Manufacturing method of ceramic plate with various flow cloud surface decoration effect
The ceramic plate manufacturing method enhances surface decoration by combining underglaze, top glaze, roller printing, and metallic luster to create a flowing cloud effect, addressing the limitations of existing techniques and achieving vibrant, durable, and easy-to-clean ceramic surfaces.
Patent Information
- Application Number
- JP2023554912
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-09
- Filing Date
- 2021-12-03
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-12-03
AI Technical Summary
Existing ceramic plate production techniques limit the variety and vibrancy of surface decoration effects, primarily relying on inkjet technology for single-colored or polished surfaces, lacking a vivid and dynamic visual appeal.
A manufacturing method involving press-molding, application of underglaze and top glaze with metal oxides, roller printing, and metallic luster liquid application to create a flowing cloud effect with iridescent properties, utilizing specific glaze compositions and firing processes to achieve a three-dimensional, colorful surface.
The method produces ceramic plates with vivid, colorful, and strong hierarchical decoration effects, resistant to wear and easy to clean, suitable for various applications without environmental limitations, offering a long service life and market appeal.
Smart Images

Figure 0007578846000001
Abstract
Description
[Technical field]
[0001] The present invention belongs to the field of architectural ceramics, and specifically relates to a ceramic plate with colorful flowing cloud surface decoration effect and a manufacturing method thereof. [Background technology]
[0002] In recent years, with the maturity of ceramic plate manufacturing technology, the application market of ceramic plates is expanding more and more, and ceramic plates are favored by customers. However, due to the limitations of existing production technology, the surface decoration effect of ceramic plates is also limited. At present, most ceramic products on the market are made by inkjet technology, and are mainly polished products and dry grain products with natural surface, and the overall decoration effect is relatively single. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] China Patent Application Publication No. 109455934 [Patent Document 2] China Patent Application Publication No. 102515876 Summary of the Invention [Problem to be solved by the invention]
[0004] In response to the above-mentioned defects, the present invention proposes a ceramic plate with a colorful flowing cloud surface decoration effect and a manufacturing method thereof. The manufacturing method of the present invention does not use inkjet printing, and is different from the conventional multicolor effect (a phenomenon in which light is directly irradiated onto a medium, causing refraction and reflection to produce colorful light), and uses a vividly colored top glaze to roller-print a white cloud pattern on the top surface of the top glaze, thereby forming a flowing cloud effect on the surface of the top glaze. Furthermore, a metallic gloss liquid (colored gloss liquid) is used to attach colored metal to the surface of the ceramic plate, which forms a rainbow effect when irradiated with light. The flowing cloud effect and the rainbow effect of the colored gloss liquid are superimposed to form colorful flowing clouds when irradiated directly with light. [Means for solving the problem]
[0005] In a first aspect, the present invention provides a method for producing a method for treating a cancer cell comprising the steps of: A step of press-molding the ceramic substrate to obtain a ceramic plate base; applying an underglaze to the surface of the base to cover the base color and defects; A step of applying an overglaze containing 0.2 to 0.7 wt% of color-developing metal oxide to the surface of the base glazed with the underglaze so as to develop a vivid color; roller printing the top glaze onto the surface of the glazed base; A step of drying the base material after roller printing and firing it in a kiln; The present invention provides a method for manufacturing a ceramic plate with a variety of flowing cloud surface decoration effects, including:
[0006] The above-mentioned overglaze is preferably a high-silicon overglaze. In some technical solutions, the chemical composition of the above-mentioned overglaze further includes, in mass percentage, ignition loss: 6.5-7.5%, SiO2: 48-53%, Al2O3: 8-10%, TiO2: 7-8%, CaO: 10-13%, MgO: 2.0-3.0%, K2O: 3.0-4.0%, and ZnO: 9-11%, in addition to the color-producing metal oxide. More preferably, the content of the color-producing metal oxide in the overglaze is 0.2-0.6 wt%.
[0007] Preferably, the specific gravity of the top glaze is 1.55 to 1.58 g / cm 3 , glaze amount is 380~410 g / m 2 It is.
[0008] Preferably, the color-forming metal oxide is a mixture of one or more of copper oxide, cobalt oxide, nickel oxide, and manganese oxide.
