How to bond and separate two substrates
The use of a metallized temporary bonding layer addresses the limitations of polymer-based adhesives by enabling efficient, environmentally friendly, and cost-effective separation of substrates in microelectronics, allowing for higher processing temperatures and substrate reuse.
Patent Information
- Application Number
- JP2022564851
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-29
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-05-29
AI Technical Summary
The use of polymer-based temporary bonding adhesives in microelectronics and microsystems technology is disadvantageous due to environmental pollution from cleaning chemicals, high cost, and lower heat resistance, posing technical constraints on processing substrates.
A method involving a metallized temporary bonding layer made of metal or metal alloy is used to bond and separate substrates, allowing for easy separation without damaging the substrates, using focused ablation radiation to melt and evaporate the bonding layer.
This method reduces environmental impact, lowers costs, and enables higher processing temperatures without substrate damage, facilitating efficient reuse of carrier substrates and improved substrate processing.
Smart Images

Figure 0007579355000001 
Figure 0007579355000002 
Figure 0007579355000003
Abstract
Description
[Technical field]
[0001] The invention relates to a method for bonding and debonding two substrates according to the independent claims, as well as a corresponding substrate stack and a corresponding device.
[0002] The miniaturization of almost all parts of microelectronics and microsystems technology leads to a continuous development of all technologies, which allows a higher density of functional elements of any type on a substrate, such as microcontrollers, memory chips, MEMS, sensors of any type or microfluidic components.
[0003] The technology for lateral densification of these functional elements has improved significantly in recent years. In some areas of microelectronics and microsystem technology, it is even the case that further lateral densification of the functional elements is no longer possible. In the manufacture of microchips, the maximum achievable resolution of the structures to be produced by lithography has already been reached. In a few years, therefore, further lateral densification of the functional elements will no longer be possible due to physical or technical limitations. The industry has already been addressing this issue for several years with the development of 2.5D and 3D technologies. These technologies make it possible to align functional elements of the same or even different nature, stack them one on top of the other, permanently connect them to each other and cross-link them with corresponding strip conductors.
[0004] One of the key technologies for realizing such structures is temporary bonding, which is understood as a method for connecting substrates together in such a way that they can be separated without being destroyed.
[0005] In the prior art there are several methods to peel / separate two substrates (product substrate and carrier substrate). Most of the methods use so-called bonding adhesives to temporarily bond the two substrates together in such a way that they can be separated relatively easily. Bonding adhesives are mainly polymers, especially thermoplastics.
[0006] However, the use of polymers as temporary bonding adhesives has proven to be disadvantageous, especially due to the environmental pollution caused by cleaning chemicals and the cost of consumables. Furthermore, all polymer-based temporary bonding adhesives have the disadvantage that they have a much lower heat resistance compared to other processing temperatures of the product substrate. Thus, temporary bonding with polymers brings about technical constraints for the processing of the product substrate.
[0007] It is therefore an object of the present invention to at least partially, in particular completely, overcome the disadvantages mentioned in the prior art, in particular to provide an improved bonding and debonding method.
[0008] The problem of the invention is solved by the features of the independent claims. Advantageous developments of the invention are defined in the dependent claims. All combinations of at least two features shown in the description, claims and / or drawings are also included within the scope of the invention. In the stated value ranges, values that are inside the stated limits are also considered as disclosed limits and can be claimed in any combination.
[0009] The present invention provides a method for temporarily bonding a product substrate and a carrier substrate, comprising the steps of: - producing a metallized temporary bonding layer on the product substrate and / or on the carrier substrate; - bonding the product substrate and the carrier substrate on the metallized temporary bonding layer; The present invention relates to a method comprising at least the steps of:
[0010] The invention further relates to a substrate stack, in particular manufactured using the method according to the invention, comprising a product substrate and a carrier substrate, wherein the product substrate and the carrier substrate are connected by a metallized temporary bonding layer.
[0011] The temporary bonding layer is preferably the only layer used in the bonding or peeling process according to the invention, which gives a further advantage over the prior art where several polymer layers, usually one above the other, are used, one for bonding and the other for peeling.
[0012] The invention furthermore relates to an apparatus for temporarily bonding a product substrate and a carrier substrate, in particular by a method according to at least one of the previous embodiments, comprising: - on the product substrate and / or the carrier substrate, a metallized temporary bonding layer can be produced, - the product substrate and the carrier substrate can be bonded on the metallized temporary bonding layer; Regarding the device.
[0013] Hereinafter, the metallized temporary bonding layer is also referred to as metallization.
[0014] The metallized temporary bonding layer can be produced directly on the carrier substrate and / or directly on the product substrate, or a protective layer can be disposed between the metallized temporary bonding layer and the product substrate.
[0015] The protective layer preferably has a high reflectivity to protect the product substrate from ablating radiation.
[0016] Thus, according to the invention, the temporary bonding layer consists of a metal or a metal alloy.
[0017] In a preferred embodiment, it is provided for applying a protective layer to the substrate surface of the product substrate prior to metallization.
[0018] In another preferred embodiment it is provided that the temporary bonding layer is produced over the entire area, in particular on the protective layer on the product substrate.
[0019] In another preferred embodiment it is provided for the temporary bonding layer to be produced locally, and more preferably on elevated areas of the carrier substrate.
[0020] In a further preferred embodiment it is provided that before producing the metallized temporary bonding layer on the product substrate and / or the carrier substrate, a protective layer is applied to the product substrate.
[0021] Another preferred embodiment provides that the bonding is carried out thermally.
[0022] In another preferred embodiment, it is provided that the carrier substrate is formed in a structured state, the carrier substrate has elevations and cavities, the elevations are stably connected to the product substrate via metal contacts, and the cavities are arranged between the elevations.
[0023] A further possible embodiment provides for a layer lying on the carrier substrate, in which layer cavities are generated by structuring.
[0024] For example, it is conceivable to apply polymers which can be easily structured by photolithography or imprint lithography.
[0025] Sol-gel could also be used to generate connections that are easy to imprint and structure, yet harden very strongly like SiO2.
[0026] In such layers, cavities can be produced particularly easily. In particular, such carriers can be very easily reused by removing the applied layers by cleaning. The metal deposited in the cavities is also very easily removed en masse by such cleaning.
[0027] The cavities can be of any shape and arranged in any arrangement, but preferably they have the simplest possible geometric shape and are regularly arranged.
[0028] Particularly preferred shapes of the cavity wall contour are: - Rectangles, especially squares - Round - Oval - triangle It is.
[0029] In particular, triangular shapes can be produced very easily by etching into (111) oriented silicon wafers.
