Zinc alloy plated steel and its manufacturing method
A zinc alloy-plated steel material with a controlled microstructure and cooling process enhances corrosion resistance in both cross-sections and processed parts, addressing brittleness issues in Zn-Al-Mg alloys.
Patent Information
- Application Number
- JP2020535192
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-12-26
- Filing Date
- 2018-12-13
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2038-12-13
AI Technical Summary
Existing zinc alloy-plated steel materials face issues with reduced corrosion resistance in processed parts due to brittleness and damage to the plating layer, particularly in Zn-Al-Mg alloys, which are more prone to cracking during machining.
A zinc alloy-plated steel material with a specific microstructure comprising a Zn phase, MgZn phase, and Al phase, along with a suppression layer of intermetallic compounds like Fe4Al13 and Fe2Al5, is formed with controlled cooling and wiping processes to ensure a ternary alloy phase layer at the interface, enhancing corrosion resistance.
The material achieves excellent corrosion resistance in both cross-sections and processed parts, preventing discoloration and maintaining surface quality, expanding its usable areas.
Smart Images

Figure 0007579142000005 
Figure 0007579142000006 
Figure 0007579142000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a plated steel material that can be used in automobiles, home appliances, building materials, etc., and more particularly to a zinc alloy plated steel material having excellent surface quality and corrosion resistance, and a method for producing the same. [Background technology]
[0002] Zinc plating, which inhibits corrosion of iron through cathodic protection, is widely used to manufacture steel materials with excellent corrosion resistance and cost-effectiveness. In particular, hot-dip galvanized steel materials, in which a plating layer is formed by immersing a steel material in molten zinc, have a simpler manufacturing process and a lower product price than electrolytic galvanized steel materials, and therefore demand for hot-dip galvanized steel materials is increasing across industries such as automobiles, home appliances, and building materials.
[0003] When hot-dip galvanized steel is exposed to a corrosive environment, zinc, which has a lower redox potential than iron, corrodes first, suppressing the corrosion of the steel, providing a sacrificial corrosion protection property. Furthermore, the zinc in the coating layer is oxidized to form dense corrosion products on the steel surface, isolating the steel from the oxidizing atmosphere and improving the corrosion resistance of the steel.
[0004] However, with the advancement of industry, the worsening of air pollution and corrosive environments, and strict regulations on resource and energy conservation, there is an increasing need to develop steel materials with better corrosion resistance than conventional zinc-plated steel materials. As part of this, various researches are being conducted on manufacturing technologies for zinc alloy-plated steel materials that improve the corrosion resistance of steel materials by adding elements such as aluminum (Al) and magnesium (Mg) to the zinc plating bath. Active research is being conducted on manufacturing technologies for Zn-Al-Mg-plated steel materials, which are representative zinc alloy-plated steel materials, in which Mg is additionally added to the Zn-Al plating composition (Patent Document 1).
[0005] Many plated steel materials used in industry are often manufactured into final products by undergoing various processes such as cutting, bending, and stretching. In this case, there is a problem that the base steel is exposed on the cut surface or processed surface, or the plating layer is damaged, resulting in a decrease in corrosion resistance. In particular, in the case of Zn-Al-Mg alloy plating, the plating layer is more brittle than general zinc plating, so the processed surface can be weaker. However, there has not been much research on improving the corrosion resistance of the processed parts. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2002-332555 A Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a zinc alloy plated steel material having excellent surface quality and capable of ensuring excellent corrosion resistance not only in cross sections but also in processed areas, and a method for producing the same.
[0008] The problems to be solved by the present invention are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]
[0009] One aspect of the present invention relates to a zinc alloy plated steel material having excellent surface quality and corrosion resistance, comprising: a base steel; a zinc alloy plating layer formed on the base steel; and an inhibition layer formed between the base steel and the zinc alloy plating layer, wherein a Zn phase on a surface of the zinc alloy plating layer accounts for 15 to 90% by area; and a ternary alloy phase layer of Zn / MgZn2 / Al formed on the inhibition layer to a thickness of 2 μm or less, the ternary alloy phase layer being formed in a proportion of 30 to 90% of a total area.
