Positive electrode active material and lithium secondary battery including the same

A lithium composite oxide with a concentration gradient of doping metals in secondary particles addresses the stability issues of high-Ni type electrodes, enhancing electrochemical performance and structural stability in lithium secondary batteries.

JP7579310B2Active Publication Date: 2024-11-07ECOPRO BM CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022159874
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-06
Filing Date
2022-10-04
Publication Date
2024-11-07
Estimated Expiration
2042-10-04

AI Technical Summary

Technical Problem

High-Ni type positive electrode active materials for lithium secondary batteries face a trade-off between high capacity characteristics and structural stability, leading to rapid deterioration at high and room temperatures due to Li/Ni cation mixing and the generation of LiOH and Li2CO3 by-products, which cause swelling and reduce cycle life.

Method used

A positive electrode active material with a lithium composite oxide structure that includes nickel, cobalt, and a doping metal, where secondary particles are formed by aggregating primary particles with a concentration gradient of the doping metal from the grain boundaries toward the center, reducing Li by-products and stabilizing the structure through controlled concentration gradients.

Benefits of technology

The concentration gradient stabilizes the structure, reducing side reactions and Li by-products, thereby improving electrochemical properties and extending the life and efficiency of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579310000015
    Figure 0007579310000015
  • Figure 0007579310000016
    Figure 0007579310000016
  • Figure 0007579310000017
    Figure 0007579310000017
Patent Text Reader

Abstract

To provide a positive electrode active material with improved electrochemical characteristics and stability and a lithium secondary battery using a positive electrode including the same.SOLUTION: In secondary particles formed by aggregation of multiple primary particles, aggregates of primary particles in which a doping metal concentration gradient is formed in a direction from the grain boundary between the primary particles toward the center of the primary particles.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material having improved electrochemical properties and stability, the secondary particles being formed by agglomeration of a plurality of primary particles, the secondary particles being provided as agglomerates of primary particles in which a concentration gradient of a doping metal is formed in a direction from a grain boundary between the primary particles toward a center of the primary particles, and a lithium secondary battery using the positive electrode including the same. [Background technology]

[0002] Batteries store electricity by using materials capable of electrochemical reactions at the positive and negative electrodes. A representative example of such batteries is a lithium secondary battery, which stores electrical energy by the difference in chemical potential when lithium ions are intercalated / deintercalated at the positive and negative electrodes.

[0003] The lithium secondary battery is manufactured by using a material capable of reversible intercalation / deintercalation of lithium ions as a positive electrode and a negative electrode active material, and filling an organic electrolyte or a polymer electrolyte between the positive electrode and the negative electrode.

[0004] Lithium composite oxides are used as the positive electrode active material for lithium secondary batteries, and examples of these include LiCoO 2 , LiMn 2 O 4 , LiNiO 2 , LiMnO 2 Composite oxides such as these are being researched.

[0005] Among the positive electrode active materials, LiCoO 2 is the most widely used due to its excellent life characteristics and charge / discharge efficiency, but has the disadvantage of being expensive due to the limited availability of cobalt as a raw material, limiting its price competitiveness.

[0006] LiMnO 2 , LiMn2 O 4 Lithium manganese oxides such as LiNiO have the advantages of being thermally safe and inexpensive, but they have problems such as small capacity and poor high-temperature properties. 2 Although these positive electrode active materials show high discharge capacity as battery characteristics, they are difficult to synthesize due to the problem of cation mixing between Li and transition metals, which causes serious problems in rate characteristics.

[0007] In addition, a large amount of Li by-products will be generated depending on the depth of such cation mixing. Most of these Li by-products are LiOH and Li 2 CO 3 This causes problems such as gelling during the manufacture of the positive electrode paste and gas generation during charge and discharge after the electrode is manufactured. 2 CO 3 Not only does it increase cell swelling and reduce cycles, it also causes the battery to swell.

[0008] To make up for these shortcomings, the demand for high-Ni type positive electrode active materials with Ni content of 50% or more as positive electrode active materials for secondary batteries has increased. However, while such high-Ni type positive electrode active materials exhibit high capacity characteristics, they have the problem of structural instability due to Li / Ni cation mixing caused by the increased Ni content in the positive electrode active material. Due to the structural instability of such positive electrode active materials, lithium secondary batteries can rapidly deteriorate not only at high temperatures but also at room temperature.

[0009] Meanwhile, there are prior arts such as Korean Patent Publication No. 10-2014-0022681 (Patent Document 1) that relate to positive electrode active materials for lithium secondary batteries.

[0010] The above-mentioned Patent Document 1 discloses that, among the compounds represented by Chemical Formula 1 below, a doping metal represented by Me can improve the electrochemical properties of a positive electrode active material by forming a concentration gradient that decreases from the surface to the center of a positive electrode active material particle.

[0011] Li 1+X M 1-k Me k O 2

[0012] However, the reality is that the concentration gradient of the doping metal present only in a limited manner on the surface of the positive electrode active material (secondary particles) is insufficient to simultaneously improve the electrochemical properties and structural stability of the positive electrode active material (especially in the case of high-Ni).

[0013] Therefore, the reality is that there is a need to develop a positive electrode active material that can overcome the problems of such high-Ni type positive electrode active materials. [Prior art documents] [Patent documents]

[0014] [Patent Document 1] Korean Patent Publication No. 10-2014-00022681 (Publication date 2014.02.25) Summary of the Invention [Problem to be solved by the invention]

[0015] As described above, a certain trade-off relationship may be established between some indicators showing the electrochemical properties of the positive electrode active material and some indicators showing the stability of the positive electrode active material for lithium secondary batteries. Therefore, if the capacity characteristics of the positive electrode active material are excessively improved, the structural stability of the particles constituting the positive electrode active material may be reduced, and the positive electrode active material may not exhibit stable charge and discharge performance.

[0016] Therefore, an object of the present invention is to provide a positive electrode active material that can maintain the high electrochemical properties of existing positive electrode active materials for lithium secondary batteries, particularly high-Ni type positive electrode active materials, while eliminating the low structural stability.

[0017] Specifically, an object of the present invention is to provide a positive electrode active material having improved electrochemical properties and stability, in which secondary particles are formed by agglomerating a plurality of primary particles, and the secondary particles are provided as agglomerates of primary particles in which a concentration gradient of a doping metal is formed in a direction from a crystal grain boundary between the primary particles to a center of the primary particles.

[0018] It is yet another object of the present invention to provide a lithium secondary battery using a positive electrode comprising the positive electrode active material defined herein. [Means for solving the problem]

[0019] According to one aspect of the present invention, there is provided a positive electrode active material comprising a layered lithium composite oxide that contains at least nickel, cobalt and a doping metal and is capable of intercalating / deintercalating lithium.

[0020] Here, the lithium composite oxide includes secondary particles which are aggregates in which a plurality of primary particles are aggregated to form crystal grains between adjacent primary particles, and the secondary particles are aggregates of primary particles in which the concentration of the doping metal exhibits a negative concentration gradient from the crystal grain boundaries between the primary particles toward the center of the primary particles.

[0021] Here, the primary particles are represented by the following formula 1.

[0022] Li a Ni 1-(b+c+d+e) Co b M1 c M2 d M3 e O f

[0023] (where: M1 is at least one selected from Mn and Al; M2 and M3 are each independently selected from Al, Ba, B, Ce, Cr, Mg, Mn, Mo, Na, K, P, V, Sr, Ti, W, Nb, and Zr; M1 to M3 are different from each other, [ka]

[0024] In one embodiment, the secondary particles may be aggregates of primary particles that exhibit a concentration gradient in which the concentration of at least one selected from M2 and M3 decreases from the grain boundaries between the primary particles toward the center of the primary particles.

[0025] In addition, there may be a first concentration gradient section in which the concentration of the doping metal has a (-) gradient from the surface portion of the secondary particle to the center portion of the secondary particle, and a second concentration gradient section in which the concentration of the doping metal has a (+) gradient.

[0026] According to another aspect of the present invention, there is provided a positive electrode comprising the positive electrode active material defined herein.