[0009] The surface of the substrate may be coated with roller effect glaze and then roller printed. In some technical solutions, the chemical composition of the roller effect glaze is, by mass percentage, SiO2: 47-50%, Al2O3: 7-9%, TiO2: 12-13%, CaO: 10-13%, MgO: 2.0-3.0%, K2O: 2.0-3.0%, Na2O: 3.0-4.0%, and ZnO: 10-12%.
[0010] Preferably, the flow rate of the roller effect glaze is 17-20 s and the specific gravity is 1.28-1.32 g / cm 3 , glaze amount is 40~50g / m 2 It is.
[0011] Preferably, the maximum firing temperature is 1210 to 1230° C. and the firing time is 90 to 100 minutes.
[0012] Preferably, during firing, a metallic luster liquid is sprayed onto the surface of the base material at 750 to 850°C to form a metallic luster liquid film layer. The amount of the metallic luster liquid applied is 50 to 60 g / m 2 The thickness of the formed metallic luster liquid film layer may be 5 to 6 mm.
[0013] Preferably, the chemical composition of the underglaze includes, by mass percentage, SiO2: 65-67%, Al2O3: 15-17%, MgO: 1.0-1.2%, K2O: 1.0-1.2%, Na2O: 1.7-2.0%, and ZrO2: 8-10%, the application method of the underglaze is spray application, and the specific gravity of the underglaze is 1.35-1.38 g / cm 3 , glaze amount is 200~230 g / m 2 It is.
[0014] In a second aspect, the present invention provides a ceramic plate having a colorful flowing cloud surface decoration effect obtained by any one of the manufacturing methods described above. Preferably, the ceramic plate has a size of 1800-3600 mm in length x 900-1600 mm in width x 5.5-10.5 mm in height. Effect of the Invention
[0015] The present invention has the following beneficial effects:
[0016] As an innovation, the manufacturing method of the present invention combines a vividly colored top glaze, utilizes rollers with different pattern textures, and prints specially developed roller effect glazes on the surface of the ceramic product to form different texture effects; finally, sprays metallic luster liquid on the surface of the ceramic tile at a certain temperature during cooling after high-temperature firing, thereby forming a ceramic plate with a strong three-dimensional colorful flowing cloud effect.
[0017] In terms of excellent decorative effects, compared with general ceramic plates made by inkjet, the ceramic plate of the present invention has a particularly vivid surface color and a particularly strong sense of hierarchy. A colorful metallic effect is generated on the surface of the ceramic plate sprayed with metallic luster liquid, and a unique colorful flowing cloud effect can be formed by the light.
[0018] With a wide range of applications, the present invention is not affected by environmental factors and can be widely used in various interior and exterior walls, ground decoration, large-scale board background walls, etc.
[0019] In terms of ease of cleaning, the ceramic plate of the present invention is fully sintered and the water absorption rate is controlled within 0.5wt%, which makes it a ceramic tile with high gloss. No polishing process is required, and almost no pores are visible on the surface of the tile. After spraying the metallic luster liquid, a thin film with metallic texture is formed, which is resistant to dirt and easy to clean.
[0020] In terms of durability and long life, the ceramic plate of the present invention has stable performance, is less affected by time and environment, has high wear resistance, can be maintained like new for a long time, has a long service life, and has extensive market economic benefits. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a diagram showing the tile surface effect of a ceramic plate having a colorful flowing cloud surface decoration effect according to Example 1 of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The present invention will be further described below in connection with the embodiments. The following embodiments are for explaining the present invention, but are not intended to limit the present invention. In the following, each "%" means "mass %" unless otherwise specified.
[0023] Hereinafter, a method for manufacturing a ceramic plate having a colorful flowing cloud surface decoration effect according to the present invention will be described by way of example.
[0024] The ceramic substrate (also referred to as "powdered substrate material") is press-molded to obtain the substrate of the ceramic plate. The chemical composition and raw material composition of the ceramic substrate are not limited, and a ceramic substrate commonly used in this field may be used. As an example, the chemical composition of the ceramic substrate may include, in mass percentage, ignition loss (IL): 3.5-4.5%, SiO2: 58-63%, Al2O3: 25-30%, Fe2O3: 0.5-0.8%, TiO2: 0.3-0.6%, CaO: 0.3-0.5%, MgO: 1.1-1.5%, K2O: 2.0-2.5%, and Na2O: 2.3-2.7%. In some embodiments, the raw material composition of the ceramic substrate may include, by mass percentage, 18-21% sodium powder, 15-18% gold sand, 5-8% Shaoguan clay, 10-13% washed clay, 2-3% black talc, 13-18% calcined bauxite, 20-25% potassium aluminum sand, 2-3% bentonite, and 5-8% Zhongshan black mud.