[0010] Another aspect of the present invention relates to a method for producing a zinc alloy-plated steel material having excellent surface quality and corrosion resistance, comprising the steps of providing a base steel, immersing the base steel in a coating bath to coat the base steel, and wiping and cooling the plated base steel, the cooling step satisfying the following relational expression 1: [Equation 1] 0.7Vc≦Vc'≦1.5Vc Here, Vc is the cooling rate until solidification of the coating layer is completed immediately after wiping, and Vc' is the cooling rate until solidification of the coating layer begins immediately after wiping. Effect of the Invention
[0011] According to the present invention, it is possible to provide a zinc alloy plated steel material and a manufacturing method thereof, which can prevent discoloration of the plated layer surface, ensure excellent surface characteristics, and have excellent corrosion resistance not only at the cross section but also at the processed portion, and which has the advantage of being able to expand the range of use to areas where use was previously limited. [Brief description of the drawings]
[0012] [Figure 1] 1 is a photograph showing a cross section of a plating layer in Example 3 of the present invention. [Diagram 2] 1 is a photograph showing a cross section of a plating layer in Comparative Example 2 of an embodiment of the present invention. [Diagram 3] This is a photograph in which the ternary alloy phase layer of Zn / MgZn2 / Al formed on the inhibition layer in the photograph of FIG. 1 is observed. [Figure 4] FIG. 2 is a schematic diagram showing a plated steel material and a wiping nozzle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] While normal zinc plating solidifies as a single Zn phase, Zn-Al-Mg zinc alloy plating consists of a coexistence of Zn phase, Mg and Zn alloy phase, Al phase, etc. This plating structure forms a very complex plating structure depending on the trace elements in the plating bath and the physical and chemical state of the base steel surface caused by the manufacturing process, etc.
[0014] The alloy phases of Zn and Mg in the plating structure of the Zn-Al-Mg zinc alloy plating layer (hereinafter referred to as the zinc alloy plating layer or plating layer) are MgZn2, Mg2Zn 11 The coating layer may be made of various intermetallic compounds such as Fe and Al, and the hardness of these compounds reaches Hv250 to 300. An inhibition layer made of an intermetallic compound of Fe and Al may be formed at the interface between the coating layer and the base steel. The intermetallic compound of Fe and Al is Fe4Al. 13 , Fe2Al5, etc. These intermetallic compounds are also highly brittle, so they are prone to cracking in the plating layer when physically deformed.
[0015] The zinc alloy plated steel material of the present invention includes a base steel, a zinc alloy plated layer formed on the base steel, and an inhibition layer formed between the base steel and the zinc alloy plated layer.
[0016] The composition of the zinc alloy plating layer is not particularly limited, but a preferred example contains, by weight, 0.5 to 3.5% Mg, 0.5 to 20.0% Al, and the remainder Zn and unavoidable impurities.
[0017] The magnesium (Mg) plays a very important role in improving the corrosion resistance of zinc-based plated steel materials, and effectively prevents corrosion of the zinc-based plated steel materials by forming a dense zinc hydroxide-based corrosion product on the surface of the plating layer in a corrosive environment. To achieve this effect, the magnesium content is preferably 0.5% by weight or more, and more preferably 0.8% by weight or more. However, if the content is excessive, there is a problem that Mg oxide dross rapidly increases on the surface of the plating bath. To prevent this, the magnesium content is preferably 3.5% by weight or less, and more preferably 2.0% by weight or less.
[0018] The aluminum (Al) suppresses the formation of Mg oxide dross in the coating bath and reacts with Zn and Mg in the coating bath to form a Zn-Al-Mg intermetallic compound, thereby improving the corrosion resistance of the plated steel. In order to obtain the above effects, the Al content is preferably 0.5% by weight or more, and more preferably 0.8% by weight or more. However, if the content is excessive, the weldability and phosphating property of the plated steel may deteriorate. In order to prevent this, the Al content is preferably 20.0% by weight or less, and more preferably 6.0% by weight or less, and in order to speed up the solidification behavior of the coating bath, it is more preferably 3.0% by weight or less.
[0019] The remainder includes zinc (Zn) and inevitable impurities.
