Positive electrode active material for lithium secondary battery, positive electrode for lithium secondary battery, and lithium secondary battery

A layered cobalt-free lithium nickel-based composite oxide with tailored particle sizes and nickel concentrations addresses the scarcity of cobalt, enhancing capacity, efficiency, and longevity in lithium secondary batteries.

JP7577772B2Active Publication Date: 2024-11-05SAMSUNG SDI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023001337
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-05-30
Filing Date
2023-01-06
Publication Date
2024-11-05
Estimated Expiration
2043-01-06

AI Technical Summary

Technical Problem

The demand for high-capacity lithium secondary batteries has increased, but the scarcity of cobalt, a key component in traditional positive electrode active materials, poses challenges in ensuring structural stability, capacity, efficiency, and longevity, particularly in layered cobalt-free materials.

Method used

A layered cobalt-free lithium nickel-based composite oxide is developed with a specific particle size distribution and nickel concentration balance, combining secondary and single particles to maintain structural integrity and enhance lithium transfer, thereby improving capacity, efficiency, and life characteristics.

Benefits of technology

The solution ensures high capacity, efficiency, and long-life characteristics in lithium secondary batteries by balancing nickel concentrations and particle sizes, addressing the limitations of traditional cobalt-free materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577772000004
    Figure 0007577772000004
  • Figure 0007577772000005
    Figure 0007577772000005
  • Figure 0007577772000006
    Figure 0007577772000006
Patent Text Reader

Abstract

To provide: a positive electrode active material for a lithium secondary battery, which is a layered cobalt-free positive electrode active material, and by which a capacity and efficiency characteristics are secured, at the same time, structural deterioration due to charge and discharge is suppressed, and thereby, the life characteristics are improved; a positive electrode for the lithium secondary battery, which contains the same; and the lithium secondary battery.SOLUTION: The positive electrode active material for the lithium secondary battery includes a first positive electrode active material that contains a layered cobalt-free lithium-nickel-based composite oxide, has a form of a secondary particle which is formed of a plurality of agglomerated primary particles, and has an average particle size (D50) of 8 μm to 20 μm; and a second positive electrode active material that contains a layered cobalt-free lithium-nickel-based composite oxide, has a form of single-particle form, and has the average particle size (D50) of 1 μm to 7 μm. A molar content of nickel with respect to all elements except for lithium and oxygen in the second positive electrode active material is further greater than a molar content of nickel with respect to all elements except for lithium and oxygen in the first positive electrode active material by 1% by mole to 10% by mole.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a positive electrode for a lithium secondary battery containing the same, and a lithium secondary battery. [Background technology]

[0002] Lithium secondary batteries, which have high energy density and are easy to carry, are mainly used as the driving power source for mobile information terminals such as mobile phones, notebook computers, and smartphones. Recently, active research has been conducted on using high-energy-density lithium secondary batteries as driving power sources or power storage power sources for hybrid and electric vehicles.

[0003] In order to meet these applications, positive electrode active materials that can achieve high capacity, high stability, and long life performance have been studied, and ternary positive electrode active materials of Ni, Co, Mn or Ni, Co, Al are generally used. However, while the demand for large-scale or high-capacity lithium secondary batteries has recently increased rapidly, it is predicted that the supply of positive electrode active materials containing the rare metal cobalt is insufficient. That is, since cobalt is expensive and there are not many remaining reserves, it is necessary to develop a cobalt-free positive electrode active material that does not use cobalt in order to manufacture large-scale or high-capacity batteries. Since the cobalt element plays a key role in forming the structure of the positive electrode active material, removing cobalt causes structural defects, increases resistance, making it difficult to ensure a long life, and causes problems such as reduced capacity and efficiency, resulting in performance degradation.

[0004] Conventionally known cobalt-free positive electrode active materials have an olivine crystal structure such as lithium iron phosphate (LFP), lithium manganese phosphate (LMP), and lithium manganese iron phosphate (LMFP) that do not have a layered structure, and a spinel crystal structure such as lithium manganese oxide (LMO). Although these materials have high structural stability, they have a limitation in that the amount of soluble lithium that can be utilized within the structure is small, resulting in low capacity. Cobalt-free positive electrode active materials with a layered structure have a relatively high lithium content within the structure and excellent capacity and efficiency characteristics, making them suitable as materials for high-capacity batteries, but are structurally unstable and have difficulty in ensuring long life characteristics. Therefore, there is a need to develop a layered cobalt-free positive electrode active material that can achieve high capacity while also improving structural stability to ensure the capacity, efficiency, and life characteristics of lithium secondary batteries at the same time. Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention provides a layered cobalt-free positive electrode active material that ensures capacity and efficiency characteristics, while at the same time suppressing structural deterioration due to charging and discharging, thereby improving life characteristics, a positive electrode, and a lithium secondary battery. [Means for solving the problem]

[0006] In one embodiment, the present invention provides a positive electrode active material for a lithium secondary battery, comprising: a first positive electrode active material including a layered cobalt-free lithium nickel-based composite oxide, which is in the form of secondary particles formed by agglomeration of a plurality of primary particles, and has an average particle size (D50) of 8 μm to 20 μm; and a second positive electrode active material including a layered cobalt-free lithium nickel-based composite oxide, which is in the form of a single particle, and has an average particle size (D50) of 1 μm to 7 μm, wherein the molar content of nickel in the second positive electrode active material relative to all elements excluding lithium and oxygen is 1 mol % to 10 mol % higher than the molar content of nickel in the first positive electrode active material relative to all elements excluding lithium and oxygen.

