Vanadium electrolyte and its manufacturing method and application

A cost-effective and efficient process for producing vanadium electrolyte using vanadium ore and chemical treatments addresses the complexity and expense of existing methods, achieving high-purity electrolytes with low energy consumption and minimal waste, supporting the industrialization of vanadium batteries.

JP7579913B2Active Publication Date: 2024-11-08HUNAN YINFENG NEW ENERGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023099339
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-30
Filing Date
2023-06-16
Publication Date
2024-11-08
Estimated Expiration
2043-06-16

AI Technical Summary

Technical Problem

The production process of vanadium electrolyte is complicated and expensive, with high raw material costs due to the use of ammonium metavanadate or vanadium pentoxide, making it difficult to control production costs and limit the industrialization of vanadium batteries.

Method used

A method involving the use of vanadium ore, sulfuric acid, and a series of chemical treatments including leaching, impurity removal, and back-extraction to produce a vanadium electrolyte, which includes steps such as aging, mixing, leaching, adding impurity removing agents, and using specific oxidizing and reducing agents to achieve high purity and low energy consumption.

Benefits of technology

The method significantly reduces production costs, achieves low energy consumption, low pollution, and high purity of the electrolyte, with stable quality and controllable ions, meeting first-class requirements for vanadium redox flow battery electrolytes, and promotes resource recovery and utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579913000001
    Figure 0007579913000001
  • Figure 0007579913000002
    Figure 0007579913000002
  • Figure 0007579913000003
    Figure 0007579913000003
Patent Text Reader

Abstract

To provide a vanadium electrolyte, a manufacturing method of them, and an application.SOLUTION: A manufacturing method of a vanadium electrolyte, contains: a step of taking out a vanadium ore, adding sulfuric acid therein, mixing uniformly them, and obtaining a mixture; a step of aging the mixture, and obtaining an aging material; a step of immersing the aging material with water, and obtaining vanadium content immersion liquid; a step of adding a first impurity removal agent to the vanadium content immersion liquid, and obtaining first cleaning liquid; a step of adding an oxidant, an iron phosphate hydrate seed crystal, and a second impurity removal agent to the first cleaning liquid, and obtaining second cleaning liquid; a step of adding a reductant agent and a flocculant to the second cleaning liquid, and obtaining filtrate after filtration; a step of mixing the filtrate and extraction liquid, and obtaining an organic phase carrying vanadium by extracting; a step of reversely extracting the organic phase carrying vanadium, and obtaining reverse extraction liquid; and a step of removing the organic phase from the reverse extraction liquid, and obtaining a vanadium electrolyte.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the metallurgical technology field, in particular to a vanadium electrolyte and its preparation method and application. [Background technology]

[0002] Vanadium batteries, as one of the currently rapidly developing environmentally friendly batteries, have characteristics such as energy storage capacity and power adjustable, large current lossless deep discharge, easy operation and maintenance, high safety, excellent reliability, long life, low pollution, etc., and have unparalleled advantages compared with other batteries in the direction of large-scale energy storage. However, the application is limited due to cost issues. Vanadium electrolyte, as the core energy storage module of vanadium batteries, accounts for 41% of the total cost of the entire vanadium battery, so how to control the production cost of electrolyte is the key to promoting the industrialization and large-scale application of vanadium batteries.

[0003] At present, the method for producing vanadium electrolyte involves producing high-purity vanadium pentoxide using ammonium metavanadate or vanadium pentoxide, and then using the high-purity vanadium pentoxide to produce electrolyte by methods such as low-temperature dissolution reduction, electrolysis, and high-temperature reduction and dissolution.

[0004] In these methods, the process of producing the electrolyte is complicated and expensive. Moreover, ammonium metavanadate or vanadium pentoxide is used as the raw material, which is also obtained from vanadium ore or vanadium waste through a series of complicated metallurgical processes, and the cost is relatively high, making it difficult to control the cost of the vanadium electrolyte. Summary of the Invention [Problem to be solved by the invention]

[0005] The technical problem to be solved by the present invention is to provide a vanadium electrolyte, its preparation method and application, so as to solve the technical problems of the prior art that the preparation process of vanadium electrolyte is complicated and the cost is high. [Means for solving the problem]

[0006] In order to solve the above technical problems, the technical solutions of the present invention are as follows:

[0007] A method for producing a vanadium electrolyte, comprising the steps of: (1) taking vanadium ore, adding sulfuric acid thereto, and mixing uniformly to obtain a mixture; (2) aging the mixture obtained in step (1) to obtain an aged material; (3) leaching the aged material obtained in step (2) with water to obtain a vanadium-containing leachate; (4) adding a first impurity removing agent to the vanadium-containing leachate obtained in step (3) to obtain a first purified solution; (5) adding an oxidizing agent, iron phosphate dihydrate seed crystals, and a second impurity removing agent to the first purified solution obtained in step (4) to obtain a second purified solution; (6) adding a reducing agent and a flocculant to the second purified liquid obtained in step (5), and filtering the liquid to obtain a filtrate; (7) mixing the filtrate and the extract obtained in step (6) and extracting to obtain an organic phase loaded with vanadium; (8) stripping the vanadium-loaded organic phase obtained in step (7) to obtain a stripped solution; (9) removing the organic phase from the stripped solution obtained in step (8) to obtain a vanadium electrolyte solution.

[0008] Preferably, in step (1), the sulfuric acid is a sulfuric acid solution having a mass concentration of 90 to 98%, Optionally, in step (1), the mass ratio of the sulfuric acid to the vanadium ore is 1:(4-20).

[0009] Preferably, in step (1), when the sulfuric acid is added, the temperature of the mixture is 50 to 130° C. Preferably, the addition rate of the sulfuric acid is 0.05 to 10 mL min -1 ·g -1 It is.

[0010] Optionally, in step (1), water is added before sulfuric acid is added. Preferably, the mass ratio of water to the vanadium ore is (0.001-0.2):1.

