Particulate material made of novel MXene nanosheets, dispersion containing said particulate material, and method for producing said dispersion
The described method produces ultra-thin, stable MXene nanosheets through bead milling with controlled dispersion, addressing the limitations of existing exfoliation techniques and enabling effective conductive and shielding films.
Patent Information
- Application Number
- JP2023520702
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-05-13
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-05-13
AI Technical Summary
Existing methods struggle to exfoliate MXene particles thinner than a single layer or larger in size, leading to difficulties in creating ultra-thin conductive and electromagnetic shielding films, and the exfoliated nanosheets are prone to oxidation, limiting their industrial application.
A method involving bead milling with specific conditions using microbeads and a dispersion medium containing water or dimethyl sulfoxide to produce MXene nanosheets with a thickness of 1.0 to 3.5 nm and size of 1.5 to 2.0 μm, stabilized in a dispersion medium, ensuring efficient peeling and oxidation resistance.
The method achieves stable, ultra-thin MXene nanosheets suitable for forming dense conductive and electromagnetic shielding films, enhancing their conductivity and extending their lifespan for industrial applications.
Smart Images

Figure 0007579550000004 
Figure 0007579550000005 
Figure 0007579550000006
Abstract
Description
Technical Field
[0001] The present invention relates to a particulate material composed of novel MXene nanosheets, a dispersion liquid containing the particulate material, and a method for producing the same.
Background Art
[0002] Conventionally, a particulate material composed of an MXene layered compound obtained by removing Al by acid treatment from MAX phase ceramic powders such as Ti3AlC2, which is a layered compound (hereinafter, may be appropriately referred to as "MXene particulate material", "MXene nanosheet", "layered compound particulate material", or simply "particulate material") is known (Patent Documents 1, 2, 3, 4). Since these MXene layered compounds can store / desorb Na ions or Li ions in the void layer from which the Al layer has been removed, they are used as negative electrode active material for secondary batteries (storage batteries) and capacitors, and are expected to be applied to electromagnetic shielding thin films and conductive thin films because of their excellent conductivity.
[0003] MAX phase ceramics are layered compounds, and the general formula is M n+1 AX n and is represented by. In the formula, M is a transition metal (Ti, Sc, Cr, Zr, Nb, etc.), A is a group A element, X is C, or [C (1.0-x) N x (0 < x ≦ 1.0)], and n is from 1 to 3.
[0004] Among them, when A is Al, since the bond between M - A is weaker than the bond between M - X, the Al layer is selectively removed by acid treatment. The present inventors have proposed a method for preparing MXene nanosheets by thinning them with a bead mill using micro-sized beads (Patent Documents 5, 6).
[0005] The methods described in Patent Documents 5 and 6 disclose that MXene particle material having an average thickness of 3.5 nm to 20 nm and an average size of 0.05 μm to 0.3 μm can be obtained by peeling using a bead mill treatment with beads of 10 μm to 300 μm in ethanol or isopropanol (IPA) without removing the unpeeled portions by centrifugation. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2016-63171 A [Patent Document 2] JP 2017-76739 A [Patent Document 3] US Patent Application Publication No. 2017 / 0294546 [Patent Document 4] US Patent Application Publication No. 2017 / 0088429 [Patent Document 5] Patent No. 6564553 [Patent Document 6] Patent No. 6564552 Summary of the Invention [Problem to be solved by the invention]
[0007] Here, although the methods of Patent Documents 5 and 6 provide sufficiently thin and large particles, the present inventors have conducted further studies with the aim of peeling off even thinner (for example, to a monolayer level) and obtaining even larger nanosheet-like particle materials. By stacking and densely arranging thin and large nanosheet-like particle materials on a substrate, it is possible to produce extremely thin conductive thin films and electromagnetic wave shielding thin films. For example, thin films using metal plating or metal particle ink are granular, so electromagnetic waves penetrate through the gaps when electromagnetic waves penetrate. If a dense thin film oriented and stacked along the C axis is produced using the particle material of the present invention, electromagnetic waves will penetrate from the C axis direction, and the electromagnetic waves will surely pass through MXene, making it an effective electromagnetic wave shielding thin film. In this case, an MXene thin film may be formed on a thin film using metal plating or metal particle ink. Alternatively, an MXene thin film may be formed on an organic film in which metal particles are dispersed.
[0008] In addition, the nanosheet particle material obtained, exfoliated to the MXene monolayer level, is easily oxidized if left as is, so it was desirable to extend its lifespan for industrial application.