[0030] The cavities are preferably arranged along a two-dimensional rectangular, in particular square, grid.
[0031] In another embodiment according to the invention, the cavities may be arranged along a two-dimensional rectangular, in particular square, face-centered lattice.
[0032] The total volume of the cavities is preferably more than 10 times the volume of the temporary bonding layer, preferably more than 100 times, even more preferably more than 1000 times, very preferably more than 10000 times, and most preferably more than 100000 times, because the temporary bonding layer melts and evaporates or sublimes, and the gas volume occupies several times the solid volume.
[0033] The depth of the cavities is between 1 nm and 100 μm, preferably between 10 nm and 50 μm, even more preferably between 50 nm and 30 μm, very preferably between 70 nm and 20 μm, and most preferably between 100 nm and 10 μm.
[0034] The lateral dimensions of the cavities (eg the diameter of a circular cavity, or the side length of a rectangular cavity) are from 10 nm to 5 mm, preferably from 50 nm to 1 mm, even more preferably from 100 nm to 500 μm, very preferably from 500 nm to 100 μm, and most preferably from 1 μm to 50 μm.
[0035] After bonding, the bonded substrate stack consisting of at least the carrier substrate, the metallized temporary bond layer, and the product substrate can be further processed.
[0036] The present invention further provides a method of peeling a product substrate from a carrier substrate, the product substrate and the carrier substrate being connected by a metallized temporary bonding layer to form a substrate stack, the method comprising the steps of: - mounting and fixing the substrate stack to a substrate holder; - focusing a delaminating radiation, in particular a laser beam, through the carrier substrate onto the metallized temporary bonding layer, thereby melting, evaporating and / or sublimating the metallized temporary bonding layer; - separating the product substrate from the carrier substrate; The present invention relates to a method comprising at least the steps of:
[0037] The invention furthermore relates to an apparatus for peeling a product substrate from a carrier substrate, in particular by a method according to at least one of the previous embodiments, in which the product substrate and the carrier substrate are connected by a metallized temporary bonding layer to form a substrate stack, the apparatus comprising: - a substrate holder for mounting and fixing the substrate stack; - a radiation source for focusing a stripping radiation, in particular a laser beam, through the carrier substrate onto the metallized temporary bonding layer, thereby melting, evaporating and / or sublimating the metallized temporary bonding layer; - a separation means for separating the product substrate from the carrier substrate; The present invention relates to an apparatus comprising at least
[0038] The separating means may in particular be mechanical separating means, such as for example blades.
[0039] In a further embodiment according to the invention, the separating means may be a fluid stream pressing between the two substrates instead of a blade.
[0040] In a more preferred embodiment according to the invention, the separation means is a substrate holder, to which the product substrate and the carrier substrate are fixed. In a first embodiment according to the invention, a simple relative movement between the two substrate holders, in particular in a direction perpendicular to the substrate surface, is performed after the complete release according to the invention. In a second embodiment according to the invention, at least one of the two substrate holders is tilted about a rotation axis so that the separation of the two substrates starts at the periphery. In a third embodiment according to the invention, at least one of the substrate holders is designed so that it can be bent as well as tilted. In this case, the substrate holder is preferably a flexible plate. One of the two substrates, preferably the carrier substrate, is then continuously peeled off starting from its periphery while being fixed to the flexible substrate holder. The rigidity of the flexible substrate holder allows the lift-off process to be controlled very precisely.
[0041] In a further, less preferred embodiment according to the invention, the separating means is a substrate holder that is displaceable parallel to its fixing surface or to the substrate surface. The two substrates are then separated from each other by a shearing process. This embodiment is known in the prior art as the "slide-off" technique and is used in particular for substrates that are temporarily bonded by a polymer-based bonding adhesive. In the prior art, the substrates, and thus the bonding adhesive, are then heated by a heating device until they can be separated from each other by a shearing process. However, in the method according to the invention, this shearing process works without destruction only if it can be ensured that there are virtually no metal contacts between the product substrate and the carrier substrate. However, if there are only a few metal contacts between the product substrate and the carrier substrate, the shearing process can cause plastic deformation of the metal contacts, which allows a non-destructive separation.
[0042] In particular, the above-mentioned separation means can be combined with one another.
[0043] Preferably, the thermal conductivity of the carrier substrate is specified to be 0.1 W / (m·K) to 5000 W / (m·K), more preferably 1 W / (m·K) to 2500 W / (m·K), and even more preferably 0.5 W / (m·K) to 1000 W / (m·K).
[0044] Preferably, it is further provided that the substrate stack is heated and / or cooled by a heating section and / or a cooling section.
[0045] Preferably, it is further provided that the stripping radiation is focused in a pulsed manner onto the metallized temporary bond layer.
[0046] Preferably, it is further provided to measure the energy input of the ablation radiation into the metallized temporary bond layer and to control the radiation output of the ablation radiation.
[0047] Preferably, it is further provided that at least the carrier substrate is transparent to the ablation radiation. It is possible, although unlikely, that the product substrate is transparent to the ablation radiation.
[0048] Preferably, it is further provided that, before separating the product substrate from the carrier substrate, the melted, evaporated and / or sublimated metallized temporary bonding layer condenses and solidifies and / or re-sublimes in the cavity.
[0049] In particular, the locally heated metal vapor is absorbed into a cavity around the carrier substrate, where it can either resublime or first condense and then solidify.
[0050] In other words, the temporary bonding layer is locally removed in particular by laser radiation.
[0051] Particularly preferred lasers and their wavelengths are: - YAG (1.64μm) - Ho:YLF(2.05μm) - Ho:YAG (2.09μm) - Cr:ZnS It is.
[0052] In a further optional method step, the carrier substrate can be measured to ascertain whether the metallization deposited in the cavities needs to be removed, in order to be able to reuse the carrier substrate, which can then be used for the temporary bonding of other product substrates.
[0053] Carrier Board The carrier substrate can have any arbitrary shape, but is preferably circular. The diameter of the substrate is in particular industrially standardized. For wafers, the industrially standard diameters are 1", 2", 3", 4", 5", 6", 8", 12" and 18". The carrier substrate is sized and shaped to match the size and shape of the product substrate so that the handling technology employed is as simple as possible. Different substrate sizes require so-called bridge tools, which are configured more complexly than the devices and tools for one substrate size.
[0054] In principle, however, the present invention can handle any substrate, regardless of its diameter. The carrier substrate of the temporary bonding and debonding method according to the present invention can be implemented as a wafer. Preferably, the carrier substrate is a glass substrate.
[0055] According to the invention it is envisaged that the described temporary bonding method can be used to fasten non-circular substrate panels which can then be processed and separated from a carrier substrate.