[0020] In the zinc alloy plated steel sheet, an inhibition layer, a so-called inhibition layer, is formed between the zinc alloy plated layer and the base steel. The inhibition layer is an intermetallic compound of Fe and Al (e.g., Fe4Al 13 , Fe2Al5, etc.). The inhibition layer is composed of fine crystal grains, but if the crystal grains are coarse, the inhibition layer becomes brittle. Therefore, when external stress is applied to the steel sheet, the inhibition layer is destroyed, and there is a concern that the plating layer may peel off or the corrosion resistance may decrease due to processing cracks. Therefore, the crystal grain size of the inhibition layer is preferably 300 nm or less, and the average crystal grain size is preferably 100 nm or less.
[0021] A ternary alloy phase layer of Zn, MgZn2, and Al formed with a thickness of 2 μm or less is preferably formed on the inhibition layer. At the interface between the base iron and the zinc alloy plating layer, a sacrificial cathodic reaction is initiated primarily in a corrosive environment. When such a ternary alloy phase is formed at the interface between the base iron and the zinc alloy plating layer, when the cross section of the product is exposed to a corrosive environment, the effect of sacrificial corrosion protection increases from the interface, and the effect of sacrificial corrosion protection is continuously produced. This is because Zn and Mg, which mainly participate in sacrificial corrosion protection, and Al, which is advantageous for the formation of a passive film, are concentrated at the interface between the plating layer and the base iron. The ternary alloy phase layer is preferably formed on the inhibition layer, and is preferably formed over 30% or more of the total area. However, if it is formed excessively, the hardness of the upper part of the plating layer is reduced, and the friction properties of the plating layer may be deteriorated, so it is preferable that the layer does not exceed 90%. As an example of a method for confirming the ternary alloy phase layer, a method of confirming the ternary alloy phase layer by enlarging the cross section magnification with a scanning electron microscope (SEM) or a transmission electron microscope (TEM) can be mentioned. Another method is to dissolve the plating layer in an aqueous solution of hydrochloric acid (HCl) and then observe the surface to observe the ternary alloy phase layer remaining on the top of the inhibition layer. On the other hand, when observing the cross section, it is also possible to measure the length of the inhibition layer along the boundary of the cross section, where the ternary phase is formed on the inhibition layer.
[0022] If the thickness of the ternary alloy phase layer of Zn, MgZn2, and Al formed on the inhibition layer exceeds 2 μm, the sacrificial corrosion protection effect at the interface between the base steel and the zinc alloy plating layer decreases, and the effect of improving the corrosion resistance of the cross section also decreases. Therefore, it is important to adjust the material state and cooling conditions so that the thickness of the ternary alloy phase layer does not exceed 2 μm.
[0023] The zinc alloy plating layer is a Zn phase, an alloy phase of Mg and Zn (e.g., MgZn2, Mg2Zn 11etc.), and Al phase. The microstructure observed on the surface of the zinc alloy plating layer of the present invention preferably contains 15 to 90% of Zn phase in terms of area fraction. The microstructure appearing on the surface of the plating layer is very closely related to the surface characteristics of the plating layer. If the proportion of Zn phase on the surface of the plating layer is small, there is a problem that the hue of the plating surface darkens due to the effect of Mg oxidation during long-term storage of the plated steel sheet, so the Zn phase on the surface is preferably 15% or more. On the other hand, if the proportion of Zn phase exceeds 90%, excessive cooling is required, which is undesirable as it reduces productivity.
[0024] As described above, the zinc alloy plating layer contains various phases, among which the Zn phase and the MgZn2 phase may contain a binary phase having a lamellar structure. In the zinc alloy plating layer of the present invention, the average widthwise thickness of the Zn phase and the MgZn2 phase in the lamellar structure of the Zn phase and the MgZn2 phase contained in the zinc alloy plating layer is preferably 1.5 μm or less. Since the MgZn2 phase is more brittle than the Zn phase, when the structure of the lamellar structure is formed coarsely, there is a high possibility of destruction due to external stress. Therefore, the average widthwise thickness of the Zn phase and the MgZn2 phase in the lamellar structure of the Zn phase and the MgZn2 phase formed from the surface to the inside of the plating layer is preferably 1.5 μm or less (excluding 0). The lamellar structure of the Zn phase and the MgZn2 phase contained in the zinc alloy plating layer is preferably a lamellar structure that exists on the surface of the zinc alloy plating layer up to 70% of the plating layer. The widthwise thickness can be determined by measuring 10 or more points of the lamellar structure present in the plating layer to obtain an average value.