[0011] Preferably, the step (1) further includes a step of crushing the vanadium ore. Preferably, the vanadium ore is crushed into powder having a particle size of less than 2 mm and a particle size within a range of 1 to 2 mm, with 50% or more of the mass of the vanadium ore being contained therein.

[0012] Preferably, in step (2), the aging temperature is 40 to 130° C. and the aging time is longer than 12 hours. More preferably, the aging is carried out in a moist environment.

[0013] Preferably, step (2) further comprises the step of crushing the aged material. Preferably, the aged material is crushed to a particle size of less than 5 mm.

[0014] Preferably, in step (3), the mass ratio of water to the aging material is (0.5-5):1.

[0015] Preferably, in step (3), the leaching temperature is 10 to 90°C.

[0016] Preferably, in step (4), the pH value of the vanadium-containing leachate is first adjusted to 1.0-2.0, and then the first impurity removing agent is added; Optionally, the first impurity removing agent is one or more of sodium fluoride, potassium fluoride, ammonium fluoride, lithium fluoride, hydrofluoric acid, sodium hexafluorophosphate, potassium hexafluorophosphate.

[0017] Preferably, the molar ratio of the first impurity removing agent to aluminum ions in the vanadium-containing leachate is (0.5-10):1.

[0018] Preferably, step (4) further comprises a step of filtering after adding the first impurity removing agent.

[0019] Preferably, in step (4), after the first impurity removing agent is added, the impurity removing reaction is carried out at 5 to 90°C.

[0020] Preferably, in step (4), the pH value of the vanadium-containing leachate obtained in the adjusting step (3) is adjusted to 1.0-2.0, and the vanadium ore in step (1) is used. After adjusting the pH value to 1.0-2.0, the vanadium-containing leachate and the wet ore are obtained by solid-liquid separation.

[0021] Preferably, in step (5), the oxidizing agent is one or more of sodium chlorate, sodium hypochlorite, and hydrogen peroxide; Optionally, the second impurity removing agent is one or more of phosphoric acid, sodium phosphate, disodium hydrogen phosphate, monosodium hydrogen phosphate, potassium phosphate, dipotassium hydrogen phosphate, monopotassium hydrogen phosphate, ammonium hydrogen phosphate.

[0022] Preferably, the molar ratio of the oxidizing agent to the divalent iron ions in the first purification solution is (0.2-1:1).

[0023] Preferably, the molar ratio of the second impurity removing agent to the iron ions in the first purification liquid is (0.5-2):1.

[0024] Preferably, the molar ratio of the iron phosphate dihydrate seed crystals to the iron ions in the first purification solution is (0.01-0.2):1.

[0025] Preferably, the method further comprises the step of adjusting the pH value of the first purification liquid to 1.5 to 2.5 after adding the oxidizing agent in step (5).

[0026] Preferably, the method further comprises the step of filtering the reaction liquid obtained after adding the second impurity removing agent in step (5).

[0027] Preferably, in step (5), after the second impurity removing agent is added, the impurity removing reaction is carried out at 5 to 90°C.

[0028] Preferably, in step (6), the reducing agent is one or more of sulfite, sulfur dioxide, elemental sulfur, zinc powder, organic sulfur compounds, oxalates, ascorbic acid, and carbon monoxide; Optionally, the flocculant is one or more of polyacrylamide, sodium polyacrylate.

[0029] Preferably, the molar ratio of the reducing agent to the pentavalent vanadium ions in the second purification liquid is (1-3):1.

[0030] Preferably, the molar ratio of the flocculant to the vanadium ions in the second purification liquid is (0.01-0.1):1.

[0031] Preferably, the method further comprises the step of adjusting the pH value of the second purification liquid to 1.7 to 2.2 after adding the reducing agent in step (6).

[0032] Preferably, in step (6), after adding the flocculant, the mixture is stirred for 1 to 2 hours to react, and then filtered using an ultrafiltration membrane to obtain a filtrate.

[0033] Preferably, in step (7), the extraction liquid is a mixture of an extractant, tributyl phosphate, and sulfonated kerosene, and the extractant is one or more of P204, N235, and P507, where P204 refers to bis(2-ethylhexyl) phosphate, N235 refers to trioctylamine, and P507 refers to 2-ethylhexyl phosphate.

[0034] Preferably, the extract is prepared by mixing the following ingredients in parts by weight: Extractant 10-25 parts, Tributyl phosphate 4 to 10 parts, Sulfonated kerosene 65-86 parts.

[0035] Preferably, in step (7), the volume ratio of the filtrate to the extract is 1:(0.2 to 1).

[0036] Preferably, step (8) specifically includes washing the vanadium-loaded organic phase obtained in step (7) with a sulfuric acid solution having a pH value of 1.5 to 2.0, and then back-extracting the organic phase with a 1.5 to 2.5 mol / L sulfuric acid solution to obtain a back-extracted solution.

[0037] Preferably, in step (8), the volume ratio of the sulfuric acid solution having a pH value of 1.5-2.0 to the vanadium-loaded organic phase is (0.5-5):1.

[0038] Preferably, in step (8), the volume ratio of the 1.5-2.5 mol / L sulfuric acid solution to the vanadium-loaded organic phase is (0.05-0.6):1.

[0039] Preferably, step (9) specifically includes subjecting the stripped solution to diffusion dialysis to obtain a dialysate, then extracting and stripping the dialysate to obtain a secondary stripped solution, and then passing the secondary stripped solution through an activated carbon adsorption column to remove the organic phase and obtain a vanadium electrolyte solution.

[0040] Preferably, in step (9), the sulfuric acid solution is recovered through a diffusion dialysis membrane. In the diffusion dialysis, the flow rate of the stripping solution is 0.15 to 0.30 × 10 -3 m 3 / (hm 2 ), and the flow rate ratio of water to the stripping liquid was (0.5-1.5:1).

