Ceramic nuclear fuel dispersed in an alloy matrix.

Incorporating ceramic particles in an alloy matrix for metallic nuclear fuel addresses the challenges of conventional fuels by ensuring efficient incineration and denaturing plutonium, providing safe and non-proliferation benefits while maintaining thermal conductivity and compatibility with existing databases.

JP7579127B2Active Publication Date: 2024-11-07ADVANCED REACTOR CONCEPTS LLC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2020205476
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2014-04-14
Filing Date
2020-12-11
Publication Date
2024-11-07
Estimated Expiration
2035-04-07

AI Technical Summary

Technical Problem

Conventional nuclear power plants face challenges in meeting increasing energy demands due to technical and public acceptance issues, and existing nuclear fuels require improvements to address environmental concerns and disposal of spent nuclear fuel.

Method used

The production of metallic nuclear fuel incorporating ceramic particles, such as pulverized light water reactor spent nuclear fuel, thorium oxide, and americium oxide, dispersed in an alloy matrix through processes like bottom pour casting, injection casting, and powder metallurgy, ensuring a continuous matrix of metal fuel with uniform ceramic distribution to maintain thermal conductivity and prevent resegregation.

Benefits of technology

This approach enables efficient incineration of transuranic elements, denatures plutonium isotopes, and provides nuclear non-proliferation benefits by creating a fuel composition unattractive for weapons, while maintaining compatibility with existing performance databases and ensuring safe operation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a method of fabricating a metal nuclear fuel pin.SOLUTION: A method of fabricating a metal nuclear fuel pin is provided, comprising: adding particulate metal nuclear fuel feedstocks; adding ceramic particles to the particulate metal nuclear fuel feedstocks; blending the crushed ceramic particles to the particulate metal nuclear fuel feedstocks to create a homogeneous mixture; and compacting the mixture into a steel cladding. In the method, the ceramic particles includes a composition having over approximately 90% uranium oxide with approximately 6% fission products and approximately 1.5% transuranics.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to nuclear fuels, and in particular to metallic nuclear fuels. [Background technology]

[0002] World electricity demand is expected to double by 2030 and quadruple by 2050. The increase in world electricity demand is projected to come from developed countries and, to a significant extent, from developing countries. Nuclear power would be a viable and cost-effective energy source to meet this rapid increase in demand.

[0003] Increasing energy supplies from other sources, such as contributions from natural gas electricity generation, will be constrained by concerns about high and volatile gas prices, greenhouse gas emissions, and long-term dependence on unstable sources. Meanwhile, alternative forms of energy (such as solar, wind, biomass, and hydroelectric) may be useful in meeting some of the growing demand. But they will not grow fast enough to provide enough additional electricity generating capacity in most markets to meet any significant portion of the new electricity demand.

[0004] Coal power plants would provide some additional supply, but burning large amounts of coal poses significant political obstacles given its adverse environmental impacts. Conventional nuclear power plants could meet some of the additional demand, but they entail many technical and public acceptance hurdles to overcome. New types of nuclear fuel would also be required.

[0005] Certain fast reactor-based power plants may have 20-year refueling intervals maintained by a closed fuel cycle based on pyrometallurgical recycling technology. For initial core loading, alloy fuel forms of U / Plutonium / Zr composition or enriched U / Zr composition can be used. Remote injection casting process can be used to manufacture the fuel pins. A very extensive irradiation database exists for the steady-state, transient and safety performance of fuel. Ternary alloy recycling pins can be highly radioactive and the technology for their manufacture using remote handling behind shielding at temperatures of 1500-1600 °C is well established. Summary of the Invention

[0006] An embodiment of the present invention may include a method for producing metallic nuclear fuel incorporating ceramic particles. In certain embodiments, the ceramic particles may include crushed light water reactor (LWR) spent nuclear fuel (SNF). In certain embodiments, the ceramic particles may include thorium oxide and / or americium oxide. In certain embodiments, materials from spent nuclear reactor fuel may be added to the alloy mixture. For example, ceramic particles such as light water reactor spent nuclear fuel may be crushed and dispersed in the matrix of the alloy.

