Adhesives for optical films, coatings and optical films

By integrating a specific polyol-derived structural unit and aromatic polyisocyanate into the polyurethane resin, the adhesive for optical films achieves improved adhesion in high humidity and heat environments, addressing the adhesion issues of conventional polyurethane resin water dispersions.

JP7579308B2Active Publication Date: 2024-11-07DKS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022151908
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-04-04
Filing Date
2022-09-22
Publication Date
2024-11-07
Estimated Expiration
2042-09-22

AI Technical Summary

Technical Problem

Conventional polyurethane resin water dispersions used as adhesives for optical films suffer from insufficient adhesion to substrates, particularly in high humidity and heat environments.

Method used

Incorporating a structural unit derived from a specific polyol, such as a polyester polyol with structures from terephthalic acid and neopentyl glycol, into a polyurethane resin, along with an aromatic polyisocyanate, to create a polyurethane resin with a weight average molecular weight of 5000 to 50000 and an acid value of 5 to 15 mgKOH/g, enhances adhesion.

Benefits of technology

The adhesive exhibits excellent adhesion to substrates even under high humidity and heat conditions, maintaining strong bonding properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579308000001
    Figure 0007579308000001
  • Figure 0007579308000002
    Figure 0007579308000002
Patent Text Reader

Abstract

To provide an adhesive for an optical film which can enhance adhesion to a base material under high humidity heat environment.SOLUTION: An adhesive for an optical film contains a water dispersion containing a polyurethane resin (X), wherein the polyurethane resin (X) has at least a structural unit derived from polyol (A) and a structural unit derived from polyisocyanate (B), the polyol (A) contains polyester polyol (a) having a structure derived from terephthalic acid and a structure derived from neopentyl glycol, and dimethylolpropionic acid (b), the polyol (A) contains 85 mass% or more of the polyester polyol (a), the weight average molecular weight of the polyurethane resin (X) is 5,000-50,000, the polyurethane resin (X) contains 98 mass% or more of a bifunctional component, and the polyurethane resin (X) has an acid value of 5-15 mgKOH / g.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive for optical films, a coating, and an optical film. [Background technology]

[0002] Polyurethane resin aqueous dispersions are capable of forming coating films having excellent mechanical properties, solvent resistance, and water resistance, and are therefore used in a wide range of fields, such as aqueous coating agents, adhesives, etc. From this perspective, active development has been made of polyurethane resin aqueous dispersions with improved dispersibility and polyurethane resin compositions capable of imparting various functions to films when used as adhesives.

[0003] For example, Patent Document 1 discloses a technique for producing an aqueous polyurethane resin dispersion by reacting a raw material containing a fluoropolyether having a hydroxyl group and / or a carboxyl group at its terminal with a polyisocyanate in water. The aqueous polyurethane resin dispersion thus obtained is said to be capable of forming a coating film that is excellent not only in water repellency, oil repellency, and antifouling properties, but also in blocking resistance and surface smoothness. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-145598 Summary of the Invention [Problem to be solved by the invention]

[0005] Polyurethane resin water dispersions are widely used as adhesives in various fields such as optical films, but adhesives using conventional polyurethane resin water dispersions sometimes have insufficient adhesion to substrates, leaving room for improvement. In particular, adhesives using conventional polyurethane resin water dispersions have a problem in that their adhesion is significantly reduced when placed in a high-humidity and heat environment. From this perspective, adhesives for optical films containing polyurethane resin water dispersions are required to have the ability to further increase adhesion to substrates even in a high-humidity and heat environment.

[0006] The present invention has been made in view of the above, and aims to provide an adhesive for optical films, a coating, and an optical film that can improve adhesion to a substrate even in a high-humidity and high-heat environment. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted intensive research to achieve the above object and have found that the above object can be achieved by introducing a structural unit derived from a specific polyol into a polyurethane resin, thereby completing the present invention.

[0008] That is, the present invention includes, for example, the subject matter described in the following sections. Item 1 An adhesive for optical films, comprising an aqueous dispersion containing a polyurethane resin (X), The polyurethane resin (X) has at least a structural unit derived from a polyol (A) and a structural unit derived from a polyisocyanate (B), The polyol (A) contains a polyester polyol (a) having a structure derived from terephthalic acid and a structure derived from neopentyl glycol, and dimethylolpropionic acid (b), The polyol (A) contains 85 mass% or more of the polyester polyol (a), The weight average molecular weight of the polyurethane resin (X) is 5,000 to 50,000; The polyurethane resin (X) contains 98% by mass or more of a bifunctional component, The polyurethane resin (X) has an acid value of 5 to 15 mgKOH / g. Section 2 Item 2. The adhesive for optical films according to item 1, wherein the polyisocyanate (B) includes an aromatic polyisocyanate. Section 3 Item 3. A coating comprising a dried product of the adhesive for optical films according to item 1 or 2. Section 4 Item 4. An optical film comprising the coating according to item 3 as an adhesive layer. Effect of the Invention

[0009] The adhesive for optical films of the present invention can enhance adhesion to substrates even in high humidity and heat environments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expressions "containing" and "comprise" include the concepts of "containing", "comprises", "consists essentially of" and "consists only of".