[0041] Preferably, in step (9), the method further comprises adding water and / or a sulfuric acid solution to the vanadium electrolytic solution to adjust the vanadium ion concentration in the vanadium electrolytic solution to 1.3 to 1.8 mol / L and the sulfate ion concentration in the vanadium electrolytic solution to 4.0 to 4.5 mol / L. The mass concentration of the sulfuric acid solution is 90 to 98%.

[0042] The present invention further provides a vanadium electrolyte produced by the method for producing a vanadium electrolyte.

[0043] The present invention further provides an application of said vanadium electrolyte in the field of batteries. Effect of the Invention

[0044] The above solution of the present invention includes at least the following beneficial effects:

[0045] (1) A method for producing a vanadium electrolyte solution of the present invention includes the steps of: taking vanadium ore, adding sulfuric acid thereto, and mixing uniformly to obtain a mixture; aging the mixture to obtain an aged material; leaching the aged material with water to obtain a vanadium-containing leachate; adding a first impurity remover to the vanadium-containing leachate to obtain a first purified solution; adding an oxidizing agent, iron phosphate dihydrate seed crystals, and a second impurity remover to the first purified solution to obtain a second purified solution; adding a reducing agent and a flocculant to the second purified solution, filtering, and then obtaining a filtrate; mixing the filtrate and an extract, and extracting to obtain an organic phase supporting vanadium; stripping the organic phase supporting vanadium to obtain a stripped solution; and removing the organic phase from the stripped solution to obtain a vanadium electrolyte solution. The vanadium electrolyte preparation method of the present invention not only greatly reduces the electrolyte preparation cost, but also has low energy consumption, small pollution, high purity of the prepared electrolyte product, controllable impurity ions in the electrolyte, stable quality, strong applicability, and can be applied to various electrolyte application environments.

[0046] (2) In the method for producing vanadium electrolyte of the present invention, in steps (1) to (3), vanadium ore is used as raw material to directly produce finished vanadium electrolyte, and an aging method is used to ensure that the valence state of vanadium in the vanadium-containing leachate is mainly tetravalent, so that the valence state of vanadium in the entire process is basically consistent with that of the final vanadium electrolyte, which in turn reduces the oxidation-reduction costs in the process.

[0047] (3) The method for producing vanadium electrolyte of the present invention uses vanadium ore as raw material to directly produce a finished vanadium electrolyte, and does not involve a vanadium precipitation process. Therefore, no ammonia nitrogen wastewater is generated throughout the entire process, and the amount of process wastewater to be treated throughout the entire production method is relatively small. Only the raffinate needs to be treated, and the raffinate can be fully reused after impurity removal treatment, thereby realizing "zero" emissions and relatively low treatment costs.

[0048] (4) The method for producing vanadium electrolyte of the present invention further includes a step of crushing the vanadium ore in step (1). The vanadium ore is crushed into powder having a particle size of less than 2 mm and a particle size in the range of 1 to 2 mm, with the mass of the vanadium ore being 50% or more. By controlling the particle size of the vanadium ore, the cost of crushing the ore can be reduced, selective leaching of vanadium in the vanadium ore can be realized, impurities in the leaching solution can be reduced, and the cost of subsequent impurity removal can be reduced.

[0049] (5) In the method for producing a vanadium electrolyte solution of the present invention, in step (1), when the sulfuric acid is added, the temperature of the mixture is 50 to 130° C. The rate of addition of the sulfuric acid is 0.05 to 10 ML min -1 ·g -1 By controlling the rate of addition of the sulfuric acid, the mixture is heated to 50 to 130°C, and then in the maturation process of step (2), the mixture is maturated by keeping the temperature constant, so that the heat required for maturation can be secured without external heat energy, and the property of releasing heat when the sulfuric acid is added is fully utilized, so that the temperature required for maturation is secured, and energy consumption costs are significantly reduced.

[0050] (6) In the method for producing vanadium electrolyte of the present invention, in step (4), the pH value of the vanadium-containing leachate obtained in step (3) is adjusted to 1.0-2.0, and the vanadium ore in step (1) is adopted. By using vanadium ore to neutralize the acid in the vanadium-containing leachate, the acid-consuming substances in the vanadium ore are consumed in advance, thus reducing the acid consumption required for maturation, while replacing other neutralizing agents, thereby reducing the cost of neutralization, reducing the loss of vanadium, and also reducing the amount of waste residue.

[0051] (7) In the method for preparing vanadium electrolyte of the present invention, in steps (4) to (6), aluminum, iron, and magnesium are removed by chemical precipitation before the extraction in step (7), which not only solves the problem of co-extraction of aluminum, iron, magnesium, and vanadium, but also obtains cryolite and iron phosphate, thereby realizing the recovery and utilization of resources.

[0052] (8) In the method for producing vanadium electrolyte of the present invention, in step (6), the coagulant is added, and then the mixture is stirred for 1 to 2 hours to react, and then filtered using an ultrafiltration membrane to obtain a filtrate. By combining the coagulant and the filtration using an ultrafiltration membrane, fine particles and some anions in the solution can be effectively removed. This not only realizes the purification and removal of impurities, but also reduces the emulsification phenomenon during the extraction process.

[0053] (9) In the method for producing vanadium electrolyte of the present invention, in step (9), the stripping solution is subjected to diffusion dialysis to obtain a dialysate, and then the obtained dialysate is extracted and stripped to obtain a second stripping solution, and then the second stripping solution is passed through an activated carbon adsorption column to remove the organic phase to obtain a vanadium electrolyte. When sulfuric acid is recovered from the stripping solution by diffusion dialysis, on the one hand, the concentration of sulfuric acid in the stripping solution is relatively high, and in the alkali neutralization method, the alkali consumption is large, and the solution itself has been purified several times, so its impurity content is not high, and the alkali neutralization method introduces impurity ions, increases the loss of vanadium, and generates a large amount of waste residue. When sulfuric acid is recovered from the stripping solution by diffusion dialysis, the cost is relatively low, impurity ions are not introduced, the loss of vanadium is small, and no waste residue is generated. On the other hand, the sulfuric acid solution recovered by diffusion dialysis can be directly returned to the process without treatment, which greatly reduces the consumption of sulfuric acid in the process.