[0007] In another embodiment, a positive electrode for a lithium secondary battery is provided, comprising a current collector and a positive electrode active material layer disposed on the current collector, the positive electrode active material layer comprising the positive electrode active material described above.

[0008] In another embodiment, a lithium secondary battery is provided that includes a positive electrode containing the positive electrode active material, a negative electrode, and an electrolyte. Effect of the Invention

[0009] The positive electrode active material for a lithium secondary battery according to an embodiment is a layered cobalt-free positive electrode active material, and can simultaneously ensure the capacity, efficiency, and life characteristics of a lithium secondary battery. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic diagram illustrating a lithium secondary battery according to an embodiment. [Diagram 2] 1 is a scanning electron microscope photograph of the positive electrode active material of Example 1. [Diagram 3] 1 is a scanning electron microscope photograph of the positive electrode active material of Example 1. [Figure 4] 1 is a scanning electron microscope photograph of the positive electrode active material of Comparative Example 1. [Diagram 5] 1 is a scanning electron microscope photograph of the positive electrode active material of Comparative Example 1. [Figure 6] 1 is a graph showing high-temperature life characteristics of batteries produced in Example 1 and Comparative Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention is not limited to the embodiments described herein, but may be embodied in many different forms, and should not be construed as limited to the embodiments described herein.

[0012] The terms used herein are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless otherwise clearly indicated in the context.

[0013] As used herein, "combinations thereof" refers to mixtures, laminates, composites, copolymers, alloys, blends, reaction products, and the like of compositions.

[0014] It should be understood that the terms "including," "comprising," or "having" are intended to specify the presence of embodied features, numerals, steps, components, or combinations thereof, and do not preclude the presence or additional possibility of one or more other features, numerals, steps, components, or combinations thereof.

[0015] In the drawings, the thickness of the various layers and regions is exaggerated for clarity, and similar parts are designated by the same reference numerals throughout the specification. When a part such as a layer, film, region, plate, etc. is said to be "on" or "on" another part, this includes not only the case where it is "directly on" the other part, but also the case where there is another part between them. Conversely, when a part is said to be "directly on" another part, it means that there is no other part between them.

[0016] Further, the term "layer" includes not only a shape formed on the entire surface, but also a shape formed on a portion of the surface when observed in a plan view.

[0017] The average particle size can be measured by a method well known to those skilled in the art, for example, by a particle size analyzer or by an optical microscope such as a transmission electron microscope or a scanning electron microscope. Alternatively, the average particle size can be calculated by measuring using a dynamic light scattering method, counting the number of particles for each particle size range, and then calculating the average particle size. Unless otherwise defined, the average particle size can mean the diameter of particles with a cumulative volume of 50% by volume (D50) in the particle size distribution.

[0018] As used herein, "or" is not to be construed in its exclusive sense; for example, "A or B" is to be construed as including A, B, A+B, etc.

[0019] positive electrode active material In one embodiment, the present invention provides a positive electrode active material for a lithium secondary battery, the positive electrode active material comprising: a first positive electrode active material including a layered cobalt-free lithium-nickel based composite oxide, the first positive electrode active material being in the form of secondary particles formed by agglomeration of a plurality of primary particles, and having an average particle size (D50) of 8 μm to 20 μm; and a second positive electrode active material including a layered cobalt-free lithium-nickel based composite oxide, the second positive electrode active material being in the form of a single particle, and having an average particle size (D50) of 1 μm to 7 μm, the second positive electrode active material having a molar content of nickel relative to all elements excluding lithium and oxygen that is 1 mol % to 10 mol % higher than the first positive electrode active material having a molar content of nickel relative to all elements excluding lithium and oxygen.

[0020] In order to stably maintain the layered structure of the positive electrode active material, typically, cobalt element is generally used. However, in one embodiment, a method for maintaining and stabilizing the layered structure without using cobalt is presented.

[0021] As described above, as the demand for high-capacity lithium secondary batteries increases and the rare metal cobalt element is depleted, the development of cobalt-free positive electrode active materials is required, and in particular, the development of layered cobalt-free positive electrode active materials that can achieve high capacity is required. Generally, layered cobalt-free positive electrode active materials have a problem of structural deterioration due to charging and discharging, but in one embodiment, the layered structure that deteriorates is physically maintained by introducing a single particle form. However, in order to compensate for the problem of low lithium diffusion rate in the case of single particles, small particles with an average particle size of 1 μm to 7 μm, preferably 2 μm to 5 μm, i.e., a single particle form is introduced into the second positive electrode active material. This aims to balance the lithium migration rate of the first and second positive electrode active materials and ensure long-term life characteristics by equally dividing the degree of deterioration of the cobalt-free positive electrode active material into polycrystalline structure and single crystal structure.