[0011] The adhesive for optical films of the present invention contains an aqueous dispersion containing a polyurethane resin (X). The polyurethane resin (X) has at least a structural unit derived from a polyol (A) and a structural unit derived from a polyisocyanate (B), and the polyol (A) contains a polyester polyol (a) having a structure derived from terephthalic acid and a structure derived from neopentyl glycol, and dimethylolpropionic acid (b). The polyol (A) contains 85% by mass or more of the polyester polyol (a), the weight average molecular weight of the polyurethane resin (X) is 5000 to 50000, the polyurethane resin (X) contains 98% by mass or more of a bifunctional component, and the polyurethane resin (X) has an acid value of 5 to 15 mgKOH / g. Note that "the polyurethane resin (X) contains 98% by mass or more of a bifunctional component" can be read as "the polyurethane resin (X) contains 98% by mass or more of a bifunctional compound-derived structural unit."

[0012] Because the adhesive for optical films of the present invention contains the polyurethane resin (X), it is possible to form an adhesive that has excellent adhesion to the substrate, and even in a high-humidity and high-heat environment, it is possible to form an adhesive that has excellent adhesion to the substrate.

[0013] The constitution of the aqueous dispersion containing the polyurethane resin (X) (aqueous polyurethane resin dispersion) contained in the adhesive for optical films of the present invention will be described in detail below.

[0014] (Polyol (A)) The polyurethane resin (X) has at least a structural unit derived from the polyol (A).

[0015] In the present invention, the polyol (A) is a composition containing at least two or more compounds having multiple hydroxyl groups (preferably compounds having two hydroxyl groups). In particular, in the present invention, the polyol (A) contains at least a polyester polyol (a) having a structure derived from terephthalic acid and a structure derived from neopentyl glycol, and dimethylolpropionic acid (b). This allows the adhesive for optical films of the present invention to form an adhesive having excellent adhesion to the substrate even in a high humidity and heat environment. Just to be clear, since dimethylolpropionic acid (b) is a compound having two hydroxyl groups, such a compound is a bifunctional compound.

[0016] The polyester polyol (a) is, for example, a compound formed by a dehydration condensation reaction between a glycol compound and a carboxyl group-containing compound, and has a structure derived from the glycol and a structure derived from the carboxyl group-containing compound. Therefore, in the present invention, the polyester polyol (a) is, for example, a polyester polyol compound that can be formed by a dehydration condensation reaction between a glycol containing neopentyl glycol and a carboxyl group-containing compound containing terephthalic acid.

[0017] The polyester polyol (a) may contain a structure derived from other compounds in addition to the structure derived from terephthalic acid and the structure derived from neopentyl glycol, so long as the effects of the present invention are not impaired. Examples of such other compounds include a wide range of compounds used to produce known polyester polyols, such as isophthalic acid, adipic acid, succinic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, maleic anhydride, fumaric acid, 1,3-cyclopentanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, naphthalic acid, biphenyldicarboxylic acid, and 1,2-bis(phenoxy)ethane-p,p'-dicarboxylic acid, and other carboxyl group-containing compounds; anhydrides of such compounds; and glycol components such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycols having a molecular weight of 6000 or less, dipropylene glycol, tripropylene glycol, bishydroxyethoxybenzene, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, bisphenol A, hydrogenated bisphenol A, and hydroquinone.

[0018] Among these, it is preferred that the polyester polyol (a) further has a structure derived from at least one compound selected from the group consisting of adipic acid and ethylene glycol, in which case the adhesive for optical films of the present invention can enhance adhesion to the substrate even in a high-humidity and high-heat environment.

[0019] In the polyester polyol (a), the content ratio of the structure derived from terephthalic acid and the structure derived from neopentyl glycol is not particularly limited. For example, the content ratio of the structure derived from terephthalic acid is preferably 10 to 70 mass%, more preferably 10 to 60 mass%, and even more preferably 15 to 45 mass% relative to the total structural units of the polyester polyol (a). Moreover, the content ratio of the structure derived from neopentyl glycol is preferably 20 to 60 mass%, and more preferably 30 to 55 mass% relative to the total structural units of the polyester polyol (a).

[0020] When the polyester polyol (a) contains a structure derived from other compounds in addition to the structure derived from terephthalic acid and the structure derived from neopentyl glycol, the content ratio of the structure derived from other compounds is not particularly limited. For example, the content ratio of the structure derived from other compounds is preferably 5 to 50 mass%, more preferably 7 to 48 mass%, and even more preferably 10 to 45 mass% relative to the total structural units of the polyester polyol (a). In other words, the content ratio of the structure derived from terephthalic acid and the structure derived from neopentyl glycol is preferably 50 to 95 mass%, more preferably 52 to 93 mass%, and even more preferably 55 to 90 mass% relative to the total structural units of the polyester polyol (a).

[0021] Furthermore, when the polyester polyol (a) has a structure derived from at least one carboxylic acid compound selected from the group consisting of terephthalic acid and adipic acid, the content of these structures is not particularly limited, and is, for example, preferably 70 mass% or less, and more preferably 60 mass% or less, of the total structural units of the polyester polyol (a).

[0022] Furthermore, when the polyester polyol (a) has a structure derived from ethylene glycol, the content of such a structure is not particularly limited, and for example, is preferably 5 mass% or less, and more preferably 3 mass% or less, relative to the total structural units of the polyester polyol (a).

[0023] The polyester polyol (a) preferably contains 98% by mass or more, more preferably 99% by mass or more, of a bifunctional polyester polyol. In these cases, the remainder may be, for example, a trifunctional or higher polyester polyol. The polyester polyol (a) may be composed of only a bifunctional polyester polyol.