[0056] The material of the carrier substrate can be a semiconductor material, in particular silicon. Preferably, advantageous polycrystalline silicon wafers can be used as the carrier substrate. In a particularly preferred embodiment according to the invention, the carrier substrate is made of technical glass.
[0057] The carrier substrate preferably has at least one of the following features: - Particle-free and / or - CMOS compatible and / or - mechanical stiffness and / or - Thermal conductivity that matches or exceeds that of the product substrate and / or - Heat resistance above the maximum processing temperature and / or - Thermal stability above the maximum processing temperature and / or - Minimal, and preferably no, outgassing, also described as low vapor pressure, resulting in high vacuum compatibility; and / or - Thermal expansion and / or thermal expansion characteristics to match the product substrate - Transparency to abrasive radiation.
[0058] The transparency is preferably expressed by the transmittance, which indicates the ratio of the transmitted radiation to the incident radiation. However, the transmittance is not a purely material-specific property, since it depends on the thickness of the object to be transmitted. The transmittance values are therefore given per unit length of 1 cm. For a selected thickness of 1 cm and for the respective selected wavelength, the material has in particular a transmittance of more than 70%, preferably more than 80%, even more preferably more than 90%, very preferably more than 95% and most preferably more than 99%. The transparency is particularly preferably related to the wavelength of the ablation radiation.
[0059] For the functionality of the carrier substrate, its thermal conductivity is equally important, since it is desirable for the action of the ablation radiation as localized heating to dissipate quickly. The thermal conductivity of the carrier substrate is preferably 0.1 W / (m·K) to 5000 W / (m·K), more preferably 1 W / (m·K) to 2500 W / (m·K), even more preferably 0.5 W / (m·K) to 1000 W / (m·K).
[0060] In a particularly preferred embodiment of the carrier substrate, the carrier substrate is implemented in a structured manner. The carrier substrate comprises high points which are stably connected to the product substrate via metal contacts and low points which are present as channels or cavities between the high points. As a characteristic factor for the nature of the carrier substrate, the bearing area ratio can be determined, i.e. the ratio of the determined area of the high points to the total area of the carrier substrate. The bearing area ratio of the carrier substrate is preferably less than 80%, more preferably less than 75%, particularly preferably less than 50%, very particularly preferably less than 25%, ideally less than 10%. However, the product substrate can be connected to the carrier substrate very firmly, so that the substrate stack can be further processed as a monolithic body and no undesired separation occurs.
[0061] The idea behind the arrangement of the cavities and the elevations is to allow an efficient holding and a fast and efficient separation of the product substrate from the carrier substrate by structuring the carrier substrate or the elevations of the carrier substrate in such a way that there is only a defined pattern of metal connection points with the product substrate and no surface metallization.
[0062] Alternatively, in another embodiment of the carrier substrate, it is contemplated that a temporary metal bond with the product substrate is created over the entire area.
[0063] Furthermore, in an exemplary embodiment of the carrier substrate, a temporary metallic bond with the product substrate is preferably generated near the edge of the carrier substrate, in particular in a completely closed annular body, and it is conceivable that further elevations of the carrier substrate (preferably uniformly across the inner surface of the metallized annular body) support the product substrate in a point-like and / or small-area manner without metallic contact.
[0064] It is possible that not all elevations are in metallic contact with the product substrate, but preferably only at certain points distributed around the periphery of the substrate stack.
[0065] It is therefore more advantageous according to the invention if the surface of the metallization area is coplanar with the surface of the higher non-metallization area. According to the invention, this can be easily achieved by producing the metallization itself at small low points. For example, it would be conceivable to produce a complete annular groove at the periphery of the carrier wafer. Then, according to the invention, the metallization is produced only in this groove, while the higher points inside the groove, which are intended to stabilize and support the product substrate, are free of metallization. The various method steps for metallizing only the groove while leaving the area near the center metallized will not be dealt with further here. The skilled person knows how the inner part of the carrier substrate can be masked and protected.
[0066] Such a structure of the carrier substrate allows the evaporated or liquefied metal near the high points, especially the point-like high points, to condense and solidify and / or resublime in the cold cavity during separation. In this way, material is selectively removed locally from the temporary bonding layer. Thus, once the temporary bonding layer has finally undergone a phase transition to the solid phase, no new metal is brazed and / or bonded. Thus, as a result, the substrate stack can be easily separated after the selective destruction of all the bonds.
[0067] In a particularly preferred embodiment of the carrier substrate, the elevation has a flatness, expressed as total thickness variation (TTV), of less than 100 μm, preferably less than 10 μm, more preferably less than 1 μm, very preferably less than 100 nm, most preferably less than 10 nm, and very preferably less than 1 nm. In this way, the product substrate can retain a particularly flat surface.
[0068] In another particularly preferred embodiment of the carrier substrate, the elevations are implemented as individual cambered areas, so that preferably point-like contact occurs between the carrier substrate and the product substrate, and the self-aligned form of metallization allows a reduction in the area of metal contacts that are temporarily bonded, preferably by capillary action.
[0069] It is furthermore conceivable that the carrier substrate can be partially treated prior to metallization to make it metal-repellent, so that only the desired elevated areas are wetted, in particular by the immersion metallization.
[0070] Advantageously, it is conceivable to adapt the respective areas of the height of the carrier substrate to the diameter of the stripping radiation.As a concrete numerical example, in particular in the case of a laser spot size of 30 micrometers in diameter, the height can be embodied as an area having a diameter of 30 micrometers, preferably 28 micrometers, particularly preferably 25 micrometers.
[0071] Typically this means that the height is less than 95% of the cleavage spot size, preferably less than 90% of the cleavage spot size, and particularly preferably less than 85% of the cleavage spot size, in order to achieve fast, efficient and energetic energy uptake during separation of the substrate stack.
[0072] Temporary Joining Method It is preferably conceivable to provide the product substrate with a protective layer prior to temporary bonding to the substrate surfaces to be bonded. The formation of the protective layer on the product substrate can be carried out spatially and / or temporally separate from the further method step of temporary bonding.
[0073] In a preferred embodiment, the protective layer can act as a diffusion barrier for the metallization to protect the product substrate from the temporary bond layer.
[0074] In a further preferred embodiment, the protective layer is capable of protecting the structured substrate surface of the product substrate, in particular by releasable filling and covering of cavities.
[0075] In a further preferred embodiment of the protective layer, the protective layer can act as an adhesion promoter between the product substrate and the metallization.
[0076] The metallization is applied to the prepared substrate surfaces to be bonded. In an alternative embodiment of the method, the metallization is applied to the protective layer.
