Phenolic compound, phenolic curing agent, thermosetting resin composition, and method for producing phenolic compound

A phenol compound with a specific structure is used as a curing agent to improve the handling properties and thermal performance of thermosetting resin compositions, resulting in a cured product with enhanced thermal conductivity and heat resistance.

JP7577932B2Active Publication Date: 2024-11-06SUMITOMO BAKELITE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020090455
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-25
Publication Date
2024-11-06
Estimated Expiration
2040-05-25

AI Technical Summary

Technical Problem

Conventional thermosetting resin compositions, such as those described in Patent Document 1, suffer from poor handling properties and have cured products with inadequate thermal conductivity and heat resistance.

Method used

A phenol compound represented by a specific general formula is used as a curing agent, which improves the handleability of the thermosetting resin composition and enhances the thermal conductivity and heat resistance of the cured product.

Benefits of technology

The phenol compound provides a thermosetting resin composition with excellent handling properties and a cured product exhibiting high thermal conductivity and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577932000017
    Figure 0007577932000017
  • Figure 0007577932000018
    Figure 0007577932000018
  • Figure 0007577932000001
    Figure 0007577932000001
Patent Text Reader

Abstract

To provide.SOLUTION: A phenolic compound is represented by General formula (1). (In the General formula (1), X and Q independently represent a C1-6 alkyl group or a C1-6 alkoxy group. A plurality of X or a plurality of Q may be the same or different).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel phenolic compound, a phenolic curing agent, a thermosetting resin composition, and a method for producing the phenolic compound. [Background technology]

[0002] Phenol compounds have been used in various applications such as resin additives, antioxidants, pharmaceuticals, agricultural chemicals, dyes, etc. Among these, they are widely used as curing agents for thermosetting resin compositions.

[0003] In recent years, there has been an increasing demand for insulating materials constituting electric and electronic devices with improved heat dissipation properties, and various developments have been made to improve the heat dissipation properties of insulating materials. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a thermosetting resin composition containing a bisphenol A type epoxy resin, a novolac type phenolic resin, and an imidazole-based curing accelerator. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-193504 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, as a result of investigations by the present inventors, it was found that the thermosetting resin composition described in Patent Document 1 has room for improvement in terms of handleability, and furthermore, the cured product obtained from the composition has room for improvement in terms of thermal conductivity and heat resistance. [Means for solving the problem]

[0006] The present inventors have newly discovered a phenolic compound having a specific structure, and further discovered that when the phenolic compound is used as a curing agent, a thermosetting resin composition containing the curing agent has improved handleability, and further discovered that a cured product obtained from the composition has excellent thermal conductivity and heat resistance, thereby completing the present invention. That is, the present invention can be described as follows.

[0007] According to the present invention, A phenol compound represented by the following general formula (1) is provided. [ka] (In general formula (1), X and Q each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. A plurality of X's or a plurality of Q's may be the same or different.) According to the present invention, A curing agent containing a phenol compound represented by the general formula (1) is provided. According to the present invention, A thermosetting resin composition is provided, comprising a thermosetting resin and the curing agent. According to the present invention, The following general formula (a) [ka] (In general formula (a), X represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. A plurality of X's may be the same or different.) and a compound represented by the following general formula (b): [ka] (In general formula (b), Q represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. A plurality of Q's may be the same or different.) and a step of reacting a compound represented by the general formula (1) with the compound represented by the general formula (1). Effect of the Invention

[0008] According to the novel phenol compound of the present invention, by using the phenol compound as a curing agent, it is possible to provide a thermosetting resin composition having excellent handleability, and further to provide a cured product having excellent thermal conductivity and heat resistance. [Brief description of the drawings]

[0009] [Figure 1] 1 is a schematic cross-sectional view showing a configuration of a metal base substrate according to an embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing a configuration of a power module according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference symbols, and descriptions will be omitted as appropriate. The drawings are schematic views and do not correspond to actual dimensional ratios. Furthermore, "~" indicates "above" to "below" unless otherwise specified.

[0011] [Phenol compounds] The novel phenol compound of the present embodiment can be represented by the following general formula (1).

[0012] [ka]

[0013] In general formula (1), X and Q each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. A plurality of X's or a plurality of Q's may be the same or different.

[0014] Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a hexyl group, etc. The number of carbon atoms in the alkyl group is preferably 1 to 4, and more preferably 1 to 3.

[0015] Examples of the alkoxy group having 1 to 6 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a pentyloxy group, a hexyloxy group, etc. The number of carbon atoms of the alkoxy group is preferably 1 to 4, and more preferably 1 to 3.

[0016] From the viewpoint of the effects of the present invention, X is preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and particularly preferably a hydrogen atom.

[0017] From the viewpoint of the effects of the present invention, Q is preferably a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and particularly preferably a hydrogen atom.

[0018] The phenol compound of the present embodiment can be used in various applications such as a curing agent for a thermosetting resin composition, an additive such as an antioxidant, and the like, and can be particularly suitably used as a curing agent for a thermosetting resin composition. By using the phenol compound as a curing agent, it is possible to provide a thermosetting resin composition that is easy to handle, and further to provide a cured product that is excellent in thermal conductivity and heat resistance.