[0009] The present invention was completed in consideration of the above-mentioned situation, and the problem to be solved by this invention is to provide a particulate material consisting of a novel MXene nanosheet, a dispersion containing this particulate material, and a method for producing the same. [Means for solving the problem]
[0010] The particulate material of the present invention that solves the above problems is a Ti3Al4O5 having an average thickness of 1.0 to 3.5 nm, an average size of 1.5 to 2.0 μm, and an interlayer distance of the (002) plane of 1.350 nm to 1.400 nm. a (C x N 1-x )2, x=0.97 to 0.70, and a is greater than 0.02.
[0011] The dispersion of the present invention, which solves the above-mentioned problems, is a dispersion comprising the above-mentioned particulate material, and a dispersion medium in which the particulate material is dispersed at 0.1% by mass to 0.4% by mass and which contains 50% by mass or more of dimethyl sulfoxide (DMSO). It is more preferable that the dispersion medium contains 100% by mass of dimethyl sulfoxide (DMSO).
[0012] The method for producing a particulate material of the present invention, which solves the above problems, is a method for producing a particulate material made of MXene nanosheets, which comprises a peeling step of exfoliating the MXene to form an exfoliated product by colliding microbeads between layers of a mixture of a dispersion medium containing 50% by mass or more of water and MXene dispersed in the dispersion medium at a particle concentration of 10.0 mg / mL to 20.0 mg / mL in a bead mill using beads of 10 μm to 300 μm. In particular, the dispersion medium preferably contains 80% by mass or more of water. It is even more preferable that the dispersion medium contains 100% by mass of water. Effect of the Invention
[0013] The particulate material of the present invention has the above-mentioned configuration, thereby providing a particulate material made of MXene that is small in thickness and large in size. Furthermore, the dispersion of the present invention has the above-mentioned configuration, thereby being able to hold the particulate material made of MXene in a very stable state. The method for producing the particulate material of the present invention has the above-mentioned configuration, thereby being able to obtain a particulate material made of MXene that is small in thickness and large in size. [Brief description of the drawings]
[0014] [Figure 1] 1 shows AFM images of peeled products of Examples 1 and 2 and Comparative Example 1. [Diagram 2] 1 shows SEM photographs of peeled products of each of the Examples and Comparative Examples. [Diagram 3] 1 shows XRD profiles of Examples 1 and 2 and Comparative Examples 1 and 3. [Figure 4]6 shows spectra showing the wavelength dependence of transmittance of thin films obtained by spin-coating the peeled products of Examples 1 and 2 and Comparative Example 1. Note that, from the top, (a) to (c) show the number of spin coats applied 1, 2, 3, 4, and 5 times. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The particulate material, its manufacturing method, and dispersion of the present invention will be described in detail below based on the embodiments. The particulate material of the present embodiment is a particulate material made of MXene, which is small in thickness and large in size, and has excellent electrical properties such as electrical conductivity. Since the particulate material is small in thickness and large in size, it is possible to form a C-axis oriented, laminated, dense, and conductive thin film. The obtained thin film can be used as a conductive thin film, an electromagnetic wave shielding thin film, and the like. The MXene thin film can also be formed on a metal-plated substrate, on a thin film made of a metal particle ink, or on an organic film in which metal particles are dispersed. (particle material) The particulate material of the present embodiment is a particulate material made of large, thin-flaked MXene for application to electromagnetic wave shielding thin films, conductive thin film materials, etc. The particulate material made of thin-flaked MXene is obtained by exfoliating MXene, which is a powdered layered compound.
[0016] In this specification, when multiple upper and lower limit values are set for a certain parameter, the upper and lower limit values can be arbitrarily combined unless otherwise limited. The particulate material of this embodiment may be in the form of a plate, leaf, flake, sheet, etc., collectively referred to as a sheet.
[0017] The particle material of this embodiment is a layered compound consisting of three layers of titanium and two layers of carbon, or MXene, a layered compound in which part of the carbon is replaced with nitrogen. a (C x N 1-xThe particle material is made of MXene represented by the formula (2): where x=0.97 to 0.70, and a is greater than 0.02. The upper limit of a is preferably 0.05. (Hereinafter, this will be referred to as "MXene" where appropriate.) In addition to these elements, O, OH, and halogen groups can be present as surface functional groups.
[0018] The MXene constituting the particulate material has a "thickness" in the direction in which the layers of the layered compound are stacked, and a direction perpendicular to that thickness is the "sheet spreading direction," and the value measured in this direction is the size of the particulate material of this embodiment.