[0022] However, the single particle type positive electrode active material has a short lithium migration path, excellent crystal structure orientation, and high structural stability, which gives it superior life characteristics, but on the other hand, the lithium migration path is restricted and the specific surface area is small, so that the capacity and efficiency that can be obtained with the same composition are inferior. In one embodiment, in order to solve this trade-off characteristic, the nickel concentration in the second positive electrode active material, which is a small particle in the single particle form, is designed to be further increased to 1 mol% to 10 mol% compared to the nickel concentration in the first positive electrode active material, which is a large particle in the secondary particle form, thereby balancing the deterioration characteristic of the small particles to the large particle level, and successfully securing long life characteristics without decreasing capacity and efficiency.

[0023] For example, when the nickel concentration of the second positive electrode active material minus the nickel concentration of the first positive electrode active material is less than 1 mol%, for example, when the nickel concentrations are the same or the nickel concentration of the first positive electrode active material is higher than that of the second positive electrode active material, the lithium solubility of the second positive electrode active material decreases, resulting in a problem of reduced capacity, and the balance between the amount of lithium solubility and the degradation rate between large particles and small particles is not matched, thereby reducing the extent to which life characteristics can be improved.

[0024] That is, in the field of batteries, capacity, efficiency, and life characteristics are in a trade-off relationship with each other, so it is common to sacrifice one of them to gain other characteristics, but one embodiment presents a method that can simultaneously ensure capacity, efficiency, and life characteristics without such a trade-off.

[0025] The positive electrode active material for lithium secondary batteries may be expressed as a layered cobalt-free positive electrode active material, a cobalt-free nickel-based positive electrode active material, or a cobalt-free nickel-manganese-based positive electrode active material. The term "cobalt-free" may mean that there is no cobalt, that no cobalt is used, or that only a very small amount of cobalt is included. The term "single particle form" means a structure in which particles are not mutually aggregated in morphology and exist as an independent phase, and means that there is no grain boundary within the particle and that the particle exists independently and consists of one particle. The single particle may be expressed as a single body structure, a non-aggregated particle, a monolith structure, or the like, and may be a single crystal.

[0026] In one embodiment, the first positive active material in the form of secondary particles has an average particle diameter of 8 μm to 20 μm, and the second positive active material in the form of single particles has an average particle diameter of 1 μm to 7 μm. Here, the average particle diameter means the diameter of particles with a cumulative volume of 50% by volume in the particle size distribution, i.e., D50. The average particle diameter may be measured through an optical microscope such as a scanning electron microscope or a transmission electron microscope. For example, 30 particles in the form of secondary particles are arbitrarily selected from the scanning electron microscope photograph of the positive active material, and their sizes (particle diameter or major axis length) are measured to obtain a particle size distribution, and D50 is calculated from this, which can be taken as the average particle diameter of the first positive active material. Also, 30 particles in the form of single particles are arbitrarily selected from the scanning electron microscope photograph of the positive active material, and their sizes (particle diameter or major axis length) are measured to obtain a particle size distribution, and D50 is calculated from this, which can be taken as the average particle diameter of the second positive active material.

[0027] The first positive electrode active material may have an average particle size of, for example, 9 μm to 19 μm, 10 μm to 18 μm, or 11 μm to 17 μm. The second positive electrode active material may have an average particle size of, for example, 1 μm to 6 μm, 1 μm to 5 μm, or 2 μm to 4 μm. When the average particle sizes of the first and second positive electrode active materials are within the above ranges, a lithium secondary battery including the first and second positive electrode active materials can achieve high density and high energy density, which is advantageous in simultaneously improving the capacity, efficiency, and life characteristics of the lithium secondary battery.

[0028] In addition, the method of measuring the molar content of nickel may be to perform Energy Dispersive X-ray Spectroscopy (EDS) on a scanning electron microscope photograph of the positive electrode active material, obtain the nickel content in atomic % relative to the total content of elements excluding lithium and oxygen through quantitative analysis, and convert it to mole %. In this case, 30 particles of the first positive electrode active material in the form of secondary particles are selected from the scanning electron microscope photograph of the positive electrode active material, the nickel content of each is calculated, and the arithmetic average is taken as the "molar content of nickel relative to the total content of elements excluding lithium and oxygen in the first positive electrode active material", and 30 particles of the second positive electrode active material in the form of single particles are selected from the scanning electron microscope photograph, the nickel content of each is calculated, and the arithmetic average is taken as the "molar content of nickel relative to the total content of elements excluding lithium and oxygen in the second positive electrode active material". In addition to SEM-EDS, other methods for measuring the nickel content include inductively coupled plasma-mass spectrometry (ICP-MS) and inductively coupled plasma optical emission spectroscopy (ICP-OES).

[0029] In one embodiment, the value obtained by subtracting the "molar content of nickel in the first positive electrode active material relative to all elements excluding lithium and oxygen" from the "molar content of nickel in the second positive electrode active material relative to all elements excluding lithium and oxygen" thus calculated satisfies 1 mol% to 10 mol%. The value obtained by subtracting the nickel concentration of the first positive electrode active material from the nickel concentration of the second positive electrode active material may be, for example, 2 mol% to 10 mol%, 3 mol% to 10 mol%, 4 mol% to 9 mol%, or 1 mol% to 8 mol%. By designing in this way, the capacity, efficiency, and life of a lithium secondary battery using a layered cobalt-free positive electrode active material can be improved at the same time.