[0054] (10) In the method for producing vanadium electrolyte of the present invention, in step (9), the dialysate obtained is extracted and stripped to obtain a secondary stripped solution, which can not only remove impurity ions but also concentrate the vanadium ions to ensure that the vanadium ions reach the required concentration in the vanadium electrolyte.

[0055] (11) The impurity ion concentrations of the vanadium electrolyte of the present invention are 30 mg / L or less for iron, aluminum, magnesium, calcium, sodium, and potassium, and 5 mg / L or less for silicon ions, and all other impurity ions meet the first-class requirements of the "GB / T 37204-2018-All-Vanadium Redox Flow Battery Electrolyte" standard. Some impurities are much lower than the first-class requirements of the GB / T 37204-2018 "All-Vanadium Redox Flow Battery Electrolyte" standard, especially iron, aluminum, calcium, sodium, potassium, silicon, chromium, molybdenum, etc., which are relatively difficult to remove. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0056] In each embodiment of the present invention, those without specific conditions are carried out according to conventional conditions or conditions proposed by the manufacturers. Among the reagents or equipment used, those without manufacturers are all conventional products available on the market, and raw materials of different manufacturers and models do not affect the implementation of the technical solutions and the realization of the technical effects of the present invention.

[0057] Example 1 The method for producing the vanadium electrolyte of this embodiment includes the following steps.

[0058] (1) Take vanadium ore and crush it into powder with a particle size of less than 2 mm and a particle size of 1 to 2 mm in the range of 50% or more by mass. Add water to the vanadium ore and then add 0.05 mL min -1 ·g -1A sulfuric acid solution having a mass concentration of 90% is added at a rate of 0.01 to 0.01 g / l and mixed uniformly at 50°C to obtain a mixture.

[0059] Here, the mass ratio of the water to the vanadium ore is 0.1:1, and the mass ratio of the sulfuric acid solution to the vanadium ore is 1:12.

[0060] (2) aging the mixture obtained in step (1) to obtain aged material, and crushing the aged material to a particle size of less than 5 mm.

[0061] Here, the aging is carried out in a moist environment, the aging temperature is 40° C., and the aging time is longer than 12 hours.

[0062] (3) The aged material obtained in step (2) is leached with water at 10° C. to obtain a vanadium-containing leachate.

[0063] Here, the mass ratio of water to the aging material is 0.5: 1. The vanadium-containing leachate can be obtained by solid-liquid separation. After solid-liquid separation, the vanadium-containing leachate and leach residue are obtained.

[0064] (4) First, adjust the pH value of the vanadium-containing leachate obtained in step (3) to 1.0, then add a first impurity removing agent to the vanadium-containing leachate to carry out an impurity removing reaction at 5°C, and filter the reaction liquid to obtain a first purified liquid.

[0065] Here, the first impurity removing agent is a mixture of sodium fluoride and ammonium fluoride in a weight ratio of 30: 8. The molar ratio of the first impurity removing agent to aluminum ions in the vanadium-containing leachate is 0.5: 1. Aluminum ions are removed by the first impurity removing agent, and sodium hexafluoroaluminate, which is cryolite, is obtained.

[0066] In a preferred embodiment of this embodiment, the vanadium ore of step (1) is used to adjust the pH value of the vanadium-containing leachate obtained in step (3) to 1.0. After adjusting the pH value to 1.0, the vanadium-containing leachate and the wet ore are obtained by solid-liquid separation. In addition, as an alternative embodiment of this embodiment, a chemical reagent may be used to adjust the pH value of the vanadium-containing leachate obtained in step (3) to 1.0.

[0067] In order to facilitate efficient utilization of resources, the vanadium ore from step (1) may be mixed with the wet ore produced in step (4).

[0068] (5) An oxidizing agent is added to the first purified liquid obtained in step (4), and the pH value of the first purified liquid is adjusted to 2.5. Then, iron phosphate dihydrate seed crystals and a second impurity removing agent are added thereto to carry out an impurity removing reaction at 5°C, and the resulting reaction liquid is filtered to obtain a second purified liquid.

[0069] Here, the oxidizing agent is sodium chlorate, and the molar ratio of the oxidizing agent to the divalent iron ions in the first purification solution is 0.6:1.

[0070] The second impurity removing agent is sodium phosphate. The molar ratio of the second impurity removing agent to the iron ions in the first purification solution is 2:1. The iron ions are removed by the second impurity removing agent to obtain iron phosphate.

[0071] The molar ratio of the iron phosphate dihydrate seed crystals to the iron ions in the first purification solution is 0.1:1.

[0072] (6) A reducing agent is added to the second purified liquid obtained in step (5) to reduce the pentavalent vanadium in the second purified liquid to tetravalent vanadium, and the pH value of the second purified liquid is adjusted to 2.2, and then a coagulant is added thereto, and the mixture is stirred for 2 hours to react, and then filtered using an ultrafiltration membrane to obtain a filtrate.

[0073] Here, the reducing agent is sodium sulfite, and the molar ratio of the reducing agent to the pentavalent vanadium ions in the second purification liquid is 3:1.

[0074] The flocculant is polyacrylamide, and the molar ratio of the flocculant to the vanadium ions in the second purification liquid is 0.01:1.

[0075] (7) The filtrate and the extract obtained in step (6) are mixed and extracted to obtain an organic phase loaded with vanadium.

[0076] In addition, a raffinate is also produced during the extraction. In order to make full use of resources, the water that has been neutralized and subjected to impurity removal can be used as the water used for leaching in step (3) or the water added to the vanadium ore in step (1).

[0077] Here, the extract contains the following weight parts of raw materials: 25 parts of extractant, 4 parts of tributyl phosphate, and 65 parts of sulfonated kerosene. The extractant is a mixture of P204 and P507 in a weight ratio of 1:9. The volume ratio of the filtrate to the extract is 1:0.5.

