Titanium oxide thin film, its manufacturing method and photocatalytic functional member

The titanium oxide thin film with controlled oxygen coordination and crystallinity structure addresses carrier recombination issues, enhancing photocatalytic performance by promoting carrier movement to the surface, thereby improving deodorizing and sterilizing capabilities.

JP7578957B2Active Publication Date: 2024-11-07KONICA MINOLTA INC +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021142980
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-02
Publication Date
2024-11-07
Estimated Expiration
2041-09-02

AI Technical Summary

Technical Problem

Existing titanium oxide photocatalysts face challenges in effectively decomposing organic compounds and bacteria due to high carrier recombination rates, limiting their photocatalytic performance, especially in oxidation reactions beyond nitrogen oxide removal.

Method used

A titanium oxide thin film with a structured surface and inner region, characterized by varying oxygen coordination numbers and crystallinity, is produced using magnetron sputtering with controlled magnetic flux density, facilitating carrier movement to the surface and reducing recombination.

Benefits of technology

The structured titanium oxide thin film enhances photocatalytic ability by suppressing carrier recombination and increasing the reactivity of reduction and oxidation reactions, demonstrating improved performance in deodorizing and sterilizing effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578957000001
    Figure 0007578957000001
  • Figure 0007578957000002
    Figure 0007578957000002
  • Figure 0007578957000003
    Figure 0007578957000003
Patent Text Reader

Abstract

To provide a titanium oxide thin film having photocatalytic function enhanced, a production method thereof, and a photocatalytic functional member.SOLUTION: A titanium oxide thin film of the invention contains titanium oxide having photocatalytic function. The thin film has a surface and an internal face opposite to the surface. The coordination number of oxygen to a titanium ion decreases as going from the intermediate region located between the internal face and the surface to the surface side region. The coordination number 6 is relatively frequent in the internal side region including the internal face, where the coordination number 4 is relatively frequent in the surface side region including the surface. The internal side region has a crystal structure, where the surface side region has an amorphous structure.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a titanium oxide thin film, a method for producing the same, and a photocatalytic functional member. More specifically, the present invention relates to a titanium oxide thin film having improved photocatalytic activity, a method for producing the same, and a photocatalytic functional member. [Background technology]

[0002] In recent years, photocatalysts have attracted attention and research and development has been promoted from the viewpoint of decomposing and detoxifying harmful chemical substances and environmental pollutants in the air using only light energy. Titanium oxide is a well-known example of such a photocatalyst. For example, by coating the surface of a film, glass, tile, etc. with a thin film containing titanium oxide (hereinafter also referred to as "titanium oxide thin film"), it is possible to impart a deodorizing effect and a sterilizing effect.

[0003] "Photocatalytic reaction" refers to a reaction in which excited electrons and holes (hereinafter collectively referred to as "carriers") generated in a photocatalyst by light cause reduction and oxidation, respectively. For example, oxidation reactions can decompose organic compounds and bacteria, resulting in deodorizing and sterilizing effects.

[0004] However, carriers have the property of easily recombining, and once recombination occurs, the reduction and oxidation reactions do not occur and the photocatalytic activity is not expressed. Therefore, it has been thought that by reducing the crystal defects that are the centers of carrier recombination and creating a highly crystalline structure, it is possible to suppress carrier recombination and obtain high photocatalytic activity.

[0005] On the other hand, since reduction and oxidation reactions take place on the surface of the photocatalyst, it is preferable from the viewpoint of reactivity that carriers generated inside the photocatalyst migrate to the surface. Therefore, research and development has been conducted on methods for migrating carriers to the surface of the photocatalyst while suppressing carrier recombination.

[0006] Patent Document 1 discloses a photocatalytic technology that can remove nitrogen oxides in gas not only in the absence of oxygen but also in the presence of oxygen without producing highly corrosive substances such as nitric acid by including titanium oxide in which the Ti species has a 4-coordinate structure in addition to a 6-coordinate structure. However, this technology selectively performs only a reduction reaction, and its effect is limited to the removal of nitrogen oxides. Therefore, further research has been conducted on photocatalysts that are highly reactive in oxidation reactions and can decompose and remove substances other than nitrogen oxides. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 11-342344 Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide a titanium oxide thin film with improved photocatalytic activity, a method for producing the same, and a photocatalytic functional member. [Means for solving the problem]

[0009] The present inventors have investigated the causes of the above problems in order to solve the above problems, and as a result have found that, in a titanium oxide thin film containing titanium oxide having photocatalytic activity, when one side of the thin film is the surface and the surface opposite to the surface is the internal surface, the coordination number of oxygen to titanium ions decreases from the intermediate region existing between the internal surface and the surface to the surface side region, such that 6-coordination is relatively more common in the internal surface region including the surface, and 4-coordination is relatively more common in the surface side region including the surface, and that the internal side region has a crystalline structure and the surface side region has a non-crystalline structure, thereby improving photocatalytic activity, which led to the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.