[0007] U.S. Patent No. 8,571,167, U.S. Patent Application Publication No. 2011 / 0194666, and U.S. Patent Application Publication No. 2011 / 0206173 are each incorporated herein by reference in their entirety.

[0008] In certain embodiments, the ceramic oxide LWR-SNF particles can be combined with metallic fast reactor fuel by any of the following three processes: 1. Bottom pour casting fuel slugs. SNF fuel particles can be added to the molten metallic fuel charge prior to bottom pour casting of annular (or cylindrical) fuel slugs. The charge can be inductively heated using dual frequencies, and the change in frequency will result in mixing of the SNF particles in the melt. 2. Injection casting of solid fuel slugs. SNF fuel particles can be added to the molten metallic fuel charge prior to injection casting of solid, cylindrical fuel slugs. The charge would be heated as described in 1. 3. Powder metallurgy processes. Metallic fuel particles produced by powder metallurgy processes can be combined (mixed) with SNF fuel particles.

[0009] The maximum amount of SNF fuel particles that can be added to the metallic fuel must be an amount that results in a continuous matrix of metallic fuel. Regardless of which manufacturing process is used, after brief irradiation, the fuel microstructure can be made identical, substantially identical, and / or functionally identical to the microstructure of injection cast fuel without the milled ceramic particles. Thus, an extensive database of injection cast fuel without the SNF particles would provide a good guide to expected irradiation throughput.

[0010] The process details and attributes of each process for producing fuel rods are described below. Each process contributes to solving the SNF problem by burning off the transuranium elements over multiple recycles, and all of them will denature Pu239 in the process. In certain embodiments, fuel rods can be produced using reprocessed metal fuel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Bottom pouring casting In certain installations, bottom casting techniques can be used to produce slugs for insertion into steel clad fuel pins. The slugs can be annular zirconium (Zr) sheathed slugs. Upon irradiation, the as-fabricated pins can be rapidly reconstructed to the traditional morphology produced by the original injection casting manufacturing process, so that the current extensive performance database for such fuel pins still applies.

[0012] Although the following description is directed to an exemplary embodiment for manufacturing annular fuel pins, it should be understood that bottom pour casting can be used to manufacture any of a variety of fuel pins, including cylindrical or other shaped fuel pins.

[0013] The raw materials for the annular fuel pins can be charged into a bottom pouring crucible and melted in an induction furnace. Melting times, temperatures, pressures, and other operating conditions can be selected based on the raw materials being charged. The raw materials can be selected to obtain the desired composition of metallic uranium (U) and transuranic elements as well as molybdenum (Mo) and / or zirconium (Zr). In certain embodiments, the raw materials include, for example, uranium, zirconium, transuranic elements, reprocessed metallic fuel, and combinations thereof. In certain embodiments, a preformed thin-walled zirconium tube can be inserted into an interference-fit hole in a graphite mold. A rod can be placed in the center of the hole in the graphite mold. The plug at the bottom of the crucible can be raised and the alloy melt will flow into the mold and solidify.

[0014] In this manner, in certain embodiments, an annular fuel pin slug can be produced that is radially surrounded by Zr cladding. The annular fuel pin slug can be removed from the mold and inserted into an interference fit steel cladding. End caps can be welded on. Bundles of such pins can be assembled into multi-pin fuel assemblies.

[0015] In certain embodiments, a charge of ground ceramic particles can be added to the melt after the metal melt is in a molten state. The frequency of the induction furnace can be adjusted to create a turbulent flow regime of the molten metal. The turbulent flow regime will help the ceramic particles to mix uniformly in the molten metal phase. Induction heating of U / Plutonium / Zirconium and U / Zr is known from current injection casting processes, and it is also known that the turbulent flow regime can be created by adjusting the frequency.

[0016] After a period of time, the agitation can be stopped. The length of time for agitation can be selected to achieve uniform or near-uniform mixing of the mixture. Underpouring can be performed as described above.