[0027] Furthermore, according to another aspect of the present invention, there is provided a lithium secondary battery using the positive electrode defined herein. Effect of the Invention

[0028] Generally, high-Ni type positive electrode active materials for realizing high capacity lithium secondary batteries have a problem of low stability. However, the positive electrode active material according to the present invention improves the low stability of high-Ni type positive electrode active materials and contributes to the exhibiting stable electrochemical characteristics by implementing the secondary particles constituting the positive electrode active material as aggregates of primary particles that exhibit a concentration gradient with a (-) gradient of the doping metal concentration from the grain boundaries between primary particles toward the center of the primary particles.

[0029] On the other hand, in the case of high-Ni type positive electrode active material, LiOH and Li are present on the surface compared to positive electrode active material with relatively low Ni content. 2 CO 3 The Li by-products may cause gelation during preparation of a positive electrode paste using the positive electrode active material, or may cause gas generation during charge / discharge and / or storage of a lithium secondary battery.

[0030] However, in the positive electrode active material according to the present invention, a concentration gradient of the doping metal is formed not only on the surface of the secondary particles but also from the grain boundaries between the primary particles constituting the secondary particles, thereby making it possible to reduce the content of Li by-products inside and outside the positive electrode active material.

[0031] In addition, in the positive electrode active material, not only the surfaces of the secondary particles but also the grain boundaries within the secondary particles (i.e., crystal grain boundaries between primary particles) are regions where side reactions with the electrolyte can occur during charging / discharging and / or storage of the lithium secondary battery.

[0032] In this case, the larger the surface area of ​​the positive electrode active material, the larger the area where side reactions can occur, and therefore the higher the possibility of side reactions. Such side reactions can induce phase transformation, which changes the crystal structure of the lithium composite oxide that constitutes the positive electrode active material (e.g., from layered structure to rock salt structure). Such phase transformation of the crystal structure within the surface of the positive electrode active material has been pointed out as one of the causes of the decrease in electrochemical characteristics, such as the life characteristics, of lithium secondary batteries.

[0033] In the positive electrode active material according to the present invention, a concentration gradient of the doping metal is formed not only on the surface of the secondary particles but also from the grain boundaries between the primary particles constituting the secondary particles, thereby reducing the surface area where side reactions with the electrolyte may occur during charging / discharging and / or storage of the lithium secondary battery, thereby improving the charging / discharging and / or storage stability by reducing the possibility of side reactions with the electrolyte during charging / discharging and / or storage of the lithium secondary battery.

[0034] As a result, the positive electrode active material according to the present invention includes secondary particles provided as aggregates of primary particles in which a concentration gradient of a doping metal is formed in a direction from a grain boundary between the primary particles toward a center of the primary particles, which may contribute to improving various physical properties including structural stability of the positive electrode active material as well as electrochemical properties such as life characteristics and efficiency characteristics.

[0035] In addition to the above effects, specific effects of the present invention will be described below while explaining specific matters for carrying out the invention. [Brief description of the drawings]

[0036] [Figure 1] 1 is a graph showing a concentration gradient of secondary particles contained in a cathode active material according to an embodiment of the present invention, the graph shown in FIG. 1 is a graph showing an example of an EDX analysis result obtained by line scanning a doping metal called M2 and / or M3 in a direction from a surface of the secondary particles to a center of the secondary particles. [Diagram 2] 1 is a graph showing a line scanning of the content of doping metal in the secondary particles confirmed through EDX analysis of a cross-sectional SEM image obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Examples 1 to 7 and processing the cross-section using FIB (Ga-ion source). [Diagram 3] 1 is a graph showing a line scanning of the content of doping metal in the secondary particles confirmed through EDX analysis of a cross-sectional SEM image obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Examples 1 to 7 and processing the cross-section using FIB (Ga-ion source). [Figure 4]1 is a graph showing a line scanning of the content of doping metal in the secondary particles confirmed through EDX analysis of a cross-sectional SEM image obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Examples 1 to 7 and processing the cross-section using FIB (Ga-ion source). [Diagram 5] 1 is a graph showing a line scanning of the content of doping metal in the secondary particles confirmed through EDX analysis of a cross-sectional SEM image obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Examples 1 to 7 and processing the cross-section using FIB (Ga-ion source). [Figure 6] 1 is a graph showing a line scanning of the content of doping metal in the secondary particles confirmed through EDX analysis of a cross-sectional SEM image obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Examples 1 to 7 and processing the cross-section using FIB (Ga-ion source). [Figure 7] 1 is a graph showing a line scanning of the content of doping metal in the secondary particles confirmed through EDX analysis of a cross-sectional SEM image obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Examples 1 to 7 and processing the cross-section using FIB (Ga-ion source). [Figure 8] 1 is a graph showing a line scanning of the content of doping metal in the secondary particles confirmed through EDX analysis of a cross-sectional SEM image obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Examples 1 to 7 and processing the cross-section using FIB (Ga-ion source). [Figure 9] 1 is a graph showing line scanning of the doping metal content in the secondary particles confirmed through EDX analysis of a cross-sectional SEM image obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Comparative Examples 1 to 3 and processing the cross-section using FIB (Ga-ion source). [Figure 10] 1 is a graph showing line scanning of the doping metal content in the secondary particles confirmed through EDX analysis of a cross-sectional SEM image obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Comparative Examples 1 to 3 and processing the cross-section using FIB (Ga-ion source). [Figure 11] 1 is a graph showing line scanning of the doping metal content in the secondary particles confirmed through EDX analysis of a cross-sectional SEM image obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Comparative Examples 1 to 3 and processing the cross-section using FIB (Ga-ion source). [Figure 12] 1 is a graph showing the content of doping metal in the secondary particles confirmed through EDX analysis of a cross-sectional SEM image obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Reference Examples 1 and 2 and processing the cross-section using FIB (Ga-ion source), by line scanning. [Figure 13] 13 is a graph showing line scanning of the doping metal content in the secondary particles confirmed through EDX analysis of cross-sectional SEM images obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials according to Reference Examples 1 and 2 and processing the cross-sections using an FIB (Ga-ion source). Here, Figs. 2 to 13 show excerpts of line scanning results from the surface of the secondary particles contained in each positive electrode active material to a depth of 3 μm (3,000 nm). [Figure 14] 1 shows the results of XRD analysis of the positive electrode active materials according to Examples 1 to 3. [Figure 15] 1 shows the results of XRD analysis of the positive electrode active materials according to Examples 1 to 3. [Figure 16] 1 shows the results of XRD analysis of the positive electrode active materials according to Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0037] In order to make the present invention easier to understand, certain terms are defined herein for convenience. Unless otherwise defined herein, scientific and technical terms used in the present invention shall have the meanings commonly understood by those of ordinary skill in the art. Furthermore, unless otherwise specified by the context, singular terms shall be understood to include their plural forms, and plural terms shall be understood to include their singular forms.

[0038] Hereinafter, the positive electrode active material according to the present invention and the lithium secondary battery using the positive electrode containing the positive electrode active material will be described in more detail.

[0039] positive electrode active material According to one aspect of the present invention, there is provided a positive electrode active material including a lithium composite oxide having a layered structure capable of lithium intercalation / deintercalation.

[0040] The lithium composite oxide includes secondary particles that are aggregates of a plurality of primary particles that are aggregated to form grain boundaries between adjacent primary particles.

[0041] Here, a primary particle means a single crystal grain or crystallite, and a secondary particle means an aggregate formed by the aggregation of a plurality of primary particles. The secondary particles may also be called bulk particles. The primary particles may be rod-shaped, elliptical, and / or circular, or may be irregular in shape.

[0042] A gap and / or a grain boundary may exist between the primary particles constituting the secondary particle. For example, the primary particles may be separated from adjacent primary particles inside the secondary particle to form an internal gap. Also, the primary particles may contact adjacent primary particles to form an internal gap without forming a grain boundary, thereby forming a surface present within the secondary particle.

[0043] On the other hand, the surface of the primary particle that is present on the outermost surface of the secondary particle and is exposed to the outside air forms the surface of the secondary particle.

[0044] Here, the average particle size of the primary particles is within a range of 0.1 μm to 10 μm, preferably 0.1 μm to 5 μm, so that the optimal density of the positive electrode manufactured using the positive electrode active material according to various embodiments of the present invention can be realized. Also, the average particle size of the secondary particles may be 3 μm to 20 μm, depending on the number of aggregated primary particles.