[0010] 1. A titanium oxide thin film containing titanium oxide having photocatalytic activity, When one surface of the thin film is defined as a surface and the surface opposite to the surface is defined as an inner surface, the surface side region is a region within a range of 2 nm or less in a direction from the surface of the thin film to the internal surface, the inner region is a region within a range of 10 nm or more from the surface of the thin film in a direction toward the inner surface, titanium ions having an oxygen coordination number of 4 are present in greater amounts in the surface region than in the inner region; titanium ions having an oxygen coordination number of 6 are present in greater amounts in the inner region than in the surface region; and, The inner region has a crystalline structure, and the surface region has a non-crystalline structure. A titanium oxide thin film characterized by:

[0011] 2. The titanium oxide thin film formed on a substrate, The surface side region has a shape such that, in a direction from the surface of the thin film to the substrate, 2nm or less is an area within the range The inner region is a region within a range of 10 nm or more from the surface of the thin film in a direction toward the substrate to the inner surface in contact with the substrate. 2. The titanium oxide thin film according to claim 1,

[0012] 3. In the range of 456 to 465 eV of the energy loss spectrum of the titanium oxide thin film measured by electron energy loss spectroscopy, The inner region has two loss peaks, The surface side region has one loss peak, A loss peak position in the surface side region is between two loss peak positions in the inner side region. 3. The titanium oxide thin film according to claim 1 or 2,

[0013] 4. A method for producing a titanium oxide thin film according to any one of items 1 to 3, comprising the steps of: The method includes a step of forming a film by a magnetron sputtering method, In the film-forming step, the maximum magnetic flux density in the direction perpendicular to the target surface is 0.14 T or more. A method for producing a titanium oxide thin film comprising the steps of:

[0014] 5. The titanium oxide thin film according to any one of items 1 to 3 is provided. A photocatalytic functional member characterized by: Effect of the Invention

[0015] By the above-mentioned means of the present invention, it is possible to provide a titanium oxide thin film having improved photocatalytic activity, a method for producing the same, and a photocatalytic functional member.

[0016] Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows.

[0017] As mentioned above, in order to improve photocatalytic performance, it is necessary to suppress carrier recombination and move the carriers generated inside the photocatalyst to the surface by reducing crystal defects that serve as carrier recombination centers and creating a highly crystalline structure.

[0018] In the titanium oxide thin film of the present invention, the coordination number of oxygen to titanium ions is reduced from the intermediate region between the internal face and the surface to the surface region, resulting in a smooth band bending, and carriers generated in the relatively stable internal region can be transported to the relatively unstable surface region.

[0019] Furthermore, by forming the surface side region to have a low crystallinity structure having an appropriate amount of crystal defects, carriers are captured, and therefore the carriers can be held in the surface side region. [Brief description of the drawings]

[0020] [Figure 1] Schematic diagram showing each region in the titanium oxide thin film of the present invention. [Diagram 2] Basic configuration of the magnetron sputtering apparatus used in the present invention [Diagram 3]FIG. 1 is a schematic diagram showing the main components of one embodiment of a reactive RF magnetron sputtering apparatus used in the present invention. [Figure 4] Energy loss spectrum of the titanium oxide thin film of the present invention measured by electron energy loss spectroscopy [Diagram 5] TEM images and diffraction images of the titanium oxide thin film of the present invention [Figure 6] Graph showing the results of acetaldehyde decomposition performance test DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The titanium oxide thin film of the present invention is a titanium oxide thin film containing titanium oxide having photocatalytic activity, and when one surface of the thin film is defined as a front surface and the surface opposite to the front surface is defined as an inner surface, the surface side region is a region within a range of 2 nm or less in a direction from the surface of the thin film toward the internal surface, the internal side region is a region within a range of 10 nm or more in a direction from the surface of the thin film toward the internal surface, titanium ions having an oxygen coordination number of 4 are present in greater amounts in the surface side region than in the internal side region, and titanium ions having an oxygen coordination number of 6 are present in greater amounts in the internal side region than in the surface side region, The inner region has a crystalline structure, and the surface region has a non-crystalline structure. This feature is a technical feature common to or corresponding to the following embodiments.

[0022] In one embodiment of the present invention, from the viewpoint of suppressing recombination of carriers, in the titanium oxide thin film formed on a substrate, the surface side region has a thickness in a direction from the surface of the thin film to the substrate, 2nm or less and the inner region is preferably a region within a range of 10 nm or more from the surface of the thin film in a direction toward the substrate to the inner surface in contact with the substrate.

[0023] Furthermore, from the viewpoint of suppressing carrier recombination, it is preferable that, within a specific range of the energy loss spectrum of the titanium oxide thin film measured by electron energy loss spectroscopy, the inner region has two loss peaks, the surface region has one loss peak, and the position of the loss peak in the surface region is between the positions of the two loss peaks in the inner region.

[0024] The method for producing a titanium oxide thin film of the present invention includes a step of forming a film by magnetron sputtering, and is characterized in that in the film forming step, the maximum magnetic flux density in the direction perpendicular to the target surface is 0.14 T or more.

[0025] The titanium oxide thin film of the present invention is suitably provided in a photocatalytic functional member.

[0026] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values ​​before and after the symbol "to" are included as the lower limit and upper limit.

