of the film PF (CD before film formation) and calculate the required film formation amount of the film PF. Then, film formation conditions for the film PF may be determined according to the calculated film formation amount. The film formation conditions include the number of cycles CYA, the gas flow rates (the flow rates of the first gas and the second gas), and the magnitude of the electric bias EB. The number of cycles CYA may be determined based on the film formation amount of the film PF per cycle CYA. The gas flow rate and / or the electric bias EB may be determined so that a relationship between the film formation position (position MP) of the film PF or the distribution of the film formation amount of the film PF with respect to the gas flow rate and / or the electric bias EB is acquired in advance, and a desired distribution of the film formation amount of the film PF is obtained based on the relationship.
[0089] Also, using a system that optically measures the pattern shape, the width of the recess OP after the formation of the film PF (CD after deposition), and the deposition amount and / or deposition position of the film PF may be compared with their desired values. If the width of the recess OP after the formation of the film PF (CD after deposition), and the deposition amount and / or deposition position of the film PF have an unacceptable error from the desired values, the deposition conditions may be corrected. In the method MT, the next substrate may be processed under the corrected deposition conditions.
[0090] The system for optically measuring the pattern shape may be incorporated in the substrate processing system. In one example, the system for optically measuring the pattern shape may be connected to a load port (an apparatus including the stages 2a-2d and the containers 4a-4d) of the substrate processing system PS. Alternatively, the system for optically measuring the pattern shape may be connected to the transfer chamber TC. The system for optically measuring the pattern shape may be a system independent of the substrate processing system PS.
[0091] Below, some experiments performed to evaluate Method MT are described, but the experiments described below are not intended to limit the present disclosure.
[0092] (Experiments 1 to 4)
[0093] In the first to fourth experiments, a plurality of sample substrates having the same structure as the substrate W shown in FIG. 4 were prepared. In each of the sample substrates, the mask MK was made of polycrystalline silicon and had a thickness of about 300 nm (0.3 μm). In each of the sample substrates, the film EF was made of a silicon oxide film. The recess OP had a depth of about 2000 nm (2.0 μm). In the first to fourth experiments, the alternate repetition of steps STa and STb was applied to the sample substrates to form a film PF on the side wall surface SS. The first gas was O 2 gas, and CF 4 The flow rates of the second gas in the step STb in the first to fourth experiments were 0 sccm, 50 sccm, 100 sccm, and 150 sccm, respectively. Other conditions in the first to fourth experiments are shown below. <Conditions of Experiments 1 to 4> Process STa Process gas containing precursor gas: aminosilane gas, O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) Processing time: 2 seconds Process STP1 Gas supplied into chamber 10: O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) Processing time: 1.5 seconds Process STb First gas and second gas: O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) High frequency power HF:0W High frequency power LF: 40MHz, 150W Processing time: 2 seconds Process STP2 Gas supplied into chamber 10: O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) Processing time: 1 second Number of times step STa and step Sb are alternately repeated: 50 times
[0094] In the first to fourth experiments, the difference between the width of the recess OP before the formation of the film PF and the width of the recess OP after the formation of the film PF, that is, the distribution of ΔCD in the depth direction in the recess OP was obtained. Here, ΔCD reflects the thickness of the film PF. FIG. 11(a), FIG. 11(b), FIG. 11(c), and FIG. 11(d) are graphs showing the distribution of ΔCD in the depth direction obtained in the first to fourth experiments, respectively. In these figures, Z on the vertical axis indicates the position in the depth direction in the recess OP. The position where Z is 0.0 μm is the position of the upper surface of the mask MK. The absolute value of the negative value of Z represents the distance in the depth direction from the upper surface of the mask MK. When the second gas was not supplied in the process STb, the thickness of the film PF was large near the opening of the recess OP, as shown in FIG. 11(a). On the other hand, as shown in (b), (c), and (d) of FIG. 11, it was confirmed that the thickness of the film PF at the opening of the recess OP can be reduced by supplying the second chemical species derived from the second gas to the substrate in the step STb. That is, it was confirmed that the blocking of the recess OP by the film PF can be suppressed by supplying the second gas into the chamber and supplying the second chemical species to the substrate in the step STb. It was also confirmed that the position where the film PF is formed in the recess OP is adjusted to a deeper position as the flow rate of the second gas used in the step STb is higher. It was also confirmed that, as shown in (d) of FIG. 11, when the flow rate of the second gas used in the step STb is relatively high, the formation of the film PF at a deep position of the recess OP is suppressed.
