Friction material for disc brake pads and manufacturing method thereof

A friction material for disc brake pads with a scorched black skin surface layer addresses stability and fade resistance issues, enhancing performance and reducing environmental impact by eliminating the need for surface polishing.

JP7578437B2Active Publication Date: 2024-11-06AKEBONO BRAKE IND CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020144600
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-28
Publication Date
2024-11-06
Estimated Expiration
2040-08-28

AI Technical Summary

Technical Problem

Conventional friction materials for disc brake pads face issues with effectiveness stability and fade resistance, and the manufacturing process generates abrasive powder leading to environmental pollution.

Method used

A friction material for disc brake pads is produced with a scorched black skin surface layer, omitting the surface polishing process, using a mixture of friction modifiers, fiber base materials, and binders, and incorporating a scorch treatment to enhance stability and fade resistance.

Benefits of technology

The friction material exhibits excellent effectiveness stability and fade resistance without the need for surface polishing, reducing labor and environmental contamination from abrasive powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578437000001
    Figure 0007578437000001
  • Figure 0007578437000002
    Figure 0007578437000002
  • Figure 0007578437000003
    Figure 0007578437000003
Patent Text Reader

Abstract

To provide a friction material for disc brake pads that has satisfactory stable effect and fading resistance even when a surface polishing process is not performed during production.SOLUTION: A friction material for disc brake pads contains a friction modifier, a fiber substrate and a binder, the friction material having a mill scale face on its surface, and having a layer in which the mill scale face has been scorched.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a friction material for disc brake pads used in automobiles, railway vehicles, industrial machines, etc., and a method for producing the same. [Background technology]

[0002] Conventionally, when manufacturing friction materials, surface polishing is performed in order to maintain the flatness of the friction material, etc. However, the surface polishing generates polishing powder, which requires labor to dispose of and causes environmental pollution.

[0003] In view of this, as a method for producing a friction material without performing a surface polishing treatment, Patent Document 1 discloses a method for producing a friction material that can omit the polishing step, in which a powdered friction material molding material is charged into a molding die, and then molded by applying ultrasonic vibrations while a static mold clamping force is applied, followed by a short heat treatment.

[0004] Patent Document 2 also describes a process for preparing a friction member composition that contains base fibers with a fiber diameter of 50 μm or less, an organic material such as a resin binder and rubber, and an inorganic filler with a particle diameter of 50 μm or less, and in which the organic material that becomes fluid during molding is 20 to 30 vol % when the total volume of the obtained friction member is taken as 100 vol %, and the obtained friction member composition is compressed in a mold at a pressure of 200 to 400 kg / cm 2 This publication discloses a method for producing a non-abrasive molded friction member, which is characterized by sequentially carrying out a molding step of producing a molded body by heating and molding while applying a pressure of 1000 g / m², and a heat treatment step of heating the obtained molded body. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 58-203010 [Patent Document 2] Japanese Patent Application Publication No. 63-069833 Summary of the Invention [Problem to be solved by the invention]

[0006] However, according to the investigations of the present inventors, there is a problem in that the friction material obtained by the method described in Patent Document 1 or the method described in Patent Document 2 may have deteriorated friction stability and fade resistance.

[0007] The present invention has been made in consideration of the above-mentioned conventional situation, and an object of the present invention is to provide a friction material for disc brake pads that has excellent effectiveness stability and fade resistance even without a surface polishing treatment step during production. [Means for solving the problem]

[0008] As a result of extensive investigations, the present inventors have found that the above problems can be solved by incorporating a layer in which the black surface is scorched into the friction material, and have thus completed the present invention.

[0009] That is, the present invention provides the following <1> ~ <2> This is regarding. <1> A friction material for a disc brake pad, comprising a friction modifier, a fiber base material, and a binder, It has a black surface, The black surface has a layer subjected to a scorch treatment. Friction material for disc brake pads. <2> A method for producing a friction material for a disc brake pad, the friction material comprising a friction modifier, a fiber base material, and a binder as raw materials, comprising: mixing the raw materials to obtain a raw material mixture; A step of pressurizing the raw material mixture to obtain a preform; a step of hot-pressing and molding the preform to obtain a hot-pressed molded body; a step of heat-treating the hot-pressed molded body to obtain a heat-treated molded body; and a step of scorching the heat-treated molded body without surface polishing to obtain a scorched layer. A method for manufacturing friction material for disc brake pads. Effect of the Invention

[0010] The friction material for disc brake pads of the present invention has excellent effectiveness stability and fade resistance. In addition, since the friction material for disc brake pads of the present invention does not require a surface polishing process during production, problems such as the labor required for processing polishing powder and the progression of environmental pollution can be prevented. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below, however, these are examples of preferred embodiments and the present invention is not limited to the contents thereof.