[0019] The thickness of MXene can be measured by dropping MXene onto a hydrophilized Si wafer and performing AFM analysis. The average thickness is 1.0 to 3.5 nm, and preferably 1.50 to 2.00 nm. The average thickness is calculated as the average value of the values measured for 100 randomly selected particles. The size of the nanosheet can be measured by dropping MXene onto a hydrophilized Si wafer and observing it with an SEM. The average size in the spreading direction of the nanosheet is 1.5 to 2.0 μm, and preferably 1.50 to 1.70 μm. If the maximum value in the direction perpendicular to the thickness is the "long side" and the minimum value is the "short side," the average value of [(long side + short side) / 2] measured by SEM for 100 randomly selected particles is taken as the average size in the spreading direction.
[0020] The interlayer distance of the (002) plane of MXene can be measured by X-ray diffraction analysis, and is preferably 1.350 nm to 1.400 nm, and more preferably 1.350 nm to 1.370 nm.
[0021] The zeta potential of MXene in water at pH 6 to pH 8 is preferably in the range of -29.0 mV to -34.0 mV. (Method of manufacturing particulate material) The method for producing a particulate material of this embodiment includes a peeling step and other necessary steps. Peeling process The peeling process involves the layered Ti3Al a (Cx N 1-x )2, x=0.97-0.70, a is more than 0.02. This is a process for obtaining sheet-like exfoliated material by exfoliating MXene by colliding microbeads between layers in a dispersion medium. The obtained exfoliated material becomes an exfoliated material suspension suspended in a dispersion medium. This exfoliated material suspension can be directly subjected to the mixing step, or the dispersion medium can be removed before being subjected to the mixing step. There is no particular limitation on the method for obtaining layered MXene as a material, but the following methods can be exemplified.
[0022] Ti3Al a (C x N 1-x )2, x = 0.97 to 0.70, a is greater than 0.02. MXene is obtained by acid-treating a raw material consisting of a Ti3-layer MAX phase ceramic powder to partially dissolve the Al layer. An example of a method for producing MXene will be described later as a pretreatment process. The raw material to be subjected to the peeling process can have the same composition as the material constituting the above-mentioned particle material. The composition does not change much in the peeling process.
[0023] This particulate material is treated with acid to dissolve some of the Al and turn it into MXene. This MXene is then mixed into a solvent whose main component is water to form a mixture. This mixture is then subjected to a peeling process in which it is processed in a bead mill that rotates at high speed using beads of 10 μm to 300 μm, resulting in an exfoliation suspension in which sheet-like MXene exfoliation material is suspended.
[0024] The dispersion medium used in the peeling step is not particularly limited except that it contains 50% by mass or more of water, but may also contain alcohols such as methanol, ethanol, isopropanol, ketones such as methyl ethyl ketone and acetone, dimethylformamide, dimethylsulfoxide, etc. In particular, the lower limit of the water content may be 60% by mass, 70% by mass, 80% by mass, 90% by mass, or 100% by mass.
[0025] The concentration of MXene in the mixture used in the peeling step is not particularly limited, but can be about 10.0 mg / mL to 20.0 mg / mL. The liquid property of the mixture is not particularly limited, but can be about pH 6.0 to 8.0.
[0026] The specific bead mill treatment in the peeling process will be described below. Peeling can be performed using a bead mill equipped with a mechanism for classifying a mixture of small beads and a slurry-like mixture by centrifugation. The peeled material peeled off by the bead mill treatment can be separated from the mixture before peeling by centrifugation at any time, and ultimately all of the MXene can be made into the peeled material.
[0027] For example, the lower limit of the bead size can be 10 μm, 15 μm, 20 μm, 30 μm, or 40 μm, and the upper limit can be 300 μm, 200 μm, or 100 μm. If the size is 10 μm or more, it is easy to classify the beads and the slurry. If beads of 300 μm or less are used, peeling can be prioritized over reducing the size of the particulate material. These lower and upper limits can be used in any combination. If the size of the beads is within the appropriate range, the energy applied can be increased and peeling can be prioritized, so it is most preferable to use beads of 50 μm to 100 μm.
