Fuel cell and fuel cell stack

The use of porous metal layers in the fuel cell design addresses the ohmic loss issue, enhancing power generation efficiency and durability by facilitating uniform gas supply and low-resistance current flow.

JP7578018B2Active Publication Date: 2024-11-06NISSAN MOTOR CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021023712
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-17
Publication Date
2024-11-06
Estimated Expiration
2041-02-17

AI Technical Summary

Technical Problem

The large ohmic loss in solid oxide fuel cells due to current flow through thin electrode catalyst layers and lattice-shaped current collectors, leading to energy loss in the fuel cell stack.

Method used

A fuel cell design incorporating first and second porous metal layers that sandwich the anode and cathode layers, respectively, with these layers having a flat plate shape and interconnected pores to facilitate uniform gas supply and low-resistance current flow.

Benefits of technology

Reduces ohmic loss, enhances power generation efficiency, and improves durability by ensuring uniform gas supply and reducing electrical resistance in the current flow path.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578018000001
    Figure 0007578018000001
  • Figure 0007578018000002
    Figure 0007578018000002
  • Figure 0007578018000003
    Figure 0007578018000003
Patent Text Reader

Abstract

To provide a solid oxide type fuel battery cell and a solid oxide type fuel battery stack capable of reducing an ohmic loss.SOLUTION: A fuel battery cell (a cell 10) is configured by laminating an anode electrode layer 41, a cathode electrode layer 42, and a solid electrolyte layer 43 sandwiched between the anode electrode layer 41 and the cathode electrode layer 42. The fuel battery cell further comprises a first metal porous body layer 45, a first metal frame 31, a second metal porous body layer 46, and a second metal frame 34. The first metal porous body layer 45 is formed in a flat plate shape by a metal porous body having a plurality of vacancies communicated in a planer direction, holding the anode electrode layer 41 together with the solid electrolyte layer 43, and thus, allows the anode electrode layer 41 to be supplied with an anode gas through the plurality of vacancies. The second metal porous body layer 46 is formed in a flat plate shape by the metal porous body, holding the cathode electrode layer 42 together with the solid electrolyte layer 43, and thus, allows the cathode electrode layer 42 to be supplied with a cathode gas through the plurality of vacancies.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fuel cell and a fuel cell stack that constitute a solid oxide fuel cell. [Background technology]

[0002] Patent Document 1 describes a fuel cell stack composed of cells in which current collectors with lattice-shaped openings are joined to both sides of a flat-plate-shaped electrode reactant. In the fuel cell stack of Patent Document 1, adjacent cells are electrically connected by connecting external lead-out terminals located point-symmetrically in each cell with the current collectors. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 06-060905 Summary of the Invention [Problem to be solved by the invention]

[0004] The electrode catalyst layer of a fuel cell is generally formed of a thin film of about several tens of microns, and therefore, when a current flows in the planar direction, ohmic loss is large. When a current collector with lattice-shaped openings is used as the current collector, current flows through the current collector in the lattice portion connected to the current collector. However, in the opening portion, the current flows in the planar direction within the electrode catalyst layer. Therefore, when a current collector with lattice-shaped openings is used, ohmic loss is large. As a result, there is a problem that the generated power (energy) of the fuel cell stack is lost.

[0005] An object of the present invention is to provide a solid oxide fuel cell and a fuel cell stack with reduced ohmic losses. [Means for solving the problem]

[0006] A fuel cell according to an embodiment of the present invention is a fuel cell configured by stacking an anode layer, a cathode layer, and a solid electrolyte layer sandwiched between the anode layer and the cathode layer. The fuel cell further includes a first metal porous body layer, a first metal frame, a second metal porous body layer, and a second metal frame. The first metal porous body layer is formed in a flat plate shape by a metal porous body having a plurality of pores communicating in the surface direction, and sandwiches the anode layer together with the solid electrolyte layer, and supplies anode gas to the anode layer through the plurality of pores. The first metal frame is electrically connected to the anode layer via the first metal porous body layer by electrically connecting to the outer periphery of the first metal porous body layer, and supports the first metal porous body layer. The second metal porous body layer is formed in a flat plate shape by a metal porous body, sandwiches the cathode layer together with the solid electrolyte layer, and supplies cathode gas to the cathode layer through the plurality of pores. The second metal frame is electrically connected to the second metal porous body layer at the outer periphery of the second metal porous body layer, thereby being electrically connected to the cathode electrode layer via the second metal porous body layer and supporting the second metal porous body layer. Effect of the Invention

[0007] According to the present invention, it is possible to provide a solid oxide fuel cell and a fuel cell stack with reduced ohmic losses. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is an external perspective view of a cell stack. [Diagram 2] FIG. 2 is an exploded perspective view of the cell stack. [Diagram 3] FIG. 3 is an exploded perspective view of the cell. [Figure 4] FIG. 4 is a cross-sectional view of the cell. [Diagram 5] FIG. 5 is a partial cross-sectional view of the stack. [Figure 6] FIG. 6 is an explanatory diagram showing the flow of the anode gas. [Figure 7] FIG. 7 is an explanatory diagram showing the flow of the cathode gas. [Figure 8] FIG. 8 is an explanatory diagram showing a state in which the anode gas and the cathode gas are supplied via a metal porous layer. [Figure 9] FIG. 9 is an explanatory diagram showing paths along which current flows in a cell and a cell stack. [Figure 10] FIG. 10 is a cross-sectional view of the cell of the first comparative example. [Figure 11] FIG. 11 is an explanatory diagram showing the path of a current flowing through a cell of the first comparative example. [Figure 12] FIG. 12 is an explanatory diagram showing a defect caused by misalignment of a grid current collector. [Figure 13] FIG. 13 is a schematic cross-sectional view of a cell stack and a cell according to a second comparative example. [Figure 14] FIG. 14 is an explanatory diagram showing the shape of the active area, the installation range of the bus bar, and the path of the current. [Figure 15] FIG. 15 is an explanatory diagram showing the installation range of the busbar and the path of the current. [Figure 16] FIG. 16 is a graph showing the temperature distribution in the active area. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0010] [Cell stack structure] FIG. 1 is an external perspective view of a cell stack 100. The cell stack 100 is a fuel cell stack (solid oxide fuel cell stack) used in a solid oxide fuel cell (SOFC). The cell stack 100 is formed by arranging a plurality of solid oxide fuel cells (fuel cell) in a stacked manner and electrically connecting each of the solid oxide fuel cell cells. A fuel cell system is configured using one or a plurality of cell stacks 100. Hereinafter, each solid oxide fuel cell constituting the cell stack 100 will be referred to as a fuel cell, or more simply as a cell 10. The cell 10 may generally be referred to as a single cell.

[0011] 1, the cell stack 100 is generally flat as a whole. Therefore, the cells 10 that make up the cell stack 100 are also flat. The cell stack 100 is generally rectangular, and the surface perpendicular to the stacking direction of the cells 10 (hereinafter referred to as the stacking direction) is generally rectangular.

[0012] Hereinafter, with respect to the cell stack 100 and the cells 10, etc., the surface perpendicular to the stacking direction of the cells 10 will simply be referred to as the surface, regardless of whether it is the front or back. The short side direction of the surface is the X direction, the long side direction is the Y direction, and the stacking direction of the cells 10 is the Z direction. In the cell stack 100 and the cells 10, etc., the surfaces parallel to the Z direction are referred to as the side. Also, with respect to the cell stack 100 and the cells, etc., the X direction, Y direction, and Z direction may be referred to as the horizontal direction, vertical direction, and height direction (or thickness direction), respectively. The positive direction of each of the X, Y, and Z directions is defined to form a right-handed system.

[0013] Moreover, the negative end in each of the X, Y and Z directions is referred to as the "base end", and the positive end is referred to as the "tip end". With respect to the direction of the cell stack 100 and the cells 10, etc., "upper" refers to the positive side in the Z direction, and "lower" refers to the negative side in the Z direction. With respect to the length of the cell stack 100 and the cells 10, etc., the length in the X direction is referred to as the "length", and the length in the Y direction is referred to as the "width". In this embodiment, the direction in which the anode gas and the cathode gas flow in the cell stack 100 is the positive side in the Y direction. The Z direction is the thickness direction of the cell stack 100. Note that the cross-sectional views of this embodiment shown in FIG. 4 and the like below are cross-sections at the position indicated by AA in FIG. 1.

[0014] The cell stack 100 includes an inlet 11, an outlet 12, an active area 13, and bus bars 14 and 15.

[0015] The inlet 11 is a gas supply hole for supplying the anode gas and the cathode gas to the cell stack 100. In this embodiment, the inlet 11 is provided on the base end side of the cell stack 100 in the X direction. The anode gas is a fuel or a reformed fuel (reformed fuel), for example, a hydrocarbon fuel such as hydrogen or methane. The cathode gas is a so-called oxidizer, for example, air. In this embodiment, the inlet 11 includes, as gas supply holes, an anode gas supply hole 16b for supplying the anode gas, and cathode gas supply holes 16a and 16c for supplying the cathode gas. In the inlet 11 of this embodiment, the cathode gas supply hole 16a, the anode gas supply hole 16b, and the cathode gas supply hole 16c are arranged in a line in this order. However, the number and arrangement of the anode gas supply holes and the cathode gas supply holes are arbitrary.

