Plasma etching method, plasma etching apparatus, and method for manufacturing element chip

The plasma etching method alternates power levels to monitor emission intensity, ensuring precise silicon layer etching completion, enhancing accuracy and efficiency in plasma etching processes.

JP7580046B2Active Publication Date: 2024-11-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021006540
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-19
Publication Date
2024-11-11
Estimated Expiration
2041-01-19

AI Technical Summary

Technical Problem

Existing plasma etching methods struggle with accurately detecting the end point of silicon layer etching, leading to unnecessary etching of unintended areas due to time delays in gas supply adjustments and plasma stabilization.

Method used

A plasma etching method that alternates between high and low power etching steps to monitor plasma emission intensity, allowing for precise detection of the silicon layer completion, using a plasma etching apparatus with optical measurement and control units to manage the process.

Benefits of technology

Enables rapid and accurate determination of the etching end point, preventing over-etching and maintaining efficient etching rates while minimizing defects like notching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580046000001
    Figure 0007580046000001
  • Figure 0007580046000002
    Figure 0007580046000002
  • Figure 0007580046000003
    Figure 0007580046000003
Patent Text Reader

Abstract

To provide a plasma etching method by which an end point of silicon layer etching can be sensed appropriately and easily.SOLUTION: A method disclosed herein comprises an etching process for etching a part of a silicon layer 11. The etching process is performed by repeating a group of steps including a silicon layer-etching step of forming a concave portion 11v, a protection film-forming step of forming a protection film 21 and a protection film-etching step of removing the protection film 21 located on a bottom of the concave portion 11v in this order. At least one step of the silicon layer-etching step and the protection film-etching step includes: an etching step (x); and an etching step (y) of plasma etching by high-frequency electric power smaller than that in the etching step (x). The judgment about whether the etching of the silicon layer 11 is completed is performed on a plasma light emission intensity in the at least one step.SELECTED DRAWING: Figure 2F
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a plasma etching method, a plasma etching apparatus, and a method for manufacturing element chips. [Background technology]

[0002] Conventionally, the so-called Bosch process has been used as a method for dividing a silicon layer (e.g., a silicon substrate) by deep digging using plasma etching. In the Bosch process, a step of etching a part of a silicon layer to form a recess, a step of forming a protective film on the surface of the recess, and a step of removing a part of the protective film are repeated multiple times in this order.

[0003] If plasma etching is continued after the division of the silicon layer is completed, the etching will proceed in the in-plane direction, resulting in etching of areas that should not be etched (notching). Therefore, it is important to detect the completion of the division of the silicon layer and terminate the plasma etching at the appropriate time.

[0004] Patent Document 1 (JP Patent Publication 2008-53678 A) discloses "a method for etching a Si film of a silicon substrate having a Si film formed on a surface side and an underlayer film formed under the Si film, the method being a plasma etching method for supplying an etching gas containing SF6 gas, generating plasma to etch the Si film, the method comprising repeating at least two steps of a large-amount supply step of supplying a large amount of SF6 gas for treatment, and then a small-amount supply step of reducing the supply amount and supplying a small amount of SF6 gas for treatment, and measuring the emission intensity of Si or SiFx in the plasma in the small-amount supply step, and determining that the etching has ended when the measured emission intensity becomes equal to or less than a preset reference value, thereby terminating the treatment." [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2008-53678 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the method of Patent Document 1, the gas supply amount is changed to detect the end point. However, in the method of changing the gas supply amount, it may take time to open and close the valve that adjusts the gas supply amount, and it may take time for the pressure and plasma density in the chamber to stabilize even after the gas supply amount is switched. Therefore, there is a problem that the end point detection cannot be started immediately. Currently, there is a demand for a plasma etching method that can appropriately and easily detect the end point of etching of a silicon layer. One of the objectives of the present disclosure is to provide such a method. [Means for solving the problem]

[0007] One aspect of the present disclosure relates to a plasma etching method for etching a substrate including a silicon layer by plasma etching using plasma, the plasma etching method including an etching step of etching a part of the silicon layer until the silicon layer is penetrated, the etching step being performed by repeating a group of steps including, in this order, a silicon layer etching step of plasma-etching the part of the silicon layer to form a recess in the silicon layer, a protective film forming step of forming a protective film inside the recess, and a protective film etching step of removing the protective film present at the bottom of the recess by plasma etching, at least one step selected from the group consisting of the silicon layer etching step and the protective film etching step includes an etching step (x) of generating the plasma by high frequency power and performing plasma etching, and an etching step (y) of generating the plasma by high frequency power smaller than the high frequency power applied in the etching step (x), and a determination of whether the recess has penetrated the silicon layer and etching of the silicon layer has been completed is performed based on the emission intensity of the plasma in the at least one step.