[0030] The layered cobalt-free lithium nickel composite oxide of the first positive electrode active material can be represented by, for example, Chemical Formula 1 below.

[0031] [Chemical formula 1] Li x1 Ni a1 Mn b1 M 1 (1-a1-b1) O2

[0032] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Cu, F, Fe, Mg, Mo, Nb, P, S, Si, Sr, Ti, V, W, and Zr, and 0.9≦x1≦1.2, 0.6≦a1≦1, and 0≦b1≦0.4.

[0033] In the above Chemical Formula 1, 0.6≦a1≦0.99 and 0.01≦b1≦0.4 may be satisfied, or 0.6≦a1≦0.90 and 0.10≦b1≦0.4, 0.6≦a1≦0.85 and 0.15≦b1≦0.4, 0.6≦a1≦0.80 and 0.20≦b1≦0.4, or 0.7≦a1≦0.90 and 0.10≦b1≦0.3 may be satisfied.

[0034] The layered cobalt-free lithium nickel composite oxide of the second positive electrode active material can be represented by, for example, Chemical Formula 2 below.

[0035] [Chemical formula 2] Li x2 Ni a2 Mn b2 M 2 (1-a2-b2) O2

[0036] In the above chemical formula 2, M 2 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Cu, F, Fe, Mg, Mo, Nb, P, S, Si, Sr, Ti, V, W, and Zr, and 0.9≦x2≦1.2, 0.6≦a2≦1, and 0≦b2≦0.4.

[0037] In the above Chemical Formula 2, 0.6≦a2≦0.99 and 0.01≦b2≦0.4 may be satisfied, or 0.6≦a2≦0.90 and 0.10≦b2≦0.4, 0.6≦a2≦0.85 and 0.15≦b2≦0.4, 0.6≦a2≦0.80 and 0.20≦b2≦0.4, or 0.7≦a2≦0.90 and 0.10≦b2≦0.3 may be satisfied.

[0038] According to one embodiment, the molar content of nickel in the second positive electrode active material relative to all elements excluding lithium and oxygen is 1 mol% to 10 mol% higher than the molar content of nickel in the first positive electrode active material relative to all elements excluding lithium and oxygen, so that the relationship between Formula 1 and Formula 2 may satisfy 0.02≦(a2-a1)≦0.10, for example, 0.04≦(a2-a1)≦0.10, 0.05≦(a2-a1)≦0.10, or 0.02≦(a2-a1)≦0.80. In this case, it is possible to simultaneously improve capacity, efficiency, and life characteristics while applying a layered cobalt-free positive electrode active material.

[0039] The first positive electrode active material in the form of secondary particles may be, for example, spherical or nearly spherical, and the second positive electrode active material in the form of single particles may be, for example, polyhedral, irregular, or spherical.

[0040] The positive electrode active material for the lithium secondary battery may include 65% to 95% by weight of the first positive electrode active material and 5% to 35% by weight of the second positive electrode active material. For example, the positive electrode active material for the lithium secondary battery may include 65% to 90% by weight of the first positive electrode active material and 10% to 35% by weight of the second positive electrode active material, or 70% to 90% by weight of the first positive electrode active material and 10% to 30% by weight of the second positive electrode active material, or 70% to 80% by weight of the first positive electrode active material and 20% to 30% by weight of the second positive electrode active material. When the above mixing ratio is satisfied, the capacity, efficiency and life characteristics of the lithium secondary battery can be improved at the same time while applying the layered cobalt-free positive electrode active material. For example, if the second positive electrode active material exceeds 35 wt %, the balance with the first positive electrode active material is lost due to lithium solubility, and a trade-off characteristic may occur in which the life characteristics are superior but the capacity and efficiency are poor.

[0041] positive electrode In one embodiment, a positive electrode for a lithium secondary battery is provided, the positive electrode for the lithium secondary battery comprising the positive electrode active material described above. The positive electrode for the lithium secondary battery comprises a current collector and a positive electrode active material layer disposed on the current collector, the positive electrode active material layer comprising the positive electrode active material described above, and may further comprise a binder and / or a conductive material.

[0042] The binder serves to adhere the positive electrode active material particles to each other and to the current collector. Representative examples of the binder include, but are not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin, nylon, etc.

[0043] The positive electrode active material layer may have a binder content of about 1 wt % to about 5 wt % based on the total weight of the positive electrode active material layer.

[0044] The conductive material is used to impart conductivity to the electrodes, and any material that does not cause a chemical change in the constructed battery and is electronically conductive can be used. Examples of the conductive material that can be used include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, carbon nanofiber, and carbon nanotube; metal-based materials containing copper, nickel, aluminum, silver, etc. in the form of metal powder or metal fiber; conductive polymers such as polyphenylene derivatives; and conductive materials containing mixtures of these.

[0045] The positive electrode active material layer may have a conductive material content of 1 wt % to 5 wt % based on the total weight of the positive electrode active material layer.

