Positive electrode active material, positive electrode containing the same, and lithium secondary battery
A lithium nickel composite oxide with controlled composition and grain size distribution addresses thermal and structural instability in lithium secondary batteries, ensuring high capacity and safety through reduced nickel disorder and enhanced particle strength.
Patent Information
- Application Number
- JP2023529104
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-11-30
- Filing Date
- 2021-11-30
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-11-30
AI Technical Summary
Lithium nickel composite metal oxides used in lithium secondary batteries suffer from poor thermal stability and structural instability due to high nickel content, leading to potential battery explosions and fires, and existing solutions do not adequately address these issues while maintaining high capacity and capacity retention.
A positive electrode active material with a specific composition and particle size distribution, represented by Li x1 [Ni a1 Co b1 Mn c11 Al c12 Zr d1 M 1 e1 ]O 2, where the large and small particle sizes have a grain size difference of less than 40 nm, and a controlled lithium content, enhances structural stability and particle strength, reducing nickel disorder.
The proposed active material achieves improved capacity characteristics and capacity retention rates, even at high temperatures, by minimizing nickel disorder and increasing particle strength, thereby enhancing battery safety and performance.
Smart Images

Figure 0007578333000001 
Figure 0007578333000002 
Figure 0007578333000003
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of priority to Korean Patent Application No. 10-2020-0164820, filed on November 30, 2020, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a positive electrode active material, and a positive electrode and a lithium secondary battery containing the same. [Background technology]
[0003] As technological development and demand for mobile devices increases, the demand for secondary batteries as an energy source is rapidly increasing. Among these secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, are becoming more common and are being used widely.
[0004] Lithium transition metal composite oxides are used as the positive electrode active material for lithium secondary batteries, and among these, the lithium cobalt composite metal oxide LiCoO2, which has a high working voltage and excellent capacity characteristics, is mainly used. However, LiCoO2 has very poor thermal properties due to the instability of its crystal structure caused by delithiation, and is also expensive, so there are limitations to its mass use as a power source in fields such as electric vehicles.
[0005] Lithium manganese composite metal oxides (LiMnO2 or LiMn2O4, etc.), lithium iron phosphate compounds (LiFePO4, etc.), and lithium nickel composite metal oxides (LiNiO2, etc.) have been developed as alternative materials to LiCoO2. Among these, research and development on lithium nickel composite metal oxides, which have a high reversible capacity of about 200mAh / g and can easily be used to create large-capacity batteries, is being actively conducted. However, LiNiO2 has poorer thermal stability than LiCoO2, and if an internal short circuit occurs due to external pressure while charging, the positive electrode active material itself decomposes, resulting in the battery exploding and catching fire.
[0006] For this reason, in order to improve on the low thermal stability of LiNiO2 while maintaining the excellent reversible capacity, nickel-cobalt-manganese-based lithium composite transition metal oxides in which part of the Ni is replaced with Mn and Co, and nickel-cobalt-aluminum-based lithium composite transition metal oxides in which part of the Ni is replaced with Mn and Al have been developed.
[0007] On the other hand, in the case of lithium transition metal composite oxides with a high nickel content, there is a problem of increased disorder of nickel in the crystal structure of the positive electrode active material, which increases the variation in the crystal structure of the positive electrode active material, weakening the strength of the particles and making them more susceptible to cracking, and there is also a problem of rock-salt structure NiO being formed on the surface of the particles due to side reactions.
[0008] Therefore, there is a need to develop a positive electrode active material that can realize a battery having a high nickel content, a low degree of nickel disorder in the crystal structure, high particle strength, and excellent capacity characteristics and capacity retention rate, even though it contains a lithium transition metal composite oxide with a high nickel content. Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention is intended to solve the above problems, and provides a positive electrode active material and a manufacturing method thereof that can realize a battery having a high nickel content, a low degree of nickel disorder in a crystal structure, high particle strength, and excellent capacity characteristics and capacity retention rate, despite including a lithium transition metal composite oxide having a high nickel content. [Means for solving the problem]
[0010] The present invention relates to a large particle size lithium transition metal oxide and an average particle size (D 50The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide each have a composition represented by the following Chemical Formula 1, and the crystal grain size is 100 nm to 150 nm, and the difference in crystal grain size between the large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide is less than 40 nm. [Chemical formula 1] Li x1 [Ni a1 Co b1 Mn c11 Al c12 Zr d1 M 1 e1 ]O2 In the above Chemical Formula 1, Said M 1 is one or more selected from B, Mg, Ca, V, Cr, Fe, Zn, Ga, Y, Nb, Mo, Ta and W, 1.0 <x1≦1.10、0.7≦a1<1、0<b1<0.3、0<c11<0.3、0.001<c12<0.05、0.001≦d1≦0.0065、0≦e1≦0.1、a1+b1+c11+c12+d1+e1=1である。
[0011] The present invention also provides a positive electrode including the positive electrode active material, and a lithium secondary battery including the positive electrode. Effect of the Invention
[0012] Although the present invention is a positive electrode active material having a high nickel content, the degree of nickel disorder in the crystal structure is low and the particle strength is high. Furthermore, when the positive electrode active material is applied to a battery, the battery has excellent capacity characteristics and capacity retention rate at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted as meanings and concepts that are consistent with the technical idea of the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to best describe his or her invention.
[0014] In this specification, the terms "comprise", "include", "comprise", "have" and the like are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, components, or combinations thereof.
[0015] In this specification, "particle" refers to a particle of a micrometer unit, which can be divided into "grains" with a crystal form of a few tens of nanometers when observed under magnification. When observed under even greater magnification, it is possible to confirm separate regions in which atoms form a lattice structure in a certain direction, which are called "crystal grains." The size of particles observed by X-ray diffraction (XRD) is defined as the size of crystal grains. The size of crystal grains can be obtained by using XRD data and the Rietveld method. Specifically, the size of crystal grains can be obtained by placing a sample in a groove in a general powder holder, cleaning the surface of the sample using a slide glass and making the height the same as the edge of the holder, and then analyzing the XRD data measured (2θ=15°~90°, Step size=0.02°, total scan time:20min) using an X-ray diffraction analyzer (Bruker, D8 Endeavor) through the Fundamental Parameter Approach built into Bruker's TOPAS program based on the Rietveld method.
[0016] In this specification, particle strength was measured by placing particles on a plate, increasing the compressive force using a Micro Compression Testing Machine (Shimadzu, MCT-W500), and measuring the force at which the particles were broken, and this was taken as the particle strength value.