[0019] [Method of producing phenolic compounds] The method for producing a phenol compound represented by general formula (1) of this embodiment includes reaction steps shown in the following reaction scheme.

[0020] [ka]

[0021] In formula (a), X has the same meaning as in formula (1), and in formula (b), Q has the same meaning as in formula (1).

[0022] Specifically, in this step, hydroxyphenols (a) represented by general formula (a), benzoic acids (b) represented by general formula (b), a condensing agent, and a reaction solvent are added, stirred and mixed to react the compound (a) with the compound (b), thereby synthesizing the phenol compound (1) represented by general formula (1). The compound can also be synthesized by a dehydration condensation reaction using an acid catalyst. The reaction temperature is about 0 to 100°C, the mixing time is 30 minutes to 48 hours, and the reaction pressure is normal pressure. Examples of the reaction solvent include acetone, THF, DMF, toluene, xylene, NMP, MEK, cyclohexanone, MIBK, PGME, and PGMEA.

[0023] The condensing agent may be a conventionally known one, such as N-(3-dimethylaminopropyl)-N-ethylcarbodiimide hydrochloride, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride, triphenyl phosphite, dicyclohexylcarbodiimide, N,N'-carbonyldiimidazole, dimethoxy-1,3,5-triazinylmethylmorpholinium, O-(benzotriazol-1-yl)-N,N,N',N'-tetramethyluronium tetrafluoroborate, O-(benzotriazol-1-yl)-N,N,N',N'-tetramethyluronium hexafluorophosphate, (2,3-dihydro-2-thioxo-3-benzoxazolyl)diphenylphosphonate, dicyclohexylcarbodiimide, etc. The amount of the condensing agent used is preferably 2 to 3 times the molar amount of the benzoic acids (b), more preferably 2 to 2.5 times the molar amount.

[0024] After the reaction step, purification steps such as concentration, extraction, and drying of the reaction solution are carried out by a conventional method, whereby the phenol compound (1) represented by the general formula (1) can be synthesized.

[0025] [Thermosetting resin composition] The thermosetting resin composition of the present embodiment contains a thermosetting resin and a curing agent containing a phenol compound (1) represented by general formula (1).

[0026] (thermosetting resin) As the thermosetting resin, any known thermosetting resin can be used as long as it can exhibit the effects of the present invention. In the present embodiment, examples of the thermosetting resin include a thermosetting compound containing a mesogenic structure (mesogenic skeleton) in the molecule and a thermosetting compound not containing a mesogenic structure in the molecule.

[0027] Examples of the thermosetting resin include epoxy resin, phenoxy resin, polyimide resin, benzoxazine resin, unsaturated polyester resin, phenol resin, melamine resin, silicone resin, bismaleimide resin, acrylic resin, and phenol derivatives and their derivatives, etc. As these thermosetting resins, monomers, oligomers, and polymers having two or more reactive functional groups in one molecule can be used, and the molecular weight and molecular structure thereof are not particularly limited. These may be used alone or in combination of two or more.

[0028] The content of the thermosetting resin is, for example, preferably 0.1% by mass or more and 80% by mass or less, more preferably 0.5% by mass or more and 70% by mass or less, based on the resin component (100% by mass) of the thermosetting resin composition not including the filler. When the content is equal to or more than the lower limit, the curability is improved and it is easy to form the resin layer. When the content is equal to or less than the upper limit, the storage stability of the resin layer is further improved, and the thermal conductivity of the resin layer is further improved.

[0029] (hardening agent) The curing agent contains a phenol compound (1) represented by general formula (1). In this embodiment, by including the phenol compound (1), it is possible to provide a cured product having excellent thermal conductivity and heat resistance.

[0030] The curing agent may include other curing agents besides the phenol compound (1). The other curing agents are selected according to the type of thermosetting resin, and are not particularly limited as long as they react with the thermosetting resin. Other curing agents include phenolic resin curing agents, amine curing agents, acid anhydride curing agents, mercaptan curing agents, etc. These may be used alone or in combination of two or more.

[0031] Examples of the phenolic resin-based curing agent include novolac-type phenolic resins such as phenol novolac resin, cresol novolac resin, naphthol novolac resin, aminotriazine novolac resin, novolac resin, and trisphenylmethane-type phenol novolac resin; modified phenolic resins such as terpene-modified phenolic resin and dicyclopentadiene-modified phenolic resin; aralkyl-type resins such as phenol aralkyl resins having a phenylene skeleton and / or a biphenylene skeleton and naphthol aralkyl resins having a phenylene skeleton and / or a biphenylene skeleton; bisphenol compounds such as bisphenol A and bisphenol F; and resol-type phenolic resins. These may be used alone or in combination of two or more. In this embodiment, from the viewpoint of the effects of the present invention, it is preferable that the curing agent consists only of the phenol compound (1).

