Battery separator, electrode assembly, non-aqueous electrolyte secondary battery, and method for manufacturing battery separator

The battery separator with a porous layer of heat-resistant and organic particles addresses adhesion and heat resistance issues, ensuring effective lithium ion movement and maintaining battery output characteristics.

JP7577963B2Active Publication Date: 2024-11-06TORAY INDUSTRIES INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020172967
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-14
Publication Date
2024-11-06
Estimated Expiration
2040-10-14

AI Technical Summary

Technical Problem

Lithium ion secondary batteries face issues with adhesion between electrodes and battery separators during the manufacturing process, leading to decreased battery output characteristics due to blocked lithium ion movement, and require improved heat resistance and DRY adhesion to enhance safety and performance.

Method used

A battery separator is developed with a porous layer containing heat-resistant particles and organic particles, specifically polyethylene particles with a melting point between 60°C and 90°C, where the thickness of the heat-resistant particle layer is 1.5 μm to 5.0 μm, and the ratio of the average particle diameter of organic particles to the thickness of the heat-resistant particle layer is 1.1 to 2.0 times, ensuring both heat resistance and DRY adhesion.

Benefits of technology

The battery separator provides excellent heat resistance, DRY adhesion, and maintains battery output characteristics by preventing lithium ion obstruction, enhancing safety and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577963000001
    Figure 0007577963000001
Patent Text Reader

Abstract

To provide a battery separator capable of successfully exhibiting both heat resistance and DRY adhesiveness, and also capable of giving good output characteristics to a nonaqueous secondary battery by the loss of adhesiveness after electrolyte injection.SOLUTION: There is provided a battery separator including a polyolefin microporous membrane and a porous layer laminated on at least one face of the polyolefin microporous membrane. The porous layer includes organic particles and heat resistant particles. The organic particles are polyethylene and have a melting point of 60°C or more and 90°C or less. When the cross section of the porous layer is observed using a scanning electron microscope, the thickness of a heat resistant particle layer is 1.5 μm or more and 5.0 μm or less on one face where heat resistant particles exist, the magnification of number average particle size of the organic particles with respect to the thickness of the heat resistant particle layer is 1.1 times or more and 2.0 times or less, and the porous layer includes 10 pts.vol. or more and 40 pts.vol. or less of the organic particles with respect to 100 pts.vol. of the total of the organic particles and the heat resistant particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a battery separator, an electrode assembly, a non-aqueous electrolyte secondary battery, and a method for producing a battery separator. [Background technology]

[0002] Non-aqueous electrolyte secondary batteries, especially lithium ion secondary batteries, are widely used in small electronic devices such as mobile phones and personal digital assistants. Examples of the form of non-aqueous electrolyte secondary batteries include cylindrical batteries, square batteries, and laminated batteries. In general, these batteries have a configuration in which an electrode body in which a positive electrode and a negative electrode are arranged with a battery separator interposed therebetween, and a non-aqueous electrolyte is housed in an exterior body. Examples of the structure of the electrode body include a laminated electrode body in which a positive electrode and a negative electrode are laminated with a separator interposed therebetween, and a wound electrode body in which a positive electrode and a negative electrode are wound in a spiral shape with a battery separator interposed therebetween. Conventionally, microporous membranes made of polyolefin resins (also called polyolefin microporous membranes) have been mainly used as battery separators. Polyolefin microporous membranes have ion permeability due to impregnation with an electrolyte, and are excellent in electrical insulation, electrolyte resistance, and oxidation resistance. When the battery abnormally heats up, the pores of the separator are blocked at a temperature of about 120 to 150°C, thereby cutting off the flow of current and preventing fires, etc. In recent years, attempts have been made to improve safety in battery separators by providing a functional layer on one or both sides of the polyolefin microporous membrane.

[0003] For example, Patent Document 1 describes that by providing a porous layer containing an inorganic filler and a resin binder on at least one side of a porous film, the thermal shrinkage rate at 140°C can be suppressed to less than 5.0%, thereby providing a nonaqueous electrolyte battery with high safety. Patent Document 2 proposes that by providing a particle-containing layer containing a cellulose resin, inorganic particles, and thermoplastic resin particles having a melting point of 100 to 140°C on at least one side of a polyolefin-based porous film, the shutdown temperature of the porous film can be lowered in addition to improving heat resistance, thereby achieving both excellent battery performance and safety.

[0004] On the other hand, in lithium ion secondary batteries, partial separation is likely to occur at the interface between the separator and the electrode due to swelling and shrinkage of the electrode accompanying charging and discharging. As a result, this leads to swelling of the battery, an increase in resistance inside the battery, and a decrease in cycle performance. For this reason, battery separators that exhibit adhesion to the electrodes in the battery after the electrolyte is injected have been proposed in recent years. For example, Patent Document 3 proposes that a non-aqueous secondary battery functional layer composition containing inorganic particles and organic particles having a core-shell structure that can swell in the electrolyte is used for the battery separator, thereby simultaneously exhibiting a protective function and an adhesive function to the electrode accompanying the swelling of the organic particles. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-195564 A [Patent Document 2] JP 2011-168048 A [Patent Document 3] WO2016 / 152026 A1 Summary of the Invention [Problem to be solved by the invention]

[0006] In the manufacturing process of lithium-ion secondary batteries, there is a method of bonding electrodes and battery separators in the absence of electrolyte to improve transportability of wound electrode bodies and suppress yields. Therefore, battery separators are required to have adhesion to electrodes (also called dry adhesion because it is adhesion in the absence of electrolyte) in addition to conventional heat resistance. On the other hand, if the electrode and battery separator are dry bonded and the adhesive strength is maintained inside the battery after electrolyte injection, the surface of the bonded electrode active material will be blocked, preventing the movement of lithium ions and leading to a decrease in the output characteristics of the battery. The present invention has been made in consideration of the above problems, and aims to provide a battery separator that has both excellent heat resistance and dry adhesion, and also excellent battery output characteristics, a manufacturing method for the battery separator, and an electrode assembly and secondary battery that use the battery separator. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved by providing a porous layer containing heat-resistant particles and organic particles made of polyethylene having a specific melting point, and by carefully examining the ratio of organic particles in the porous layer, the thickness of the heat-resistant particle layer, and the magnification of the average particle size of the organic particles to the thickness of the heat-resistant particle layer, and have completed the present invention. More specifically, the present invention relates to a battery separator that can exhibit both heat resistance and dry adhesion by constructing a porous layer using heat-resistant particles and polyethylene particles with a thickness equal to or greater than that of the heat-resistant particle layer on at least one side of a polyolefin microporous membrane, and that can provide low resistance to a non-aqueous secondary battery by losing adhesion after injection of an electrolyte. That is, the present invention has the following configuration. (1) a polyolefin microporous membrane; A battery separator comprising: a porous layer laminated on at least one surface of the polyolefin microporous membrane, the porous layer includes organic particles and heat-resistant particles; the organic particles are polyethylene; The organic particles have a melting point of 60° C. or more and 90° C. or less, A cross section of the porous layer is observed using a scanning electron microscope, and the thickness of the heat-resistant particle layer on one side on which the heat-resistant particles are present is 1.5 μm or more and 5.0 μm or less, the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer is 1.1 times or more and 2.0 times or less; The amount of the organic particles in the porous layer is 10 parts by volume or more and 40 parts by volume or less relative to 100 parts by volume of the total of the organic particles and the heat-resistant particles. (2) The heat-resistant particles include alumina, boehmite, or barium sulfate. (3) An electrode assembly comprising a positive electrode, a negative electrode, and the battery separator according to (1) or (2). (4) A non-aqueous secondary battery using the battery separator according to (1) or (2) above. (5) A method for producing the battery separator according to (1) or (2) above, the method comprising the following steps (a) to (e) in that order: (a) A process of adding a dispersant to a solvent mainly composed of water, and then adding heat-resistant particles and stirring to obtain a mixed liquid. (b) A step of dispersing the mixture using a bead mill disperser to obtain a master batch liquid. (c) A step of adding the organic particles and a binder to the master batch liquid, and further adding other additives to obtain a coating composition. (d) coating at least one surface of the microporous polyolefin membrane with a coating composition. (e) After the coating, the solvent is dried with a dryer to form a porous layer. Effect of the Invention

[0008] The present invention provides a battery separator that has excellent heat resistance and dry adhesion between an electrode and a separator, and also has excellent battery output characteristics, an electrode assembly and a secondary battery that use the battery separator, and a method for manufacturing the battery separator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] 1. Battery separators [Polyolefin microporous membrane] The thickness of the polyolefin microporous membrane in the embodiment of the present invention is not particularly limited as long as it has the function of a battery separator, but is preferably 25 μm or less. More preferably, it is 7 μm or more and 20 μm or less, and even more preferably, it is 9 μm or more and 16 μm or less. When the thickness of the polyolefin microporous membrane is 25 μm or less, it is possible to achieve both practical membrane strength and pore blocking function, and the area per unit volume of the battery case is not restricted, which is suitable for increasing the capacity of the battery.