[0025] An embodiment of the method for producing a zinc alloy-plated steel material of the present invention will be described in detail below. The method for producing a zinc alloy-plated steel material of the present invention includes providing a base steel, immersing the provided base steel in a plating bath to plate it, wiping it, adjusting the thickness of the plating layer, and cooling it.
[0026] When preparing the base iron, it is preferable to first make the metal structure of the hot-rolled steel uniform. For this purpose, the average grain size of the hot-rolled steel is preferably 1 to 100 μm. The grains of the hot-rolled steel are preferably in the surface layer (within 1 / 8 of the total thickness based on the surface). When the structure of the hot-rolled steel, particularly the surface structure, is nonuniform, the inhibition layer is not formed uniformly due to the nonuniformity of the surface shape during cold rolling and the nonuniform diffusion of Fe from the base iron required for the formation of the inhibition layer, and the ternary phase formed on the upper part of the inhibition layer is also formed nonuniformly, which may reduce the corrosion resistance of the cross section. For this purpose, the average grain size of the hot-rolled steel is preferably 1 to 100 μm. More preferably, the grain size is 1 to 50 μm or 5 to 30 μm.
[0027] When the grain size of the hot-rolled steel is less than 1 μm, it is advantageous for ensuring strength, but the surface roughness due to the grains may increase during cold rolling. On the other hand, when the grain size exceeds 100 μm, it is advantageous for homogenizing the shape, but there is a concern that scale defects may occur due to an excessive increase in the hot rolling temperature, and the manufacturing cost of the product may also increase. As an example of a method for obtaining the grain size of the hot-rolled steel, there is a method of maintaining the hot rolling temperature at a minimum of 800° C. or higher, or increasing the coiling temperature after hot rolling to 550° C. or higher.
[0028] When the above hot rolled steel material is cold rolled to produce a cold rolled steel material, it is preferable to produce the cold rolled steel material so that the surface roughness (Ra) of the cold rolled steel material is 0.2 to 1.0 μm and the steepness is 0.2 to 1.2.
[0029] The surface roughness is determined according to the pressure and surface shape of the roll when the roll rolls the material. If the surface roughness exceeds 1.0 μm, the roughness becomes large and a non-uniform inhibiting layer may be formed when the plating layer is formed, and the non-uniformity of the formation of the phases in the plating layer may increase. On the other hand, if the surface roughness is less than 0.2 μm, the surface friction coefficient decreases and the steel material may slip on the roll.
[0030] The steepness is measured by placing a steel material having a width of 1 m or more and a length of 2 m or more on a flat surface plate so that the surface of the steel material is firmly attached, and then measuring the degree of bending of the steel material. The steepness is expressed by dividing the height (H) of the bending by the wavelength (P) and multiplying it by 100. That is, it is expressed by the formula: height (H) / wavelength (P)×100. The smaller the steepness, the better the flatness of the steel material. Also, if the steepness exceeds 1.2, the bending of the steel material becomes large, which causes deviation in the surface flow when the steel material passes through the plating bath, adversely affecting the formation of the inhibition layer and the homogenization of the plating layer. The lower the steepness, the more advantageous it is. In order to control the steepness to less than 0.2, for example, there is a method of lowering the cold rolling speed, but this is not preferable because it requires excessive process costs.
[0031] The method for controlling the roughness and steepness to an appropriate range is not limited to any one of them. It is preferable to set the rolling reduction in the final stage of cold rolling to a range of 2 to 5%. It is necessary to apply an appropriate tension to the steel sheet during rolling. As an example of imparting surface roughness, the steel surface can be subjected to plasma treatment. That is, since the final shape can be determined by the last rolling roll during the cold rolling, it is preferable to set the rolling reduction to 5% or less. However, in the case of a thin plate with a thickness of 0.5 mm, it is preferable to set it to 2% or more in order to reduce overload in the previous stage rolling.