[0012] [Friction material for disc brake pads] The friction material for disc brake pads of the present invention contains a friction modifier, a fibrous base material and a binder.

[0013] <Friction adjustment material> Friction modifiers are used to impart desired friction characteristics, such as wear resistance, heat resistance, and fade resistance, to the friction material.

[0014] Examples of friction modifiers include inorganic fillers, organic fillers, abrasives, lubricants, and metal powders.

[0015] Examples of inorganic fillers include titanates such as potassium titanate, lithium titanate, lithium potassium titanate, sodium titanate, calcium titanate, magnesium titanate, and magnesium potassium titanate, as well as inorganic materials such as barium sulfate, calcium carbonate, calcium hydroxide, vermiculite, and mica. These may be used alone or in combination of two or more.

[0016] The inorganic filler is preferably used in an amount of 5 to 60 mass %, more preferably 10 to 55 mass %, based on the entire friction material.

[0017] Examples of organic fillers include various rubber powders (raw rubber powder, tire powder, etc.), rubber dust, resin dust, cashew dust, tire tread, melamine dust, etc. These may be used alone or in combination of two or more.

[0018] The organic filler is preferably used in an amount of 1 to 20 mass %, more preferably 3 to 15 mass %, based on the entire friction material.

[0019] Examples of the abrasive include zirconium oxide, alumina, silica, magnesium oxide, zirconia, zirconium silicate, chromium oxide, iron oxide trioxide (Fe3O4), chromite, etc. These may be used alone or in combination of two or more.

[0020] The abrasive is preferably used in an amount of 1 to 30 mass %, more preferably 5 to 25 mass %, of the entire friction material.

[0021] Examples of lubricants include graphite, coke, antimony trisulfide, molybdenum disulfide, tin sulfide, polytetrafluoroethylene (PTFE), etc. These may be used alone or in combination of two or more.

[0022] The lubricant is preferably used in an amount of 3 to 40 mass %, more preferably 5 to 30 mass %, based on the total mass of the friction material.

[0023] Examples of the metal powder include aluminum, tin, zinc, copper, etc. These may be used alone or in combination of two or more.

[0024] The metal powder is preferably used in an amount of 1 to 10 mass %, more preferably 1 to 7 mass %, based on the entire friction material.

[0025] From the viewpoint of imparting the above-mentioned desired friction characteristics to the friction material sufficiently, the friction modifier is used in an amount of preferably 60 to 90 mass %, and more preferably 70 to 90 mass %, of the entire friction material.

[0026] <Fiber base material> As the fibrous substrate, various commonly used fibrous substrates can be used, specifically, organic fibers, inorganic fibers, and metal fibers.

[0027] Examples of organic fibers include aromatic polyamide (aramid) fibers, flame-resistant acrylic fibers, etc. These may be used alone or in combination of two or more.

[0028] Examples of inorganic fibers include biosoluble inorganic fibers, ceramic fibers, glass fibers, carbon fibers, rock wool, etc. Examples of biosoluble inorganic fibers include biosoluble ceramic fibers such as SiO2-CaO-MgO fibers, SiO2-CaO-MgO-Al2O3 fibers, and SiO2-MgO-SrO fibers, and biosoluble rock wool, etc. These may be used alone or in combination of two or more.

[0029] Examples of metal fibers include steel fibers, iron fibers, brass fibers, etc. These may be used alone or in combination of two or more.

[0030] In order to ensure sufficient strength of the friction material, the fibrous base material is preferably used in an amount of 3 to 30 mass %, more preferably 5 to 20 mass %, of the entire friction material.

[0031] <Binding material> As the binder, various binders that are commonly used can be used, specifically, phenolic resins, various modified phenolic resins such as elastomers, melamine resins, epoxy resins, polyimide resins, and other thermosetting resins.

[0032] Examples of elastomer-modified phenolic resins include acrylic rubber-modified phenolic resins, silicone rubber-modified phenolic resins, nitrile rubber (NBR)-modified phenolic resins, etc. These may be used alone or in combination of two or more.

[0033] From the viewpoint of ensuring the mechanical strength of the friction material, the binder is used in an amount of preferably 1 to 20 mass %, more preferably 3 to 15 mass %, and even more preferably 5 to 12 mass % of the entire friction material.

[0034] When the friction material for disc brake pads of the present invention contains an organic filler, the total content of the organic filler and binder in the entire friction material is preferably 5 to 25 mass %, more preferably 6 to 23 mass %, from the viewpoints of effectiveness stability and fade resistance.

[0035] <Black surface> The friction material for disc brake pads of the present invention has a black surface on its surface. The black surface refers to a black surface formed on the surface of a heat-treated molded body described below, and is formed when a phenolic resin or the like seeps out onto the surface of the heat-pressure molded body due to the pressure and heat during heat-pressure molding and turns black by the heat treatment.