[0032] (Cure accelerator) The thermosetting resin composition of the present embodiment may contain a curing accelerator as necessary. As the curing accelerator, known compounds can be used as long as they can exert the effects of the present invention, and an appropriate one can be selected from the viewpoints of reaction rate, reaction temperature, storage properties, and the like.

[0033] Examples of the curing accelerator include imidazoles, organic phosphorus compounds, tertiary amines, phenolic compounds, organic acids, etc. These may be used alone or in combination of two or more. Among these, from the viewpoint of improving heat resistance, it is preferable to use nitrogen atom-containing compounds such as imidazoles.

[0034] Examples of the imidazoles include 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 2,4-diethylimidazole, 2-phenyl-4-methyl-5-hydroxyimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-phenylimidazolium trimellitate.

[0035] Examples of the tertiary amines include triethylamine, tributylamine, 1,4-diazabicyclo[2.2.2]octane, and 1,8-diazabicyclo(5,4,0)undecene-7.

[0036] Examples of the phenol compound include phenol, bisphenol A, nonylphenol, and 2,2-bis(3-methyl-4-hydroxyphenyl)propane. Examples of the organic acid include acetic acid, benzoic acid, salicylic acid, and p-toluenesulfonic acid.

[0037] The content of the curing accelerator may be 0.01% by mass to 10% by mass, 0.02% by mass to 5% by mass, or 0.05% by mass to 1.5% by mass relative to 100% by mass of the total of the thermosetting resin and the curing agent.

[0038] (Filler) The thermosetting resin composition of the present embodiment may contain a filler, if necessary. As the filler, an inorganic filler or an organic filler is used.

[0039] Examples of inorganic fillers include silica such as fused crushed silica, fused spherical silica, crystalline silica, and secondary agglomerated silica; alumina; titanium white; aluminum hydroxide; talc; clay; mica; and glass fiber. Examples of the organic filler include organosilicone powder and polyethylene powder. These may be used alone or in combination of two or more.

[0040] (Thermal conductive filler) The thermosetting resin composition may contain a thermally conductive filler as a filler. The thermally conductive filler may contain, for example, highly thermally conductive inorganic particles having a thermal conductivity of 20 W / m·K or more. The highly thermally conductive inorganic particles may contain, for example, at least one selected from alumina, aluminum nitride, boron nitride, silicon nitride, silicon carbide, and magnesium oxide. These may be used alone or in combination of two or more.

[0041] The thermally conductive filler may contain boron nitride in the form of monodisperse particles, agglomerated particles, or a mixture thereof, of scaly boron nitride. The scaly boron nitride may be granulated. By using agglomerated particles of scaly boron nitride, the thermal conductivity can be further increased. The agglomerated particles may be sintered particles or non-sintered particles.

[0042] The use of agglomerated particles of scaly boron nitride (aggregates of scaly filler) can increase the thermal conductivity in the thickness direction. Although the detailed mechanism is unclear, it is thought that this is because some of the scaly filler is crushed during press molding, and an isotropic heat conduction path is formed without the scaly filler agglomerates being oriented in one direction. It is also thought that the above-mentioned isotropic heat conduction path can be realized by adopting a mixing method that enables dispersion while suppressing the collapse of the scaly filler agglomerates, such as by using a planetary mixer or homogenizer.

[0043] The content of the thermally conductive filler is 100% by mass to 400% by mass, preferably 150% by mass to 350% by mass, and more preferably 200% by mass to 300% by mass, based on the resin component (100% by mass) of the thermosetting resin composition not including the filler. By making the content equal to or greater than the lower limit, the thermal conductivity can be improved. By making the content equal to or less than the upper limit, the deterioration of processability can be suppressed.

[0044] (cyanate resin) The thermosetting resin composition of the present embodiment may contain a cyanate resin as necessary. The cured product of the thermosetting resin composition may have low linear expansion and improved elastic modulus and rigidity. It may also contribute to improving the heat resistance and moisture resistance of the resulting electronic device.

[0045] In addition, the cyanate resin may be used alone or in combination of two or more kinds, or one or more kinds may be used in combination with a prepolymer thereof.

[0046] The cyanate resin may include one or more selected from the following: novolac cyanate resin; bisphenol cyanate resin such as bisphenol A cyanate resin, bisphenol E cyanate resin, and tetramethyl bisphenol F cyanate resin; naphthol aralkyl cyanate resin obtained by reacting naphthol aralkyl phenol resin with cyanogen halide; dicyclopentadiene cyanate resin; and biphenylene skeleton-containing phenol aralkyl cyanate resin. Among these, from the viewpoint of reducing the linear expansion of the cured product of the thermosetting resin composition and improving the elastic modulus and rigidity, it is more preferable to include at least one of novolac cyanate resin and naphthol aralkyl cyanate resin, and particularly preferable to include novolac cyanate resin. As the novolac type cyanate resin, for example, one represented by the following general formula (I) can be used.