[0032] On the other hand, the above cold-rolled material can be annealed at a temperature of 600 to 850°C as necessary. The atmosphere in the annealing furnace is preferably a gas containing 1 to 10 volume % of hydrogen (H2) in nitrogen (N2). If the hydrogen concentration is less than 1 volume %, it is difficult to reduce the oxides on the steel surface, and if it exceeds 10 volume %, the production cost increases, so it is preferable to contain 1 to 10 volume % of hydrogen.
[0033] Since the dew point temperature in the atmosphere during the annealing differs, not only the ratio of components constituting the oxide film formed on the surface of the base steel differs, but also the ratio of internal oxidation differs, so it is preferable to control the dew point temperature at -60 to -10°C. If the dew point temperature is less than -60°C, excessive costs may be incurred in controlling the purity of the raw material gas, which is not preferable. On the other hand, if the dew point temperature exceeds -10°C, the reduction of contaminants on the surface of the base steel may not be performed smoothly, and an oxide film of trace elements and impurities such as B and Mn contained in the steel may be formed, which may hinder plating wettability.
[0034] The zinc alloy plated steel material is manufactured through a plating process in which the base steel prepared as described above is immersed in a plating bath and then withdrawn. The plating bath contains, by weight, 0.5 to 20.0% Al, 0.5 to 3.5% Mg, and the remainder Zinc and unavoidable impurities. The explanation of each of the above components is the same as the explanation of the zinc alloy plating layer described above.
[0035] An inhibition layer of Fe and Al is formed on the surface of the base steel immersed in the coating bath, and a coating layer similar to the components of the coating bath is formed on the inhibition layer, and the steel sheet is then drawn out of the coating bath. At this time, the temperature of the coating bath is preferably 430 to 500°C. If the temperature of the coating bath is less than 430°C, the decomposition of the surface oxide of the base steel does not proceed smoothly even when the base steel is immersed in the coating bath, which is disadvantageous for the formation of the inhibition layer. On the other hand, if the temperature of the coating bath exceeds 500°C, dross is generated on the surface of the coating bath and significant oxidation of Mg occurs, which is undesirable.
[0036] The plating step may be performed by immersing the parts individually in a plating bath, or by continuously passing a steel material (particularly a steel sheet) through a plating bath to form a plating layer. The steel material passing speed in the continuous hot-dip plating is preferably 60 to 200 MPM (passing distance per minute, meter per min.). If the passing speed is less than 60 MPM, the productivity of the product decreases, and if it exceeds 200 MPM, the inhibition layer and the plating layer may become non-uniform.
[0037] The zinc alloy plated steel material drawn out of the plating bath is cooled and the thickness of the plating layer is adjusted by a wiping nozzle called an air knife located above the plating bath. The wiping nozzle adjusts the thickness of the plating layer by spraying air or an inert gas. The temperature of the plating layer and the steel material as they pass through the wiping nozzle, and the adjustment of the wiping nozzle affect the formation of the plating layer structure.
[0038] FIG. 4 is a schematic diagram showing a plated steel material and a wiping nozzle. Referring to FIG. 4, the present invention relates to the gas injection pressure (P) in the wiping nozzle, the relationship between the wiping nozzle and the steel material, Material The distance (D), the thickness (t) of the wiping nozzle slot, the steel material threading speed (S), and the plating bath temperature (T) are expressed by the following formula: 2 It is preferable that the working index calculated by the above formula is in the range of 0.5 to 40. [Equation 2]
number
[0039] The above working index is a shape factor of the base iron before plating, and is suitable for forming a preferable plating structure when forming a plating layer in a state of surface roughness (Ra) of 0.2 to 1.0 μm and steepness of 0.2 to 1.2. In other words, it can refine the lamellar structure in the plating layer and facilitate the formation of a ternary eutectic alloy directly above the inhibition layer at the interface between the plated iron and the base iron. When the above working index is 0.5 less than In this case, the ratio of the Zn phase in the plating surface layer decreases, discoloration of the plating surface is likely to occur, and the lamellar structure becomes coarse, making plating cracks more likely to occur during processing. On the other hand, if the working index exceeds 40, defects such as flow patterns are likely to occur on the surface of the plating layer. Therefore, the working index defined by the above Relational Formula 2 is preferably 0.5 to 40.