[0036] The friction material for disc brake pads of the present invention has a black surface, and therefore the surface of the friction material has a high organic component content.

[0037] <Scorch treatment layer> The friction material for disc brake pads of the present invention also has a layer (scorched layer) obtained by scorching the black surface. Specific conditions for the scorch treatment will be described later.

[0038] The friction material for disc brake pads of the present invention has a scorch treatment layer on the black surface, which increases the amount of organic components on the black surface, making it easier to achieve the effects of the scorch treatment with less energy, and therefore capable of exhibiting excellent effectiveness stability and fade resistance.

[0039] The presence of the black surface and the scorched layer can be confirmed by visual inspection or by observing the cross section of the friction material with an optical microscope.

[0040] [Method of manufacturing friction material for disc brake pads] The method for producing the friction material for disc brake pads of the present invention, which contains a friction modifier, a fiber base material, and a binder as raw materials, comprises the steps of: mixing the raw materials to obtain a raw material mixture; A step of pressurizing the raw material mixture to obtain a preform; a step of hot-pressing and molding the preform to obtain a hot-pressed molded body; a step of heat-treating the hot-pressed molded body to obtain a heat-treated molded body; and a step of scorching the heat-treated molded body without surface polishing to obtain a scorched layer.

[0041] <Step of mixing raw materials to obtain a raw material mixture> In the method for producing a friction material for a disc brake pad of the present invention, first, the raw materials (friction modifier, fibrous base material, and binder) are mixed together.

[0042] The method for mixing the raw materials is not particularly limited and any known method can be used as long as the raw materials are mixed uniformly. The raw material mixture is obtained by mixing the raw materials using a mixer or the like for, for example, 1 to 15 minutes, preferably 3 to 10 minutes.

[0043] <Step of pressure molding the raw material mixture to obtain a preform> The method for pressure molding the raw material mixture is not particularly limited, and any known method can be used. For example, the preform can be obtained by putting the raw material mixture into a mold and pressure molding it.

[0044] The pressure molding may be performed under a pressure condition of, for example, 10 to 100 MPa for, for example, 1 to 30 seconds. In the step of obtaining the preform, it is not necessary to heat the mold, and the pressure molding may be performed at room temperature (about 15°C to 25°C).

[0045] <Step of hot-pressing and molding the preform to obtain a hot-pressed molded body> The method for hot-press molding the preform is not particularly limited, and any known method can be used. For example, the hot-press molded product can be obtained by putting the preform and a pressure plate into a thermoforming mold and hot-press molding the preform.

[0046] The hot pressing may be carried out at a temperature of, for example, 130 to 180° C., preferably 140 to 170° C., and at a pressure of, for example, 30 to 80 MPa, preferably 40 to 70 MPa, for example, for 2 to 10 minutes, preferably 3 to 8 minutes.

[0047] The pressure plate may be formed into a predetermined shape by a sheet metal press, degreased, chemically treated, primed, etc., and coated with an adhesive.

[0048] <Step of heat treating the hot-pressed molded body to obtain a heat-treated molded body> The heat treatment method of the hot-pressed molded product is not particularly limited, and a known method can be used. The heat-treated molded product can be obtained by heat-treating the hot-pressed molded product at a temperature of, for example, 150 to 350°C, preferably 200 to 300°C, for example, for 1 to 5 hours, preferably 2 to 4 hours.

[0049] In the present invention, a black surface is formed on the surface of the heat-treated molded body by heat treatment of the hot-pressed molded body.

[0050] <Step of obtaining a scorched layer by subjecting a heat-treated molded body to a scorch treatment without surface polishing treatment> In the present invention, the heat-treated molded body is not subjected to a surface polishing treatment, which eliminates the need to dispose of the polishing powder generated by the surface polishing treatment and prevents the polishing powder from polluting the natural environment.

[0051] The method for scorching the heat-treated molded body is not particularly limited, and any known method can be used. The scorch-treated layer is obtained by baking the surface of a heat-treated molded body having a black surface at a temperature of, for example, 400 to 800° C. for, for example, 30 to 300 seconds.

[0052] Furthermore, the method for producing a friction material for disc brake pads of the present invention may include a surface polishing step for removing burrs and a finishing step such as painting, after the step of obtaining the scorched layer. EXAMPLES

[0053] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples in any way.

[0054] {Test Example 1} [Example 1] [Manufacturing of friction material for disc brake pads] <Preparation of raw material mixture> A raw material mixture was prepared by mixing the raw materials having the composition shown in Table 1 in a mixer (conditions: 6 minutes).

[0055] <Preparation of preform> The raw material mixture was poured into a mold and pressure-molded (conditions: 15 MPa, 10 seconds) to produce a preform.

