Negative electrode active material, and electrochemical device and electronic device using the same
By optimizing negative electrode active materials with specific parameters, the cycle characteristics of lithium-ion batteries are improved, achieving high capacity and reduced thickness expansion, addressing the challenges faced in existing technologies.
Patent Information
- Application Number
- JP2022552970
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-20
- Filing Date
- 2021-02-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-02-09
AI Technical Summary
Lithium-ion batteries face challenges in cycle characteristics, particularly in medium- and large-sized batteries used for electric vehicles and energy storage systems, due to issues with the active materials in the electrodes.
The development of negative electrode active materials with specific parameters such as median diameter, specific surface area, and crystallite size, along with controlled carbon-to-oxygen ratios and porosity, enhances the strength and stability of the electrodes, reducing particle crushing and SEI film formation.
This approach improves the balance between high capacity and low cycle thickness expansion, resulting in enhanced performance and efficiency of lithium-ion batteries.
Smart Images

Figure 0007579873000004 
Figure 0007579873000001 
Figure 0007579873000002
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of energy storage, and more particularly to anode active materials and electrochemical and electronic devices using the same. [Background technology]
[0002] Electrochemical devices (e.g., lithium-ion batteries) are widely used due to their environmental friendliness, high operating voltage, large specific capacity, long cycle life, etc., and are the most promising new green chemical power source in the world today. Small lithium-ion batteries are usually used as power sources for portable electronic communication devices (e.g., camcorders, mobile phones, or laptops), especially for high-performance portable devices. In recent years, medium- and large-sized lithium-ion batteries with high output characteristics have been developed for application in electric vehicles (EVs) and large-scale energy storage systems (ESSs). With the widespread use of lithium-ion batteries, their cycle characteristics have become a technical problem that needs to be solved urgently. Improving the active material in the electrodes is one of the research directions to solve the above problems.
[0003] In view of this situation, there is a need to provide improved negative electrode active materials, and electrochemical and electronic devices using same. Summary of the Invention
[0004] SUMMARY OF THE DISCLOSURE The present invention solves, at least in part, at least one problem in the related art by providing negative electrode active materials and electrochemical and electronic devices using same.
[0005] According to one aspect of the present invention, the median diameter is D 1 v50, and the median diameter at a pressure of 1t is D 2 When v50 is used, D 2 v50 / D 1 In some embodiments, the negative electrode active material has a v50 of 0.8 or more.2 v50 / D 1 In some embodiments, the negative electrode active material has a D v50 of 0.9 or more. 2 v50 / D 1 v50 is 0.8, 0.85, 0.9, 0.95 or 1.0.
[0006] According to an embodiment of the present invention, the specific surface area of the negative electrode active material is determined by BET 1 The specific surface area of the negative electrode active material at a pressure of 1 t is calculated by BET 2 When the above BET 1 is 0.6m 2 / g~2.0m 2 / g, (BET 2 -BET 1 ) / BET 1 In some embodiments, the BET 1 is 0.7m 2 / g~1.8m 2 / g. In some embodiments, the BET 1 is 0.8m 2 / g~1.6m 2 / g. In some embodiments, the BET 1 is 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.7m 2 / g, 1.8m 2 / g, 1.9m 2 / g or 2.0m 2 / g.
[0007] According to an embodiment of the present invention, the negative electrode active material includes graphite particles, and the graphite particles include: (a)D 1 v50 is 10μm~25μm, (b)D 1 v90 and D 1 v10 is D 1 v90 / D 1 v10<3.5 and (c) the graphite particles have a crystallite size La of 160 nm to 165 nm along the horizontal direction and a crystallite size Lc of 30 nm to 32 nm along the vertical direction, as determined by an X-ray diffraction method; At least one of the conditions is satisfied.
[0008] In some embodiments, the D of the graphite particles 1 In some embodiments, the D of the graphite particles is 15 μm to 20 μm. 1 v50 is 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, 22 μm or 25 μm.
[0009] In some embodiments, the D of the graphite particles 1 v90 / D 1 In some embodiments, the D of the graphite particles is less than 3.0. 1 v90 / D 1 In some embodiments, the D of the graphite particles is less than 2.5. 1 v90 / D 1 v10 is less than 2.0.
[0010] In some embodiments, the graphite particles have a crystallite size La along the horizontal direction of 160 nm, 161 nm, 162 nm, 163 nm, 164 nm, or 165 nm, and a crystallite size Lc along the vertical direction of the graphite particles is 30 nm, 31 nm, or 32 nm, as measured by X-ray diffraction.
[0011] According to another aspect of the invention, there is provided an electrochemical device comprising an anode comprising an anode current collector and an anode active material layer, said anode active material layer comprising the anode active material according to the invention.
[0012] According to an embodiment of the present invention, the negative electrode active material layer comprises: (d) the negative electrode active material layer contains carbon and oxygen, and the ratio of the carbon content to the oxygen content is 2:3 to 990:1; (e) a ratio C004 / C110 of a peak area C004 of a (004) plane of the negative electrode active material layer to a peak area C110 of a (110) plane thereof obtained by X-ray diffraction pattern measurement is 5.7 to 18; (f) the porosity of the negative electrode active material layer is 20% to 30%; At least one of the conditions is satisfied.
[0013] In some embodiments, the ratio of the carbon content to the oxygen content is 1:1 to 800:1. In some embodiments, the ratio of the carbon content to the oxygen content is 5:1 to 500:1. In some embodiments, the ratio of the carbon content to the oxygen content is 10:1 to 300:1. In some embodiments, the ratio of the carbon content to the oxygen content is 50:1 to 100:1. In some embodiments, the ratio of the carbon content to the oxygen content is 2:3, 1:1, 5:1, 10:1, 20:1, 50:1, 100:1, 200:1, 300:1, 400:1, 500:1, 600:1, 700:1, 800:1, 900:1, or 990:1.
