Coated zirconia fine particles and method for producing same
Coating zirconia fine particles with metal elements like Mg, Ca, Al, and rare earth elements addresses the challenges of uniformity and productivity in zirconia production, resulting in stable and dense sintered bodies with reduced manufacturing costs.
Patent Information
- Application Number
- JP2021567523
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-24
- Filing Date
- 2020-12-23
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-12-23
AI Technical Summary
Conventional methods for producing zirconia fine particles face challenges in achieving uniform particle shapes, poor dispersibility, and low productivity due to the difficulty in mixing zirconium and yttrium at the atomic level, leading to issues such as cracking and destruction of sintered bodies during high-temperature processing.
The production of coated zirconia fine particles involves reacting zirconia fine particles with ions of metal elements like Mg, Ca, Al, and rare earth elements in an aqueous dispersion to form a coating layer, which stabilizes the particles and enhances their properties, allowing for a simple and efficient manufacturing process.
The coated zirconia fine particles exhibit improved stability and strength, reducing cracking and enhancing the density of sintered bodies, while also enabling cost-effective industrial-scale production.
Smart Images

Figure 0007579276000005 
Figure 0007579276000006 
Figure 0007579276000001
Abstract
Description
[Technical field]
[0001] The present invention relates to coated zirconia fine particles and a method for producing the same.
[0002] Background technology Zirconia (ZrO 2 ) has many excellent characteristics, such as a high refractive index, high strength, toughness, high abrasion resistance, high lubricity, high corrosion resistance, high oxidation resistance, insulation, low thermal conductivity, and high transparency in the visible light range, and is therefore used in a wide range of applications, including automobile exhaust catalysts, capacitors, grinding balls, dental materials, glass additives, thermal barriers, solid electrolytes, and optical materials.
[0003] Zirconia is used to manufacture various products by molding and sintering fine particles, but as a single substance, it has a tetragonal crystal structure at high temperatures and a monoclinic crystal structure at low temperatures, and therefore has the problem that the sintered body is prone to cracking and breaking due to volume expansion and contraction caused by temperature changes. For this reason, yttria (Y 2 O 3 ), calcia (CaO), magnesia (MgO), ceria (CeO 2 A method is used to prevent phase transition by dissolving stabilizers such as zirconia in a solid solution. Zirconia that is partially stabilized by adding a stabilizer is called partially stabilized zirconia.
[0004] Partially stabilized zirconia can be produced by various methods similar to those used for producing zirconia, such as a neutralization method, a hydrolysis method, a hydrothermal reaction method, an alkoxide method, a gas phase method, or a spray pyrolysis method.
[0005] Japanese Patent Application Laid-Open No. 2008-24555 discloses a method for producing a fine zirconia powder containing one or more of yttria, calcia, magnesia, and ceria as a stabilizer, by adding a compound such as yttrium to a hydrated zirconium sol, drying the sol, and calcining the sol at a temperature in the range of 1000 to 1200°C.
[0006] Japanese Patent Application Laid-Open Publication No. 2010-137998 discloses a method for producing partially stabilized zirconia porcelain containing zirconia and yttria in a specified range, in which a composite of yttria fine particle powder or yttrium salts uniformly dispersed in zirconium hydroxide as a starting material containing Zr is heat-treated in a temperature range of 1100 to 1400°C to obtain zirconia, which is then pulverized to obtain a ceramic powder, which is then molded and fired.
[0007] Japanese Patent Application Laid-Open Publication No. 2015-221727 discloses a method for producing a predetermined zirconia sintered body containing 0.05-3 mass% alumina and an yttria concentration of 2-4 mol%, in which the average particle size of secondary particles is 0.1-0.4 μm, the ratio of the average particle size of the secondary particles / the average particle size of primary particles measured with an electron microscope is 1-8, and zirconia powder containing 0.05-3 mass% of an aluminum compound in terms of alumina and having an yttria concentration of 2-4 mol% is molded and pre-sintered at 1100-1200°C, and the obtained pre-sintered body is subjected to hot isostatic pressing at a pressure of 50-500 MPa and a temperature of 1150-1250°C.
[0008] Japanese Patent Application Laid-Open No. 2009-227507 discloses a method for producing zirconia composite fine particles, which comprises adding an alkali carbonate solution to a zirconia acidic dispersion containing rare earth element ions and / or alkaline earth metal ions to produce a neutralized precipitate, drying the neutralized precipitate, subjecting the dried neutralized precipitate to a heat treatment at a temperature of 400° C. or more and 600° C. or less, and then washing to remove the alkali carbonate component.
[0009] Japanese Patent Laid-Open Publication No. 5-170442 discloses a method for producing a crystalline zirconia-based sol having a rare earth element oxide, calcia or magnesia as a solid solution, which comprises mixing a solution of a zirconium salt with a solution of one type of salt selected from rare earth elements, calcium or magnesium in advance, adding the mixed solution to a basic solution or a slurry of a basic substance, heating the resulting slurry at a temperature of 80 to 200°C, adding an acid, and then separating and washing the resulting slurry.
[0010] Japanese Patent Application Laid-Open No. 2017-154927 discloses zirconium oxide nanoparticles coated with a carboxylic acid, the zirconium oxide nanoparticles containing yttrium and at least one type of transition metal other than rare earth elements.