[0025] Dry the green body. It may be dried in a drying kiln. The drying process is determined according to specific requirements. For example, the drying time may be 1-1.2 hours, and the moisture content of the green body after drying is controlled within 0.5wt%.
[0026] After drying, the surface of the body is coated with underglaze, mainly to cover the body color and defects. At the same time, it is necessary to ensure that the expansion coefficients of the body and the underglaze are compatible, that is, the expansion coefficient of the underglaze is close to that of the body. Zirconium white underglaze is preferred.
[0027] In some embodiments, the chemical composition of the underglaze may include, by mass percentage, SiO2: 65-67%, Al2O3: 15-17%, MgO: 1.0-1.2%, K2O: 1.0-1.2%, Na2O: 1.7-2.0%, and ZrO2: 8-10%. For example, the chemical composition of the underglaze may include, by mass percentage, IL: 2.5-4.5%, SiO2: 65-67%, Al2O3: 15-17%, Fe2O3: 0.3-0.5%, TiO2: 0.05-0.3%, CaO: 0.2-0.3%, MgO: 1.0-1.2%, K2O: 1.0-1.2%, Na2O: 1.7-2.0%, and ZrO2: 8-10%.
[0028] The raw material composition of the underglaze may include, by mass percentage, 30-35% potassium feldspar, 17-20% nepheline, 30-35% quartz, 1-1.5% calcined talc, 10-12% kaolin, 3-4% calcined clay, 1.0-2.0% aluminum oxide, and 8-10% zirconium silicate.
[0029] The method of applying the underglaze may be spraying. The specific gravity of the underglaze is 1.35 to 1.38 g / cm 3 , glaze amount is 200~230g / m 2 may be also possible.
[0030] The top glaze is applied to the surface of the base that has been glazed with the under glaze. A suitable amount of color-producing metal oxide is added to the top glaze to make the color more vivid. If the process of applying the under glaze is omitted and the top glaze is applied directly to the surface of the base, the color will be darker and less vivid, even with the same amount of top glaze applied.
[0031] The content of the color-producing metal oxide in the above-mentioned top glaze is preferably 0.2-0.7wt%. If an excessive amount of the color-producing metal oxide is used, the color of the top glaze becomes dark, the luster of the glaze layer is lost, and the colorful flowing cloud effect cannot be obtained. The above-mentioned color-producing metal oxide includes, but is not limited to, copper oxide, cobalt oxide, nickel oxide, manganese oxide, etc. Different color-producing metal oxides exhibit different colors in the above-mentioned top glaze system, for example, when copper oxide is used, it exhibits a fresh green color, when cobalt oxide is used, it exhibits a blue color, and when manganese oxide is used, it exhibits a reddish brown color.
[0032] The chemical composition of the above-mentioned overglaze may include, by mass percentage, IL: 6.5-7.5%, SiO2: 48-53%, Al2O3: 8-10%, TiO2: 7-8%, CaO: 10-13%, MgO: 2.0-3.0%, K2O: 3.0-4.0%, ZnO: 9-11%, and color-developing metal oxides: 0.2-0.7%. The above-mentioned overglaze is a high-silicon overglaze, mainly high in silicon and low in aluminum, and at the same time, a large amount of calcium oxide is introduced (for example, by frit) to reduce the viscosity of the glaze and improve the flowability and gloss of the glaze. Titanium oxide and zinc oxide are also added to the overglaze to increase the stability of the color development of the oxides.
[0033] In some embodiments, the chemical composition of the top glaze includes, by mass percentage, IL: 6.5-7.5%, SiO2: 48-53%, Al2O3: 8-10%, Fe2O3: 0.1-0.2%, TiO2: 7-8%, CaO: 10-13%, MgO: 2.0-3.0%, K2O: 3.0-4.0%, Na2O: 0.2-0.3%, CuO 0.3-0.5%, ZnO 9-11%, and CoO 0.15-0.2%.