[0017] The present invention will now be described in more detail.
[0018] positive electrode active material The inventors have found that, despite being a positive electrode active material with a high nickel content, the average particle size (D 50 The present invention has been completed by finding that when the large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide each have a composition represented by the following formula 1, the crystal grain size is 100 nm to 150 nm, and the difference in crystal grain size between the large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide is less than 40 nm, the degree of disorder of nickel in the crystal structure of the positive electrode active material is low, the particle strength of the positive electrode active material is high, and when applied to a battery, the capacity characteristics and capacity retention rate of the battery can be improved.
[0019] The positive electrode active material according to the present invention is a large particle size lithium transition metal oxide and an average particle size (D 50 The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide each have a composition represented by the following Chemical Formula 1, have a crystal grain size of 100 nm to 150 nm, and the difference in crystal grain size between the large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide is less than 40 nm. [Chemical formula 1] Li x1 [Ni a1 Co b1 Mn c11 Al c12 Zr d1 M 1 e1 ]O2 In the chemical formula 1, the M 1 is one or more selected from B, Mg, Ca, V, Cr, Fe, Zn, Ga, Y, Nb, Mo, Ta, and W, 1.0 < x1 ≤ 1.10, 0.7 ≤ a1 < 1, 0 < b1 < 0.3, 0 < c11 < 0.3, 0.001 < c12 < 0.05, 0.001 ≤ d1 ≤ 0.0065, 0 ≤ e1 ≤ 0.1, and a1 + b1 + c11 + c12 + d1 + e1 = 1.
[0020] The x1 means the number of moles of lithium when the total number of moles of metals (Ni, Co, Zr, M 1 ) excluding lithium contained in the large-particle-size or small-particle-size lithium transition metal oxide is 1, and 1.0 < x1 ≤ 1.10, or 1.03 ≤ x1 ≤ 1.07. When the x1 value is within the above range, Li and Ni are in a competitive relationship in the reaction occupying the Li position in the crystal structure, and by increasing the content ratio of lithium, the degree of disorder of nickel in the crystal structure can be reduced. As a result, a battery with excellent capacity characteristics and capacity retention rate can be realized. On the other hand, when the x1 value is 1.0 or less, there is a problem that the degree of disorder of nickel in the crystal structure increases as the content ratio of lithium decreases, and when the x1 value exceeds 1.10, the amount of lithium that cannot participate in the reaction increases, resulting in an increase in lithium by-products, a decrease in the initial discharge capacity, and a decrease in the initial efficiency. On the other hand, when the lithium by-products increase, there is a problem that it is difficult to control in the manufacturing process of the positive electrode active material.
[0021] The a1 means the atomic fraction of nickel among the metal elements excluding lithium in the large-particle-size or small-particle-size lithium transition metal oxide, and 0.7 ≤ a1 < 1, 0.8 ≤ a1 < 1, or 0.85 ≤ a1 ≤ 0.95. When the a1 value is 0.7 or more, specifically 0.8 or more, that is, in the case of a positive electrode active material with a high nickel content, as the content of nickel that can participate in the redox reaction increases, there is an advantage that the capacity increases.
[0022] Said b1 means the atomic fraction of cobalt among the metal elements excluding lithium in the large-particle-size or small-particle-size lithium transition metal oxide, and 0 < b1 < 0.3, 0 < b1 < 0.2 or 0 < b1 < 0.15.
[0023] Said c11 means the atomic fraction of manganese among the metal elements excluding lithium in the large-particle-size or small-particle-size lithium transition metal oxide, and 0 < c11 < 0.3, 0 < c11 < 0.2 or 0 < c11 < 0.15.
[0024] Said c12 means the atomic fraction of aluminum among the metal elements excluding lithium in the large-particle-size or small-particle-size lithium transition metal oxide, and 0.001 < c12 < 0.05, 0.005 < c12 < 0.04 or 0.01 < c12 < 0.03. When the c12 value is within the above range, there is an advantage that the thermal stability is improved and the high-temperature life characteristics are improved. In particular, when aluminum is doped with the above content together with zirconium atoms, there is an advantage that the high-temperature life characteristics are further improved.
[0025] Said d1 means the atomic fraction of zirconium among the metal elements excluding lithium in the large-particle-size or small-particle-size lithium transition metal oxide, and 0.001 ≤ d1 ≤ 0.0065 or 0.002 ≤ d1 ≤ 0.0045. When the d1 value is within the above range, zirconium is substituted at the metal site to enhance the binding force with oxygen, thereby enhancing the stability of the crystal structure, strengthening the particle strength, and increasing the high-temperature life. On the other hand, when the d1 value is less than 0.001, that is, when the content of zirconium in the lithium transition metal oxide is less than 940 ppm, the content is too low to achieve the effect of strengthening the structural stability and particle strength. And when the d1 value exceeds 0.0065, that is, when the content of zirconium in the lithium transition metal oxide exceeds 6,000 ppm, there is a problem that the number of inactivation regions in the metal site increases and the capacity decreases.
[0026] Said e1 means M among the metal elements excluding lithium in the large-particle-size or small-particle-size lithium transition metal oxide 1e1 means the atomic fraction of an element, and 0≦e1≦0.1 or 0≦e1≦0.05.
[0027] The crystal grain size of the large or small particle lithium transition metal oxide is 100 nm to 150 nm, specifically 100 nm to 140 nm, more specifically 110 nm to 130 nm. When the crystal grain size of the large or small particle lithium transition metal oxide is within the above range, there is an advantage in that the contraction and expansion of the crystal structure during charging and discharging is small, thereby improving structural stability. On the other hand, when the crystal grain size is less than 100 nm, there is a problem that the crystal structure cannot be fully developed and the degree of disorder of nickel is large, resulting in low particle strength, and when it exceeds 150 nm, there is a problem that the contraction and expansion of the active material particles (especially the primary particles) during charging and discharging is large, increasing particle cracks and deteriorating structural stability.
[0028] The difference in crystal grain size between the large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide is less than 40 nm, specifically less than 30 nm. That is, the difference in crystal grain size between the large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide is small. More specifically, the crystal grain size of the large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide is the same. In this case, excessive cracking of the small particle size lithium transition metal oxide or the large particle size lithium transition metal oxide particles during rolling can be prevented, and thus the battery life characteristics are excellent when the positive electrode active material is applied to a battery.