[0008] Another aspect of the present disclosure relates to a plasma etching apparatus, the plasma etching apparatus including a chamber having a gas inlet in which a substrate is placed, an electrode for generating plasma in the chamber, a light measuring unit for measuring the emission intensity of the plasma, and a control unit, the control unit performing an etching process for etching a part of the silicon layer until the silicon layer is penetrated when etching a substrate including a silicon layer by plasma etching using the plasma, the etching process including a silicon layer etching step for plasma etching the part of the silicon layer to form a recess in the silicon layer, a protective film forming step for forming a protective film on the inside of the recess, and a protective film forming step for plasma etching the protective film present at the bottom of the recess. and a protective film etching step of removing the silicon layer by etching the protective film by etching the silicon layer, in this order, wherein at least one step selected from the group consisting of the silicon layer etching step and the protective film etching step includes an etching step (x) of generating the plasma by high-frequency power and performing plasma etching, and an etching step (y) of generating the plasma by high-frequency power smaller than the high-frequency power applied in the etching step (x), and the control unit determines whether or not the recess has penetrated the silicon layer and etching of the silicon layer has been completed based on the emission intensity of the plasma in the at least one step.

[0009] Another aspect of the present disclosure relates to a method for manufacturing an element chip using a substrate including a silicon layer, the method including an etching step of etching a part of the silicon layer by plasma etching using plasma until the silicon layer is penetrated, the etching step being performed by repeating a group of steps including, in this order, a silicon layer etching step of plasma-etching the part of the silicon layer to form a recess in the silicon layer, a protective film forming step of forming a protective film inside the recess, and a protective film etching step of removing the protective film present at the bottom of the recess by plasma etching, at least one step selected from the group consisting of the silicon layer etching step and the protective film etching step includes an etching step (x) of generating the plasma by high frequency power and performing plasma etching, and an etching step (y) of generating the plasma by high frequency power smaller than the high frequency power and performing plasma etching, and a determination of whether the recess has penetrated the silicon layer and etching of the silicon layer has been completed is performed based on the emission intensity of the plasma in the at least one step. Effect of the Invention

[0010] According to the present disclosure, the etching end point of a silicon layer can be appropriately and simply detected. [Brief description of the drawings]

[0011] [Figure 1] 1 is a diagram illustrating an example of a configuration of a plasma etching apparatus according to the present disclosure. [Figure 2A] 1 is a cross-sectional view showing a step of an example of a plasma etching method of the present disclosure. [Figure 2B] FIG. 2B is a cross-sectional view showing an example of a step subsequent to FIG. 2A. [Figure 2C] FIG. 2C is a cross-sectional view showing an example of a step subsequent to FIG. 2B. [Figure 2D] FIG. 2D is a cross-sectional view showing an example of a step subsequent to FIG. 2C. [Figure 2E]FIG. 2E is a cross-sectional view showing an example of a step subsequent to FIG. 2D. [Figure 2F] FIG. 2C is a cross-sectional view showing an example of a step subsequent to FIG. 2E. [Figure 2G] FIG. 2C is a cross-sectional view showing an example of a step subsequent to FIG. 2F. [Figure 2H] FIG. 11 is a cross-sectional view showing an example of a state where excessive etching has been performed. [Diagram 3] 1 is a flow chart showing an example of a silicon layer etching step in the plasma etching method of the present disclosure. [Figure 4] 1 is a graph showing the results of an example of the method of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In the following, the embodiment of the present disclosure will be described with examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​and materials may be exemplified, but other numerical values ​​and materials may be applied as long as the effects of the present disclosure can be obtained. In this specification, when a "range of numerical value A to numerical value B" is mentioned, the range includes numerical value A and numerical value B.

[0013] (Plasma Etching Method) The plasma etching method according to the present disclosure is a method for etching a substrate including a silicon layer by plasma etching using plasma. Hereinafter, the plasma etching method may be referred to as an etching method (EM).

[0014] The substrate including the silicon layer may be a silicon substrate, or may be a substrate including a silicon layer and another layer. For example, the substrate may be a substrate including a silicon layer on a glass layer. For example, the substrate may be a substrate that is divided into a plurality of element chips. Such a substrate may include a silicon layer and an element layer in which elements are formed, and may further include a wiring layer, etc.