[0011] Summary of the Invention JP 2008-24555 A, JP 2010-137998 A, JP 2015-221727 A, and JP 2009-227507 A disclose methods utilizing a neutralization method and / or a hydrolysis method, but these require firing at high temperatures to achieve a solid solution, and the particle shape tends to become non-uniform due to particle growth, resulting in particles with poor dispersibility. On the other hand, JP-A-5-170442 and JP-A-2017-154927 use a hydrothermal reaction method, and since they do not require a calcination process, fine particle diameters can be obtained, which is considered to be advantageous for obtaining zirconia fine particles of several tens of nm. However, since yttrium salts, which are often used as stabilizers, generally have a lower solubility than zirconium salts, it is difficult to mix zirconium and yttrium uniformly at the atomic level in industrial-scale production using a hydrothermal reaction method, and yttria tends to be unevenly distributed. In addition, since the reaction takes a long time, there are still problems in terms of productivity.
[0012] In view of the above circumstances, the present invention provides stable zirconia fine particles and a simple method for producing the same.
[0013] The present invention provides coated zirconia fine particles comprising zirconia fine particles and a coating layer that coats the surfaces of the fine particles, The coating layer contains one or more metal elements selected from Mg, Ca, Al, and rare earth elements, The average particle size is 3 to 100 nm, Specific surface area is 20 to 500 m 2 / g, The present invention relates to coated zirconia fine particles.
[0014] The present invention also relates to a method for producing coated zirconia fine particles, which comprises reacting ions of one or more metal elements selected from Mg, Ca, Al and rare earth elements with an additive that reacts with the ions to form a water-insoluble compound in an aqueous dispersion containing zirconia fine particles, thereby precipitating a compound containing the metal element on the surfaces of the zirconia fine particles, thereby obtaining coated zirconia fine particles.
[0015] According to the present invention, stable coated zirconia fine particles and a simple method for producing the same are provided. The coated zirconia fine particles of the present invention have the advantage over conventional zirconia fine particles that cracks and breakage of the sintered body are suppressed when subjected to a firing process and that high density can be achieved, and therefore the coated zirconia fine particles of the present invention are suitable for use as various ceramic materials, dental materials, capacitors, coating materials, etc. In addition, the coated zirconia fine particles of the present invention can be produced by a simple method, which allows reduction in production costs and makes them useful for industrial-scale production. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a transmission electron microscope (TEM) image of the coated zirconia fine particles obtained in Example 2. [Diagram 2] FIG. 2 is a scanning electron microscope / energy dispersive X-ray spectroscopy (SEM-EDX) image showing the element distribution of zirconium and yttrium in the coated zirconia fine particles obtained in Example 2 and Comparative Example 2.
[0017] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS [Coated zirconia particles] The present invention relates to coated zirconia fine particles containing zirconia fine particles and a coating layer that coats the surfaces of the fine particles, the coating layer containing one or more metal elements selected from Mg, Ca, Al and rare earth elements, having an average particle diameter of 3 to 100 nm and a specific surface area of 20 to 500 m. 2 / g.
[0018] The specific surface area of zirconia particles is 20 to 500 m2 / g is preferable, and 40 to 200m 2 / g is more preferable, and 70 to 150m 2 / g. It is more preferable that the specific surface area of the zirconia fine particles is 20 m 2 When the specific surface area of the zirconia fine particles is 500 m / g or more, the particle size of the resulting coated zirconia fine particles is appropriately controlled, and a high-density sintered body is easily obtained. In addition, the stabilizing effect of the metal elements in the coating layer tends to be easily manifested. 2 When the surface of the coated zirconia fine particles is coated with the zirconia nanoparticles, the particle size is appropriately large and the cohesive force is not excessively large. This facilitates monodispersion during surface coating and improves the filling properties during molding when the coated zirconia fine particles are used. Here, the specific surface area of the zirconia fine particles can be measured by the BET method using a BET specific surface area measuring device, for example, a fully automatic BET specific surface area measuring device (Macsorb HM Model-1210) manufactured by Mountex Corporation, by adsorption and desorption of nitrogen gas on a sample degassed at 150°C.
[0019] The average particle size of the zirconia fine particles is preferably 3 to 100 nm, more preferably 5 to 50 nm, and further preferably 7 to 20 nm. In the present invention, the average particle size of the zirconia fine particles can be determined by measuring the particle sizes of 200 or more arbitrary particles from a TEM image at a magnification of 200,000 times based on observation with a transmission electron microscope, and averaging the particle sizes.
[0020] The coated zirconia fine particles of the present invention have a coating layer on the surface of the zirconia fine particles, the coating layer containing one or more metal elements selected from Mg, Ca, Al and rare earth elements. At least one metal selected from Mg, Ca, Al and rare earth elements contributes to the stabilization of the zirconia fine particles. The rare earth element is preferably Y (yttrium). The coating layer may contain a compound (hereinafter also referred to as a coating compound) containing one or more metal elements selected from Mg, Ca, Al, and rare earth elements. The coating layer may contain one or more selected from the group consisting of hydroxides of one or more metal elements selected from Mg, Ca, Al and rare earth elements, carbonates of the above metal elements and oxides of the above metal elements. The coating layer may preferably contain one or more selected from the group consisting of hydroxides of one or more metal elements selected from Mg, Ca, Al and Y, carbonates of the above metal elements and oxides of the above metal elements. The coating layer preferably contains Y, and more preferably contains an yttrium compound such as yttrium hydroxide, or further a hydroxide.