[0029] On the other hand, if the difference in crystal grain size between the large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide is 40 nm or more and the crystal grain size of the small particle size lithium transition metal oxide is smaller than the crystal grain size of the large particle size lithium transition metal oxide, the small particle size lithium transition metal oxide particles will crack excessively during rolling, resulting in an increase in the amount of small-sized differential generation. On the other hand, if the crystal grain size of the large particle size lithium transition metal oxide is smaller than the crystal grain size of the small particle size lithium transition metal oxide, the large particle size lithium transition metal oxide particles will crack excessively during rolling, resulting in a decrease in electrical conductivity.
[0030] In particular, the positive electrode active material according to the present invention is a positive electrode active material having a high nickel content, but the positive electrode active material contains a specific content of Zr, and the molar ratio of lithium to the total moles of transition metals contained in the positive electrode active material is greater than 1.0 and less than or equal to 1.10. The crystal grain size of the positive electrode active material is in the range of 100 nm to 150 nm, so that the degree of disorder of nickel in the crystal structure of the positive electrode active material is low, and the particle strength of the positive electrode active material is high. In addition, the degree of contraction and expansion of the primary particles of the active material exhibited during high-temperature charge and discharge is reduced. As a result, when the positive electrode active material is applied to a battery, the capacity retention rate of the battery can be improved.
[0031] According to the present invention, the average particle size (D 50 The average particle size (D) of the small particle size lithium transition metal oxide is 8 μm to 15 μm, specifically 8 μm to 13 μm. 50 The lithium transition metal oxide has an average particle size (D 50 Large-particle lithium transition metal oxides with average particle size (D 50 The weight ratio of the large particle size lithium transition metal oxide to the small particle size lithium transition metal oxide is 5:5 to 9:1, specifically 6:2 to 9:1, more specifically 7:3 to 9:1. In this case, as the rolling density increases, the high loading (20 mg / cm 2 As mentioned above, the electrodes are easy to manufacture and the cracking of particles during rolling can be reduced.
[0032] Meanwhile, a coating layer containing B, Zr, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Sr, Ba, Ce, F, P, S, and Y may be formed on the surface of the lithium transition metal oxide. Specifically, a boron coating layer containing boron may be formed on the surface of the lithium transition metal oxide.
[0033] According to the present invention, the positive electrode active material has a nickel disorder (Ni disorder) of 1.5% or less, specifically 1.4% or less, preferably 0 to 1.3%. In this case, the positive electrode active material according to the present invention can realize a battery having excellent capacity characteristics and capacity retention rate despite its high nickel content. Meanwhile, in this specification, the nickel disorder value is calculated by obtaining XRD data using an X-ray diffraction analyzer (Bruker, D8 Endeavor) and then performing atomic structure analysis using the Rietveld method to determine the Ni occupying the lithium site. 2+ Disordered Ni on the lithium sites obtained by analyzing the relative amount of ions and the relative occupancy of the oxygen sites by oxygen, respectively. 2+ The percentage of ions is indicated.
[0034] According to the present invention, the large particle size lithium transition metal oxide has a particle strength of 140 MPa to 180 MPa, specifically 145 MPa to 180 MPa, more specifically 145 MPa to 165 MPa. And, the small particle size lithium transition metal oxide has a particle strength of 110 MPa to 150 MPa, specifically 115 MPa to 145 MPa, more specifically 120 MPa to 145 MPa. In this case, cracking of primary particles during charging and discharging is reduced, improving structural stability, and a battery having improved capacity retention rate, especially at high temperatures, can be realized.
[0035] The positive electrode active material according to the present invention can be prepared by the following method. Specifically, the positive electrode active material according to the present invention is prepared by mixing a large particle size lithium transition metal oxide and a large particle size lithium transition metal oxide having an average particle size (D 50 The lithium transition metal oxide particles having a small particle diameter and a small particle diameter are mixed together to produce the lithium transition metal oxide particles.
[0036] The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide can be prepared by a method including the steps of (A) preparing a mixture by mixing a large or small particle size transition metal precursor containing nickel of 70 mol % or more based on the total moles of transition metals, an aluminum-containing raw material, a zirconium-containing raw material, and a lithium-containing raw material, and (B) preparing a large or small particle size lithium transition metal oxide by firing the mixture at a temperature of 720° C. to 780° C. In this case, the lithium-containing raw material is mixed in an amount such that the molar ratio of lithium to the total moles of transition metals contained in the large or small particle size lithium transition metal oxide to be prepared (Li / transition metal) is more than 1.0 and not more than 1.10, the zirconium-containing raw material is mixed in an amount of 940 ppm to 6,000 ppm with respect to the transition metal precursor, and the aluminum-containing raw material is mixed in an amount of 300 ppm to 13,700 ppm with respect to the transition metal precursor.
[0037] The large particle size or small particle size transition metal precursor has a composition represented by the following formula 2 or 3, respectively. [Chemical formula 2] [Ni a2 Co b2 Mn c21 Al c22 M 1 d2 ](OH)2 [Chemical formula 3] [Ni a2 Co b2 Mn c21 Al c22 M 1 d2 ]OOH In the above Chemical Formula 2 and Chemical Formula 3, Said M 1 is one or more selected from B, Mg, Ca, V, Cr, Fe, Zn, Ga, Y, Nb, Mo, Ta, and W; 0.7≦a2<1, 0 <b2<0.3、0<c21<0.3、0.001<c22<0.05、0≦d2≦0.1、a2+b2+c21+c22+d2=1である。
[0038] The a2 means the atomic fraction of nickel among the metal elements in the large-particle-size or small-particle-size transition metal precursor, and is 0.7≦a2<1, 0.8≦a2<1, or 0.85≦a2≦0.95.
[0039] The b2 represents the atomic fraction of cobalt among the metal elements in the large-particle or small-particle transition metal precursor; <b2<0.3、0<b2<0.2または0<b2<0.15である。
[0040] The c21 represents the atomic fraction of manganese element among the metal elements in the large particle size or small particle size transition metal precursor, and 0 <c21<0.3、0<c21<0.2または0<c21<0.15である。
[0041] The c22 means the atomic fraction of aluminum element among metal elements in the large particle size or small particle size transition metal precursor, and is 0.001 <c22<0.05、0.005<c22<0.04または0.01<c22<0.03である。
[0042] The d2 is M among the metal elements in the large particle size or small particle size transition metal precursor. 1 means the atomic fraction of an element, and 0≦d2≦0.1 or 0≦d2≦0.05.