[0077] In an alternative embodiment of the method according to the invention, the metallization can be applied to a carrier substrate.
[0078] Advantageously, low-melting metals or alloys, in particular eutectic alloys, can be used. Particularly advantageously, the applied metallization of the product substrate does not penetrate into the structure of the product substrate, so that the method does not cause any doping or any contamination.
[0079] In a further preferred embodiment, the metallization may be comprised of the metal or alloy of the permanent bond layer used in further processing, such that diffusion of the metallization does not adversely affect the product substrate.
[0080] In particular, CMOS compatible metals and / or alloys can be used.
[0081] In particular, the following compounds or elements may be included in the metallization: - Metals, especially Cu, Ag, Au, Al, Fe, Ni, Co, Pt, W, Cr, Pb, Ti, Ta, Zn, Sn - Compounds, in particular nitride compounds, in particular AlN, GaN, TiN, TaN.
[0082] Preferably, the metals and / or alloys for the temporary bonding layer are selected from metals that have sufficient strength for processing at a sufficiently low melting temperature.
[0083] As alloys, it is particularly advantageous to use eutectic alloys as metallization.
[0084] When using alloys with a eutectic concentration, the eutectic concentration can be generated during the production of the metallization or can be adjusted during the joining. Eutectic alloys are characterized by the lowest melting point of all possible alloys that can be produced by changing the alloy composition. By exceeding the eutectic temperature, i.e. the temperature at which the liquid phase is in equilibrium with the solid phase of the eutectic, the eutectic melts completely. The liquid phase of the eutectic concentration that is created wets the surfaces of the two substrates that are to be joined together in the areas that are not yet liquefied. Then, during the solidification process, this liquid phase solidifies into a eutectic and forms a connection layer between the two substrates as a temporary joining layer.
[0085] According to the invention, it is particularly conceivable that during the production of the metallization, one alloy component is applied to the product substrate and one alloy component is applied to the carrier substrate.
[0086] According to the invention, it is particularly conceivable to apply the metallization to the product substrate as a layer sequence of different metals and / or alloys as alloy components and / or as a complete metallization.
[0087] According to the invention, in an alternative embodiment of the method it is possible, inter alia, for the metallization to be applied to the carrier substrate as a layer sequence of alloy components and / or as a complete metallization.
[0088] It should be noted in particular that, in order to be able to carry out the third method step optimally, the layers produced, i.e. the protective layer and the at least one metallization, should not show any degradation and / or corrosion phenomena at room temperature and in normal atmosphere. Alternatively, the metallized substrate can be stored under protective conditions in an inert atmosphere and / or in vacuum.
[0089] As application techniques for the metallization, plating, evaporation, sputtering and electrochemical deposition processes such as chemical vapor deposition (CVD) are particularly suitable.
[0090] In a further method step, the product substrate is connected together with a carrier substrate in a temporary bonding method for metal temporary bonding, in particular thermally. According to the invention, it is particularly conceivable for the temporary bonding to be carried out in a vacuum bonding chamber.
[0091] In a preferred embodiment, the temperature of the temporary bonding method may be sufficiently lower than the further processing temperature of the product substrate, particularly to retard or preferably prevent undesirable diffusion processes.
[0092] It is particularly advantageous according to the invention that the use of metal-metal bonds reduces the particle loading of the substrate, in particular from particles of organic residues.
[0093] According to the invention, it is particularly advantageous for the temporary molten metal bond layer to incorporate particles as inclusions within itself, whereby a better bond quality can be achieved.
[0094] In particular, according to the invention it is contemplated that the metal-metal temporary bonding is carried out as a transient-liquid-phase (TLP) bond.
[0095] In particular, it is conceivable according to the invention that a metallization for the temporary bond is applied to the carrier substrate, such that a temporary bond occurs between the metallized substrate surface of the carrier substrate and the protective layer of the product substrate.
[0096] In particular, it is also conceivable according to the invention for a metallization for the temporary bonding to be applied to the carrier substrate, so that a temporary bond occurs between the metallized substrate surface of the carrier substrate and the substrate surface of the product substrate to be bonded.
[0097] In particular, according to the invention, it is conceivable to connect the used metal joints to one another in a fusion bonding method as well as in a hybrid bonding method with subsequent heat treatment to produce a temporary joint. Fusion bonding occurs mainly at the surface of non-metallic-non-organic materials. In this case, if the surface parts of the product substrate and the carrier substrate are particularly intimately bonded to one another, hydrogen-bridged bonds can be generated, so that the substrates are particularly protected and can be transported for further processing, such as heat treatment. The fusion bonding itself is merely for pre-fixing, so that the metal areas to be connected to one another can be held in place. This pre-fixing is called pre-bonding in the prior art.
[0098] The pre-bonding method refers to a process in which two substrates are bonded to each other only by van der Waals forces. This bonding process is mainly carried out between silicon and / or silicon oxide substrates. The bond thus produced is called pre-bonding because it is a preliminary step for a further connection. In the semiconductor industry, it is very often desired to separate again the (temporary) connection produced by pre-bonding if, after pre-bonding, it turns out that the two substrates are not optimally positioned relative to each other, or even incorrectly positioned. Two substrates connected to each other by pre-bonding can usually be separated from each other again without damage.
[0099] In other words, a fusion bond is created as a pre-bond at the non-metallic surface portions between the product substrate and the carrier substrate for pre-fixing the substrate stack.
[0100] The metallized planar surface portion of the carrier substrate can then be metallurgically temporarily bonded to the product substrate by a heat treatment.
[0101] The method according to the invention for fusion bonding of a product substrate and a carrier substrate comprises the following method steps in one exemplary embodiment: In a first method step of the exemplary method, the surfaces to be joined of the product substrate and / or the carrier substrate are prepared and structured.
[0102] In a second method step, the surfaces to be joined of the product substrate and / or the carrier substrate are activated by plasma treatment, in particular in a plasma chamber.
[0103] In a third method step, the surfaces to be joined are cleaned, in particular with pure water, so that any particles that may have formed are likewise removed.
[0104] In a fourth method step, the product substrate and the carrier substrate are aligned with respect to one another at least purely mechanically.
[0105] In a fifth method step, the product substrate and the carrier substrate are brought into contact with one another at at least one point and a bond wave is generated, the passage of which pre-bonds the substrate stack to one another.
[0106] In a sixth method step, the substrate stack consisting of the product substrate and the carrier substrate is subjected to a heat treatment to generate a metal-metal temporary bond, the bonding force (van der Waals forces) of the preliminary bond being smaller than the holding force of the metallic temporary bond layer.
[0107] Unlike typical hybrid bonding techniques, the present temporary bonding method does not involve permanent planar bonding of non-metallic substrate surfaces.