[0016] The outlet 12 is a gas exhaust hole for exhausting anode off-gas and cathode off-gas. In this embodiment, the outlet 12 is provided on the tip side of the cell stack 100 in the X direction. The anode off-gas and cathode off-gas are anode gas and the like and cathode gas and the like exhausted from the cell stack 100. In this embodiment, the outlet 12 includes, as gas exhaust holes, an anode off-gas exhaust hole 17b for exhausting anode off-gas and cathode off-gas exhaust holes 17a, 17c for exhausting cathode off-gas. The cathode off-gas exhaust hole 17a, the anode off-gas exhaust hole 17b, and the cathode off-gas exhaust hole 17c are arranged in a line in this order. However, the number and arrangement of the anode off-gas exhaust holes and the cathode off-gas exhaust holes are arbitrary.

[0017] Hereinafter, the gas supply holes constituting the inlet 11 and the gas exhaust holes constituting the outlet 12 are collectively referred to as gas circulation holes. Furthermore, when it is not necessary to distinguish between anode gas and cathode gas in the explanation, anode gas, anode off-gas, cathode gas, and cathode off-gas will be collectively referred to simply as gas.

[0018] The active area 13 is an area where power generation actually occurs using the anode gas and the cathode gas. The active area 13 is formed between the inlet 11 and the outlet 12, that is, in the central portion of the cell stack 100.

[0019] The bus bars 14 and 15 are current collectors that electrically connect the cells 10 constituting the cell stack 100, thereby collecting the power generated by the cells 10. The bus bars 14 and 15 are made of, for example, a metal, and have electrical conductivity that is sufficient to prevent substantial loss of power generated by electricity generation. The bus bar 14 is attached to the side surface on the positive side in the X direction along the longitudinal direction of the cell stack 100. The bus bar 15 is attached to the side surface on the negative side in the X direction along the longitudinal direction of the cell stack 100. In this embodiment, the bus bars 14 and 15 connect the stacked cells 10 in series.

[0020] Fig. 2 is an exploded perspective view of the cell stack 100. As shown in Fig. 2, the cell stack 100 has a stack structure in which a plurality of cells 10 and gasket assemblies 18a, 18b are alternately stacked.

[0021] Each cell 10 has openings at positions corresponding to the inlet 11 and the outlet 12. That is, each cell 10 has a plurality of openings that form an anode gas supply hole 16b and cathode gas supply holes 16a, 16c, respectively, corresponding to the inlet 11. Similarly, each cell 10 has a plurality of openings that form an anode off-gas discharge hole 17b and cathode off-gas discharge holes 17a, 17c, respectively, corresponding to the outlet 12.

[0022] The structure of each cell 10 is the same, and in each cell 10, the electrode catalyst layer 32 is exposed in the active area 13. The electrode catalyst layer 32 is a laminate in which an anode electrode, a solid electrolyte, a cathode electrode, etc. are laminated, and the surface of the electrode catalyst layer 32 is divided into a surface that functions as an anode and a surface that functions as a cathode. Therefore, the cell 10 also has a front and a back. Hereinafter, the surface of the cell 10 that functions as an anode is referred to as an anode surface 22, and the surface that functions as a cathode is referred to as a cathode surface 23. The cell stack 100 has a cell arrangement in which a plurality of cells 10 are alternately stacked while being inverted so that the anode surfaces 22 face each other and the cathode surfaces 23 face each other. The structure of the cell 10 and the layer structure of the electrode catalyst layer 32 will be described in detail later.

[0023] In the above cell arrangement, two adjacent cells 10 are spaced apart by a predetermined distance. The distance between the cells 10 is adjusted by the thickness of the gasket assemblies 18a and 18b disposed between the cells 10.

[0024] The gasket assembly 18a is made of an insulator and is disposed at a position where the anode faces 22 of adjacent cells 10 face each other in the above cell arrangement. That is, the gasket assembly 18a is for the anode. The gasket assembly 18a includes an outer edge sealant 26, a gas flow hole sealant 27, and a ventilation support 28 (gas passage support).

[0025] When the cell stack 100 is formed, the peripheral sealing material 26 comes into contact with adjacent cells 10 to seal the spaces between those cells 10 (hereinafter referred to as inter-cell spaces). Therefore, the peripheral sealing material 26 isolates the inter-cell spaces from the outside (outside the cell stack 100).

[0026] The gas flow hole sealant 27 seals a part of the gas flow holes forming the inlet 11 and the outlet 12 at their outer peripheries. More specifically, the gas flow hole sealant 27 has an opening that forms a gas flow hole, for example, in its center. Therefore, the gas flow hole sealant 27 does not impede the flow of gas in the stack direction. On the other hand, when the cell stack 100 is formed, the gas flow hole sealant 27 is sandwiched between the upper and lower cells 10, thereby blocking the flow of gas into and out of the inter-cell space.

[0027] In the anode gasket assembly 18a, the gas flow hole sealant 27 seals the outer periphery of each of the cathode gas supply holes 16a, 16c and the cathode off-gas exhaust holes 17a, 17c. That is, the gas flow hole sealant 27 of the gasket assembly 18a blocks the flow of the cathode gas into and out of the inter-cell space while allowing the flow of the cathode gas and the cathode off-gas in the stack direction.

[0028] When the cell stack 100 is formed, the ventilation support material 28 supports the upper and lower cells 10 at the outer periphery of some of the gas circulation holes. Like the gas circulation hole sealing material 27, the ventilation support material 28 has an opening that forms a gas circulation hole, for example, in its center. Therefore, the ventilation support material 28 does not hinder the flow of gas in the stack direction. On the other hand, unlike the gas circulation hole sealing material 27, the ventilation support material 28 has a plurality of ventilation grooves (gas passage grooves) radially from the opening, for example. Therefore, the ventilation support material 28 does not hinder the flow of gas. Therefore, the ventilation support material 28 supports the upper and lower cells 10 in a manner that allows ventilation (gas passage).

[0029] In the anode gasket assembly 18a, the ventilation support 28 supports the upper and lower cells 10 on the outer periphery of the anode gas supply hole 16b and the anode off-gas discharge hole 17b, thereby allowing the anode gas and anode off-gas to flow into and out of the inter-cell space.

[0030] The gasket assembly 18b is disposed at a location where the cathode faces 23 of adjacent cells 10 face each other in the above-mentioned cell arrangement. That is, the gasket assembly 18b is for the cathode.

[0031] The gasket assembly 18b for the cathode is formed of an insulator, similar to the gasket assembly 18a for the anode, and includes an outer edge sealant 26, a gas flow hole sealant 27, and an airflow supporter 28. However, in the gasket assembly 18b, the gas flow hole sealant 27 seals the outer periphery of the anode gas supply hole 16b and the anode off-gas exhaust hole 17b. In the gasket assembly 18b for the cathode, the airflow supporter 28 supports the upper and lower cells 10 on the outer periphery of the cathode gas supply holes 16a, 16c and the cathode off-gas exhaust holes 17a, 17c. Therefore, the gasket assembly 18b blocks the flow of the anode gas into and out of the inter-cell space, and allows the flow of the cathode gas.

[0032] [Structure of cell and electrode catalyst layer] Fig. 3 is an exploded perspective view of the cell 10. As shown in Fig. 3, the cell 10 includes a first metal frame 31, an electrode catalyst layer 32, a seal cell 33, and a second metal frame .

[0033] The first metal frame 31 is a metal support that supports the electrode catalyst layer 32 at its outer periphery 48 (see FIG. 4). The first metal frame 31 is electrically connected to the electrode catalyst layer 32 at the outer periphery 48 (see FIG. 4) of the electrode catalyst layer 32. Specifically, the first metal frame 31 supports the electrode catalyst layer 32 while electrically connecting to it on the anode layer 41 side of the electrode catalyst layer 32. Therefore, the first metal frame 31 is connected to the first porous metal layer 45. As a result, the first metal frame 31 is electrically connected to the anode layer 41 via the first porous metal layer 45 and supports the first porous metal layer 45. As a result, the first metal frame 31 constitutes a current collector that becomes the anode electrode in the cell 10.

[0034] The first metal frame 31 exposes the electrode catalyst layer 32 through an opening provided in the center. That is, of the surfaces of the cell 10, the surface on which the first metal frame 31 is provided is the anode surface 22, and the first metal porous layer 45 is exposed. At least the portion of the electrode catalyst layer 32 exposed from the first metal frame 31 forms the active area 13. In addition, the first metal frame 31 has openings that form gas circulation holes, and connection portions that connect to the bus bars 14, 15.

[0035] The electrode catalyst layer 32 assists the reaction between the anode gas and the cathode gas by isolating the anode gas and the cathode gas while allowing the conduction of predetermined ions. The electrode catalyst layer 32 includes, as a basic component for causing a reaction between the anode gas and the cathode gas, a stack (hereinafter referred to as a basic stack 44 (see FIG. 4)) in which at least an anode electrode layer 41, a solid electrolyte layer 43 (see FIG. 4), and a cathode electrode layer 42 (see FIG. 4) are stacked in this order.