[0010] The air resistance of the polyolefin microporous membrane is preferably 300 sec / 100 cc Air or less. More preferably, it is 200 sec / 100 cc Air or less, and even more preferably, it is 150 sec / 100 cc Air or less. The preferable lower limit is not particularly limited. When the air resistance is 300 sec / 100 cc Air or less, the battery has sufficient charge / discharge characteristics, particularly ion permeability (charge / discharge operating voltage) and battery life (closely related to the amount of electrolyte retained), and can fully function as a battery. The sufficient mechanical strength and insulation properties are obtained, reducing the possibility of short circuit during charge / discharge.

[0011] The porosity of the polyolefin microporous membrane is preferably 30% or more and 70% or less. More preferably, it is 35% or more and 60% or less, and even more preferably, it is 40% or more and 55% or less. When the porosity is 30% or more and 70% or less, the battery has sufficient charge / discharge characteristics, particularly ion permeability (charge / discharge operating voltage) and battery life (closely related to the amount of electrolyte retained), and can fully function as a battery. Also, sufficient mechanical strength and insulation properties are obtained, reducing the possibility of short circuit during charge / discharge.

[0012] The polyolefin resin constituting the polyolefin microporous membrane is not particularly limited, but polyethylene or polypropylene is preferred. It may be a single polyolefin resin or a mixture of two or more different polyolefin resins, such as a mixture of polyethylene and polypropylene, or a copolymer of different olefins. This is because, in addition to basic properties such as electrical insulation and ion permeability, it has a pore-blocking effect that cuts off the current and suppresses excessive temperature rise when the battery temperature rises abnormally.

[0013] Among them, polyethylene is particularly preferred from the viewpoint of excellent pore-blocking performance. Hereinafter, the polyolefin resin used in the present invention will be described in detail using polyethylene as an example, but the embodiment of the present invention is not limited thereto.

[0014] Examples of polyethylene include ultra-high molecular weight polyethylene, high density polyethylene, medium density polyethylene, and low density polyethylene. There is no particular limitation on the polymerization catalyst, and examples thereof include Ziegler-Natta catalysts, Phillips catalysts, and metallocene catalysts. These polyethylenes may be not only homopolymers of ethylene, but also copolymers containing small amounts of other α-olefins. Suitable α-olefins other than ethylene include propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, (meth)acrylic acid, esters of (meth)acrylic acid, and styrene.

[0015] The polyethylene may be a single substance, but is preferably a mixture of two or more kinds of polyethylene. The polyethylene mixture may be a mixture of two or more kinds of ultra-high molecular weight polyethylenes having different weight average molecular weights (Mw), a mixture of similar high density polyethylene, medium density polyethylene, and low density polyethylene, or a mixture of two or more kinds of polyethylenes selected from the group consisting of ultra-high molecular weight polyethylene, high density polyethylene, medium density polyethylene, and low density polyethylene.

[0016] The polyolefin microporous film is required to have a function of blocking pores when an abnormality occurs in a charge / discharge reaction. Therefore, the melting point of the resin constituting the film is preferably 70°C or more and 150°C or less. More preferably, it is 80°C or more and 140°C or less, and even more preferably, it is 100°C or more and 130°C or less. When the melting point of the resin constituting the film is 70°C or more and 150°C or less, the pore blocking function does not occur during normal use, which prevents the battery from becoming unusable, and the pore blocking function occurs during an abnormal reaction, which ensures safety.

[0017] [Method of producing polyolefin microporous membrane] The method for producing the polyolefin microporous film is not particularly limited as long as it can produce a polyolefin microporous film with desired properties, and can use a conventionally known method.The method for producing the polyolefin microporous film can be, for example, the method described in Japanese Patent No. 2132327 and Japanese Patent No. 3347835, International Publication No. 2006 / 137540, etc.The following describes an example of the method for producing the polyolefin microporous film.The method for producing the polyolefin microporous film is not limited to the following method.

[0018] The method for producing a microporous polyolefin membrane can include the following steps (1) to (5), and can further include at least one of the following steps (6) to (8).

[0019] (1) A step of melt-kneading the polyolefin resin and a membrane-forming solvent to prepare a polyolefin solution. (2) extruding the polyolefin solution and cooling it to form a gel-like sheet. (3) A first stretching step of stretching the gel-like sheet (4) A step of removing the membrane-forming solvent from the stretched gel-like sheet. (5) A step of drying the sheet after removing the membrane-forming solvent. (6) A second stretching step of stretching the dried sheet (7) A step of heat treating the dried sheet (8) A step of subjecting the sheet after the stretching step to a crosslinking treatment and / or hydrophilization treatment Each step will be described below.

[0020] (1) Preparation of polyolefin solution A suitable membrane-forming solvent is added to the polyolefin resin, and then the mixture is melt-kneaded to prepare a polyolefin solution. As a melt-kneading method, for example, a method using a twin-screw extruder as described in Japanese Patent No. 2132327 and Japanese Patent No. 3347835 can be used. The melt-kneading method is well known, so a description thereof will be omitted.

[0021] The blending ratio of the polyolefin resin and the membrane-forming solvent in the polyolefin solution is not particularly limited, but is preferably 20 to 30 parts by mass of the polyolefin resin and 70 to 80 parts by mass of the membrane-forming solvent. When the ratio of the polyolefin resin is within the above range, swelling and necking at the die outlet during extrusion of the polyolefin solution can be prevented, and the moldability and self-supporting property of the extrusion molded body (gel-like molded body) are improved.

[0022] (2) Gel-like sheet formation process The polyolefin solution is fed from the extruder to a die and extruded into a sheet. A plurality of polyolefin solutions having the same or different compositions may be fed from the extruder to a single die, where they are layered and extruded into a sheet.

[0023] The extrusion method may be either a flat die method or an inflation method. The extrusion temperature is preferably 140 to 250°C, and the extrusion speed is preferably 0.2 to 15 m / min. The film thickness can be adjusted by adjusting the extrusion amount of each polyolefin solution. As the extrusion method, for example, the methods disclosed in Japanese Patent No. 2132327 and Japanese Patent No. 3347835 can be used.

[0024] The gel-like sheet is formed by cooling the obtained extrusion molding. As a method for forming the gel-like sheet, for example, the methods disclosed in Japanese Patent No. 2132327 and Japanese Patent No. 3347835 can be used. The cooling is preferably performed at a rate of 50°C / min or more at least to the gelation temperature. The cooling is preferably performed at 25°C or less. The microphase of the polyolefin separated by the membrane-forming solvent can be fixed by cooling. When the cooling rate is within the above range, the crystallinity is kept within an appropriate range, and a gel-like sheet suitable for stretching is obtained. As a cooling method, a method of contacting with a refrigerant such as cold air or cooling water, a method of contacting with a cooling roll, etc. can be used, but it is preferable to cool by contacting with a roll cooled with a refrigerant.

[0025] (3) First stretching step Next, the gel-like sheet obtained is stretched at least uniaxially. Since the gel-like sheet contains the membrane-forming solvent, it can be stretched uniformly. After heating, the gel-like sheet is preferably stretched at a predetermined magnification by a tenter method, a roll method, an inflation method, or a combination of these. The stretching may be uniaxial or biaxial, but biaxial stretching is preferred. In the case of biaxial stretching, simultaneous biaxial stretching, sequential stretching, or multi-stage stretching (for example, a combination of simultaneous biaxial stretching and sequential stretching) may be used. Good too.

[0026] The stretching ratio (area stretching ratio) in this step is preferably 9 times or more, more preferably 16 times or more, and particularly preferably 25 times or more. The stretching ratios in the machine direction (MD) and the transverse direction (TD) may be the same or different. The stretching ratio in this step refers to the area stretching ratio of the microporous membrane immediately before being subjected to the next step, based on the microporous membrane immediately before this step.

[0027] The stretching temperature in this step is preferably within the range of the crystal dispersion temperature (Tcd) of the polyolefin resin to Tcd+30° C., more preferably within the range of the crystal dispersion temperature (Tcd)+5° C. to the crystal dispersion temperature (Tcd)+28° C., and particularly preferably within the range of Tcd+10° C. to Tcd+26° C. For example, when a polyethylene resin is used as the polyolefin resin, the stretching temperature is preferably 90 to 140° C., more preferably 100 to 130° C. ° C. The crystal dispersion temperature (Tcd) is determined by measuring the temperature characteristics of dynamic viscoelasticity according to ASTM D4065.

[0028] The stretching described above causes cleavage between polyolefin lamellae, resulting in the refinement of the polyolefin phase and the formation of numerous fibrils. The fibrils form a three-dimensionally irregularly connected network structure. Stretching improves mechanical strength and enlarges pores, but by stretching under appropriate conditions, it is possible to control the through-hole diameter and achieve a high porosity even with a thin film thickness.

[0029] Depending on the desired physical properties, the film may be stretched with a temperature distribution in the thickness direction, which results in a microporous film with excellent mechanical strength. The details of this method are described in Japanese Patent No. 3347854.