[0108] The basic idea of the temporary bonding method defined in this specification is to produce a substrate stack consisting of at least a carrier substrate, a metallic temporary bonding layer and a product substrate.
[0109] In other words, the temporary bonding method of the present disclosure produces a substrate stack, in which the temporary bonding layer is a metal or metal alloy layer, which can be removed from the product substrate in a particularly residue-free and particle-free manner. A further advantage is that the substrates of the substrate stack can absorb higher processing forces than when using a polymer interlayer. The separation method described below allows the substrate stack to be separated with little force and / or with little distortion and / or with little stress. Furthermore, it is advantageous that no solvents and / or chemicals, in other words wet chemistry, need to be used for the separation.
[0110] Thus, a product substrate protected and supported in this manner as part of a substrate stack can be further processed more conveniently, material-friendly, and cost-effectively than a substrate stack secured with an adhesive polymer.
[0111] Peeling Method A method for separating a carrier substrate from a product substrate comprises, in one exemplary embodiment, the following steps, particularly in the following order: In a first method step the temporarily bonded substrate stack is attached and fixed to a substrate holder.
[0112] The substrate holder and the fixing means serve to fix the substrate. The fixing means includes: 1. Mechanical fastening means, especially 1.1. Clamp 2. Vacuum fixing means, in particular 2.1. Individually controllable vacuum tracks 2.2. Interconnected vacuum tracks having Electrical fastening means, in particular 3.1. Electrostatic Fixation Means 4. Magnetic fastening means 5. Adhesive fastening means, in particular gel pack fastening means and / or 6. Fixing means with an adhesive, particularly controllable, surface It may be.
[0113] The fixing means are in particular electronically controllable.
[0114] The vacuum fastening means is a preferred fastening type. It preferably consists of a number of vacuum tracks which emerge at the surface of the substrate holder. The vacuum tracks are preferably individually controllable. In technically feasible applications, a number of vacuum tracks are integrated to form vacuum track segments which are individually controllable and thus can be individually evacuated or flooded. However, each vacuum segment is independent of the other vacuum segments. In this way, the possibility of configuring individually controllable vacuum segments is obtained. The vacuum segments are preferably annular. This allows a targeted radially symmetrical fastening and / or detachment of the substrate, in particular the product substrate, from the substrate holder, in particular from the inside to the outside.
[0115] In a second method step, at least one energy beam flux, in particular a laser beam, having at least one wavelength is focused through the carrier substrate onto the metal temporary bonding layer, thereby melting and evaporating or sublimating the temporary bonding layer.
[0116] In an alternative embodiment, multiple beams can be introduced in parallel for energy input into the temporary bond layer.
[0117] In a preferred embodiment, the substrate stack is brought to a predetermined temperature on the substrate holder and can be cooled or heated, which in particular allows a larger thermal gradient for crack formation to be achieved. Furthermore, the advantage of the temperature treatment, in particular cooling, is that the gaseous products of the ablation radiation can condense and / or resublime more quickly.
[0118] The energy input for the phase transformation of the metallic temporary bond layer is preferably introduced into the temporary bond layer in a pulsed manner, which reduces undesired global heating of the substrate stack.
[0119] The energy input is in particular through the carrier substrate, which is at least generally transparent to the stripping radiation, and directly into the temporary bonding layer, whereby the product substrate, which is optionally doped and / or metallized to be opaque to the stripping radiation, can be separated from the carrier substrate.
[0120] According to the invention, it is particularly advantageous to measure the reflected radiation, in particular continuously, during the energy input of the delamination radiation into the temporary bonding layer. This allows the radiation output of the delamination device to be controlled, in particular in real time. Furthermore, it is possible to deduce from the amount of reflected radiation whether local separation has occurred or not. The proportion of reflected radiation changes during the delamination process.
[0121] In a third method step, the locally heated metal vapor is resublimated or condensed and solidified, particularly in the deeper peripheral cavities of the carrier substrate.
[0122] In an alternative embodiment, locally heated metal vapor in a deeper peripheral cavity of the carrier substrate may first condense and then solidify.
[0123] In other words, in a third method step the temporary bonding layer is locally removed by means of a pulsed laser beam.
[0124] In that case, the carrier substrate is designed in such a way that the metal vapor is transported into the cavity with a specifically optimized flow, so that resublimation or condensation and solidification is a controlled process and is not subject to physical action.
[0125] This can be influenced in particular by the following actively adjustable parameters: - the design of the carrier substrate (percentage of support area, shape and location of cavities, pressure in the cavities of the substrate stack) and / or - the energy input of the ablation radiation (parameters: time, wavelength, energy density, area of the laser spot) and / or - the overall temperature of the substrate stack and / or the temperature gradient between the spot heated by the delamination radiation high on the carrier substrate and the bottom of the cavity).
[0126] In order to influence the delamination process in a targeted manner, it is particularly conceivable according to the invention to cool one side of the substrate stack and heat the other side of the substrate stack, in particular by heating the product substrate and simultaneously cooling the carrier substrate, in particular by dry ice or liquid nitrogen rinsing, in order to locally influence a targeted condensation and / or resublimation.
[0127] The removed metallization is in particular embedded in cavities in the carrier substrate.
[0128] In particular, a protective layer applied to a product substrate can absorb a portion of the metallization that has re-sublimated or condensed and solidified.
[0129] In a fourth method step, the carrier substrate and the product substrate are suitably separated from each other.
[0130] In a fifth optional method step, the carrier substrate can be measured to ascertain whether the deposited metallization should be removed, after which the carrier substrate can be used for temporary bonding of other product substrates.
[0131] The method may proceed in an automated manner within the device, for which each method step may be stored and executed as a recipe.
[0132] A recipe is a collection of optimized values of functionally or process-technically relevant parameters. The use of recipes makes it possible to ensure the reproducibility of production processes.
[0133] Metal temporary joining device The apparatus used for the temporary bonding according to the present invention is a bonding apparatus for metal temporary bonding.
[0134] The functionally significant components of the temporary joining device may in particular be modular and may include the following modules: - Joint Module - Alignment Module - Cleaning module - Activation module - Metallization Module - Coating Module - Mobile devices and / or - Supply modules especially for compressed air, vacuum.
[0135] The temporary bonding method according to the invention is carried out in a bonding module, for which the substrate is preferably held fixedly on a substrate holder and bonded thermally, such that a functional integration of the thermal bonding chuck and the substrate holder can be achieved.
[0136] According to the invention it is particularly conceivable that the temporary bonding according to the invention is carried out by means of a permanent bonding device.