[0036] The seal cell 33 is a sealing member that seals the side surface of the electrode catalyst layer 32 when the cell 10 is formed. The seal cell 33 is also made of an insulator, and is sandwiched between the first metal frame 31 and the second metal frame 34 when the cell 10 is formed. Therefore, the seal cell 33 also functions as an insulating support for the first metal frame 31 and the second metal frame 34. Therefore, the seal cell 33 has an opening that exposes the entire surface of the electrode catalyst layer 32. The seal cell 33 also has an opening that forms a gas circulation hole.

[0037] The second metal frame 34 is a metal support that supports the electrode catalyst layer 32. The second metal frame 34 is electrically connected to the electrode catalyst layer 32 at an outer periphery 49 of the electrode catalyst layer 32. Specifically, the second metal frame 34 is connected to and supports the electrode catalyst layer 32 on the cathode layer 42 side of the electrode catalyst layer 32. Therefore, the second metal frame 34 is connected to the second porous metal layer 46. As a result, the second metal frame 34 is electrically connected to the cathode layer 42 via the second porous metal layer 46 and supports the second porous metal layer 46. As a result, the second metal frame 34 constitutes a current collector that serves as the cathode electrode in the cell 10.

[0038] The second metal frame 34 has an opening in the center to expose the electrode catalyst layer 32. That is, of the surfaces of the cell 10, the surface on which the second metal frame 34 is provided is the cathode surface 23, and the second metal porous layer 46 is exposed. At least the portion of the electrode catalyst layer 32 exposed from the second metal frame 34 forms the active area 13. In addition, the second metal frame 34 has openings that form gas circulation holes, and connection portions that connect to the bus bars 14, 15.

[0039] Fig. 4 is a cross-sectional view of the cell 10. As shown in Fig. 4, the electrode catalyst layer 32 includes a basic laminate 44 made up of an anode layer 41, a cathode layer 42, and a solid electrolyte layer 43 sandwiched between the anode layer 41 and the cathode layer 42.

[0040] The anode layer 41 is a flat thin film that functions as a so-called fuel electrode. The anode layer 41 is made of, for example, ceramic or a cermet made of ceramic and metal. The anode layer 41 has gas permeability, electrical conductivity, and ion conductivity that allow the anode gas to pass through it, to an extent that the anode layer 41 can function as a fuel electrode. The anode layer 41 also functions as a catalyst that promotes the reaction between the anode gas and oxide ions (e.g., oxygen ions) that have been transferred through the solid electrolyte layer 43.

[0041] The cathode layer 42 is a flat thin film that functions as a so-called oxidizer electrode (air electrode). The cathode layer 42 is formed of, for example, a metal oxide. The cathode layer 42 has gas permeability that allows the cathode gas to pass through, electrical conductivity, and ion conductivity to such an extent that the cathode layer 42 can function as an oxidizer electrode. The cathode layer 42 also functions as a catalyst that promotes ionization of an oxidizer (e.g., oxygen) contained in the cathode gas.

[0042] The solid electrolyte layer 43 is a flat thin film of a solid electrolyte having ion conductivity, and conducts oxidant ions. The solid electrolyte layer 43 is formed of, for example, solid oxide ceramic. The term "ceramic" refers to a sintered body of an inorganic material, and includes not only nonmetallic oxides but also metallic oxides.

[0043] The electrode catalyst layer 32 of this embodiment further includes, in addition to the basic laminate 44, a first metal porous body layer 45 and a second metal porous body layer 46.

[0044] The first metal porous layer 45 is a flat metal thin film formed so as to uniformly cover at least the anode layer 41 in the active area 13, and supports the basic stack 44 from the anode layer 41 side. Therefore, in the layer structure of the electrode catalyst layer 32, the first metal porous layer 45 sandwiches the anode layer 41 together with the solid electrolyte layer 43. The first metal porous layer 45 is formed thicker than the anode layer 41 to an extent that it can support the basic stack 44. For example, the first metal porous layer 45 is formed thicker than the anode layer 41 by about one order of magnitude.

[0045] The first porous metal layer 45 is formed of a porous metal. The porous metal is a porous body made of metal. The first porous metal layer 45 is formed of, for example, stainless steel (SUS) containing nickel, chromium, etc. The porous body refers to a member that contains countless minute pores (not shown) substantially randomly and that these pores are substantially randomly connected. Therefore, the multiple pores contained in the first porous metal layer 45 are connected in the surface direction (XY plane direction). The multiple pores contained in the first porous metal layer 45 are connected between the surfaces, and the distribution of the pores in the surface is substantially uniform.

[0046] Therefore, the first metal porous layer 45 is a good conductor having uniform electrical conductivity in the plane direction (XY in-plane direction) and thickness direction (Z direction), and behaves as a substantially continuous metal plate as a whole. In addition, the first metal porous layer 45 allows the anode gas to permeate substantially uniformly from one exposed surface (surface on the negative side in the Z direction) to the other surface (surface on the positive side in the Z direction) joined to the anode layer 41, due to the multiple pores. Therefore, when the anode gas is supplied to one exposed surface, the first metal porous layer 45 supplies the anode gas to the anode layer 41 through the multiple pores.

[0047] The second metal porous layer 46 is a flat metal thin film formed so as to uniformly cover the cathode layer 42 at least in the active area 13, and supports the basic stack 44 from the cathode layer 42 side. Therefore, in the layer structure of the electrode catalyst layer 32, the second metal porous layer 46 sandwiches the cathode layer 42 together with the solid electrolyte layer 43. The first metal porous layer 45 is formed thicker than the cathode layer 42 to an extent that it can support the basic stack 44. For example, the second metal porous layer 46 is formed thicker than the cathode layer 42 by about one order of magnitude.

[0048] The second metal porous layer 46 is formed of a metal porous body, similar to the first metal porous layer 45. Therefore, the second metal porous layer 46 is a good conductor having uniform electrical conductivity in the surface direction (XY in-plane direction) and thickness direction (Z direction), and behaves as a substantially continuous metal plate as a whole. In addition, the plurality of pores contained in the second metal porous layer 46 communicate with each other in the surface direction (XY in-plane direction). The plurality of pores contained in the second metal porous layer 46 communicate with each other between the surfaces, and the distribution of the pores in the surface is substantially uniform. Therefore, the second metal porous layer 46 allows the cathode gas to pass through substantially uniformly from one exposed surface (surface on the positive side in the Z direction) to the other surface (surface on the negative side in the Z direction) joined to the cathode electrode layer 42, due to the plurality of pores. Therefore, when the cathode gas is supplied to one exposed surface, the second metal porous layer 46 supplies the cathode gas to the cathode layer 42 through the plurality of pores.

[0049] As described above, the electrode catalyst layer 32 has a structure in which the basic laminate 44 is supported from both sides by the first metal porous layer 45 and the second metal porous layer 46. The electrode catalyst layer 32 is also joined to the first metal frame 31 and the second metal frame 34 by the first metal porous layer 45 and the second metal porous layer 46. Specifically, the first metal porous layer 45 is electrically connected to the first metal frame 31 at a part or all of its outer periphery 48. In this embodiment, in order to better reduce the electrical resistance (ohmic loss) at the connection portion, the first metal porous layer 45 and the first metal frame 31 are joined by a metal joining method such as welding at almost the entirety of the outer periphery 48. Similarly, the second metal porous layer 46 is electrically connected to the second metal frame 34 at a part or all of its outer periphery 49. In this embodiment, in order to better reduce electrical resistance (ohmic loss) at the connection portion, the second metal porous layer 46 and the second metal frame 34 are joined by a metal joining method such as welding around almost the entire outer periphery 49.

[0050] As described above, the cell 10 is a so-called metal-supported cell. In a typical conventional metal-supported cell, only one of the anode layer 41 side or the cathode layer 42 side is supported by a metal support. On the other hand, the cell 10 in this embodiment is supported by metal supports on both the anode side and the cathode side. Therefore, while a typical conventional metal-supported cell is a one-sided metal-supported cell, the cell 10 in this embodiment is, so to speak, a two-sided metal-supported cell.

[0051] The first and second porous metal layers 45 and 46 may be formed by any method. The first and second porous metal layers 45 and 46 may be formed of felt or nonwoven fabric made of metal fibers, or a sintered body of metal particles. However, the first and second porous metal layers 45 and 46 are preferably sintered bodies of metal particles. Compared with the cases formed by other methods, sintered bodies of metal particles have excellent electrical conductivity and rigidity (strength). For this reason, the first and second porous metal layers 45 and 46 are preferably formed of metal particles.

[0052] In this embodiment, the first metal porous body layer 45 and the second metal porous body layer 46 are formed as a sintered body integral with the basic laminate 44 by co-firing. Specifically, first, a first metal porous body slurry, an anode slurry, an electrolyte slurry, a cathode slurry, and a second metal porous body slurry are prepared as slurries for forming each layer of the electrode catalyst layer 32. Next, each of the slurries is formed into a sheet shape, and the sheets are laminated and bonded together in the order of lamination in the electrode catalyst layer 32 to form a molded slurry laminate. Thereafter, the molded slurry laminate is degreased and co-fired to form the electrode catalyst layer 32.