[0043] The lithium-containing raw material includes at least one selected from the group consisting of lithium hydroxide hydrate, lithium carbonate, and lithium hydroxide. The lithium-containing raw material is specifically lithium hydroxide hydrate, more specifically LiOH·H2O. In this case, the reactivity of the lithium-containing raw material with a precursor having a high atomic fraction of nickel among metal elements in the precursor can be improved.
[0044] The lithium-containing raw material may be mixed in an amount that makes the molar ratio of lithium to the total number of moles of transition metals contained in the lithium transition metal oxide to be greater than 1.0 and less than 1.10 (Li / transition metal), specifically, 1.03 to 1.07. When the lithium-containing raw material is mixed in an amount that makes the molar ratio of lithium to the total number of moles of transition metals contained in the lithium transition metal oxide to be less than 1.0 (Li / transition metal), there is a problem that the degree of disorder of nickel in the crystal structure increases as the lithium content ratio decreases, and when the lithium-containing raw material is mixed in an amount that makes the amount of lithium that cannot participate in the reaction increases, and thus the initial discharge capacity of the positive electrode active material to be produced decreases, resulting in a problem that the initial efficiency decreases.
[0045] The zirconium-containing raw material may be an acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, or oxyhydroxide containing zirconium, etc. For example, when the zirconium-containing raw material is an oxide containing zirconium, it is ZrO2.
[0046] The zirconium-containing raw material is mixed with the transition metal precursor at a content of 940 ppm to 6,000 ppm, specifically 1,000 ppm to 6,000 ppm, more specifically 2,000 ppm to 4,000 ppm. If the zirconium-containing raw material is mixed with the transition metal precursor at a content of less than 940 ppm, there is a problem that the zirconium content is low and the effect of strengthening the structural stability and particle strength cannot be achieved, and if it is mixed with the transition metal precursor at a content of more than 6,000 ppm, there is a problem that the capacity is reduced due to an increase in the inactive region at the metal site.
[0047] The aluminum-containing raw material may be an aluminum-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, etc. For example, when the aluminum-containing raw material is an oxide containing aluminum, it is Al2O3.
[0048] The aluminum-containing raw material is mixed with the transition metal precursor at a content of 300 ppm to 13,700 ppm, specifically 1,400 ppm to 11,000 ppm, more specifically 2,800 ppm to 8,300 ppm. If the aluminum-containing raw material is mixed with the transition metal precursor at a content of less than 300 ppm, there is a problem that the aluminum content is low and the effect of enhancing thermal stability and structural stability cannot be achieved, and if it is mixed at a content of more than 13,700 ppm, there is a problem that the non-activated region at the metal site increases, resulting in a low capacity.
[0049] Step (B) may further include, if necessary, a step of rinsing the sintered product produced by sintering the mixture at a temperature of 720°C to 780°C in a water washing solution and then drying the sintered product. Step (B) may further include a step of mixing a coating element-containing raw material with the dried sintered product and heat-treating the mixture to form a coating layer.
[0050] The calcination is carried out at 720°C to 780°C. The calcination temperature is specifically 730°C to 770°C, more specifically 740°C to 760°C. When the calcination temperature is within the above range, crystals can be formed with an appropriate size, and the process cost may not be so high. In particular, a lithium transition metal oxide with a crystal grain size of 100nm to 150nm can be produced.
[0051] Meanwhile, the firing temperature when preparing the large particle size lithium transition metal oxide may be higher than the firing temperature when preparing the small particle size lithium transition metal oxide, thereby making it possible to prepare a positive electrode active material having a difference in crystal grain size of less than 40 nm, specifically less than 30 nm, more specifically 0 nm. Specifically, the firing temperature when preparing the large particle size lithium transition metal oxide may be about 10° C. to 50° C. higher than the firing temperature when preparing the small particle size lithium transition metal oxide.
[0052] The firing is carried out in an oxygen atmosphere, in which case a fired product having a structurally stable phase can be formed.
[0053] The water washing is a process of removing impurities such as residual lithium using a washing solution such as deionized water or distilled water, and the drying is a process of removing moisture from the positive active material containing moisture through washing with water, and may be performed by a method known in the art.
[0054] The step of forming the coating layer is a step for forming a coating layer on the surface of the lithium transition metal oxide, and can be performed by a method known in the art.
[0055] positive electrode The present invention also provides a positive electrode for a lithium secondary battery, which includes the positive electrode active material produced by the above-mentioned method.
[0056] Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector and including the positive electrode active material.
[0057] The positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and may be, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The positive electrode current collector may generally have a thickness of 3 μm to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0058] The positive electrode active material layer may include a conductive material and a binder in addition to the positive electrode active material.
[0059] The positive electrode active material may be included in an amount of 80 wt % to 99 wt %, more specifically, 85 wt % to 98 wt %, based on the total weight of the positive electrode active material layer, and excellent capacity characteristics may be exhibited when included in the above content range.
[0060] The conductive material is used to give conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing a chemical change in the battery. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and the like, and one or more of these may be used alone or in combination. The conductive material may be included in an amount of 1 wt % to 30 wt % based on the total weight of the positive electrode active material layer.
[0061] The binder serves to improve adhesion between the positive electrode active material particles and adhesion between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 wt% to 30 wt% based on the total weight of the positive electrode active material layer.
[0062] The positive electrode may be manufactured by a typical method for manufacturing a positive electrode, except for using the positive electrode active material. Specifically, the positive electrode active material and, optionally, a binder and a conductive material may be dissolved or dispersed in a solvent to prepare a composition for forming a positive electrode active material layer, which may be coated on a positive electrode current collector, and then dried and rolled. In this case, the types and contents of the positive electrode active material, binder, and conductive material are as described above.
[0063] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, taking into consideration the coating thickness of the slurry and the manufacturing yield, and to have a viscosity that allows excellent thickness uniformity when the slurry is applied to manufacture a positive electrode.
[0064] As another method, the positive electrode may be produced by casting the composition for forming a positive electrode active material layer on a separate support, peeling the composition from the support, and then laminating the resulting film on a positive electrode current collector.
[0065] Lithium secondary battery In addition, the present invention can provide an electrochemical device including the positive electrode. The electrochemical device may be a battery, a capacitor, or the like, and more specifically, a lithium secondary battery.
[0066] Specifically, the lithium secondary battery includes a positive electrode, a negative electrode facing the positive electrode, and a separator and an electrolyte interposed between the positive electrode and the negative electrode. Since the positive electrode is as described above, a detailed description thereof will be omitted, and only other components will be described in detail below.