[0014] In some embodiments, the negative electrode active material layer has a C004 / C110 of 6.0 to 10.0, or the negative electrode active material layer has a C004 / C110 of 7.0 to 8.0.
[0015] In some embodiments, the porosity of the negative electrode active material layer is 20% to 25%. In some embodiments, the porosity of the negative electrode active material layer is 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, or 30%.
[0016] According to an embodiment of the present invention, in the electrochemical device in a fully discharged state, the ratio C004' / C110' of the peak area C004' of the (004) plane of the negative electrode active material layer to the peak area C110' of the (110) plane of the negative electrode active material layer obtained by X-ray diffraction pattern measurement is 6.8 to 17.2. In some embodiments, C004' / C110' of the negative electrode active material layer is 7.0 to 16.6. In some embodiments, C004' / C110' of the negative electrode active material layer is 10.0 to 16.0. In some embodiments, C004' / C110' of the negative electrode active material layer is 11.0 to 15.5.
[0017] According to an embodiment of the present invention, in the electrochemical device in a fully discharged state, the median diameter of the negative electrode active material is D a v50, and the median diameter of the negative electrode active material at a pressure of 1 t is D b When v50 is used, D b v50 / D a In some embodiments, the negative electrode active material has a D v50 of 0.9 or more. b v50 / D a In some embodiments, the negative electrode active material has a D v50 of 0.91 or more. b v50 / D a v50 is 0.92, 0.95, 0.98 or 1.0.
[0018] According to an embodiment of the present invention, in the electrochemical device in a fully discharged state, the median diameter D a In some embodiments, the D of the negative electrode active material is 8 μm to 20 μm. a In some embodiments, the D of the negative electrode active material is 10 μm to 15 μm. a v50 is 8 μm, 10 μm, 12 μm, 15 μm, 18 μm or 20 μm.
[0019] According to an embodiment of the present invention, in the electrochemical device in a fully discharged state, the specific surface area of the negative electrode active material is a The specific surface area of the negative electrode active material at a pressure of 1 t is calculated by BET bThen, (BET b -BET a ) / BET a <0.6.
[0020] According to a further aspect of the present invention, there is provided an electronic device comprising an electrochemical device as described herein.
[0021] Other aspects and advantages of the invention are set forth in part in the description that follows, are illustrated in part, or may be learned through the practice of embodiments of the invention. [Brief description of the drawings]
[0022] In the following, in order to explain the embodiments of the present invention, the necessary drawings for explaining the embodiments of the present invention or the prior art will be briefly described. Obviously, the drawings described below are only a part of the embodiments of the present invention. Those skilled in the art can still obtain drawings of other embodiments according to the results illustrated in these drawings without making creative efforts. [Figure 1] FIG. 1 is a diagram showing the expansion rate of the lithium ion batteries according to Example 22 of the present invention and Comparative Example 1 at 45° C. as a function of the number of cycles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] The embodiments of the present invention will be described in detail below. The embodiments described in the present invention and the drawings are exemplary and schematic, and are used to generally understand the present invention. The embodiments of the present invention should not be construed as limiting the present invention.
[0024] In specific embodiments and claims, a list of terms connected by the term "at least one of" means any combination of the listed terms. For example, if terms A and B are listed, "at least one of A and B" means A only, B only, or A and B. In other examples, if terms A, B, and C are listed, "at least one of A, B, and C" means A only, or B only, or C only, or A and B (excluding C), or A and C (excluding B), or B and C (excluding A), or all of A, B, and C. Term A may include a single element or multiple elements. Term B may include a single element or multiple elements. Term C may include a single element or multiple elements.
[0025] As used in this specification, "Dv50" refers to the particle size at which the cumulative volume from the small diameter side is 50% in the volume-based particle size distribution of the negative electrode active material. In other words, the volume of the negative electrode active material smaller than this particle size accounts for 50% of the total volume of the negative electrode active material.
[0026] As used in this specification, "Dv10" refers to the particle size at which the cumulative volume from the small diameter side in the volume-based particle size distribution of the negative electrode active material is 10%. In other words, the volume of the negative electrode active material smaller than this particle size occupies 10% of the total volume of the negative electrode active material.
[0027] As used in this specification, "Dv90" refers to the particle size at which the cumulative volume from the small diameter side is 90% in the volume-based particle size distribution of the negative electrode active material. In other words, the volume of the negative electrode active material smaller than this particle size accounts for 90% of the total volume of the negative electrode active material.
[0028] The Dv50, Dv10 and Dv90 of the negative electrode active material can be measured by a method known in the art, for example, by a laser particle size analyzer (for example, a Malvern particle size analyzer).
[0029] As used in this specification, the term "fully discharged state" refers to a state in which the electrochemical device is discharged in an environment of 25°C using a constant current method at a discharge current of 1C (i.e., a current value that completely discharges the theoretical capacity within one hour) to a voltage of 3.0V.
[0030] The electrochemical devices of the present invention are at a 50% state of charge (SOC) unless otherwise specified.
[0031] During the cycling process of an electrochemical device (hereinafter, taking a lithium ion battery as an example), the electrochemical device expands due to the insertion of lithium ions, and this phenomenon is particularly serious at high temperatures. Increasing the degree of composite of the negative electrode active material (e.g., graphite particles) is one of the means to improve the cycling characteristics of a lithium ion battery. The primary particles of the negative electrode active material can be composited to form secondary particles by using a binder with high viscosity or increasing the amount of binder. The present invention achieves a balance between high capacity and thickness expansion during the cycling process of a lithium ion battery by improving the strength of the secondary particles.