[0021] By adding the metal element, the phase transition from tetragonal to monoclinic is suppressed in the zirconia fine particles, and the strength, durability and dimensional accuracy are improved. From this viewpoint, the amount of the metal element can be adjusted. For example, in the present invention, the amount of the coating compound in the coating layer is preferably 3 to 45 mol%, more preferably 5 to 40 mol%, even more preferably 6 to 36 mol%, and even more preferably 12 to 28 mol% relative to the zirconia of the zirconia fine particles. When the amount of the coating compound in the coating layer is equal to or more than the lower limit, the tetragonal crystal ratio in the crystal structure after high-temperature sintering is appropriately increased, the effect of suppressing cracks and breakage of the sintered body is large, and in addition, the production of the molded body is also easy. In addition, when the amount of the metal element in the coating layer is equal to or less than the upper limit, the bending strength and fracture toughness can be maintained, and in addition, impurity phases derived from the stabilizer are less likely to be generated after high-temperature sintering, and the strength, insulation and other properties of the sintered body are also good. The amount of the coating compound in the coating layer can be measured by XRF analysis or the like. In addition, the coating compound can be estimated by specifying the coating compound and calculating the amount of the coating compound to be used, and the type of neutralizing agent if the compound is neutralized.
[0022] The coated zirconia fine particles of the present invention have an average particle size of 3 to 100 nm, preferably 5 to 50 nm, and more preferably 7 to 20 nm. The average particle size of the coated zirconia fine particles is determined by measuring the particle sizes of 200 or more random particles from a TEM image at a magnification of 200,000 times based on observation with a transmission electron microscope, and averaging the measured particle sizes. By controlling the particle size, the transparency of a composition containing the coated zirconia fine particles can be improved. In addition, the coated zirconia fine particles have excellent low-temperature sintering properties.
[0023] The coated zirconia fine particles of the present invention have a specific surface area of 20 to 500 m 2 / g, 40 to 200m 2 / g is preferable, and 70 to 150m 2 / g is more preferable. 2 / g or more, the particle size is appropriately controlled to produce fine particles, making it easy to obtain a high-density sintered body. In addition, the stabilizing effect of the metal elements in the coating layer tends to be easily manifested. In addition, when the specific surface area of the coated zirconia fine particles is 500 m 2 When the particle size is 1 / g or less, the particle size becomes appropriately large and the cohesive force does not become excessively large, resulting in good filling properties during molding.
[0024] The coated zirconia fine particles of the present invention can be suitably used for various ceramic materials, dental materials, capacitors, coating materials, and the like.
[0025] [Method of manufacturing coated zirconia particles] The present invention relates to a method for producing coated zirconia fine particles, which comprises reacting ions of one or more metal elements selected from Mg, Ca, Al and rare earth elements with an additive that reacts with the ions to form a water-insoluble compound in an aqueous dispersion containing zirconia fine particles, thereby precipitating a compound (coating compound) containing the metal element on the surface of the zirconia fine particles to obtain coated zirconia fine particles. The matters described for the coated zirconia fine particles of the present invention can be appropriately applied to the production method of the present invention. The coated zirconia fine particles of the present invention can be obtained by the production method of the present invention. For example, the preferred aspects of the raw zirconia fine particles and the metal elements are the same as those described for the coated zirconia fine particles of the present invention.
[0026] The additive may be, for example, an alkaline agent. Examples of the alkaline agent include hydroxides such as NaOH and KOH; 2 CO 3 , K 2 CO 3 , Ammonium Carbonate, NaHCO 3 , K.H.C.O. 3 Examples of the alkaline agent include carbonates such as ammonium carbonate, etc., and ammonia. These alkaline agents can be used in the form of an aqueous solution, a powder, a solid, or a crystal, but an aqueous solution is preferred in terms of ease of handling. An aqueous ammonia solution can also be used as the alkaline agent. When the alkaline agent is used in the form of an aqueous solution, the concentration is preferably 5 to 50% by mass, more preferably 10 to 30% by mass.
[0027] In the present invention, the ions of the metal element can be introduced into the aqueous dispersion of zirconia fine particles by, for example, mixing an aqueous solution of a compound containing the metal element with the aqueous dispersion of the zirconia fine particles. In the present invention, the aqueous dispersion, the aqueous solution of the compound containing the metal element, and the additive can be mixed to react the ions with the additive. In this case, the aqueous solution of the compound containing the metal element and the additive are used so that the amount of the coating compound formed from the compound and the additive is preferably 3 to 45 mol%, more preferably 5 to 40 mol%, even more preferably 6 to 36 mol%, and even more preferably 12 to 28 mol% relative to the zirconia of the zirconia fine particles, in terms of the maximum theoretical value.
[0028] In the present invention, after the coated zirconia fine particles are obtained, the additives can be removed from the coated zirconia fine particles For example, after the coated zirconia fine particles are obtained, the coated zirconia fine particles can be washed with water.
[0029] In the present invention, the obtained coated zirconia particles can be dried at a temperature at which the coated zirconia fine particles are not sintered, for example, 200° C. or lower.
[0030] In the present invention, an alkaline agent is added to an aqueous dispersion containing zirconia fine particles and mixed uniformly, and then an aqueous solution of a compound containing the metal element is added to cause a neutralization reaction, thereby uniformly coating the particle surfaces of the zirconia fine particles with the metal compound. In addition, in the present invention, an aqueous solution of a compound containing the metal element is added to an aqueous dispersion containing zirconia fine particles, and then an alkaline agent is added to cause a neutralization reaction, thereby making it possible to uniformly coat the particle surfaces of the zirconia fine particles with the metal compound. In the present invention, an aqueous solution of a compound containing the metal element and an alkaline agent are simultaneously added to an aqueous dispersion containing zirconia fine particles, and a neutralization reaction is carried out, thereby making it possible to uniformly coat the particle surfaces of the zirconia fine particles with the metal compound.