[0027] <Titanium oxide thin film overview> The titanium oxide thin film of the present invention is a titanium oxide thin film containing titanium oxide having photocatalytic activity, and when one surface of the thin film is defined as a front surface and the surface opposite to the front surface is defined as an inner surface, the surface side region is a region within a range of 2 nm or less in a direction from the surface of the thin film toward the internal surface, the internal side region is a region within a range of 10 nm or more in a direction from the surface of the thin film toward the internal surface, titanium ions having an oxygen coordination number of 4 are present in greater amounts in the surface side region than in the internal side region, and titanium ions having an oxygen coordination number of 6 are present in greater amounts in the internal side region than in the surface side region, The inner region has a crystalline structure, and the surface region has a non-crystalline structure.

[0028] From the viewpoints of photocatalytic activity and durability, the thickness of the titanium oxide thin film of the present invention is preferably 0.1 μm or more, and more preferably 0.4 μm or more, and from the viewpoint of preventing peeling, cracking, or warping, the thickness is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less.

[0029] The mass per unit area of ​​the titanium oxide thin film of the present invention is 0.04 g / m from the viewpoints of photocatalytic activity and durability. 2 It is preferable that the content is 0.12 g / m or more. 2 More preferably, it is 0.2 g / m or more. 2 From the viewpoint of suppressing peeling, cracking, or warping, it is more preferable that the thickness is 20 g / m or more. 2 It is preferable that the thickness is less than 12 g / m 2 More preferably, it is 5 g / m or less. 2 It is even more preferable that:

[0030] 1 is a schematic diagram showing each region in a titanium oxide thin film. The titanium oxide thin film of the present invention is preferably formed directly on a substrate, which will be described later. In the titanium oxide thin film of the present invention, the "surface" refers to the interface having the largest area in the titanium oxide thin film, and the "internal surface" refers to the surface opposite to the above surface, that is, the surface that comes into contact with the substrate when the titanium oxide thin film is formed on a substrate.

[0031] 1, the titanium oxide thin film 100 of the present invention is divided into three regions: a surface side region 101, an intermediate region 102, and an internal side region 103. In the direction from the surface of the titanium oxide thin film toward the substrate 104, a region within a range of 0 to 2 nm including the surface is called the "surface side region," a region within a range of 2 to 10 nm is called the "intermediate region," and a region of 10 nm or more up to the internal surface in contact with the substrate is called the "internal side region."

[0032] The titanium oxide contained in the titanium oxide thin film of the present invention has photocatalytic activity. Representative crystal systems of titanium oxide include the tetragonal anatase type and rutile type, and the orthorhombic brookite type. In nature, the rutile type is the most common, with the anatase type and brookite type rarely occurring.

[0033] In both crystal systems, the semiconductor has a band gap equivalent to the energy of ultraviolet light, with the valence band being composed of the 2p orbital of oxygen and the conduction band being composed of the 3d orbital of Ti. Therefore, in titanium oxide semiconductors, when light with energy exceeding the band gap is incident, electrons are excited from the valence band to the conduction band, and electrons (e - ) and holes (h +) are generated. Of these excited electrons (also called "free electrons" or "conduction electrons") and holes (hereinafter, collectively referred to as "charge carriers" or simply "carriers" as carriers that carry negative (-) or positive (+) charges, respectively), those present near the surface of the titanium oxide thin film contribute to reduction and oxidation reactions. For example, oxidation reactions can break down organic compounds and bacteria, resulting in deodorizing and sterilizing effects.

[0034] Since carriers tend to disappear due to recombination, it is necessary to suppress the recombination of carriers and extend their lifetime in order to improve photocatalytic activity. The lifetime of carriers is greatly affected by recombination at recombination centers.

[0035] "Recombination" refers to the process in which excited electrons and holes combine and disappear. In some cases, excited electrons and holes recombine directly, but in most cases, they recombine indirectly via a recombination center. Moreover, the "recombination center" refers to an energy level generated by impurities other than donors and acceptors, crystal defects, etc., and serves as an intermediary for the recombination of electrons and holes. Therefore, by reducing the number of impurities and crystal defects that act as recombination centers, it is possible to suppress the recombination of carriers and improve the photocatalytic activity.

[0036] However, in order for the carriers to contribute to reduction and oxidation reactions, they need to be held near the surface of the titanium oxide thin film, and the titanium oxide thin film of the present invention holds the carriers by having "trapping centers" in the surface region.

[0037] A "trap center" is a metastable energy level that temporarily captures carriers but releases them again before they can recombine. Therefore, the carriers can be held while suppressing recombination of the carriers.

[0038] In the titanium oxide thin film of the present invention, the crystallinity is changed by changing the coordination number of oxygen to titanium ions, so that the inner region has relatively few crystal defects, while the surface region has a moderate amount of crystal defects, thereby improving the photocatalytic activity.

[0039] In addition, by gradually decreasing the coordination number of oxygen to titanium ions from the intermediate region to the surface region, a smooth band bending occurs, allowing carriers generated in the relatively stable inner region to move to the relatively unstable surface region, further enhancing the reactivity of reduction and oxidation reactions.