[0032] Specifically, the present invention defines a median diameter D 1 v50, and the median diameter at a pressure of 1t is D 2 When v50 is used, D 2 v50 / D 1 In some embodiments, the negative electrode active material has a v50 of 0.8 or more. 2 v50 / D 1 In some embodiments, the negative electrode active material has a D v50 of 0.9 or more. 2 v50 / D 1 v50 is 0.8, 0.85, 0.9, 0.95 or 1.0. 2 v50 / D 1 The v50 can indicate the particle size change rate of the pressed negative electrode active material particles. 2 v50 / D 1The larger the v50, the smaller the degree of particle crushing of the pressed negative electrode active material, the fewer the number of crushed particles, the lower the ratio of crushed particles to the total particles of the negative electrode active material (i.e., the particle crushing rate), and the higher the strength of the negative electrode active material. This reduces the cross section of the negative electrode active material that is not coated with the binder caused by pressing, which can reduce the formation of a solid electrolyte interface (SEI) film and help improve the capacity, initial efficiency, and cycle thickness expansion rate of lithium ion batteries. D of the negative electrode active material 2 v50 / D 1 When the v50 is within the above range, the negative electrode active material has high strength and can help achieve a balance between high capacity per gram and low cycle thickness expansion rate in lithium ion batteries.
[0033] The negative electrode active material of the present invention can be obtained by adding a high-viscosity additive to primary particles of a negative electrode active material to obtain a mixture, and then calcining the mixture to obtain secondary particles of the negative electrode active material, wherein the high-viscosity additive includes at least one of an oil-based high-temperature pitch, a coal-based high-temperature pitch, and a resin polymer material, and the content of the high-viscosity additive is 30 wt% or less based on the total weight of the negative electrode active material.
[0034] According to an embodiment of the present invention, the median diameter D 1 In some embodiments, the D of the negative electrode active material is 10 μm to 25 μm. 1 In some embodiments, the D of the negative electrode active material is 15 μm to 20 μm. 1 v50 is 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, 22 μm or 25 μm.
[0035] According to an embodiment of the present invention, the median diameter D of the negative electrode active material at a pressure of 1t 2 In some embodiments, the D of the negative electrode active material is 8 μm to 20 μm. 2 In some embodiments, the D of the negative electrode active material is 10 μm to 15 μm.2 v50 is 8 μm, 10 μm, 12 μm, 15 μm, 18 μm or 20 μm.
[0036] According to an embodiment of the present invention, the negative electrode active material D 1 v90 and D 1 v10 is D 1 v90 / D 1 In some embodiments, the negative electrode active material has a D of less than 3.5. 1 v90 / D 1 In some embodiments, the D of the negative electrode active material is less than 3.0. 1 v90 / D 1 In some embodiments, the D of the negative electrode active material is less than 2.5. 1 v90 / D 1 v10 is less than 2.0.
[0037] According to an embodiment of the present invention, the negative electrode active material includes crystallites, and the crystallite size La along the horizontal direction of the crystallite is 160 nm to 165 nm, and the crystallite size Lc along the vertical direction of the crystallite is 30 nm to 32 nm, according to an X-ray diffraction method. In some embodiments, the negative electrode active material includes crystallites, and the crystallite size La along the horizontal direction of the crystallite is 161 nm to 164 nm, and the crystallite size Lc along the vertical direction of the crystallite is 30.5 nm to 31.5 nm, according to an X-ray diffraction method. In some embodiments, the crystallite size La along the horizontal direction of the graphite particles is 160 nm, 161 nm, 162 nm, 163 nm, 164 nm, or 165 nm, and the crystallite size Lc along the vertical direction of the graphite particles is 30 nm, 31 nm, or 32 nm, according to an X-ray diffraction method.
[0038] According to an embodiment of the present invention, the negative electrode active material includes graphite particles, and the graphite particles have the same D as the negative electrode active material. 1 v50, D 2 v50, D 1 v90 and D 1 In some embodiments, the negative electrode active material is graphite particles.
[0039] According to an embodiment of the present invention, the specific surface area of the negative electrode active material is determined by BET 1 The specific surface area of the negative electrode active material at a pressure of 1 t is calculated by BET 2 When the above BET 1 is 0.6m 2 / g~2.0m 2 / g, (BET 2 -BET 1 ) / BET 1 ≦1. The negative electrode active material is (BET 2 -BET 1 ) / BET 1 When the ratio satisfies ≦1, the increase in the specific surface area of the pressed negative electrode active material is 100% or less compared to the non-pressed negative electrode active material. The smaller the increase in the specific surface area of the negative electrode active material, the higher the strength of the negative electrode active material, the smaller the cross section of the negative electrode active material that is not coated with the binder caused by pressing, and the smaller the solid electrolyte interface (SEI) film formed. This can help improve the capacity, initial efficiency, and cycle thickness expansion rate of lithium ion batteries.
[0040] In some embodiments, the BET 1 is 0.7m 2 / g~1.8m 2 / g. In some embodiments, the BET 1 is 0.8m 2 / g~1.6m 2 / g. In some embodiments, the BET 1 is 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.7m 2 / g, 1.8m2 / g, 1.9m 2 / g or 2.0m 2 / g.
[0041] According to an embodiment of the present invention, the specific surface area BET 2 is 1.2m 2 / g~4.0m 2 In some embodiments, the BET 2 is 1.5m 2 / g~3.0m 2 In some embodiments, the BET 2 is 1.2m 2 / g, 1.5m 2 / g, 2m 2 / g, 2.5m 2 / g, 3m 2 / g, 3.5m 2 / g or 4.0m 2 / g.
[0042] The parameters of the negative electrode active material at a pressure of 1 t can be obtained by referring to the steps of the national standard GB / T24533-2009 of the People's Republic of China.
[0043] The specific surface area of the negative electrode active material can be obtained by the following method. Using a specific surface area analyzer (e.g., Tristar II 3020M), the specific surface area of the negative electrode active material is measured by a nitrogen adsorption / desorption method in which a sample of the negative electrode active material is dried in a vacuum drying oven, placed in a sample tube, and measured with the analyzer.
[0044] The present invention further provides an electrochemical device including a negative electrode comprising a negative electrode current collector and a negative electrode active material layer.