[0030] (4) Removal of membrane-forming solvent The membrane-forming solvent is removed (washed) using a washing solvent. Since the polyolefin phase is phase-separated from the membrane-forming solvent phase, when the membrane-forming solvent is removed, a porous membrane is obtained that is made of fibrils that form a fine three-dimensional network structure and has holes (voids) that are three-dimensionally irregularly connected. Washing solvents and methods for removing the membrane-forming solvent using them are publicly known, so a description thereof will be omitted. For example, methods disclosed in Japanese Patent Publication No. 2132327 and Japanese Patent Laid-Open Publication No. 2002-256099 are known. The following method can be used.

[0031] (5) Drying The microporous membrane from which the membrane-forming solvent has been removed is dried by heat drying or air drying. The drying temperature is preferably equal to or lower than the crystal dispersion temperature (Tcd) of the polyolefin resin, and particularly preferably 5° C. or more lower than Tcd. Drying is preferably carried out until the amount of remaining washing solvent is 5 parts by mass or less, and more preferably 3 parts by mass or less, per 100 parts by mass (dry mass) of the microporous membrane. When the amount of remaining washing solvent is within the above range, the subsequent microporous membrane stretching step and When the heat treatment step is performed, the porosity of the microporous membrane is maintained, and deterioration of ion permeability is suppressed.

[0032] (6) Second stretching step The dried microporous membrane is preferably stretched at least uniaxially. The microporous membrane can be stretched by a tenter method or the like while heating in the same manner as above. The stretching may be uniaxial or biaxial. In the case of biaxial stretching, either simultaneous biaxial stretching or sequential stretching may be used. The stretching temperature in this step is not particularly limited, but is usually preferably 90 to 135°C, more preferably 95 to 130°C.

[0033] In this step, the stretching ratio in one axial direction of the microporous membrane (area stretching ratio) is 1.0 to 2.0 times in the machine direction or width direction in the case of uniaxial stretching. In the case of biaxial stretching, the lower limit of the area stretching ratio is preferably 1.0 times, more preferably 1.1 times, and even more preferably 1.2 times. The upper limit is preferably 3.5 times. The stretching ratios in the machine direction and width direction are each 1.0 to 2.0 times, and the stretching ratios in the machine direction and width direction may be the same or different. In addition, The stretching ratio in this step refers to the stretching ratio of the microporous membrane immediately before being subjected to the next step, based on the microporous membrane immediately before this step.

[0034] (7) Heat treatment Furthermore, the microporous membrane after drying can be subjected to a heat treatment. The heat treatment stabilizes the crystals and makes the lamellae uniform. Heat setting and / or heat relaxation can be used as the heat treatment method. Heat setting is a heat treatment in which the membrane is heated while maintaining its dimensions unchanged. Heat relaxation is a heat treatment in which the membrane is thermally shrunk in the machine direction and width direction during heating. The heat setting is preferably performed by a tenter method or a roll method. For example, The relaxation treatment method may be the method disclosed in JP 2002-256099 A. The heat treatment temperature is preferably within the range of Tcd to Tm of the polyolefin resin, more preferably within the range of the stretching temperature of the microporous membrane ±5°C, and particularly preferably within the range of the second stretching temperature of the microporous membrane ±3°C.

[0035] (8) Cross-linking treatment, hydrophilization treatment Furthermore, the dried microporous membrane can be further subjected to crosslinking and hydrophilization. For example, the microporous membrane is crosslinked by irradiating it with ionizing radiation such as α-rays, β-rays, γ-rays, or electron beams. In the case of electron beam irradiation, the electron beam dose is preferably 0.1 to 100 Mrad, and the acceleration voltage is preferably 100 to 300 kV. The crosslinking treatment increases the meltdown temperature of the microporous membrane. The hydrophilization treatment can be carried out by monomer grafting, surfactant treatment, This can be done by corona discharge, etc. The monomer grafting is preferably carried out after the crosslinking treatment.

[0036] 2.Porous layer The battery separator according to the embodiment of the present invention comprises a porous layer provided on at least one surface of the polyolefin microporous membrane, and contains heat-resistant particles, organic particles, a dispersant, a binder, and a surfactant.

[0037] [Heat-resistant particles] Examples of heat-resistant particles in an embodiment of the present invention include calcium carbonate, calcium phosphate, amorphous silica, crystalline glass filler, kaolin, talc, titanium dioxide, alumina, silica-alumina composite oxide particles, barium sulfate, calcium fluoride, lithium fluoride, zeolite, molybdenum sulfide, mica, boehmite, etc. Among these, alumina, boehmite, and barium sulfate are preferable because they are inexpensive and easily available. The average particle size of the heat-resistant particles is not particularly limited, but the upper limit is preferably 1.5 μm or less, more preferably 1.2 μm or less, and even more preferably 1.0 μm or less. If the average particle size of the heat-resistant particles exceeds 1.5 μm, the gaps between the individual heat-resistant particles in the porous layer become wider, making the structure of the porous layer fragile, and it may be difficult to suppress the shrinkage of the polyolefin microporous film due to heat. In addition, the lower limit of the average particle size of the heat-resistant particles is preferably 0.3 μm or more, more preferably 0.4 μm or more, and even more preferably 0.5 μm or more. If the average particle size of the heat-resistant particles is less than 0.3 μm, the gaps between the individual heat-resistant particles in the porous layer become narrower, and the increase in air resistance per 1 μm of the thickness of the porous layer may be 10.0 sec / 100 ccAir or more. When the average particle size of the heat-resistant particles is 0.3 μm or more and 1.5 μm or less, the increase in air resistance per 1 μm of the porous layer thickness is 10.0 sec / 100 ccAir or less, and shrinkage of the polyolefin microporous membrane due to heat can be suppressed.

[0038] [Organic particles] The organic particles in the embodiment of the present invention are polyethylene particles having a melting point of 60°C to 90°C, preferably a water-dispersible resin, and preferably a water dispersion of polyethylene particles. By selecting polyethylene particles having a melting point of 60°C to 90°C, dry adhesion to the electrode can be exhibited. Furthermore, by having a low interaction with the electrode active material and a high interaction with the electrolyte, the electrolyte can penetrate into the porous layer / electrode interface that is dry-adhered in the battery, which contributes to the loss of dry adhesion and the improvement of the output characteristics of the battery. For example, when acrylic particles are selected as the organic particles, the interaction with the electrode becomes high, making it difficult for the electrolyte to penetrate into the porous layer / electrode interface, and the adhesion is maintained, which is a concern for the surface of the electrode active material to have a reduced lithium ion permeability and a reduced output characteristics.

[0039] The average particle size of the organic particles is not particularly limited, but is preferably in a range exceeding the thickness of the heat-resistant particle layer. If the average particle size of the organic particles is equal to or smaller than the thickness of the heat-resistant particle layer, the organic particles will not be able to protrude from the surface of the porous layer, which may impair the dry adhesive strength. The upper limit of the melting point of the organic particles is preferably 90°C or less, more preferably 85°C or less, and even more preferably 80°C or less. If the melting point exceeds 90°C, the temperature may rise when the electrodes and the battery separator are thermocompressed in the battery assembly process, which may affect the process. The lower limit of the melting point of the organic particles is preferably 60°C or more, more preferably 65°C or more, and even more preferably 70°C or more. If the melting point of the organic particles is less than 60°C, the organic particles may soften and melt easily in the drying process of coating, and may adhere to the conveying roll, which may deteriorate the appearance of the battery separator. In addition, the organic particles may melt and block the pores of the polyolefin microporous membrane and the porous layer, which may reduce the lithium ion permeability in the battery and increase the resistance.