[0137] For temporary bonding, an alignment module can create a pre-bond, similar to hybrid bonding, and a bonding module, such as a temperature controlled oven, can metallurgically connect multiple substrate stacks together simultaneously, especially in a batch process.
[0138] The alignment accuracy between the product substrate and the carrier substrate can occur by mechanical alignment or in particular optical alignment of the substrate edges. In some cases alignment using alignment marks on the substrate and / or the substrate holder is also possible.
[0139] The alignment accuracy between the product substrate and the carrier substrate is less than ±150 micrometers, preferably less than ±100 micrometers, particularly preferably less than ±50 micrometers, very particularly preferably less than ±25 micrometers, optimally less than ±10 micrometers and ideally less than ±1 micrometer relative to the center point and / or peripheral edge of the substrates and / or any present alignment marks.
[0140] It is particularly advantageous in accordance with the present invention that a bonding apparatus capable of producing a temporary metal bond between substrates can be used for a permanent metal bond as well.
[0141] In a temporary bonding apparatus for metal temporary bonding, in particular high points of a carrier substrate are metallurgically bonded and thus connected to corresponding areas of a product substrate, in other words a substrate stack is produced in the temporary bonding apparatus, in which high points of the carrier substrate are connected to the product substrate by means of a metal temporary bonding layer for further processing of the latter.
[0142] The bonding force required to bond the product substrate to the carrier substrate will vary depending on what substrate size and / or what metallization and / or what metallized bonding surface is required by the industry.
[0143] A joining force of 10N to 100kN, preferably 10kN to 90kN, particularly preferably 30kN to 80kN, can be used. With this joining force, a particularly good contact between the substrates can be obtained. It has been found that a relatively high joining force is advantageous for metal joining, in which case the starting material for the metallization can develop a thin native oxide layer, which can be destroyed by the joining force.
[0144] Metal temporary joint peeling device The apparatus used for the peeling according to the present invention is a peeling apparatus for metal temporary bonding.
[0145] Stripping devices for temporary metal bonding can in particular be constructed in a modular manner: if the stripping device is constructed as an individual device without modules, the designations of the modules are regarded as characteristics of the individual functional groups and / or components.
[0146] In particular, at least the following modules may be present in the stripping device: - Peeling module - More modules.
[0147] Further modules may include the following modules: - A cleaning module, especially for removing the protective layer - Cleaning module for removing excess metallization from the carrier substrate - Modules for carrier flip-flops, especially tape or laminate modules for fastening thin product substrates - Measuring modules for metallization and / or - Separate laser module for peeling module.
[0148] According to the invention, it is advantageously possible, in particular, to generate the stripping radiation by a separate laser module and to introduce only "cold" radiation into the stripping module. In this way, auxiliary heat sources in the apparatus can be reduced. The laser module can be transferred to the grey room of the clean room with the optical elements of the laser module appropriately sealed, while ensuring proper cooling of the radiation source. The properly air-conditioned clean room is thus not heated, and thus the waste heat can be better removed from the apparatus.
[0149] The radiation source of the ablation module generates the ablation radiation, in particular a laser beam, but it is also possible to use an electron beam as the ablation radiation.
[0150] Regarding electromagnetic radiation, we disclose the use of various electromagnetic sources that can be used in the separation according to the present invention to generate the ablation radiation: - Microwave source - Infrared sources, especially those emitting mid-infrared (MIR) radiation - visible light radiation source - UV light sources and / or - X-ray source.
[0151] In particular, radiation sources suitable for causing the inventive separation of the carrier substrate from the product substrate by electromagnetic waves, in particular by disintegration, very preferably by sublimation, of the metal connection layer, are considered.
[0152] Yet another aspect of the present invention is that metals have a very high absorption capacity for infrared radiation, so that the metal temporary bonding layer is very well suited for destruction by an infrared laser.
[0153] The electromagnetic radiation of such sources may be incoherent or coherent. Sources that emit coherent electromagnetic radiation (lasers) are preferred. Microwave sources that emit coherent microwave radiation are called masers.
[0154] In the remainder of this patent specification, coherent means spatial and / or temporal coherence.
[0155] The wavelength of the ablation radiation is between 10 nm and 10 mm, preferably between 150 nm and 200 micrometers, particularly preferably between 400 nm and 30 micrometers and very particularly preferably between 1 micrometer and 10 micrometers.
[0156] According to the invention, it is particularly advantageous if the maximum absorbance of the metal temporary bonding layer and the wavelength of the delamination radiation source are adjusted to each other, so that delamination can occur effectively. It is also advantageous according to the invention if the maximum absorbance of the metal temporary bonding layer, the maximum transmittance of the carrier substrate and the wavelength of the delamination radiation are adjusted to each other. For this purpose, the skilled person can use the well-known Beer-Lambert law.
[0157] According to the invention it is provided that if no ablation radiation is used but the radiation source remains switched on, the ablation radiation from the continuously operating radiation source can be interrupted by an electromechanical chopper and / or mirror system and / or sent to a sink.
[0158] In the case of a switchable radiation source, such as an LED laser, the pulse duration of the ablation radiation can be electronically controlled and / or adjusted.
[0159] Stripping radiation is directed at the metallurgically connected regions of the substrate stack in the stripping apparatus.
[0160] An important physical parameter of the electromagnetic radiation used is its intensity. The intensity is expressed in watts. The intensity of the electromagnetic radiation is in particular greater than 0.1 watt, preferably greater than 1 watt, even more preferably greater than 100 watts, very preferably greater than 1000 watts, and most preferably greater than 10 kilowatts.
[0161] In the ablation device, the intensity profile, i.e. the progression of the intensity along the direction through the emission form of the ablation radiation, can be arbitrarily adjusted by means of optical elements. A preferred intensity profile is: - Gaussian profile - Rectangular Profile - Triangular profile and / or - Oval profiles, especially circular profiles It is.
[0162] The laser power, measured as the optical power, in particular the radiative power, that can be continuously delivered to the substrate stack, in particular the temporary bonding layer, is in particular at least 5 W, preferably more than 10 W, even more preferably more than 15 W, very preferably more than 17 W and most preferably more than 30 W.
[0163] The preferred wavelength range of the laser is from 100 nm to 10000 nm, preferably from 250 nm to 1100 nm, even more preferably from 270 nm to 430 nm, and very preferably from 280 nm to 380 nm.
[0164] In another embodiment, the preferred wavelength range of the laser is from 1000 nm to 10000 nm.
[0165] In a particularly preferred embodiment, the wavelength of the laser is tunable and / or filterable by means of a frequency converter, in particular an acousto-optical modulator, in particular a Bragg cell.