[0067] The lithium secondary battery may optionally further include a battery container that houses an electrode assembly including the positive electrode, the negative electrode, and a separator, and a sealing member that seals the battery container.
[0068] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector.
[0069] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of typically 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, the negative electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.
[0070] The negative electrode active material layer optionally includes a binder and a conductive material in addition to the negative electrode active material.
[0071] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β(0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites and Sn-C composites, among which one or a mixture of two or more can be used. Also, a thin film of metallic lithium can be used as the negative electrode active material. Also, both low-crystalline carbon and high-crystalline carbon can be used as the carbon material. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, scaly, spherical or fibrous natural or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.
[0072] The negative electrode active material may be included in an amount of 80 wt % to 99 wt % based on the total weight of the negative electrode active material layer.
[0073] The binder is a component that aids in bonding between the conductive material, the active material, and the current collector, and may be added in an amount of 0.1% by weight to 10% by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0074] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10% by weight or less, specifically 5% by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it has conductivity without causing a chemical change in the battery, and may be, for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; conductive fibers such as carbon fibers or metal fibers; metal powders such as carbon fluoride, aluminum, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive materials such as polyphenylene derivatives.
[0075] For example, the negative electrode active material layer can be manufactured by coating a negative electrode composite prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, on a negative electrode current collector and drying the coated negative electrode composite. Alternatively, the negative electrode composite can be cast on a separate support, peeled off from the support, and the resulting film can be laminated on the negative electrode current collector.
[0076] The negative electrode active material layer may be manufactured, for example, by coating a negative electrode composite prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent on a negative electrode current collector, and then drying the coated negative electrode composite, or by casting the negative electrode composite on a separate support, peeling the negative electrode composite from the support, and laminating the resulting film on the negative electrode current collector.
[0077] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode to provide a passage for lithium ions to move. Any separator generally used in lithium secondary batteries may be used without any particular limitation. In particular, a separator having low resistance to ion movement of the electrolyte and excellent humidification ability of the electrolyte is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, or the like, may be used. In addition, a separator coated with a ceramic component or a polymer material to ensure heat resistance or mechanical strength may be used, and may be selectively used in a single layer or multilayer structure.
[0078] In addition, the electrolyte used in the present invention may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, or the like that can be used in manufacturing a lithium secondary battery, but is not limited thereto.
[0079] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0080] The organic solvent may be any solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as polycarbonate (PC), alcohol-based solvents such as ethanol and isopropyl alcohol, nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant, which can improve the charge and discharge performance of the battery, and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to about 1:9 to provide excellent electrolyte performance.
[0081] The lithium salt may be any compound capable of providing lithium ions used in lithium secondary batteries without any particular limitations. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2.LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within a range of 0.1M to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0082] In addition to the electrolyte components, the electrolyte may further include one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in battery capacity, improving the discharge capacity of the battery, etc. In this case, the additives may be included in an amount of 0.1 wt % to 5 wt % based on the total weight of the electrolyte.
[0083] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore useful in portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).
[0084] Accordingly, the present invention can provide a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.
[0085] The battery module or the battery pack can be used as a power source for one or more medium- to large-sized devices, including a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.
[0086] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, or a coin shape.
[0087] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but also as a unit battery for a medium- to large-sized battery module including a large number of battery cells.
[0088] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may, however, be embodied in several different forms and should not be construed as limited to the embodiments set forth herein.
[0089] Manufacturing Example Manufacturing Example 1 Nickel sulfate, cobalt sulfate, and manganese sulfate were mixed in deionized water in a molar ratio of 87:6:7 to prepare a metal salt aqueous solution with a concentration of 2 M. In addition, a 4 M NaOH aqueous solution and a 7% NH4OH aqueous solution were prepared.
[0090] The containers containing the metal salt aqueous solution, NaOH aqueous solution, and NH4OH aqueous solution were connected to a batch-type reactor (volume: 5 L) set at 60°C. 3 L of deionized water was added to the reactor, and nitrogen gas was purged at a rate of 2 L / min to remove dissolved oxygen in the deionized water, creating a non-oxidizing atmosphere inside the reactor. Thereafter, the NaOH aqueous solution was added and the temperature was maintained at 60°C to pH 12.0. Thereafter, the metal salt aqueous solution was added at a rate of 180 ml / hr, the NaOH aqueous solution at 180 ml / hr, and the NH4OH aqueous solution at 10 ml / hr, respectively, to carry out a coprecipitation reaction for 10 hours, and Ni was obtained with an average particle size of 10 μm. 0.87 Co 0.06 Mn 0.07 Large particle size transition metal precursors with the composition (OH)2 were prepared.
[0091] Manufacturing Example 2 The same method as in Example 1 was used to prepare Ni zeolite with an average particle size of 5 μm, except that the coprecipitation reaction time was reduced to 3 hours. 0.87 Co 0.06 Mn 0.07 Small particle size transition metal precursors with the composition (OH)2 were prepared.
[0092] Examples and Comparative Examples Example 1 (1) Manufacturing of large particle size lithium transition metal oxide A mixture was prepared by uniformly mixing the large particle size transition metal precursor prepared in Preparation Example 1, LiOH·H2O as a lithium-containing raw material, and ZrO2 and Al2O3 as doping element-containing raw materials. The LiOH·H2O was added in an amount such that the molar ratio of lithium to the total moles of transition metals contained in the large particle size lithium transition metal oxide (Li / transition metal) was 1:1.05, the ZrO2 was added in an amount of 3,000 ppm relative to the large particle size transition metal precursor, and the Al2O3 was added in an amount of 4,700 ppm relative to the large particle size transition metal precursor.
[0093] The mixture was sintered at 760°C for 16 hours in an oxygen atmosphere to produce a sintered product. The sintered product was washed with deionized water and then dried using a vacuum pump to remove moisture. The dried sintered product was mixed with 0.1% by weight of boric acid (H3BO3) and heat-treated at 400°C for 5 hours in an air atmosphere to produce a large-particle lithium transition metal oxide (average particle size: 10.0 μm, composition: Li 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 120 nm) was produced.
[0094] (2) Production of small particle size lithium transition metal oxide A small particle size lithium transition metal oxide (average particle size: 5.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in (1) of Example 1, except that the small particle size transition metal precursor prepared in Preparation Example 2 was used instead of the large particle size transition metal precursor prepared in Preparation Example 1 and the calcination temperature was adjusted to 740° C. 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 120 nm) was produced.