[0031] An example of the method for producing the coated zirconia fine particles of the present invention will be described below. First, zirconia fine particles are uniformly dispersed in water. In order to uniformly disperse the zirconia fine particles, it is preferable to adjust the pH and use a dispersing machine such as an ultrasonic homogenizer, a planetary ball mill, a Henschel mixer, a colloid mill, a wet jet mill, or a wet bead mill. A mechanical stirrer can also be used.
[0032] The aqueous dispersion of zirconia fine particles thus obtained is mixed with a composition containing ions of one or more metal elements selected from Mg, Ca, Al, and rare earth elements, and water. The composition is preferably an aqueous solution of a compound of the metal element, such as a salt. Examples of the salt containing the metal element include inorganic salts such as sulfates, nitrates, and chlorides. Organic compounds such as metal alkoxides can also be used. Inorganic salts are preferred in terms of solubility and easy availability. The concentration of the aqueous solution is preferably 0.001 to 10 mol / L, more preferably 0.01 to 5 mol / L.
[0033] Next, an additive that reacts with the ions to produce a water-insoluble compound is mixed into a mixture obtained by mixing an aqueous dispersion of zirconia microparticles with a composition containing ions of the metal element and water, preferably an aqueous solution of a compound containing the metal element (e.g., a salt), and the mixture is mixed with the additive.
[0034] The additive includes the above-mentioned alkaline agents, for example, an aqueous solution of an alkaline agent. When a salt containing the metal element is used, the alkaline agent is added in an amount such that the degree of neutralization of the salt is, for example, 0.8 or more. The temperature at which the alkaline agent is added is not particularly limited, but may be, for example, 100° C. or lower.
[0035] In the present invention, for example, it can be confirmed from the state of a TEM image of the zirconia fine particles that the surface of the zirconia fine particles is covered with the compound containing the metal element.
[0036] The aqueous dispersion containing the zirconia fine particles uniformly coated with the metal compound is appropriately subjected to processes such as filtration, washing, drying, and crushing to obtain the coated zirconia fine particles. In one example, the coating layer is made of hydroxides or carbonates of Mg, Ca, Al, and rare earth elements, and is in an amorphous state. The coating layer may be made into a crystalline state of oxide by heat treatment.
[0037] The coated zirconia fine particles of the present invention can be used in the form of powder, dispersion, nanocomposite, etc. Examples of the dispersion include those using water or an organic compound as a dispersion medium. Examples of the nanocomposite include nanocomposites in which the coated zirconia fine particles are uniformly dispersed in an organic compound such as a monomer, oligomer, or resin.
[0038] As an example of the manufacturing method of the present invention, there is a manufacturing method of coated zirconia fine particles, which comprises mixing an aqueous dispersion of zirconia fine particles with an aqueous solution of a water-soluble salt of one or more metal elements selected from Mg, Ca, Al, and rare earth elements, and then mixing an alkali agent into the mixture so that the pH of the mixture is 8 to 13, preferably 12 to 13, to precipitate a compound containing the metal element on the surface of the zirconia fine particles, thereby obtaining coated zirconia fine particles. In this case, the alkali agent can be added so that the neutralization degree of the water-soluble salt is 0.8 or more. In addition, in the present invention, the coated zirconia particles can be washed with water until the detected amount of the alkali agent is 0.01 mass% or less. The water-soluble salt can be one having a solubility in water at 20°C of 5.0 g / 100 g water or more.
[0039] The present invention provides a method for producing zirconia fine particles, which comprises reacting, in an aqueous dispersion containing zirconia fine particles, ions of one or more metal elements selected from Mg, Ca, Al and rare earth elements with an additive that reacts with the ions to form a water-insoluble compound. According to the present invention, there is provided a method for producing zirconia fine particles, which comprises mixing an aqueous dispersion of zirconia fine particles with an aqueous solution of a water-soluble salt of one or more metal elements selected from Mg, Ca, Al, and rare earth elements, and then mixing an alkaline agent into the mixture so that the pH of the mixture is 8 to 13, preferably 12 to 13. The aqueous solution may contain the water-soluble salt at a concentration of 0.001 to 10 mol / L. The alkaline agent can be added so that the degree of neutralization of the water-soluble salt is 0.8 or more. In the present invention, the coated zirconia particles can be washed with water until the detected amount of the alkaline agent is 0.01 mass% or less. The water-soluble salt may have a solubility in water at 20°C of 5.0 g / 100 g water or more.
[0040] According to the present invention, there is provided a method for producing a zirconia sintered body, comprising a step of producing coated zirconia fine particles by the method of the present invention, and a step of sintering the produced coated zirconia fine particles. The matters described in the coated zirconia fine particles and the method for producing coated zirconia fine particles of the present invention can be appropriately applied to the production method of this zirconia sintered body. The sintering of the coated zirconia fine particles can be carried out according to a known method for sintering zirconia fine particles, taking into consideration the use of the sintered body, etc. One example is a method of sintering at 1300 to 1600°C for 1 to 15 hours.
[0041] The present invention provides a method for producing a coated zirconia fine particle dispersion, which comprises dispersing the coated zirconia fine particles of the present invention in a dispersion medium (hereinafter also referred to as a dispersion medium for dispersion). The matters described in relation to the coated zirconia fine particles of the present invention and the method for producing the coated zirconia fine particles can be appropriately applied to the production method of this coated zirconia fine particle dispersion.