[0047] [ka]

[0048] The average repeating unit number n of the novolac cyanate resin represented by the general formula (I) is any integer. The average repeating unit number n is not particularly limited, but is preferably 1 or more, more preferably 2 or more. When the average repeating unit number n is equal to or more than the lower limit, the heat resistance of the novolac cyanate resin is improved, and the elimination and volatilization of low molecular weight compounds during heating can be further suppressed. In addition, the average repeating unit number n is not particularly limited, but is preferably 10 or less, more preferably 7 or less. When n is equal to or less than the upper limit, the melt viscosity can be suppressed from increasing, and the moldability of the insulating layer 102 can be improved.

[0049] As the cyanate resin, naphthol aralkyl type cyanate resin represented by the following general formula (II) is also preferably used. The naphthol aralkyl type cyanate resin represented by the following general formula (II) is obtained by condensing a naphthol aralkyl type phenol resin obtained by reacting naphthols such as α-naphthol or β-naphthol with p-xylylene glycol, α,α'-dimethoxy-p-xylene, 1,4-di(2-hydroxy-2-propyl)benzene, etc., with a cyanogen halide. The repeating unit n in the general formula (II) is preferably an integer of 10 or less. When the repeating unit n is 10 or less, a more uniform insulating layer 102 can be obtained. In addition, intramolecular polymerization is less likely to occur during synthesis, and separation during washing with water is improved, which tends to prevent a decrease in yield.

[0050] [ka]

[0051] (In the general formula (II), each R independently represents a hydrogen atom or a methyl group, and n represents an integer of 1 or more and 10 or less.)

[0052] The lower limit of the content of the cyanate resin is, for example, 5% by mass or more, preferably 10% by mass or more, based on the resin component (100% by mass) of the thermosetting resin composition not containing a filler. This makes it possible to more effectively reduce the linear expansion and increase the elastic modulus of the cured product of the thermosetting resin composition. On the other hand, the upper limit of the content of the cyanate resin is, for example, 60% by mass or less, preferably 50% by mass or less, more preferably 45% by mass or less, based on the resin component (100% by mass) of the thermosetting resin composition not containing a filler. This makes it possible to balance the properties of the thermosetting resin composition.

[0053] (Other Ingredients) The thermosetting resin composition of the present embodiment may contain other components in addition to the above-mentioned components. Examples of the other components include a dispersion stabilizer, a silane coupling agent, an antioxidant, and a surface conditioner (a leveling agent or a surfactant). These may be used alone or in combination of two or more. The thermosetting resin composition of the present embodiment may contain a dispersion stabilizer, if necessary.

[0054] By using a dispersion stabilizer, it is possible to suppress the settling of the thermally conductive filler. For example, by adding a nano component, the varnish viscosity of the thermosetting resin composition is increased, so that the settling of the thermally conductive filler can be suppressed. This allows the filler to be uniformly dispersed, making it possible to obtain a composite molding without molding defects, and it is believed that stable thermal conductivity can be expressed.

[0055] Examples of the dispersion stabilizer include inorganic nanoparticles such as nanosilica particles, alkylsulfonic acid compounds, quaternary ammonium compounds, higher alcohol alkylene oxide compounds, polyhydric alcohol ester compounds, alkylpolyamine compounds, polyphosphoric acid compounds, polycarboxylic acid compounds, polyethylene glycol compounds, polyether compounds, anionic surfactants, cationic surfactants, and nonionic surfactants.

[0056] The nanosilica particles may be fumed silica or colloidal silica. Fumed silica is preferred in terms of cost and performance. These may be used alone or in combination of two or more.

[0057] The particle diameter of the nanosilica particles is, for example, 1 nm to 100 nm, and preferably 2 nm to 50 nm. By setting the particle diameter to this range, it is believed that the uniformity of the distribution of the thermally conductive particles described above can be further improved. The particle size here means the average primary particle size determined by a laser diffraction method.

[0058] The content of the dispersion stabilizer is, for example, 0.01% by mass to 10% by mass, preferably 0.02% by mass to 5.0% by mass, and more preferably 0.05% by mass to 3.0% by mass, based on the resin component (100% by mass) of the thermosetting resin composition not including the filler. By making the content equal to or greater than the lower limit, the thermal conductivity can be increased. On the other hand, by making the content equal to or less than the upper limit, the moldability and the formability of the thermal conduction path can be increased.

[0059] The amount of the nanosilica particles is, for example, 0.1 to 5% by mass, and preferably 0.2 to 3% by mass, relative to the resin component (100% by mass) of the thermosetting resin composition not including the filler.

[0060] The thermosetting resin composition of the present embodiment may contain a silane coupling agent, if necessary. This can improve the compatibility of the thermally conductive filler in the thermosetting resin composition. The coupling agent may be added to the thermosetting resin composition, or may be used by treating the surface of the thermally conductive filler.

[0061] The silane coupling agent may include, for example, one or more selected from the group consisting of epoxy-based silane coupling agents, amino-based silane coupling agents, mercapto-based silane coupling agents, ureido-based silane coupling agents, cationic-based silane coupling agents, titanate-based coupling agents, and silicone oil-based coupling agents. These may be used alone or in combination of two or more.