[0056] <Preparation of hot-pressed molded body> The preform was placed in a thermoforming mold, and a metal plate (pressure plate) to which an adhesive had been applied was placed on top of it, followed by hot-press molding (conditions: 150° C., 35.0 MPa, 5 minutes) to produce a hot-press molded body.

[0057] <Preparation of heat-treated molded body> The hot-pressed molded body was heat-treated (conditions: 250° C., 3 hours) to produce a heat-treated molded body.

[0058] <Preparation of scorched layer> The surface of the heat-treated molded body was subjected to a scorch treatment (conditions: 650° C., 120 seconds) to form a scorched treatment layer, which was then finished by painting to produce a friction material.

[0059] [Evaluation of friction materials for disc brake pads] <Efficacy Stability> A friction performance test was conducted in accordance with JASO C406. Specifically, the maximum value (Maxμ) and minimum value (Minμ) of the friction coefficient of the obtained friction material were measured using a brake dynamometer before the friction material was checked for friction before being rubbed together, and the value of Maxμ-Minμ (E value) was calculated and evaluated based on the following criteria. The results are shown in Table 1.

[0060] ○: 0.00<“difference in E value”≦0.02. △: -0.04<“difference in E value”≦0.00. ×: "Difference in E value" was ≦-0.04. Here, "difference in E value" means "E value of Reference Example 1 - E value of Example 1" and "E value of Reference Example 1 - E value of Comparative Example 1."

[0061] <Fade resistance> A friction performance test was conducted in accordance with JASO C406. Specifically, the minimum friction coefficient (μ) of the obtained friction material at the first fade was measured using a brake dynamometer, and the results were evaluated based on the following criteria. The results are shown in Table 1.

[0062] ◯: The minimum friction coefficient μ was ≧0.22. ×: The minimum friction coefficient μ was <0.22.

[0063] <Appearance> The obtained friction materials were checked for the presence or absence of cracks or blisters. Cases where no cracks or blisters were found were marked with "○", and cases where cracks or blisters were found were marked with "×". The results are shown in Table 1.

[0064] The obtained friction materials were checked for the presence or absence of a black surface. The cases where a black surface was confirmed on the surface were marked with "○", and the cases where a black surface was not confirmed on the surface were marked with "×". The results are shown in Table 1.

[0065] [Comparative Example 1, Reference Example 1] The friction material was produced and evaluated in the same manner as in Example 1, except that the blending composition of the raw materials and the production conditions of the friction material were as shown in Table 1. The results are shown in Table 1. In Table 1, "surface polishing treatment performed" means that the heat-treated molded body before the scorch treatment was subjected to surface polishing treatment. The same applies to Tables 2 and 3.

[0066] [Table 1]

[0067] {Test Example 2} [Example 2, Comparative Example 2, Reference Example 2] The friction materials were produced and evaluated in the same manner as in Test Example 1, except that the blending composition of the raw materials and the production conditions of the friction materials were as shown in Table 2. The results are shown in Table 2.

[0068] [Table 2]

[0069] {Test Example 3} [Example 3, Comparative Example 3, Reference Example 3] The friction materials were produced and evaluated in the same manner as in Test Example 1, except that the blending composition of the raw materials and the production conditions of the friction materials were as shown in Table 3. The results are shown in Table 3.

[0070] [Table 3]

[0071] From the results of Tables 1 to 3, it was found that the friction materials for disc brake pads of Examples 1 to 3 had excellent effectiveness stability and fade resistance. In addition, the friction materials for disc brake pads of Examples 1 to 3 did not require a surface polishing process during production, so no polishing powder was generated.

Claims

1. A friction material for a disc brake pad, comprising a friction modifier, a fiber base material, and a binder, The friction modifier contains tin sulfide, It has a black surface, The black surface has a layer subjected to a scorch treatment. Friction material for disc brake pads.

2. A method for producing a friction material for a disc brake pad, the friction material comprising a friction modifier, a fiber base material, and a binder as raw materials, comprising: The friction modifier contains tin sulfide, mixing the raw materials to obtain a raw material mixture; A step of pressurizing the raw material mixture to obtain a preform; a step of hot-pressing and molding the preform to obtain a hot-pressed molded body; a step of heat-treating the hot-pressed molded body to obtain a heat-treated molded body; and a step of scorching the heat-treated molded body without surface polishing to obtain a scorched layer. A method for manufacturing friction material for disc brake pads.

3. 3. The method for producing a friction material for a disc brake pad according to claim 2, wherein the scorch treatment is surface baking at a temperature of 400 to 800° C. for 30 to 300 seconds.

Citation Information

Patent Citations

  • Manufacture of friction material

    JP1983203010A

  • Production of unground and molded friction member

    JP1988069833A

  • Frictional member for brake and its manufacture

    JP1995332414A

  • Friction material

    JP1997250586A

  • Friction material and its manufacturing method

    JP2009221303A