[0034] As a result of the experiment, the high silicon top glaze was changed to a general-purpose top glaze (i.e., one that adds zirconium silicate to help the color development of general-purpose pigments), but it was found that the color looked dull and it was not possible to achieve vivid color development, and the fluidity of the glaze was poor, affecting the overall sense of hierarchy.
[0035] In some embodiments, the raw material composition of the top glaze may include, by mass percentage, 25-30% potassium feldspar, 10-15% quartz, 10-15% calcite, 7-10% calcined zinc oxide, 5-8% Zhongshan black mud, 6-8% titanium dioxide, 5-8% calcined talc, 23-28% frit A, 5-8% frit B, and 0.2-0.5% color-developing oxide. The chemical composition of frit A, in mass percentage, is as follows: IL: 0.5-1.5%, SiO2: 27-30%, Al2O3: 8-10%, Fe2O3: 0.1-0.2%, TiO2: 0.2-0.5%, CaO: 25-35%, MgO: 0.5-1.0%, K2O: 2.0-3.0%, Na2O: 0.2-0.3%, and ZnO: 27-30%. The chemical composition of frit B, in mass percentage, is as follows: IL: 0.5-1.5%, SiO2: 48-50%, Al2O3: 9-12%, Fe2O3: 0.1-0.2%, TiO2: 1-2%, CaO: 23-28%, MgO: 1.5-2.0%, K2O: 3.0-4.0%, Na2O: 2.0-3.0%, and ZnO: 8-10%.
[0036] The initial melting temperature of the upper glaze is 950-1100° C. By controlling the initial melting temperature of the upper glaze within the above range, gases harmful to the sintering process can be completely discharged, and the glaze layers can be blended without interpenetration, improving the flatness of the glaze surface and favoring the maintenance of the colorful layered feeling of flowing clouds.
[0037] The method of applying the top glaze may be spray glaze. The specific gravity of the top glaze is 1.55 to 1.58 g / cm 3 , glaze amount is 380~410 g / m 2 By controlling the amount of top glaze applied within the above range, it is possible to prevent the amount of top glaze applied being too small, resulting in a dull color, or the amount of top glaze applied being too large, resulting in a dark color. If the amount of top glaze applied is too large, the maturation temperature of the glaze becomes high, making it impossible to maturate at the specified firing temperature in the kiln, resulting in defects such as dullness, and if the amount of oxides in the glaze increases, the transparency of the glaze layer decreases, further affecting the layered appearance of the product.
[0038] The top glaze is roller printed on the surface of the glazed base material. The pattern texture with different ups and downs is roller printed, and various pattern effects are presented in combination with the top glaze with vivid coloring. The roller printing can adopt a single roll or a multi-roll combination. Inkjet printing is poor in the sense of hierarchy because the ink does not color on the surface of the top glaze and is repelled. Furthermore, titanium dioxide is used as an opacifier in the top glaze and roller effect glaze of the present invention, and the ink cannot color in this glaze system, and the colorful flowing cloud effect cannot be realized. Therefore, the inkjet printing method is not applicable to the present invention. The pattern by silk screen printing is fixed as a single pattern, and the pattern cannot be flexibly changed. The present invention forms a pattern by roller printing, which has excellent over-the-top effect with ups and downs of the pattern, and can realize random combination of patterns during continuous production, which is more artistic.
[0039] This roller print effect is achieved by applying a roller effect glaze (also called "effect glaze" or "roller effect pattern glaze") to the surface of the base material. The chemical composition of the roller effect glaze may include, by mass percentage, SiO2: 47-50%, Al2O3: 7-9%, TiO2: 12-13%, CaO: 10-13%, MgO: 2.0-3.0%, K2O: 2.0-3.0%, Na2O: 3.0-4.0%, and ZnO: 10-12%. The roller effect glaze mainly uses the opalescence effect of titanium oxide to create a cloud pattern.