[0046] The positive electrode current collector may be, but is not limited to, an aluminum foil.

[0047] Lithium secondary battery In one embodiment, a lithium secondary battery is provided that includes a positive electrode and a negative electrode that include the above-described positive electrode active material, a separator positioned between the positive electrode and the negative electrode, and an electrolyte.

[0048] 1 is a schematic diagram showing a lithium secondary battery according to an embodiment. Referring to FIG 1, a lithium secondary battery 100 according to an embodiment includes a battery cell including a positive electrode 114, a negative electrode 112 facing the positive electrode 114, a separator 113 disposed between the positive electrode 114 and the negative electrode 112, and a lithium secondary battery electrolyte impregnated in the positive electrode 114, the negative electrode 112, and the separator 113, a battery container 120 in which the battery cell is housed, and a sealing member 140 for sealing the battery container 120.

[0049] The negative electrode for a lithium secondary battery includes a current collector and a negative electrode active material layer located on the current collector. The negative electrode active material layer includes a negative electrode active material, and may further include a binder and / or a conductive material.

[0050] The negative electrode active material includes a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, a lithium metal alloy, a material capable of being doped and dedoped with lithium, or a transition metal oxide.

[0051] The material capable of reversibly intercalating / deintercalating lithium ions may be a carbon-based negative electrode active material, and may include, for example, crystalline carbon, amorphous carbon, or a combination thereof. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon, hard carbon, mesophase pitch carbide, and calcined coke.

[0052] As the lithium metal alloy, an alloy of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn can be used.

[0053] The material capable of doping and dedoping lithium may be a Si-based negative electrode active material or a Sn-based negative electrode active material. Examples of the Si-based negative electrode active material include silicon, silicon-carbon composite, and SiO x(0 < x < 2), Si-Q alloy (wherein Q is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a Group 15 element, a Group 16 element, a transition metal, a rare earth element, and combinations thereof, and is not Si), examples of the Sn-based negative electrode active material include Sn, SnO2, Sn-R alloy (wherein R is an element selected from the group consisting of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a Group 15 element, a Group 16 element, a transition metal, a rare earth element, and combinations thereof, and is not Sn), etc., and at least one of these can be mixed with SiO2 and used. As the elements Q and R, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and those selected from the group consisting of combinations thereof can be used.

[0054] The silicon-carbon composite may be, for example, a silicon-carbon composite including a core including crystalline carbon and silicon particles, and an amorphous carbon coating layer located on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. The amorphous carbon precursor may be coal-based pitch, mesophase pitch, petroleum-based pitch, coal-based oil, petroleum-based heavy oil, or polymer resin such as phenol resin, furan resin, or polyimide resin. In this case, the content of silicon may be 10% by weight to 50% by weight based on the total weight of the silicon-carbon composite. The content of the crystalline carbon may be 10% by weight to 70% by weight based on the total weight of the silicon-carbon composite, and the content of the amorphous carbon may be 20% by weight to 40% by weight based on the total weight of the silicon-carbon composite. The thickness of the amorphous carbon coating layer may be 5 nm to 100 nm. The average particle size (D50) of the silicon particles may be 10 nm to 20 μm. The average particle size (D50) of the silicon particles may be preferably 10 nm to 200 nm. The silicon particles are present in an oxidized form, and at this time, the atomic ratio of Si:O in the silicon particles, which indicates the degree of oxidation, may be 99:1 to 33:67. x In this case, SiO x In the above, x may range from more than 0 to less than 2. Unless otherwise defined herein, the average particle size (D50) refers to the diameter of particles whose cumulative volume is 50% by volume in the particle size distribution.

[0055] The Si-based or Sn-based negative electrode active material may be mixed with a carbon-based negative electrode active material. When the Si-based or Sn-based negative electrode active material is mixed with the carbon-based negative electrode active material, the mixing ratio by weight may be 1:99 to 90:10.

[0056] The negative active material layer may have a negative active material content of 95 wt % to 99 wt % based on the total weight of the negative active material layer.

[0057] In one embodiment, the negative active material layer may further include a binder and may optionally further include a conductive material. The content of the binder in the negative active material layer may be 1 wt% to 5 wt% based on the total weight of the negative active material layer. In addition, when the negative active material layer further includes a conductive material, the negative active material layer may include 90 wt% to 98 wt% of the negative active material, 1 wt% to 5 wt% of the binder, and 1 wt% to 5 wt% of the conductive material.

[0058] The binder serves to adhere the negative active material particles to each other and to the current collector. The binder may be a water-insoluble binder, a water-soluble binder, or a combination thereof.

[0059] The non-water-soluble binder may be polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, a polymer containing ethylene oxide, an ethylene propylene copolymer, polystyrene, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.

[0060] The water-soluble binder may be a rubber-based binder or a polymeric resin binder. The rubber-based binder may be selected from styrene butadiene rubber, acrylated styrene butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, and combinations thereof. The polymeric resin binder may be selected from polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.