[0166] In a further preferred embodiment of the device, the laser beam comprises at least one of the following wavelengths: 1064 nm, 420 nm, 380 nm, 343 nm, 318 nm, 308 nm, 280 nm.
[0167] In particular, the use of a laser beam having at least two wavelengths is particularly advantageous in that it makes it possible to produce a process which combines, in particular, a photochemical and a photothermal treatment in the temporary bonding layer.
[0168] In one particularly preferred embodiment of the device, the radiation source is a diode laser.
[0169] The total energy of the laser beam per substrate is set in the range particularly from 0.01 mJ to 5000 kJ, preferably from 0.1 mJ to 4000 kJ, and particularly preferably from 100 mJ to 2000 kJ.
[0170] The laser beam can be operated in a continuous mode or can be pulsed.
[0171] The pulse frequency is set in particular between 0.1 Hz and 300 MHz, preferably between 100 Hz and 500 kHz, particularly preferably between 10 kHz and 400 kHz, very particularly preferably between 100 kHz and 300 kHz.
[0172] The number of pulses per substrate stack is, depending on the total energy required, preferably more than 1 million pulses, preferably more than 3 million pulses, particularly preferably more than 5 million pulses, very particularly preferably 6 million pulses.
[0173] The energy directed at the substrate stack per pulse is in particular set to between 0.1 nJ and 1 J, preferably between 1 nJ and 900 μJ, particularly preferably between 10 nJ and 500 μJ.
[0174] The irradiation area per pulse is 1 μm 2 ~100,000μm 2 , preferably 10000 μm 2 ~50,000μm2 , particularly preferably 1000 μm 2 ~40,000μm 2 , very particularly preferably 2500 μm 2 ~26000μm 2 It is.
[0175] A synonym for the illuminated area is known to those skilled in the art as spot size, laser spot size.
[0176] Irradiation of larger areas can be performed over the entire area or by a scanning process. If the area with the temporary bonding layer is approximately the same size as the irradiation area, a simple non-scanning irradiation is performed. If the area with the temporary bonding layer is larger than the irradiation area, preferably a scanning irradiation is performed.
[0177] The shape of the illuminated area is in particular circular, in another preferred embodiment elliptical and in a particularly preferred embodiment rectangular.
[0178] The ablation radiation is preferably focussable. The length over which the focal position can be varied is in particular more than 0.1 mm, preferably more than 1 mm, even more preferably more than 5 mm, very preferably more than 10 mm and most preferably more than 20 mm.
[0179] According to a preferred development of the present invention, the pulse mode operation of the source used for the electromagnetic peeling radiation is provided. The relatively high intensity and power density may cause heat conduction from the temporary bonding layer to the substrate. In order to prevent such heat conduction as much as possible, it is preferable to use pulsed electromagnetic radiation. The pulse duration is in particular less than 10 seconds, preferably less than 1 second, even more preferably less than 1 microsecond, very preferably less than 1 nanosecond, and most preferably less than 1 picosecond.
[0180] The purpose of pulsed mode operation of the delamination radiation is rapid, localized, point-wise heating of the temporary bond layer, preferably causing it to sublime, and less preferably causing it to first melt and then transition to a vapor phase.
[0181] By controlling the delamination radiation, the temperature profile, and in particular the temperature gradient, can be influenced, so that the resublimation or condensation and solidification of the disrupted temporary bond layer can be targeted locally.
[0182] Thus, by controlling the stripping radiation, the resublimation or condensation and solidification of the temporary bonding layer can be determined as well.
[0183] Further advantages, features and details of the invention will become apparent from the following description of preferred embodiments and from the drawings. [Brief description of the drawings]
[0184] [Figure 1] 1 shows a schematic diagram of a substrate stack according to the invention in a first embodiment; [Diagram 2] 3 shows a schematic view of a substrate stack according to the invention in a second embodiment during delamination. [Diagram 3] 5a-c show schematic views of a carrier substrate in different embodiments.
[0185] In the drawings, identical components or components having identical functions are designated by the same reference numerals. The drawings are not necessarily to scale with respect to the actual embodiment, since any illustrations may be shown enlarged for purposes of presentation.
[0186] 1 is a schematic diagram of a substrate stack 6 according to the invention. The substrate stack 6 comprises a structured carrier substrate 1, a temporary bonding layer 2, in particular made of metal, a protective layer 3 and a product substrate 4.
[0187] In this embodiment, the temporary bonding layer 2 is applied as a metallization over the entire area to a protective layer 3 as shown, which may be a thin atomic or molecular barrier layer.
[0188] 2 is a schematic view of another substrate stack 6' according to the invention during peeling. In this embodiment of the substrate stack 6', the metallization 2' is applied only to the elevated points 1'e of the carrier substrate 1', so that the metallization 2' represents only the intended partial areas of the temporary bonding layer. In other words, the temporary bonding layer 2' is applied in the form of islands. A protective layer 3' separates the product substrate 4' from the metallic temporary bonding layer 2'.
[0189] The stripping radiation 5 passes through the carrier substrate 1' and strikes a location on the temporary bonding layer 2' applied at the elevation 1'e.
[0190] The movement of the temporary bonding layer 2' into the peripheral cavity 1'k of the carrier substrate 1' is not shown. The convergence of the delamination radiation 5 represents both a deflection and a focusing of the delamination radiation 5 according to the target.
[0191] Fig. 3a shows a further embodiment according to the invention of a particularly transparent carrier substrate 1''. The carrier substrate 1'' has a number of elevations 1''e which can support a product substrate (not shown) and which form contact points for a temporary bonding layer (not shown).
[0192] The elevations 1''e can be particularly uniformly distributed on the carrier substrate, linearly or in a grid, so as to enable uniform force absorption of the processing forces. Between the elevations 1''e the cavities 1''k of the carrier substrate 1'' are arranged.
[0193] The deposition of residual temporary bonding layer after resublimation or condensation and solidification is not shown.
[0194] FIG. 3b represents a further embodiment according to the invention of a particularly transparent carrier substrate 1'''. The carrier substrate 1''' has a number of elevations 1''''e which can support a product substrate (not shown) and form contact points for a temporary bonding layer (not shown). In this embodiment of the carrier substrate 1''', the elevations 1''''e have a convex surface, which allows in particular a point-like contact with the product substrate (not shown). Compared to the embodiment of FIG. 3a, due to the capillary action of the convex elevations 1''''e, the effective area of the temporary bonding layer (not shown) is reduced. On the one hand, therefore, a material saving can be achieved by the temporary bonding layer. On the other hand, due to the reduced support area, an effective peeling can be achieved.