[0078] (8) The vanadium-loaded organic phase obtained in step (7) is washed with a sulfuric acid solution having a pH value of 1.5, and then back-extracted with a 2.0 mol / L sulfuric acid solution to obtain a back-extracted solution.

[0079] Here, the volume ratio of the sulfuric acid solution having a pH value of 1.5 to the organic phase carrying the vanadium was 0.5:1.

[0080] The volume ratio of the 2.0 mol / L sulfuric acid solution to the vanadium-loaded organic phase was 0.3:1.

[0081] In order to realize efficient utilization of resources, the water washed with the sulfuric acid solution can be used as the water used for leaching in step (3).

[0082] (9) The stripped solution obtained in step (8) is subjected to diffusion dialysis, and the sulfuric acid solution is recovered through a diffusion dialysis membrane to obtain a dialysate. The dialysate is then extracted and stripped to obtain a secondary stripped solution. The secondary stripped solution is then passed through an activated carbon adsorption column to remove the organic phase, and a vanadium electrolyte solution is obtained.

[0083] In order to obtain a vanadium electrolyte solution of an appropriate concentration, water and / or a sulfuric acid solution may be added to the vanadium electrolyte solution, and the vanadium ion concentration in the vanadium electrolyte solution is adjusted to 1.8 mol / L, and the sulfate ion concentration is adjusted to 4.5 mol / L. Here, the mass concentration of the sulfuric acid solution is 98%.

[0084] In the diffusion dialysis, the flow rate of the stripping solution is 0.30×10 -3 m 3 / (hm 2 ), and the flow rate ratio of water to the stripping solution is 1:1. In this embodiment, extraction and stripping are performed to obtain the secondary stripping solution, which may be performed in the same manner as in steps (7) and (8), or other reagents may be selected to perform extraction and stripping according to the actual situation.

[0085] In order to realize efficient utilization of resources, the sulfuric acid solution recovered through the diffusion dialysis membrane can be used for the water or sulfuric acid solution added in step (1).

[0086] Example 2 The method for producing the vanadium electrolyte of this embodiment includes the following steps.

[0087] (1) Take vanadium ore and crush it into powder with a particle size of less than 2 mm and with a particle size of 1 to 2 mm in the range of 50% or more by mass. Add water to the vanadium ore and then add 10 mL min -1 ·g -1 A sulfuric acid solution having a mass concentration of 94% is added at a rate of 0.01 to 0.01 and mixed uniformly at 130° C. to obtain a mixture.

[0088] Here, the mass ratio of the water to the vanadium ore is 0.2:1, and the mass ratio of the sulfuric acid solution to the vanadium ore is 1:4.

[0089] (2) maturing the mixture obtained in step (1) to obtain a maturated material, and crushing the maturated material to a particle size of less than 5 mm.

[0090] Here, the aging is carried out in a moist environment, the aging temperature is 130° C., and the aging time is longer than 12 hours.

[0091] (3) The aged material obtained in step (2) is leached with water at 50° C. to obtain a vanadium-containing leachate.

[0092] Here, the mass ratio of water to the aging material is 5: 1. The vanadium-containing leachate can be obtained by solid-liquid separation. After solid-liquid separation, the vanadium-containing leachate and leach residue are obtained.

[0093] (4) First, adjust the pH value of the vanadium-containing leachate obtained in step (3) to 1.5, then add a first impurity removing agent to the vanadium-containing leachate to carry out an impurity removing reaction at 90°C, and filter the reaction liquid to obtain a first purified liquid.

[0094] Here, the first impurity removing agent is potassium fluoride. As an alternative embodiment of this embodiment, the first impurity removing agent may be one or more of ammonium fluoride, lithium fluoride, hydrofluoric acid, sodium hexafluorophosphate, and potassium hexafluorophosphate. The molar ratio of the first impurity removing agent to the aluminum ions in the vanadium-containing leachate is 5:1. The aluminum ions are removed by the first impurity removing agent to obtain sodium hexafluoroaluminate, which is cryolite.

[0095] In a preferred embodiment of this embodiment, the pH value of the vanadium-containing leachate obtained in step (3) is adjusted to 1.5, and the vanadium ore obtained in step (1) is used. After adjusting the pH value to 1.5, the vanadium-containing leachate and the wet ore are obtained by solid-liquid separation. In addition, as an alternative embodiment of this embodiment, a chemical reagent may be used to adjust the pH value of the vanadium-containing leachate obtained in step (3) to 1.5.

[0096] In order to facilitate efficient utilization of resources, the vanadium ore of step (1) may be mixed with the wet ore produced in step (4).

[0097] (5) An oxidizing agent is added to the first purified liquid obtained in step (4), and the pH value of the first purified liquid is adjusted to 2.0. Then, iron phosphate dihydrate seed crystals and a second impurity removing agent are added thereto, and an impurity removing reaction is carried out at 90°C. The resulting reaction liquid is filtered to obtain a second purified liquid.

[0098] Here, the oxidizing agent is sodium hypochlorite, and the molar ratio of the oxidizing agent to the divalent iron ions in the first purification solution is 0.2:1.

[0099] The second impurity removing agent is phosphoric acid. As an alternative embodiment of this embodiment, the second impurity removing agent may be one or more of sodium phosphate, disodium hydrogen phosphate, monosodium hydrogen phosphate, potassium phosphate, dipotassium hydrogen phosphate, monopotassium hydrogen phosphate, and ammonium hydrogen phosphate. The molar ratio of the second impurity removing agent to the iron ions in the first purification liquid is 1.2:1. The iron ions are removed by the second impurity removing agent to obtain iron phosphate.

[0100] The molar ratio of the iron phosphate dihydrate seed crystals to the iron ions in the first purification solution is 0.2:1.