[0053] [Detailed structure of the cell stack] Fig. 5 is a partial cross-sectional view of the cell stack 100. As shown in Fig. 5, due to the cell arrangement in which the anode faces 22 face each other and the cathode faces 23 face each other, and the internal structure of the gasket assemblies 18a, 18b, the inter-cell space between the opposing anode faces 22 becomes an anode gas flow path FPa through which the anode gas flows. Similarly, the inter-cell space between the opposing cathode faces 23 becomes a cathode gas flow path FPc through which the cathode gas flows.

[0054] The anode gas flow path FPa supplies anode gas to two adjacent cells 10. That is, in the cell stack 100, the anode gas flow path FPa serves two cells 10. The height H1 of the anode gas flow path FPa can be adjusted as desired by changing the thickness of the gasket assembly 18a. Therefore, the cross-sectional area of ​​the anode gas flow path FPa can be adjusted as desired.

[0055] The cathode gas flow path FPc supplies cathode gas to two adjacent cells 10. That is, in the cell stack 100, the cathode gas flow path FPc serves two cells 10. The height H2 of the cathode gas flow path FPc can be adjusted as desired by changing the thickness of the gasket assembly 18b. Therefore, the cross-sectional area of ​​the cathode gas flow path FPc can also be adjusted as desired.

[0056] When the cell stack 100 generates power, for example, the flow rate of the cathode gas is usually greater than the flow rate of the anode gas. For this reason, in this embodiment, the pressure loss of the anode gas in the anode gas flow passage FPa and the pressure loss of the cathode gas in the cathode gas flow passage FPc are individually adjusted according to the flow rates of the anode gas and the cathode gas. Specifically, the height H2 of the cathode gas flow passage FPc is set to be higher than the height H1 of the anode gas flow passage FPa. That is, the gasket assembly 18b is formed thicker than the gasket assembly 18a, and as a result, H2>H1. As a result, in the cell stack 100, the cross-sectional area of ​​the cathode gas flow passage FPc is larger than the cross-sectional area of ​​the anode gas flow passage FPa. In this way, when the pressure losses in the anode gas flow passage FPa and the cathode gas flow passage FPc are each reduced, the power consumption of devices that supply the anode gas and the cathode gas to the cell stack 100, such as a blower and a pump (not shown), is reduced. Furthermore, when the pressure losses of the anode gas and cathode gas are appropriately adjusted, the power generation reaction and the like occur almost uniformly in the active area 13. Therefore, by reducing the pressure losses of the anode gas and cathode gas, temperature distribution is less likely to occur in the active area 13.

[0057] The bus bars 14, 15 are joined to the first metal frame 31 and the second metal frame 34 of each cell 10 by metal joining such as welding. In this way, the bus bars 14, 15 electrically connect the adjacent cells 10 to each other.

[0058] In this embodiment, the bus bar 14 connects the first metal frame 31, which is the anode of a certain cell 10 (the cell 10 in the middle row of FIG. 5), to the cell 10 in the upper row of FIG. 5 adjacent to this cell 10, at the second metal frame 34, which is the cathode. The bus bar 15 connects the cell 10 in the middle row of FIG. 5, to which the bus bar 14 connects to the first metal frame 31, at the second metal frame 34, which is the cathode. Furthermore, the bus bar 15 connects the cell 10 in the lower row of FIG. 5, to which the bus bar 14 connects to the second metal frame 34, at the first metal frame 31, which is the anode. That is, the bus bar 14 connects two adjacent cells 10 in series, and the bus bar 15 further connects the set of cells 10 connected in series by the bus bar 14 in series. Conversely, it can be said that the bus bar 15 connects two adjacent cells 10 in series, and the bus bar 14 further connects the set of cells 10 connected in series by the bus bar 15 in series.

[0059] [Anode and cathode gas flow] 6 is an explanatory diagram showing the flow of the anode gas. As shown by the thick arrows in FIG. 6, the anode gas flowing through the anode gas supply holes 16b is jetted radially from the ventilation grooves of the ventilation support material 28 into the anode gas flow path FPa. As a result, the anode gas is supplied to the anode gas flow path FPa. In the anode gas flow path FPa, the anode gas flows substantially parallel to and substantially uniformly along the anode surface 22 toward the positive side in the X direction. The anode gas is then discharged to the anode off-gas discharge hole 17b through the ventilation grooves of the ventilation support material 28 provided in correspondence with the anode off-gas discharge hole 17b.

[0060] FIG. 7 is an explanatory diagram showing the flow of the cathode gas. As shown by the thick dashed arrows in FIG. 7, the cathode gas flowing through the cathode gas supply holes 16a and 16c is radially ejected from the two ventilation support members 28 through the respective ventilation grooves. This allows the cathode gas to be supplied to the cathode gas flow path FPc. In the cathode gas flow path FPc, the cathode gas flows substantially parallel to and substantially uniformly along the cathode surface 23 toward the positive side in the X direction. Thereafter, the cathode gas is discharged to the cathode offgas discharge hole 17a and the cathode offgas discharge hole 18c through the ventilation grooves of the two ventilation support members 28 provided corresponding to the cathode offgas discharge holes 17a and 17c, respectively.

[0061] FIG. 8 is an explanatory diagram showing the supply state of the anode gas and the cathode gas through the metal porous body layer. As shown in FIG. 8, the anode gas comes into contact with the first metal porous body layer 45 while flowing through the anode gas flow passage FPa as described above. As a result, the anode gas passes through the pores of the first metal porous body layer 45 and is supplied to the anode electrode layer 41. Since the very small pores of the first metal porous body layer 45 are uniformly formed, the anode gas is uniformly supplied to the entire surface of the anode electrode layer 41 at least within the range of the active area 13. That is, at least in the active area 13, there is no part where the anode gas does not reach the anode electrode layer 41 due to the presence of the first metal porous body layer 45. Therefore, the anode gas reaches the entire surface of the anode electrode layer 41 substantially uniformly.

[0062] In addition, the cathode gas comes into contact with the second metal porous layer 46 while flowing through the cathode gas flow path FPc as described above. As a result, the cathode gas passes through the pores of the second metal porous layer 46 and is supplied to the cathode electrode layer 42. Since the minute pores of the second metal porous layer 46 are uniformly formed, the cathode gas is supplied uniformly to the entire surface of the cathode electrode layer 42 at least within the range of the active area 13. That is, at least in the active area 13, there is no portion where the cathode gas does not reach the cathode electrode layer 42 due to the presence of the second metal porous layer 46. Therefore, the cathode gas reaches the entire surface of the cathode electrode layer 42 substantially uniformly.

[0063] [Current flow in cells and cell stacks] Fig. 9 is an explanatory diagram showing paths along which current flows in a cell 10 and a cell stack 100. As indicated by thick arrows in Fig. 9, in a cell 10 in the lower part of Fig. 9, current flows into the second metal frame 34, which is the cathode, via the bus bar 14. This current flows in the planar direction along the second porous metal layer 46 connected to the second metal frame 34. This is because the second porous metal layer 46 is a good conductor and has a lower electrical resistance than the cathode layer 42.

[0064] Furthermore, as indicated by the thick dashed arrow, when this cell 10 generates electricity, the current that flows into the second metal porous layer 46 and the current generated by the power generation pass through the basic laminate 44 (cathode electrode layer 42, solid electrolyte layer 43, and anode electrode layer 41) and flow into the first metal porous layer 45.

[0065] Here, the basic laminate 44 is thinner than the first metal porous layer 45 and the second metal porous layer 46, and has poor electrical conductivity. Therefore, the electrical resistance in the planar direction of the basic laminate 44 is greater than the electrical resistance in the planar direction of the first metal porous layer 45 and the second metal porous layer 46. In addition, since the first metal porous layer 45 and the second metal porous layer 46 supply the anode gas and the cathode gas to the active area 13 almost uniformly, power is generated almost uniformly in the entire range of the active area 13. For these reasons, the propagation of current in the planar direction is mainly performed by the first metal porous layer 45 and the second metal porous layer 46. Therefore, in the cell 10, the current flow in the basic laminate 44 is in a direction almost perpendicular to the surface of the electrode catalyst layer 32.

[0066] The current that has flowed into the first porous metal layer 45 propagates in the planar direction along the first porous metal layer 45. Then, the current propagates through the bus bar 15 and flows into the second metal frame 34 of the adjacent cell 10 in the upper part of FIG.

[0067] The current that flows into the adjacent cell 10 flows into the second metal porous layer 46 in the same manner as the cell 10 in the lower row of Fig. 9, as indicated by the thick arrow. Then, as the adjacent cell 10 generates power, the current that has flowed in and the current generated by the power generation flow almost vertically through the basic laminate 44, as indicated by the thick dashed arrow, and flows into the first metal porous layer 45. The current that has flowed into the first metal porous layer 45 propagates in the direction of the surface, propagates through the first metal frame 31 and the bus bar 14, and flows into the second metal frame 34 of the next cell 10. The above process is repeated thereafter.