[0015] The substrate including the silicon layer may include a layer (e.g., a silicon oxide layer, etc.) disposed on the side opposite to the side where plasma etching is initiated. The substrate may be disposed on a film or the like and plasma etched. Examples of such films include sheets called dicing tape and die attach film. Hereinafter, the layer or film present on the main surface opposite to the side where plasma etching is initiated of the two main surfaces of the silicon layer may be referred to as an "underlayer". The underlayer is a layer made of a material other than the silicon layer.

[0016] The etching method (EM) includes an etching step of etching a part of the silicon layer until the silicon layer is penetrated. The etching step may be referred to as an "etching step (E)" below. The etching step (E) is performed by repeating a step group including, in this order, a silicon layer etching step of forming a recess in the silicon layer by plasma etching a part of the silicon layer, a protective film forming step of forming a protective film inside the recess, and a protective film etching step of removing the protective film present at the bottom of the recess by plasma etching. That is, the etching step (E) includes a step group that is repeated multiple times. Each step group includes, in this order, a silicon layer etching step, a protective film forming step, and a protective film etching step. By repeating the step groups, the recess in the silicon layer is deepened and the silicon layer is penetrated. Hereinafter, the number of times the step group is repeated may be referred to as a "cycle number".

[0017] Etching of a portion of the silicon layer can be carried out, for example, by covering the remaining portion with a resist film, which may be a known resist film (for example, a photoresist film).

[0018] The above steps may be applied under conditions used in the known Bosch process or may be applied with modifications of the conditions, but the above steps are different from the known process in that they have the following feature (1). (1) At least one step selected from the group consisting of a silicon layer etching step and a protective film etching step includes an etching step (x) and an etching step (y).

[0019] Hereinafter, the at least one step may be referred to as an “etching step (S).” Either the silicon layer etching step or the protective film etching may be the etching step (S), or both of them may be the etching step (S).

[0020] The etching step (x) is an etching step in which plasma is generated by high frequency power to perform plasma etching, and the etching step (y) is an etching step in which plasma is generated by applying a high frequency power HPy that is smaller than the high frequency power HPx applied in the etching step (x) to perform plasma etching.

[0021] When the silicon layer etching step is the etching step (S), the silicon layer is etched in the etching steps (x) and (y). When the protective film etching step is the etching step (S), the protective film is etched in the etching steps (x) and (y), but when the protective film is etched to expose the silicon layer, the silicon layer is etched.

[0022] HPy (unit: W) is smaller than HPx (unit: W), and may be, for example, in the range of 0.1 to 0.5 times HPx (for example, in the range of 0.2 to 0.5 times). By setting it in this range, the etching end point can be appropriately determined without excessively slowing down the etching rate. There is no particular limitation on HPx, and it may be set appropriately depending on the size of the chamber, the pressure inside the chamber, and the like. In one example, HPx may be in the range of 2000 to 5000 W.

[0023] In this specification, "generating plasma by high frequency power" means generating plasma by applying high frequency power to an electrode for generating plasma. More specifically, it means generating plasma by applying high frequency power to an electrode for turning a specific gas into plasma in a state where a substrate to be etched is placed in a chamber. By applying high frequency power to the electrode, the gas in the chamber is excited to generate plasma. In the etching step, a gas for etching is introduced into the chamber. In the protective film forming step, a gas for forming the protective film is introduced into the chamber.

[0024] There is no particular limitation on the time for the etching step (x) and the etching step (y), and the time may be set in consideration of the depth of the recess formed by them. The etching step (x) and the etching step (y) may each be performed independently for only 1 to 10 seconds. The time Tx for which the etching step (x) is performed may be in the range of 2 to 5 times the time Ty for which the etching step (y) is performed. It is preferable that the time Tx is longer than the time Ty, since the etching rate of the etching step (x) is higher and the total time required for the etching process can be shortened.

[0025] In the etching method (EM), whether or not the etching of the silicon layer is completed with the recess penetrating the silicon layer is determined based on the emission intensity of the plasma in the etching step (S). When the recess penetrates the silicon layer and reaches the underlayer, the type and / or composition ratio of the substances released into the plasma by the plasma etching changes. As a result, the type and / or composition ratio of the substances emitting light in the plasma changes, which changes the emission spectrum of the plasma. From this change in the emission spectrum, it is possible to determine whether or not the etching of the silicon layer is completed. The etching may be terminated when it is determined that the recess penetrates the silicon layer. Alternatively, the etching may be terminated after it is determined that a substantially vertical through groove is formed. That is, the etching may be continued for a certain period of time after the recess penetrates the silicon layer.