[0101] (6) A reducing agent is added to the second purified liquid obtained in step (5) to reduce the pentavalent vanadium in the second purified liquid to tetravalent vanadium, and the pH value of the second purified liquid is adjusted to 1.7, and then a coagulant is added thereto, and the mixture is stirred for 2 hours to react, and then filtered using an ultrafiltration membrane to obtain a filtrate.

[0102] Wherein, the reducing agent is sulfur dioxide. In an alternative embodiment of this embodiment, the reducing agent may be one or more of elemental sulfur, zinc powder, organic sulfur compounds, oxalates, ascorbic acid, and carbon monoxide, and the molar ratio of the reducing agent to the pentavalent vanadium ions in the second purification solution is 1:1.

[0103] The flocculant is sodium polyacrylate, and the molar ratio of the flocculant to the vanadium ions in the second purification liquid is 0.1:1.

[0104] (7) The filtrate and the extract obtained in step (6) are mixed and extracted to obtain an organic phase loaded with vanadium.

[0105] In addition, a raffinate is also produced during the extraction. In order to make full use of resources, the water that has been neutralized and subjected to impurity removal can be used as the water used for leaching in step (3) or the water added to the vanadium ore in step (1).

[0106] Here, the extract contains the following weight parts of raw materials: 18 parts of extractant, 7 parts of tributyl phosphate, and 86 parts of sulfonated kerosene. The extractant is N235. The volume ratio of the filtrate to the extract is 1:0.2.

[0107] (8) The vanadium-loaded organic phase obtained in step (7) is washed with a sulfuric acid solution having a pH value of 2.0, and then back-extracted with a 2.5 mol / L sulfuric acid solution to obtain a back-extracted solution.

[0108] Here, the volume ratio of the sulfuric acid solution having a pH value of 2.0 to the organic phase carrying the vanadium was 5:1.

[0109] The volume ratio of the 2.5 mol / L sulfuric acid solution to the vanadium-loaded organic phase was 0.05:1.

[0110] In order to realize efficient utilization of resources, the water washed with the sulfuric acid solution can be used as the water used for leaching in step (3).

[0111] (9) The stripped solution obtained in step (8) is subjected to diffusion dialysis, and the sulfuric acid solution is recovered through a diffusion dialysis membrane to obtain a dialysate. The dialysate is then extracted and stripped to obtain a secondary stripped solution. The secondary stripped solution is then passed through an activated carbon adsorption column to remove the organic phase, and a vanadium electrolyte solution is obtained.

[0112] In order to obtain a vanadium electrolyte solution of an appropriate concentration, water and / or a sulfuric acid solution may be added to the vanadium electrolyte solution, and the vanadium ion concentration in the vanadium electrolyte solution is adjusted to 1.3 mol / L, and the sulfate ion concentration is adjusted to 4.2 mol / L. Here, the mass concentration of the sulfuric acid solution is 94%.

[0113] In the diffusion dialysis, the flow rate of the stripping solution is 0.15×10 -3 m 3 / (hm 2 ) and the flow rate ratio of water to the stripping solution is 0.5:1.

[0114] In order to realize efficient utilization of resources, the sulfuric acid solution recovered through the diffusion dialysis membrane can be used for the water or sulfuric acid solution added in step (1).

[0115] Example 3 The method for producing the vanadium electrolyte of this embodiment includes the following steps.

[0116] (1) Take vanadium ore and crush it into powder with a particle size of less than 2 mm and a particle size of 1 to 2 mm in the range of 50% or more by mass. Add water to the vanadium ore and then add 5 mL min -1·g -1 A sulfuric acid solution having a mass concentration of 98% is added at a rate of 0.01 to 0.01 and mixed uniformly at 90° C. to obtain a mixture.

[0117] Here, the mass ratio of the water to the vanadium ore is 0.1:1, and the mass ratio of the sulfuric acid solution to the vanadium ore is 1:20.

[0118] (2) maturing the mixture obtained in step (1) to obtain a maturated material, and crushing the maturated material to a particle size of less than 5 mm.

[0119] Here, the aging is carried out in a moist environment, the aging temperature is 85° C., and the aging time is longer than 12 hours.

[0120] (3) The aged material obtained in step (2) is leached with water at 90° C. to obtain a vanadium-containing leachate.

[0121] Here, the mass ratio of water to the aging material is 2.5: 1. The vanadium-containing leachate can be obtained by solid-liquid separation. After solid-liquid separation, the vanadium-containing leachate and leach residue are obtained.

[0122] (4) First, adjust the pH value of the vanadium-containing leachate obtained in step (3) to 2.0, then add a first impurity removing agent to the vanadium-containing leachate to carry out an impurity removing reaction at 47°C, and filter the reaction liquid to obtain a first purified liquid.

[0123] Here, the first impurity removing agent is sodium hexafluorophosphate. The molar ratio of the first impurity removing agent to aluminum ions in the vanadium-containing leachate is 10:1. Aluminum ions are removed by the first impurity removing agent to obtain sodium hexafluoroaluminate, which is cryolite.

[0124] In a preferred embodiment of this embodiment, the pH value of the vanadium-containing leachate obtained in step (3) is adjusted to 2.0, and the vanadium ore obtained in step (1) is used. After adjusting the pH value to 2.0, the vanadium-containing leachate and the wet ore are obtained by solid-liquid separation. In addition, as an alternative embodiment of this embodiment, a chemical reagent may be used to adjust the pH value of the vanadium-containing leachate obtained in step (3) to 2.0.

[0125] In order to facilitate efficient utilization of resources, the vanadium ore of step (1) may be mixed with the wet ore produced in step (4).

[0126] (5) An oxidizing agent is added to the first purified liquid obtained in step (4), and the pH value of the first purified liquid is adjusted to 1.5. Then, iron phosphate dihydrate seed crystals and a second impurity removing agent are added thereto, and an impurity removing reaction is carried out at 45°C. The resulting reaction liquid is filtered to obtain a second purified liquid.

[0127] Here, the oxidizing agent is hydrogen peroxide, and the molar ratio of the oxidizing agent to the divalent iron ions in the first purification liquid is 1:1.