[0040] The difference in chemical composition between the roller effect glaze and the top glaze should not be too large, so that the two composition systems are close to each other and do not repel each other, and can be better blended, so that the top glaze and the roller effect glaze cooperate to realize a clear hierarchical cloud effect. Preferably, the initial melting temperature of the top glaze is 5-10°C higher than that of the roller effect glaze. This is to improve the penetration transient characteristics of the edge where the roller effect glaze contacts the top glaze. If the initial melting temperature of the top glaze used is lower than that of the effect glaze, the top glaze will cover the top surface of the effect glaze locally, and the effect glaze will sink into the top glaze, making it impossible to achieve the purpose of the present invention. In addition, it should be noted that when color-developing metal oxides are added to the roller effect glaze, when using a multi-roll combination, the overlap of oxides in the glaze will cause poor edge transient between the top glaze and the roller effect glaze, and the colorful flowing cloud effect will be reduced. The present invention prints a cloud pattern on the surface of the top glaze by roller printing, forming a clear contrast with the color of the top glaze, and better forming a visually clear effect.
[0041] In some embodiments, the chemical composition of the roller effect glaze includes, by mass percentage, IL: 5.5-7.0%, SiO2: 47-50%, Al2O3: 7-9%, Fe2O3: 0.1-0.2%, TiO2: 12-13%, CaO: 10-13%, MgO: 2.0-3.0%, K2O: 2.0-3.0%, Na2O: 3.0-4.0%, and ZnO: 10-12%.
[0042] The raw material composition of the roller effect glaze may include, by mass percentage, 10-15% potassium feldspar, 15-20% albite, 12-15% quartz, 10-12% calcite, 10-13% calcined zinc oxide, 5-8% Zhongshan black mud, 12-15% titanium dioxide, 5-6% calcined talc, 15-20% frit A, and 3-5% frit B. The chemical composition of frit A may include, in mass percentage, IL: 0.5-1.5%, SiO2: 27-30%, Al2O3: 8-10%, Fe2O3: 0.1-0.2%, TiO2: 0.2-0.5%, CaO: 25-28%, MgO: 0.5-1.0%, K2O: 2.0-3.0%, Na2O: 0.2-0.3%, and ZnO: 27-30%. The chemical composition of frit B may include, in mass percentage, IL: 0.5-1.5%, SiO2: 48-50%, Al2O3: 9-12%, Fe2O3: 0.1-0.2%, TiO2: 1-2%, CaO: 23-25%, MgO: 1.5-2.0%, K2O: 3.0-4.0%, Na2O: 2.0-3.0%, and ZnO: 8-10%.
[0043] Experimental results show that the introduction of a large amount of calcined zinc oxide and titanium oxide into the raw material composition of the roller effect glaze leads to poor flowability of the roller effect glaze. Therefore, in the present invention, the performance of the roller effect glaze is significantly improved by adjusting the ratio of glaze slurry of the roller effect glaze, and the pattern can be perfectly printed on the surface of the substrate by roller printing to form colorful flowing clouds. In some embodiments, the glaze slurry of the roller effect glaze includes, by weight, 100 parts by weight of roller effect glaze, 100-150 parts by weight of printing ink, 10-30 parts by weight of adhesive remover, 0.1-0.5 parts by weight of sodium carboxymethylcellulose, 0.1-0.5 parts by weight of sodium tripolyphosphate, and 1-10 parts by weight of water. Thus, the roller effect pattern has excellent flowability, high definition, good three-dimensional effect, does not stick to the roll, and can be continuously produced. In some embodiments, the flow rate of the roller effect glaze is 17-20 seconds, and the specific gravity is 1.28-1.32 g / cm 3 , glaze amount is 40~50g / m 2If the flow rate and specific gravity of the roller effect glaze are low and the amount of glaze applied is the same, the cloud pattern may be blurred. On the contrary, if the specific gravity and flow rate of the roller effect glaze are high, the effect glaze will not be transparent when melted at high temperature, so the boundary will be clear and it will be impossible to form a colorful flowing cloud effect. In addition, if the amount of roller effect glaze applied is too much, the glaze surface may lose its luster.
[0044] The top glaze and roller effect glaze of the present invention with the above chemical composition can form a glaze layer with high gloss when melted at high temperature, and has a good degree of vitrification and no defects such as pinholes on the surface. Therefore, in the manufacturing method of the present invention, it is not necessary to apply a transparent frit layer on the surface of the ceramic body on which the colorful flowing cloud pattern is formed.