[0024] The number average molecular weight of the polyester polyol (a) is not particularly limited, and is, for example, preferably 500 or more, more preferably 1000 or more, and even more preferably 1500 or more, and is preferably 5000 or less, more preferably 4000 or less, and even more preferably 3000 or less.

[0025] The polyester polyol (a) contained in the polyol (A) may be one type alone or two or more types.

[0026] The polyester polyol (a) can be obtained, for example, by a method similar to a known production method, or can be obtained from a commercial product, etc. For example, as described above, the polyester polyol (a) can be produced by a dehydration condensation reaction between a glycol compound and a carboxy group-containing compound.

[0027] The polyol (A) may contain other polyol compounds in addition to the polyester polyol (a) and dimethylolpropionic acid (b). Examples of the other polyol compounds include a wide variety of known polyols, such as polyester polyol compounds other than the polyester polyol (a), polycarbonate polyols, polyether polyols, hydrocarbon polyols, low molecular weight polyols having a molecular weight of 400 or less, and compounds containing at least one active hydrogen group and at least one carboxy group (or a salt thereof) other than the dimethylolpropionic acid (b).

[0028] The polycarbonate polyol is not particularly limited, and can be a wide variety of known polycarbonate polyols for forming urethane resins.For example, the polycarbonate polyol can be a compound obtained by reacting glycols such as 1,4-butanediol, 1,6-hexanediol, and diethylene glycol with diphenyl carbonate and phosgene.The polycarbonate polyol can be obtained, for example, by a method similar to a known manufacturing method, or can be obtained from a commercial product.

[0029] The polyether polyol is not particularly limited, and may be, for example, a wide variety of known polyether polyols for forming urethane resins. For example, polyether polyols obtained by addition polymerization of a polyol compound and an alkylene oxide may be used. Examples of polyol compounds for forming polyester polyols include various aliphatic polyols and alicyclic polyols. Examples of alkylene oxides include alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide. Polyether polyols may be obtained, for example, by a method similar to a known manufacturing method, or may be obtained from a commercially available product. Examples of commercially available products include the "Newpol BPE" (registered trademark) series from Sanyo Chemical Industries, Ltd.

[0030] The hydrocarbon polyol is not particularly limited, and may be, for example, a wide variety of known hydrocarbon polyols for forming urethane resins. For example, the hydrocarbon polyol may be one in which the end of the hydrocarbon chain is terminated with a hydroxyl group, such as polybutadiene polyol, polyisoprene polyol, hydrogenated polybutadiene polyol, or hydrogenated polyisoprene polyol.

[0031] Examples of low molecular weight polyols having a molecular weight of 400 or less include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,3-butanediol, 1,4-butanediol, 3-methylpentanediol (MPD), 1,6-hexanediol (1,6-HD), 1,8-octanediol, 2-methyl-1,3-propanediol, bisphenol A, hydrogenated bisphenol A, cyclohexanedimethanol, glycerin, and trimethylolpropane.

[0032] Examples of compounds containing at least one each of active hydrogen groups and carboxy groups (or salts thereof) (excluding dimethylolpropionic acid (b)) include carboxylic acid-containing compounds such as 2,2-dimethylolbutyric acid, 2,2-dimethylolvaleric acid, dioxymaleic acid, 2,6-dioxybenzoic acid, and 3,4-diaminobenzoic acid, as well as derivatives and salts thereof. Other examples of compounds containing at least one each of active hydrogen groups and carboxy groups (or salts thereof) include amino acids such as alanine, aminobutyric acid, aminocaproic acid, glycine, glutamic acid, aspartic acid, and histidine, and carboxylic acids such as succinic acid, adipic acid, maleic anhydride, phthalic acid, and trimellitic anhydride.

[0033] The polyol (A) contains 85% by mass or more of the polyester polyol (a). That is, the content of the polyester polyol (a) is 85% by mass or more relative to the total mass of the polyol (A). This allows the adhesive for optical films of the present invention to form an adhesive that has excellent adhesion to the substrate even in a high-humidity and high-heat environment. If the content of the polyester polyol (a) is less than 85% by mass relative to the total mass of the polyol (A), the adhesion to the substrate in a high-humidity and high-heat environment decreases. It is more preferable that the polyol (A) contains 85% by mass or more of the bifunctional polyester polyol (a).

[0034] Here, the total mass of the polyol (A) means the total mass of the polyester polyol (a), dimethylolpropionic acid (b), and other polyol compounds (compounds having two or more hydroxyl groups).

[0035] The polyol (A) preferably contains 87% by mass or more of the polyester polyol (a) (preferably a bifunctional polyester polyol (a)), more preferably 90% by mass or more, even more preferably 92% by mass or more, and particularly preferably 95% by mass or more. The polyol (A) preferably contains 99% by mass or less of the polyester polyol (a) (preferably a bifunctional polyester polyol (a)), more preferably 97% by mass or less.

[0036] The content of dimethylolpropionic acid (b) is preferably 1 to 10 parts by mass, more preferably 2 to 8 parts by mass, further preferably 2.5 to 7 parts by mass, and particularly preferably 3 to 6 parts by mass, per 100 parts by mass of the total mass of polyester polyol (a). Dimethylolpropionic acid is also called "2,2-dimethylolpropionic acid".