[0128] The second impurity removing agent is potassium phosphate. The molar ratio of the second impurity removing agent to the iron ions in the first purified liquid is 0.5:1. The iron ions are removed by the second impurity removing agent to obtain iron phosphate.

[0129] The molar ratio of the iron phosphate dihydrate seed crystals to the iron ions in the first purification solution is 0.01:1.

[0130] (6) A reducing agent is added to the second purified liquid obtained in step (5) to reduce the pentavalent vanadium in the second purified liquid to tetravalent vanadium, and the pH value of the second purified liquid is adjusted to 2.0, and then a coagulant is added thereto, and the mixture is stirred for 1 hour to react, and then filtered using an ultrafiltration membrane to obtain a filtrate.

[0131] Here, the reducing agent is a mixture of elemental sulfur and zinc powder in a weight ratio of 1: 1. The molar ratio of the reducing agent to the pentavalent vanadium ions in the second purification liquid is 2:1.

[0132] The flocculant is polyacrylamide, and the molar ratio of the flocculant to the vanadium ions in the second purification liquid is 0.05:1.

[0133] (7) The filtrate and the extract obtained in step (6) are mixed and extracted to obtain an organic phase loaded with vanadium.

[0134] In addition, a raffinate is also produced during the extraction. In order to make full use of resources, the water that has been neutralized and subjected to impurity removal can be used as the water used for leaching in step (3) or the water added to the vanadium ore in step (1).

[0135] Here, the extract contains the following parts by weight of raw materials: 10 parts of extractant, 10 parts of tributyl phosphate, and 76 parts of sulfonated kerosene. The extractant is a mixture of P204, N235, and P507 in a weight ratio of 1:3:1. The volume ratio of the filtrate to the extract is 1:1.

[0136] (8) The vanadium-loaded organic phase obtained in step (7) is washed with a sulfuric acid solution having a pH value of 1.8, and then back-extracted with a 1.5 mol / L sulfuric acid solution to obtain a back-extracted solution.

[0137] Here, the volume ratio of the sulfuric acid solution having a pH value of 1.8 to the organic phase carrying the vanadium was 2.7:1.

[0138] The volume ratio of the 1.5 mol / L sulfuric acid solution to the vanadium-loaded organic phase was 0.6:1.

[0139] In order to realize efficient utilization of resources, the water washed with the sulfuric acid solution can be used as the water used for leaching in step (3).

[0140] (9) The stripped solution obtained in step (8) is subjected to diffusion dialysis, and the sulfuric acid solution is recovered through a diffusion dialysis membrane to obtain a dialysate. The dialysate is then extracted and stripped to obtain a secondary stripped solution. The secondary stripped solution is then passed through an activated carbon adsorption column to remove the organic phase, and a vanadium electrolyte solution is obtained.

[0141] In order to obtain a vanadium electrolyte solution of an appropriate concentration, water and / or a sulfuric acid solution may be added to the vanadium electrolyte solution, and the vanadium ion concentration in the vanadium electrolyte solution is adjusted to 1.5 mol / L, and the sulfate ion concentration is adjusted to 4.0 mol / L, where the mass concentration of the sulfuric acid solution is 90%.

[0142] In the diffusion dialysis, the flow rate of the stripping solution is 0.22×10 -3 m 3 / (hm 2 ) and the flow rate ratio of water to the stripping solution is 1.5:1.

[0143] In order to realize efficient utilization of resources, the sulfuric acid solution recovered through the diffusion dialysis membrane can be used for the water or sulfuric acid solution added in step (1).

[0144] Example 4 This embodiment employs the same method for producing a vanadium electrolyte as in Example 1, except that secondary extraction and stripping are not performed in step (9).

[0145] In this embodiment, step (9) specifically includes: subjecting the stripped solution obtained in step (8) to diffusion dialysis, passing through a diffusion dialysis membrane to recover a sulfuric acid solution, thereby obtaining a dialysate; and then passing the obtained dialysate through an activated carbon adsorption column to remove an organic phase, thereby obtaining a vanadium electrolyte solution.

[0146] Example 5 In this embodiment, the vanadium ore in step (1) is mixed with the wet mineral material produced in step (4) to form a vanadium ore mixture, and the mass ratio of the water to the vanadium ore and the mass ratio of the sulfuric acid to the vanadium ore mixture are changed, and the same method for producing the vanadium electrolyte as in Example 1 is adopted.

[0147] In this embodiment, step (1) specifically includes the following steps: taking vanadium ore, crushing the vanadium ore into powder having a particle size of less than 2 mm and a particle size of 1 to 2 mm, and the mass of vanadium ore being 50% or more; mixing the crushed vanadium ore with the wet ore produced in step (4) in a mass ratio of 1:2.5 to obtain a vanadium ore mixture; adding water to the vanadium ore mixture, and then adding 0.05 mL min -1 ·g -1 and mixing the mixture uniformly at 50° C. to obtain a mixture.

[0148] Here, the mass ratio of the water to the vanadium ore mixture is 0.001:1, and the mass ratio of the sulfuric acid solution to the vanadium ore mixture is 1:13.

[0149] Example 6 In this embodiment, the vanadium ore in step (1) is mixed with the wet ore material produced in step (4) to form a vanadium ore mixture, and the water added is replaced with the sulfuric acid solution recovered by the counter-diffusion dialysis membrane in step (9), and the mass ratio of the sulfuric acid solution with a mass concentration of 90% to the vanadium ore is changed. The same vanadium electrolyte manufacturing method as in Example 1 is adopted, except that.

[0150] In this embodiment, step (1) specifically includes the steps of: taking vanadium ore, crushing the vanadium ore into powder having a particle size of less than 2 mm and a particle size of 1 to 2 mm, and the vanadium ore having a particle size of 50% or more by mass; mixing the crushed vanadium ore with the wet ore produced in step (4) in a mass ratio of 1:0.6 to obtain a vanadium ore mixture; and adding 0.05 mL min of the sulfuric acid solution recovered by the counter-current diffusion dialysis membrane in step (9) to the vanadium ore mixture. -1 ·g -1 and mixing the mixture uniformly at 50° C. to obtain a mixture.