[0095] (3) Manufacture of positive electrode active material The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide were mixed in a weight ratio of 8:2 to prepare a positive electrode active material.
[0096] Example 2 (1) Manufacturing of large particle size lithium transition metal oxide A large-particle lithium transition metal oxide (average particle size: 10.0 μm, composition: LiOH·H2O) having a boron coating layer formed on its surface was prepared in the same manner as in Example 1(1), except that LiOH·H2O was added in an amount such that the molar ratio of lithium to the total moles of transition metal contained in the large-particle lithium transition metal oxide (Li / transition metal) was 1:1.07. 1.07 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 130 nm) was produced.
[0097] (2) Production of small particle size lithium transition metal oxide A small particle size lithium transition metal oxide (average particle size: 5.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(2), except that LiOH·H2O was added in an amount such that the mole ratio of lithium to the total moles of transition metal contained in the small particle size lithium transition metal oxide (Li / transition metal) was 1:1.07. 1.07 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 130 nm) was produced.
[0098] (3) Manufacture of positive electrode active material The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide were mixed in a weight ratio of 8:2 to prepare a positive electrode active material.
[0099] Example 3 (1) Manufacturing of large particle size lithium transition metal oxide A large-particle lithium transition metal oxide (average particle size: 10.0 μm, composition: Li) having a boron coating layer formed on its surface was prepared in the same manner as in Example 1(1), except that LiOH·H2O was added in an amount such that the mole ratio of lithium to the total moles of transition metal contained in the large-particle lithium transition metal oxide (Li / transition metal) was 1:1.03. 1.03 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 110 nm) was produced.
[0100] (2) Production of small particle size lithium transition metal oxide A small particle size lithium transition metal oxide (average particle size: 5.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(2), except that LiOH·H2O was added in an amount such that the mole ratio of lithium to the total moles of transition metal contained in the small particle size lithium transition metal oxide (Li / transition metal) was 1:1.03. 1.03 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 110 nm) was produced.
[0101] (3) Manufacture of positive electrode active material The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide were mixed in a weight ratio of 8:2 to prepare a positive electrode active material.
[0102] Comparative Example 1 (1) Manufacturing of large particle size lithium transition metal oxide A large particle size lithium transition metal oxide (average particle size: 10.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(1), except that ZrO was added at a content of 500 ppm to the large particle size transition metal precursor. 1.05 (Ni 0.87 Co0.06 Mn 0.07 ) 0.9825 Zr 0.00053 Al 0.017 O2, grain size: 120 nm) was produced.
[0103] (2) Production of small particle size lithium transition metal oxide A small particle size lithium transition metal oxide (average particle size: 5.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(2) except that ZrO2 was added at a content of 500 ppm to the small particle size transition metal precursor. 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.9825 Zr 0.00053 Al 0.017 O2, grain size: 120 nm) was produced.
[0104] (3) Manufacture of positive electrode active material The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide were mixed in a weight ratio of 8:2 to prepare a positive electrode active material.
[0105] Comparative Example 2 (1) Manufacturing of large particle size lithium transition metal oxide A large particle size lithium transition metal oxide (average particle size: 10.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(1) except that ZrO2 was added at a content of 7,500 ppm to the large particle size transition metal precursor. 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.975 Zr 0.0081 Al 0.017 O2, grain size: 120 nm) was produced.
[0106] (2) Production of small particle size lithium transition metal oxide A small particle size lithium transition metal oxide (average particle size: 5.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(2), except that ZrO2 was added at a content of 7,500 ppm to the small particle size transition metal precursor. 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.975 Zr 0.0081 Al 0.017 O2, grain size: 120 nm) was produced.
[0107] (3) Manufacture of positive electrode active material The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide were mixed in a weight ratio of 8:2 to prepare a positive electrode active material.
[0108] Comparative Example 3 (1) Manufacturing of large particle size lithium transition metal oxide A large particle size lithium transition metal oxide (average particle size: 10.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(1), except that LiOH·H2O was added in an amount such that the molar ratio of lithium to the total moles of transition metal contained in the large particle size lithium transition metal oxide (Li / transition metal) was 1:1.0 and the firing temperature was adjusted to 770°C. 1.0 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 120 nm) was produced.
[0109] (2) Production of small particle size lithium transition metal oxide A small particle size lithium transition metal oxide (average particle size: 5.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(2), except that LiOH·H2O was added in an amount such that the molar ratio of lithium to the total moles of transition metal contained in the small particle size lithium transition metal oxide (Li / transition metal) was 1:1.0 and the firing temperature was adjusted to 750°C.1.0 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 120 nm) was produced.
[0110] (3) Manufacture of positive electrode active material The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide were mixed in a weight ratio of 8:2 to prepare a positive electrode active material.
[0111] Comparative Example 4 (1) Manufacturing of large particle size lithium transition metal oxide A large particle size lithium transition metal oxide (average particle size: 10.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(1), except that LiOH·H2O was added in an amount such that the molar ratio of lithium to the total moles of transition metal contained in the large particle size lithium transition metal oxide (Li / transition metal) was 1:1.11 and the firing temperature was adjusted to 740°C. 1.11 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 120 nm) was produced.
[0112] (2) Production of small particle size lithium transition metal oxide A small particle size lithium transition metal oxide (average particle size: 5.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(2), except that LiOH·H2O was added in an amount such that the molar ratio of lithium to the total moles of transition metal contained in the small particle size lithium transition metal oxide (Li / transition metal) was 1:1.11 and the firing temperature was adjusted to 720°C. 1.11 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017O2, grain size: 120 nm) was produced.
[0113] (3) Manufacture of positive electrode active material The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide were mixed in a weight ratio of 8:2 to prepare a positive electrode active material.
[0114] Comparative Example 5 (1) Manufacturing of large particle size lithium transition metal oxide A large-grained lithium transition metal oxide (average grain size: 10.0 μm, composition: Li) having a boron coating layer formed on its surface was prepared in the same manner as in Example 1(1) except that the baking temperature was adjusted to 730° C. 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 90 nm) was produced.
[0115] (2) Production of small particle size lithium transition metal oxide A small particle size lithium transition metal oxide (average particle size: 5.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(2) except that the baking temperature was adjusted to 710° C. 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 90 nm) was produced.