[0061] When a water-soluble binder is used as the negative electrode binder, a cellulose-based compound capable of imparting viscosity as a thickener may be further included. As the cellulose-based compound, one or more of carboxymethylcellulose, hydroxypropylmethylcellulose, methylcellulose, or alkali metal salts thereof may be mixed. As the alkali metal, Na, K, or Li may be used. The amount of the thickener used may be 0.1 to 3 parts by weight based on 100 parts by weight of the negative electrode active material.

[0062] The conductive material is used to impart conductivity to the electrodes, and any material that does not cause a chemical change in the constructed battery and is electronically conductive can be used. Examples of the conductive material that can be used include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, carbon nanofiber, and carbon nanotube; metal-based materials in the form of metal powder or metal fiber, including copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; and conductive materials including mixtures thereof.

[0063] The current collector may be selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0064] The electrolyte includes a non-aqueous organic solvent and a lithium salt.

[0065] The non-aqueous organic solvent acts as a medium through which ions involved in the electrochemical reaction of the battery can move. The non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, alcohol-based, or aprotic solvent. The carbonate-based solvent may be dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. The ester solvent may be methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, decanolide, valerolactone, mevalonolactone, caprolactone, etc. The ether solvent may be dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, etc., and the ketone solvent may be cyclohexanone, etc. In addition, examples of the alcohol solvent that can be used include ethyl alcohol and isopropyl alcohol, and examples of the aprotic solvent that can be used include nitriles such as R-CN (wherein R is a hydrocarbon group having a linear, branched, or cyclic structure and having 2 to 20 carbon atoms, which may contain a double bond, an aromatic ring, or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes.

[0066] The non-aqueous organic solvent may be used alone or in combination of two or more thereof. When two or more thereof are used in combination, the mixing ratio may be appropriately adjusted depending on the desired battery performance, which should be widely understood by those skilled in the art.

[0067] In addition, in the case of the carbonate-based solvent, a cyclic carbonate and a chain carbonate can be mixed and used. In this case, when the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to about 1:9, the performance of the electrolyte is excellent.

[0068] The non-aqueous organic solvent may further include an aromatic hydrocarbon-based organic solvent in addition to the carbonate-based solvent, and the carbonate-based solvent and the aromatic hydrocarbon-based organic solvent may be mixed in a volume ratio of about 1:1 to about 30:1.

[0069] The aromatic hydrocarbon solvent may be an aromatic hydrocarbon compound represented by the following formula I:

[0070] [ka]

[0071] In the above formula I, R 4 ~R 9 are the same or different and are selected from the group consisting of hydrogen, halogen, an alkyl group having 1 to 10 carbon atoms, a haloalkyl group having 1 to 10 carbon atoms, and combinations thereof.

[0072] Specific examples of the aromatic hydrocarbon solvent include benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene, or combinations thereof.

[0073] The electrolyte may further include vinylene carbonate or an ethylene carbonate-based compound of the following formula II as a life-improving additive in order to improve the battery life.

[0074] [ka]

[0075] In the above formula II, R 10 and R 11 are the same or different and are selected from the group consisting of hydrogen, a halogen group, a cyano group, a nitro group, and a fluorinated alkyl group having 1 to 5 carbon atoms, 10 and R 11 At least one of R is selected from the group consisting of a halogen group, a cyano group, a nitro group, and a fluorinated alkyl group having 1 to 5 carbon atoms, with the proviso that10 and R 11 But it's not all hydrogen.

[0076] Representative examples of the ethylene carbonate-based compound include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, fluoroethylene carbonate, etc. When such a life-improving additive is further used, the amount of the additive used can be appropriately adjusted.

[0077] The lithium salt is a material that is dissolved in a non-aqueous organic solvent and acts as a source of lithium ions in a battery to enable basic operation of a lithium secondary battery and to promote the movement of lithium ions between a positive electrode and a negative electrode.

[0078] Representative examples of lithium salts are LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide, LiFSI), LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiN(C x F 2x+1 SO2)(C y F 2y+1 and lithium difluoro(bisoxalato)phosphate, LiCl, LiI, LiB(C2O4)2 (lithium bis(oxalato)borate, LiBOB), and lithium difluoro(oxalato)borate (LiDFOB).

[0079] The concentration of the lithium salt is preferably within the range of 0.1 M to 2.0 M. If the concentration of the lithium salt is within this range, the electrolyte has appropriate conductivity and viscosity, and therefore can exhibit excellent electrolyte performance, and lithium ions can be effectively transferred.

[0080] The separator 113 separates the positive electrode 114 and the negative electrode 112 and provides a path for lithium ions to move, and any separator that is generally used in lithium ion batteries can be used. That is, the separator can be one that has low resistance to the movement of electrolyte ions and has excellent electrolyte humidification ability. For example, the separator can include glass fiber, polyester, polyethylene, polypropylene, polytetrafluoroethylene, or a combination thereof, and can be in the form of a non-woven or woven fabric. For example, polyolefin-based polymer separators such as polyethylene and polypropylene are mainly used in lithium ion batteries, and coated separators containing ceramic components or polymer materials to ensure heat resistance or mechanical strength can also be used, and can be selectively used in a single-layer or multi-layer structure.