[0045] The lithium composite oxide may contain at least nickel, cobalt, and a doping metal. If the lithium composite oxide further contains manganese in addition to nickel, cobalt, and a doping metal, the lithium composite oxide may be an NCM type composite oxide. If the lithium composite oxide further contains aluminum in addition to cobalt and a doping metal, the lithium composite oxide may be an NCA type composite oxide.

[0046] As described above, the secondary particles constituting the lithium composite oxide are aggregates formed by agglomeration of a plurality of primary particles. In this case, the boundary surface between adjacent primary particles or the joining surface between adjacent primary particles may be defined as a grain boundary between the primary particles. In addition, the grain boundary between adjacent primary particles may coincide with the surface of the primary particle forming the grain boundary.

[0047] Here, the primary particles constituting the secondary particles may exhibit a concentration gradient in which the concentration of the doping metal has a negative gradient from the grain boundaries between the primary particles toward the center of the primary particles.

[0048] The change in concentration of the doping metal in the primary particles formed in a direction from the surface portion of the secondary particle toward the center portion of the secondary particle may be measured through EDX analysis (line scanning) of a cross section of the secondary particle.

[0049] If the secondary particles are agglomerates of primary particles that exhibit a concentration gradient with a negative (-) slope for the doping metal from the grain boundaries between the primary particles toward the center of the primary particles, the EDX analysis results for the secondary particles show that the concentration gradient pattern for the doping metal is repeated.

[0050] For example, when line scanning is performed on the primary particles present on the outermost surface of the secondary particles in a direction from the surface of the secondary particles to the center of the secondary particles, a concentration gradient of the doping metal in the primary particles from the outermost surface of the secondary particles with a (-) gradient may appear, and conversely, a concentration gradient of the doping metal in the primary particles relatively close to the center of the secondary particles with a (+) gradient may appear. Even in this case, when viewed based on the primary particles, the concentration of the doping metal in a single primary particle shows a concentration gradient with a (-) gradient from the surface of the primary particles (in this case, the surface of the primary particles means the grain boundary between multiple primary particles) to the center of the primary particles.

[0051] On the other hand, since the concentration of the doping metal exhibits a concentration gradient with a (-) slope from the grain boundary between the primary particles toward the center of the primary particles, when viewed from the secondary particle as a reference, there are a first concentration gradient section with a (-) slope of the doping metal concentration from the surface portion of the secondary particle toward the center of the secondary particle and a second concentration gradient section with a (+) slope. Also, the first concentration gradient section with a (-) slope of the doping metal concentration from the surface portion of the secondary particle toward the center of the secondary particle and the second concentration gradient section with a (+) slope may be alternately present.

[0052] Here, the ordinal numbers used to refer to the concentration gradient sections having a (+) and / or (-) slope are merely used to distinguish between concentration gradient sections having a (+) slope and concentration gradient sections having a (-) slope.

[0053] Also, a concentration gradient with a (+) slope means that the concentration of the doping metal increases significantly between the start and end points of the line scanning. On the other hand, a concentration gradient with a (-) slope means that the concentration of the doping metal decreases significantly between the start and end points of the line scanning. For example, a significant increase or decrease in the concentration of the doping metal means that the concentration change of the doping metal is 2 at% or more between the start and end points of the concentration gradient section.

[0054] Showing a concentration gradient with a slope of (+) means that the gradient of the concentration of the doping metal is (+) between the start point and the end point of the line scanning, and does not take into account changes in the slope due to slight differences in the concentration of the doping metal in a portion of the section between the start point and the end point of the line scanning.

[0055] Similarly, it should be understood that indicating a concentration gradient with a negative slope is sufficient if the gradient for the concentration of the doping metal is negative between the start and end points of the line scanning, thereby not taking into account changes in the slope due to slight differences in the concentration of the doping metal in a portion of the section between the start and end points of the line scanning.

[0056] The primary particles constituting the secondary particles defined in the present application are represented by Chemical Formula 1 below.

[0057] Li a Ni 1-(b+c+d+e) Co b M1 c M2 d M3 e O f

[0058] (where: M1 is at least one selected from Mn and Al; M2 and M3 are each independently selected from Al, Ba, B, Ce, Cr, Mg, Mn, Mo, Na, K, P, V, Sr, Ti, W, Nb, and Zr; M1 to M3 are different from each other, [ka] It is.)

[0059] The primary particles may be a high-Ni type lithium composite oxide in which the concentrations (mol %) of Ni, Co, M1, M2 and M3 in Chemical Formula 1 satisfy the following formula 1.

[0060]

number

[0061] The primary particles may be a high-Ni / low-Co type lithium composite oxide in which the concentrations (mol%) of Ni, Co, M1, M2 and M3 satisfy the formula 1, and the Co content is 10 mol% or less, preferably 5 mol% or less.

[0062] That is, in the primary particles, the concentrations (mol %) of Ni, Co, M1, M2 and M3 in Chemical Formula 1 can satisfy the following Formula 2.

[0063]

number

[0064] It is generally known that in lithium composite oxides containing at least Ni and Co, the structural instability of the lithium composite oxide due to Li / Ni cation mixing increases as the Ni content increases. It has also been reported that in lithium composite oxides containing at least Ni and Co, the initial overpotential (resistance) increases as the Co content decreases, which inevitably leads to a decrease in rate characteristics.

[0065] However, the lithium composite oxide included in the cathode active material according to an embodiment of the present invention exhibits a concentration gradient of the doping metal with a negative gradient from the grain boundary between the primary particles constituting the secondary particles to the center of the primary particles, thereby mitigating and / or preventing the structural instability and the deterioration of the rate characteristics of the high-Ni type or high-Ni / low-Co type lithium composite oxide.

[0066] Meanwhile, in Chemical Formula 1, M2 and / or M3 may correspond to the above-mentioned doping metal, and thus the secondary particles may be aggregates of primary particles exhibiting a concentration gradient in which the concentration of at least one selected from M2 and M3 decreases from the grain boundary between the primary particles toward the center of the primary particles.

[0067] 1 is a graph showing a concentration gradient of secondary particles included in a cathode active material according to an embodiment of the present invention, which is a schematic diagram showing an example of an EDX analysis result in which a doping metal called M2 and / or M3 is line scanned in a direction from the surface of the secondary particle to the center of the secondary particle.

[0068] 1, the concentration of the doping metal may have a negative gradient from the outermost surface of the secondary particle toward the center of the secondary particle, and the section showing the concentration gradient with the negative gradient is referred to as a first concentration gradient section s1.

[0069] In this way, since the concentration of the doping metal has a negative slope from the outermost surface of the secondary particle toward the center of the secondary particle, a first peak (p0) for the concentration of the doping metal may appear at a position on the graph corresponding to the outermost surface of the secondary particle.

[0070] When the average particle size of the primary particles is r, the concentration gradient within the primary particles may exist within a depth of 0.2r from the grain boundaries between the primary particles. If the concentration gradient within the primary particles exists to a depth exceeding 0.2r from the grain boundaries between the primary particles, this may cause instability in the crystal structure within the primary particles or may deteriorate the electrochemical properties.

[0071] Meanwhile, after the first concentration gradient section (s1), a concentration maintaining section (s3) may be present in which the concentration of the doping metal is maintained for a predetermined depth.

[0072] The concentration maintenance section not only means a section in which the concentration of the doping metal does not change significantly and is almost uniform, but also refers to all sections in which the absolute value of the concentration change of the doping metal is 3 at% or less, preferably 2 at% or less. The absolute value of the concentration change of the doping metal in the concentration maintenance section may vary depending on the type of the doping metal and the content of the doping metal in the primary particles, but the concentration change of the doping metal in the concentration maintenance section will be an insignificant change when compared with the first concentration gradient section (s1) and the second concentration gradient section (s2).

[0073] Inside the concentration maintenance section, the concentration of the doping metal may have a (+) gradient toward the center of the secondary particle. In this case, the section where the concentration gradient with the (+) gradient appears is referred to as a second concentration gradient section (s2).