[0037] The polyol (A) may contain a trifunctional or higher low-chain polyol, but the content is preferably 0.75 mass% or less, more preferably 0.40 mass% or less, and even more preferably 0.30 mass% or less, based on the total mass of the polyol (A). This allows the adhesive for optical films of the present invention to have better adhesion to the substrate even under high humidity and heat conditions. Examples of trifunctional or higher low-chain polyol compounds include polyhydric alcohols having a molecular weight of 150 or less, and specifically, trimethylolpropane and pentaerythritol. The polyol (A) does not need to contain a trifunctional or higher low-chain polyol.

[0038] The polyol (A) preferably contains 98% by mass or more, more preferably 99% by mass or more, of a bifunctional polyol (i.e., a polyol having two hydroxyl groups). In these cases, the remainder may be, for example, a trifunctional or higher polyol. The polyol (A) may be composed only of a bifunctional polyol.

[0039] (Polyisocyanate (B)) The polyurethane resin (X) has a structural unit derived from a polyisocyanate (B). The polyisocyanate (B) is not particularly limited, and may be, for example, a wide variety of polyisocyanate compounds used to form polyurethane resins, such as compounds having two or more isocyanate groups, and more preferably compounds having two isocyanate groups.

[0040] Specific examples of the polyisocyanate (B) include bifunctional isocyanate compounds such as aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, and araliphatic diisocyanates.

[0041] Examples of the aliphatic polyisocyanate include tetramethylene diisocyanate, dodecamethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2-methylpentane-1,5-diisocyanate, and 3-methylpentane-1,5-diisocyanate.

[0042] Examples of alicyclic polyisocyanates include isophorone diisocyanate, hydrogenated xylylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate (hereinafter, can be referred to as "H12MDI"), 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, 1,3-bis(isocyanatemethyl)cyclohexane, and the like.

[0043] Examples of aromatic polyisocyanates include tolylene diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, polymethylene polyphenyl polyisocyanate, 4,4'-dibenzyl diisocyanate, 1,5-naphthylene diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, and 1,4-phenylene diisocyanate.

[0044] Examples of the aromatic aliphatic polyisocyanate include dialkyldiphenylmethane diisocyanate, tetraalkyldiphenylmethane diisocyanate, α,α,α,α-tetramethylxylylene diisocyanate, and the like.

[0045] In addition, a modified organic polyisocyanate may be used as the polyisocyanate (B). The modified organic polyisocyanate is not particularly limited, and examples thereof include carbodiimide, allophanate, biuret, isocyanurate, and adduct. The polyisocyanate may be used alone or in combination of two or more kinds.

[0046] The number average molecular weight of the polyisocyanate (B) is not particularly limited, but is preferably 100 or more and 400 or less, more preferably 120 or more and 300 or less, and even more preferably 150 or more and 280 or less.

[0047] The polyisocyanate (B) is preferably an aromatic polyisocyanate, more preferably a bifunctional aromatic polyisocyanate. The aromatic polyisocyanate is preferably tolylene diisocyanate (TDI) or 4,4'-diphenylmethane diisocyanate (MDI).

[0048] The polyisocyanate (B) can be obtained by a known production method, or can be obtained from a commercial product. The polyisocyanate (B) may be one type alone or may contain two or more types.

[0049] The polyisocyanate (B) preferably contains 98% by mass or more, more preferably 99% by mass or more, of a difunctional isocyanate. In these cases, the remainder may be, for example, a trifunctional or higher polyisocyanate. The polyisocyanate (B) may be composed only of a difunctional polyol.

[0050] (Polyurethane resin (X)) The polyurethane resin (X) has a structural unit derived from the polyol (A) and a structural unit derived from the polyisocyanate (B). In addition to these structural units, the polyurethane resin (X) may also contain, for example, a structure derived from a blocking agent or a structure derived from a chain extender, which will be described later. The polyurethane resin (X) may also be formed only from the structural unit derived from the polyol (A) and the structural unit derived from the polyisocyanate (B).

[0051] The polyurethane resin (X) may have a structural unit derived from a compound having a monofunctional active hydrogen group, which will be described later. When the polyurethane resin (X) contains a structural unit derived from a compound having a monofunctional active hydrogen group, the content of the structural unit is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less, based on the total structural units of the polyurethane resin (X). This allows the adhesive for optical films of the present invention to have excellent adhesion to the substrate even under high humidity and heat conditions.

[0052] In addition, the polyurethane resin (X) may have a structural unit derived from a short-chain amine compound such as a polyamine (chain extender) used as a chain extender described below.

[0053] In the polyurethane resin (X), the content ratio of each structural unit is not particularly limited. For example, the polyurethane resin (X) preferably contains 5 to 50 parts by mass, and more preferably 10 to 40 parts by mass, of the structural unit derived from the polyisocyanate, relative to 100 parts by mass of the total of the structural units derived from the polyol (A) and the structural units derived from the polyisocyanate (B).

[0054] The polyurethane resin (X) contains 98% by mass or more of a bifunctional constituent (i.e., a constituent unit derived from a bifunctional compound). This allows the adhesive for optical films of the present invention to have superior adhesion to the substrate even under high humidity and heat environments. The polyurethane resin (X) preferably contains 99% by mass or more of a bifunctional constituent. The polyurethane resin (X) may be formed only from a bifunctional constituent. Here, the bifunctional constituent is, for example, a bifunctional polyol (A) and a bifunctional polyisocyanate (B).