[0017] Freezing the mixture (preferably rapidly) will prevent resegregation of the relatively low density ceramic from the metallic phase. The time and temperature of cooling can be selected to prevent resegregation.

[0018] The resulting fuel slug will be a Zr-sheathed annular slug of cermet composition, with the fissile alloy forming a continuous matrix, with the majority of the fissile mass present as metallic phase. The ratio of metal fuel to ceramic can be selected such that upon irradiation, the fuel pin will produce a continuous matrix of metal fuel, thereby ensuring sufficient thermal conductivity. In certain embodiments, the dispersed ceramic particles will have a composition of greater than about 90% uranium oxide, about 6% fission products, and about 1.5% transuranium elements. These casting operations can be performed remotely, which is typically required when manufacturing with light water reactor spent nuclear fuel.

[0019] There are many potential operational advantages to annular fuel compacts, and providing the ability to manage spent nuclear fuel would provide further benefits. Injection casting In certain installations, known injection casting techniques have been used to produce solid (i.e., non-annular) slugs for insertion into steel clad fuel pins. The slugs can be solid fuel slugs that are inserted into a loose fit steel cladding and sodium, and are bonded to the sodium to provide good thermal conductivity between the slug and the cladding. Upon irradiation, the as-fabricated pins can be rapidly reconstructed into conventional fission gas filled porous configurations produced by the injection casting manufacturing process, to which an extensive current performance database is applied.

[0020] In certain embodiments, the injection casting process can be modified to incorporate ceramic particulates, such as crushed light water reactor spent nuclear fuel, into metal fuel pins. The raw materials for the fuel pins can be loaded into a crucible and melted in an induction furnace. The raw materials can be selected to obtain the desired composition of metallic uranium (U), transuranium elements, and / or zirconium (Zr).

[0021] In certain embodiments, a feedstock of ground ceramic particles can be added to the melt after the metal melt is in a molten state. The frequency of the induction furnace can be adjusted to create a turbulent flow regime of the molten metal. The turbulent flow regime will aid in the uniform mixing of the ceramic particles into the metal phase.

[0022] After a period of time, the agitation can be stopped. The length of time for agitation can be selected to achieve uniform or near uniform mixing of the mixture. An injection molding process can be performed to force the melt into a mold.

[0023] Cooling (preferably rapid cooling) of the mixture in the mold will prevent resegregation of the relatively low density ceramic from the metallic phase. The time and temperature of cooling can be selected to prevent resegregation.

[0024] The resulting fuel slug will be a solid fuel pin of cermet composition with approximately greater than 50% by volume of fissile bearing metal matrix, with the majority of the fissile material present as the metallic phase. The ratio of metal fuel to ceramic can be selected such that upon irradiation, the fuel pin will produce a continuous matrix of metal fuel (permeated with fission gases) to ensure sufficient thermal conductivity. In certain embodiments, the dispersed ceramic particles will have a composition of greater than about 90% uranium oxide, about 6% fission products, and about 1.5% transuranium elements. These injection casting operations can be performed remotely, which is typically required when manufacturing with light water reactor spent nuclear fuel.

[0025] Powdered fuel metallurgy Powder metallurgy facilitates the production of cermet fuel compositions, whereby ceramic particles can be embedded in a matrix of metallic phases. This capability, as well as the production methods of cermet fuel pins by bottom pouring and injection casting, allows the selection of crushed ceramic fuels, such as LWR spent fuel, and the introduction of crushed ceramic fuels into the closed fuel cycle that sustains fast reactor-based power plants. This would provide an effective solution for dealing with the difficult LWR spent fuel disposal problem. By limiting the volume fraction of the ceramic phase, it would be possible to maintain the applicability of previous fuel performance databases.

[0026] Fuel characteristics In all three embodiments, there will be a range of ceramic volume fractions that must be ensured to maintain applicability of previous databases for metallic fuel, maintain acceptable thermal conductivity ranges, and achieve the required level of fissile density. For enriched U / Zr initial fuel charges, the ceramic volume fraction will be such that there is a continuous metal matrix. For U / Pu / Zr recycled fuel charges, the ceramic weight fraction will be approximately 10 wt.% (this is just enough to recover the weight fraction of the burned heavy metals).