[0074] 1, when the secondary particle is used as a reference, it can be seen that the first concentration gradient section (s1), the concentration maintenance section (s3), and the second concentration gradient section (s2) are repeatedly present from the surface of the secondary particle toward the center of the secondary particle. However, even in this case, it can be seen that the second concentration gradient section (s2) appears through a concentration gradient having a negative slope from the grain boundary between the primary particles toward the center of the primary particle.

[0075] In other words, only when the secondary particle is an agglomeration of primary particles in which the concentration of the doping metal exhibits a concentration gradient with a (-) slope from the crystal grain boundary between the primary particles toward the center of the primary particle, a first concentration gradient section in which the concentration of the doping metal has a (-) slope and a second concentration gradient section in which the concentration of the doping metal has a (+) slope may be repeatedly present from the surface portion of the secondary particle toward the center of the secondary particle.

[0076] Meanwhile, since a first concentration gradient section having a (-) gradient and a second concentration gradient section having a (+) gradient of the doping metal concentration are repeatedly present from the surface portion of the secondary particle toward the center portion of the secondary particle, at least one peak (p1, p2) may appear after a first peak (p0) of the doping metal concentration at a position corresponding to the outermost surface of the secondary particle.

[0077] The second peak (p1) that first appears after the first peak (p0) may appear due to the presence of the first concentration gradient section s1 after the second concentration gradient section (s2). In this case, the second peak (p1) may be formed by the second concentration gradient section (s2) existing in the primary particles existing at the outermost surface of the secondary particles and the first concentration gradient section (s1) existing in the primary particles adjacent to the primary particles. In this case, the second concentration gradient section (s2) existing in the primary particles existing at the outermost surface of the secondary particles and the first concentration gradient section (s1) existing in the primary particles adjacent to the primary particles may be collectively defined as a peak region (a1), and the peak existing in the peak region (a1) may be defined as a second peak (p1). In this case, the position where the second peak p1 appears may be a grain boundary formed between two adjacent primary particles.

[0078] The first concentration gradient section (s1) existing after the first peak (p0) appearing on the surface of the secondary particles can improve the stability on the surface of the secondary particles. For example, the presence of the first concentration gradient section (s1) for the doping metal on the surface of the secondary particles can reduce the content of Li by-products on the surface of the secondary particles or reduce the specific surface area of ​​the secondary particles to reduce the possibility of side reactions with the electrolyte.

[0079] Meanwhile, the primary particles exhibit a concentration gradient with a negative gradient of the doping metal concentration from the grain boundaries between the primary particles toward the center of the primary particles, so that the first concentration gradient section (s1), the concentration maintenance section (s3), and the second concentration gradient section (s2) are sequentially present within the primary particles from the center of the secondary particles toward the surface of the secondary particles. In this manner, the first concentration gradient section (s1), the concentration maintenance section (s3), and the second concentration gradient section (s2) are sequentially present within the primary particles from the center of the secondary particles toward the surface of the secondary particles, so that the structural stability of the primary particles can be improved.

[0080] In addition, the concentration gradient pattern of the doping metal reduces the content of Li by-products not only on the surfaces of the secondary particles but also in the grain boundaries between the primary particles, and reduces the exposed area inside the secondary particles, thereby reducing the possibility of side reactions with the electrolyte.

[0081] Meanwhile, there are a first concentration gradient section (s1) having a negative gradient and a second concentration gradient section (s2) having a positive gradient in the concentration of the doping metal from the surface of the secondary particle to the center of the secondary particle, and it is preferable that the first concentration gradient section (s1) and the second concentration gradient section (s2) are repeated at least twice. In this case, the concentration maintenance section (s3) may be present at least between the first concentration gradient section (s1) and the second concentration gradient section (s2) that exist within the same primary particle.

[0082] The first concentration gradient section (s1) and the second concentration gradient section (s2) are repeated from the surface portion of the secondary particle toward the center portion of the secondary particle, so that a peak region is repeatedly formed from the surface portion of the secondary particle along the depth direction.

[0083] In addition, the peak region may be present not only adjacent to the surface of the secondary particle, but also adjacent to the center of the secondary particle or at the center of the secondary particle. However, in order to make the peak region exist up to the center of the secondary particle depending on the type of doping metal, the content of the raw material containing the doping metal added during the process of synthesizing the positive electrode active material may need to be excessively increased. If the content of the raw material containing the doping metal added during the process of synthesizing the positive electrode active material is excessively high, the content of the doping metal in the primary particles may be unnecessarily high, or the content of the compound derived from the doping metal present at at least a part of the grain boundaries between the primary particles and the surface of the secondary particles may be excessively high, which may rather deteriorate the electrochemical properties and stability of the positive electrode active material.

[0084] Therefore, preferably, the first concentration gradient section (s1) and the second concentration gradient section (s2) are repeated at least two times from the surface portion of the secondary particle toward the center portion of the secondary particle, but the upper limit of the number of times the first concentration gradient section (s1) and the second concentration gradient section (s2) are repeated may be appropriately adjusted in consideration of the composition of the positive electrode active material, the type of the doping metal, etc.

[0085] For example, when the radius of the secondary particle is R, if the first concentration gradient section (s1) and the second concentration gradient section (s2) are limited to a depth of 0 to 0.2R from the surface portion of the secondary particle, this may be advantageous in terms of electrochemical properties and stability of the positive electrode active material.

[0086] If the first concentration gradient section (s1) and the second concentration gradient section (s2) are generally present from the surface portion to the central portion of the secondary particle, it is preferable that the number of times that the first concentration gradient section (s1) and the second concentration gradient section (s2) existing within a depth of 0 to 0.2R from the surface portion of the secondary particle are repeated (or the number of times that the peaks (p1, p2, ...) exist, or the number of times that the peak regions (a1, ...) exist) are greater than the number of times that the first concentration gradient section (s1) and the second concentration gradient section (s2) existing within a depth of 0.2R to R from the surface portion of the secondary particle are repeated (or the number of times that the peaks (p1, p2, ...) exist, or the number of times that the peak regions (a1, ...) exist).

[0087] In addition, the positive electrode active material according to some embodiments of the present invention may include a coating layer that covers at least a portion of the surface of the primary particles (e.g., grain boundaries between the primary particles) and / or secondary particles formed by aggregation of the primary particles.

[0088] For example, the coating layer may be present to cover at least a portion of the exposed surface of the primary particles, particularly, the coating layer may be present to cover at least a portion of the exposed surface of the primary particles that are present on the outermost side of the secondary particles.

[0089] Thus, the coating layer may exist as a layer that continuously or discontinuously coats the surfaces of the primary particles and / or the secondary particles formed by agglomeration of the primary particles. When the coating layer exists discontinuously, it may exist in the form of islands.

[0090] The coating layer thus present can contribute to maintaining high electrochemical properties of the positive electrode active material, particularly the high-Ni type positive electrode active material, while resolving low structural stability.

[0091] In addition, the coating layer may exist in the form of a solid solution that does not form a boundary with the primary particles and / or the secondary particles formed by agglomeration of the primary particles.

[0092] The coating layer may contain at least one compound represented by the following Chemical Formula 2. That is, the coating layer may be defined as a region in which the compound represented by the following Chemical Formula 2 is present.

[0093] Li g M4 h O i

[0094] (where: M4 is at least one selected from Mn, Al, Co, Ti, Zr, Sr, Mg, V, B, Mo, Zn, Nb, Ba, Ca, Ta, Fe, Cr, Sn, Hf, Ce, and W; [ka] It is.)

[0095] The coating layer may be in a form in which different compounds are simultaneously present in one layer, or different compounds represented by Chemical Formula 2 are present in separate layers.

[0096] The compound represented by Chemical formula 2 may be in a state of being physically and / or chemically bonded to the primary particles represented by Chemical formula 1. In addition, the compound may be present in a state of forming a solid solution with the primary particles represented by Chemical formula 1.

[0097] The positive electrode active material according to the present embodiment includes a coating layer covering at least a portion of the surface of the primary particles (e.g., interfaces between the primary particles) and / or secondary particles formed by agglomeration of the primary particles, thereby enhancing structural stability. In addition, when such a positive electrode active material is used in a lithium secondary battery, the high-temperature storage stability and life characteristics of the positive electrode active material can be improved. In addition, the compound reduces residual lithium in the positive electrode active material and acts as a pathway for lithium ions, thereby improving the efficiency characteristics of the lithium secondary battery.