[0040] [Dispersant] The dispersant in the embodiment of the present invention may be, for example, a cellulose-based resin, an anionic surfactant, a cationic surfactant, a nonionic surfactant, or a silicone-based surfactant. Representative examples of cellulose-based resins include carboxymethylcellulose and its derivatives. Specific examples include 1120, 1220, SP200, SE400, and DN-100L manufactured by Daicel FineChem Co., Ltd., "Sunrose" (registered trademark) FJ08HC and A04SH manufactured by Nippon Seishi Co., Ltd., and "Cellogen" (registered trademark) 7A and WS-C manufactured by Daiichi Kogyo Seiyaku Co., Ltd. Specific examples of anionic surfactants include DL-40 and TL-37 manufactured by Nippon Shokubai Co., Ltd., and "Aron" (registered trademark) A-6012 and A-6114 manufactured by Toa Gosei Co., Ltd. Specific examples of cationic surfactants include SN Dispersant 4215 and Nopcosperse 092 manufactured by San Nopco Co., Ltd. Specific examples of amphoteric surfactants include Amphitol 20BS and Amphitol 20N manufactured by Kao Chemical Co., Ltd. Specific examples of nonionic surfactants include Emulgen 103 and Emulgen 705 manufactured by Kao Chemical Co., Ltd. Specific examples of silicone surfactants include SN Wet 125 manufactured by San Nopco Co., Ltd. Among them, water-soluble polymers are preferred in order to allow the dispersant to act efficiently on heat-resistant particles and organic particles. Among them, carboxymethylcellulose derivatives are more preferred because they are oxidation-resistant, easily available, and also contribute to improving heat resistance. The content of the dispersant in the porous layer is not particularly specified, but is preferably 0.8 parts by volume or more, more preferably 1.4 parts by volume or more, and even more preferably 2.0 parts by volume or more, and is 5.9 parts by volume or less, more preferably 4.5 parts by volume or less, and even more preferably 3.0 parts by volume or less, based on 100 parts by volume of the total of the heat-resistant particles, the organic particles, the dispersant and the binder. If the content of the dispersant is less than 0.8 parts by volume, the aggregates of individual heat-resistant particles cannot be sufficiently dispersed during the dispersion process, and the aggregated particles remain in the porous layer, so that the structure of the porous layer is likely to have gaps larger than the particle diameter of the heat-resistant particles, and the shrinkage of the polyolefin microporous membrane due to heat may not be suppressed.If the amount of the dispersant added is more than 5.9 parts by volume, the individual heat-resistant particles once disintegrated in the step (b) are again aggregated by the dispersant, and undispersed aggregates remain in the porous layer, so that the structure of the porous layer is likely to have gaps larger than the particle diameter of the heat-resistant particles, and the shrinkage of the polyolefin microporous membrane due to heat may not be suppressed.

[0041] [binder] The binder in the embodiment of the present invention has both the effect of binding the heat-resistant particles constituting the porous layer together and the effect of adhering the porous layer to the polyolefin microporous membrane. Specifically, acrylic resins, polyvinyl alcohol, poly-N-vinylacetamide, etc. can be used, and commercially available aqueous solutions or aqueous dispersions can be used. Specific examples of acrylic resins include "Jurymer" (registered trademark) AT-210, ET-410, "Aron" (registered trademark) A-104, AS-2000, and NW-7060 manufactured by Toa Gosei Co., Ltd., "LIOACCUM" (registered trademark) series manufactured by Toyochem Co., Ltd., TRD202A and TRD102A manufactured by JSR Corporation, "Polystron" 117, 705, and 1280 manufactured by Arakawa Chemical Industry Co., Ltd., "Kogam" (registered trademark) series manufactured by Showa Denko K.K., and WEM-200U and WEM-3000 manufactured by Taisei Fine Chemical Co., Ltd. Specific examples of polyvinyl alcohol include Kuraray Poval (registered trademark) 3-98 and 3-88 manufactured by Kuraray Co., Ltd., and Gohsenol (registered trademark) N-300 and GH-20 manufactured by Mitsubishi Chemical Corporation. Specific examples of poly-N-vinylacetamide include GE191-104 manufactured by Showa Denko K.K. Among them, acrylic resins are preferred because they are highly versatile and easily bond heat-resistant particles together. The content of the binder in the porous layer is not particularly specified, but is preferably 3.2 parts by volume or more, more preferably 5.6 parts by volume or more, and even more preferably 8.0 parts by volume or more, based on 100 parts by volume of the total of the heat-resistant particles, the organic particles, the dispersant, and the binder, and is 24.0 parts by volume or less, more preferably 18.5 parts by volume or less, and even more preferably 12.1 parts by volume or less.

[0042] If the binder content is less than 3.2 parts by volume, there will be insufficient binder binding the individual heat-resistant particles and organic particles, and the structure of the porous layer will not be maintained, making it difficult to suppress shrinkage of the polyolefin microporous membrane due to heat.

[0043] If the binder content is more than 24.0 parts by volume, the gaps between the heat-resistant particles and the organic particles in the porous layer are clogged with the binder, making it impossible to keep the increase in air permeability resistance per 1 μm of the porous layer thickness below 10.0 sec / 100 ccAir. In addition, when the battery separator is exposed to heat, the binder present in the gaps between the heat-resistant particles and the organic particles shrinks, making it difficult to suppress the shrinkage of the polyolefin microporous membrane due to heat.

[0044] [solvent] In the present invention, the solvent is not only a liquid that dissolves the water-soluble resin or water-dispersible resin, but also includes in a broad sense a dispersion medium used to disperse the water-soluble resin or water-dispersible resin in a particulate form. The solvent in the embodiment of the present invention is mainly water. The water used in the present invention is preferably ion-exchanged water or distilled water. The solvent may be only water, but if necessary, a water-soluble organic solvent such as alcohols may be mixed and used. By using these water-soluble organic solvents, the drying speed and coating properties can be improved. As the water-soluble organic solvent, for example, a mixed liquid in which alcohols such as ethanol, isopropyl alcohol, benzyl alcohol, etc. are mixed in a ratio of 0.1 to 10 parts by mass in the total coating liquid is preferable. Furthermore, organic solvents other than alcohols may be mixed in a range in which they can be dissolved, so long as the amount is less than 1 part by mass. However, the total amount of alcohols and other organic solvents in the coating liquid is less than 10 parts by mass. Furthermore, if necessary, components other than the fine particles and the water-soluble resin or water-dispersible resin may be contained in a range that does not impair the object of the present invention. Examples of such components include dispersants and pH adjusters.

[0045] [Surfactants] The coating composition may contain a surfactant as appropriate in order to form a porous layer with a more uniform thickness on the polyolefin microporous membrane. The surfactant is a wetting agent, a leveling agent, an antifoaming agent, etc. The surfactant is preferably added last after the binder is sufficiently mixed in order not to destroy the dispersion state of the heat-resistant particles.

[0046] [Thickness of heat-resistant particle layer] In the embodiment of the present invention, the thickness of the heat-resistant particle layer is preferably 1.5 to 5.0 μm, which is the average value of the portion composed only of heat-resistant particles on one side where the heat-resistant particles are present, when the cross section of the porous layer of the battery separator is observed using a scanning electron microscope. The upper limit of the thickness of the heat-resistant particle layer is 5.0 μm or less, 4.5 μm or less, and more preferably 4 μm or less. If the thickness of the heat-resistant particle layer exceeds 5.0 μm, the thickness of the battery separator also increases, and the distance between the electrodes in the battery increases, which may result in a decrease in output characteristics. Furthermore, the increase in the thickness of the battery separator may impair the volumetric energy density in non-aqueous electrolyte secondary batteries such as cylindrical batteries, square batteries, and laminate batteries. The lower limit of the thickness of the heat-resistant particle layer is 1.5 μm or more, more preferably 2 μm or more, and even more preferably 3.0 μm or more. If the thickness of the heat-resistant particle layer is less than 1.5 μm, it may be difficult to suppress the shrinkage of the polyolefin microporous membrane due to heat.

[0047] [Ratio of average particle size of organic particles to thickness of heat-resistant particle layer] In the embodiment of the present invention, the ratio of the average particle diameter of the organic particles to the thickness of the heat-resistant particle layer is preferably 1.1 times or more and 2.0 times or less, which indicates the ratio of the average particle diameter of the organic particles to the thickness of the heat-resistant particle layer. The upper limit of the ratio of the average particle diameter of the organic particles to the thickness of the heat-resistant particle layer is 2.0 times or less, preferably 1.8 times or less, and more preferably 1.5 times or less. If the ratio of the average particle diameter of the organic particles to the thickness of the heat-resistant particle layer exceeds 2.0 times, the organic particles may fall off during the conveying process. The lower limit of the ratio of the average particle diameter of the organic particles to the thickness of the heat-resistant particle layer is 1.1 times or more, preferably 1.2 times or more, and more preferably 1.3 times or more. If the ratio of the average particle diameter of the organic particles to the thickness of the heat-resistant particle layer is less than 1.1 times, the organic particles are covered by the heat-resistant particles and cannot be exposed to the porous layer surface, which may cause a loss of dry adhesion.

[0048] [Volume ratio of organic particles in the porous layer] The upper limit of the volume ratio of the organic particles in the porous layer is 40 parts by volume or less, preferably 35 parts by volume or less, more preferably 30 parts by volume or less, relative to 100 parts by volume of the total of the heat-resistant particles and the organic particles. If the volume ratio of the organic particles exceeds 40 parts by volume relative to 100 parts by volume of the total of the heat-resistant particles and the organic particles, the proportion of the thermoplastic part in the porous layer increases, and the heat resistance may be impaired. The lower limit of the volume ratio of the organic particles in the porous layer is 10 parts by volume or more, preferably 15 parts by volume or more, more preferably 20 parts by volume or more, relative to 100 parts by volume of the total of the heat-resistant particles and the organic particles. If the volume ratio of the organic particles is less than 10 parts by volume relative to 100 parts by volume of the total of the heat-resistant particles and the organic particles, sufficient dry adhesive strength cannot be obtained when the electrodes and the battery separator are thermocompressed in the battery assembly process, leading to a decrease in productivity. The density of polyethylene particles, which are organic particles, is 0.91 g / cm 3 , and the heat-resistant alumina particles are 4.0 g / cm 3 , and barium sulfate is 4.5 g / cm 3 , and boehmite is 3.07 g / cm 3 The calculation was done as follows.