[0116] (3) Manufacture of positive electrode active material The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide were mixed in a weight ratio of 8:2 to prepare a positive electrode active material.
[0117] Comparative Example 6 (1) Manufacturing of large particle size lithium transition metal oxide A large-grained lithium transition metal oxide (average grain size: 10.0 μm, composition: Li) having a boron coating layer formed on its surface was prepared in the same manner as in Example 1(1) except that the firing temperature was adjusted to 790° C. 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 160 nm) was produced.
[0118] (2) Production of small particle size lithium transition metal oxide A small particle size lithium transition metal oxide (average particle size: 5.0 μm, composition: Li 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 160 nm) was produced.
[0119] (3) Manufacture of positive electrode active material The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide were mixed in a weight ratio of 8:2 to prepare a positive electrode active material.
[0120] Comparative Example 7 The large particle size lithium transition metal oxide (average particle size: 10.0 μm, composition: Li 1.07 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, crystal grain size: 130 nm) and the small-grained lithium transition metal oxide (average grain size: 5.0 μm, composition: Li 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.003 Al 0.017O2, crystal grain size: 90 nm) in a weight ratio of 8:2 to prepare a positive electrode active material.
[0121] Comparative Example 8 The large particle size lithium transition metal oxide (average particle size: 10.0 μm, composition: Li 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.003 Al 0.017 O2, crystal grain size: 90 nm) and the small-grained lithium transition metal oxide (average grain size: 5.0 μm, composition: Li 1.07 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, crystal grain size: 130 nm) in a weight ratio of 8:2 to prepare a positive electrode active material.
[0122] Comparative Example 9 (1) Manufacturing of large particle size lithium transition metal oxide A large particle size lithium transition metal oxide (average particle size: 10.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(1), except that Al2O3 was added at a content of 280 ppm relative to the large particle size transition metal precursor. 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.9958 Zr 0.0032 Al 0.001 O2, grain size: 120 nm) was produced.
[0123] (2) Production of small particle size lithium transition metal oxide A small particle size lithium transition metal oxide (average particle size: 5.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(2), except that Al2O3 was added at a content of 280 ppm relative to the small particle size transition metal precursor. 1.05 (Ni 0.87 Co 0.06Mn 0.07 ) 0.9958 Zr 0.0032 Al 0.001 O2, grain size: 120 nm) was produced.
[0124] (3) Manufacture of positive electrode active material The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide were mixed in a weight ratio of 8:2 to prepare a positive electrode active material.
[0125] Comparative Example 10 (1) Manufacturing of large particle size lithium transition metal oxide A large particle size lithium transition metal oxide (average particle size: 10.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(1), except that Al2O3 was added at a content of 13,700 ppm relative to the large particle size transition metal precursor. 1.05 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.9469 Zr 0.0032 Al 0.05 O2, grain size: 120 nm) was produced.
[0126] (2) Production of small particle size lithium transition metal oxide A small particle size lithium transition metal oxide (average particle size: 5.0 μm, composition: Li) having a boron coating layer formed on the surface was prepared in the same manner as in Example 1(2) except that Al2O3 was added at a content of 13,700 ppm relative to the small particle size transition metal precursor. 1.0 (Ni 0.87 Co 0.06 Mn 0.07 ) 0.98 Zr 0.0032 Al 0.017 O2, grain size: 120 nm) was produced.
[0127] (3) Manufacture of positive electrode active material The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide were mixed in a weight ratio of 8:2 to prepare a positive electrode active material.
[0128] Experimental Example Experimental example 1: Evaluation of nickel disorder (Ni disorder) The positive electrode active materials prepared in Examples 1 to 3 and Comparative Examples 1 to 10 were each subjected to XRD data acquisition using an X-ray diffraction analyzer (Bruker, D8 Endeavor), and then subjected to atomic structure analysis using the Rietveld method to determine Ni occupying the lithium site. 2+ The disordered Ni at the lithium site obtained by analyzing the relative amount of ions and the relative occupancy of the oxygen sites by oxygen, respectively. 2+ The amount of ions (%) was taken as the nickel disorder value and is shown in Table 1 below.
[0129] Experimental example 2: Particle strength evaluation The large particle size lithium transition metal oxide particles and the small particle size lithium transition metal oxide particles prepared in Examples 1 to 3 and Comparative Examples 1 to 10 were subjected to increasing compression force using a Micro Compression Testing Machine (Shimadzu, MCT-W500) to measure the force at which the particles break. The particle strength values are shown in Table 1 below.
[0130] [Table 1]
[0131] Experimental Example 3: Half-cell Characterization Coin-type half batteries were manufactured using the positive electrode active materials prepared in Examples 1 to 3 and Comparative Examples 1 to 10, and the initial charge capacity, initial discharge capacity, and capacity retention rate of each battery were evaluated.
[0132] Specifically, the positive electrode active materials prepared in Examples 1 to 3 and Comparative Examples 1 to 10 were mixed with carbon black conductive material and PVdF binder in a weight ratio of 97.5:1.0:1.5 in NMP solvent to prepare positive electrode slurries. The positive electrode slurries were applied to one side of an aluminum current collector, dried at 130°C, and rolled to prepare positive electrodes. Meanwhile, Li metal disks were used as negative electrode active materials. An electrode assembly was prepared by interposing a separator between the positive electrode and the Li metal disk negative electrode prepared as above, and the assembly was placed inside a battery case, and an electrolyte was injected into the case to prepare a coin-type half cell. In this case, an electrolyte prepared by dissolving 1M LiPF6 in an organic solvent of EC / EMC / DEC (3 / 3 / 4, vol%) was used as the electrolyte.
[0133] The battery prepared as above was charged at 25° C. at a constant current of 0.1 C until the voltage reached 4.25 V, and then charged at a constant voltage (CV) until the charging current reached 0.05 mAh, and then discharged at a constant current of 0.1 C until the voltage reached 3.0 V. The initial charge capacity and initial discharge capacity are shown in Table 2.
[0134] In addition, the charge / discharge cycle was repeated 50 times at 45°C and a constant current of 1C in the range of 3.0 to 4.25V to measure the discharge capacity of the lithium secondary battery. In particular, the ratio of the 50th cycle discharge capacity to the 1st cycle discharge capacity was defined as the capacity retention rate, which is shown in Table 2 below.
[0135] [Table 2]
[0136] Referring to Tables 1 and 2, it can be seen that the positive electrode active material according to the present invention has a low degree of nickel disorder in a crystal structure and high particle strength, and also has excellent capacity characteristics and capacity retention rate at high temperatures when the positive electrode active material is applied to a battery.