[0081] Lithium secondary batteries can be classified into lithium ion batteries, lithium ion polymer batteries, and lithium polymer batteries depending on the type of separator and electrolyte used, into cylindrical, square, coin, pouch, etc. types depending on the shape, and into bulk and thin film types depending on the size. The structure and manufacturing method of these batteries are widely known in this field, so a detailed description will be omitted.

[0082] The lithium secondary battery according to an embodiment has a high capacity and is excellent in storage stability, life characteristics, and high rate characteristics at high temperatures, and can be used in electric vehicles (EVs), hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs), and portable electronic devices.

[0083] Examples of the present invention and comparative examples are described below. The following examples are merely examples of the present invention, and the present invention is not limited to the following examples. EXAMPLES

[0084] Example 1 (1) Manufacturing of positive electrode active material It is in the form of secondary particles formed by agglomeration of multiple primary particles, LiNi 0.75 Mn 0.22 Al 0.03 The first positive electrode active material is 80% by weight of O2 composition, and is a single particle of LiNi 0.80 Mn 0.20 A positive electrode active material is prepared by mixing 20% ​​by weight of a second positive electrode active material having an O2 composition.

[0085] 2 and 3 are scanning electron microscope images of the positive electrode active material prepared in Example 1. Referring to Figs. 2 and 3, it can be seen that the first positive electrode active material, which is in the form of secondary particles and is nearly spherical, and the second positive electrode active material, which is in the form of single particles, are mixed together. The average particle size (D50) of the first positive electrode active material is estimated to be about 12μm, and the average particle size (D50) of the second positive electrode active material is estimated to be at the level of about 2.5μm. In the composition of Example 1, the nickel concentration (80mol%) of the second positive electrode active material was designed to be about 5mol% higher than the nickel concentration (75mol%) of the first positive electrode active material.

[0086] (2) Manufacturing of positive electrodes 95% by weight of the prepared positive electrode active material, 3% by weight of polyvinylidene fluoride binder, and 2% by weight of carbon nanotube conductive material are mixed in N-methylpyrrolidone solvent to prepare a positive electrode active material slurry. The positive electrode active material slurry is applied to an aluminum current collector, dried, and then rolled to prepare a positive electrode.

[0087] (3) Manufacture of lithium secondary batteries A coin half cell is manufactured by using the prepared positive electrode and lithium metal counter electrode, placing a polyethylene polypropylene multilayer separator between them, and injecting an electrolyte solution of 1.0 M LiPF6 lithium salt added to a solvent of ethylene carbonate and diethyl carbonate mixed in a volume ratio of 50:50.

[0088] Example 2 The first positive electrode active material was the same as that used in Example 1, and LiNi was used as the second positive electrode active material. 0.80 Mn 0.20 Although it has an O2 composition, it uses single particles with an average particle size (D50) of approximately 4 μm.

[0089] A positive electrode and a lithium secondary battery are manufactured in the same manner as in Example 1, except that the positive electrode active material is used.

[0090] Comparative Example 1 The first positive electrode active material was the same as that used in Example 1, and LiNi was used as the second positive electrode active material. 0.80 Mn 0.20 Although it has O2 composition, it has a secondary particle form rather than a single particle form. Figures 4 and 5 are scanning electron microscope images of the positive electrode active material of Comparative Example 1. Referring to Figures 4 and 5, it can be seen that the first positive electrode active material (large particles) in the form of secondary particles and the second positive electrode active material (small particles) in the form of secondary particles are mixed together. In Comparative Example 1, the average particle size (D50) of the first positive electrode active material is estimated to be about 12μm, and the average particle size (D50) of the second positive electrode active material is estimated to be at the level of about 2.5μm.

[0091] A positive electrode and a lithium secondary battery were manufactured in the same manner as in Example 1, except that the positive electrode active material was used.

[0092] Comparative Example 2 The first positive electrode active material was the same as that used in Example 1, and LiNi was used as the second positive electrode active material. 0.75 Mn 0.25Although it is O2 composition, single particles having an average particle size (D50) of about 4 μm are used. In the composition of Comparative Example 2, the nickel concentration of the first positive electrode active material and the nickel concentration of the second positive electrode active material are at the same level.

[0093] A positive electrode and a lithium secondary battery are manufactured in the same manner as in Example 1, except that the positive electrode active material is used.

[0094] Comparative Example 3 LiNi 0.80 Mn 0.18 Al 0.02 The first positive electrode active material is O2 composition and has an average particle size (D50) of about 12 μm. The second positive electrode active material is LiNi 0.75 Mn 0.25 The second positive electrode active material has a composition of O2 and uses single particles with an average particle size (D50) of about 4 μm. In the composition of Comparative Example 3, the nickel concentration of the second positive electrode active material is designed to be about 5 mol% lower than the nickel concentration of the first positive electrode active material. A positive electrode and a lithium secondary battery are manufactured in the same manner as in Comparative Example 2, except for using such a positive electrode active material.