[0151] Here, the sulfuric acid solution recovered by the countercurrent diffusion dialysis membrane has a concentration of 1.1 mol / L and a mass ratio of the vanadium ore mixture to the sulfuric acid solution having a mass concentration of 90% is 1:14.

[0152] By adding the sulfuric acid solution recovered by the counter-current diffusion dialysis membrane in step (9), the step of adding water can be replaced, while the amount of sulfuric acid solution having a mass concentration of 90% can be reduced.

[0153] Comparative Example In order to verify the technical effect of the method for producing vanadium electrolyte according to the present invention, the following tests are carried out.

[0154] The vanadium electrolytes obtained in Examples 1 to 4 and Comparative Examples 1 to 3 are inspected according to the method specified in GB / T 37204-2018 "Electrolyte for all-vanadium redox flow battery" to measure the components of the vanadium electrolytes.

[0155] The results of the experiment are as follows: [Table 1] [Table 2] [Table 3] [Table 4] [Table 5] [Table 6]

[0156] In the above examples, as can be seen from Example 4, when extraction is performed only once, some impurity ions in the electrolyte are difficult to meet the GB / T 37204-2018 "electrolyte for all-vanadium redox flow battery" standard requirements, while in the remaining examples, all impurity ions meet the first-class requirements in the GB / T 37204-2018 "electrolyte for all-vanadium redox flow battery" standard, and there is no obvious difference. In Examples 5-6, the amount of acid and water used for aging is reduced to a certain extent in meeting the first-class requirements in the GB / T 37204-2018 "electrolyte for all-vanadium redox flow battery" standard, and the amount of sulfuric acid solution with a mass concentration of 90% is significantly reduced compared with Example 1, thus better realizing resource utilization.

[0157] As is known from a technical common sense, the present invention can be realized by other embodiments that do not deviate from the spirit or essential characteristics of the present invention. Therefore, the above disclosed embodiments are merely illustrative in each respect and are not exclusive. All modifications within the scope of the present invention or within the scope equivalent to the present invention are included in the present invention.

Claims

1. A method for producing a vanadium electrolyte, comprising the steps of: (1) taking vanadium ore, adding sulfuric acid thereto, and mixing uniformly to obtain a mixture; (2) aging the mixture obtained in step (1) to obtain an aged material, the aging temperature is 40-130° C., and the aging time is longer than 12 hours; (3) leaching the aged material obtained in step (2) with water to obtain a vanadium-containing leachate; (4) adding a first impurity removing agent to the vanadium-containing leachate obtained in step (3) to obtain a first purified solution; (5) adding an oxidizing agent, iron phosphate dihydrate seed crystals, and a second impurity removing agent to the first purified solution obtained in step (4) to obtain a second purified solution; (6) adding a reducing agent and a flocculant to the second purified liquid obtained in step (5), and filtering the liquid to obtain a filtrate; (7) mixing the filtrate and the extract obtained in step (6) and extracting to obtain an organic phase loaded with vanadium; (8) stripping the vanadium-loaded organic phase obtained in step (7) to obtain a stripped solution; (9) removing the organic phase from the stripped solution obtained in step (8) to obtain a vanadium electrolyte solution; A method for producing a vanadium electrolyte solution, comprising:

2. In step (1), the sulfuric acid is a sulfuric acid solution having a mass concentration of 90 to 98%, The mass ratio of the sulfuric acid to the vanadium ore is 1:(4-20); 2. The method for producing a vanadium electrolyte solution according to claim 1, wherein water is added before the addition of the sulfuric acid.

3. In step (4), the pH value of the vanadium-containing leachate is first adjusted to 1.0-2.0, and then a first impurity removing agent is added; 2. The method for producing a vanadium electrolyte solution according to claim 1, wherein the first impurity remover is one or more of sodium fluoride, potassium fluoride, ammonium fluoride, lithium fluoride, hydrofluoric acid, sodium hexafluorophosphate, and potassium hexafluorophosphate.

4. In step (5), the oxidizing agent is one or more of sodium chlorate, sodium hypochlorite, and hydrogen peroxide; 2. The method for producing a vanadium electrolyte according to claim 1, wherein the second impurity remover is one or more of phosphoric acid, sodium phosphate, disodium hydrogen phosphate, monosodium hydrogen phosphate, potassium phosphate, dipotassium hydrogen phosphate, monopotassium hydrogen phosphate, and ammonium hydrogen phosphate.

5. In step (6), the reducing agent is one or more of sulfite, sulfur dioxide, elemental sulfur, zinc powder, organic sulfur compounds, oxalates, ascorbic acid, and carbon monoxide; 2. The method for producing a vanadium electrolyte solution according to claim 1, wherein the flocculant is one or more of polyacrylamide and sodium polyacrylate.

6. 2. The method for producing vanadium electrolyte according to claim 1, wherein in step (7), the extracting solution is a mixture of an extractant, tributyl phosphate, and sulfonated kerosene, and the extracting solution is one or more of P204, N235, and P507.

7. Step (9) specifically includes: subjecting the stripped solution to diffusion dialysis to obtain a dialysate; then extracting and stripping the dialysate to obtain a secondary stripped solution; Then, the secondary stripped solution is passed through an activated carbon adsorption column to remove the organic phase, thereby obtaining a vanadium electrolyte solution.

2. The method for producing a vanadium electrolyte solution according to claim 1, further comprising:

Citation Information

Patent Citations

  • Recovery method of vanadium-containing neutralizing slag

    CN109666796A

  • Method for directly preparing vanadium electrolyte from stone coal vanadium ore

    CN112843786A

  • Process for extracting high-purity vanadium pentoxide from stone coal vanadium ore

    CN114262808A

  • Vanadium extraction from disparate shale ores

    WO2021146797A1