[0045] Different from the use of transparent glaze with high refractive index to form colorful pearlescent, the present invention uses a vividly colored top glaze, roller prints different patterns to form a drifting cloud effect, and finally sprays metallic luster liquid and bakes it on the surface of the glaze layer by high temperature action, forming a colorful drifting cloud surface decoration effect with a pearlescent sense under light irradiation. Among them, the main technical challenges in forming colorful drifting clouds are, firstly, that the glaze layer needs to satisfy the high silicon and low aluminum system which is favorable for the adhesion of the colored luster liquid to the glaze layer surface, and secondly, that the formulation of the top glaze and the roller effect glaze is similar, and the effect glaze and the top glaze are blended without repelling each other, realizing a clear hierarchical cloud group effect (layered cloud effect).
[0046] After roller printing, the base material is dried and then fired in a kiln.
[0047] In the firing process, the maximum firing temperature is 1210-1230°C, and the firing time is 90-100min. Preferably, the metallic luster liquid is sprayed on the surface of the base material at 750-850°C during firing. By applying the metallic luster liquid to the glaze surface, it will exhibit a metallic or pearlescent luster when fired at a temperature of 750-800°C. The luster liquid can be obtained from a commercial product, for example, an organic liquid pigment produced by mixing bismuth or various metal salts with resin to make a metal soap and dissolving it in an oil mixture is used. In the embodiment for carrying out the invention, the metallic luster liquid is purchased from Foshan Sencailiang Decoration Material Co., Ltd. and has a product number of 25A.
[0048] The application rate of the metallic luster liquid is 50-60 g / m 2 In this way, the color effect of the metallic luster liquid is vivid, the visual effect is good, and the production requirements can be met.
[0049] In some embodiments, a swing-arm type automatic spray gun is installed on the top of the kiln, and the metallic luster liquid is sprayed onto the surface of the ceramic plate by the swing-arm automatic spray gun during the high-temperature cooling stage during firing, for example, when cooling to 750 to 850°C. The thickness of the metallic luster liquid film layer is controlled by adjusting the moving speed of the spray gun and the application amount of the metallic luster liquid. The moving speed of the spray gun may be 55 to 65 m / min. The thickness of the metallic luster liquid film layer may be 5 to 6 mm.
[0050] Finally, the edges are polished and graded before packaging. The product has a bright mirror effect, the glaze surface is smooth and pinhole-free, and at the same time, the polishing liquid forms a film on the surface of the base material and adheres to the surface of the ceramic plate, which, combined with the drifting cloud effect formed by the roller effect glaze, finally forms a ceramic plate with colorful drifting cloud effect. The above product does not require polishing, so the energy consumption caused by polishing can be avoided during production.
[0051] The present invention will be described in more detail with reference to the following examples. The following examples are merely for further explanation of the present invention and do not limit the scope of protection of the present invention. Non-essential improvements and modifications made by those skilled in the art based on the above content of the present invention are also within the scope of protection of the present invention. The specific process parameters in the following examples are merely examples within the applicable range, that is, those skilled in the art can select within an appropriate range based on the description of the present invention, and are not limited to the specific numerical values in the following examples.
[0052] Example 1 The manufacturing method of ceramic plates with colorful flowing cloud surface decoration effects is as follows: Step 1 is to press-mold the ceramic base material to obtain a green body, and then place the green body in a drying kiln to dry it; The surface density of the dried material is 1.35 g / cm 3 , glaze amount is 200~230 g / m 2 Step 2 is to spray the underglaze, The surface of the base with the underglaze sprayed on has a specific gravity of 1.56 g / cm 3 , glaze amount is 380~410 g / m 2 Step 3 is to spray the top glaze. The surface of the base material sprayed with the top glaze is then roller printed, and different patterns are created by the roller texture and the printing of the roller effect glaze, the specific gravity of which is 1.28-1.32 g / cm 3 So step 4, After roller printing, the base material is placed in a kiln to be baked, and the baking temperature is cooled to 750-800°C. A swing-arm type automatic spray gun is installed on the top of the kiln, and the thickness of the metallic luster liquid film layer is controlled by adjusting the movement speed of the automatic spray gun and the spray amount of the metallic luster liquid. The spray amount of the metallic luster liquid is 50-60g / m 2 Step 5, and step 6 of polishing the edges and packaging.