[0040] [Structure of titanium oxide thin film] The titanium oxide thin film of the present invention is characterized in that the inner region has a crystalline structure and the surface region has a non-crystalline structure.

[0041] In the present invention, the term "crystal structure" refers to a structure having periodic regularity (long-range order) over a wide range. Moreover, the term "non-crystalline structure" refers to a structure that does not have this kind of regularity. In other words, in a "non-crystalline structure," there is no long-range order, but it is not completely disordered, and "short-range order" exists. Specifically, when considered as a crystalline structure, it refers to a structure that has many crystal defects. Hereinafter, "having a crystalline structure" refers to a relatively high degree of crystallinity, and "having a non-crystalline structure" refers to a relatively low degree of crystallinity.

[0042] Furthermore, in the titanium oxide thin film of the present invention, the coordination number of oxygen to titanium ions is gradually reduced from the intermediate region to the surface region, resulting in a smooth band bending, which enables carriers generated in the relatively stable inner region to move to the relatively unstable surface region, further enhancing the reactivity of reduction and oxidation reactions.

[0043] In the present invention, the basic crystal structure is not changed, but the coordination number of oxygen to titanium ions is gradually decreased to generate crystal defects, resulting in a structure in which the crystallinity is gradually decreased. The coordination number of oxygen can be adjusted by the magnetic flux density during the production of the titanium oxide thin film.

[0044] The crystal defects include titanium interstitial defects in addition to oxygen defects. Hereinafter, the oxygen defects will be described.

[0045] Specifically, the structure of the titanium oxide thin film of the present invention is characterized in that the coordination number of oxygen to titanium ions decreases from the intermediate region between the internal face and the surface to the surface region, with six-fold coordination being relatively more common in the internal region including the internal face and four-fold coordination being relatively more common in the surface region including the surface. In this specification, the term "coordination number" refers to the coordination number of oxygen with respect to titanium ion.

[0046] Titanium is most stable in its tetravalent form, and the crystal structure of titanium(IV) oxide is a titanium atom with six oxygen atoms coordinated to it, and the centers of the six oxygen atoms are connected to form an octahedron. This six-coordinate structure is a relatively stable structure for titanium oxide.

[0047] On the other hand, titanium oxide, in which four (or five) oxygen atoms are coordinated around a titanium atom, is in a coordination unsaturated state with two (or one) bonds open, making it unstable and highly reactive compared to a six-coordinated structure. The presence of such a four- or five-coordinated structure on the surface of a titanium oxide thin film allows the substrate to be adsorbed. In addition, in such a four- or five-coordinated structure, carriers are captured at the defective sites, but since this is temporary, the carriers tend to remain without recombining.

[0048] In the present invention, the inner region has a relatively large number of 6-coordinate structures, which reduces the number of crystal defects that act as recombination centers and suppresses recombination, while the surface region has a relatively large number of 4-coordinate structures, which provides an appropriate number of crystal defects that act as trap centers and makes it easier to retain carriers in the surface region.

[0049] Furthermore, in the intermediate region, the relatively predominant coordination number is gradually decreased from 6 to 5 to 4, resulting in a smooth band bending, which makes it easier for carriers generated in the relatively stable inner region to move to the relatively unstable surface region.

[0050] In the present invention, since the "non-crystalline structure" is a structure having many crystal defects, it is preferable to evaluate the degree of crystallinity based on the amount of crystal defects. In addition, in the present invention, since the crystal defects are considered to be caused by a decrease in the coordination number of oxygen to titanium ions, the degree of crystallinity can be evaluated by electron energy loss spectroscopy.

[0051] <Electron Energy Loss Spectroscopy> Electron Energy Loss Spectroscopy (EELS) is a spectroscopic technique that analyzes the composition of a sample and the bonding state of elements by measuring the energy lost when an incident electron beam excites electrons in the sample.

[0052] Specifically, a thin sample is irradiated with an electron beam, and an electron energy loss spectrum is obtained using a transmission electron microscope (TEM) or a scanning transmission electron microscope (STEM). The energy resolution of the TEM or STEM is preferably 1 eV or less, more preferably 0.5 eV or less. The lower limit is not particularly limited, but is usually 0.1 eV or more.

[0053] (Electron beam irradiation step) In the electron beam irradiation step, an electron beam is irradiated onto a thin sample prepared from a titanium oxide thin film formed on a substrate.

[0054] The method for preparing the thin specimen may be, for example, a method of cutting the specimen from a titanium oxide thin film using a microtome. From the viewpoint of electron transparency, the thickness of the thin specimen is preferably 200 nm or less, more preferably 100 nm or less. From the viewpoint of ease of handling, the thickness is preferably 10 nm or more, more preferably 50 nm or more.

[0055] The acceleration voltage for irradiating the electron beam is preferably adjusted appropriately according to the sample to be analyzed, and specifically, is preferably 30 kV or more, more preferably 100 kV or more, and is preferably 300 kV or less, more preferably 200 kV or less.