[0062] Among these, a silane coupling agent having at least one of an epoxy group, an amino group, a mercapto group, a ureido group, or a hydroxyl group as a functional group can be used. Also, from the viewpoint of improving compatibility with the resin component, a silane coupling agent having a non-reactive phenyl group can be used.

[0063] Specific examples of the silane coupling agent having the functional group include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptotriethoxysilane, 3-ureidopropyltriethoxysilane, and the like. Examples of the silane coupling agent containing a phenyl group include 3-phenylaminopropyltrimethoxysilane, 3-phenylaminopropyltriethoxysilane, N-methylanilinopropyltrimethoxysilane, N-methylanilinopropyltriethoxysilane, 3-phenyliminopropyltrimethoxysilane, 3-phenyliminopropyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, triphenylmethoxysilane, and triphenylethoxysilane.

[0064] The amount of the coupling agent added is, for example, preferably from 0.05% by mass to 3% by mass, and particularly preferably from 0.1% by mass to 2% by mass, relative to 100% by mass of the thermally conductive filler.

[0065] [Method for producing thermosetting resin composition] The thermosetting resin composition of the present embodiment can be produced, for example, by the following method. The resin varnish (thermosetting resin composition in varnish form) can be prepared by dissolving, mixing, and stirring the above-mentioned components other than the thermally conductive filler in a solvent. For this mixing, various mixers such as ultrasonic dispersion type, high-pressure collision type dispersion type, high-speed rotation dispersion type, bead mill type, high-speed shear dispersion type, and rotation-revolution type dispersion type can be used.

[0066] The solvent is not particularly limited, but examples thereof include methyl ethyl ketone, methyl isobutyl ketone, propylene glycol monomethyl ether, and cyclohexanone.

[0067] In addition, a thermosetting resin composition in a B-stage state can be obtained by adding a thermally conductive filler to the resin varnish and kneading the mixture using a three-roll mill or the like. By adding the filler during kneading, the thermally conductive filler can be dispersed more uniformly in the thermosetting resin, but this is not limited thereto. The thermally conductive filler may be added during kneading, or may be added during mixing of the resin varnish. From the viewpoint of dispersibility, it is preferable to add the nanoparticles dispersed in a specific solvent (nanoparticle dispersion) to the resin varnish.

[0068] (Resin sheet) The resin sheet of the present embodiment includes a carrier substrate and a resin layer formed on the carrier substrate and made of the thermosetting resin composition of the present embodiment.

[0069] The resin sheet can be obtained, for example, by applying a varnish-like thermosetting resin composition onto a carrier substrate to obtain a coating film (resin layer) and then carrying out a solvent removal treatment. The solvent content in the resin sheet can be 10% by weight or less based on the entire thermosetting resin composition. For example, the solvent removal treatment can be carried out under conditions of 80°C to 150°C and 1 minute to 30 minutes. This makes it possible to sufficiently remove the solvent while suppressing the progress of curing of the thermosetting resin composition.

[0070] The resin sheet (resin layer with carrier substrate) may be in a roll shape that can be wound up, or in a rectangular sheet shape. The surface of the resin film of the resin sheet may be, for example, exposed, or may be covered with a protective film (cover film). As the protective film, a film having a known protective function may be used, and for example, a PET film may be used.

[0071] In this embodiment, the carrier substrate may be, for example, a polymer film or a metal foil. Examples of the polymer film include, but are not limited to, polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polycarbonates, release papers such as silicone sheets, and thermoplastic resin sheets having heat resistance such as fluorine-based resins and polyimide resins. Examples of the metal foil include, but are not limited to, copper and / or copper-based alloys, aluminum and / or aluminum-based alloys, iron and / or iron-based alloys, silver and / or silver-based alloys, gold and gold-based alloys, zinc and zinc-based alloys, nickel and nickel-based alloys, and tin and tin-based alloys. Among these, a sheet made of polyethylene terephthalate is most preferable because it is inexpensive and the peel strength can be easily adjusted. This makes it easy to peel the carrier substrate from the resin layer with the carrier substrate with an appropriate strength.

[0072] The thermosetting resin composition of the present embodiment can be used as a heat dissipating and insulating material for electric and electronic devices, etc. This heat dissipating and insulating material can be used, for example, as a substrate material for mounting electronic components, or an adhesive material.

[0073] The electric and electronic devices may be, for example, ordinary semiconductor devices (electronic devices having semiconductor elements as electronic components) or power modules (electronic devices having power semiconductor elements as electronic components). Power semiconductor elements use wide band gap materials such as SiC, GaN, Ga2O3, or diamond, and are designed to be used at high voltages and large currents, so they generate more heat than ordinary silicon chips (semiconductor elements), and therefore operate in even higher temperature environments. Power semiconductor elements are required to be used for long periods of time in high temperature operating environments, for example, at 200°C or higher or 250°C or higher. Specific examples of power semiconductor elements include, for example, rectifier diodes, power transistors, power MOSFETs, insulated gate bipolar transistors (IGBTs), thyristors, gate turn-off thyristors (GTOs), and triacs. According to the thermosetting resin composition of the present embodiment, a heat dissipation and insulation material that can be used in a power module can be provided.