[0053] Comparative Example 1 This comparative example is basically the same as Example 1, with the difference being that the chemical composition of the top glaze contains, in mass percentage, IL: 2.5-4.5%, SiO2: 60-63%, Al2O3: 12-15%, Fe2O3: 0.3-0.5%, TiO2: 0.05-0.3%, CaO: 7.5-10.5%, MgO: 2.0-4.5%, K2O: 1.0-2.0%, Na2O: 0.5-1.0%, and ZrO2: 8-10%, and the raw material composition of the top glaze contains, in mass percentage, frit C: 15-18%, potassium feldspar: 35-38%, calcite: 12-16%, talc: 8-10%, kaolin: 8-10%, Zhongshan black mud: 3-5%, zinc oxide: 3-5%, nepheline: 8-10%, and porphyrin: 8-10%. The chemical composition of frit C is, by mass percentage, IL: 0.3-0.5%, SiO2: 55-58%, Al2O3: 13-15%, Fe2O3: 0.1-0.2%, TiO2: 0.02-0.05%, CaO: 10-12%, MgO: 2.0-2.5%, K2O: 5.0-6.5%, Na2O: 0.3-0.6%, ZnO: 3-5%. When using the above overglaze, the only thing that needs to be added to the overglaze is to add 1-10% of a general-purpose pigment, specifically Golden Brown 816, Vanadium Zirconium Blue or Cobalt Blue to assist in color development.
[0054] However, the ceramic plate obtained in this comparative example was not able to develop a sufficiently vivid color, had poor fluidity, and was unable to realize a clearly defined layered appearance.
[0055] Comparative Example 2 This comparative example is basically the same as Example 1, the only difference being that the chemical composition of the roller effect glaze contains, by mass percentage, IL: 0.3-0.5%, SiO2: 56-59%, Al2O3: 12-15%, Fe2O3: 0.1-0.2%, TiO2: 0.02-0.05%, CaO: 8-10%, MgO: 2.0-2.5%, K2O: 3.0-3.5%, Na2O: 0.3-0.6%, ZnO: 3-5%, ZrO2: 5-8%. In this case, the flowability of the roller effect glaze is improved, but the color development is poor, pinholes are easily generated, and the hierarchical appearance is not good. In addition, general-purpose pigments with weak coloring tend to develop a yellow and dark color in high-calcium and high-magnesium gloss glazes. At the same time, because they have a low initial melting point and a large difference in composition with the top glaze, the different components react and blend, resulting in poor layering effects and causing phenomena such as localized drying of the glaze and pinholes.
[0056] Comparative Example 3 This comparative example is basically the same as Example 1, with the difference being that the chemical composition of the top glaze is, in mass percentage, IL: 0.5-1.5%, SiO2: 52-55%, Al2O3: 5-8%, Fe2O3: 0.1-0.2%, TiO2: 1-2%, CaO: 23-28%, MgO: 1.5-2.0%, K2O: 3.0-4.0%, Na2O: 2.0-3.0%, ZnO: 8- The only difference is that the glaze contains 10% of aluminum oxide, and the chemical composition of the roller effect glaze contains, by mass percentage, IL: 0.5-1.5%, SiO2: 48-50%, Al2O3: 9-12%, Fe2O3: 0.1-0.2%, TiO2: 1-2%, CaO: 23-25%, MgO: 1.5-2.0%, K2O: 3.0-4.0%, Na2O: 2.0-3.0%, and ZnO: 8-10%. The initial melting temperature of the glaze is adjusted to be low and the content of aluminum oxide is reduced, so that the glaze has good color and obvious crystal flowers, but the glaze is easily stuck to the edge of the base. In addition, in this case, the roller effect glaze and the glaze are blended too much, which blurs the drifting cloud effect on the tile surface, and causes pinhole swelling and glaze drying in some places. This is mainly due to the incompatibility of the top glaze with the roller effect glaze due to the lowering of the initial melting point of the top glaze.