[0028] The material of the beads is not particularly limited, but ceramics such as zirconia, alumina, and silicon nitride can be used. Partially stabilized zirconia, which has high fracture toughness, is particularly preferred. On the other hand, in a commonly used bead mill that classifies beads and slurry in a micro-sized gap using beads over 300 μm, reducing the size of the particulate material takes precedence over peeling. In addition, in a ball mill such as a planetary ball mill using beads and balls over 300 μm, reducing the size of the particulate material takes precedence over peeling. As a result, only a portion can be peeled off, and it becomes necessary to classify and collect a portion of the peeled MXene, and it is not possible to obtain an exfoliated MXene particulate material that can be used in industry. In particular, when a planetary ball mill is used, surface oxidation progresses, making it unsuitable for MXene, and in fact, it has not been considered. On the other hand, in the method of irradiating ultrasonic waves to a solvent, which has been used conventionally as a method of peeling MXene, cavitation occurs when ultrasonic waves are irradiated to the solvent, and the peeling of the layers that make up the layered compound progresses through a mechanism in which the powders collide with each other due to the crushing. However, even when water, which is prone to cavitation, was used, only a small portion of the MXene nanosheets were peeled off. The nanosheets were produced by a method in which only a portion of the MXene nanosheets was extracted by classification using centrifugation, which was not at a level suitable for industrial use.
[0029] The peripheral speed in the peeling step can be 6 m / sec to 12 m / sec. A peripheral speed of 8 m / sec to 10 m / sec is preferable. A peripheral speed of 6 m / sec or more provides good peeling efficiency, while a peripheral speed of 12 m / sec or less suppresses the application of excessive energy and suppresses the temperature rise of the obtained particulate material, thereby suppressing the progress of oxidation on the surface of the obtained particulate material and reducing electrical resistance. A slurry feed rate of 100 mL / min to 300 mL / min can be used. A slurry particle concentration of 20.0 mg / mL to 10.0 mg / mL can be used. A concentration of 17.0 mg / mL to 10.0 mg / mL is more preferable. A concentration of 15.0 mg / mL to 10.0 mg / mL is even more preferable.
[0030] A concentration of 20.0 mg / mL or less is preferable because it allows sufficient exfoliation and reduces the need to select flaky particulate material by classification using centrifugation, etc. Furthermore, it makes it possible to keep the particle size of the slurry small. A concentration of 10.0 mg / mL or more improves the efficiency of exfoliation.
[0031] The slurry temperature is preferably in the range of 35° C. or less. If the temperature is 35° C. or less, surface oxidation can be suppressed and the electrical resistance of the particulate material can be kept low.
[0032] The bead filling amount can be 40% to 80% by volume. If it is 40% by volume or more, the peeling efficiency improves, and if it is 80% by volume or less, it becomes easy to classify the beads and the slurry. Whether or not the particulate material containing a large amount of the desired flaky particles has been produced can be determined by observation with SEM, TEM, etc. In particular, the thickness of the particulate material can be determined by AFM analysis. The particulate material obtained in the peeling process can be classified by a method such as centrifugation if necessary and used. The optimal conditions for the peeling process vary depending on the size of the device, so these numerical values are not limited.
[0033] It is preferable that all of the MXene is exfoliated by bead mill treatment. If the exfoliation process is completed under conditions where all of the MXene is exfoliated, it becomes possible to use the MXene as is without removing the unexfoliated MXene. To remove MXene other than the exfoliated MXene, it can be separated by centrifugation, filtration, etc.
[0034] MXene in which some of the carbon sites are replaced with nitrogen is more susceptible to adsorption of OH groups in water, weakening the interlayer bonding strength. Therefore, by changing the amount of nitrogen substituted, the thickness and size of the resulting MXene can be controlled. a (C x N 1-x)2, by making x=0.97 to 0.70 and a exceeding 0.02, a thin and large nanosheet can be obtained. It is more preferable that x is 0.85 to 0.70. It is even more preferable that x is 0.80 to 0.70. In either case, a exceeds 0.02.
[0035] The raw material used in the pretreatment process is Ti3Al a (C x N 1-x )2, x=0.97-0.70, and a=1.00. Furthermore, the amount of Al to be removed is adjusted so that the amount of Al (corresponding to x) remaining in the MAX phase ceramic powder produced by acid treatment with an acidic substance exceeds 0.02. It is also possible to remove all of the Al, and in that case, it is preferable not to proceed with the acid treatment beyond the removal of the Al.
[0036] The amount of Al removed can be adjusted by changing the contact time with the acidic substance (such as an acid aqueous solution) (the longer the contact time, the greater the amount removed), the concentration of the acidic substance (the higher the concentration, the greater the amount removed), the amount of acidic substance (the greater the absolute amount of acidic substance, the greater the amount that can be removed), and the contact temperature (the higher the temperature, the greater the amount removed).