[0027] Established methods are known for comminution of LWR spent fuel, capture of released gaseous fission products, and tailoring of particle size distribution. Particle size may average between about 1 micron and about 100 microns. Uniform distribution of ceramic particles within the as-cast pin may be a relevant consideration for the present disclosure.

[0028] Regarding wetting, small amounts of ceramic contamination from impurities have been found in fuel pins manufactured by current injection casting manufacturing processes. Wetting could be achieved by these processes.

[0029] Regarding particle agglomeration, even if ceramic particle agglomeration occurs during manufacturing, some degree of agglomeration will not significantly degrade core performance because particle agglomeration does not lead to the formation of high fission density "hot spots" in the fuel, since enrichment in LWR spent nuclear fuel particles is about 1-2%, while enrichment in the metallic matrix would be greater than about 10%. Agglomeration may lead to the formation of localized "cool spots", but this does not pose a performance problem. Even if the manufacturing process never results in perfect homogeneity, hot spot problems will not occur.

[0030] Furthermore, the swelling of the core will not result in particle agglomeration. During approximately the initial 1-1.5% of the core burnup, fission gas microbubbles will form and the ductile metallic phase matrix will flow into the approximately 25% free volume, which exists in the central hole for annular pins, in the gap between the fuel slug and the cladding for injection cast pins, and in the open pores for powder metallurgy manufactured fuel. The flow of the metallic matrix will entrain the embedded ceramic particles, thereby increasing the average separation distance between the particles. Agglomeration will not be induced.

[0031] The ceramic particles will be primarily U238. U238 can be responsible for negative Doppler reactivity feedback during power-up transients. In some reactor configurations, the thermal time constant of the low thermal conductivity ceramic particles will prevent the rapidity of the negative reactivity feedback. However, its effect on other types of fast reactor transient performance will be negligible for several reasons. First, Doppler will not be the dominant reactivity feedback in (small) fast reactors. Instead, radial thermal expansion will dominate. Second, in the recycle charge, more than about 80% of the U238 (more than about 65% of the U238 in the initial fuel charge) will be present in the matrix of the metallic phase of the cermet fuel, in which case the heating will be instantaneous or near instantaneous. The rapid feedback from the metallic phase will dominate over the slightly delayed feedback from the ceramic phase. In addition, the ceramic particles will be very small, from about one micron to about several hundred microns, and will be well bonded to the surrounding metallic phase. Therefore, the thermal time delay of the ceramic particles will be very small.

[0032] Safeguards and the Benefits of Nuclear Non-Proliferation Introducing crushed LWR spent fuel particles into the alloy fuel pins would provide a nuclear non-proliferation benefit. This benefit would be especially advantageous for the initial core charge, which is enriched below 20% uranium and does not contain any transuranic elements (which are non-radioactive in themselves). For the initial core, after irradiation, the resulting fuel composition will contain plutonium enriched in Pu239, but without substantial contamination with Pu240 and Pu241, whereas the recycled core, on the other hand, will form a mixture of plutonium isotopes that would be unattractive for weapons use. Thus, adding crushed LWR-SNF to the initial charge could provide several nuclear non-proliferation benefits.

[0033] First, oxide particles from pulverized LWR spent fuel contain fission products that provide a self-protecting radiation field for the initial core charge, which is initially non-radioactive alloy-enriched uranium / Zr fresh fuel that is not protected by a radiation field during its operation in the reactor.

[0034] Importantly, the ceramic particles can contain the isotopes Pu240 and Pu241. The particle size would be small enough, and the temperature of the fuel high enough, that significant migration of the isotopes would occur across all particle-matrix interfaces when bombarded with radiation in a nuclear reactor. Thus, Pu240 and Pu241 atoms can enter the metal matrix and intimately mix with the newly grown Pu239 (and vice versa) in the metal matrix. (Any oxygen that migrates to the metal phase will be "gettered" by Zr.) Thus, the newly grown Pu239 would become contaminated with Pu240 and Pu241 after only a short exposure in a nuclear reactor, which would make it unattractive for use in nuclear weapons.