[0057] Comparative Example 4 This comparative example is basically the same as Example 1, with the difference being that the chemical composition of the top glaze is, in mass percentage, IL: 1.5-4.5%, SiO2: 58-65%, Al2O3: 13-20%, The chemical composition of roller effect glaze contains, by mass percentage, IL: 0.5-1.5%, SiO2: 48-50%, Al2O3: 9-12%, Fe2O3: 0.1-0.2%, TiO2: 1-2%, CaO: 23-25%, MgO: 1.5-2.0%, K2O: 3.0-4.0%, Na2O: 2.0-3.0%, P2O5: 0.2-0.3%, and the chemical composition of roller effect glaze contains, by mass percentage, IL: 0.5-1.5%, SiO2: 48-50%, Al2O3: 9-12%, Fe2O3: 0.1-0.2%, TiO2: 1-2%, CaO: 23-25%, MgO: 1.5-2.0%, K2O: 3.0-4.0%, Na2O: 2.0-3.0%, ZnO: 8-10%. In this comparative example, the top glaze system and the effect glaze are significantly different, and the oxides added to the top glaze are unable to develop color or are clearly unable to develop color in this experiment, so the requirements cannot be met, and the effect glaze sinks into the top glaze, causing phenomena such as localized drying and swelling of the glaze.
Claims
1. A step of press-molding the ceramic substrate to obtain a ceramic plate base; applying an underglaze to the surface of the base to cover the base color and defects; A top glaze is applied to the surface of the base that has been glazed with an under glaze, and 0.2 to 0.7 wt% of color-producing metal oxide is introduced into the top glaze to produce a vivid color. The chemical composition of the top glaze, in addition to the color-producing metal oxide, is, in mass percentage, ignition loss: 6.5 to 7.5%, SiO 2 : 48-53%, Al 2 O 3 : 8-10%, TiO 2 :7-8%, CaO: 10-13%, MgO: 2.0-3.0%, K 2 The specific gravity of the upper glaze is 1.55 to 1.58 g / cm 3 , glaze amount is 380-410 g / m 2 and A roller effect glaze is applied to the surface of the base material on which the top glaze is applied, and a cloud pattern is printed on the surface of the top glaze by roller printing, and the chemical composition of the roller effect glaze is, in mass percentage, SiO 2 : 47-50%, Al 2 O 3 : 7-9%, TiO 2 :12-13%, CaO: 10-13%, MgO: 2.0-3.0%, K 2 O: 2.0-3.0%, Na 2 Contains 3.0-4.0% O, 10-12% ZnO, and has a specific gravity of 1.28-1.32 g / cm 3 , glaze amount is 40~50g / m 2 The initial melting temperature of the upper glaze is 5-10°C higher than that of the roller effect glaze, so the edge where the roller effect glaze contacts with the upper glaze has a permeation transient characteristic with ups and downs of the pattern; After roller printing, the substrate is dried and then fired in a kiln. During firing, the metallic luster liquid is sprayed onto the surface of the substrate at 750-850°C to form a metallic luster liquid film layer. The application amount of the metallic luster liquid is 50-60 g / m 2and the thickness of the formed metallic luster liquid film layer is 5-6 mm; A method for producing a ceramic plate having a colorful flowing cloud surface decoration effect, comprising the steps of:
2. 2. The method according to claim 1, wherein the color-producing metal oxide is a mixture of one or more of copper oxide, cobalt oxide, nickel oxide, and manganese oxide.
3. The method according to claim 1, characterized in that the maximum firing temperature is 1210-1230°C and the firing time is 90-100 min.
4. The chemical composition of the underglaze is, by mass percentage, SiO 2 : 65-67%, Al 2 O 3 : 15~17%, MgO: 1.0~1.2%, K 2 O: 1.0-1.2%, Na 2 O: 1.7-2.0%, ZrO 2 : 8-10%, the method of application of the underglaze is spray application, and the specific gravity of the underglaze is 1.35-1.38 g / cm 3 , glazing amount is 200-230 g / m 2 The method according to claim 1 ,
Citation Information
Patent Citations
Resin acid titanium-iron-bismuth system yellow-series electro-optic water and preparation method thereof
CN102515876A
Silver glaze with metallic luster and preparation method thereof
CN106631172A
Flowing color decorative effect ceramic tile and preparation method thereof
CN109455934A
Metal color archaized brick and production method thereof
CN111039697A
Metal dry granular glaze, metallic luster ceramic tile and preparation method of metallic luster ceramic tile