[0095] (Experiments 5 to 7)
[0096] In the fifth to seventh experiments, a plurality of sample substrates having the same structure as the substrate W shown in FIG. 4 were prepared. In each of the sample substrates, the mask MK was made of polycrystalline silicon and had a thickness of about 300 nm (0.3 μm). In each of the sample substrates, the film EF was made of a silicon oxide film. The recess OP had a depth of about 2000 nm (2.0 μm). In the fifth to seventh experiments, the process STa and the process STb were alternately repeated for the sample substrates to form a film PF on the side wall surface SS. The first gas was O 2 gas, and CF 4 Gas was used. The magnitude of the high frequency power LF in the process STb in the fifth to seventh experiments was 150 W, 250 W, and 500 W. Other conditions in the fifth to seventh experiments are as follows. <Conditions of Experiments 5 to 7> Process STa Process gas containing precursor gas: aminosilane gas, O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) Processing time: 2 seconds Process STP1 Gas supplied into chamber 10: O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) Processing time: 1.5 seconds Process STb First gas and second gas: O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) High frequency power HF:0W High frequency power LF: 40MHz Processing time: 2 seconds Process STP2 Gas supplied into chamber 10: O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) Processing time: 1 second Number of times step STa and step Sb are alternately repeated: 50 times
[0097] In the fifth to seventh experiments, the distribution of ΔCD in the depth direction in the recess OP was obtained in the same manner as in the first to fourth experiments. FIG. 12(a), FIG. 12(b), and FIG. 12(c) are graphs showing the distribution of ΔCD in the depth direction obtained in the fifth to seventh experiments, respectively. As shown in FIG. 12(a), FIG. 12(b), and FIG. 12(c), it was confirmed that the film PF is formed at a deeper position in the recess OP as the magnitude of the high frequency power LF (i.e., the electric bias EB) used in the process STb increases. It was also confirmed that the adjustment of the magnitude of the electric bias EB makes it possible to adjust the position (position MP) where the film PF is formed in a range including a deeper position, compared to the adjustment of the flow rate of the second gas.
[0098] (Experiments 8 to 10)
[0099] In the eighth to tenth experiments, a plurality of sample substrates having the same structure as the substrate W shown in FIG. 4 were prepared. In each of the sample substrates, the mask MK was made of polycrystalline silicon and had a thickness of about 300 nm (0.3 μm). In each of the sample substrates, the film EF was made of a silicon oxide film. The recess OP had a depth of about 2000 nm (2.0 μm). In the eighth to tenth experiments, a deposit DP made of silicon oxide was formed on the side wall surface SS of each of the sample substrates by plasma CVD to obtain a sample substrate having the same structure as the substrate W shown in FIG. 9. Then, in the eighth to tenth experiments, the alternate repetition of steps STa and STb was applied to the sample substrates to form a film PF on the side wall surface SS. The first gas was O 2 gas, and CF 4 The process gas used in the process STb of the eighth to tenth experiments was CF 4 The gas flow rate is O2 Specifically, the flow rate of the O 2 gas in the process gas used in step STb of the eighth experiment was higher than that of the O 3 gas. 2 Gas flow rate and CF 4 The flow rates of the gases were 170 sccm and 280 sccm. In addition, the O 2 Gas flow rate and CF 4 The flow rates of the gases were 100 sccm and 280 sccm. In addition, the O 2 Gas flow rate and CF 4 The gas flow rates were 20 sccm and 280 sccm. Other conditions for the eighth to tenth experiments are as follows. <Conditions for Experiments 8 to 10> Process STa Process gas containing precursor gas: aminosilane gas, O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) Processing time: 2 seconds Process STP1 Gas supplied into chamber 10: O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) Processing time: 1.5 seconds Process STb First gas and second gas: O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) High frequency power HF:0W High frequency power LF: 40MHz, 250W Processing time: 2 seconds Process STP2 Gas supplied into chamber 10: O 2 Gas and CF 4 Gas Mixture Gas pressure in chamber 10: 10 mTorr (1.333 Pa) Processing time: 1 second Number of times step STa and step Sb are alternately repeated: 50 times
[0100] In the eighth to tenth experiments, the distribution of ΔCD in the depth direction at the recess OP was obtained in the same manner as in the first to seventh experiments. Fig. 13(a), Fig. 13(b), and Fig. 13(c) are graphs showing the distribution of ΔCD in the depth direction obtained in the eighth to tenth experiments, respectively. As shown in Fig. 13(a), Fig. 13(b), and Fig. 13(c), the ΔCD obtained in the eighth to tenth experiments had negative values at the position where Z was 0.0 μm, that is, at the position in the depth direction near the opening of the recess OP. From this, it can be seen that the CF 4 Gas flow rate is O 2 It was confirmed that when the flow rate of the CF gas was greater than that of the gas, the deposit DP was etched. Furthermore, the ΔCD obtained in the eighth to tenth experiments was 0 or more at a position deeper than the opening of the recess OP. From this, it was confirmed that the side wall surface SS was protected in the eighth to tenth experiments. Furthermore, when the CF gas in the processing gas was 4 Gas flow rate is O 2 It was confirmed that the greater the gas flow rate, the thinner the thickness of the film PF formed.