[0037] A layered compound MAX phase ceramic powder (A element is Al) is subjected to an acid treatment to remove part of the Al, resulting in a layered compound having a void layer that constitutes a particle material. An acidic substance that is a combination of hydrofluoric acid and hydrochloric acid is used as the acid for removing part of the Al layer. In order to realize the combination of hydrofluoric acid and hydrochloric acid, it is preferable to mix a salt of hydrofluoric acid (KF, LiF, etc.) with hydrochloric acid to obtain a mixture of hydrofluoric acid and hydrochloric acid.
[0038] In particular, aqueous solutions of these acids are used as the acidic substances. There is no particular limitation on the mixed concentration of hydrofluoric acid and hydrochloric acid formed when the fluoride salt is assumed to be completely dissociated. The lower limit of the hydrofluoric acid concentration can be about 1.7 mol / L, 2.0 mol / L, or 2.3 mol / L, and the upper limit can be about 2.5 mol / L, 2.6 mol / L, or 2.7 mol / L. The lower limit of the hydrochloric acid concentration can be about 2.0 mol / L, 3.0 mol / L, or 4.0 mol / L, and the upper limit can be about 13.0 mol / L, 14.0 mol / L, or 15.0 mol / L.
[0039] The mixing ratio (molar ratio) of hydrofluoric acid and hydrochloric acid formed when the fluoride salt is assumed to be completely dissociated is not particularly limited, but the lower limit of hydrofluoric acid may be 1:13, 1:12, or 1:11, and the upper limit may be about 1:5, 1:6, or 1:7. The concentrations and mixing ratios of hydrofluoric acid and hydrochloric acid shown here may be arbitrarily combined. The acid treatment temperature is preferably 10°C to 30°C. More preferably, it is 10°C to 20°C.
[0040] The zeta potential of the obtained MXene nanosheet particle material was measured in water at pH 6 to pH 8. Ti3Al a (C x N 1-x )2, the values were -29.0mV at X=0.97, -31.5mV at X=0.95, -32.1mV at X=0.90, -32.4mV at X=0.85, -33.1mV at X=0.75, and -34.0mV at X=0.70. On the other hand, the values were -28.9mV at X=1.00 and -34.5mV at X=0.65. The zeta potentials in water at pH 6 to 8 were all negative, and hydrophilic functional groups such as OH and halogens were adsorbed by acid treatment in water and by treatment with a micro-sized bead mill in water, and a larger absolute value of the zeta potential means that more hydrophilic functional groups were adsorbed. If the absolute value of the zeta potential becomes too large, the material will be crushed into pieces by the applied physical force. It was found that thin and large MXene nanosheets could be formed by increasing the absolute value of the zeta potential from 29.0 to 34.0.
[0041] The chemical composition of the MXene nanosheets was calculated using the atom % of Ti, Al, C, and N, assuming Ti to be 3, to calculate the amount of Al, C, and N. For chemical analysis, the sample was weighed onto a platinum dish, nitric acid + sulfuric acid + hydrofluoric acid were added, and the sample was dissolved by heating (to about 120°C), and then heated at a higher temperature (300°C) to evaporate the nitric acid and hydrofluoric acid to prepare a sample solution (sulfuric acid), which was then appropriately diluted and quantitatively analyzed by ICP. (dispersion) The dispersion of this embodiment is a dispersion of the particulate material of this embodiment in a dispersion medium. The particulate material dispersed in the dispersion is MXene, which is easily oxidized and cannot normally exist stably, but in this embodiment, it can exist stably for a long period of time. This makes it possible to store the MXene in the form of a dispersion for a long period of time, making it possible to dramatically expand the application fields of MXene. By applying this dispersion to an appropriate substrate and drying it, it becomes possible to form a conductive thin film and an electromagnetic wave shielding thin film made of MXene on the substrate. It can also be applied to other cases where MXene is used.