[0045] negative electrode In the electrochemical device of the present invention, the negative electrode active material layer contains the negative electrode active material according to the present invention.
[0046] According to an embodiment of the present invention, the negative electrode active material layer includes carbon and oxygen, and the ratio of the carbon content to the oxygen content is 2:3 to 990:1. In some embodiments, the ratio of the carbon content to the oxygen content is 1:1 to 800:1. In some embodiments, the ratio of the carbon content to the oxygen content is 5:1 to 500:1. In some embodiments, the ratio of the carbon content to the oxygen content is 10:1 to 300:1. In some embodiments, the ratio of the carbon content to the oxygen content is 50:1 to 100:1. In some embodiments, the ratio of the carbon content to the oxygen content is 2:3, 1:1, 5:1, 10:1, 20:1, 50:1, 100:1, 200:1, 300:1, 400:1, 500:1, 600:1, 700:1, 800:1, 900:1, or 990:1. When the ratio of the carbon content to the oxygen content in the negative electrode active material layer is within the above range, the particle size and graphitization degree of the negative electrode active material particles are within an appropriate range, which can help improve the capacity and cycle thickness expansion rate of the lithium ion battery.
[0047] According to an embodiment of the present invention, in the negative electrode active material layer, the ratio C004 / C110 of the peak area C004 of the (004) plane of the negative electrode active material layer to the peak area C110 of the (110) plane of the negative electrode active material layer obtained by X-ray diffraction pattern measurement is 5.7 to 11.2. The value of C004 / C110 of the negative electrode active material layer obtained by X-ray diffraction pattern measurement may indicate the anisotropy of the negative electrode active material particles. The smaller the value of C004 / C110, the smaller the anisotropy, which can be useful for improving the cycle thickness expansion rate of a lithium ion battery. In some embodiments, C004 / C110 of the negative electrode active material layer is 6.0 to 10.0. In some embodiments, C004 / C110 of the negative electrode active material layer is 7.0 to 8.0.
[0048] According to an embodiment of the present invention, the porosity of the negative electrode active material layer is 20% to 30%. In some embodiments, the porosity of the negative electrode active material layer is 20% to 25%. In some embodiments, the porosity of the negative electrode active material layer is 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, or 30%.
[0049] According to the embodiment of the present invention, in the electrochemical device in a fully discharged state, the ratio C004' / C110' of the peak area C004' of the (004) plane of the negative electrode active material layer to the peak area C110' of the (110) plane of the negative electrode active material layer obtained by X-ray diffraction pattern measurement is 6.8 to 17.2. In some embodiments, C004' / C110' of the negative electrode active material layer is 7.0 to 16.5. In some embodiments, C004' / C110' of the negative electrode active material layer is 10.0 to 15.0. In some embodiments, C004' / C110' of the negative electrode active material layer is 12.0 to 14.0. When C004' / C110' of the negative electrode active material layer is within the above range, the anisotropy of the negative electrode active material particles in the electrochemical device in a fully discharged state is still relatively low, which may indicate that the negative electrode active material has high strength.
[0050] According to an embodiment of the present invention, in the electrochemical device in a fully discharged state, the median diameter of the negative electrode active material is D a v50, and the median diameter of the negative electrode active material at a pressure of 1 t is D b When v50 is used, D b v50 / D a The v50 is 0.9 or more. b v50 / D a v50 may indicate the degree of particle crushing of the pressed negative electrode active material in an electrochemical device in a fully discharged state. b v50 / D aThe larger the v50, the smaller the degree of particle crushing of the pressed negative electrode active material in the electrochemical device in a fully discharged state, the fewer the number of crushed particles, the lower the ratio of the crushed particles to the total particles of the negative electrode active material (i.e., the particle crushing rate), and the higher the strength of the negative electrode active material. b v50 / D a When the v50 is in the above range, the negative electrode active material in the electrochemical device in a fully discharged state still has high strength, which can further improve the initial efficiency of the lithium ion battery and help to reduce the cycle thickness expansion rate. In some embodiments, the D b v50 / D a v50 is 0.92, 0.95, 0.98 or 1.0.
[0051] According to an embodiment of the present invention, in the electrochemical device in a fully discharged state, the median diameter D a In some embodiments, the D of the negative electrode active material is 8 μm to 20 μm. a In some embodiments, the D of the negative electrode active material is 10 μm to 15 μm. a v50 is 8 μm, 10 μm, 12 μm, 15 μm, 18 μm or 20 μm.
[0052] According to an embodiment of the present invention, in the electrochemical device in a fully discharged state, the median diameter D b In some embodiments, the D of the negative electrode active material is 7.2 μm to 18 μm. b In some embodiments, the D of the negative electrode active material is 8 μm to 15 μm. b v50 is 7.2μm, 8μm, 10μm, 12μm, 15μm or 18μm.
[0053] According to an embodiment of the present invention, in the electrochemical device in a fully discharged state, the specific surface area of the negative electrode active material is a The specific surface area of the negative electrode active material at a pressure of 1 t is calculated by BET b Then, (BETb -BET a ) / BET a <0.6. b -BET a ) / BET a <0.6, the increase rate of the specific surface area of the pressed negative electrode active material is less than 60% compared with that of the non-pressed negative electrode active material. When the specific surface area of the negative electrode active material in the electrochemical device in a fully discharged state satisfies the above relationship, it can be shown that the strength of the negative electrode active material is relatively high.
[0054] According to an embodiment of the present invention, in the electrochemical device in a fully discharged state, the specific surface area BET a is 0.6m 2 / g~2.0m 2 In some embodiments, the specific surface area BET a is 0.8m 2 / g~1.5m 2 In some embodiments, the specific surface area BET a is 1.0m 2 / g~1.2m 2 In some embodiments, the specific surface area BET a is 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.7m 2 / g, 1.8m 2 / g, 1.9m 2 / g or 2.0m 2 / g.