[0068] [Functions of cells and cell stacks] The operation of the cell 10 and cell stack 100 configured as described above will be explained below by comparing a first comparative example with a second comparative example.

[0069] (1) Comparison with the first comparative example 10 is a cross-sectional view of a cell 210 of the first comparative example. The cell 210 of the first comparative example is configured by replacing the first metal porous layer 45 and the second metal porous layer 46 of the cell 10 according to the above embodiment with a lattice current collector 211 having lattice-shaped openings, and the other configuration is the same as that of the above embodiment. In the first comparative example, the cell 210 is configured to form a cell stack with the same cell arrangement as that of the above embodiment.

[0070] The lattice collector 211 is formed by providing a plurality of openings in a metal sheet. Therefore, the anode gas and the cathode gas are blocked by the lattice collector 211. That is, as shown in FIG. 10, the anode gas reaches the anode electrode layer 41 only at the openings of the lattice collector 211. Similarly, the cathode gas reaches the cathode electrode layer 42 only at the openings of the lattice collector 211. Therefore, the two lattice collectors 211 are aligned so that the positions of the openings are aligned. The active area of ​​the cell 210 of the first comparative example is limited to the range where the openings of the two lattice collectors 211 are aligned in the Z direction.

[0071] FIG. 11 is an explanatory diagram showing the path of a current flowing through a cell 210 of the first comparative example. As shown in FIG. 11, in a certain cell 210, the current flows into the lattice current collector 211 on the cathode layer 42 side through the second metal frame 34 as shown by the thick arrow, and propagates along the lattice current collector 211. However, since the lattice current collector 211 has an opening, the current propagates in the surface direction through not only the lattice current collector 211 but also the cathode layer 42. That is, when the lattice current collector 211 is used, a current flows through the cathode layer 42 in the surface direction to a certain extent. Since the cathode layer 42 is formed extremely thin, the electrical resistance in the surface direction is very high. Therefore, the current flowing in the surface direction through the cathode layer 42 generates energy loss (so-called ohmic loss) due to this high electrical resistance.

[0072] In the cell 210 of the first comparative example, the active area is limited to the opening, so that the current flowing into the lattice collector 211 on the cathode layer 42 side and the current generated by power generation flow toward the anode layer 41 at the opening of the lattice collector 211, as shown by the thick dashed arrow. Therefore, the current that reaches the anode layer 41 propagates in the surface direction of the anode layer 41 and flows into the lattice collector 211 provided on the anode layer 41 side. The anode layer 41 is formed extremely thin like the cathode layer 42, so the electrical resistance in the surface direction is very high. Therefore, the current that reaches the anode layer 41 further generates ohmic loss due to this high electrical resistance.

[0073] When a cell stack is constructed using the cells 210 of the first comparative example, the above-mentioned ohmic loss occurs in each cell 210. In particular, the more cells 210 are connected in series to ensure a desired output voltage, the greater the ohmic loss becomes.

[0074] Comparing the cell 10 according to the present embodiment with the cell 210 according to the first comparative example, the cell 10 according to the present embodiment uses the first metal porous layer 45 and the second metal porous layer 46, so that the ohmic loss that occurs in the cell 210 according to the first comparative example is hardly generated. That is, the cell 10 according to the present embodiment reduces the ohmic loss compared to the cell 210 according to the first comparative example. Since the cell stack is composed of a plurality of cells, this feature is more prominent in the cell stack. That is, since the cell stack 100 according to the present embodiment is composed of the cells 10, the ohmic loss is significantly reduced compared to the cell stack composed of the cells 210 according to the first comparative example. In particular, since the cell stack 100 according to the present embodiment connects the cells 10 in series, the ohmic loss is particularly significantly reduced compared to the cell stack in which the cells 210 according to the first comparative example are connected in series.

[0075] Moreover, in the cell 10 according to this embodiment, the entire region where the first metal porous layer 45 and the second metal porous layer 46 are exposed is the active area 13. Therefore, in the cell 10 according to this embodiment, the area of ​​the electrode catalyst layer 32 that contributes to power generation is larger than that of the cell 210 of the first comparative example. As a result, the cell 10 according to this embodiment has better power generation efficiency per area, i.e., better power generation performance, than the cell 210 of the first comparative example. By forming the cell stack 100, this feature becomes more pronounced.

[0076] Fig. 12 is an explanatory diagram showing a defect caused by misalignment of the lattice current collector 211. As shown in Fig. 12, in the cell 210 of the first comparative example, it is assumed that the front and back lattice current collectors 211 are misaligned due to manufacturing errors or the like. In the cell 210 of the first comparative example, the active area is limited to the range where the openings of the two lattice current collectors 211 are aligned, and if there is such misalignment of the two lattice current collectors 211, the effective active area AE becomes even narrower than the openings of the lattice current collectors 211.

[0077] In contrast, the cell 10 according to this embodiment uses the first metal porous layer 45 and the second metal porous layer 46 which are substantially uniform, and therefore does not suffer from positional deviation as occurs with the lattice current collector 211. Therefore, in the cell 10 according to this embodiment, almost the entire surface of the exposed electrode catalyst layer 32 becomes the active area 13. Therefore, compared to the cell 210 of the first comparative example, the cell 10 according to this embodiment can obtain good power generation performance without being dependent on extremely slight manufacturing errors and the like.

[0078] Furthermore, in the cell 210 of the first comparative example, localized stress occurs due to misalignment of the lattice current collectors 211 on the front and back sides. This may result in cracks 212 in the basic laminate 44 (see FIG. 11). If cracks 212 occur, then depending on the extent of the cracks, part or all of the cell 210 may cease to function. The cracks 212 may occur during manufacturing, such as when bonding the lattice current collectors 211 to the basic laminate 44, but may also occur due to thermal expansion and contraction caused by repeated use and discontinuance of the cell 210.

[0079] In contrast, in the cell 10 according to this embodiment, the first metal porous layer 45 and the second metal porous layer 46 uniformly cover the anode layer 41 and the cathode layer 42, respectively. Therefore, the first metal porous layer 45 and the second metal porous layer 46 do not generate local stress in the basic laminate 44. Therefore, in the cell 10 according to this embodiment, cracks caused by the first metal porous layer 45 and the second metal porous layer 46 are hardly generated in the basic laminate 44 during manufacturing and repeated use. Therefore, the cell 10 according to this embodiment is superior in manufacturing suitability to the cell 210 of the first comparative example. In addition, the cell 10 according to this embodiment has high durability against thermal expansion and contraction and is stable against repeated use.

[0080] The cell 10 according to the present embodiment has a layer structure in which the basic laminate 44 is sandwiched between the first metal porous body layer 45 and the second metal porous body layer 46, which are approximately one order of magnitude thicker than the basic laminate 44. When the electrode catalyst layer 32 expands and contracts, the expansion and contraction of the first metal porous body layer 45 and the second metal porous body layer 46 is dominant. The first metal porous body layer 45 and the second metal porous body layer 46 are disposed symmetrically with respect to the basic laminate 44, and are substantially the same in terms of properties related to expansion and contraction, warping, and the like. For this reason, the cell 10 having the first metal porous body layer 45 and the second metal porous body layer 46 is unlikely to generate internal stress that causes warping (bending) of the basic laminate 44 during manufacture or repeated use. From this viewpoint as well, the cell 10 according to the present embodiment has excellent manufacturability and is stable against repeated use.

[0081] (2) Comparison with the second comparative example FIG. 13 is a schematic cross-sectional view of a cell stack 300 and a cell 310 according to a second comparative example. The cell stack 300 and the cell 310 according to the second comparative example are of a typical conventional form. As shown in FIG. 13, the cell 310 is a so-called one-side metal support cell. That is, the cell 310 is configured by removing the first metal porous layer 45 and the first metal frame 31 from the cell 10 according to this embodiment. Therefore, in the cell 310, on the anode layer 41 side, the surface of the anode layer 41 is exposed, not the first metal porous layer 45. On the other hand, on the cathode layer 42 side, the second metal porous layer 46 is exposed, similar to the cell 10 according to this embodiment.

[0082] The cell stack 300 is formed by stacking a plurality of cells 310 with separators 311 interposed therebetween. In the cell stack 300, the cells 310 are stacked with a fixed front-back relationship. For example, in FIG. 13, the lower cell 310 is arranged with the second metal porous layer 46 facing the negative side in the Z direction and the anode layer 41 facing the positive side in the Z direction. The upper cell 310 is stacked on the lower cell 310 with the second metal porous layer 46 facing the negative side in the Z direction and the anode layer 41 facing the positive side in the Z direction, similar to the lower cell 310.

[0083] The separator 311 is provided with a plurality of grooves extending in parallel in the Y direction. The tops 311a and 311c of the separator 311 formed by these grooves come into contact with the anode layer 41 and the second metal porous layer 46 of the adjacent cells 310 when the cell stack 300 is formed. As a result, the inter-cell space formed between the adjacent cells 310 is divided into a plurality of parallel sections by the separator 311. Of these sections, the section adjacent to the anode layer 41 is used as an anode gas flow path FPa. On the other hand, the section adjacent to the second metal porous layer 46 (cathode layer 42) is used as a cathode gas flow path FPc.