[0101] From the foregoing, it will be understood that various embodiments of the present disclosure have been described herein for purposes of illustration, and that various modifications may be made without departing from the scope and spirit of the present disclosure. Accordingly, the various embodiments disclosed herein are not intended to be limiting, with the true scope and spirit being indicated by the appended claims. [Explanation of symbols]
[0102] Reference Signs List 1: plasma processing apparatus, 10: chamber, 14: substrate support, 50: exhaust device, 62: high frequency power source, 64: bias power source, GS: gas supply unit, 80: control unit.
Claims
1. (a) adsorbing a precursor onto a sidewall surface of a substrate, the sidewall surface defining a recess in the substrate; (b) supplying a first chemical species and a second chemical species to the substrate, the first chemical species forming a film from the precursor on the sidewall surface and the second chemical species inhibiting an increase in thickness of the film; (c) after the alternating repetition of (a) and (b), etching the etching film of the substrate with chemical species from plasma generated from an etching gas so as to increase the depth of the recess; A substrate processing method comprising:
2. The method of claim 1 , wherein the second chemical species is a halogen chemical species.
3. The method of claim 2 , wherein the second chemical species is a fluorine chemical species.
4. 4. The method of claim 3, wherein the second chemical species is generated from at least one of a fluorocarbon, a hydrofluorocarbon, nitrogen trifluoride, and sulfur hexafluoride.
5. The method for processing a substrate according to any one of claims 2 to 4, wherein the precursor contains silicon.
6. The substrate processing method of claim 1 , wherein the deposit on the sidewall surface is etched in (b).
7. 7. The substrate processing method according to claim 6, further comprising the step of etching the etching film with chemical species from plasma generated from an etching gas so as to form the recess before the steps (a) and (b) are alternately repeated, the step being such that the deposit is formed on the sidewall surface by the etching of the etching film.
8. the deposit and the precursor contain silicon; the first chemical species is provided from a plasma formed from an oxygen-containing gas; the second chemical species is provided from a plasma formed from a fluorine-containing gas; The substrate processing method according to claim 6 or 7.
9. 9. The substrate processing method according to claim 8, wherein in (b), plasma is generated from a process gas containing the oxygen-containing gas and the fluorine-containing gas, and a flow rate of the fluorine-containing gas in the process gas is greater than a flow rate of the oxygen-containing gas in the process gas.
10. 10. The substrate processing method according to claim 8, wherein the fluorine-containing gas includes at least one of a fluorocarbon, a hydrofluorocarbon, nitrogen trifluoride, and sulfur hexafluoride.
11. 11. The substrate processing method according to claim 1, wherein in (b), an electric bias is applied to a lower electrode of a substrate support that supports the substrate, for attracting ions to the substrate.
12. The substrate processing method according to claim 11 , wherein the magnitude of the electrical bias for attracting ions to the substrate is changed during alternating repetitions of (a) and (b).
13. a first cycle and a second cycle each including alternating repetitions of (a) and (b) and (c) are carried out in sequence; 13. The substrate processing method according to claim 1, wherein a magnitude of an electric bias applied to a lower electrode of a substrate support supporting the substrate in (b) in the first cycle to attract ions to the substrate is different from a magnitude of the electric bias applied to the lower electrode in (b) in the second cycle to attract ions to the substrate.
14. 14. The method of claim 13, wherein a magnitude of the electrical bias used to attract ions to the substrate in (b) in the second cycle is greater than a magnitude of the electrical bias used to attract ions to the substrate in (b) in the first cycle.
15. The substrate processing method according to any one of claims 1 to 14, further comprising the step of purging an internal space of a chamber housing the substrate therein between (a) and (b) and / or between (b) and (a).
16. A chamber; a gas supply configured to supply a precursor gas, a first gas, a second gas, and an etching gas into the chamber; a plasma generating unit configured to generate plasma from the first gas, the second gas, and the etching gas; A control unit configured to control the gas supply unit and the plasma generation unit; Equipped with The control unit is (a) controlling the gas supply unit to supply a precursor gas into the chamber, so that a precursor contained in the precursor gas is adsorbed onto a sidewall surface of a substrate; (b) controlling the gas supply unit and the plasma generator to generate plasma from a first gas and a second gas in the chamber, to generate a first chemical species from the first gas that forms a film from the precursor on the sidewall surface, and generate a second chemical species from the second gas that suppresses an increase in thickness of the film; (c) after alternately repeating (a) and (b), controlling the gas supply unit and the plasma generating unit to generate plasma from the etching gas in the chamber, and etching an etching film of the substrate with chemical species from the plasma generated from the etching gas so as to increase a depth of a recess in the substrate defined by the sidewall surface; It is configured as follows: Plasma processing equipment.
Citation Information
Patent Citations
Manufacturing method of semiconductor device
JP2005150399A
Method of etching film and plasma processing apparatus
JP2019207911A
Technique to deposit sidewall passivation for high aspect ratio cylinder etch
US20160343580A1