[0055] When the polyurethane resin (X) has a structure derived from a tri- or higher functional compound, the content thereof is preferably 3 mass % or less, more preferably 0.75 mass % or less, further preferably 0.40 mass % or less, and particularly preferably 0.30 mass % or less, based on the total mass of the polyurethane resin (X).

[0056] In the present invention, the weight average molecular weight of the polyurethane resin (X) is 5,000 to 50,000. This allows the adhesive for optical films of the present invention to have excellent adhesion to a substrate even in a high-humidity and heat environment. If the weight average molecular weight of the polyurethane resin (X) is less than 5,000, the adhesive for optical films of the present invention will have reduced adhesion to a substrate in a high-humidity and heat environment. If the weight average molecular weight of the polyurethane resin (X) is more than 50,000, the adhesive for optical films of the present invention will have reduced adhesion to a substrate in a high-humidity and heat environment.

[0057] The weight average molecular weight of the polyurethane resin (X) is measured by a GPC apparatus using N,N-dimethylformamide (DMF) as a solvent, and is determined as a polystyrene equivalent value. The specific measurement conditions are as follows. Column: Shodex OHPak SB-806M HQ Column temperature: 50℃ Detector: Differential refractive index detector RID-20A (Shimadzu Corporation) Flow rate: 0.5ml / min That is, in the present invention, the weight average molecular weight of the polyurethane resin is defined by the above-mentioned measurement method, and particularly means the weight average molecular weight of the polyurethane resin of the solvent-soluble component.

[0058] The weight average molecular weight of the polyurethane resin (X) is preferably 7000 or more, more preferably 8000 or more, even more preferably 9000 or more, and particularly preferably 10000 or more. The weight average molecular weight of the polyurethane resin (X) is preferably 48000 or less, more preferably 45000 or less, even more preferably 43000 or less, and particularly preferably 40000 or less.

[0059] In the present invention, the polyurethane resin (X) has an acid value of 5 to 15 mgKOH / g. In this case, the adhesive for optical films of the present invention is an adhesive that is particularly excellent in adhesion to the substrate even under a high humidity and heat environment. If the acid value is less than 5 mgKOH / g, the adhesion decreases, and moreover, emulsification and dispersion are difficult in the production of the polyurethane resin (X), making it difficult to form the adhesive. If the acid value exceeds 15 mgKOH / g, the adhesion decreases significantly. The acid value of the polyurethane resin (X) is more preferably 7 mgKOH / g or more, even more preferably 8 mgKOH / g or more, and particularly preferably 9 mgKOH / g or more. The acid value of the polyurethane resin (X) is more preferably 14 mgKOH / g or less, and even more preferably 13 mgKOH / g or less.

[0060] The method for adjusting the acid value is not particularly limited, and for example, a wide variety of known methods can be used. For example, the acid value of the polyurethane resin (X) can be adjusted by adjusting the ratio of the components constituting the polyol (A).

[0061] The acid value of the polyurethane resin composition can be measured in accordance with JIS K0070-1992.

[0062] (Polyurethane resin water dispersion) The polyurethane resin water dispersion contains the polyurethane resin (X) as a solid content and a solvent containing water as a medium. The solvent may be water alone or a mixed solvent of water and a lower alcohol compound having 1 to 3 carbon atoms.

[0063] The content of the polyurethane resin in the polyurethane resin water dispersion is not particularly limited. For example, the polyurethane resin may be contained in an amount of 10 to 50 parts by mass, and preferably 20 to 40 parts by mass, per 100 parts by mass of the aqueous solvent.

[0064] In the polyurethane resin water dispersion, the particle size of the polyurethane resin (X) is not particularly limited, and may be, for example, within the same range as the particle size of the polyurethane resin in a known polyurethane resin water dispersion for adhesives. For example, the volume average particle size D50 of the polyurethane resin (X) is 1 to 500 nm, preferably 3 to 300 nm, more preferably 5 to 250 nm.

[0065] The polyurethane resin water dispersion may contain components other than the polyurethane resin (X) and water, and may contain, for example, raw materials used in producing the polyurethane resin water dispersion. Such raw materials include, for example, surfactants, unreacted monomers, unreacted chain extenders, by-products, catalysts, etc. Examples of the catalyst include metal catalysts and amine catalysts. Examples of the metal catalyst include tin catalysts such as dibutyltin dilaurate, dioctyltin dilaurate, and dibutyltin dioctate, lead catalysts such as lead octylate, lead octenate, and lead naphthenate, and bismuth catalysts such as bismuth octylate and bismuth neodecanoate. Examples of the amine catalyst include tertiary amine compounds such as triethylenediamine, etc.

[0066] The method for producing the polyurethane resin is not particularly limited, and for example, a wide variety of known production methods can be used. In particular, it is preferable to produce the polyurethane resin by a production method utilizing emulsion dispersion, which will be described later.

[0067] The method for producing the polyurethane resin water dispersion is not particularly limited, and for example, any known method for producing a polyurethane resin water dispersion can be widely adopted. In particular, it is preferable to produce the polyurethane resin water dispersion by a production method utilizing an emulsified dispersion.

[0068] In a production method using emulsion dispersion, for example, a urethane prepolymer is prepared by mixing polyol (A) and polyisocyanate (B), and this urethane prepolymer is then emulsified and dispersed to produce polyurethane resin (X), thereby obtaining an aqueous polyurethane resin dispersion.