[0042] The dispersion medium contains 50% by mass or more of dimethyl sulfoxide, and the lower limit of the content is 60%, 70%, 80%, 90%, 95%, or 100% by mass. The higher the content of dimethyl sulfoxide, the more preferable it is. In particular, it is preferable that no dispersion medium other than dimethyl sulfoxide is contained. The composition of the dispersion medium that can contain other than dimethyl sulfoxide is not particularly limited, but it is preferable that it contains a hydrophilic material. For example, ethanol and isopropyl alcohol can be contained. The content of dimethyl sulfoxide can be 50% by mass or more, preferably 80% by mass or more, or 90% by mass or more, based on the mass of the entire dispersion medium. It is more preferable that it is 100% by mass. For example, water can be not contained. The content of water can be 5% by mass or less, preferably 2% by mass or less, or 1% by mass or less, based on the mass of the entire dispersion medium. When water coexists, the surface oxidation of the MXene nanosheet particle material progresses and the conductivity deteriorates. The concentration of the particle material in the dispersion liquid of this embodiment is 0.1% by mass to 0.4% by mass. EXAMPLES
[0043] The particulate material, the method for producing the same, and the dispersion of the present invention will be described in detail below with reference to examples. Example 1 Pre-treatment process 11.7 g of TiC powder (TI-30-10-0020, Rare Metallic Co., Ltd.), 0.6 g of TiN powder (TN-30-10-0020, Rare Metallic Co., Ltd.), 4.9 g of Ti powder (TIE07PB 3N, Kojundo Chemical Co., Ltd.), and 2.8 g of Al powder (ALE15PB 3NG, Kojundo Chemical Co., Ltd.) were mixed in isopropanol (IPA) using a ball mill for 12 hours, and the IPA was removed using an evaporator to obtain a uniformly mixed dry powder.
[0044] The uniformly mixed dry powder was placed in an alumina crucible and sintered in an Ar gas flow at 1450°C for 2 h (heating rate: 10°C / min) using a graphite resistance furnace to obtain Ti3Al(C) as a MAX phase ceramic. 0.95 N 0.05)2 was obtained. The obtained Ti3Al(C 0.95 N 0.05 After coarsely pulverizing Ti3Al(C)2 using a mortar and pestle, it was ground in IPA using a ball mill with 5 mm zirconia balls for 24 hours. Then, it was ground in a planetary ball mill with 0.5 mm zirconia balls (200 rpm, 15 min, 3 times) to obtain a suspension. The IPA was removed from the suspension using an evaporator, and Ti3Al(C)2 ground to about 3 μm was obtained. 0.95 N 0.05 ) 2 powder was obtained.
[0045] Prepare an acid solution by adding 18 g of LiF to 300 mL of concentrated HCl. While cooling with ice, add 10 g of Ti3Al(C 0.95 N 0.05 )2 powder was added to the mixture and stirred with a magnetic stirrer for 24 hours in a controlled environment of 20 to 30°C. This etched and removed the Al, leaving Ti3Al0.02(C 0.95 N 0.05 ) A particulate material consisting of 2MXene was obtained. After etching, the material was washed with water until the pH reached about 6, and finally the water was replaced with ethanol. This procedure resulted in the particulate material being a suspension of MXene suspended in ethanol.
[0046] The particle concentration in the raw suspension was measured, and water was added so that the particle concentration of MXene became 15.0 mg / mL, thereby obtaining MXene dispersed in water as a dispersion medium (raw suspension). Peeling process This raw material suspension was treated with a bead mill with ZrO2 beads of 50μm diameter at a slurry feed rate of 150mL / min and a ZrO2 bead loading of 80% to produce exfoliated material made of MXene. By repeating this treatment three times, the particulate material made of MXene contained in the raw material suspension was almost entirely converted into exfoliated material, and an exfoliated material suspension containing the exfoliated material was obtained.
[0047] The obtained suspension of exfoliated material was dropped onto a Si substrate that had been piranha-treated (immersed in a mixed solution of H2SO4:H2O2 = 3 parts by volume:1 part by volume), and an AFM analysis was performed. The AFM image is shown in Figure 1. One hundred exfoliated materials (nanosheets) were randomly selected, and the average thickness measured by AFM was calculated and shown in Table 1. Furthermore, the results of SEM observation are shown in Figure 2. One hundred exfoliated materials were randomly selected, and the vertical (maximum diameter in the direction perpendicular to the thickness direction) and horizontal (directions perpendicular to the vertical and thickness directions) dimensions were measured from the SEM photograph, and the average value was defined as the size of the exfoliated material. The average size of the 100 exfoliated materials is shown in Table 1.
[0048] Ti3Al(C) used in the pretreatment process 0.95 N 0.05 Powder A in 2) and the exfoliated product (MXene nanosheet) were subjected to XRD measurement, and the results are shown in Figure 3. The interlayer distance of the (002) plane from each XRD profile is shown in Table 2.
[0049] The suspension of the exfoliated material (15.0 mg / ml) was centrifuged at 37000G (17000 rpm) for 30 minutes, the supernatant was discarded, and 5.0 g of dimethyl sulfoxide (DMSO) was added per 1.25 g of sediment, and the mixture was suspended by stirring at 140 rpm and amplitude 45 mm for 1.5 hours in a shaker. These operations were repeated three times to replace the entire dispersion medium with DMSO, and a DMSO suspension was obtained.