[0084] The separator 311 is made of, for example, metal. Therefore, the top 311a of the separator 311 abuts against the second metal porous layer 46, thereby electrically connecting the separator 311 to the cathode layer 42 of a certain cell 310 (the cell 310 in the upper part of FIG. 13) via the second metal porous layer 46. The top 311c of the separator 311 abuts against the anode layer 41, thereby electrically connecting the separator 311 to the anode layer 41 of an adjacent cell 310 (the cell 310 in the lower part of FIG. 13). The end of the separator 311 is provided so as to extend outside the inter-cell space. Therefore, the separator 311 functions as a current collector.

[0085] Comparing the cell 10 according to the present embodiment with the cell 310 according to the second comparative example configured as described above, the cell 10 according to the present embodiment is different in that the first metal porous layer 45 is provided on the anode layer 41 side, whereas the cell 310 according to the second comparative example does not have this. Therefore, in the cell 10 according to the present embodiment, the current propagating in the surface direction on the anode layer 41 side flows through the first metal porous layer 45 with low electrical resistance, whereas in the cell 310 according to the second comparative example, the current flows through the anode layer 41 with high electrical resistance before flowing into the separator 311. Therefore, in the cell 10 according to the present embodiment, the ohmic loss is reduced compared to the cell 310 according to the second comparative example.

[0086] In addition, when comparing the cell stack 100 according to the present embodiment with the cell stack 300 of the second comparative example, the cell stack 300 of the second comparative example uses a separator 311, whereas the cell stack 100 according to the present embodiment does not use the separator 311. In the cell stack 300 of the second comparative example, the separator 311 is used, and as a result, the anode gas flow passage FPa and the cathode gas flow passage FPc are divided into a plurality of narrowed flow passages. In contrast, in the cell stack 100 according to the present embodiment, the entire inter-cell space functions as one anode gas flow passage FPa or cathode gas flow passage FPc, and therefore the cross-sectional areas of these flow passages are larger than those of the cell stack 300 of the second comparative example. Therefore, the cell stack 100 according to the present embodiment has a reduced pressure loss of the anode gas flowing through the anode gas flow passage FPa and a reduced pressure loss of the cathode gas flowing through the cathode gas flow passage FPc, compared to the cell stack 300 of the second comparative example. As a result, the cell stack 100 according to this embodiment reduces the power consumption of devices that supply anode gas and cathode gas to the cell stack 100, such as blowers and pumps (not shown).

[0087] In the cell stack 300 of the second comparative example, each anode gas flow path FPa and cathode gas flow path FPc supplies anode gas and cathode gas to one cell 310. In contrast, in the cell stack 100 of the present embodiment, one anode gas flow path FPa and cathode gas flow path FPc supplies anode gas and cathode gas to two adjacent cells 10, respectively. That is, the cell stack 100 of the present embodiment is configured by combining two flow paths required in the cell stack 300 of the second comparative example into one flow path. Therefore, the cell stack 100 of the present embodiment can be formed thinner and smaller than the cell stack 300 of the second comparative example. In addition, the cell stack 100 of the present embodiment can be highly integrated compared to the cell stack 300 of the second comparative example.

[0088] In particular, in the cell stack 100 according to this embodiment, the anode gas flow path FPa and the cathode gas flow path FPc are not divided into thin sections. Also, the pressure loss of the anode gas and the cathode gas is reduced. Therefore, the heights H1, H2 of the anode gas flow path FPa and the cathode gas flow path FPc can be set lower than in the second comparative example. This also contributes to making the cell stack 100 according to this embodiment thinner, more compact, and more highly integrated.

[0089] [Active cell shape and busbar installation range] In the cell 10 and cell stack 100 according to the above embodiment, the shape of the active area 13 and the installation range of the bus bars 14, 15 are arbitrary. However, it is preferable that the shape of the active area 13 and the installation range of the bus bars 14, 15 are determined as follows.

[0090] 14 is an explanatory diagram showing the shape of the active area 13, the installation range of the bus bars 14 and 15, and the current path. As shown in FIG. 14, the width of the active area 13 is "W1" and the length of the active area 13 is "L1". In this case, it is preferable that the shape of the active area 13 has a high aspect ratio in which the aspect ratio L1 / W1, which is the ratio of the length L1 to the width W1, is greater than 1. For example, it is particularly preferable that the active area 13 has a generally rectangular shape in which the length L1 is greater than the width W1.

[0091] In other words, when the flow direction (Y direction) of the anode gas and cathode gas is defined as a first direction and the direction perpendicular to this first direction (X direction) is defined as a second direction, it is preferable that the active area 13 has a shape that is longer in the first direction (Y direction) than in the second direction (X direction).

[0092] In this way, when the active area 13 has a shape with a high aspect ratio, the anode gas is distributed well in the anode gas flow channel FPa, and the anode gas flows almost uniformly in the anode gas flow channel FPa. Similarly, the cathode gas is distributed well in the cathode gas flow channel FPc, and the cathode gas flows almost uniformly in the cathode gas flow channel FPc.

[0093] The bus bars 14 and 15 are attached to the cell array in parallel to a first direction (Y direction) that is the flow direction of the anode gas and cathode gas. It is preferable that the length L2 of the bus bars 14 and 15 along the first direction (Y direction) is equal to or greater than the length L1 of the active area 13 along the first direction (Y direction).

[0094] In this way, when the length L2 of the busbars 14, 15 is made equal to or greater than the length L1 of the active area 13, the generated electricity (current) flows through the active area 13 from one busbar 14 to the other busbar 15, generally parallel to the second direction (X direction), and uniformly in the first direction (Y direction), as shown by the thick arrow in Fig. 14. That is, the current density of the current flowing from the busbar 14 to the busbar 15 is approximately uniform (constant) throughout the active area 13. Therefore, heat generated by the current flow is generated uniformly in the active area 13, and the occurrence of local or overall heat distribution in the active area 13 is suppressed. Therefore, when the busbars 14, 15 are made equal to or greater than the length L1 of the active area 13, power generation is performed uniformly and efficiently using the entire surface of the active area 13.

[0095] In particular, as described above, when the active area 13 has a shape with a high aspect ratio, the width W1 of the active area 13 is shorter than the length L1, so that the distance that electricity generated by power generation travels through the active area 13 is short. This reduces ohmic loss in the active area 13. As a result, the recovery rate (utilization rate) of electricity generated by power generation is high. In other words, when the length L2 of the bus bars 14, 15 is made equal to or greater than the length L1 of the active area 13, the power generation performance of the cell stack 100 is improved.

[0096] It is particularly preferable that the length L2 of the busbars 14, 15 is approximately equal to the length L1 of the active area 13. This is because the length of the cells 10 and the cell stack 100 can be made as short as possible while improving the power generation performance of the cell stack 100 as described above. The length L2 of the busbars 14, 15 being "approximately equal" to the length L1 of the active area 13 means that the length L2 of the busbars 14, 15 has a length that can improve the power generation performance of the cell stack 100 as described above. Therefore, it is also acceptable for the length L2 of the busbars 14, 15 to be slightly shorter than the length L1 of the active area 13.

[0097] Fig. 15 is an explanatory diagram showing the installation range of the bus bars 14, 15 and the current path. As shown in Fig. 15, when the anode gas and the cathode gas flow in parallel in the cell stack 100, the length L2 of the bus bars 14, 15 may be shorter than the length L1 of the active area 13. In this case, it is preferable that the bus bars 14, 15 are provided unevenly on the upstream side (negative side in the Y direction) of the anode gas and the cathode gas with respect to the active area 13. Note that "parallel" in relation to the flow of the anode gas and the cathode gas means that the flow paths of the anode gas and the cathode gas are approximately parallel and that the anode gas and the cathode gas flow in the same direction.

[0098] In this way, when the bus bars 14, 15 are unevenly located on the upstream side of the anode gas and the cathode gas, the current flowing through the active area 13 from the bus bar 14 to the bus bar 15 is concentrated in a part of the active area 13, as shown by the thick arrow. In current concentrated area 401 where the current is concentrated in this way, more heat (Joule heat) is generated than in current sparse area 402 where the current is relatively sparse. When the anode gas and the cathode gas flow in parallel, a temperature distribution may occur in the active area 13, but by unevenly locating the bus bars 14, 15 as described above, the temperature distribution is corrected.

[0099] Fig. 16 is a graph showing the temperature distribution of the active area 13. As shown by the dashed line in Fig. 16, when the anode gas and the cathode gas flow in parallel and in the same direction, a temperature distribution may occur in the active area 13 in which the temperature increases from the inlet 11 to the outlet 12. For this reason, if the bus bars 14, 15 are unevenly located upstream of the anode gas and the cathode gas to generate a current concentration area 401 on the upstream side of the active area 13, the temperature of the current concentration area 401 increases. As a result, as shown by the solid line, the temperature distribution of the active area 13 is corrected. Note that the two-dot chain line in Fig. 16 indicates the ideal temperature at which power generation efficiency is maximized.