[0137] In contrast, it can be seen that the positive electrode active material of Comparative Example 1, which has a small Zr atomic fraction, has a low doping content and low particle strength, and the positive electrode active material of Comparative Example 2, which has a large Zr atomic fraction, has a problem of increasing the inactive region of the metal site and low initial charge / discharge capacity. It can also be seen that the positive electrode active material of Comparative Example 3, which has a Li / Me ratio of 1.0, has a problem of high Ni disorder, and the positive electrode active material of Comparative Example 4, which has a Li / Me ratio of 1.11, has a problem of increasing lithium by-products, making process control difficult, and low initial discharge capacity. It can also be seen that the positive electrode active material of Comparative Example 5, which has a crystal grain size of 90 nm, has insufficient crystal growth, high Ni disorder, and low particle strength, and the positive electrode active material of Comparative Example 6, which has a crystal grain size of 160 nm, has a problem of excessive shrinkage and expansion of primary particles during charging and discharging, increasing particle cracking. In the case of the positive electrode active material of Comparative Example 7, in which the difference in the size of the crystal grains between the large-particle-size lithium transition metal oxide and the small-particle-size lithium transition metal oxide is 40 nm or more and the size of the crystal grains of the small-particle-size lithium transition metal oxide is smaller than the size of the crystal grains of the large-particle-size lithium transition metal oxide, it can be confirmed that the amount of differential generation of small sizes increases and the capacity retention rate is low. In the case of the positive electrode active material of Comparative Example 8, in which the difference in the size of the crystal grains between the large-particle-size lithium transition metal oxide and the small-particle-size lithium transition metal oxide is 40 nm or more and the size of the crystal grains of the large-particle-size lithium transition metal oxide is smaller than the size of the crystal grains of the small-particle-size lithium transition metal oxide, it can be confirmed that the large-particle-size lithium transition metal oxide particles are excessively cracked, the conductivity is reduced, and the capacity retention rate is low. In the case of Comparative Example 9, in which the amount of aluminum doping is low, the driving stability is reduced, and the capacity retention rate is low. In the case of Comparative Example 10, in which the amount of aluminum doping is high, the inactive region of the metal site is increased, and the initial charge / discharge capacity is reduced.
[0138] Experimental Example 4: Differential Scanning Calorimetry (DSC) Evaluation Among the coin-type half-cells prepared in Experimental Example 3, the coin-type half-cells prepared using the positive electrode active materials of Example 1 and Comparative Example 9 were evaluated by a differential scanning calorimeter (DSC).
[0139] Specifically, a coin cell (CHC) was charged to 4.25V (SOC 100%) using a Setaram HP-DSC device. Specifically, the coin cell was charged to 4.25V at 0.1C constant current at 25°C, and then charged at a constant voltage until the charging current was 0.05nAh. It was then discharged at 0.1C constant current until the voltage reached 3.0V. It was also charged at 0.1C constant current until the voltage reached 4.25V, and then charged at a constant voltage until the charging current was 0.05nAh. After this, the electrodes were disassembled and washed with dimethyl carbonate (DMC), and the electrodes were punched out to a diameter of 5mm, and 20μl of electrolyte was injected into the high-pressure PAN. The temperature was raised from room temperature to 400°C at a rate of 10°C / min, and the temperature at which heat generation began was measured.
[0140] [Table 3]
[0141] As can be seen from the results of Tables 2 and 3, in the case of Comparative Example 9 in which the atomic fraction of Al is small, the capacity is increased but there is a problem that the capacity retention rate and the DSC thermal safety are decreased, and in the case of Comparative Example 10 in which the atomic fraction of Al is large, the capacity retention rate and the DSC thermal safety are improved but there is a problem that the capacity is significantly decreased.
Claims
1. The large particle size lithium transition metal oxide and the average particle size (D 50 ) small particle size lithium transition metal oxide, The large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide each have a composition represented by the following formula 1, and have a crystal grain size of 100 nm to 150 nm, the difference in crystal grain size between the large-grain lithium transition metal oxide and the small-grain lithium transition metal oxide is less than 40 nm; The nickel disorder is 1.5% or less; [Chemical formula 1] Li x1 [Ni a1 Co b1 Mn c11 Al c12 Zr d1 M 2 e1 ]O 2 In the above Chemical Formula 1, Said M 2 is one or more selected from B, Mg, Ca, V, Cr, Fe, Zn, Ga, Y, Nb, Mo, Ta and W; A positive electrode active material, wherein 1.03≦x1≦1.07, 0.7≦a1<1, 0<b1<0.3, 0<c11<0.3, 0.001<c12<0.05, 0.001≦d1≦0.0065, 0≦e1≦0.1, and a1+b1+c11+c12+d1+e1=1.
2. The positive electrode active material according to claim 1 , wherein a1 satisfies 0.8≦a1<1.
3. The positive electrode active material according to claim 1 , wherein d1 satisfies the condition 0.002≦d1≦0.0045.
4. 2 . The positive electrode active material of claim 1 , wherein the large particle size lithium transition metal oxide and the small particle size lithium transition metal oxide each independently have a crystal grain size of 100 nm to 140 nm.
5. 2. The positive electrode active material of claim 1, wherein the large particle size lithium transition metal oxide has a particle strength of 140 MPa to 180 MPa.
6. 2. The positive electrode active material of claim 1, wherein the small particle size lithium transition metal oxide has a particle strength of 110 MPa to 150 MPa.
7. The average particle size (D 50 2. The positive electrode active material according to claim 1, wherein the thickness of the first electrode is 8 μm to 15 μm.
8. The average particle size (D 50 2. The positive electrode active material according to claim 1, wherein the average particle diameter is 3 μm to 7 μm.
9. 2. The positive electrode active material of claim 1, wherein a weight ratio of the large particle size lithium transition metal oxide to the small particle size lithium transition metal oxide is 5:5 to 9:
1.
10. A positive electrode comprising the positive electrode active material according to claim 1 .
11. A lithium secondary battery comprising the positive electrode according to claim 10.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery positive electrode active material and method for producing same, and nonaqueous electrolyte secondary battery which uses positive electrode active material
CN111295787A
Positive electrode active material, its manufacturing method, and lithium secondary battery including the same
JP2020514972A
Positive electrode active substance for non-aqueous electrolyte secondary cell, and non-aqueous electrolyte secondary cell
WO2020003642A1