[0055] According to an embodiment of the present invention, in the electrochemical device in a fully discharged state, the specific surface area BET b is 0.96m 2 / g~3.2m 2 In some embodiments, the BET b is 1.0m 2 / g~3.0m 2 In some embodiments, the BET b is 1.5m 2 / g~2.0m 2 In some embodiments, the BET b is 0.96m 2 / g, 1.0m 2 / g, 1.2m 2 / g, 1.5m 2 / g, 1.8m 2 / g, 2.0m 2 / g, 2.2m 2 / g, 2.5m 2 / g, 2.8m 2 / g, 3.0m 2 / g or 3.2m 2 / g.
[0056] According to an embodiment of the present invention, the negative electrode current collector used in the present invention may be selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, conductive metal coated polymer substrate, and combinations thereof.
[0057] According to an embodiment of the present invention, the negative electrode further comprises a conductive layer. In some embodiments, the conductive material of the conductive layer may comprise any conductive material as long as it does not cause a chemical change. Non-limiting examples of the conductive material include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, carbon nanotube, graphene, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., e.g., copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives), and mixtures thereof.
[0058] According to an embodiment of the present invention, the negative electrode further includes a binder, and the binder is at least one selected from polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, a polymer containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, poly(1,1-difluoroethylene), polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc.
[0059] According to embodiments of the present invention, the negative electrode can be manufactured by any method known in the prior art. In some embodiments, the negative electrode can be formed by adding an adhesive and a solvent to the negative electrode active material, and optionally adding a thickener, a conductive material, a filler, etc. to prepare a slurry, applying the slurry to a current collector, drying, and pressing.
[0060] According to an embodiment of the present invention, when the negative electrode includes an alloy material, the negative electrode active material layer may be formed using a method such as a deposition method, a sputtering method, or a plating method.
[0061] positive electrode The positive electrode includes a positive electrode current collector and a positive electrode active material disposed on the positive electrode current collector. The specific type of the positive electrode active material is not particularly limited and can be selected as necessary.
[0062] According to an embodiment of the present invention, the positive electrode active material includes a compound that reversibly inserts and extracts lithium ions. In some embodiments, the positive electrode active material can include a composite oxide, the composite oxide including lithium and at least one element selected from cobalt, manganese, and nickel. In still other embodiments, the positive electrode active material can include lithium cobalt oxide (LiCoO2), lithium nickel manganese cobalt ternary material, lithium manganate (LiMn2O4), lithium nickel manganese oxide (LiNi0.5 Mn 1.5 O4), and lithium iron phosphate (LiFePO4).
[0063] According to an embodiment of the present invention, the positive electrode active material layer may have a coating layer on the surface, or may be mixed with another compound having a coating layer. The coating layer may include at least one coating element compound selected from oxides of coating elements, hydroxides of coating elements, oxyhydroxides of coating elements, oxycarbonates of coating elements, and hydroxycarbonates of coating elements. The compound used in the coating layer may be amorphous or crystalline. The coating elements included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, F, or a mixture thereof. The coating layer may be formed by any method as long as the method does not adversely affect the performance of the positive electrode active material. For example, the method may include any coating method known to those skilled in the art, such as spraying, dipping, etc.
[0064] According to an embodiment of the present invention, the positive electrode active material layer further includes an adhesive, and optionally further includes a positive electrode conductive material.
[0065] The adhesive can enhance the bonding between the positive electrode active material particles and also enhance the bonding between the positive electrode active material and the current collector. Non-limiting examples of the adhesive include polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, poly(1,1-difluoroethylene), polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin, nylon, etc.
[0066] The positive electrode active material layer contains a positive electrode conductive material, thereby imparting electrical conductivity to the electrode. The positive electrode conductive material may contain any conductive material as long as it does not cause a chemical change. Non-limiting examples of the positive electrode conductive material include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., e.g., copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives), and mixtures thereof.
[0067] The positive electrode current collector used in the electrochemical device according to the present invention may be, but is not limited to, aluminum (Al).
[0068] electrolyte
[0069] The electrolyte used in the embodiment of the present invention may be any electrolyte known in the prior art. The electrolyte used in the electrolyte of the embodiment of the present invention may be, for example, inorganic lithium salts such as LiClO4, LiAsF6, LiPF6, LiBF4, LiSbF6, LiSO3F, LiN(FSO2)2; for example, LiCF3SO3, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,3-hexafluoropropane disulfonimide lithium, cyclic 1,2-tetrafluoroethane disulfonimide lithium, LiN(CF3SO2)(C4F9SO2), LiC(CF3SO2)3, LiPF4(CF3)2, LiPF4 Fluorine-containing organic lithium salts such as (C2F5)2, LiPF4(CF3SO2)2, LiPF4(C2F5SO2)2, LiBF2(CF3)2, LiBF2(C2F5)2, LiBF2(CF3SO2)2, LiBF2(C2F5SO2)2; dicarboxylic acid complex lithium salts such as lithium bis(oxalato)borate, lithium difluoro(oxalato)borate, lithium tris(oxalato)phosphate, lithium difluorobis(oxalato)phosphate, and lithium tetrafluoro(oxalato)phosphate; but are not limited thereto. The electrolytes may be used alone or in combination of two or more kinds. For example, in some embodiments, the electrolyte includes a combination of LiPF6 and LiBF4. In some embodiments, the electrolyte includes a combination of an inorganic lithium salt, such as LiPF6 or LiBF4, and a fluorine-containing organic lithium salt, such as LiCF3SO3, LiN(CF3SO2)2, or LiN(C2F5SO2)2.
[0070] In some embodiments, the concentration of the electrolyte is in the range of 0.8 mol / L to 3 mol / L, such as in the range of 0.8 mol / L to 2.5 mol / L, such as in the range of 0.8 mol / L to 2 mol / L, such as in the range of 1 mol / L to 2 mol / L, such as 1 mol / L, 1.15 mol / L, 1.2 mol / L, 1.5 mol / L, 2 mol / L, or 2.5 mol / L.