[0069] The mixing treatment can be carried out in a solvent. Such a solvent is preferably inactive to isocyanate groups and capable of dissolving the urethane prepolymer produced. From this viewpoint, examples of the solvent include dioxane, methyl ethyl ketone, dimethylformamide, tetrahydrofuran, N-methyl-2-pyrrolidone, acetone, toluene, dioxane, ethyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate. It is preferable to finally remove the solvent used in the reaction.

[0070] The temperature of the mixing treatment is not particularly limited, and can be, for example, 30°C to 130°C. The time of the mixing treatment can be appropriately set according to the temperature, and is, for example, 0.5 hours to 10 hours. The reaction of the polyol (A) and the polyisocyanate (B) proceeds by the mixing treatment, and a urethane prepolymer is generated. When the mixing treatment is performed using a solvent, a urethane prepolymer solution is obtained. After the urethane prepolymer is generated, it can be neutralized with a neutralizing agent as necessary before emulsifying and dispersing.

[0071] Examples of the neutralizing agent include non-volatile bases such as sodium hydroxide and potassium hydroxide, tertiary amines such as trimethylamine, triethylamine, dimethylethanolamine, methyldiethanolamine and triethanolamine, and volatile bases such as ammonia.

[0072] A blocking agent can be added to the urethane prepolymer solution before or after the neutralization treatment, or preferably at the same time as the neutralization treatment. The blocking agent has the effect of reacting with the remaining NCO group to terminate the reaction. This makes it easier to adjust the molecular weight of the polyurethane resin (X). A wide variety of known blocking agents can be used as the blocking agent, and examples thereof include compounds having a monofunctional active hydrogen group, specifically, monohydric alcohol compounds and monohydric amino compounds (e.g., dibutylamine). The amount of the blocking agent used can be 5 parts by mass or less, preferably 3 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.8 parts by mass or less, based on 100 parts by mass of the total mass of the polyol (A) and the polyisocyanate (B).

[0073] In the mixing treatment, the amounts of the polyol (A) and the polyisocyanate (B) used are not particularly limited, and can be appropriately adjusted depending on the composition of the intended polyurethane resin.

[0074] The method for emulsifying and dispersing the urethane prepolymer obtained by the mixing process is not particularly limited, and a wide variety of known methods can be used. For example, the urethane prepolymer can be emulsified and dispersed by mixing a solution of the urethane prepolymer with an aqueous solvent and applying shear with an emulsifying disperser such as a homogenizer. The aqueous solvent may contain the neutralizing agent as necessary.

[0075] At the same time as or after the emulsification dispersion, a chain extender can be added to extend the chain. This generates urea bonds by interfacial polymerization reaction between the isocyanate group in the emulsion micelle and the chain extender, improving the crosslinking density in the emulsion micelle and forming a three-dimensional crosslinked structure. Even if a chain extender is not used, the water molecules present in the system can cause chain extension by emulsifying and dispersing the urethane prepolymer in water. The chain extender can include the polyamine. In this case, the polyurethane resin (X) finally produced has a structural unit derived from the polyamine.

[0076] Examples of polyamines (chain extenders) include diamine compounds and polyamine compounds. Examples of diamine compounds include ethylenediamine, trimethylenediamine, piperazine, isophoronediamine, diethylenetriamine, dipropylenetriamine, and amino group-containing silane coupling agents, and examples of polyamine compounds include diethylenetriamine, dipropylenetriamine, and triethylenetetramine. Other examples of polyamines include polycarbodiimide compounds, such as a crosslinking agent for Carbodilite aqueous resins from Nisshinbo Chemical Co., Ltd.

[0077] When a chain extender (polyamine) is used, the amount used is not particularly limited. For example, the amount of the chain extender used can be adjusted so that the equivalent ratio of the isocyanate groups in the urethane prepolymer to the chain extender is 1:0.5 to 1:0.9.

[0078] In emulsifying and dispersing, various surfactants can be used as necessary. Examples of surfactants include nonionic surfactants, anionic surfactants, and cationic surfactants. These surfactants may be used alone or in combination of two or more.

[0079] (Optical film adhesive) The adhesive for optical films of the present invention contains a polyurethane resin aqueous dispersion (aqueous dispersion containing a polyurethane resin (X)). The adhesive for optical films of the present invention can have the same configuration as known adhesives for optical films, so long as it contains a polyurethane resin aqueous dispersion. The adhesive for optical films can also contain other components such as additives in addition to the polyurethane resin aqueous dispersion.

[0080] A film can be formed using the adhesive for optical films of the present invention. The film formed using the adhesive for optical films of the present invention contains a dried product of the adhesive for optical films (i.e., a dried product of the aqueous dispersion of the polyurethane resin composition). Such a film can, for example, exert an adhesive function, and can increase adhesion to the substrate, and can also increase adhesion to the substrate even under a high humidity and heat environment. In particular, the adhesive for optical films of the present invention is suitable for use with optical films.

[0081] The method for forming the film is not particularly limited, and for example, the film can be formed by a known method. For example, the adhesive for optical films is coated on the surface of a substrate such as an optical film, and the aqueous solvent is volatilized by drying or the like to form a dried product of the polyurethane resin aqueous dispersion, and this dried product can be used as the film. The thickness of the film is not particularly limited, and can be adjusted to an appropriate thickness depending on the application and purpose.