[0098] In some cases, the compound may be present not only at the interfaces between the primary particles and at least a portion of the surfaces of the secondary particles, but also in internal voids formed inside the secondary particles.

[0099] The compound is a compound in which lithium and an element represented by M4 are combined, or as a compound of M4, the compound is, for example, Li a W b O c , Li a Zr b O c , Li a Ti b O c , Li a Ni b O c , Li a B b O c , W b O c , Zr b O c , Ti b O c Or B b O c Also, non-limiting examples of the compound include Li 2 B 4 O 7 , Li 3 BO 3 , Li 2 B 2 O 7 , Li2 B 8 O 13 , Li 2 VO 3 , Li 3 VO 4 , Li 6 Zr 3 O 9 , Li 2 ZrO 3 , Li 5.5 Zr 2.6 2O 8 , Li 44 Ba 19 , Li 4 Ba, Li 2 TiO 3 , LiTi 7 O 4 and LiTi 2 O 4 The above examples are merely given for the convenience of understanding, and the compounds defined in the present application are not limited to the above examples.

[0100] In another embodiment, the compound may be a compound of lithium and at least two elements represented by M4, or may further include a compound of lithium and at least two elements represented by M4. The compound of lithium and at least two elements represented by M4 may be, for example, Li a (W / Ti) b O c , Li a (W / Zr) b O c , Li a (W / Ti / Zr) b O c , Li a (W / Ti / B) b O c It may be, but is not necessarily limited to, the above.

[0101] Here, the compound may exhibit a concentration gradient that decreases from the surface portion of the secondary particle toward the center portion of the secondary particle, whereby the concentration of the compound may decrease from the surface portion of the secondary particle toward the center portion of the secondary particle.

[0102] As described above, the compound exhibits a concentration gradient that decreases from the surface of the secondary particles toward the center of the secondary particles, and thus the residual lithium present on the surface of the positive electrode active material can be effectively reduced, thereby preventing side reactions caused by unreacted residual lithium. Specifically, the residual lithium present on the surface of the secondary particles can be reduced by reacting the raw material of the compound represented by Chemical formula 2 with the residual lithium present on the surface of the secondary particles to form the compound represented by Chemical formula 2. In addition, the compound can prevent the crystallinity of the surface inner region of the positive electrode active material from decreasing. In addition, the compound can prevent the overall structure of the positive electrode active material from collapsing during an electrochemical reaction.

[0103] Further, the coating layer may include a first coating layer containing at least one compound represented by Chemical Formula 2 and a second coating layer containing at least one compound represented by Chemical Formula 2, but a different compound than the compound contained in the first coating layer.

[0104] For example, the first coating layer may be present so as to cover at least a portion of the exposed surface of the primary particles that are at the outermost part of the secondary particles, and the second coating layer may be present so as to cover at least a portion of the exposed surface of the primary particles that is not covered by the first coating layer and the surface of the first coating layer.

[0105] Lithium secondary battery According to yet another aspect of the present invention, a positive electrode may be provided, the positive electrode active material layer including a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. Here, the positive electrode active material layer may include a positive electrode active material according to various embodiments of the present invention. Therefore, since the positive electrode active material is as described above, detailed description will be omitted for convenience, and only the remaining components not described above will be described below.

[0106] The positive electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and may be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The positive electrode current collector may usually have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0107] The positive electrode active material layer may be prepared by coating a positive electrode slurry composition containing the positive electrode active material, a conductive material, and optionally a binder, on the positive electrode current collector.

[0108] At this time, the positive electrode active material may be included in an amount of 80 to 99 wt%, more specifically, 85 to 98.5 wt%, based on the total weight of the positive electrode active material layer. When included in this content range, excellent capacity characteristics can be exhibited, but the amount is not necessarily limited thereto.

[0109] The conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing chemical changes in the battery that is constructed. Specific examples include graphite such as natural graphite and artificial graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, summer black, carbon-based materials such as carbon fibers, metal powders or metal fibers such as copper, nickel, aluminum, and silver, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and conductive polymers such as polyphenylene derivatives, and the like, and one or more of these may be used alone or in combination. The conductive material may be contained in an amount of 0.1 to 15% by weight based on the total weight of the positive electrode active material layer.

[0110] The binder serves to improve the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and among these, one type alone or a mixture of two or more types may be used. The binder may be included in an amount of 0.1 to 15% by weight based on the total weight of the positive electrode active material layer.

[0111] The positive electrode may be manufactured by a typical method for manufacturing a positive electrode, except for using the positive electrode active material. Specifically, the positive electrode may be manufactured by dissolving or dispersing the positive electrode active material and, optionally, a binder and a conductive material in a solvent to prepare a positive electrode slurry composition, which is then coated on a positive electrode current collector, followed by drying and rolling.

[0112] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, and to provide a viscosity that allows excellent thickness uniformity when applied to manufacture a positive electrode, taking into consideration the coating thickness of the slurry and the production yield.

[0113] In another embodiment, the positive electrode may be manufactured by casting the positive electrode slurry composition on a separate support, peeling the positive electrode slurry composition from the support, and laminating the resulting film on a positive electrode current collector.

[0114] According to yet another aspect of the present invention, there may be provided an electrochemical device including the above-mentioned positive electrode. The electrochemical device may be, for example, a battery or a capacitor, and more specifically, a lithium secondary battery.

[0115] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode facing the positive electrode, and a separator and an electrolyte interposed between the positive electrode and the negative electrode. Here, since the positive electrode is as described above, a detailed description thereof will be omitted for convenience, and only the remaining components not described above will be described in detail below.

[0116] The lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0117] The negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0118] The negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may generally have a thickness of 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.

[0119] The negative electrode active material layer may be prepared by coating a negative electrode slurry composition containing the negative electrode active material, a conductive material, and optionally a binder, on the negative electrode current collector.

[0120] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon, metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys, and SiO β (0<β<2), SnO 2 , a metal oxide capable of doping and dedoping lithium, such as vanadium oxide or lithium vanadium oxide, or a composite containing the metallic compound and a carbonaceous material, such as a Si-C composite or a Sn-C composite, may be used. Any one or a mixture of two or more of these may be used. A thin film of metallic lithium may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbon material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include amorphous, plate-like, scaly, spherical or fibrous natural graphite or artificial graphite, kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.

[0121] The negative electrode active material may be included in an amount of 80 to 99 wt % based on the total weight of the negative electrode active material layer.

[0122] The binder is a component that aids in bonding between the conductive material, the active material, and the current collector, and may be added in an amount of usually 0.1 to 10 wt% based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0123] The conductive material may be added as a component for further improving the conductivity of the negative electrode active material in an amount of 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it has conductivity without inducing a chemical change in the battery, and may be, for example, graphite such as natural graphite or artificial graphite, carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black, conductive fibers such as carbon fibers or metal fibers, metal powders such as carbon fluoride, aluminum, or nickel powder, conductive whiskey such as zinc oxide or potassium titanate, conductive metal oxides such as titanium oxide, or conductive materials such as polyphenylene derivatives.

[0124] In one embodiment, the negative electrode active material layer may be prepared by coating a negative electrode slurry composition prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent on a negative electrode current collector and drying the coating. Alternatively, the negative electrode slurry composition may be cast on a separate support, and a film obtained by peeling the negative electrode slurry composition from the support may be laminated on the negative electrode current collector.

[0125] In another embodiment, the negative electrode active material layer may be prepared by coating a negative electrode slurry composition prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent on a negative electrode current collector and drying the coating, or by casting the negative electrode slurry composition on a separate support, peeling the negative electrode slurry composition from the support, and laminating the resulting film on the negative electrode current collector.

[0126] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode to provide a passage for lithium ions to move. Any separator generally used in lithium secondary batteries may be used without any particular limitation. In particular, it is preferable that the separator has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, or the like, may be used. In addition, in order to ensure heat resistance or mechanical strength, a separator coated with a ceramic component or a polymer material may be used, and may be selectively used as a single-layer or multi-layer structure.