[0042] The present invention also provides a method for producing a nanocomposite, which comprises dispersing the coated zirconia fine particles of the present invention in a dispersion medium (hereinafter also referred to as a dispersion medium for nanocomposite). The matters described in relation to the coated zirconia fine particles of the present invention and the method for producing the coated zirconia fine particles can be appropriately applied to this method for producing the nanocomposite.
[0043] In the method for producing a coated zirconia fine particle dispersion and the method for producing a nanocomposite of the present invention, the coated zirconia fine particles of the present invention may be treated with a surface treatment agent. Examples of the surface treatment agent include, but are not limited to, the following. For example, a (meth)acryloyloxy-based silane coupling agent, a vinyl-based silane coupling agent, an epoxy-based silane coupling agent, an amino-based silane coupling agent, a ureido-based silane coupling agent, etc. can be used.
[0044] Examples of (meth)acryloyloxy-based silane coupling agents include 3-(meth)acryloyloxypropyltrimethylsilane, 3-(meth)acryloyloxypropylmethyldimethoxysilane, 3-(meth)acryloyloxypropyltrimethoxysilane, 3-(meth)acryloyloxypropylmethyldiethoxysilane, and 3-(meth)acryloyloxypropyltriethoxysilane. Examples of acryloxy-based silane coupling agents include 3-acryloxypropyltrimethoxysilane.
[0045] Examples of vinyl-based silane coupling agents include allyltrichlorosilane, allyltriethoxysilane, allyltrimethoxysilane, diethoxymethylvinylsilane, trichlorovinylsilane, vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, and vinyltris(2-methoxyethoxy)silane.
[0046] Examples of epoxy-based silane coupling agents include diethoxy(glycidyloxypropyl)methylsilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane. Examples of styrene-based silane coupling agents include p-styryltrimethoxysilane.
[0047] Examples of amino-based silane coupling agents include N-2(aminoethyl)3-aminopropylmethyldimethoxysilane, N-2(aminoethyl)3-aminopropyltrimethoxysilane, N-2(aminoethyl)3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane.
[0048] An example of the ureido-based silane coupling agent is 3-ureidopropyltriethoxysilane.
[0049] Further examples of other surface treatment agents include the following. An example of a chloropropyl-based silane coupling agent is 3-chloropropyltrimethoxysilane. An example of a mercapto-based silane coupling agent is 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane. An example of a sulfide-based silane coupling agent is bis(triethoxysilylpropyl)tetrasulfide. An example of an isocyanate-based silane coupling agent is 3-isocyanatepropyltriethoxysilane. An example of an aluminum-based coupling agent is acetoalkoxyaluminum diisopropylate.
[0050] The dispersion medium for the dispersion used in the present invention is not particularly limited as long as it can disperse the coated zirconia fine particles. For example, water or an organic compound can be used as the dispersion medium.
[0051] When water is used as the dispersion medium for the dispersion, the pH is preferably 2 to 5, or 9 to 13, from the viewpoint of dispersibility of the coated zirconia fine particles.
[0052] The organic compound as the dispersion medium for the dispersion liquid can be selected from compounds known as organic solvents.Specifically, preferred examples include ethanol, isopropanol, butanol, cyclohexanol, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, ethyl acetate, propyl acetate, butyl acetate, methyl cellosolve, cellosolve, butyl cellosolve, cellosolve acetate, tetrahydrofuran, 1,4-dioxane, n-hexane, cyclopentane, toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, dichloromethane, trichloroethane, trichloroethylene, and hydrofluoroether.
[0053] The dispersion medium for the nanocomposite is not particularly limited as long as it can disperse the coated zirconia fine particles, and is an organic compound such as a monomer, oligomer, resin (polymer), etc. Examples of the monomer, oligomer, resin, etc. that can be used include aromatic ring-containing acrylate, alicyclic skeleton-containing acrylate, monofunctional alkyl (meth)acrylate, polyfunctional alkyl (meth)acrylate, and polymers thereof.
[0054] Examples of aromatic ring-containing acrylates, from the viewpoint of high refractive index, include phenoxyethyl acrylate, phenoxy 2-methylethyl acrylate, phenoxyethoxyethyl acrylate, 3-phenoxy-2-hydroxypropyl acrylate, 2-phenylphenoxyethyl acrylate, benzyl acrylate, phenyl acrylate, phenylbenzyl acrylate, and paracumylphenoxyethyl acrylate.
[0055] Examples of alicyclic skeleton-containing acrylates include 2-acryloyloxyethylhexahydrophthalate, cyclohexyl acrylate, dicyclopentanyl acrylate, tetrahydrofurfuryl acrylate, dicyclopentanyl methacrylate, and isobornyl methacrylate, which have a high Abbe number and are preferable as optical materials.
[0056] Furthermore, examples of the monofunctional alkyl (meth)acrylate, from the viewpoint of low viscosity, include methyl (meth)acrylate, octyl (meth)acrylate, isostearyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxyethyl (meth)acrylate, ethylene oxide-modified alkyl (meth)acrylate, propylene oxide-modified alkyl (meth)acrylate, hydroxyethyl (meth)acrylate, and hydroxypropyl (meth)acrylate.