[0074] (Resin substrate) The resin substrate of the present embodiment has an insulating layer made of the cured product of the thermosetting resin composition. This resin substrate can be used as a material for an element mounting substrate for mounting electronic components such as semiconductor elements and power semiconductors.

[0075] (Metal base board) A metal base substrate 100 of this embodiment will be described with reference to FIG. FIG. 1 is a cross-sectional view showing an example of the configuration of a metal base substrate 100. As shown in FIG.

[0076] As shown in Fig. 1, the metal base substrate 100 may include a metal substrate 101, an insulating layer 102 provided on the metal substrate 101, and a metal layer 103 provided on the insulating layer 102. The insulating layer 102 may be made of one material selected from the group consisting of a resin layer made of the thermosetting resin composition, a cured product of the thermosetting resin composition, and a laminate. Each of the resin layer and the laminate may be made of a thermosetting resin composition in a B-stage state before the circuit processing of the metal layer 103, and may be a cured product obtained by curing the resin composition after the circuit processing.

[0077] The metal layer 103 is provided on the insulating layer 102 and is subjected to circuit processing. Examples of metals constituting the metal layer 103 include one or more selected from copper, copper alloys, aluminum, aluminum alloys, nickel, iron, tin, and the like. Among these, the metal layer 103 is preferably a copper layer or an aluminum layer, and is particularly preferably a copper layer. By using copper or aluminum, the circuit processing property of the metal layer 103 can be improved. The metal layer 103 may be a metal foil available in a plate shape, or a metal foil available in a roll shape.

[0078] The lower limit of the thickness of the metal layer 103 is, for example, 0.01 mm or more, preferably 0.10 mm or more, and more preferably 0.25 mm or more. If the thickness is equal to or more than this value, heat generation in the circuit pattern can be suppressed even in applications requiring high current.

[0079] The upper limit of the thickness of the metal layer 103 is, for example, 2.0 mm or less, preferably 1.5 mm or less, and more preferably 1.0 mm or less. If the thickness is less than this range, the circuit processability can be improved, and the substrate as a whole can be made thinner.

[0080] The metal substrate 101 has a role of dissipating heat accumulated in the metal base substrate 100. The metal substrate 101 is not particularly limited as long as it is a heat dissipating metal substrate, but may be, for example, a copper substrate, a copper alloy substrate, an aluminum substrate, or an aluminum alloy substrate, with a copper substrate or an aluminum substrate being preferred, and a copper substrate being more preferred. By using a copper substrate or an aluminum substrate, the heat dissipation properties of the metal substrate 101 can be improved. The thickness of the metal substrate 101 can be appropriately set as long as it does not impair the object of the present invention.

[0081] The upper limit of the thickness of the metal substrate 101 is, for example, 20.0 mm or less, and preferably 5.0 mm or less. By using a metal substrate 101 having a thickness of this value or less, the metal base substrate 100 as a whole can be made thin. In addition, the workability of the metal base substrate 100 in the outer shape processing, cutting processing, etc. can be improved.

[0082] The lower limit of the thickness of the metal substrate 101 is, for example, 0.1 mm or more, preferably 1.0 mm or more, and more preferably 2.0 mm or more. By using a metal substrate 101 having a thickness of this value or more, the heat dissipation of the metal base substrate 100 as a whole can be improved.

[0083] In this embodiment, the metal base substrate 100 can be used for various substrate applications, but because of its excellent thermal conductivity and heat resistance, it can be used as a power module substrate for use in a power module.

[0084] The metal base substrate 100 may have a metal layer 103 that is circuitized by etching or the like into a pattern. In this metal base substrate 100, a solder resist (not shown) may be formed on the outermost layer, and connection electrodes may be exposed so that electronic components can be mounted thereon by exposure and development.

[0085] (Power Module) The power module of this embodiment will be described with reference to FIG. FIG. 2 is a cross-sectional view showing the configuration of the power module 11.

[0086] The power module 11 of this embodiment can include the metal base substrate 100 and electronic components provided on the metal base substrate 100. The electronic components can be the power semiconductor elements described above. In addition to the power semiconductor elements, other electronic components may be mounted on the metal base substrate 100. The metal base substrate 100 can function as a heat spreader for heat from the electronic components (various heat generating elements) that generate heat during operation.

[0087] 2, an example of a power module 11 has a power semiconductor element 2 mounted on a metal layer 103a (a patterned metal layer 103) of a power module circuit board (metal base substrate 100) via an adhesive layer 3. The power semiconductor element 2 is electrically connected to the metal layer 103b via a bonding wire 7. The power semiconductor element 2, the bonding wire 7, and the metal layers 103a and 103b are sealed with a sealing material 6.