[0035] The "modification" with Pu240 and Pu241 in the initial core load will be important because in that initial load the volume fraction of ceramics will approach about 50% and the weight fraction of heavy metals will be about 35%. In LWR spent fuel the weight fraction of plutonium will be about 1.5% and the weight fraction of plutonium and the (240+241) / (239+240+241) isotopic contamination of Pu239 will be about 40%. On the other hand, the corresponding asymptotic composition of the fast reactor obtained after multiple recycling will be about 25%.

[0036] After an initial 20-year irradiation period achieving approximately 8 atomic percent burnup, the initial fuel charge will have progressed approximately 10% of the way through the fissile composition, with all of the fissile composition being U235 to Pu. The Pu239 composition will have progressed from being 239-enriched to an asymptotic (240+241) contamination of Pu239.

[0037] After the first 20-year irradiation period, the initial fuel charge in the metallic phase would contribute, for example, (100-35 wt.% fuel) x (13 wt.% fissile in fuel) x (1 / 10 Pu in fissile) = 0.00845 to the breeding charge of Pu239 atoms in the fuel.

[0038] The ceramic would, for example, contribute (35 wt% fuel) x (1.5% Pu in fuel) x (40% in Pu 240 + 241) = 0.00845 to a charge of (240 + 241) atoms for each atom of Pu in the fuel.

[0039] Thus, if complete mixing were to occur, the (240+241) / (239+240+241) ratio of the cermet fuel at the time of discharge would be, for example, approximately (0.0021) / (0.00845+0.0021)=0.199. This may be considered as an asymptotic value already modified. The mixing of isotopes can be achieved by taking into account the temperature and temperature gradient of the fuel pin, the intense radiation field, and the length of time of exposure to these conditions. The migration of isotopes across the ceramic-metal interface would result in a homogeneous mixture with the multiplied Pu239. Thus, even for the first fuel charge, a significant substantial modification would be obtained. The effect would be less for the recycled fuel charge. Because the ceramic weight fraction would be reduced to about 8-10 wt%, but by that time the Pu would already be modified and the recycled fuel could be loaded with the radioactive fission products retained in the recycling process.

[0040] It should be noted that while the above description is directed to preferred embodiments of the invention, other variations and modifications will be apparent to those skilled in the art and may be made without departing from the spirit or scope of the invention. Moreover, an embodiment described with respect to one embodiment of the invention may be used in combination with other embodiments, even if not expressly stated above.

[0041] The claims of the parent application of this divisional application as filed are as follows: [1] A method for manufacturing a cermet metal fuel matrix nuclear fuel pin, comprising the steps of: melting one or more metallic nuclear fuel sources, thereby forming a molten metal melt; adding ceramic particles into a melt of molten metal, thereby forming a mixture; Stir the mixture vigorously; pouring the mixture into a mold; and allowing the mixture to solidify in the mold, thereby forming a cermet metal fuel matrix nuclear fuel pin; The method comprising: [2] The method of [1], wherein the stirring comprises turbulence of the mixture to thereby achieve a substantially uniform distribution of the particles. [3] The method according to [1], wherein the ceramic particles include pulverized light water reactor spent nuclear fuel, thorium oxide, americium oxide, and combinations thereof. [4] The method of [1], wherein the ceramic particles include thorium oxide, americium oxide, and combinations thereof. [5] The method according to [1], wherein the mold has a cylindrical hole and the rod is located approximately at the center of the cylindrical hole. [6] The method according to [5], wherein the obtained cermet metal fuel matrix nuclear fuel pin is an annular cermet metal fuel matrix nuclear fuel pin. [7] The method of [1], wherein the mold includes one or more zirconium tubes fitted within cavities in the mold. [8] The method according to [7], wherein the resulting fuel pin is a zirconium sheathed cermet metal fuel matrix nuclear fuel pin. [9] The method described in [1], wherein the distribution of ceramic particles within the cermet metal fuel matrix remains uniform after solidification by rapid cooling of the mixture.