[0195] FIG. 3c shows a particularly transparent carrier substrate 1 IV 1 shows a further embodiment of the carrier substrate 1 according to the present invention. IV 1 IV e, and these high points 1 IV e can support a product substrate (not shown) and forms a contact point for a temporary bonding layer (not shown). IV So, height 1 IV e are dot-shaped. These are cavity 1 IV In this embodiment, the carrier substrate 1 is surrounded by a substrate 2. IV High above 1 IV The uniform distribution of e is particularly advantageous and the percentage of supported area compared to the other embodiments 3a and 3b may be smaller. [Explanation of symbols]
[0196] 1,1',1'',1''',1 IV Carrier Board 1''e,1'''e,1 IV e. High places 1''k,1'''k,1 IV k Cavity 2,2' Temporary bonding layer 3,3' protective layer 4,4' Product Board 5. Stripping radiation 6,6' Board Stack
Claims
1. A product substrate (4, 4') and a carrier substrate (1, 1', 1'', 1''', 1 IV ) and a temporary bonding method, the method comprising: said product substrate (4, 4') and / or said carrier substrate (1, 1', 1'', 1''', 1 IV ) producing a metallized temporary bonding layer (2, 2') on said substrate (2, 2'); - bonding the product substrate (4, 4') and the carrier substrate (1, 1', 1'', 1''', 1''', 1') on the metallized temporary bonding layer (2, 2') IV ) and a step of joining the At least The carrier substrate (1, 1', 1'', 1''', 1 IV ) is formed in a structured state, said carrier substrate (1, 1', 1'', 1''', 1 IV ) is high (1''e, 1''e, 1 IV e) and cavity (1″k, 1′″k, 1 IV k), and said elevations (1''e, 1''e, 1 IV e) is stably connected to the product substrate (4, 4') via metal contacts, and the cavities (1''k, 1''k, 1'' IV k) is the high point (1''e, 1''e, 1 IV e) disposed between.
2. 2. The method according to claim 1, wherein the temporary bonding layer (2) is produced over the entire area, in particular on a protective layer (3, 3') on the product substrate (4, 4').
3. The temporary bonding layer (2') is partially bonded to the carrier substrate (1, 1', 1'', 1''', 1 IV ) high up (1''e, 1''e, 1 IV The method of claim 1, wherein the above-mentioned
4. The product substrate (4, 4') and / or the carrier substrate (1, 1', 1'', 1''', 1 IV 4. The method according to claim 1, further comprising the step of applying a protective layer (3, 3') to the product substrate (4, 4') before producing the metallized temporary bonding layer (2, 2') on the product substrate (4, 4').
5. 5. The method according to claim 1, wherein the bonding is performed thermally.
6. A product substrate (4, 4') and a carrier substrate (1, 1', 1'', 1''', 1 IV ), a substrate stack (6, 6') comprising the product substrate (4, 4') and the carrier substrate (1, 1', 1'', 1''', 1 IV ) are connected by a metallized temporary bonding layer (2, 2'), 1. A substrate stack (6, 6'), characterized in that the carrier substrate (1, 1', 1'', 1''', 1 IV ) is formed in a structured state, the carrier substrate (1, 1', 1'', 1''', 1 IV ) has elevations (1''e, 1'''e, 1 IV e) and cavities (1''k, 1'''k, 1 IV k), the elevations (1''e, 1'''e, 1 IV e) being stably connected to the product substrate (4, 4') via metal contacts, and the cavities (1''k, 1'''k, 1 IV k) being arranged between the elevations (1''e, 1'''e, 1 IV e).
7. Carrier substrate (1, 1', 1'', 1''', 1 IV 13. A method for peeling a product substrate (4, 4') from a carrier substrate (1, 1', 1'', 1''', 1') by a method according to claim 1 , comprising the steps of: IV ) are connected by a metallized temporary bonding layer (2, 2') to form a substrate stack (6, 6'), the method comprising the steps of: - mounting and fixing said substrate stack (6, 6') on a substrate holder; - focusing a stripping radiation (5), in particular a laser beam, through the carrier substrate onto the metallized temporary bonding layer (2, 2'), thereby melting, evaporating and / or sublimating the metallized temporary bonding layer (2, 2'); said carrier substrate (1, 1', 1'', 1''', 1 IV Separating the product substrate (4, 4') from the substrate (4, 4'); The method includes at least the following steps.
8. The carrier substrate (1, 1', 1'', 1''', 1 IV 8. The method of claim 7, wherein the thermal conductivity of the material is from 0.1 W / (m·K) to 5000 W / (m·K), preferably from 1 W / (m·K) to 2500 W / (m·K), even more preferably from 0.5 W / (m·K) to 1000 W / (m·K).
9. The method according to claim 7 or 8, characterized in that the substrate stack (6, 6') is heated and / or cooled by a heating section and / or a cooling section.
10. The method according to any one of claims 7 to 9, characterized in that the stripping radiation (5) is focused in a pulsed manner on the metallized temporary bonding layer (2, 2').
11. The method according to any one of claims 7 to 10, further comprising measuring the energy input of the delamination radiation (5) into the metallized temporary bonding layer (2, 2') and controlling the radiation power of the delamination radiation (5).
12. The carrier substrate (1, 1', 1'', 1''', 1 IV Before separating the product substrate (4, 4') from the cavity (1k, 1'k, 1''k, 1''''k, 1 IV 12. The process according to claim 7, wherein condensation and solidification and / or resublimation occur within k).
13. A carrier substrate (1, 1', 1'', 1''', 1') is formed by the method according to any one of claims 7 to 12. IV 1. An apparatus for peeling a product substrate (4, 4') from a carrier substrate (1, 1', 1'', 1''', 1 IV ) are connected by a metallized temporary bonding layer (2, 2') to form a substrate stack (6, 6'), a substrate holder for mounting and fixing said substrate stack (6, 6'), a radiation source for focusing a stripping radiation (5), in particular a laser beam, through the carrier substrate onto the metallized temporary bonding layer (2, 2'), thereby melting, evaporating and / or sublimating said metallized temporary bonding layer (2, 2'); said carrier substrate (1, 1', 1'', 1''', 1 IV a separation means for separating the product substrate (4, 4') from the substrate (4, 4'); An apparatus comprising at least
Citation Information
Patent Citations
Wafer debonding using mid-wavelength infrared radiation ablation
US20170125268A1
Wafer handler for infrared laser release
US20170170048A1
Method for the bonding and debonding of substrates
US20180233394A1
Kit, and laminate body
WO2016152598A1
Cited By
Heterogeneous annealing method and device
US12696818B2
Rapid thermal processing for direct bonding
US12757806B2
Rapid thermal processing for direct bonding
US20240079376A1