[0088] The power module 11 may also include other electronic components such as a chip capacitor 8 and a chip resistor 9 mounted on the metal layer 103 of the metal base substrate 100. The power module 11 may also have a structure in which the metal substrate 101 is connected to a heat dissipation fin 5 via a known thermally conductive grease 4.

[0089] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted as long as they do not impair the effects of the present invention. EXAMPLES

[0090] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. [Example 1] (Synthesis of phenol compound 1) 3,5-dihydroxybenzoic acid (35DHBA, manufactured by Tokyo Chemical Industry Co., Ltd.) 5.2 parts by weight, 3.7 parts by weight of hydroquinone (HQ, manufactured by Tokyo Chemical Industry Co., Ltd.) and 7.8 parts by weight of (N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (EDAC, manufactured by Tokyo Chemical Industry Co., Ltd.) were dissolved in 83.3 parts by weight of dehydrated acetone and stirred at room temperature for 24 hours. The reaction solution was concentrated and then extracted with ethyl acetate as an organic layer. After concentration and drying, the resulting solid was recrystallized from ethanol to obtain phenol compound 1 represented by the following chemical formula in a yield of 58% as a pale yellow solid. 1 The H-NMR measurement results are shown below. 1 H-NMR(300MHz,DMSO-d6)10.49(s,1H),9.5(s,2H),7.97(d,J=8.7Hz,2H),7.02-6.99(m,2H),6.91(d,J=8.7Hz,2H),6.80-6.78(m,1H).

[0091] [ka]

[0092] [Example 2, Comparative Example 1] (Preparation of filler-free thermosetting resin composition and cured product) Phenol curing agent and epoxy resin were charged in the types and amounts shown in Table 1, and melt-mixed for 10 minutes on a hot plate at 150°C. After cooling to 120°C, triphenylphosphine was added as a curing catalyst in the amount shown in Table 1, and mixed for 1 minute. After mixing, the mixture was cooled to room temperature and pulverized to produce a mixture. The mixture was compression molded under conditions of 180℃ / 2MPa / 15 minutes, and then heated in an oven at 180℃ / 3 hours to produce a cured product. The resulting cured product was processed into a 10mmΦ×1mm thickness. In addition, evaluation samples with shapes suitable for various thermal properties were processed and used for evaluation. The components listed in Table 1 are as follows:

[0093] (thermosetting resin) Epoxy resin: Biphenyl type epoxy resin represented by the following chemical formula (bifunctional epoxy compound, with mesogen structure, manufactured by Mitsubishi Chemical Corporation, YX4000)

[0094] [ka]

[0095] (hardening agent) Phenol hardener 1: Phenol compound 1 synthesized in Example 1 above Phenol hardener 2: Orthocresol novolac type phenol hardener (Sumitomo Bakelite Co., Ltd., PR-55617) (curing catalyst) Triphenylphosphine

[0096] <Evaluation method> [Thermal conductivity evaluation (thermal conductivity)] -Specific gravity of hardened product The specific gravity was measured in accordance with JIS K 6911 (general test method for thermosetting plastics). Test pieces were cut from the above-mentioned cured products to a size of 2 cm length x 2 cm width x 2 mm thickness. The unit of specific gravity (SP) is g / cm. 3 Let us assume that.

[0097] -Specific heat of hardened material The specific heat (Cp) of the obtained test piece was measured by the DSC method.

[0098] -Measurement of thermal conductivity of resin molded products From the obtained cured product, a test piece with a diameter of 10 mm and a thickness of 1 mm was cut out for measurement in the thickness direction. Next, the thermal diffusion coefficient (α) in the thickness direction of the plate-shaped test piece was measured by the laser flash method using a Xe flash analyzer TD-1RTV manufactured by ULVAC. The measurement was performed under the condition of air and room temperature of 25°C. For the resin molded article, the thermal conductivity was calculated based on the measured values ​​of the thermal diffusion coefficient (α), specific heat (Cp), and specific gravity (SP) obtained, according to the following formula. Thermal conductivity [W / m K]=α[m2 / s]×Cp[J / kg K]×Sp[g / cm 3 ]

[0099] [Heat resistance evaluation: (glass transition temperature Tg)] The obtained filler-free thermosetting resin composition was cured at 220°C for 90 minutes to obtain a cured product of about 50 mm x about 10 mm x about 3 mm. The glass transition temperature (Tg) of this cured product was measured by DMA (dynamic viscoelasticity measurement) at a heating rate of 5°C / min and a frequency of 1 Hz.

[0100] [Table 1]

[0101] From the results in Table 1, it was found that the thermosetting resin composition of Example 2 containing the phenol compound 1 synthesized in Example 1 as a curing agent has a higher thermal conductivity and glass transition temperature than the thermosetting resin composition of Comparative Example 1 containing a conventional curing agent, and therefore can provide a cured product with high thermal conductivity and excellent heat resistance.