[0049] [Porosity of porous layer] The porosity of the porous layer is preferably 30 to 90%, more preferably 40 to 70%. When the porosity of the modified porous layer is in the above-mentioned preferred range, the battery separator obtained by laminating the modified porous layer has low membrane electrical resistance, allows a large current to flow easily, and maintains membrane strength.

[0050] [Dry adhesive strength of battery separators] The upper limit of the dry adhesive strength of the battery separator is preferably 20 N / m or less, more preferably 18 N / m or less, and even more preferably 16 N / m or less. If the dry adhesive strength exceeds 20 N / m, processing such as winding or stacking the dry-bonded battery separator and electrodes during the battery assembly process may become difficult, resulting in reduced productivity. The lower limit of the dry adhesive strength of the battery separator is preferably 2 N / m or more, more preferably 4 N / m or more, and even more preferably 6 N / m or more. If the dry adhesion is less than 2 N / m, sufficient adhesive strength cannot be obtained when the electrodes and the battery separator are thermocompressed during the battery assembly process, leading to reduced productivity. When the battery separator is dry-bonded to the electrode and then an electrolyte is injected, the adhesive strength between the battery separator and the electrode is preferably reduced to 2 N / m or less, more preferably 1.8 N / m or less, and even more preferably 1.5 N / m or less. If the adhesive strength after electrolyte injection exceeds 2 N / m, the dry-bonded electrode surface is blocked, which may impede the movement of lithium ions and impair the output characteristics of the battery.

[0051] [Method of producing coating composition] A method for producing a coating composition for obtaining a porous layer according to an embodiment of the present invention comprises the following steps: (a) A process of adding a dispersant to a solvent mainly composed of water, and then adding heat-resistant particles and stirring to obtain a mixed liquid. (b) A process of dispersing the mixture in a bead mill disperser using ceramic beads having a bead diameter of 1.0 mm or less to obtain a master batch liquid. (c) A step of adding the organic particles and binder to the master batch liquid, and further adding other additives to obtain a coating composition. In the step (a), the stirring method is not particularly limited, but stirring with a dispersing blade, a rotary / revolution mixer, a paint shaker, a ball mill, an ultrasonic disperser, a homogenizer, a planetary mixer, and the like may be used. In addition, in order to allow the dispersant to effectively act on the heat-resistant particles in the solvent, it is important to add the heat-resistant particles in a state in which the dispersant is sufficiently dissolved in the solvent. Therefore, it is preferable to add the dispersant to the solvent, and then the heat-resistant particles in that order.

[0052] The step (b) is a step of crushing the heat-resistant particle aggregates contained in the mixed liquid into individual heat-resistant particles by colliding ceramic beads with the aggregates using a bead mill disperser. In the present invention, it is possible to disperse friable particles appropriately by adjusting the bead particle size and bead packing rate to suitable conditions using a bead mill disperser. In addition, when crushing friable particles such as barium sulfate, a media-less disperser that does not use ceramic beads is considered to be suitable because it causes less damage to the particles.

[0053] [Bead particle size] The particle size of the ceramic beads is not particularly limited, but the number average particle size is preferably 0.3 mm or more and 1.0 mm or less, more preferably 0.4 mm or more and 0.8 mm or less, and further preferably 0.5 mm or more and 0.7 mm or less.

[0054] If the bead particle size is less than 0.3 mm, the mass of each ceramic bead is small, and the shear stress generated between the ceramic beads is small, so that the heat-resistant particle aggregates cannot be sufficiently disintegrated, and aggregates larger than the thickness of the porous layer remain in the coating composition. As a result, gaps larger than the particle size of the heat-resistant particles are likely to be formed in the structure of the porous layer, making it impossible to suppress the shrinkage of the polyolefin microporous film due to heat, and the distance between the positive and negative electrodes of the battery cell becomes large, increasing the proportion of the separator in the battery cell capacity, which may result in a decrease in the capacity density of the battery.

[0055] If the bead particle size is larger than 1.0 mm, the number of contact points between the ceramic beads will be reduced, and aggregates larger than the thickness of the porous layer will remain in the coating composition. This will lead to the formation of gaps in the porous layer structure that are larger than the particle size of the heat-resistant particles, making it difficult to suppress the shrinkage of the polyolefin microporous film due to heat, and may increase the distance between the positive and negative electrodes of the battery cell, increasing the proportion of the separator in the battery cell capacity and decreasing the capacity density of the battery.

[0056] The material of the ceramic beads is not particularly limited, but at least one material selected from alumina, zirconia, and silicon nitride can be used.

[0057] [Beads filling rate] The bead packing rate of the ceramic beads is not particularly limited, but is preferably 65% ​​or more and 85% or less. More preferably, it is 70% or more and 80% or less. Here, the bead packing rate is defined as the ratio of the weight (g) of the ceramic beads used to the packing density (g / cm 3 ) and the resulting volume (cm 3 ) and then vessel capacity (cm 3 ) is the volume fraction of the ceramic beads divided by the volume fraction of the ceramic beads.

[0058] If the bead filling rate is less than 65%, the amount of ceramic beads in the vessel is small, which reduces the number of contact points between the ceramic beads and makes it easier for agglomerates of heat-resistant particles to remain. This can cause the agglomerates of heat-resistant particles to fall off the porous layer or increase the distance between the positive and negative electrodes of the battery cell, which increases the proportion of the separator in the battery cell capacity and reduces the capacity density of the battery.

[0059] If the bead filling rate is greater than 85%, the number of contact points between the ceramic beads will be excessively large, which will crush the individual heat-resistant particles that have already been crushed into finer particles. As a result, the finer particles will enter the gaps between the heat-resistant particles that form the porous layer, and the increase in air resistance per 1 μm of thickness of the heat-resistant coating layer may exceed 10.0 sec / 100 ccAir.

[0060] In the step (c), the stirring method is not particularly limited, but stirring with a dispersing blade, a rotating / revolving mixer, a paint shaker, a ball mill, an ultrasonic disperser, a homogenizer, a planetary mixer, and the like may be used. It is important that the organic particles and binder are not added to the mixed liquid before the bead mill dispersion treatment in the step (b). In other words, the mixed liquid is subjected to heat generated by the bead mill dispersion treatment and high shear force, so that there is a possibility that the organic particles will be crushed and the binder will gel or aggregate. Then, it becomes difficult to obtain a structure in which only the organic particles protrude from the porous layer surface, and both heat resistance and dry adhesion may not be exhibited. Therefore, it is preferable to add the binder in the step (c).

[0061] [Method of forming porous layer] The method for forming a porous layer according to the present invention has the following features: (d) coating at least one surface of the microporous polyolefin membrane with a coating composition. (e) After the coating, the solvent is dried with a dryer to form a porous layer. It is.

[0062] In the step (d), the method for coating at least one side of the polyolefin microporous membrane with a porous layer can be a known method, such as reverse roll coating, gravure coating, small-diameter gravure coater, kiss coating, roll brush, air knife coating, Mayer bar coating, pipe doctor coating, blade coating, and die coating, which can be used alone or in combination.

[0063] In the step (e), the drying temperature of the dryer is not particularly limited, but is preferably 40°C or higher and 90°C or lower. More preferably, it is 45°C or higher and 80°C or lower, and even more preferably, it is 50°C or higher and 70°C or lower. If the drying temperature is lower than 40°C, the solvent cannot be sufficiently dried, so that the solvent remains in the porous layer, and the moisture content of the battery separator may become high, particularly when the solvent is water. If the drying temperature is higher than 90°C, the polyolefin microporous membrane may shrink due to heat before the porous layer is formed. In addition, the drying temperature is preferably set to a temperature below the melting point of the organic particles within the above drying temperature range. If the drying is performed at a temperature equal to or higher than the melting point of the organic particles, the organic particles may soften or melt and adhere to the conveying roll, which may deteriorate the appearance of the battery separator. In addition, the organic particles may melt and block the pores of the polyolefin microporous membrane and the porous layer, which may reduce the lithium ion permeability in the battery and increase the resistance.

[0064] The battery separator according to the embodiment of the present invention can be used as a battery separator for secondary batteries such as nickel-hydrogen batteries, nickel-cadmium batteries, nickel-zinc batteries, silver-zinc batteries, lithium-ion secondary batteries, lithium polymer secondary batteries, and lithium-sulfur batteries, etc. In particular, it is preferable to use it as a separator for lithium-ion secondary batteries. EXAMPLES

[0065] The present invention will be described in more detail below with reference to examples, but the embodiments of the present invention are not limited to these examples. The evaluation methods, analytical methods and materials used in the examples are as follows.

[0066] (Melting point of organic particles) The organic particle dispersion was dried at 60°C to obtain a dried organic particle. Next, a DSC measurement was performed on approximately 6 mg of the dried organic particle during the heating process using a DSC device PYR IS Diamond DSC (manufactured by Perkin Elmer). The measurement temperature range was 30-230°C, and the heating rate was 10°C / min. The peak temperature of the heat flow curve obtained by the above measurement was taken as the melting point of the organic particle.