[0056] Other conditions for irradiating with electron beams (such as current amount and exposure time) are not particularly limited, and are preferably adjusted appropriately.

[0057] (Spectrum acquisition step) In the spectrum acquisition step, an energy loss spectrum is acquired for each microscopic region based on the energy of the electrons transmitted through the thin sample.

[0058] In the present invention, the spectral distribution is measured (TEM-EELS) using a transmission electron microscope. Specifically, slice samples are prepared every 2 nm in the direction from the thin film surface to the substrate, pixels are extracted from the TEM image of each slice sample, and the energy loss spectrum for each pixel is obtained by EELS. The size of the pixel is not particularly limited, and is preferably adjusted appropriately.

[0059] The degree of crystallinity can be evaluated and analyzed by comparing the spectrum distribution obtained by the above measurement method with the standard spectrum of each predicted structure. The comparison here is not of peak intensity but of the energy level (eV) at which the peak exists.

[0060] The presence or absence of a crystalline structure can also be evaluated by whether or not bright spots are observed in the diffraction image obtained by performing image analysis using a fast Fourier transform (FFT) on the TEM image of each of the above thin samples.

[0061] <Method for manufacturing titanium oxide thin film> The method for producing a titanium oxide thin film of the present invention includes a step of depositing a film by magnetron sputtering, and is characterized in that in the film depositing step, the maximum magnetic flux density in the direction perpendicular to the target surface is 0.14 T or more.

[0062] The titanium oxide thin film of the present invention is preferably formed directly on a substrate, as described below, and produced as a photocatalytic functional member.

[0063] Sputtering can form thin films of uniform thickness over a large area, and by appropriately adjusting the type of gas used, the total pressure of the sputtering atmosphere, the substrate temperature, and the like, thin films of various types can be formed.

[0064] Examples of the sputtering method include ion beam sputtering and magnetron sputtering, and magnetron sputtering is preferably used from the viewpoint of high sputtering efficiency. The "sputtering efficiency" refers to the efficiency at which atoms constituting the target are released from the target by the sputtering phenomenon.

[0065] Magnetron sputtering will now be described.

[0066] [Magnetron sputtering] Magnetron sputtering uses magnets to surround electrons in a magnetic field to create a dense plasma region, increasing the probability that argon atoms will collide with the target and increasing the speed at which they are deposited on the substrate.

[0067] Magnetron sputtering (hereinafter also simply referred to as "sputtering") includes DC (direct current) magnetron sputtering and RF (radio frequency) magnetron sputtering, and is not particularly limited in the present invention.

[0068] FIG. 2 shows the basic configuration of a magnetron sputtering apparatus used in the present invention. In magnetron sputtering, a magnet is placed on the back side of the target to generate a magnetic field. The titanium oxide thin film of the present invention can be obtained by increasing the magnetic flux density generated compared to conventional devices.

[0069] Specifically, the titanium oxide thin film of the present invention can be obtained by setting the maximum magnetic flux density in the direction perpendicular to the target surface to 0.14 T (1.4 kG) or more. It is more preferable that the maximum magnetic flux density in the direction perpendicular to the target surface is 0.14 T or more.

[0070] Since the maximum magnetic flux density in the perpendicular direction of the target surface is 0.14T (1.4kG) or more, it is exposed to Ar plasma, and the Ti-O bond is easily broken, and when the high-density Ar plasma hits the target, Ti sputtered particles fly to the substrate at a high density, which easily generates oxygen defects and titanium interstitial defects, and the crystallinity decreases. In the inner region of the thin film, crystallization occurs in a short time due to the heat generated by the energy relaxation of the flying sputtered particles, so the crystallinity is higher than that of the surface region, and it is thought that the coordination number of oxygen to titanium ions gradually decreases from the intermediate region to the surface region.

[0071] The maximum magnetic flux density in the direction perpendicular to the target surface can be adjusted by appropriately changing the strength of the magnet and the positional relationship between the magnet and the target. In the present invention, the maximum magnetic flux density was measured using a gauss meter (former FWBELL 620).

[0072] The sputtering target is not particularly limited as long as it contains titanium, and examples of the target include titanium alone, titanium oxide, titanium nitride, etc. From the viewpoint of sputtering efficiency, titanium alone is preferred.

[0073] The total pressure of the sputtering atmosphere during sputtering (hereinafter also referred to as "sputtering pressure") is preferably within the range of 0.1 to 1.0 Pa. By keeping the sputtering pressure within the above range, high crystallinity can be obtained, particularly in the inner region. The sputtering pressure can be accurately measured by an ionization vacuum gauge.

[0074] The method for producing a titanium oxide thin film of the present invention will be described in detail below with reference to a schematic diagram (FIG. 3) showing the main parts of one embodiment of a reactive RF magnetron sputtering apparatus used in the present invention. The basic configuration of the apparatus is similar to that of a known RF magnetron sputtering apparatus.

[0075] The "reactive sputtering method" refers to a method in which an active gas (oxygen in this invention) containing a composition component is mixed with a rare gas such as argon, and discharge sputtering is performed on a metal target (titanium in this invention) to form a film of a reaction product between the constituent components of the metal target and the active gas. In the present invention, it is preferable to perform sputtering in a plasma containing oxygen using elemental titanium as a target.