[0050] The obtained DMSO suspension was centrifuged at 2400G (3500rpm) and the supernatant was collected (the supernatant was named DMSO colloids). One drop of ethanol was dropped onto two drops of DMSO colloids to prepare a spin coat sample. A piranha-treated glass plate (25 x 25 x 0.7mm) was used as a substrate, and 20μL of ethanol was dropped onto the substrate and spin-coated at 4000rpm for 1 minute to produce a film.
[0051] When repeating thin film production by spin coating to control film thickness, after air drying, film production by spin coating was repeated in the same manner until the required film thickness was reached. The results of UV-vis measurement are shown in Figure 4. After vacuum drying at 200℃ for 24 hours, the surface electrical resistance was measured and the results are shown in Table 3. Example 2 The peeled product was prepared in the same manner as in Example 1, except that 9.2 g of TiC powder (TI-30-10-0020, Rare Metallic Co., Ltd.), 3.2 g of TiN powder (TN-30-10-0020, Rare Metallic Co., Ltd.), 4.9 g of Ti powder (TIE07PB 3N, Kojundo Chemical Co., Ltd.), and 2.8 g of Al powder (ALE15PB 3NG, Kojundo Chemical Co., Ltd.) were used as starting materials. Figure 1 shows an AFM image, Table 1 shows the average thickness and average size, Table 2 shows the interlayer distance, Figure 2 shows an SEM image, and Figure 3 shows the obtained Ti3Al(C 0.75 N 0.25 )2 powder, Ti3Al 0.02 (C 0.75 N 0.25 ) The XRD profile of 2MXene is shown in Figure 4, the UV-vis results are shown in Figure 4, and the surface electrical resistivity values are shown in Table 3. Comparative Example 1 The Ti3Al powder was prepared as a peeled product in the same manner as in Example 1, except that 12.3 g of TiC powder (TI-30-10-0020, Rare Metallic Co., Ltd.), 4.9 g of Ti powder (TIE07PB 3N, Kojundo Chemical Co., Ltd.), and 2.8 g of Al powder (ALE15PB 3NG, Kojundo Chemical Co., Ltd.) were used as starting materials. 0.02 C2MXene nanosheets were prepared. Figure 1 shows the AFM image, Table 1 shows the average thickness and average size, Table 2 shows the interlayer distance, Figure 2 shows the SEM image, and Figure 3 shows the obtained Ti3AlC2 powder and Ti3Al 0.02 The XRD profile of C2MXene and the surface electrical resistivity are shown in Table 3. Comparative Example 2 The Ti3Al powder was prepared as a peeled product in the same manner as in Example 1, except that 4.4 g of TiC powder (TI-30-10-0020, Rare Metallic Co., Ltd.), 4.6 g of TiN powder (TN-30-10-0020, Rare Metallic Co., Ltd.), 7.1 g of Ti powder (TIE07PB 3N, Kojundo Chemical Co., Ltd.), and 4.0 g of Al powder (ALE15PB 3NG, Kojundo Chemical Co., Ltd.) were used as starting materials. 0.02 (C 0.5 N 0.5)2MXene nanosheets were prepared. Figure 2 shows the SEM image, and Figure 3 shows the obtained Ti3Al(C 0.5 N 0.5 )2 powder, Ti3Al 0.02 (C 0.5 N 0.5 )XRD profile of 2MXene. Comparative Example 3 TiC powder (TI-30-10-0020, Rare Metallic Co., Ltd.) 12.3 g, Ti powder (TIE07PB 3N, Kojundo Chemical Co., Ltd.) 4.9 g, and Al powder (ALE15PB 3NG, Kojundo Chemical Co., Ltd.) 2.8 g were used as starting materials to prepare Ti3AlC2 powder in the same manner as in Comparative Example 2. Except for using ethanol as a dispersion medium during the peeling process, Ti3AlC2 powder was prepared as the peeled product in the same manner as in Comparative Example 2. 0.02 C2MXene nanosheets were prepared. Figure 1 shows the AFM image, Table 1 shows the average thickness and average size, Table 2 shows the interlayer distance, Figure 2 shows the SEM image, and Figure 3 shows the obtained Ti3AlC2 powder and Ti3Al 0.02 The XRD profile of C2MXene is shown.
[0052] [Table 1]
[0053] In Comparative Example 2, the particles were not crushed into a sheet, and the average thickness and average size of the sheet could not be measured.