[0067] (Average particle size of organic particles) Using a scanning electron microscope (JSM6701F manufactured by JEOL Ltd.), the LEI image of the porous layer surface was taken at a magnification of 1000 times (accelerating voltage 2.0 kV). Next, the major axis of 100 random organic particles was measured, and the number average value was taken as the average particle size. Note that, when the organic particle addition ratio was low and 100 organic particles were not present on the porous layer surface in the LEI image taken at a magnification of 1000 times, multiple LEI images were taken at the same magnification as above so that 100 organic particles could be measured by accumulating.

[0068] (Measurement of thickness of heat-resistant particle layer) Using a scanning electron microscope (JSM6701F manufactured by JEOL Ltd.), an LEI image of the separator cross section cut by ion milling was taken at a magnification of 3000 times (accelerating voltage 2.0 kV). Next, the thickness of 10 points in the part consisting only of heat-resistant particles on one side where the heat-resistant particles existed was measured, and the average value was taken as the thickness of the heat-resistant particle layer. (The ratio of the average particle size of organic particles to the thickness of the heat-resistant particle layer) The ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was calculated from the following formula.

[0069] Magnification (times) of the average particle size of organic particles to the thickness of the heat-resistant particle layer = average particle size of organic particles (μm) / thickness of the heat-resistant particle layer (μm) (DRY adhesive) An aqueous solution containing 1.5 parts by mass of carboxymethyl cellulose was added to 96.5 parts by mass of artificial graphite and mixed, and 2 parts by mass of styrene butadiene latex was further added as a solid content and mixed to prepare a negative electrode mixture-containing slurry. This negative electrode mixture-containing slurry was uniformly applied to both sides of a negative electrode current collector made of copper foil with a thickness of 8 μm and dried to form a negative electrode layer, which was then compression-molded by a roll press machine to make the density of the negative electrode layer excluding the current collector 1.5 g / cm. 3 A negative electrode was prepared by the above procedure. The negative electrode (width 40 mm, length 50 mm) and polyethylene terephthalate (PET) film (width 60 mm, length 70 mm) prepared above were prepared, and the battery separator and the negative electrode were laminated so that the central axes of the short sides were aligned and the short sides overlapped each other, and then the PET film was laminated, and another negative electrode was laminated so that it was exactly overlapped with the first prepared negative electrode. The above laminate was hot-pressed using a precision heating and pressing device (CYPT-10, manufactured by Shinto Kogyo Co., Ltd.) at 85°C, 2 MPa, and 1 second to bond the battery separator and the negative electrode.

[0070] The PET film and the unbonded negative electrode were removed, and the test specimen was attached to an aluminum plate using double-sided tape (Nichiban Nystack (R) 15 mm wide). A 2 kg rubber roller (Tester Sangyo SA-1003-B) was then rolled back and forth twice over the test specimen to fix it in place. An auxiliary paper (50 mm wide, 80 mm long) for fixing the measurement tool was attached to the short side of the battery separator that was not bonded to the negative electrode, so that the short side matched.

[0071] The paper was attached to a tabletop precision universal testing machine (SHIMAZU AGS-X) equipped with a tensile measuring jig, and a 180-degree peel test (peel speed 300mm / min) was performed by pulling up the auxiliary paper, and the average value of the stress caused by the 180-degree peel between the battery separator and the negative electrode when the pulling displacement was between 20mm and 80mm was taken as the dry adhesive strength. A mean value of 2.0N / m or more was determined to have dry adhesiveness.

[0072] (Adhesive strength after electrolyte injection) An aqueous solution containing 1.5 parts by mass of carboxymethyl cellulose was added to 96.5 parts by mass of artificial graphite and mixed, and 2 parts by mass of styrene butadiene latex was further added as a solid content and mixed to prepare a negative electrode mixture-containing slurry. This negative electrode mixture-containing slurry was uniformly applied to both sides of a negative electrode current collector made of copper foil with a thickness of 8 μm and dried to form a negative electrode layer, which was then compression-molded by a roll press machine to make the density of the negative electrode layer excluding the current collector 1.5 g / cm. 3 A negative electrode was prepared by the above procedure. The negative electrode (width 10 mm, length 100 mm) and polyethylene terephthalate (PET) film (width 25 mm, length 120 mm) prepared above were prepared, and the battery separator (width 17 mm, length 110 mm) and the negative electrode were laminated so that the central axes of the short sides were aligned and one side of each short side overlapped, and then the PET film was laminated, and another negative electrode was laminated so that it overlapped exactly with the first prepared negative electrode. The above laminate was hot-pressed using a precision heating and pressing device (CYPT-10, manufactured by Shinto Kogyo Co., Ltd.) at 85°C, 2 MPa, and 1 second to bond the battery separator and the negative electrode. An aluminum laminate with a width of 90 mm and a length of 135 mm was prepared and folded in half to a width of 45 mm and a length of 135 mm. A laminate of a dry-bonded battery separator and a negative electrode was placed on the aluminum laminate, and 100 μL of an electrolyte solution in which LiPF6 was dissolved at a ratio of 1 mol / L in a solvent of ethylene carbonate and ethyl methyl carbonate mixed at a volume ratio of 3:7 was dropped. After the electrolyte solution was absorbed, three sides of the opening of the aluminum laminate were sealed with a vacuum sealer. Next, the laminate of the battery separator and the negative electrode in the aluminum laminate was hot-pressed using a precision heating and pressing device (CYPT-10, manufactured by Shinto Kogyo Co., Ltd.) under conditions of 90° C., 0.7 MPa, and 150 seconds. The aluminum laminate was opened, and the laminate of battery separator / negative electrode was taken out. Mending tape (width 25 mm, length 18 mm) was applied to the part of the battery separator protruding about 10 mm, covering it by 5-6 mm. The electrode was attached to a bench-top precision universal testing machine (SHIMAZU AGS-X) equipped with a tensile measuring jig, and the battery separator was attached to the bottom. The negative electrode was then pulled up to perform a 180-degree peel test (peeling speed 300mm / min). The average value of the stress caused by the 180-degree peel between the battery separator and the negative electrode when the pulling displacement was between 20mm and 60mm was taken as the adhesive strength after electrolyte injection, and it was determined that there was adhesiveness after electrolyte injection when the average value exceeded 2.0N / m.

[0073] (Heat resistance test) Three 50mm square samples were prepared and placed in an oven preheated to 150 degrees, then removed after one hour and cooled. The MD (length) and TD (width) dimensions after cooling were divided by the initial MD and TD dimensions measured beforehand to calculate the thermal shrinkage rate.

[0074] Heat shrinkage rate (%) = {initial dimension (mm) - shrinkage dimension (mm)} / initial dimension (mm) x 100 At this time, a heat shrinkage rate of less than 5.0% was rated as particularly good, a heat shrinkage rate of 5% or more and less than 10% was rated as good, and a heat shrinkage rate of 10% or more was rated as poor.

[0075] (Battery evaluation) Preparation of the positive electrode An NMP solution containing 1.2 parts by mass of PVDF as a binder was added to 97 parts by mass of lithium cobalt oxide and 1.8 parts by mass of carbon black as an active material and mixed to prepare a positive electrode mixture-containing slurry. This positive electrode mixture-containing slurry was uniformly applied to both sides of a positive electrode current collector made of aluminum foil with a thickness of 20 μm and dried to form a positive electrode layer, which was then compression-molded using a roll press machine to reduce the density of the positive electrode layer excluding the current collector to 3.6 g / cm. 3 A positive electrode was prepared by the above procedure. Preparation of the negative electrode An aqueous solution containing 1.0 part by mass of sodium carboxymethylcellulose was added to and mixed with 98 parts by mass of artificial graphite as an active material, and then styrene butadiene latex containing 1.0 part by mass as a solid content as a binder was added and mixed to prepare a negative electrode mixture-containing slurry. This negative electrode mixture-containing slurry was uniformly applied to both sides of a negative electrode current collector made of copper foil with a thickness of 10 μm and dried to form a negative electrode layer, which was then compression-molded using a roll press machine and the current collector was removed. The density of the negative electrode layer was 1.45 g / cm 3 A negative electrode was prepared by the above procedure. Preparation of test batteries A wound body was prepared using the above positive and negative electrodes with tabs and each battery separator. Next, the wound body was hot-pressed at 85°C, 2 MPa, and 10 seconds using a flat press machine (Shinto Kogyo CYPT-20 Special) to bond the battery separator to the positive and negative electrodes. The hot-pressed wound body was placed in an aluminum laminate bag, and 750 μL of electrolyte (1.1 mol / L, LiPF6, ethylene carbonate / ethyl methyl carbonate / diethylene carbonate = 3 / 5 / 2 (volume ratio) with 0.5 wt% vinylene carbonate and 2 wt% fluoroethylene carbonate added) was dropped and sealed with a vacuum laminator. Next, the battery was charged to 10% of its full capacity at 0.2C (C represents the current value at which the battery can be fully charged in 1 hour, and in the case of this battery, it is set to 300mA), left overnight, and one side of the laminate was opened to allow gas to escape, and immediately sealed again with a vacuum sealer. Next, the battery was charged at a constant current and constant voltage of 0.1C, 4.35V, and a cutoff current of 0.05C, and then discharged at a constant current of 0.1C to 3V. After that, the battery was charged at a constant current and constant voltage of 0.2C, 4.35V, and a cutoff current of 0.05C, and then discharged at a constant current of 0.2C to 3V. This 0.2C charge and discharge was repeated three times. This was used as a 300mAh-class test battery. Output characteristic test An output characteristic test was carried out using the above test battery. After constant current and constant voltage charging at 0.2C, 4.35V, and cutoff current of 0.05C, the battery was discharged at a constant current of 0.2C to 3V, and this capacity was recorded as the 0.2C discharge capacity. Next, the battery was charged at a constant current and constant voltage of 0.2C, 4.35V, and cutoff current of 0.05C, and then discharged at a constant current of 3C to 3V, and this capacity was recorded as the 3C discharge capacity.