[0071] Solvents used in the electrolyte of embodiments of the present invention include, but are not limited to, carbonate compounds, ester-based compounds, ether-based compounds, ketone-based compounds, alcohol-based compounds, aprotic solvents, or combinations thereof.
[0072] Examples of carbonate ester compounds include, but are not limited to, linear carbonate ester compounds, cyclic carbonate ester compounds, fluorocarbonate ester compounds, or combinations thereof.
[0073] Examples of linear carbonate ester compounds include, but are not limited to, diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), and combinations thereof. Examples of cyclic carbonate ester compounds include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC), and combinations thereof. Examples of the fluorocarbonate compound are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate, and combinations thereof.
[0074] Examples of ester compounds include, but are not limited to, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, gamma-butyrolactone, decalactone, valerolactone, mevalonolactone, caprolactone, methyl formate, and combinations thereof.
[0075] Examples of ether compounds include, but are not limited to, dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, and combinations thereof.
[0076] An example of a ketone-based compound includes, but is not limited to, cyclohexanone.
[0077] Examples of alcohol-based compounds include, but are not limited to, ethanol and isopropyl alcohol.
[0078] Examples of aprotic solvents include, but are not limited to, dimethylsulfoxide, 1,2-dioxolane, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylmethylamide, acetonitrile, nitromethane, trimethyl phosphate, triethyl phosphate, trioctyl phosphate, and phosphate salts, and combinations thereof.
[0079] Separator In some embodiments, a separator is provided between the positive electrode and the negative electrode to prevent short circuit. The material and shape of the separator used in the embodiments of the present invention are not particularly limited and may be any of those disclosed in the prior art. In some embodiments, the separator includes a polymer or an inorganic material formed from a material that is stable against the electrolyte of the present invention.
[0080] For example, the separator may include a substrate layer and a surface treatment layer. The substrate layer is a nonwoven fabric, a membrane, or a composite membrane having a porous structure, and the material of the substrate layer is at least one selected from polyethylene, polypropylene, polyethylene terephthalate, and polyimide. Specifically, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane may be selected and used. The porous structure can improve the heat resistance, oxidation resistance, and electrolyte infiltration of the separator, and can increase the adhesion between the separator and the pole pieces.
[0081] A surface treatment layer is provided on at least one surface of the base layer, and the surface treatment layer may be a polymer layer or an inorganic layer, or may be a layer made of a mixture of a polymer and an inorganic material.
[0082] The inorganic layer includes inorganic particles and a binder, the inorganic particles being one or a combination of alumina, silica, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium oxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, and barium sulfate, and the binder being one or a combination of a polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, polyacrylic acid ester, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene, and polyhexafluoropropylene.
[0083] The polymer layer includes a polymer, and the polymer material is at least one selected from polyamide, polyacrylonitrile, polymer of acrylic ester, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, and poly(vinylidene fluoride-hexafluoropropylene).
[0084] application
[0085] The electrochemical device of the present invention includes any device in which an electrochemical reaction occurs, and specific examples thereof include all types of primary batteries, secondary batteries, fuel cells, solar cells, or capacitors. In particular, the electrochemical device is a lithium secondary battery, including a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, and a lithium ion polymer secondary battery.
[0086] The present invention further provides an electronic device comprising an electrochemical device according to the present invention.
[0087] The application of the electrochemical device of the present invention is not particularly limited, and can be used in any electronic device known in the prior art. In some embodiments, the electrochemical device of the present invention is used in, but is not limited to, notebook computers, pen-input computers, mobile computers, electronic book players, mobile phones, portable facsimiles, portable copy machines, portable printers, stereo headsets, video recorders, liquid crystal televisions, portable cleaners, portable CD players, minidiscs, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power sources, motors, automobiles, motorcycles, power-assisted bicycles, bicycles, lighting equipment, toys, game machines, watches, power tools, flashlights, cameras, large-scale household storage batteries, and lithium ion capacitors.
[0088] Hereinafter, the preparation of a lithium ion battery will be described with reference to specific examples, and those skilled in the art should understand that the preparation method described in the present invention is merely exemplary, and any other suitable preparation method is within the scope of the present invention.
[0089] Working Example Examples and comparative examples of the lithium ion battery according to the present invention will be described below, and performance evaluation will be performed.
[0090] 1. Preparation of lithium-ion batteries 1. Preparation of the negative electrode The coke was crushed to have a median diameter Dv50 in the range of 3 μm to 10 μm, and then pitch, which is a binder with a softening point of 100 to 300 ° C. (the amount of pitch added in Examples 1 to 16 and 18 to 39 was 15 wt%, and the amount of pitch added in Example 17 was 5 wt%) was added. The mixture of both was put into a granulator and granulated, and heated to a temperature of 500 ° C. to 1000 ° C. while continuously stirring during granulation, and then a graphitization process (the graphitization temperature was controlled to 2000 ° C. to 3500 ° C.) was performed to obtain graphite, which is the negative electrode active material used in the following Examples.
[0091] The coke was crushed to have a median diameter Dv50 in the range of 3 μm to 10 μm, put into a granulator and granulated. The mixture was heated to a temperature of 500°C to 1000°C while being continuously stirred during granulation, and then a graphitization process was performed (the graphitization temperature was controlled to 2000°C to 3500°C) to obtain graphite, which was the negative electrode active material used in Comparative Example 1.
[0092] The negative electrode active material prepared above, graphite, styrene butadiene rubber (SBR), and sodium carboxymethyl cellulose (CMC), were dispersed in deionized water in a weight ratio of 97.7:1.2:1.1, and thoroughly stirred to mix uniformly to obtain a negative electrode slurry. The negative electrode slurry was coated on a negative electrode current collector, dried, and cold rolled to form a negative electrode active material layer, which was then punched out and tabs were welded to obtain a negative electrode.