[0054] [Table 2]
[0055] [Table 3]
[0056] (result) It was found that Examples 1 and 2, in which x is in the range of 0.97 to 0.7, have a thinner average thickness and a larger average size than Comparative Examples 1 and 3, in which x is 1. In Comparative Example 2, in which x is 0.5, pulverization proceeded in the peeling process, and only fine particles were generated. It is preferable to replace a part of the C site with N, since it makes it easier for hydrophilic functional groups to be adsorbed, weakens the bonding strength between layers, and makes peeling easier, but if it is replaced with too much N, the bonding strength between layers is weakened, and pulverization proceeds easily and remarkably at the same time as peeling, resulting in fine powder. It was also found that Examples 1 and 2 have better light transmittance than Comparative Example 1.
[0057] In Comparative Example 3, in which the dispersion medium used in the peeling step was only ethanol, the average thickness was large and the average size was small, and the peeling could not be performed sufficiently. Furthermore, the interlayer distance of the (002) plane was also small. Thus, it was found that the use of a dispersion medium containing water is preferable to the use of a dispersion medium not containing water in the peeling step when peeling by a method using a bead mill using fine beads in order to obtain thin and large nanosheets.
[0058] MXene was exfoliated by ultrasonic irradiation, and some of the exfoliated MXene nanosheets were obtained by centrifugation, but this was not at a level suitable for industrial use. When ultrasonic waves are applied to a solvent, cavitation occurs, and the resulting collapse causes the powder particles to collide with each other, which causes the layers that make up the layered compound to peel off. However, even when water, which is prone to cavitation, is used, only some of the layers peel off. Furthermore, when using a planetary ball mill, grinding takes precedence over exfoliation, and surface oxidation progresses, so MXene has not been considered. When some of the carbon sites of MXene are replaced with nitrogen, the hydrophilic functional groups are more strongly adsorbed, weakening the interlayer bonding strength, and by selectively applying a physical force between the MXene layers in a bead mill using microbeads, we have succeeded in obtaining MXene nanosheets with a thin average thickness and a large average size without the need for classification by centrifugation. It can be said that MXene nanosheets have reached a level where they can be used industrially.
[0059] In the peeling process, by setting the MXene particle concentration to 10 mg / mL or higher, the efficiency of the peeling process was increased, and by setting it to 20 mg / mL or lower, the amount of unpeeled MXene remaining was suppressed, making it easier to turn the MXene into peeled material.
[0060] Using water in the peeling process enabled the production of peeled products with small average thickness, but degradation of MXene due to oxidation was observed when left as is. However, it was revealed that oxidation could be suppressed by replacing the dispersion medium with DMSO as in the examples. Furthermore, it was found that aggregation could be effectively suppressed by keeping the concentration in the dispersion liquid at 0.4 mass% or less.
Claims
1. Ti having an average thickness of 1.0 to 3.5 nm, an average size of 1.5 to 2.0 μm, and an interlayer distance of the (002) plane of 1.350 nm to 1.400 nm. 3 Al a (C x N 1-x ) 2 A particulate material having MXene nanosheets composed of x=0.97-0.70 and a>0.
02.
2. 2. The particulate material according to claim 1, which has a zeta potential in water at pH 6 to pH 8 in the range of -29.0 mV to -34.0 mV.
3. A particulate material according to claim 1 or 2; a dispersion medium in which the particulate material is dispersed at 0.1% by mass to 0.4% by mass and which contains 50% by mass or more of dimethyl sulfoxide; A dispersion having
4. A method for producing a particulate material consisting of MXene nanosheets, comprising a peeling step in which a mixture of a dispersion medium containing 50 mass% or more of water and MXene dispersed in the dispersion medium at a particle concentration of 10 mg / mL to 20 mg / mL is treated in a bead mill using beads of 10 μm to 300 μm to peel off the MXene and form an exfoliated product.
5. The method for producing a particulate material according to claim 4, further comprising the steps of: a step of replacing the water contained after the peeling step with dimethyl sulfoxide to obtain a dispersion liquid in which the particulate material is dispersed in dimethyl sulfoxide; A method for producing a dispersion having the formula:
Citation Information
Patent Citations
Electrode material including layer compound
JP2016063171A
Method for manufacturing electrode material for electrochemical capacitor including layer compound
JP2017076739A
MXene particle material, slurry, secondary battery, transparent electrode, and method for manufacturing MXene particle material
JP6564552B1
MXene particulate materials, methods for producing these particulate materials, and secondary batteries
JP6564553B1
Compositions comprising free-standing two-dimensional nanocrystals
US20140162130A1
Cited By
Preparation method of lithium ion battery negative electrode material
CN116375032A