[0127] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.

[0128] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0129] The organic solvent may be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone, an ether solvent such as dibutyl ether or tetrahydrofuran, a ketone solvent such as cyclohexanone, an aromatic hydrocarbon solvent such as benzene or fluorobenzene, dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that may be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, the performance of the electrolyte may be excellent if the cyclic carbonate and the chain carbonate are mixed at a volume ratio of about 1:1 to about 1:9.

[0130] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. 6 , LiClO 4 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlO 4 , LiAlCl 4 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiN(C 2 F 5 SO 3 ), LiN(C 2 F 5 SO 2 ) 2 , LiN(CF 3 SO 2 ) 2 , LiCl, LiI, or LiB(C 2 O 4 ) 2 The lithium salt may be used at a concentration within the range of 0.1 to 2.0 M. When the lithium salt concentration is within this range, the electrolyte has appropriate conductivity and viscosity, and therefore can exhibit excellent electrolyte performance and can effectively migrate lithium ions.

[0131] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in battery capacity, improving the discharge capacity of the battery, etc. In this case, the additives may be contained in an amount of 0.1 to 5% by weight based on the total weight of the electrolyte.

[0132] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore useful in the fields of portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0133] The external shape of the lithium secondary battery according to the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, etc. Furthermore, the lithium secondary battery can be used not only as a battery cell used as a power source for a small device, but also preferably as a unit battery for a medium- to large-sized battery module including a plurality of battery cells.

[0134] According to yet another aspect of the present invention, there may be provided a battery module including the lithium secondary battery as a unit cell and / or a battery pack including the same.

[0135] The battery module or the battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool, an electric vehicle (Electric Vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV), or a power storage system.

[0136] The present invention will be described in more detail below with reference to examples. However, these examples are for the purpose of illustrating the present invention, and the scope of the present invention is not to be construed as being limited by these examples.

[0137] Production Example 1. Production of positive electrode active material Example 1 Spherical Ni particles were prepared by the co-precipitation method. 0.92 Co 0.06 Mn 0.02 (OH) 2 The hydroxide precursor was synthesized.

[0138] Specifically, in a 90L reactor, nickel sulfate, cobalt sulfate, and manganese sulfate were mixed in a molar ratio of 92:6:2 to form a 1.5M composite transition metal sulfate aqueous solution, and 25 wt% NaOH and 30 wt% NH 4 The pH in the reactor was maintained at 11.5, and the temperature of the reactor was maintained at 60°C. In addition, an inert gas, N 2 was charged into the reactor to prevent the produced precursor from being oxidized.

[0139] After the synthesis of the hydroxide precursor is completed, it is washed and dehydrated using a filter press (F / P) device, and Ni 0.92 Co 0.06 Mn 0.02 (OH) 2 The hydroxide precursor was obtained.

[0140] The hydroxide precursor obtained was mixed with LiOH (Li / (Ni+Co+Mn) molar ratio = 1.05), and then heated in a calciner to 0 2 While maintaining the atmosphere, the temperature was raised to 700° C. at 2° C. per minute, and then heat treatment was performed at 700° C. for 10 hours (first heat treatment) to obtain a lithium composite oxide.

[0141] Next, the obtained lithium composite oxide was not washed with water, and TiO was weighed out so as to be 0.05 mol % in the lithium composite oxide. 2 After mixing, O 2 While maintaining the atmosphere, the temperature was raised to 700° C. at 2° C. per minute, and then further heat-treated (second heat treatment) at 700° C. for 10 hours to finally obtain a positive electrode active material.

[0142] Example 2 During the second heat treatment of the lithium composite oxide, TiO 2 Instead of 0.05 mol% ZrO 2 After mixing, O 2 A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere was maintained, the temperature was increased by 2° C. per minute to 710° C., and then a further heat treatment (second heat treatment) was performed at 710° C. for 10 hours.

[0143] Example 3 During the second heat treatment of the lithium composite oxide, TiO 2 Instead of 0.1 mol% V 2 O 3 After mixing, O 2 A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere was maintained, the temperature was increased by 2° C. per minute to 720° C., and then a further heat treatment (second heat treatment) was performed at 720° C. for 10 hours.

[0144] Example 4 During the second heat treatment of the lithium composite oxide, TiO 2 Instead of 0.2 mol% H 3 BO 3 After mixing, O 2A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere was maintained, the temperature was increased by 2° C. per minute to 720° C., and then a further heat treatment (second heat treatment) was performed at 720° C. for 10 hours.

[0145] Example 5 During the second heat treatment of the lithium composite oxide, TiO 2 Instead of 0.2 mol% WO 3 After mixing, O 2 A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere was maintained, the temperature was increased by 2° C. per minute to 700° C., and then a further heat treatment (second heat treatment) was performed at 700° C. for 10 hours.

[0146] Example 6 During the second heat treatment of the lithium composite oxide, TiO 2 Instead of 0.2 mol% Sr(OH) 2 After mixing, O 2 A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere was maintained, the temperature was increased by 2° C. per minute to 680° C., and then a further heat treatment (second heat treatment) was performed at 680° C. for 10 hours.

[0147] Example 7 During the second heat treatment of the lithium composite oxide, TiO 2 Instead of 0.2 mol% Al 2 O 3 After mixing, O 2 A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere was maintained, the temperature was increased by 2° C. per minute to 700° C., and then a further heat treatment (second heat treatment) was performed at 700° C. for 10 hours.

[0148] Example 8 Spherical Ni particles were prepared by the co-precipitation method. 0.92 Co 0.06 Mn 0.02 (OH) 2 The hydroxide precursor was synthesized.

[0149] Specifically, in a 90L reactor, nickel sulfate, cobalt sulfate, and manganese sulfate were mixed in a molar ratio of 95:4:1 to form a 1.5M composite transition metal sulfate aqueous solution, and 25 wt% NaOH and 30 wt% NH 4 The pH in the reactor was maintained at 11.5, and the temperature of the reactor was maintained at 60°C. In addition, an inert gas, N 2 was charged into the reactor to prevent the produced precursor from being oxidized.

[0150] After the synthesis of the hydroxide precursor is completed, it is washed and dehydrated using a filter press (F / P) device, and Ni 0.92 Co 0.06 Mn 0.02 (OH) 2 The hydroxide precursor was obtained.

[0151] The hydroxide precursor obtained was mixed with LiOH (Li / (Ni+Co+Mn) molar ratio = 1.05), and then heated in a calciner to 0 2 While maintaining the atmosphere, the temperature was raised to 700° C. at 2° C. per minute, and then heat treatment was performed at 700° C. for 10 hours (first heat treatment) to obtain a lithium composite oxide.

[0152] Next, the obtained lithium composite oxide was not washed with water, and TiO was weighed out so as to be 0.05 mol % in the lithium composite oxide. 2 After mixing, O 2 While maintaining the atmosphere, the temperature was raised to 700° C. at 2° C. per minute, and then further heat-treated (second heat treatment) at 700° C. for 10 hours to finally obtain a positive electrode active material.

[0153] Comparative Example 1 During the second heat treatment of the lithium composite oxide, TiO 2 A positive electrode active material was produced in the same manner as in Example 1, except that the above was not mixed.

[0154] Comparative Example 2 During the second heat treatment of the lithium composite oxide, TiO 2 Instead of 0.05 mol% ZrO 2 After mixing, O2 A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere was maintained, the temperature was increased by 2° C. per minute to 850° C., and then a further heat treatment (second heat treatment) was performed at 850° C. for 24 hours.

[0155] Comparative Example 3 During the first heat treatment, Ni 0.92 Co 0.06 Mn 0.02 (OH) 2 Hydroxide precursor, LiOH (Li / (Ni+Co+Mn) molar ratio=1.05) and Al 2 O 3 (weighed out and mixed so as to account for 0.5 mol% of the total mixture) are mixed, and then placed in a sintering furnace. 2 A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere was maintained and the temperature was increased to 700° C. at 2° C. per minute, and then the heat treatment was performed at 700° C. for 10 hours.