[0093] Graphite particles of different particle sizes can be obtained by crushing and classifying the raw materials by any known technique.
[0094] 2. Preparation of the positive electrode Lithium cobalt oxide (LiCoO2), acetylene black, and polyvinylidene fluoride (PVDF) were mixed uniformly in a weight ratio of 96:2:2 in an appropriate amount of N-methylpyrrolidone (NMP) by thorough stirring, and then coated on a positive electrode current collector, dried, and cold-rolled to form a positive electrode active material layer, and then punched out and welded a tab to obtain a positive electrode.
[0095] 3. Preparation of electrolyte In a dry argon gas atmosphere, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed in a weight ratio of 1:1:1, LiPF6 was added, and the mixture was mixed uniformly. 3% fluoroethylene carbonate was added, and the mixture was mixed uniformly to obtain an electrolyte. Here, the concentration of LiPF6 was 1.15 mol / L.
[0096] 4. Preparation of the separator A 12 μm thick porous polyethylene (PE) polymer film was used as the separator.
[0097] 5. Preparation of Lithium-ion Battery The positive electrode, separator, and negative electrode were stacked in this order so that the separator was interposed between the positive electrode and the negative electrode to play a role of isolation. Then, the battery was wound, the tabs were welded, and the battery was placed in an aluminum laminate film exterior foil. The above-prepared electrolyte was injected, and the battery was vacuum packaged, left to stand, formed, shaped, and measured for capacity, to obtain a lithium-ion battery.
[0098] 2.Measurement method 1. Method for measuring particle size of negative electrode active material The particle size of the negative electrode active material was measured using a Malvern particle sizer. The negative electrode active material sample was dispersed in ethanol, which is a dispersant, and after ultrasonic treatment for 30 minutes, the sample was placed in the Malvern particle sizer to measure the Dv50, Dv10, and Dv90 of the negative electrode active material.
[0099] 2. Method for measuring the specific surface area of negative electrode active material Using a specific surface area analyzer (Tristar II 3020M), the specific surface area of the negative active material was measured by a nitrogen adsorption / desorption method in which the negative active material sample was dried in a vacuum drying oven, placed in a sample tube, and measured with the analyzer.
[0100] 3. How to measure the capacity per gram of lithium-ion batteries The lithium-ion battery was discharged at 0.05C to 5.0mV, discharged at 50μA to 5.0mV, discharged at 10μA to 5.0mV, and charged at 0.1C to 2.0V, and the capacity of the lithium-ion battery was recorded and used as the capacity per gram. 0.05C refers to the current value at 0.05 times the designed capacity per gram, and 0.1C refers to the current value at 0.1 times the designed capacity per gram.
[0101] 4. Measurement method for thickness expansion rate of lithium-ion batteries during cycling At 45°C, the thickness of the lithium-ion battery in the initial half-charged state was measured using a micrometer with a resolution of 1 / 10000, and designated as H0. The lithium-ion battery was charged and discharged for 500 cycles at a rate of 1.5C, and the thickness of the lithium-ion battery in the fully charged state was measured every 50 cycles, and designated as H n The cycle thickness expansion rate of the lithium ion battery was calculated using the following formula. Cycle thickness expansion rate corresponding to the number of cycles = (H n -H0) / H0×100%
[0102] 5. How to measure the initial efficiency of lithium-ion batteries The lithium ion battery was charged at 0.5 C to 4.45 V and the initial charge capacity C was recorded, and then discharged at 0.5 C to 3.0 V and the discharge capacity D was recorded. The initial efficiency CE of the lithium ion battery was calculated by the following formula. CE=D / C
[0103] 3. Measurement results Table 1 shows the influence of the properties of the negative active material during the preparation of the negative active material on the capacity per gram and cycle thickness expansion rate of the lithium ion battery.
[0104] [Table 1]
[0105] As shown in Comparative Example 1, since no high viscosity binder is added when preparing the negative electrode active material, the negative electrode active material is a primary particle and is not composited to form secondary particles. The resulting lithium ion battery has a relatively large capacity per gram, but the anisotropy of the negative electrode active material is relatively large, so the cycle thickness expansion rate of the lithium ion battery is relatively high and the overall performance is poor.
[0106] As shown in Examples 1 to 20, by adding an appropriate amount of a high viscosity binder when preparing the negative electrode active material, the D 2 v50 / D 1 The v50 can be made 0.8 or more, so that the lithium-ion battery has a relatively high capacity per gram while also having a relatively low cycle thickness expansion rate, achieving a balance between high gram capacity and low cycle thickness expansion rate.
[0107] When the content of the high viscosity binder is a certain content, the median diameter D 1 When v50 gradually increases in the range of 10 μm to 25 μm, the median diameter D 2 v50 and D 1 v50 ratio D 2 v50 / D 1 v50 of the negative electrode active material decreases, and the (BET 2 -BET 1 ) / BET 1 The specific surface area of the negative electrode active material increases with the BET 1 0.6m 2 / g~2.0m 2 / g and (BET 2 -BET 1 ) / BET 1 ≦1 and / or the ratio of the carbon to oxygen contents in the negative electrode active material layer is within the range of 2:3 to 990:1, a better balance between high capacity per gram and low cycle thickness expansion rate can be achieved.
[0108] Table 2 shows the D of the negative electrode active material. 1 v90 / D 1 The effects of v10 and C004 / C110 on the initial efficiency and cycle thickness expansion rate of lithium-ion batteries are shown. Except for the parameters listed in Table 2, the conditions of Examples 21 to 39 are the same as those of Example 8.