[0076] First, substrate 6 is placed at a predetermined position in chamber 51, and chamber 51 is evacuated using a vacuum exhaust system (not shown). Next, a mixed gas of argon and oxygen is introduced into chamber 51 via flow rate regulators 7 and 8. Here, the mixture ratio of oxygen and argon can be accurately controlled by the flow rates of the flow meters 7 and 8. Also, the sputtering pressure (in this case, the sum of the oxygen partial pressure and the argon partial pressure in the chamber) can be accurately adjusted by controlling the flow rates of oxygen and argon with flow rate regulators 7 and 8, and controlling the exhaust speed of a vacuum pump (not shown) connected to exhaust port 53 with a flow rate adjustment valve (not shown).

[0077] The placed substrate 6 is heated to a predetermined temperature by a halogen lamp 9. The substrate temperature is measured by a thermocouple 10 placed in the vicinity of the back surface of the substrate 6. Next, RF power is supplied to the cathode 11 to generate plasma 12. Here, the supply of RF power to the cathode 11 is controlled by an RF power supply 19.

[0078] By controlling the mixture ratio of oxygen and argon, the sputtering pressure, the RF power, and the substrate temperature (hereinafter also referred to as "film formation conditions") to predetermined values, argon and oxygen accelerated by plasma 12 and ionized collide with a target 13 made of titanium, causing the target material (titanium atoms) that is ejected to react with oxygen and form titanium oxide on the surface of substrate 6. A freely openable shutter 14 is provided near the surface of substrate 6, and when the plasma is unstable, such as at the beginning of plasma generation or when the film formation conditions are changed, shutter 14 is closed, and when the plasma is stabilized under the predetermined film formation conditions, shutter 14 is opened, thereby forming a thin film of titanium oxide on the surface of substrate 6.

[0079] The mixture ratio of oxygen and argon (oxygen:argon) is preferably within the range of 5:95 to 20:80. Within the above range, a titanium oxide thin film is formed on the substrate. The mixture ratio of oxygen and argon can be accurately controlled by controlling the oxygen flow rate and the argon flow rate with the flow rate regulators 7 and 8.

[0080] The RF power can be specified per unit area of ​​the target, and is 2.0 to 3.0 W / cm 2 By being within the above range, a stable plasma having sufficient energy can be formed.

[0081] The substrate temperature is preferably 600° C. or less, and more preferably 500° C. or less. By keeping the temperature at 600° C. or less, the phase transition from anatase type to rutile type of titanium oxide crystals can be suppressed.

[0082] The thickness of the formed titanium oxide thin film can be measured, for example, by a stylus surface profiler. This measuring instrument can detect surface irregularities by bringing a probe into vertical contact with the portion of the substrate on which the thin film is formed and detecting the vertical movement of the probe while scanning the surface, and can measure the thickness of the thin film as a step by scanning the probe vertically across the boundary between the thin film and the substrate.

[0083] <Photocatalytic functional materials> In the present invention, the term "photocatalytic functional member" refers to a component part having a photocatalytic function, which constitutes a structure such as electronic devices, automobiles, and furniture, which will be described later. For example, the term refers to a substrate such as a film, glass, or tile, whose surface is coated with the titanium oxide thin film of the present invention.

[0084] The substrate is limited to inorganic materials from the viewpoint of heat resistance. For example, substrates made of metals such as aluminum, stainless steel, and iron, as well as glass products and ceramic products such as tiles made of ceramic materials can be used. However, inorganic crystalline substrates made of crystals with high compatibility with the crystal lattice constant of titanium oxide, such as strontium titanate, magnesium oxide, and sapphire, cannot be used.

[0085] In particular, the substrate is preferably made of a material that is not decomposed by photocatalytic reactions. Substrates whose entirety or surface are made of organic materials may be decomposed by the oxidizing power of photocatalysts, so it is preferable to cover the substrate surface with a material that is not decomposed by photocatalytic reactions. Organic materials that are not easily affected by photocatalytic reactions, such as silicone resins, may not need to be covered in some cases.

[0086] An intermediate layer may be provided between the titanium oxide thin film of the present invention and the substrate. When an intermediate layer is provided, the internal surface refers to the surface in contact with the intermediate layer. The intermediate layer is provided, for example, for the purpose of suppressing damage to the substrate caused by photoexcitation of the photocatalytic film, and for the purpose of suppressing peeling, cracking, or warping of the photocatalytic film.

[0087] Examples of the intermediate layer include thin films made of metals such as chromium, aluminum, titanium, and iron, or alloys thereof; metal oxides such as silicon, aluminum, tantalum, cerium, indium, and tin; and metal fluorides such as calcium, magnesium, and aluminum. The intermediate layer may be a single layer or two or more layers laminated on the substrate. The intermediate layer may be functionalized by including a conductive material, a heat generating material, and the like.