[0082] The type of the optical film is not particularly limited, and can be a wide variety of known optical films.The optical film can be exemplified by films such as polyester resins made of polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, etc.; cyclic polyolefin resins; cellulose acetate resins made of triacetyl cellulose, diacetyl cellulose, etc.; polycarbonate resins; acrylic resins; and olefin resins such as polyethylene and polypropylene.

[0083] The optical film may have the coating (a coating formed from the adhesive for optical films of the present invention) as an adhesive layer. The method of forming the coating on the optical film is not particularly limited, and for example, the coating can be formed on the optical film by coating the optical film with the adhesive for optical films. By bonding such a coating (adhesive layer) to other members, a laminate including the optical film can be obtained. Examples of other members include ultraviolet curing resins described below.

[0084] The adhesive for optical films of the present invention is preferably used to bond the optical film and an ultraviolet curing resin. The ultraviolet curing resin is not particularly limited, and examples thereof include acrylic resins, silicone resins, polyester resins, urethane resins, amide resins, and epoxy resins. The ultraviolet curing resin can be formed into, for example, a plate shape, a film shape, or the like.

[0085] When the optical film and the ultraviolet curable resin are bonded together using the adhesive for optical films of the present invention, the optical film is preferably made of polyethylene terephthalate.

[0086] The optical film having the coating as an adhesive layer has high adhesion between the substrate (optical film) and the coating even in a high-humidity and heat environment. In addition, even when another substrate (e.g., a PET substrate) is adhered to the adhesive layer of the optical film, the other substrate can be adhered more firmly, and can be adhered firmly even in a high-humidity and heat environment. EXAMPLES

[0087] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.

[0088] (Raw materials used) Appropriate raw materials were selected from the following raw materials to prepare an aqueous polyurethane resin dispersion. <Polyol (A)> Polyester polyol (a-1) (number average molecular weight 2000, acid value 0.5 mg KOH / g) Polyester polyol (a-2) (number average molecular weight 1000, acid value 0.5 mg KOH / g) Polyester polyol (a-3) (number average molecular weight 2000, acid value 0.5 mg KOH / g) Dimethylolpropionic acid (b) (2,2-dimethylolpropionic acid); (Bis-MPA (registered trademark) manufactured by Perstorp) (functional group number 2, molecular weight 134.13) Trimethylolpropane Sanyo Chemical Industries, Ltd.'s "Newpol BPE-20NK" (registered trademark); other polyols

[0089] Polyester polyol (a-1), polyester polyol (a-2) and polyester polyol (a-3) were produced according to the recipe shown in Table 1 below. Terephthalic acid, adipic acid, neopentyl glycol and ethylene glycol were charged into a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank and a nitrogen gas inlet tube according to the recipe in Table 1, and the temperature was raised to 250°C while stirring under a nitrogen stream. After the reaction was continued until the acid value was 5 or less, the pressure was gradually reduced and a deglycolization reaction was carried out at 1 mmHg for 5 hours to obtain solutions of polyester polyol (a-1), polyester polyol (a-2) and polyester polyol (a-3).

[0090] [Table 1]

[0091] <Polyisocyanate (B)> ·4,4'-Diphenylmethane diisocyanate (MDI) Tolylene diisocyanate (TDI)

[0092] <Blocking agents and neutralizing agents> Dibutylamine (blocking agent) ·Triethylamine (neutralizer) Ammonia (neutralizer)

[0093] A polyurethane resin water dispersion was prepared by the following procedure according to the formulation shown in Table 2. In the formulation conditions (column of raw materials used) shown in Table 2, the unit is "parts by mass", and a blank column means that the raw material was not used (i.e., "0").

[0094] Example 1 Polyol (A) consisting of 81.45 parts by mass of polyester polyol (a-1) and 2.63 parts by mass of dimethylolpropionic acid (b), polyisocyanate (B) consisting of MDI (15.92 parts by mass), and methyl ethyl ketone (100 parts by mass) were mixed and reacted at 70 to 75 ° C for 120 minutes to obtain a urethane prepolymer solution. This urethane prepolymer solution was cooled to 35 ° C, and neutralized by adding 0.11 parts by mass of dibutylamine as a blocking agent and 1.88 parts by mass of triethylamine as a neutralizing agent, and then emulsified and dispersed using a homogenizer while gradually adding water. Thereafter, methyl ethyl ketone was distilled off, and an aqueous dispersion containing a polyurethane resin having a weight average molecular weight of 30800 and an acid value of 11 was obtained, as shown in Table 2.

[0095] (Examples 2 to 12) A polyurethane resin-containing aqueous dispersion was obtained in the same manner as in Example 1, except that the types and amounts of raw materials used were changed as shown in Table 2.

[0096] (Comparative Examples 1 to 6) A polyurethane resin-containing aqueous dispersion was obtained in the same manner as in Example 1, except that the types and amounts of the raw materials used were changed as shown in Table 2. In Comparative Example 6, the acid value was too small to emulsify and disperse the resin, and the intended polyurethane resin-containing aqueous dispersion could not be obtained.

[0097] [Table 2]

[0098] (Evaluation method) Using the aqueous dispersions containing the polyurethane resins obtained in the respective Examples and Comparative Examples, "initial adhesion (PET)", "adhesion under high humidity and heat (PET)", "adhesion when three layers are stacked", and "adhesion when three layers are stacked under high humidity and heat" were evaluated as follows.