[0100] Therefore, as described above, when the anode gas and the cathode gas flow in parallel, if the bus bars 14, 15 are located on the upstream side, the power generation performance of the cells 10 and the cell stack 100 improves.

[0101] The length L2 of the busbars 14, 15 relative to the length L1 of the active area 13 is suitably determined based on an experiment, a simulation, or the like. When the busbars 14, 15 are shorter than the active area 13, the busbars 14, 15 are preferably installed from the base end of the active area 13. However, even if the installation positions of the busbars 14, 15 are slightly shifted from the base end of the active area 13 and a current insufficiency area 402 is also generated in the base end portion of the active area 13, the above-mentioned effect of improving the power generation performance is achieved. Therefore, the busbars 14, 15 may be installed such that, for example, when the current insufficiency area 402 on the tip side is compared with the current insufficiency area 402 on the base end side (not shown), the current insufficiency area 402 on the tip side is larger (longer).

[0102] Furthermore, when the cells 10 are of the so-called internal reforming type, a reforming catalyst that reforms the fuel is preferably provided in a part or all of the range of the current concentration area 401. Specifically, the first metal porous layer 45 of each cell 10 is configured to include the reforming catalyst in a part or all of the range of the current concentration area 401 that is formed in the active area 13 by the presence of the busbars 14, 15. The reforming catalyst can be provided in the first metal porous layer 45 by a method such as coating or impregnation.

[0103] Because the fuel reforming reaction is an endothermic reaction, the temperature distribution shown by the dashed dotted line in Fig. 16 becomes more pronounced. For this reason, as described above, if the reforming catalyst is provided within the current concentration area 401, the temperature drop due to the reforming reaction is compensated for by heat generated by the current concentration, and the temperature distribution of the cell 10 and the cell stack 100 can be made closer to an ideal temperature distribution. This improves the power generation performance of the cell 10 and the cell stack 100 even when the cell 10 is an internal reforming type.

[0104] In the above embodiment, when the cell stack 100 is constructed, the cells 10 are connected in series by the bus bars 14 and 15. However, some or all of the cells 10 constituting the cell stack 100 may be connected in parallel depending on the desired current and voltage to be obtained by power generation. When the cells 10 are connected in parallel, the first metal frames 31 of the adjacent cells 10 and the second metal frames 34 of the adjacent cells 10 are connected by the bus bars 14 and 15. When the cells 10 are connected in parallel, the bus bars 14 and 15 can be omitted by forming some or all of the gasket assemblies 18a and 18b from a conductive material such as metal. For example, the outer edge sealing material 26 of the gasket assemblies 18a and 18b is formed from a conductive material, so that the first metal frames 31 of the adjacent cells 10 and the second metal frames 34 of the adjacent cells 10 are electrically connected to each other. In this way, by omitting the bus bars 14 and 15, the cells 10 and the cell stack 100 can be formed more easily and at a lower cost.

[0105] In the above embodiment, the flow directions of the anode gas and the cathode gas are parallel in the cell stack 100, but the anode gas and the cathode gas can be made to flow in opposite directions. For example, an anode gas supply device (not shown) is connected to the cell 10 so that the anode gas flows from the anode gas supply hole 16b to the anode off-gas exhaust hole 17b as in the above embodiment. On the other hand, a cathode gas supply device (not shown) is connected to the cell 10 so that the cathode gas flows from the cathode off-gas exhaust holes 17a, 17c to the cathode gas supply holes 16a, 16c, in the opposite direction to the above embodiment. As a result, the anode gas and the cathode gas flow in opposite directions in the cell 10. The term "opposite" with respect to the flow of the anode gas and the cathode gas means that the flow paths of the anode gas and the cathode gas are approximately parallel and the anode gas and the cathode gas flow in opposite directions. The term "opposite" used here may be referred to as anti-parallel.

[0106] As described above, the fuel cell (cell 10) according to this embodiment is a fuel cell configured by stacking an anode layer 41, a cathode layer 42, and a solid electrolyte layer 43 sandwiched between the anode layer 41 and the cathode layer 42. This fuel cell (cell 10) further includes a first metal porous body layer 45, a first metal frame 31, a second metal porous body layer 46, and a second metal frame 34. The first metal porous body layer 45 is formed in a flat plate shape by a metal porous body having a plurality of pores communicating in the surface direction, and sandwiches the anode layer together with the solid electrolyte layer, and supplies anode gas to the anode layer through the plurality of pores. The first metal frame 31 is electrically connected to the anode layer 41 via the first metal porous body layer 45 by being electrically connected at the outer periphery 48 of the first metal porous body layer 45, and supports the first metal porous body layer 45. The second metal porous body layer 46 is formed into a flat plate shape using a porous metal body, sandwiches the cathode layer 42 together with the solid electrolyte layer 43, and supplies cathode gas to the cathode layer 42 through a plurality of pores. The second metal frame 34 is electrically connected to the second metal porous body layer 46 at an outer periphery 49 of the second metal porous body layer 46, thereby being electrically connected to the cathode layer 42 via the second metal porous body layer 46 and supporting the second metal porous body layer 46.

[0107] In this way, the fuel cell (cell 10) according to this embodiment is supported on both the anode layer 41 side and the cathode layer 42 side by the first metal porous body layer 45 and the second metal porous body layer 46, which are good conductors and have gas permeability. Therefore, when the fuel cell generates power and a current flows in the surface direction, the current flows not in the anode layer 41 or the cathode layer 42, which have high electrical resistance, but mainly in the first metal porous body layer 45 and the second metal porous body layer 46, which have low electrical resistance. Therefore, the ohmic loss is reduced in the fuel cell according to this embodiment, compared to a conventional fuel cell in which a current flows in the surface direction in the anode layer 41 or the cathode layer 42 to a certain extent. Therefore, the fuel cell according to this embodiment has good power generation performance in that electricity generated by power generation can be extracted with low loss.

[0108] Furthermore, the first metal porous layer 45 and the second metal porous layer 46 do not impede the supply of anode gas to the anode layer 41 and the supply of cathode gas to the cathode layer 42. For this reason, the fuel cell (cell 10) according to this embodiment has a large active area 13. Therefore, the fuel cell according to this embodiment has good power generation performance in that it generates a large amount of power.

[0109] Furthermore, the first metal porous layer 45 and the second metal porous layer 46 are made of metal and support the basic laminate 44 consisting of the anode layer 41, the solid electrolyte layer 43, and the cathode layer 42 in a sandwiched manner, so that the fuel cell according to this embodiment has high strength. For this reason, the fuel cell according to this embodiment is less likely to develop defects such as cracks 212 even when used repeatedly accompanied by thermal expansion and contraction.

[0110] In the fuel cell (cell 10) according to this embodiment, the first metal porous layer 45 is formed so as to uniformly cover the anode layer 41, and the second metal porous layer 46 is formed so as to uniformly cover the cathode layer 42. Therefore, the active area 13 does not have any portion (opening, etc.) where the anode layer 41 and the cathode layer 42 are exposed. In other words, there is no portion where a current is forced to flow in the planar direction through the anode layer 41 or the cathode layer 42. Therefore, in the fuel cell according to this embodiment, ohmic loss is reduced over the entire surface of the active area 13. Therefore, the fuel cell according to this embodiment has good power generation performance.

[0111] In the fuel cell (cell 10) according to this embodiment, the first metal porous layer 45 and the second metal porous layer 46 have uniform electrical conductivity in the planar direction. That is, the first metal porous layer 45 and the second metal porous layer 46 each function as a substantially uniform metal plate as a whole. Therefore, even if electricity generated by power generation flows in the planar direction through the first metal porous layer 45 and the second metal porous layer 46, there is almost no ohmic loss. Therefore, the fuel cell according to this embodiment has good power generation performance.

[0112] In the fuel cell (cell 10) according to this embodiment, the first metal porous body layer 45 and the second metal porous body layer 46 are sintered bodies of metal particles. A porous metal body formed by sintering metal particles has superior electrical conductivity compared to porous metal bodies manufactured by other methods. Therefore, since the first metal porous body layer 45 and the second metal porous body layer 46 are formed of a sintered body of metal particles, the fuel cell according to this embodiment has particularly reduced ohmic loss. Therefore, the fuel cell according to this embodiment has good power generation performance.

[0113] The fuel cell stack (cell stack 100) according to this embodiment is formed using the above fuel cell (cell 10). This fuel cell stack includes a cell arrangement in which a plurality of fuel cell units are alternately stacked at a predetermined interval while being inverted so that the anode faces 22 face each other and the cathode faces 23 face each other when the surface of the fuel cell unit where the first metal porous layer 45 is exposed is the anode face 22 and the surface of the fuel cell unit where the second metal porous layer 46 is exposed is the cathode face 23. In addition, in the fuel cell stack, an anode gas flow passage FPa through which the anode gas flows is formed in a space (inter-cell space) where the anode faces 22 face each other between adjacent fuel cell units in the above cell arrangement. In addition, in the fuel cell stack, a cathode gas flow passage FPc through which the cathode gas flows is formed in a space (inter-cell space) where the cathode faces 23 face each other between adjacent fuel cell units in the above cell arrangement. In addition, the fuel cell stack includes a bus bar that electrically connects adjacent fuel cell units in the above cell arrangement.