[0076] The 3C discharge capacity retention rate was calculated using the following formula.

[0077] 3C discharge capacity maintenance rate = [3C discharge capacity] / [0.2C discharge capacity] The same treatment was performed on a total of three test batteries, and the average 3C discharge capacity retention rate was taken as the output characteristic.

[0078] At this time, an average value of the 3C discharge capacity retention rate of 75% or more was rated as particularly good, 65% or more and less than 75% was rated as good, and less than 65% was rated as poor.

[0079] [Example 1] Alumina particles (average particle size 0.5 μm, density 4.0 g / cm3) were mixed with 49.0 parts by mass of deionized water. 3 50 parts by mass of the above-mentioned cellulose acetate solution and 1 part by mass of carboxymethyl cellulose were stirred using a disperser, and the mixture was treated seven times using a bead mill disperser (Picomiru PCM-LR manufactured by Asada Iron Works Co., Ltd.) at a frequency of 50 Hz and a flow rate of 10 kg / hour to obtain an alumina dispersion.

[0080] To 100 parts by mass of the above alumina dispersion, 7.11 parts by mass of polyethylene particle dispersion Chemipearl A100 (manufactured by Mitsui Chemicals, Inc., solid content concentration 40%, melting point 83°C) was added while stirring with a Three-One Motor (manufactured by Toki Sangyo Co., Ltd.) equipped with a dispersing blade, and further stirred for 10 minutes. Next, 4.69 parts by mass of acrylic resin water dispersion with a solid content concentration of 40% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes. Next, 0.38 parts by mass of fluorine-based surfactant with a solid content concentration of 50% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes to obtain a coating composition. The coating composition was coated on one side of a 12 μm-thick polyolefin microporous membrane by a microgravure method under conditions of a drying temperature of 50° C. and a conveying speed of 5 m / min to obtain a battery separator. The thickness of the heat-resistant particle layer of the battery separator was 3.0 μm, the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was 1.3 times, and when the total of the alumina and Chemipearl A100 in the porous layer of the battery separator was 100 volume parts, the alumina particles / Chemipearl A100=80 / 20 volume parts.

[0081] [Example 2] A battery separator was obtained in the same manner as in Example 1, except that a polyethylene particle dispersion (average particle size 4.0 μm, melting point 60° C., solid content concentration 40%) was used.

[0082] [Example 3] A battery separator was obtained in the same manner as in Example 1, except that a polyethylene particle dispersion (average particle size 4.0 μm, melting point 90° C., solid content concentration 40%) was used.

[0083] [Example 4] A battery separator was obtained in the same manner as in Example 1, except that the coating composition prepared in Example 1 was used to coat the heat-resistant particle layer so that the thickness of the heat-resistant particle layer was 3.6 μm and the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was 1.1.

[0084] [Example 5] A battery separator was obtained in the same manner as in Example 1, except that the coating composition prepared in Example 1 was used to coat the heat-resistant particle layer so that the thickness of the heat-resistant particle layer was 2.0 μm and the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was 2.0 times.

[0085] [Example 6] A polyethylene particle dispersion (average particle size 2.0 μm, melting point 83° C., solid content 40%) was used to obtain a battery separator in the same manner as in Example 1. The thickness of the heat-resistant particle layer of the obtained battery separator was 3.0 μm.

[0086] [Example 7] A polyethylene particle dispersion (average particle size 6.5 μm, melting point 83° C., solid content concentration 40%) was used to obtain a battery separator in the same manner as in Example 1. The thickness of the heat-resistant particle layer of the obtained battery separator was 5.0 μm.

[0087] [Example 8] To 100 parts by mass of the alumina dispersion obtained in the same manner as in claim 1, 3.16 parts by mass of polyethylene particles Chemipearl A100 (manufactured by Mitsui Chemicals, Inc., solid content concentration 40%, melting point 83°C) were added while stirring with a three-one motor equipped with a dispersing blade, and further stirred for 10 minutes. Next, 4.17 parts by mass of an acrylic resin water dispersion with a solid content concentration of 40% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes. Next, 0.33 parts by mass of a fluorine-based surfactant with a solid content concentration of 50% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes to obtain a coating composition. The coating composition was coated on one side of a 12 μm-thick polyolefin microporous membrane by a microgravure method under conditions of a drying temperature of 50° C. and a conveying speed of 5 m / min to obtain a battery separator. The thickness of the heat-resistant particle layer of the battery separator was 3.0 μm, the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was 1.3 times, and when the total of the alumina and Chemipearl A100 in the porous layer of the battery separator was 100 volume parts, the alumina particles / Chemipearl A100=90 / 10 volume parts.

[0088] [Example 9] To 100 parts by mass of the alumina dispersion obtained in the same manner as in claim 1, 18.96 parts by mass of polyethylene particles Chemipearl A100 (manufactured by Mitsui Chemicals, Inc., solid content concentration 40%, melting point 83°C) were added while stirring with a three-one motor equipped with a dispersing blade, and further stirred for 10 minutes. Next, 6.25 parts by mass of an acrylic resin water dispersion with a solid content concentration of 40% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes. Next, 0.5 parts by mass of a fluorine-based surfactant with a solid content concentration of 50% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes to obtain a coating composition. The coating composition was coated on one side of a 12 μm-thick polyolefin microporous membrane by a microgravure method under conditions of a drying temperature of 50° C. and a conveying speed of 5 m / min to obtain a battery separator. The thickness of the heat-resistant particle layer of the battery separator was 3.0 μm, the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was 1.3 times, and when the total of the alumina and Chemipearl A100 in the porous layer of the battery separator was 100 volume parts, the alumina particles / Chemipearl A100=60 / 40 volume parts.

[0089] [Example 10] Barium sulfate (average particle size 1.2 μm, density 4.5 g / cm3) was added to 49.0 parts by mass of deionized water. 3 50 parts by mass of the alumina dispersion liquid was obtained by stirring 50 parts by mass of the alumina dispersion liquid and 1 part by mass of carboxymethyl cellulose in a disperser and treating once using a bead mill disperser (Picomirl PCM-LR manufactured by Asada Iron Works Co., Ltd.) under conditions of a frequency of 50 Hz and a flow rate of 10 kg / hour.

[0090] 6.32 parts by mass of polyethylene particles Chemipearl A100 (manufactured by Mitsui Chemicals, Inc., solid content concentration 40%, melting point 83°C) were added to 100 parts by mass of the above alumina dispersion while stirring with a Three-One Motor (manufactured by Toki Sangyo Co., Ltd.) equipped with a dispersing blade, and further stirred for 10 minutes. Next, 4.17 parts by mass of an acrylic resin water dispersion with a solid content concentration of 40% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes. Next, 0.33 parts by mass of a fluorine-based surfactant with a solid content concentration of 50% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes to obtain a coating composition. The coating composition was coated on one side of a 12 μm-thick polyolefin microporous membrane by a microgravure method under conditions of a drying temperature of 50° C. and a conveying speed of 5 m / min to obtain a battery separator. The thickness of the heat-resistant particle layer of the battery separator was 3.0 μm, the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was 1.3 times, and when the total of the barium sulfate and Chemipearl A100 in the porous layer of the battery separator was 100 volume parts, the barium sulfate / Chemipearl A100=80 / 20 volume parts.

[0091] [Example 11] Boehmite (average particle size 1.2 μm, density 3.07 g / cm3) was added to 49.0 parts by mass of deionized water. 3 50 parts by mass of the alumina dispersion liquid was obtained by stirring 50 parts by mass of the alumina dispersion liquid and 1 part by mass of carboxymethyl cellulose in a disperser and treating once using a bead mill disperser (Picomirl PCM-LR manufactured by Asada Iron Works Co., Ltd.) under conditions of a frequency of 50 Hz and a flow rate of 10 kg / hour.