[0088] The photocatalytic functional member of the present invention is not particularly limited, and can be used in, for example, air conditioners, air purifiers, electric fans, refrigerators, microwave ovens, dishwashers and dryers, rice cookers, pots, pot lids, induction heaters, washing machines, vacuum cleaners, lighting equipment (lamps, equipment bodies, shades, etc.), sanitary products, toilets, washstands, mirrors, bathrooms (walls, ceilings, floors, etc.), building materials (indoor walls, ceiling materials, floors, exterior walls, etc.), interior products (curtains, carpets, tables, chairs, sofas, shelves, beds, bedding, etc.), glass, sashes, handrails, doors, knobs, clothing, filters used in home appliances, stationery, kitchenware, interior spaces of automobiles, etc., to obtain cleaning, deodorizing, antibacterial, etc. effects. EXAMPLES

[0089] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they represent "parts by mass" or "% by mass" unless otherwise specified.

[0090] <Preparation of titanium oxide thin film> A titanium oxide thin film with a thickness of 460 nm was formed on a synthetic quartz substrate with a thickness of 1 mm by magnetron sputtering under the following conditions: Note that the magnetic flux density is the maximum magnetic flux density in the direction perpendicular to the target surface, as described above. Magnetic flux density: 0.145T (1.45kG) Total pressure: 1.0 Pa (argon partial pressure: 0.8 Pa, oxygen partial pressure: 0.2 Pa) Coating time: 4 hours Power: 200W Target: Titanium Target-substrate distance: 42mm Substrate temperature: 300℃

[0091] <Spectral distribution measurement by electron energy loss spectroscopy> Using a diamond cutter, two pieces measuring approximately 1 mm square were cut from the thin film, and the titanium oxide surfaces were placed facing each other with resin, and then the pieces were fixed with resin into a circular copper frame with a diameter of approximately 6 mm. Next, the sample was polished and dimpled to a thickness of approximately 20 μm at the center, and then ion milled until a hole was created in the center.

[0092] The spectral distribution was measured by electron energy loss spectroscopy using an atomic resolution analytical electron microscope (JEM-ARM200F, JEOL Ltd.). To obtain sufficient signal strength for data analysis, 20 spectra (2 nm deep) were integrated, and a spectrum was obtained every 2 nm from the surface of the titanium oxide thin film to the substrate. (Measurement conditions) Accelerating voltage: 200 kV Step: 1Å Data acquisition time: 0.5s

[0093] The spectrum obtained is shown in FIG. The spectral distribution was measured every 2 nm from the surface of the titanium oxide thin film to the substrate, and the obtained spectra were shifted along the vertical axis and plotted. Comparisons were made not based on peak intensity, but on the energy levels (eV) at which the peaks existed.

[0094] In the sample with lost electron energy in the range of 456 to 465 eV at a depth of 2 nm from the surface of the titanium oxide thin film toward the substrate (hereinafter simply referred to as "2 nm"), there was one loss peak. Similarly, there was one loss peak at 4 nm. At 6 nm or more, there were two loss peaks. Furthermore, the positions of the loss peaks at 2 nm and 4 nm were between the positions of the two loss peaks at 6 nm or more.

[0095] Simulations were performed for 1) extremely high crystallinity and 6-coordinate structure, 2) extremely high crystallinity and 4-coordinate structure, and 3) extremely low crystallinity and 4-coordinate structure. Within the range of lost electron energy of 456 to 465 eV, 1) had two loss peaks, while 2) and 3) had one loss peak. The loss peak position of 2) was on the lower energy side than the loss peak of 1), and the loss peak position of 3) was between the two loss peaks of 1).

[0096] From this, compared with the simulation, it is considered that the crystallinity is low and the 4-coordinate structure is relatively more prevalent in the region of 0-2 nm from the surface of the titanium oxide thin film toward the substrate, and the crystallinity is high and the 6-coordinate structure is relatively more prevalent in the region of 10-14 nm, and similarly in the region over 14 nm, the crystallinity is high and the 6-coordinate structure is relatively more prevalent.

[0097] <Observation by transmission electron microscope (TEM)> TEM images of the above samples (2 nm and 20 nm) obtained using a transmission electron microscope (JEM-ARM200F, JEOL Ltd.) were analyzed using Fast Fourier Transform (FFT) to obtain diffraction images, which revealed bright spots for the 20 nm sample but not for the 2 nm sample (Figure 5). In Figure 5, "surface" refers to the 2 nm sample and "inner" refers to the 20 nm sample.

[0098] The presence or absence of bright spots also indicates that in the titanium oxide thin film of the present invention, the inner region has high crystallinity and the surface region has low crystallinity.

[0099] <Acetaldehyde decomposition performance test> (Preparation of comparative samples) A titanium oxide thin film with a thickness of 460 nm was formed on a synthetic quartz substrate with a thickness of 1 mm and a size of 15 mm square by magnetron sputtering under the following conditions. Note that the magnetic flux density is the maximum magnetic flux density in the direction perpendicular to the target surface, as mentioned above. Magnetic flux density: 0.145T (1.45kG) Total pressure: 1.0 Pa (argon partial pressure: 0.8 Pa, oxygen partial pressure: 0.2 Pa) Coating time: 4 hours Power: 200W Target: Titanium Target-substrate distance: 42mm Substrate temperature: 300℃ The surface of this sample was etched by argon plasma to a depth of about 25 nm to remove the surface structure. The etching conditions were as follows: Argon pressure: 1.0Pa Power: 90W Etching time: 25 minutes

[0100] The obtained titanium oxide thin films were subjected to spectral distribution measurement using the above-mentioned electron energy loss spectroscopy. It was found that all samples had two loss peaks and that not only the internal region but also the surface region had high crystallinity and a relatively large number of 6-coordinate structures.