[0095] Evaluation example: Charge / discharge capacity and high-temperature life characteristics Each of the coin half-cells according to Examples 1 and 2 and Comparative Examples 1 to 3 was charged under constant current (0.2 C) and constant voltage (4.25 V, 0.05 C cut-off) conditions, then rested for 10 minutes, and discharged under constant current (0.2 C) conditions until the battery reached 3.0 V, to perform initial charging and discharging. The initial charge capacity and initial discharge capacity were measured and shown in Table 1 below, and the ratio of the initial discharge capacity to the initial charge capacity was calculated and shown as efficiency in Table 1 below.

[0096] After the initial charge and discharge, the battery was charged and discharged 50 times at 1C at a high temperature of 45°C. The capacity retention rate, which is the ratio of the capacity at each cycle to the initial discharge capacity during the 50 cycles, was measured and shown in Figure 6. The ratio of the 50th discharge capacity to the initial discharge capacity was evaluated and shown in Table 1 below.

[0097] [Table 1]

[0098] Referring to Table 1 and FIG. 6, it can be seen that in Comparative Example 1, where the second positive active material is in the form of secondary particles and the nickel concentration of the first positive active material is the same as that of the second positive active material, the high-temperature life characteristics are lower than those of Example 1. Also, in Comparative Example 2, where the second positive active material is in the form of single particles and the nickel concentration of the first positive active material is the same as that of the second positive active material, it can be seen that the initial discharge capacity and efficiency are lowered and the life improvement is small. In Comparative Example 3, where the nickel concentration of the single particle second positive active material is lower than that of the first positive active material, it can be seen that the initial charge and discharge efficiency is lowered and the high-temperature life characteristics are also lowered. On the other hand, it can be seen that in Example 1, the capacity and efficiency are high and the high-temperature life characteristics are excellent at the same time.

[0099] Although the preferred embodiments have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concepts defined in the following claims also fall within the scope of the present invention. [Explanation of symbols]

[0100] 100: Lithium secondary battery 112: Negative electrode 113: Separator 114: Positive electrode 120:Battery container 140: Sealing member

Claims

1. A first positive electrode active material including a layered cobalt-free lithium nickel-based composite oxide, the secondary particle form being formed by agglomeration of a plurality of primary particles, and having an average particle size (D50) of 8 μm to 20 μm; A positive electrode active material for a lithium secondary battery, comprising a second positive electrode active material including a layered cobalt-free lithium nickel-based composite oxide, the second positive electrode active material being in a single particle form and having an average particle size (D50) of 1 μm to 7 μm, The molar content of nickel in the second positive electrode active material relative to all elements excluding lithium and oxygen is 1 mol % to 10 mol % higher than the molar content of nickel in the first positive electrode active material relative to all elements excluding lithium and oxygen; The layered cobalt-free lithium nickel composite oxide of the first positive electrode active material is represented by the following chemical formula 1: The layered cobalt-free lithium nickel composite oxide of the second positive electrode active material is a positive electrode active material for lithium secondary batteries represented by the following chemical formula 2: [Chemical formula 1] Li x1 Ni a1 Mn b1 M 1 (1-a1-b1) O 2 In the above formula 1, M 1 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Cu, F, Fe, Mg, Mo, Nb, P, S, Si, Sr, Ti, V, W, and Zr, and 0.9≦x1≦1.2, 0.6≦a1≦1, and 0≦b1≦0.4; [Chemical formula 2] Li x2 Ni a2 Mn b2 M 2 (1-a2-b2) O 2 In the above formula 2, M2 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Cu, F, Fe, Mg, Mo, Nb, P, S, Si, Sr, Ti, V, W, and Zr, and 0.9≦x2≦1.2, 0.6≦a2≦1, and 0≦b2≦0.4; And 0.02≦(a2−a1)≦0.

10.

2. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein the second positive electrode active material has an average particle size (D50) of 2 μm to 5 μm.

3. 2. The positive electrode active material for a lithium secondary battery according to claim 1, wherein a molar content of nickel in the second positive electrode active material relative to all elements excluding lithium and oxygen is 1 mol % to 8 mol % higher than a molar content of nickel in the first positive electrode active material relative to all elements excluding lithium and oxygen.

4. the first positive electrode active material is spherical; The positive electrode active material for a lithium secondary battery according to claim 1 , wherein the second positive electrode active material is polyhedral, irregular, or spherical.

5. 2. The positive electrode active material for a lithium secondary battery according to claim 1, comprising 65% to 95% by weight of a first positive electrode active material and 5% to 35% by weight of a second positive electrode active material.

6. 3. The positive electrode active material for a lithium secondary battery according to claim 2, comprising 65% to 95% by weight of a first positive electrode active material and 5% to 35% by weight of a second positive electrode active material.

7. A positive electrode active material layer is disposed on a current collector, The positive electrode active material layer comprises the positive electrode active material according to any one of claims 1 to 6.

8. A lithium secondary battery comprising the positive electrode according to claim 7, a negative electrode, and an electrolyte.

Citation Information

Patent Citations

  • Positive electrode active material for lithium secondary battery, manufacturing method thereof, and lithium secondary battery containing the same

    JP2023026409A

  • Positive electrode and nonaqueous electrolyte secondary battery using the same

    JP2023091566A

  • Positive electrode material, its preparation method and lithium ion battery

    JP2023501071A

  • Non-aqueous electrolyte secondary battery

    WO2023054308A1