[0092] 9.26 parts by mass of polyethylene particles Chemipearl A100 (manufactured by Mitsui Chemicals, Inc., solid content concentration 40%, melting point 83°C) were added to 100 parts by mass of the above alumina dispersion while stirring with a Three One Motor (manufactured by Toki Sangyo Co., Ltd.) equipped with a dispersing blade, and further stirred for 10 minutes. Next, 6.11 parts by mass of an acrylic resin water dispersion with a solid content concentration of 40% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes. Next, 0.49 parts by mass of a fluorine-based surfactant with a solid content concentration of 50% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes to obtain a coating composition. The coating composition was coated on one side of a 12 μm-thick polyolefin microporous membrane by a microgravure method under conditions of a drying temperature of 50° C. and a conveying speed of 5 m / min to obtain a battery separator. The thickness of the heat-resistant particle layer of the battery separator was 3.0 μm, the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was 1.3 times, and the ratio of the boehmite / Chempearl A100=80 / 20 volume parts was obtained when the total of the boehmite and Chemipearl A100 in the porous layer was 100 volume parts.

[0093] [Comparative Example 1] A monomer solution was obtained by adding 0.5 parts by mass of an oil-soluble polymerization initiator to 100 parts by mass of acrylic monomer and dissolving it. Also, a surfactant aqueous solution was obtained by adding 1 part by mass of a surfactant to 100 parts by mass of water. A monomer solution of 10 parts by mass was added to 100 parts by mass of the obtained surfactant aqueous solution, and then the mixture was stirred at high speed with a homogenizer to obtain a monomer emulsion. The obtained monomer emulsion was polymerized at 70°C for 8 hours while stirring under a nitrogen atmosphere to obtain a slurry in which acrylic particles were dispersed. The obtained slurry was passed through a 5 μm mesh filter to remove particles of 5 μm or more, and the solvent was replaced with pure water and redispersed to obtain an acrylic particle dispersion with a solid content of 15%. To 100 parts by mass of the alumina dispersion obtained in the same manner as in claim 1, 25 parts by mass of the acrylic particle dispersion was added while stirring with a three-one motor equipped with a dispersing blade, and further stirred for 10 minutes. Next, 4.69 parts by mass of an acrylic resin water dispersion with a solid content concentration of 40% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes. Next, 0.38 parts by mass of a fluorine-based surfactant with a solid content concentration of 50% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes to obtain a coating composition. The coating composition was coated on one side of a 12 μm-thick polyolefin microporous membrane by a microgravure method under conditions of a drying temperature of 50° C. and a conveying speed of 5 m / min to obtain a battery separator. The thickness of the heat-resistant particle layer of the battery separator was 3.0 μm, the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was 1.3 times, and when the total of the alumina and acrylic particles in the porous layer of the battery separator was 100 parts by volume, the alumina particles / acrylic particles was 80 / 20 parts by volume.

[0094] [Comparative Example 2] A battery separator was produced in the same manner as in Example 1, except that a polyethylene particle dispersion (average particle size 4.0 μm, melting point 55° C., solid content 40%) was used. However, the coating film was transferred to the conveying roll during coating, and a normal battery separator could not be obtained.

[0095] [Comparative Example 3] A battery separator was obtained in the same manner as in Example 1, except that a polyethylene particle dispersion (average particle size 4.0 μm, melting point 110° C., solid content concentration 40%) was used.

[0096] [Comparative Example 4] A battery separator was obtained in the same manner as in Example 1, except that the coating composition prepared in Example 1 was used to coat the heat-resistant particle layer to a thickness of 4.0 μm and the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was 1.0.

[0097] [Comparative Example 5] A battery separator was obtained in the same manner as in Example 1, except that the coating composition prepared in Example 1 was used to coat the heat-resistant particle layer so that the thickness of the heat-resistant particle layer was 1.9 μm and the magnification of the average particle size of the organic particles relative to the thickness of the heat-resistant particle layer was 2.1 times. When an LEI image of the porous layer surface was taken using a scanning electron microscope to calculate the average particle size of the polyethylene particles, it was confirmed that the polyethylene particles had fallen off, and a normal battery separator could not be obtained.

[0098] [Comparative Example 6] A polyethylene particle dispersion (average particle size 1.5 μm, melting point 83° C., solid content concentration 40%) was used to obtain a battery separator in the same manner as in Example 1. The thickness of the heat-resistant particle layer of the obtained battery separator was 1.4 μm.

[0099] [Comparative Example 7] A polyethylene particle dispersion (average particle size 6.6 μm, melting point 83° C., solid content concentration 40%) was used to obtain a battery separator in the same manner as in Example 1. The thickness of the heat-resistant particle layer of the obtained battery separator was 6.0 μm.

[0100] [Comparative Example 8] To 100 parts by mass of the alumina dispersion obtained in the same manner as in claim 1, 2.47 parts by mass of polyethylene particle dispersion Chemipearl A100 (manufactured by Mitsui Chemicals, Inc., solid content concentration 40%, melting point 83°C) was added while stirring with a three-one motor equipped with a dispersing blade, and further stirred for 10 minutes. Next, 4.08 parts by mass of an acrylic resin water dispersion with a solid content concentration of 40% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes. Next, 0.33 parts by mass of a fluorine-based surfactant with a solid content concentration of 50% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes to obtain a coating composition. The coating composition was coated on one side of a 12 μm-thick polyolefin microporous membrane by a microgravure method under conditions of a drying temperature of 50° C. and a conveying speed of 5 m / min to obtain a battery separator. The thickness of the heat-resistant particle layer of the battery separator was 3.0 μm, the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was 1.3 times, and when the total of the alumina and Chemipearl A100 in the porous layer of the battery separator was 100 volume parts, the alumina particles / Chemipearl A100=92 / 8 volume parts.

[0101] [Comparative Example 9] To 100 parts by mass of the alumina dispersion obtained in the same manner as in claim 1, 28.44 parts by mass of polyethylene particle dispersion Chemipearl A100 (manufactured by Mitsui Chemicals, Inc., solid content concentration 40%, melting point 83°C) was added while stirring with a three-one motor equipped with a dispersing blade, and further stirred for 10 minutes. Next, 7.5 parts by mass of an acrylic resin water dispersion with a solid content concentration of 40% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes. Next, 0.6 parts by mass of a fluorine-based surfactant with a solid content concentration of 50% was added to 100 parts by mass of the alumina dispersion while stirring, and further stirred for 10 minutes to obtain a coating composition. The coating composition was coated on one side of a 12 μm-thick polyolefin microporous membrane by a microgravure method under conditions of a drying temperature of 50° C. and a conveying speed of 5 m / min to obtain a battery separator. The thickness of the heat-resistant particle layer of the battery separator was 3.0 μm, the ratio of the average particle size of the organic particles to the thickness of the heat-resistant particle layer was 1.3 times, and when the total of the alumina and Chemipearl A100 in the porous layer of the battery separator was 100 volume parts, the alumina particles / Chemipearl A100=50 / 50 volume parts.

[0102] [Table 1]

Claims

1. A polyolefin microporous membrane; A battery separator comprising: a porous layer laminated on at least one surface of the polyolefin microporous membrane, the porous layer includes organic particles and heat-resistant particles; the organic particles are polyethylene; The organic particles have a melting point of 60° C. or more and 90° C. or less. a cross section of the porous layer is observed using a scanning electron microscope, and the thickness of the heat-resistant particle layer on one side on which the heat-resistant particles are present is 1.5 μm or more and 5.0 μm or less; the ratio of the number average particle size of the organic particles to the thickness of the heat-resistant particle layer is 1.1 times or more and 2.0 times or less; The porous layer contains organic particles in an amount of 10 parts by volume or more and 40 parts by volume or less relative to 100 parts by volume of the total of the organic particles and the heat-resistant particles in the porous layer. Battery separator.

2. 2. The battery separator of claim 1, wherein the heat-resistant particles comprise alumina, boehmite, or barium sulfate.

3. An electrode assembly comprising a positive electrode, a negative electrode, and the battery separator according to claim 1 or 2.

4. A non-aqueous secondary battery using the battery separator according to claim 1 or 2.

5. 3. A method for producing the battery separator according to claim 1, comprising the steps of: (a) A step of adding a dispersant to a solvent mainly composed of water, and then adding heat-resistant particles and stirring the mixture to obtain a mixed liquid. (b) A step of dispersing the mixture using a bead mill disperser to obtain a master batch liquid. (c) A step of adding the organic particles and a binder to the master batch liquid, and further adding other additives to obtain a coating composition. (d) coating at least one surface of the microporous polyolefin membrane with a coating composition. (e) After the coating, the solvent is dried with a dryer to form a porous layer.

Citation Information

Patent Citations

  • Separator for lithium-ion secondary battery

    JP2010238448A

  • Porous film and energy storage device

    JP2011168048A

  • Battery separator

    JP2017152268A

  • Nonaqueous electrolyte battery separator and nonaqueous electrolyte battery

    JP2018195564A

  • Separation membrane, lithium battery employing separation membrane, and manufacturing method of separation membrane

    JP2019133934A