[0057] Furthermore, examples of the polyfunctional alkyl (meth)acrylates that can improve the hardness of the cured product include (i) bifunctional (meth)acrylates such as (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and 1,9-nonanediol di(meth)acrylate; (ii) trifunctional (meth)acrylates such as glycerol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, phosphate tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate; and (iii) ethylene oxide and / or propylene oxide modified products of the compounds selected from (i) and (ii).
[0058] In the method for producing a coated zirconia microparticle dispersion and the method for producing a nanocomposite of the present invention, a dispersant can be used as necessary. The dispersant is not particularly limited as long as it is a compound containing a group having affinity with the coated zirconia microparticles, but preferred dispersants include anionic dispersants having an acid group such as carboxylic acid, sulfuric acid, sulfonic acid, phosphoric acid, or salts thereof. Among these, phosphate ester dispersants are preferred. The amount of dispersant used is not particularly limited, but is preferably 0.1 to 30 mass% relative to the coated zirconia microparticles.
[0059] Working Example The coated zirconia fine particles and the method for producing the same of the present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0060] The various instrumental analyses were carried out by the following methods. (1) X-ray diffraction (XRD) The measurements were performed using a Bruker AXS X-ray diffractometer (D8 ADVANCE / V), and qualitative analysis and quantitative analysis were performed using Rietveld analysis (tetragonal, monoclinic, etc.). (2) Measurement of the amount of coating metal compounds in coated zirconia particles (XRF analysis) The amount of each element in the coated inorganic microparticles was quantified using a Bruker AXS X-ray fluorescence analyzer (S8 TIGER). (3) Measurement of specific surface area (SSA) The coated zirconia fine particles were degassed at 150° C., and the specific surface area was measured by the BET method using a fully automatic BET specific surface area measuring device (Macsorb HM Model-1210) manufactured by Mountech Co., Ltd., by adsorption and desorption of nitrogen gas. (4) Measurement of average particle size, evaluation of particle shape and uniformity Using a Hitachi High-Technologies transmission electron microscope (H-7600), images of particles were taken at magnifications of 30,000 to 200,000 times, and the long diameters of 200 or more particles were measured and the average value was calculated to determine the average particle size. Particle shape was evaluated by observing TEM images, and uniformity was evaluated from the measured average particle size. (5) Evaluation of uniformity of surface coating Using a Hitachi High-Technologies field emission scanning electron microscope (SU8220) and an energy dispersive X-ray analyzer (EX-370X-MAX50), images of the particles were taken at a magnification of 3000x, and the element distribution was observed and evaluated by EDX mapping.
[0061] [Preparation of coated zirconia particles] <Example 1> Pure water was added to 27.7 g (225 mmol) of zirconia fine particle powder (manufactured by Kanto Denka Kogyo Co., Ltd.) with an average particle size of 10 nm so that the powder concentration was 20 mass%, and the mixture was stirred with a mechanical stirrer for 1 hour to prepare a zirconia water slurry. A 1 mol / L yttrium nitrate aqueous solution was added dropwise to the slurry so that the concentration was 13.5 mmol in terms of yttrium nitrate, and the mixture was stirred for 1 hour. Next, a 25 mass% aqueous sodium hydroxide solution was added dropwise to the slurry so that the degree of neutralization was 0.8 or more and the pH was 12 to 13, and the mixture was stirred for about 1 hour. The obtained slurry was suction filtered, washed with water until Na was not detected by XRF measurement, and then dried at 150 ° C until the moisture content was 1% or less. The obtained solid was crushed in a mortar and sieved (75 μm mesh).
[0062] <Examples 2 to 13, Comparative Example 1> In accordance with Example 1, various coated zirconias were prepared according to the formulations shown in Table 1. In Example 6, commercially available zirconia fine particles mainly composed of monoclinic crystals were used as the raw material. In Example 7, neutralization was performed with sodium carbonate. In Example 8, calcium chloride was used instead of yttrium nitrate. In some examples, a second compound was used. A TEM image of the coated zirconia fine particles of Example 2 is shown in Figure 1. A SEM-EDX mapping photograph of the coated zirconia fine particles of Example 2 is shown in Figure 2. The TEM photograph shows that the particles obtained in Example 2 are spherical, and the measured values of the average particle size show good uniformity.
[0063] <Comparative Example 2> Pure water was added to 27.7 g (225 mmol) of zirconia fine particle powder (manufactured by Kanto Denka Kogyo Co., Ltd.) having an average particle size of 5 to 10 nm so that the concentration was 20 mass %, and the mixture was stirred for 1 hour with a mechanical stirrer. 2 O 3) was added and stirred for 1 hour. The obtained slurry was filtered by suction, washed with water, and then dried by heating at 150°C until the moisture content was 1% or less. The obtained solid was pulverized in a mortar and passed through a sieve with 74 μm openings. A SEM-EDX mapping photograph of the coated zirconia of Comparative Example 2 is shown in FIG.
[0064] [Sintering of coated zirconia particles and changes in crystal structure] The crystal structures of the coated zirconia fine particles obtained in Examples 1 to 13 and Comparative Examples 1 and 2 after firing at 1000° C. were evaluated by the following method. The coated zirconia particles were heated in an air atmosphere from 20°C to 1000°C over 4 hours, and then sintered at 1000°C for 3 hours. The crystal structure of the resulting powder was evaluated by X-ray diffraction (XRD) measurement. Note that the physical properties of the coated zirconia particles, such as the crystal structure, vary significantly depending on the sintering conditions (temperature, time).
[0065] [Table 1]
[0066] *1 Mol% is the mol% relative to zirconia, and indicates the amount of coating compound based on the type and amount of raw material, type of neutralizer, etc. *2 Although it contains a very small amount of Hf, this amount is included and shown as the Zr mass %.