[0040] After the wiping step, the plated steel material is cooled. The cooling preferably satisfies the following relational expression 1. [Equation 1] 0.7Vc≦Vc'≦1.5Vc Here, Vc is the average cooling rate immediately after wiping until solidification of the coating layer is completed, and Vc' is the average cooling rate immediately after wiping until solidification of the coating layer begins. In order to obtain a preferred structure, the ratio (Vc' / Vc) of the average cooling rate (Vc') at the point where solidification starts after adjusting the thickness of the coating layer in the liquid phase to the average cooling rate (Vc) at the point where solidification is completed after adjusting the thickness of the coating layer in the liquid phase is preferably 0.7 to 1.5. This can act as a factor that affects the structure and growth of the phases in the coating layer. EXAMPLES
[0041] The present invention will be described in more detail below with reference to examples. However, it should be noted that the following examples are merely intended to aid in the understanding of the present invention and are not intended to limit the scope of the present invention. This is because the scope of the present invention is determined by the matters described in the claims and matters that can be reasonably inferred therefrom.
[0042] (Example) A base steel sheet for automobile exterior panels is prepared as a cold-rolled steel sheet with a thickness of 0.8 mm containing 0.03%C-0.2%Si-0.15%Mn-0.01%P-0.01%S as the base steel. The surface roughness (Ra) and steepness of the base steel sheet are as shown in Table 1 below. The above cold-rolled steel sheet coil is continuously immersed in a Zn-Al-Mg alloy plating bath and pulled out, and then subjected to a wiping process and cooling to produce a zinc alloy plated steel sheet. The specific conditions are as shown in Table 1 below.
[0043] The working index of the above Relational Equation 2 was calculated using the components of the coating layer of the zinc alloy-coated steel sheet produced above, the spray pressure of the wiping nozzle (P), the distance between the wiping nozzle and the steel sheet (D), the slot thickness of the wiping nozzle (t), the passing speed of the steel material (S), and the temperature of the coating bath (T) as shown in Table 1 below, and is also shown in Table 1 below.
[0044] The area fraction of the Zn phase observed on the surface of the zinc alloy-plated steel sheet produced as described above, the widthwise spacing of the lamellar-structured Zn phase and MgZn2 phase existing from the surface to 70% of the plating layer thickness, and the area fraction of the Zn / MgZn2 / Al ternary alloy phase layer contained within 2 μm in the inhibition layer were measured and are shown in Table 2 below.
[0045] In addition, to confirm the characteristics of each zinc alloy plated steel sheet, the surface characteristics, the corrosion resistance of the cross section and the processed part were evaluated, and the results are shown in the table below. 2The surface characteristics were measured by measuring the flow pattern and the degree of surface discoloration. The degree of surface discoloration was evaluated by measuring the color difference of the surface of each test piece, leaving the test piece at a temperature of 50°C and a humidity of 95% for 24 hours, measuring the color difference of the test piece again, and evaluating the decrease in brightness (dE). The corrosion resistance of the cross-section and processed parts was evaluated by carrying out a cyclic corrosion test for each sample as specified in ISO TC 156. The number of cycles of the cyclic corrosion test at which red rust appeared on the cut surface of the test piece, and the number of cycles of the cyclic corrosion test at which red rust appeared on the bent part after bending the test piece 180° and carrying out a corrosion experiment were recorded.
[0046] [Table 1]
[0047] [Table 2]
[0048] On the other hand, FIG. 1 is a photograph of the cross section of the coating layer of the above-mentioned Example 3 of the invention. As shown in FIG. 1, the coating layer is present on the base steel sheet 11, and a Zn single phase 12 and a lamellar structure 13 are formed in the coating layer. It can be seen that the lamellar structure 13 is formed finely, thereby reducing the occurrence of cracks during processing. FIG. 3 is a photograph of the interface between the base steel sheet 11 and the Zn single phase 12 in FIG. 1, and it can be seen that an inhibition layer 14 and a ternary alloy phase of Zn / MgZn2 / Al are formed. Specifically, it can be seen that an MgZn2 phase 15, an Al phase 16, and a Zn phase 17 are formed. In contrast, FIG. 2 is a photograph of the cross section of the coating layer of the above-mentioned Comparative Example 2, and it can be seen that a lamellar structure 23 is formed coarsely. It can therefore be seen that cracks are likely to occur during processing.