[0099] <Initial adhesion (PET)> The adhesion between the polyurethane resin adhesive and PET was evaluated by the following method. A substrate (polyethylene terephthalate (PET) ("Lumirror T-60", Toray Industries)) was degreased with isopropyl alcohol, and then an aqueous dispersion containing polyurethane resin was applied with a bar coater to a dry film thickness of 10 μm, dried at 80° C. for 10 minutes, and further dried at 120° C. for 10 minutes to obtain test piece A coated with polyurethane resin adhesive (film). A 2 mm cross-cut test was performed using this test piece A as a sample, and the adhesion between the polyurethane resin adhesive and PET was evaluated using the following formula: Adhesion (%) = 100 - (number of peeled squares) The adhesion was calculated by the above formula, and a value of 95% or more was considered to be acceptable.

[0100] <Adhesion when three layers are stacked> The adhesion between the polyurethane resin adhesive and PET in a three-layered state was evaluated by the following method. A UV-curable resin formulation was applied to the polyurethane resin adhesive of the test piece A with a bar coater to a dry film thickness of 7 μm, dried at 80° C. for 1 minute to remove the solvent, and then 600 mJ / cm 2 was applied to the surface to which the UV-curable resin formulation was applied using a high-pressure mercury lamp. 2 The specimen was irradiated with ultraviolet light of 1000 nm to obtain a test piece B. A UV-curable resin formulation was prepared using 30 parts by mass of methyl ethyl ketone, 68 parts by mass of epoxy acrylate (GX-8821L-M9, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and 2 parts by mass of a photopolymerization initiator (Irgacure 184, manufactured by Ciba Specialty Chemicals Co., Ltd.). A 2 mm cross-cut test was carried out using this test piece B as a sample, and the adhesion between the UV-curable resin, the polyurethane resin adhesive, and the PET was evaluated according to the following formula: Adhesion (%) = 100 - (number of peeled squares) The adhesion was calculated by the above formula, and a value of 70% or more was deemed to be acceptable.

[0101] <Adhesion under high humidity and heat (PET)> The test piece A was stored at a temperature of 85°C and a humidity of 85% for 168 hours, then dried at room temperature, and a 2 mm cross-cut test was carried out to evaluate the adhesion between the polyurethane resin adhesive and the PET using the following formula: Adhesion (%) = 100 - (number of peeled squares) The adhesion was calculated by the above formula, and a value of 60% or more was deemed to be acceptable.

[0102] <Adhesion under high humidity and heat when three layers are stacked> The test piece B was stored at a temperature of 85°C and a humidity of 85% for 168 hours, then dried at room temperature and subjected to a 2 mm cross-cut test to evaluate the adhesion between the UV-curable resin, the polyurethane resin adhesive, and the PET using the following formula: Adhesion (%) = 100 - (number of peeled squares) The adhesion was calculated by the above formula, and a value of 50% or more was deemed to be acceptable.

[0103] <Haze> The haze of the resulting polyurethane resin adhesive was measured in accordance with JIS K 7136:2000 using a turbidity meter (NDH4000, manufactured by Nippon Denshoku Corporation).

[0104] Table 2 shows the blending conditions used in producing the polyurethane resin aqueous dispersions prepared in each Example and Comparative Example, and the evaluation results of the adhesives obtained from those polyurethane resin aqueous dispersions. In Table 2, the unit of the acid value of the polyurethane resin is mgKOH / g.

[0105] From the results in Table 2, it was found that the polyurethane resin aqueous dispersions obtained in the Examples can form adhesives having excellent adhesion to substrates (PET films), and can form adhesives having excellent adhesion to substrates even in a high humidity and heat environment. In addition, the polyurethane resin aqueous dispersions obtained in the Examples had an acceptable level of adhesion even in a high humidity and heat environment when three layers were stacked, and therefore were also found to be capable of firmly bonding a substrate (PET film) and an ultraviolet curable resin. In Comparative Example 4, the total amount of bifunctional components was less than 98% by mass relative to the polyurethane resin, and therefore the adhesion to the substrate decreased in a high humidity and heat environment.

Claims

1. An adhesive for optical films, comprising an aqueous dispersion containing a polyurethane resin (X), The polyurethane resin (X) has at least a structural unit derived from a polyol (A) and a structural unit derived from a polyisocyanate (B), The polyol (A) contains a polyester polyol (a) having a structure derived from terephthalic acid and a structure derived from neopentyl glycol, and dimethylolpropionic acid (b), The polyol (A) contains 85% by mass or more of the polyester polyol (a), The polyisocyanate (B) consists of an aromatic polyisocyanate alone, The weight average molecular weight of the polyurethane resin (X) is 5,000 to 50,000; The polyurethane resin (X) contains 98% by mass or more of a bifunctional component, The adhesive for optical films, wherein the polyurethane resin (X) has an acid value of 5 to 15 mgKOH / g.

2. A coating comprising a dried product of the adhesive for optical films according to claim 1 .

3. An optical film comprising the coating according to claim 2 as an adhesive layer.

Citation Information

Patent Citations

  • Aqueous coating composition

    JP1994145598A

  • optical film

    JP2016540659A

  • Urethane resin composition, steel sheet surface treatment agent, and steel sheet having coating film of same