[0067] As shown in Comparative Example 1, the zirconia fine particles not coated with a metal compound had a tetragonal ratio of 0%, i.e., a monoclinic ratio of 100%, after firing at 1000°C, whereas Examples 1 to 13 showed a tetragonal ratio of 20% or more. As shown in Examples 1 to 3, it is understood that the tetragonal crystal ratio after firing increases by increasing the content of yttrium hydroxide, which is a coating compound. In particular, under these firing conditions, as shown in Examples 2 and 3, when the content is 12 mol% or more calculated as yttrium hydroxide, the tetragonal crystal ratio after firing is 95% and 93%, respectively, and it is presumed that Y enters the zirconia crystal lattice and effectively acts as a tetragonal crystal stabilizing element. As shown in Comparative Example 2, when the material was directly coated with yttria without using Y ions, the tetragonal crystal ratio was 64%, which is about 30% lower than that of Example 2, in which the surface was coated using an aqueous Y ion solution. This is thought to be due to the uneven coating of Y, as shown in the SEM-EDX mapping photograph in Figure 2, and it is easy to infer that the physical properties are unstable. In addition, since an impurity phase derived from the stabilizer is generated, there is a concern that this will affect the deterioration of properties such as strength when the material is sintered. As shown in Examples 4 to 10, the metal compound acting as a stabilizer can be not only Y, but also hydroxides and carbonates (including hydrates of carbonates) of Mg, Ca, and Al. It is also possible to combine these metal compounds. As shown in Example 6, even when raw material microparticles (particle diameter: 20 nm) mainly composed of monoclinic crystals were used as the raw material microparticles, the crystal structure after firing at 1000°C had a tetragonal ratio of 95%, showing results equivalent to those of Example 4. As shown in Example 11, even if the amount of yttrium nitrate charged was reduced, it was possible to coat the zirconia fine particles. As shown in Examples 12 and 13, it was possible to coat the zirconia fine particles even when the amount of yttrium nitrate added was increased. In Examples 12 and 13, it was presumed from the observation of the XRD pattern of yttria that some yttria was not dissolved.
[0068] <Examples 14 to 21, Comparative Example 3> The effect of the size of the zirconia particles (hereinafter referred to as raw material particles) used in the coating process will be explained. Because the raw material particles used have a wide particle size distribution, the particle size was evaluated here in terms of the specific surface area.
[0069] In accordance with Example 2, the raw material fine particles having the specific surface area shown in Table 2 were used to obtain coated zirconia fine particles. The raw material fine particles were the same as the raw material fine particles used in Example 14 (specific surface area: 140 m 2The specific surface area was adjusted by firing the powder (w / g). The coating compound was uniformly set to 12 mol% in terms of yttrium hydroxide. The obtained coated zirconia fine particles were fired at 1000°C in the same manner as in Examples 1 to 13, and the crystal structure was evaluated by XRD measurement. The tetragonal crystal ratio after firing and the specific surface area of the raw material fine particles are shown in Table 2.
[0070] [Table 2]
[0071] As shown in Table 2, it can be seen that the tetragonal crystal ratio increases as the specific surface area of the raw material fine particles increases. Under these firing conditions, particularly in Examples 14 to 17, that is, in the case where the specific surface area is 75 to 140 m 2 / g range, the tetragonal crystal ratio is approximately 90%, and Y acts more effectively as a tetragonal crystal stabilizing element. This is thought to be because the smaller the particle size, the more uniformly Y is dissolved at the molecular level.
[0072] <Reference examples 1~4> The degree of densification of the sintered body made of the coated zirconia fine particles was evaluated. [Preparation of sintered body] A green body was produced using 4 g of the coated zirconia fine particle powder at a pressure of 0.5 t using a uniaxial press. To evaluate the densification, the green body was measured with a vernier caliper before and after sintering, and the green body density was compared with the theoretical density of zirconia (6.0 g / cm 3 The relative density (%) was calculated by dividing the sintering temperature by the average sintering time. The sintering temperatures were 200°C for 1 hour, 1000°C for 3 hours, and 1200°C for 3 hours, and the heating rate was 4°C / min from 20°C to 1000°C, and 2°C / min from 1000°C to 1200°C. Table 3 shows the relative density of the sintered bodies. In Reference Example 1, zirconia fine particles not coated with a stabilizer (Comparative Example 1) were used, in Reference Example 2, the coated zirconia fine particles of Example 1 were used, in Reference Example 3, the coated zirconia fine particles of Example 4 were used, and in Reference Example 4, a commercially available partially stabilized zirconia was used.
[0073] [Table 3]
[0074] *1 Relative density (%) = (W / V) / d 0 ×100 W: mass of coated zirconia fine particle powder (g) V: Volume of molded body (cm 3 ) d 0 : Theoretical density of zirconia (= 6.0 g / cm 3 ) *2 The content of the commercially available product in Reference Example 4 is (1) Y 2 O 3 Conversion, (2) is Al 2 O 3 It is a conversion.
[0075] As shown in Reference Example 1, when zirconia fine particles not coated with a stabilizer were used, a green body could not be produced, whereas when zirconia fine particles coated only with yttria in Reference Example 2 were used, a sintered body could be produced without cracking or breaking. As shown in Reference Example 3, when a sintered body was produced using zirconia fine particles whose surfaces were coated with not only yttrium hydroxide but also aluminum hydroxide, it was possible to achieve a greater densification than the commercially available product shown in Reference Example 4.