[0114] As described above, the fuel cell stack (cell stack 100) according to this embodiment is formed using the above-mentioned fuel cell (cell 10), so that the ohmic loss in each fuel cell is small. In addition, the amount of electricity generated is large and the strength is high. Therefore, the cell stack 100 has good power generation performance.

[0115] In the fuel cell stack (cell stack 100) according to this embodiment, the bus bars 14, 15 electrically connect the first metal porous body layer 45 and the second metal porous body layer 46 between adjacent fuel cell cells in the above-mentioned cell arrangement, thereby connecting the fuel cell cells in series. Therefore, the fuel cell stack according to this embodiment has good power generation performance in that it can generate high voltage.

[0116] Furthermore, in the fuel cell stack (cell stack 100) according to this embodiment, the bus bars 14, 15 connect the first metal porous body layers and the second metal porous body layers 46 between adjacent fuel cell units in the above cell arrangement, respectively, thereby making it possible to connect the fuel cell units in parallel. Therefore, the fuel cell stack according to this embodiment has good power generation performance in that it can generate a large current.

[0117] In the fuel cell stack (cell stack 100) according to this embodiment, the height H2 of the cathode gas flow passage FPc, which is the spacing between the cathode faces 23, is greater than the height H1 of the anode gas flow passage FPa, which is the spacing between the anode faces 22. Therefore, in the fuel cell stack according to this embodiment, the pressure loss of the anode gas in the anode gas flow passage FPa and the pressure loss of the cathode gas in the cathode gas flow passage FPc are both reduced. As a result, the devices that supply the anode gas and cathode gas to the cell stack 100 consume less power.

[0118] In the fuel cell stack (cell stack 100) according to this embodiment, when the flow direction of the anode gas and cathode gas flowing in parallel or opposite directions is a first direction (Y direction) and the direction perpendicular to the first direction is a second direction (X direction), the active area 13 where power generation occurs is longer in the first direction than in the second direction. In this way, when the active area 13 is shaped to have a high aspect ratio, the distribution of the anode gas in the anode gas flow channel FPa and the distribution of the cathode gas in the cathode gas flow channel FPc are good. As a result, the fuel cell stack (cell stack 100) according to this embodiment has good power generation performance.

[0119] In the fuel cell stack (cell stack 100) according to this embodiment, the bus bars 14, 15 are attached parallel to the cell arrangement in the first direction (Y direction), and the length L2 of the bus bars 14, 15 in the first direction is equal to or greater than the length L1 of the active area 13 in the first direction. Therefore, the current density is uniform over the entire active area 13. As a result, the occurrence of local or overall heat distribution in the active area 13 is suppressed, and power is generated uniformly and efficiently using the entire surface of the active area 13.

[0120] In the fuel cell stack (cell stack 100) according to this embodiment, when the anode gas and the cathode gas flow in parallel, the bus bars 14, 15 are attached in parallel to the first direction (Y direction) with respect to the above-mentioned cell arrangement, and the length L2 of the bus bars 14, 15 along the first direction may be formed to be shorter than the length L1 of the active area 13 along the first direction. In this case, the bus bars 14, 15 are provided so as to be unevenly located on the upstream side of the anode gas and the cathode gas with respect to the active area 13. In this way, when the anode gas and the cathode gas flow in parallel, by unevenly locating the bus bars 14, 15 on the upstream side, the temperature distribution occurring in the active area 13 is corrected. As a result, the fuel cell stack according to this embodiment has good power generation performance.

[0121] Particularly in the above case, when the fuel cell is an internal reforming type, the first metal porous layer 45 is provided with a reforming catalyst that reforms the fuel in part or all of the range of the current concentration area 401 formed in the active area 13 by the presence of the busbars 14, 15. In this way, when the reforming catalyst is provided in the range of the current concentration area 401, the temperature drop due to the reforming reaction is compensated for by heat generated by the current concentration, and the temperature distribution of the fuel cell stack can be made closer to an ideal temperature distribution. This improves the power generation performance of the fuel cell stack (cell stack 100) even when the fuel cell (cell 10) is an internal reforming type.

[0122] Although the embodiments of the present invention have been described above, the configurations described in the above embodiments and the respective modified examples merely represent some of the application examples of the present invention and are not intended to limit the technical scope of the present invention. [Explanation of symbols]

[0123] 10: Cell 11: Inlet 12: Outlet 13: Active Area 14: Busbar 15: Busbar 18a: Gasket assembly 18b: Gasket assembly 31: First metal frame 32: Electrode catalyst layer 34: Second metal frame 41: Anode layer 42: Cathode layer 43: Solid electrolyte layer 45: First metal porous layer 46:Second metal porous layer 100: Cell stack

Claims

1. A fuel cell configured by stacking an anode layer, a cathode layer, and a solid electrolyte layer sandwiched between the anode layer and the cathode layer, a first metal porous body layer formed in a flat plate shape using a metal porous body having a plurality of pores communicating in a surface direction, the first metal porous body layer sandwiching the anode layer together with the solid electrolyte layer, and supplying an anode gas to the anode layer through the plurality of pores; a first metal frame that is electrically connected to the anode layer via the first metal porous body layer by being electrically connected to an outer periphery of the first metal porous body layer and that supports the first metal porous body layer; a second metal porous layer formed in a flat plate shape using the metal porous body, sandwiching the cathode layer together with the solid electrolyte layer, and supplying a cathode gas to the cathode layer through a plurality of the pores; a second metal frame that is electrically connected to the second metal porous body layer at an outer periphery of the second metal porous body layer, thereby electrically connecting to the cathode layer via the second metal porous body layer and supporting the second metal porous body layer; A fuel cell comprising:

2. The fuel cell according to claim 1 , the first metal porous layer is formed so as to uniformly cover the anode layer, The second metal porous layer is formed so as to uniformly cover the cathode layer. Fuel cell.

3. 3. The fuel cell according to claim 1 or 2, The first metal porous layer and the second metal porous layer have uniform electrical conductivity in the planar direction. Fuel cell.

4. The fuel cell according to any one of claims 1 to 3, The first metal porous layer and the second metal porous layer are sintered bodies of metal particles. Fuel cell.

5. A fuel cell stack formed using the fuel cell according to any one of claims 1 to 4, When a surface of the fuel cell where the first metal porous body layer is exposed is an anode surface and a surface of the fuel cell where the second metal porous body layer is exposed is a cathode surface, a cell array in which a plurality of the fuel cell units are stacked alternately at predetermined intervals while being inverted so that the anode surfaces face each other and the cathode surfaces face each other; an anode gas flow path formed in a space between adjacent fuel cells in the cell array where the anode surfaces face each other, and through which the anode gas flows; a cathode gas flow path formed in a space between adjacent fuel cells in the cell array where the cathode surfaces face each other, and through which the cathode gas flows; a bus bar electrically connecting adjacent fuel cell units in the cell array; A fuel cell stack comprising:

6. 6. The fuel cell stack according to claim 5, The bus bar electrically connects the first metal porous body layer and the second metal porous body layer between adjacent fuel cell cells in the cell array, thereby connecting the fuel cell cells in series.

7. 6. The fuel cell stack according to claim 5, The bus bar connects the first metal porous body layers and the second metal porous body layers between adjacent fuel cell units in the cell arrangement, thereby connecting the fuel cell units in parallel.

8. A fuel cell stack according to any one of claims 5 to 7, a height of the cathode gas flow channel, which is the distance between the cathode surfaces, is greater than a height of the anode gas flow channel, which is the distance between the anode surfaces; Fuel cell stack.

9. A fuel cell stack according to any one of claims 5 to 8, When a flow direction of the anode gas and the cathode gas flowing in parallel or opposite directions is defined as a first direction, and a direction perpendicular to the first direction is defined as a second direction, an active area in which power is generated is longer in the first direction than in the second direction. Fuel cell stack.

10. 10. The fuel cell stack of claim 9, the bus bar is attached in parallel to the cell array in the first direction; a length of the bus bar along the first direction is equal to or greater than a length of the active area along the first direction; Fuel cell stack.

11. 10. The fuel cell stack of claim 9, When the anode gas and the cathode gas flow in parallel, the bus bar is attached in parallel to the cell array in the first direction; a length of the bus bar along the first direction is shorter than a length of the active area along the first direction; The bus bar is provided on an upstream side of the anode gas and the cathode gas with respect to the active area. Fuel cell stack.

12. 12. The fuel cell stack of claim 11, the first metal porous layer is provided with a reforming catalyst for reforming fuel in a part or the whole of a range of a current concentration area formed in the active area by the presence of the bus bar; Fuel cell stack.

Citation Information

Patent Citations

  • Collected fuel cell

    JP1994060905A

  • Molten carbonate fuel battery and power generator using this battery

    JP1997259910A

  • Unit cell structure for fuel cell, and solid oxide type fuel cell using it

    JP2004303508A

  • Solid oxide fuel cell