[0156] Reference example 1 During the second heat treatment of the lithium composite oxide, 0.1 mol% of TiO 2 After mixing, O 2 A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere was maintained, the temperature was increased by 2° C. per minute to 350° C., and then a further heat treatment (second heat treatment) was performed at 350° C. for 10 hours.

[0157] Reference example 2 During the second heat treatment of the lithium composite oxide, 0.8 mol % of TiO 2 After mixing, O 2 A positive electrode active material was produced in the same manner as in Example 1, except that the atmosphere was maintained, the temperature was increased by 2° C. per minute to 720° C., and then a further heat treatment (second heat treatment) was performed at 720° C. for 24 hours.

[0158] Manufacturing Example 2. Manufacturing of lithium secondary batteries A positive electrode slurry was prepared by dispersing 94 wt% of each positive electrode active material prepared in Preparation Example 1, 3 wt% of artificial graphite, and 3 wt% of PVDF binder in 3.5 g of N-methyl-2-pyrrolidone (NMP). The positive electrode slurry was applied to a 20 μm-thick aluminum (Al) thin film as a positive electrode current collector, dried, and roll-pressed to prepare a positive electrode. The loading level of the positive electrode was 7 mg / cm. 2 and the electrode density is 3.2 g / cm 3 It was.

[0159] Lithium foil was used as a counter electrode for the positive electrode, a porous polyethylene film (Celgard 2300, thickness: 25 μm) was used as a separator, and LiPF was dissolved in a solvent of ethylene carbonate and ethyl methyl carbonate mixed in a volume ratio of 3:7. 6 A coin cell was fabricated by conventional known manufacturing processes using a liquid electrolyte in which ZnO was present at a concentration of 1.15M.

[0160] Experimental Example 1. SEM / EDX analysis of metal composite hydroxide and positive electrode active material FIGS. 2 to 8 are graphs showing line scanning of the doping metal contents in the secondary particles confirmed through EDX analysis of cross-sectional SEM images obtained after selecting secondary particles having a radius of 7.5 μm contained in the cathode active materials according to Examples 1 to 7 and processing the cross sections using an FIB (Ga-ion source). FIGS. 9 to 11 are graphs showing line scanning of the doping metal contents in the secondary particles confirmed through EDX analysis of cross-sectional SEM images obtained after selecting secondary particles having a radius of 7.5 μm contained in the cathode active materials according to Comparative Examples 1 to 3 and processing the cross sections using an FIB (Ga-ion source).

[0161] 12 and 13 are graphs showing line scanning of the doping metal content in the secondary particles confirmed through EDX analysis of cross-sectional SEM images obtained after selecting secondary particles having a radius of 7.5 μm contained in the positive electrode active materials of Reference Examples 1 and 2, respectively, and processing the cross-sections using FIB (Ga-ion source).

[0162] Here, Figs. 2 to 13 show excerpts of the results of line scanning from the surface of the secondary particles contained in each positive electrode active material to a depth of 3 µm (3,000 nm).

[0163] For reference, since Comparative Example 1 does not contain a doping metal, the line scanning graph in Fig. 9 shows a baseline. In addition, although the line scanning results for the secondary particles contained in the cathode active material according to Example 8 are not separately attached, it was confirmed that the secondary particles contained in the cathode active material according to Example 8 also show a concentration gradient pattern similar to that of the cathode active materials according to Examples 1 to 7 shown in Figs. 2 to 8.

[0164] [Table 1]

[0165] 2 to 8, it can be seen that the secondary particles contained in the positive electrode active materials according to Examples 1 to 7 are limited to a depth of 0 to 0.2R (1.5 μm) from the surface of the secondary particle, where R is the radius of the secondary particle (7.5 μm), and that a first concentration gradient section in which the concentration of the doping metal has a (-) gradient and a second concentration gradient section in which the concentration of the doping metal has a (+) gradient are repeatedly present from the surface of the secondary particle to the center of the secondary particle.

[0166] 10, it can be seen that the secondary particles included in the cathode active material according to Comparative Example 2 do not have a concentration gradient section in which the concentration of the doping metal has a (+) gradient from the surface portion of the secondary particle to the center portion of the secondary particle. That is, the secondary particles included in the cathode active material according to Comparative Example 2 have a concentration gradient in which the concentration of the doping metal gradually decreases from the surface portion of the secondary particle to the center portion of the secondary particle.

[0167] Referring to FIG. 11, it can be seen that the secondary particles contained in the positive electrode active material according to Comparative Example 3 have a substantially uniform concentration of the doping metal from the surface portion of the secondary particle to the center portion of the secondary particle without significant change.

[0168] Also, it can be seen that the secondary particles contained in the positive electrode active material according to Reference Example 1 are limited to a depth of 0 to 0.2R (1.5 μm) from the surface of the secondary particles, and that from the surface of the secondary particles to the center of the secondary particles, a first concentration gradient section having a negative gradient and a second concentration gradient section having a positive gradient are present. However, in the secondary particles contained in the positive electrode active material according to Reference Example 1, the first concentration gradient section and the second concentration gradient section do not repeatedly exist from the surface of the secondary particles to the center of the secondary particles.

[0169] Similarly to the positive electrode active materials of Examples 1 to 7, the secondary particles contained in the positive electrode active material of Reference Example 2 have a first concentration gradient section with a negative gradient and a second concentration gradient section with a positive gradient in the concentration of the doping metal from the surface portion of the secondary particle toward the center portion of the secondary particle, repeatedly existing. However, it can be confirmed that the secondary particles contained in the positive electrode active material of Reference Example 2 have the first concentration gradient section and the second concentration gradient section repeatedly existing even in a region extending beyond a depth of 0.2R (1.5 μm) from the surface portion of the secondary particle.

[0170] Experimental Example 2: XRD analysis of positive electrode active material X-ray diffraction (XRD) analysis was performed on each of the positive electrode active materials prepared in Preparation Example 1 to confirm whether or not compounds other than the lithium composite oxide having the crystal structure represented by Chemical Formula 1 were present in the positive electrode active materials. The XRD analysis was performed using a Bruker D8 Advance diffractometer using Cu Kα radiation (1.540598 Å).

[0171] 14 to 16 show the results of XRD analysis of the positive electrode active materials according to Examples 1 to 3, respectively.

[0172] 14 to 16, the positive electrode active materials according to Examples 1 to 3 were [ka] A peak corresponding to the crystal structure of the compound represented by the formula:

[0173] That is, when the lithium composite oxide obtained through the first heat treatment is not washed with water, and a raw material containing a dopant is mixed with the lithium composite oxide and then the second heat treatment is performed, it can be confirmed that the residual lithium present on the surface of the lithium composite oxide (secondary particles) obtained through the first heat treatment reacts with the raw material containing a dopant to form a compound represented by Chemical Formula 2 below.

[0174] Li g M4 h O i

[0175] (where: M4 is at least one selected from Mn, Al, Co, Ti, Zr, Sr, Mg, V, B, Mo, Zn, Nb, Ba, Ca, Ta, Fe, Cr, Sn, Hf, Ce, and W; [ka] It is.)

[0176] Experimental Example 3. Measurement of residual lithium and specific surface area of ​​positive electrode active material Residual lithium was measured by the amount of 0.1M HCl used until the pH reached 4 by pH titration. First, 5 g of each positive electrode active material prepared according to Preparation Example 1 was placed in 100 ml of DIW, stirred for 15 minutes, and then filtered. Next, 50 ml of the filtered solution was taken, and 0.1M HCl was added thereto to measure the amount of HCl consumed due to the change in pH to determine Q1 and Q2. Residual LiOH and Li were calculated according to the following formula: 2 CO 3 was calculated.

[0177]

number

[0178] The BET specific surface area was calculated from the amount of nitrogen gas adsorbed at liquid nitrogen temperature (77K) using a gas adsorption specific surface area measurement device (BELSORP-miniII, manufactured by MicrotaracBEL).

[0179] The results of the measurement of the residual lithium and the BET specific surface area are shown in Table 2 below.

[0180] [Table 2]

[0181] Referring to the results in Table 2, it can be seen that the positive active material according to Example 1 had a reduced content of residual lithium without increasing the specific surface area compared to Comparative Example 1.