[0049] From the results in Table 2 and FIGS. 1 to 3 above, it can be confirmed that the inventive examples that satisfy the conditions of the present invention ensure excellent surface properties and excellent corrosion resistance even in cross sections and processed parts.
Claims
1. With bare iron, a Zn-Al-Mg zinc alloy plating layer formed on the base steel; An inhibition layer formed between the base steel and the zinc alloy plating layer, The Zn phase on the surface of the zinc alloy plating layer has an area fraction of 15 to 90%; A Zn / MgZn layer having a thickness of 2 μm or less is formed on the suppression layer. 2 / Al ternary alloy phase layer, the ternary alloy phase layer covering the surface of the inhibition layer at an area fraction of 30 to 90%.
2. The zinc alloy plating layer is a Zn phase and an MgZn phase. 2 The Zn phase and and MgZn 2 2. The method according to claim 1, wherein the average thickness of each of the phases in the width direction is 1.5 μm or less. Zinc alloy plated steel.
3. The crystal grain size of the Fe-Al intermetallic compound of the inhibition layer is 300 nm or less. Item 3. The zinc alloy-plated steel material according to item 1 or 2.
4. The zinc alloy plating layer contains, by weight, Mg: 0.5 to 3.5%, Al: 0.5 to 20. 0%, the remainder being Zn and unavoidable impurities. Alloy plated steel.
5. A method for producing the zinc alloy plated steel material according to claim 1, providing a base iron; immersing the base steel in a zinc alloy plating bath containing Mg and Al to plate it; and wiping and cooling the plated base steel. The method for producing a zinc alloy plated steel product, wherein the cooling satisfies the following relational expression 1: [Relationship 1] 0.7Vc≦Vc'≦1.5Vc where Vc is the average cooling rate until the coating layer solidifies immediately after wiping, and Vc' is This is the average cooling rate until the coating layer starts to solidify immediately after wiping.
6. The step of providing the base iron comprises: A hot-rolled steel material having a surface layer grain size of 1 to 100 μm is provided; The hot-rolled steel material is cold-rolled to have a surface roughness of 0.2 to 1.0 μm and a steepness of 0.2 to 1.
2. The method for producing a zinc alloy plated steel material according to claim 5, further comprising producing a cold rolled steel material having the following properties: .
7. The composition of the plating bath is, in weight percent, Mg: 0.5 to 3.5%, Al: 0.5 to 20.0%, % and the remainder containing Zn and inevitable impurities. Manufacturing method.
8. The plating and wiping processes are carried out in accordance with the working index (working index) of the following formula 2:
8. The zinc alloy plated steel material according to claim 5, wherein the zinc alloy plated steel material has a surface roughness of 0.5 to 40. Manufacturing method. [Relationship 2] [0010] where P is the pressure of the wiping gas (KPa), D is the distance between the wiping nozzle and the plated steel material. distance (mm), t: slot thickness of wiping nozzle (mm), S: strip threading speed (MPM), T: Temperature of the plating bath (°C).
9. The temperature of the plating bath is 430 to 500° C. A manufacturing method of zinc alloy plated steel.
10. The threading speed during plating is 60 to 200 MPM (meter per minute). The method for producing a zinc alloy plated steel material according to any one of claims 5 to 9, wherein
Citation Information
Patent Citations
HOT-DIP Zn-Al-Mg-Si-Cr ALLOY COATED STEEL MATERIAL WITH EXCELLENT CORROSION RESISTANCE
WO2010082678A1
Hot dip zn-al-mg based alloy plated steel having excellent corrosion resistance
JP2002332555A
Hot dip plated steel sheet having satisfactory appearance
JP2006283155A