[10] The method of [1], wherein the one or more metallic nuclear fuel sources include uranium.

[11] The method of [1], wherein the one or more metallic nuclear fuel sources comprise (i) uranium, and (ii) zirconium or molybdenum.

[12] The method of [1], wherein the one or more metallic nuclear fuel sources comprise a mixture of uranium and transuranium elements.

[13] A method for manufacturing a cermet metal fuel matrix nuclear fuel pin, comprising the steps of: melting one or more metallic nuclear fuel sources, thereby forming a molten metal melt; adding ceramic particles into a melt of molten metal, thereby forming a mixture; Stir the mixture vigorously; injection casting the mixture into a mold; and allowing the mixture to solidify in the mold, thereby forming a cermet metal fuel matrix nuclear fuel pin; The method comprising:

[14] The method of

[13] , wherein the stirring comprises agitating the molten metal melt to thereby achieve uniform mixing of the ceramic particles within the molten metal melt.

[15] The method of

[13] , wherein the crushed ceramic particles comprise light water reactor spent nuclear fuel.

[16] The method of

[13] , wherein the ground ceramic particles comprise thorium oxide.

[17] The method of

[13] , wherein solidifying the mixture is by cooling.

[18] The method of

[13] , wherein the one or more metallic nuclear fuel sources include uranium.

[19] The method of

[13] , wherein the one or more metallic nuclear fuel sources include uranium and zirconium.

[20] The method of

[13] , wherein the one or more metallic nuclear fuel sources comprise a mixture of uranium and transuranium elements.

[21] A method for manufacturing metal nuclear fuel pins, comprising the steps of: adding granular metallic nuclear fuel material; Adding ceramic particles to granular metallic nuclear fuel feedstock; mixing the pulverized ceramic particles with a granular metallic nuclear fuel feedstock, thereby forming a homogeneous mixture; and pouring the mixture into a steel sheath and allowing it to harden; The method comprising:

[22] The method of

[21] , wherein the ceramic particles include pulverized light water reactor spent nuclear fuel.

[23] The method of

[21] , wherein the milled ceramic particles include thorium oxide, americium oxide, and combinations thereof.

[24] The method of

[21] , wherein the one or more metallic nuclear fuel sources comprise particles of uranium.

[25] The method of

[21] , wherein the one or more metallic nuclear fuel sources comprise particles of uranium and zirconium.

[26] The method of

[21] , wherein the one or more metallic nuclear fuel sources comprise a mixture of particles of uranium and transuranium elements.

Claims

1. 1. A method for manufacturing metal nuclear fuel pins comprising the steps of: adding granular metallic nuclear fuel material; adding crushed ceramic particles to a granular metallic nuclear fuel feedstock; mixing the granular metallic nuclear fuel feedstock with the crushed ceramic particles, thereby forming a homogeneous mixture; and placing the mixture into a steel sheath; Including, the crushed ceramic particles have a composition including greater than 90% uranium oxides, 6% fission products, and 1.5% transuranium elements; The method wherein the crushed ceramic particles have an average particle size between 1 micron and 100 microns.

2. The method of claim 1 , wherein the pulverized ceramic particles comprise pulverized light water reactor spent nuclear fuel.

3. The method of claim 1 , wherein the crushed ceramic particles include thorium oxide, americium oxide, and combinations thereof.

4. The method of claim 1 , wherein the metallic nuclear fuel source comprises particles of uranium.

5. The method of claim 1 , wherein the metallic nuclear fuel source comprises particles of uranium and zirconium.

6. 10. The method of claim 1, wherein the metallic nuclear fuel source comprises a mixture of uranium and transuranium particles.

Citation Information

Patent Citations

  • Pellet of MOX fuel and its filling

    JP1990236197A

  • Particulate metal fuels used in power generation, recycling systems, and small modular reactors.

    JP2012529051A