[0076] Example 22 100 g of the powder of the coated zirconia fine particles obtained in Example 4 was mixed into 500 g of pure water, and acetic acid was added dropwise to adjust the pH to 4 to prepare a mixed liquid. The resulting mixed liquid was stirred with a dispersion stirrer for 30 minutes to perform coarse dispersion. The resulting mixed liquid was subjected to dispersion treatment with a media-type wet disperser. The dispersion liquid of Example 22 was obtained by performing dispersion treatment while checking the particle size during the process. The dispersed particle size of the coated zirconia fine particles in the obtained dispersion liquid was measured by the following method. In addition, as Reference Example 5, a dispersion liquid similarly produced using raw zirconia fine particles that were not coated instead of the coated zirconia fine particles of Example 4 was also evaluated in the same manner. The results are shown in Table 4.
[0077] Example 23 120 g of the powder of the coated zirconia fine particles obtained in Example 4, 30.0 g of 3-methacryloyloxypropyltrimethoxysilane (product name: KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd.), and 250 g of methyl ethyl ketone (MEK) were mixed and stirred with a dispersion stirrer for 30 minutes to perform coarse dispersion. The resulting mixture was dispersed with a media-type wet disperser. A dispersion of Example 23 was obtained by performing a dispersion treatment while checking the particle size during the dispersion. The dispersed particle size of the coated zirconia fine particles in the obtained dispersion was measured by the following method. In addition, as Reference Example 6, a dispersion produced in the same manner using raw zirconia fine particles that were not coated instead of the coated zirconia fine particles of Example 4 was also evaluated in the same manner. The results are shown in Table 4.
[0078] <Method for measuring the particle size of coated zirconia particles in a dispersion> The particle size of the coated or uncoated zirconia fine particles in the dispersion liquid one day after preparation (storage at 25°C) was measured at 25°C using a dynamic light scattering particle size distribution measuring device LB-500 manufactured by Horiba, Ltd. The results are shown in Table 4. It was found that the use of the coated zirconia fine particles of the present invention also makes it possible to prepare a dispersion liquid having a good dispersed state similar to that of uncoated zirconia fine particles.
[0079] [Table 4]
Claims
1. A coated zirconia fine particle comprising a zirconia fine particle and a coating layer coating the surface of the fine particle, the coating layer contains one or more metal elements selected from Mg, Ca, Al, and rare earth elements; The metal element includes at least Y, The average particle size is 3 to 50 nm, Specific surface area is 20 to 500 m 2 / g, Coated zirconia particles.
2. 2. The coated zirconia fine particles according to claim 1, wherein the coating layer contains a compound containing one or more metal elements selected from the group consisting of Mg, Ca, Al and rare earth elements, and the metal elements contain at least Y.
3. 3. The coated zirconia fine particles according to claim 1, wherein the coating layer contains one or more compounds selected from hydroxides of one or more metal elements selected from Mg, Ca, Al and rare earth elements, carbonates of said metal elements and oxides of said metal elements, and said metal elements include at least Y.
4. 4. The coated zirconia fine particles according to claim 1, wherein the coating layer contains 3 to 45 mol % of a compound containing one or more metal elements selected from Mg, Ca, Al, and rare earth elements, relative to the zirconia of the zirconia fine particles, and the metal element contains at least Y.
5. A method for producing coated zirconia fine particles, comprising reacting ions of one or more metal elements selected from Mg, Ca, Al and rare earth elements with an additive which reacts with the ions to form a water-insoluble compound in an aqueous dispersion containing zirconia fine particles, thereby precipitating a compound containing the metal element on the surfaces of the zirconia fine particles to obtain coated zirconia fine particles, comprising the steps of: The metal element includes at least Y, The average particle size of the zirconia fine particles is 3 to 50 nm, The specific surface area of the zirconia fine particles is 20 to 500 m 2 / g. A method for producing coated zirconia fine particles.
6. The method for producing coated zirconia fine particles according to claim 5 , wherein the additive is an alkaline agent.
7. 7. The method for producing coated zirconia fine particles according to claim 5, further comprising the step of removing said additive from the coated zirconia fine particles after the coated zirconia fine particles are obtained.
8. 8. The method for producing coated zirconia fine particles according to claim 5, wherein after the coated zirconia fine particles are obtained, the coated zirconia fine particles are washed with water.
9. 9. The method for producing coated zirconia fine particles according to claim 5, wherein the obtained coated zirconia particles are dried at 200° C. or less.
10. 10. The method for producing coated zirconia fine particles according to claim 5, further comprising mixing the aqueous dispersion, the aqueous solution of the compound containing the metal element, and the additive.
11. A method for producing a zirconia sintered body, comprising the steps of producing coated zirconia fine particles by the method according to any one of claims 5 to 10, and sintering the produced coated zirconia fine particles.
12. A method for producing a dispersion of coated zirconia fine particles, comprising a step of dispersing the coated zirconia fine particles according to any one of claims 1 to 4 in a dispersion medium.
13. A method for producing a nanocomposite, comprising a step of dispersing the coated zirconia fine particles according to any one of claims 1 to 4 in a dispersion medium.
Citation Information
Patent Citations
Zirconia based ceramics in high intensity and toughness, and preparation method
CN1562879A
Stabilized metal oxide and its production
JP1993208819A
Zirconium oxide nanoparticles
JP2017066021A
Exhaust gas clarification catalyst
WO2002066155A1