[0102] [Example 3, Comparative Example 2] (Preparation of Filler-Containing Thermosetting Resin Composition and Cured Product) The raw materials shown in Table 2 were weighed out by specified weight, melted and mixed, and then pulverized to produce a composite powder. The composite powder (mixture) produced was compression molded under conditions of 180°C / 2 MPa / 15 minutes, and then heated in an oven at 180°C / 3 hours to produce a cured product. The obtained cured product was processed into a size of 10 mm diameter x 1 mm thickness. In addition, evaluation samples were processed into shapes suitable for various thermal properties and used for evaluation. Evaluations other than those for thermal conductivity and heat resistance were performed using the following methods. Among the components listed in Table 2, the components not mentioned above are as follows.

[0103] Alumina filler: DAB-30FC (manufactured by Denka, average particle size 13 μm) Alumina fine powder: DAW-02 (manufactured by Denka, average particle size 2.7 μm) Coupling agent: CF-4083 (N-phenyl-γ-aminopropyltrimethoxysilane, manufactured by Dow Corning Toray Co., Ltd.) Curing catalyst: Tetraphenylphosphonium 2,3-dihydroxynaphthalate (manufactured by Sumitomo Bakelite Co., Ltd.) Fluidity imparting agent: 2,3-dihydroxynaphthalene (Tokyo Chemical Industry Co., Ltd.) Release agent (wax): WE-4 (Montan acid ester wax manufactured by Clariant Japan) Colorant: Carbon black (Carbon #5, manufactured by Mitsubishi Chemical Corporation) · Low stress agent: Silicone oil (FZ-3730, manufactured by Toray Dow Corning)

[0104] <Evaluation method> [Measurement of storage modulus E' at 25℃] The obtained thermosetting resin composition was transfer molded under 175°C conditions and further cured in an oven at 175°C for 4 hours to produce a cured product with a width of about 10 mm, a thickness of about 1 mm, and a length of about 55 mm. The obtained cured product was placed in a measuring device (Hitachi High-Tech Science Corporation, DMS6100) and subjected to dynamic viscoelasticity measurement (DMA) in tension mode at a frequency of 1 Hz. This allowed the storage modulus E' (MPa) at 25°C and the loss modulus E" (MPa) at 25°C to be measured.

[0105] [Softening point] The softening point of the thermosetting resin composition was measured in accordance with JIS K 2207. The apparatus used was ASP-M2SP manufactured by Meitec Corporation.

[0106] [Linear expansion coefficient] Using the results of the measurement of the glass transition temperature, the average linear expansion coefficient α1 (ppm / °C) at 40 to 60°C and the average linear expansion coefficient α2 (ppm / °C) at 200 to 220°C were determined.

[0107] [Table 2]

[0108] From the results in Table 2, it was found that even when a thermally conductive filler was contained, Example 3, which contained the phenol compound 1 synthesized in Example 1 as a curing agent, had higher thermal conductivity and glass transition temperature than Comparative Example 2, and therefore could provide a cured product with high thermal conductivity and excellent heat resistance. Furthermore, it was confirmed that the thermosetting resin composition of Example 3 had a high softening point and excellent handleability. [Explanation of symbols]

[0109] 2. Power semiconductor elements 3 Adhesive layer 4. Thermal grease 5 Heat dissipation fins 6. Encapsulating materials 7 Bonding Wire 8 Chip Capacitors 9 Chip Resistor 10 Solder resist 11 Power Module 100 Metal base board 101 Metal Substrate 102 Insulating layer 103 Metal layer 103a Metal layer 103b Metal layer

Claims

1. A phenol compound represented by the following formula (P): 【Chemistry 1】

2. A curing agent comprising a phenol compound represented by the following general formula (1): 【Chemistry 2】 (In general formula (1), X and Q each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. A plurality of Xs or a plurality of Qs may be the same or different.)

3. A thermosetting resin; A curing agent according to claim 2; A thermosetting resin composition comprising:

4. The thermosetting resin composition according to claim 3 , further comprising a curing accelerator.

5. The thermosetting resin composition according to claim 3 or 4, further comprising a filler.

6. The thermosetting resin composition according to claim 5 , wherein the filler comprises a thermally conductive filler.

7. The following general formula (a) 【Chemistry 3】 (In general formula (a), X represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. A plurality of X's may be the same or different.) and a compound represented by the following general formula (b): 【Chemistry 4】 (In general formula (b), Q represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkoxy group having 1 to 6 carbon atoms. A plurality of Q's may be the same or different.) The method for producing the curing agent according to claim 2, comprising the step of reacting a compound represented by the following general formula (1) with a compound represented by the following general formula (1): 【Chemistry 5】 (In general formula (1), X has the same meaning as in general formula (a), and Q has the same meaning as in general formula (b).)

Citation Information

Patent Citations

  • High-thermal-conductivity polyimine thermosetting resin containing aromatic ester structure and preparation method thereof

    CN111100259A

  • Hydroxybenzoate and production thereof

    JP1986293952A

  • Boron nitride particle, resin composition and heat-conductive sheet

    JP2015193504A

  • Photoreproduction process utilizing photosensitive thianthrene compositions

    US3386829A