[0182] In addition, in the case of the positive electrode active material according to Comparative Example 2, in which the concentration of the doping metal gradually decreases from the surface portion of the secondary particle to the center portion of the secondary particle, it can be seen that the content of residual lithium is excessively high compared to Examples 1 to 7.

[0183] On the other hand, in the case of Reference Example 1 in which the first concentration gradient section and the second concentration gradient section for the doping metal do not exist repeatedly from the surface portion of the secondary particle toward the center portion of the secondary particle, and in the case of Reference Example 2 in which the first concentration gradient section and the second concentration gradient section exist repeatedly even in a region exceeding a depth of 0.2R (1.5 μm) from the surface portion of the secondary particle, it can be confirmed that the effect of reducing residual lithium is negligible compared to the positive electrode active material of Example 1, and rather the specific surface area is increased.

[0184] 12, in the case of the positive electrode active material of Reference Example 1, the first concentration gradient section and the second concentration gradient section do not repeatedly occur from the surface portion of the secondary particle toward the center portion of the secondary particle, and therefore, it is expected that the effect of reducing residual lithium in the region close to the center portion of the secondary particle is insufficient compared to Example 1. In the case of the positive electrode active material of Reference Example 2, the number of repetitions of the first concentration gradient section and the second concentration gradient section increases from the surface portion of the secondary particle toward the center portion of the secondary particle due to the heat treatment maintained for a relatively long time, and it is expected that lithium is dissolved again in the form of an impurity from the lithium composite oxide, and the content of residual lithium increases.

[0185] Experimental Example 4. Evaluation of capacity and life characteristics of lithium secondary batteries A charge / discharge experiment was performed on the lithium secondary battery (coin cell) manufactured in Manufacturing Example 2 using an electrochemical analyzer (Toyo, Toscat-3100) at 25° C., voltage range of 3.0 V to 4.3 V, and discharge rate of 0.1 C, to measure the charge and discharge capacities.

[0186] In addition, the same lithium secondary battery was charged / discharged 50 times at 25° C. and 1C / 1C within a driving voltage range of 3.0V to 4.4V, and then the ratio of the discharge capacity at the 50th cycle to the initial capacity (cycle capacity retention) was measured.

[0187] The measurement results are shown in Table 3 below.

[0188] [Table 3]

[0189] Referring to the results in Table 3, it can be seen that the charge / discharge efficiency and cycle capacity retention rate of the lithium secondary batteries using the positive electrode active materials according to Examples 1 to 8 were improved compared to Comparative Example 1 in which there was no concentration gradient for the doping metal in the secondary particles.

[0190] In addition, in the case of Comparative Example 2, in which the concentration of the doping metal gradually decreases from the surface of the secondary particle to the center of the secondary particle, it was confirmed that the cycle capacity retention rate was slightly improved compared to Comparative Example 1, but the charge / discharge efficiency was decreased.

[0191] Furthermore, in the case of Reference Examples 1 and 2 in which the first concentration gradient section and the second concentration gradient section for the doping metal are not repeated from the surface portion of the secondary particle toward the center portion of the secondary particle (i.e., at least two peaks (p1, p2) are not present after the first peak (p0) for the concentration of the doping metal that appears at a position corresponding to the outermost surface of the secondary particle), or the first concentration gradient section and the second concentration gradient section are repeated excessively, resulting in peaks due to the first concentration gradient section and the second concentration gradient section even in the region close to the center of the secondary particle, it can be confirmed that the improvement effect on the charge / discharge efficiency and / or cycle capacity retention rate is negligible compared to Comparative Example 1.

[0192] Although the above describes an embodiment of the present invention, a person having ordinary knowledge in the art can modify and change the present invention in various ways by adding, changing, deleting or adding components without departing from the concept of the present invention described in the claims, and this can also be said to be within the scope of the present invention.

Claims

1. A positive electrode active material including a lithium composite oxide having a layered structure that includes at least nickel, cobalt, and a doping metal and is capable of lithium intercalation / deintercalation, The lithium composite oxide includes secondary particles that are aggregates of a plurality of primary particles, and crystal grain boundaries are formed between adjacent primary particles, The secondary particles are aggregates of primary particles, in which the concentration of the doping metal exhibits a negative concentration gradient from the grain boundaries between the primary particles toward the center of the primary particles. When the radius of the secondary particle is R, within a depth of 0 to 0.2R from the surface of the secondary particle, there are a first concentration gradient section having a negative gradient and a second concentration gradient section having a positive gradient, a concentration maintenance section in which the absolute value of the concentration change of the doping metal is 3 at % or less is present between the first concentration gradient section and the second concentration gradient section.

2. The positive electrode active material according to claim 1 , wherein the primary particles are represented by the following Chemical Formula 1. Li a Ni 1-(b+c+d+e) Co b M1 c M2 d M3 e O f (where: M1 is at least one selected from Mn and Al; M2 and M3 are each independently selected from Al, Ba, B, Ce, Cr, Mg, Mn, Mo, Na, K, P, V, Sr, Ti, W, Nb, and Zr; M1 to M3 are different from each other, 【Chemistry 1】 It is.)

3. The positive electrode active material according to claim 2 , wherein the concentrations (mol %) of Ni, Co, M1, M2 and M3 in the primary particles represented by Chemical Formula 1 satisfy the following Formula 2: [0010]

4. 3. The positive electrode active material according to claim 2, wherein the secondary particles are aggregates of primary particles that exhibit a concentration gradient in which the concentration of at least one selected from M2 and M3 decreases from a crystal grain boundary between the primary particles toward a center of the primary particles.

5. 5 . The positive electrode active material according to claim 4 , wherein the first concentration gradient section and the second concentration gradient section are repeated at least twice from the surface portion of the secondary particle toward the center portion of the secondary particle.

6. 2. The positive electrode active material according to claim 1, wherein a compound represented by the following Chemical Formula 2 is present at least in a part of the crystal grain boundaries between the primary particles and on the surface of the secondary particles. Li g M4 h O i (where: M4 is at least one selected from Mn, Al, Co, Ti, Zr, Sr, Mg, V, B, Mo, Zn, Nb, Ba, Ca, Ta, Fe, Cr, Sn, Hf, Ce, and W; 【Chemistry 2】 It is.)

7. Li is present in at least a part of the grain boundaries between the primary particles and the surfaces of the secondary particles. 2 B 4 O 7 , Li 3 B.O. 3 , Li 2 B 2 O 7 , Li 2 B 8 O 13 , Li 2 V.O. 3 , Li 3 V.O. 4 , Li 6 Zr 3 O 9 , Li 2 ZrO 3 , Li 5.5 Zr 2.6 2O 8 , Li 44 Ba 19 , Li 4 Ba, Li 2 TiO 3 , LiTi 7 O 4 and LiTi 2 O 4 2. The positive electrode active material of claim 1, wherein at least one compound selected from the group consisting of:

8. 2. The positive electrode active material according to claim 1, wherein the primary particles have an average particle size of 0.1 μm to 10.0 μm.

9. 9. The positive electrode active material according to claim 8, wherein a concentration gradient within the primary particles exists within a depth of 0 to 0.2r from a crystal grain boundary between the primary particles, where r is an average particle size of the primary particles.

10. 2. The positive electrode active material according to claim 1, wherein the secondary particles have an average particle size of 3 μm to 20 μm.

11. A positive electrode comprising the positive electrode active material according to any one of claims 1 to 10.

12. A lithium secondary battery using the positive electrode according to claim 11.

Citation Information

Patent Citations

  • Lithium transition-metal compound powder, its manufacturing method, spray drying object acquired during spray drying process, positive electrode for lithium secondary battery using it, and lithium secondary battery

    JP2009081130A

  • Positive electrode active material for secondary battery and manufacturing method thereof

    JP2019091692A

  • Lithium composite oxide, positive electrode active material for lithium secondary battery and lithium secondary battery comprising the same

    JP2020029396A

  • Cathode active material for lithium secondary battery, method for preparing cathode active material for lithium secondary battery and lithium secondary battery including cathode active material

    KR1020140022681A

  • Positive electrode active material for lithium ion secondary batteries, method for producing same and lithium ion secondary battery

    WO2015151606A1