[0026] The type of change in the emission intensity that indicates the end point of etching may be determined depending on the structure of the substrate and the etching conditions. When the recess does not penetrate the silicon layer, the silicon layer is etched to generate a product containing Si (hereinafter, may be referred to as a "Si-containing product"). When the recess penetrates the silicon layer and reaches the underlayer, the amount of silicon layer etched per unit time decreases, and the emission intensity originating from the Si-containing product decreases. Therefore, the decrease in the emission intensity originating from the silicon-containing product may be considered as the change that indicates the end point of etching. Alternatively, the increase after the decrease in the emission intensity originating from the silicon-containing product may be considered as the change that indicates the end point of etching.

[0027] In addition, for the determination based on the emission intensity, the average value of the emission intensity in the etching step (x) and / or the etching step (y) may be used, or a value other than the average value (for example, the maximum value or an integrated value) may be used.

[0028] In etching a recess, the intensity of the luminescence originating from the products (Si-containing products) released from the etched silicon layer is not very high. Also, the intensity of the luminescence originating from other substances (e.g., gas for generating plasma) is high. Therefore, when plasma etching is performed under normal conditions, it is difficult to detect the luminescence of the Si-containing products.

[0029] The present inventors have found that the ratio of (intensity of light emitted from Si-containing products) / (intensity of other light emitted from other sources) can be increased by reducing the high-frequency power applied to generate plasma. The present disclosure is based on this new finding.

[0030] On the other hand, if the applied high frequency power is reduced, the etching rate decreases. Therefore, in the etching method (EM), etching is performed by an etching step (S) including an etching step (x) in which high frequency power is applied and an etching step (y) in which a low frequency power is applied compared to the etching step (x). This makes it easier to properly detect the end point of etching and maintain a sufficient etching rate.

[0031] Usually, in the initial step group, the recess does not penetrate the silicon layer. Therefore, in the initial step group, only the etching step (x) may be performed in the etching step (S) without performing the etching step (y). For example, in the etching step (S), only the etching step (x) may be performed without performing the etching step (y) until the cycle number at which the depth of the recess is expected to reach a range of 0 to 90% of the thickness of the silicon layer. According to this configuration, the processing time can be shortened and the end point of the etching can be appropriately determined. Even in this configuration, in the step group where the recess is expected to penetrate the silicon layer, the etching step (x) and the etching step (y) are performed in the etching step (S).

[0032] In the etching method (EM), the apparatus (D) described later, and the manufacturing method (PM) described later, in at least one of the steps (etching step (S)), the etching step (x) may be performed after the etching step (y), or the etching step (y) may be performed after the etching step (x).

[0033] Typically, one etching step (S) is composed of one etching step (x) and one etching step (y). However, one etching step (S) may include multiple etching steps (x) or multiple etching steps (y). In either case, the etching steps (x) and the etching steps (y) are performed alternately.

[0034] In the etching method (EM), the apparatus (D), and the manufacturing method (PM), the above judgment may be made based on the emission intensity of the plasma in the etching step (y). As described above, this configuration allows more accurate end point detection. By performing the etching step (x) after the etching step (y) and making the above judgment in the etching step (y), it is possible to prevent excessive etching. Alternatively, the above judgment may be made based on both the emission intensity of the plasma in the etching step (x) and the emission intensity of the plasma in the etching step (y).

[0035] The etching of the silicon layer is more often completed in the silicon layer etching step than in the protective film forming step. Therefore, in the etching method (EM), the apparatus (D), and the manufacturing method (PM), at least one etching step (S) preferably includes a silicon layer etching step, and may be a silicon layer etching step.

[0036] In the etching method (EM), the apparatus (D), and the manufacturing method (PM), either one or both of the following (a) and (b) may be satisfied. (a) In the silicon layer etching step, an etching gas containing SF6 gas is used. (b) The above determination is based on the presence of Si and / or SiF in the plasma. x This is based on the emission intensity.

[0037] In the etching method (EM), the apparatus (D), and the manufacturing method (PM), the aperture ratio of the recess may be 40% or less (e.g., 10% or less, 5% or less, or 1% or less). There is no particular limit to the lower limit of the aperture ratio, but the aperture ratio may be 0.5% or more. In this specification, the aperture ratio means the ratio of the area of ​​the opening of the recess to the area of ​​the surface of the silicon layer (the surface on which the recess is formed). When the aperture ratio is small, it becomes particularly difficult to determine whether the recess has penetrated the silicon layer (detecting the end point). Therefore, when the aperture ratio is 1% or less, the method of the present disclosure is particularly effective.