[0109] [Table 2]
[0110] As a result, the negative electrode active material D 1 v90 / D 1 When v10 is less than 3.5, the initial efficiency of the lithium-ion battery is significantly improved. 1 v90 / D 1 When v10 gradually decreases within the range of less than 3.5, the initial efficiency of the lithium ion battery does not change much, and the cycle thickness expansion rate gradually decreases. When C004 / C110 of the negative electrode active material layer gradually decreases within the range of 5.7 to 18, the crystallite size La of the graphite particles decreases, Lc increases, the porosity increases, the cycle thickness expansion rate of the lithium ion battery gradually decreases, and the initial efficiency decreases slightly. Overall, the negative electrode active material material is D 1 v90 / D 1 A lithium-ion battery can achieve a balance between initial efficiency and cycle thickness expansion rate if v10 is less than 3.5, C004 / C110 is in the range of 5.7-18, La is 160 nm-165 nm, Lc is 30 nm-32 nm, and / or the porosity is 20%-30%.
[0111] Table 3 shows the influence of the characteristics of the negative electrode active material of a lithium ion battery in a fully discharged state on the initial efficiency and cycle thickness expansion rate of the lithium ion battery.
[0112] [Table 3]
[0113] As a result, in a fully discharged lithium-ion battery, the negative electrode active material D b v50 / D a v50 and the (BET b -BET a ) / BET a This affects the improvement of the initial efficiency of the lithium ion battery, and also affects the cycle thickness expansion rate of the lithium ion battery.
[0114] 1 shows the cycle thickness expansion rate depending on the number of cycles of the lithium ion batteries of Example 8 and Comparative Example 1. The results show that the lithium ion battery of Example 8 has a significantly lower cycle thickness expansion rate than that of Comparative Example 1. As the number of cycles increases, the difference between the cycle thickness expansion rates of the two batteries becomes larger.
[0115] Throughout the specification, references to "an embodiment," "some of the embodiments," "one embodiment," "another example," "example," "embodiment," or "some of the examples" mean that at least one embodiment or example of the invention includes a particular feature, structure, material, or characteristic described in that embodiment or example. Thus, the appearances of, for example, "in some embodiments," "in an embodiment," "in another example," "in one example," "in a particular example," or "example" in various places throughout the specification do not necessarily refer to the same embodiment or example of the invention. Furthermore, particular features, structures, materials, or characteristics herein may be combined in any suitable manner in one or more embodiments or examples.
[0116] Although exemplary embodiments have been described and illustrated, those skilled in the art should understand that the above-described embodiments are not to be construed as limiting the present invention, and that modifications, substitutions, and alterations to the embodiments are possible without departing from the spirit, principle, and scope of the present invention.
Claims
1. A negative electrode active material, The median diameter is D 1 v50, and the median diameter after pressing at a pressure of 1 t is D 2 When v is set to 50, D 2 v50 / D 1 v50 is 0.8 to 1.0, The negative electrode active material contains graphite particles, D 1 v90 and D 1 v10 is D 1 v90 / D 1 v10<3.5 is satisfied, The graphite particles have a crystallite size Lc of 30 nm to 32 nm along the perpendicular direction as measured by an X-ray diffraction method.
2. The specific surface area of the negative electrode active material is calculated by BET 1 The specific surface area of the negative electrode active material after being pressed at a pressure of 1 t is calculated by BET 2 When the BET 1 is 0.6m 2 / g to 2.0 m 2 / g, (BET 2 -BET 1 ) / BET 1 2. The negative electrode active material according to claim 1, wherein the anode active material has a molecular weight of 1.0 or less.
3. The graphite particles are (a) D 1 v50 is 10 μm to 25 μm; (b) the graphite particles have a crystallite size (La) along the horizontal direction of 160 nm to 165 nm as determined by an X-ray diffraction method; The negative electrode active material according to claim 1 , which satisfies at least one of the following conditions:
4. An electrochemical device including a negative electrode including a negative electrode current collector and a negative electrode active material layer, The negative electrode active material layer comprises the negative electrode active material according to any one of claims 1 to 3. An electrochemical device.
5. The negative electrode active material layer is (c) the negative electrode active material layer contains carbon and oxygen, and the weight ratio of the carbon content to the oxygen content is 2:3 to 990:1; (d) a ratio C004 / C110 of a peak area C004 of a (004) plane of the negative electrode active material layer to a peak area C110 of a (110) plane thereof obtained by X-ray diffraction pattern measurement is 5.7 to 18; (e) the porosity of the negative electrode active material layer is 20% to 30%; The electrochemical device according to claim 4 , which satisfies at least one of the following conditions:
6. 5. The electrochemical device according to claim 4, wherein in the electrochemical device in a fully discharged state, a ratio C004' / C110' of a peak area C004' of a (004) plane of the negative electrode active material layer obtained by X-ray diffraction pattern measurement to a peak area C110' of a (110) plane is 6.8 to 17.
2.
7. In the electrochemical device in a fully discharged state, the median diameter of the negative electrode active material is D a v50, and the median diameter of the negative electrode active material after being pressed with a pressure of 1 t is D b When v is set to 50, D b v50 / D a 5. The electrochemical device of claim 4, wherein v50 is 0.9 or greater.
8. In the electrochemical device in a fully discharged state, the median diameter D of the negative electrode active material a The electrochemical device of claim 4, wherein v50 is between 8 μm and 20 μm.
9. In the electrochemical device in a fully discharged state, the specific surface area of the negative electrode active material is calculated by BET a The specific surface area of the negative electrode active material after being pressed at a pressure of 1 t is calculated by BET b Then, (BET b -BET a ) / BET a 5. The electrochemical device of claim 4, wherein:
10. An electronic device comprising an electrochemical device according to any one of claims 4 to 9.
Citation Information
Patent Citations
Negative electrode material for nonaqueous secondary cells, negative electrode for nonaqueous secondary cells, and nonaqueous secondary cell
WO2006025376A1
Method for producing negative electrode active material for lithium secondary battery, and lithium secondary battery including same
WO2019035580A1