[0101] The titanium oxide thin film of the present invention and the comparative sample obtained above were placed in a container, and the container was filled with acetaldehyde so that the initial concentration was 50 ppm. Then, in an environment of 25±1°C and 50±5% RH, the container was irradiated with a light intensity of 100 mW / cm per unit time using UV LA-310UV-1 (manufactured by Hayashi Watch Co., Ltd.). 2 The container was irradiated with ultraviolet light for 120 minutes as a sample. Gas was collected from the container using a microsyringe, and the carbon dioxide concentration was measured using a gas chromatograph to calculate the concentration of remaining acetaldehyde.

[0102] The results are shown in Figure 6. The horizontal axis of the graph is the UV irradiation time, the left vertical axis is the acetaldehyde concentration, and the right vertical axis is the carbon dioxide concentration. The titanium oxide thin film functions as a photocatalyst, decomposing acetaldehyde and generating carbon dioxide.

[0103] In the graph, plots A and B show the change in acetaldehyde and carbon dioxide concentrations versus UV irradiation time in the titanium oxide thin film of the present invention, while plots C and D show the change in acetaldehyde and carbon dioxide concentrations versus UV irradiation time in the comparative sample.

[0104] As can be seen from the graph, when the titanium oxide thin film of the present invention is used, the concentration of acetaldehyde drops rapidly, whereas when the comparative sample is used, the concentration of acetaldehyde drops slowly. In other words, the titanium oxide thin film of the present invention has a higher photocatalytic activity than the comparative sample.

[0105] It has been conventionally believed that high photocatalytic activity can be obtained by increasing the crystallinity of a titanium oxide thin film, but it has been found that the titanium oxide thin film of the present invention exhibits even higher photocatalytic activity. [Explanation of symbols]

[0106] 6 Substrate 7 Flow regulator 8 Flow regulator 9 Halogen lamp 10 Thermocouples 11 Cathode 12. Plasma 13. Target 14 Shutter 19 RF power supply 51 Chamber 53 Exhaust port 100 Titanium oxide thin film 101 Surface area 102 Intermediate area 103 Internal area 104 Substrate A. Change in acetaldehyde concentration in the titanium oxide thin film of the present invention B. Change in carbon dioxide concentration in the titanium oxide thin film of the present invention C. Change in acetaldehyde concentration in the comparison sample D. Change in carbon dioxide concentration in the comparison sample

Claims

1. A titanium oxide thin film containing titanium oxide having photocatalytic activity, When one surface of the thin film is defined as a surface and the surface opposite to the surface is defined as an inner surface, the surface side region is a region within a range of 2 nm or less in a direction from the surface of the thin film to the internal surface, the inner region is a region within a range of 10 nm or more from the surface of the thin film in a direction toward the inner surface, titanium ions having an oxygen coordination number of 4 are present in greater amounts in the surface region than in the inner region; Titanium ions having a coordination number of oxygen of 6 are present in greater amounts in the inner region than in the surface region, and The inner region has a crystalline structure, and the surface region has a non-crystalline structure. A titanium oxide thin film characterized by:

2. In the titanium oxide thin film formed on a substrate, the surface side region is a region within a range of 2 nm or less in a direction from the surface of the thin film to the substrate, The inner region is a region within a range of 10 nm or more from the surface of the thin film in a direction toward the substrate to the inner surface in contact with the substrate.

2. The titanium oxide thin film according to claim 1 .

3. In the range of 456 to 465 eV of the energy loss spectrum of the titanium oxide thin film measured by electron energy loss spectroscopy, The inner region has two loss peaks, The surface side region has one loss peak, A loss peak position in the surface side region is between two loss peak positions in the inner side region.

3. The titanium oxide thin film according to claim 1 or 2.

4. A method for producing a titanium oxide thin film according to any one of claims 1 to 3, comprising the steps of: The method includes a step of forming a film by a magnetron sputtering method, In the film-forming step, the maximum magnetic flux density in the direction perpendicular to the target surface is 0.14 T or more. A method for producing a titanium oxide thin film comprising the steps of:

5. The titanium oxide thin film according to any one of claims 1 to 3 is provided. A photocatalytic functional member characterized by:

Citation Information

Patent Citations

  • Photocatalyst containing titanium oxide

    JP1999342344A

  • Member with antimicrobial function and its production

    JP2000186008A

  • Method for forming thin-film by plasma sputtering and film-forming apparatus

    JP2003301268A

  • Co2 reduction method, artificial photosynthesis induction substance and co2 reduction apparatus

    JP2004344720A