[0038] (Plasma Etching Equipment) The apparatus of the present disclosure is a plasma etching apparatus. Hereinafter, the plasma etching apparatus of the present disclosure may be referred to as an apparatus (D). In the apparatus (D), the above-mentioned etching method (EM) is executed. The matters described for the etching method (EM) are applicable to the apparatus (D), so duplicated explanations will be omitted. In addition, the matters described for the apparatus (D) are applicable to the etching method.

[0039] The apparatus (D) includes a chamber having a gas inlet in which a substrate is placed, an electrode for generating plasma in the chamber, a light measuring unit for measuring the emission intensity of the plasma, and a control unit. The apparatus (D) further includes components necessary for performing etching. Examples of components that the apparatus (D) may include include a high-frequency power source necessary for generating plasma, a pressure reducing device for reducing the pressure inside the chamber, and a mass flow controller for controlling the flow rate of gas introduced into the chamber.

[0040] The control unit performs an etching step of etching a part of the silicon layer until the silicon layer is penetrated when etching a substrate including a silicon layer by plasma etching using plasma. Since this etching step is the same as the etching step (E) described above, it may be referred to as the etching step (E) below. As described above, the etching step (E) is performed by repeating a step group including a silicon layer etching step, a protective film forming step, and a pre-protective film etching step in this order. That is, the control unit performs control so that such an etching step (E) is performed.

[0041] As described above, at least one etching step (S) selected from the group consisting of a silicon layer etching step and a protective film etching step includes an etching step (x) and an etching step (y).The control unit determines whether the recess penetrates the silicon layer and etching of the silicon layer is completed based on the emission intensity of the plasma in the etching step (S).The device (D) can provide the same effects as those described for the etching method (EM).

[0042] The control unit includes a calculation processing unit and a storage device. Known calculation processing units and storage devices can be used. However, the storage device stores a program for controlling the device (D) to perform each step and a program for making the above-mentioned judgment.

[0043] The components other than the control unit may be those of a known plasma etching device. For example, the measurement unit that measures the emission intensity of the plasma may be the same as a measurement device used in a known inductively coupled plasma optical emission spectrometer (ICP optical emission spectrometer).

[0044] (Method of manufacturing element chip) The manufacturing method disclosed herein is a method for manufacturing an element chip, and is a manufacturing method that uses a substrate including a silicon layer. This manufacturing method may be referred to hereinafter as the "manufacturing method (PM)." The manufacturing method (PM) may be implemented using the etching method (EM) described above. Since matters explained regarding the etching method (EM) are applicable to the manufacturing method (PM), duplicated explanations may be omitted. Furthermore, matters explained regarding the manufacturing method (PM) are applicable to the etching method (EM).

[0045] The manufacturing method (PM) includes an etching step of etching a part of the silicon layer by plasma etching using plasma until the silicon layer is penetrated. Since this etching step is the same as the above-mentioned etching step (E), it may be referred to as the etching step (E) below. As described above, the etching step (E) is performed by repeating a step group including, in this order, a silicon layer etching step, a protective film forming step, and a protective film etching step.

[0046] As described above, at least one etching step (S) selected from the group consisting of a silicon layer etching step and a protective film etching step includes an etching step (x) and an etching step (y). Whether or not the recess penetrates the silicon layer and etching of the silicon layer is completed is determined based on the emission intensity of the plasma in the etching step (S). According to the manufacturing method (PM), the same effects as those described for the etching method (EM) can be obtained.

[0047] An example of a substrate used in the manufacturing method (PM) includes a silicon layer and a device region layer formed on the silicon layer. The device region layer includes a plurality of device regions. Each device region corresponds to a device region included in one device chip. The device chip can be obtained by dividing the silicon layer so that each device region is divided. The division of the silicon layer is performed by the etching step (E) described above.

[0048] The substrate may include layers other than the silicon layer and the element region layer. For example, the substrate may include a wiring layer. When dividing the substrate, layers other than the silicon layer may be removed by an etching step other than the etching step (E).

[0049] Hereinafter, examples of embodiments according to the present disclosure will be specifically described with reference to the drawings. The above-mentioned components can be applied to the components of the method and device described below. In addition, the method and device described below can be modified based on the above description. In addition, the matters described below may be applied to the above-mentioned embodiments. In addition, in the embodiments described below, components that are not essential to the method and device of the present disclosure may be omitted.

[0050] (Embodiment 1)

[0051] In the first embodiment, an example of an etching method (EM), an etching apparatus (D), and a manufacturing method for element chips (PM) according to the present disclosure will be described.

[0052] An example of the apparatus used in the first embodiment is shown in FIG. 1. The apparatus 100 of the first embodiment includes a chamber 110, a first electrode 121, a first high frequency power supply 122, a first matching circuit 123, a substrate stage 131, a second high frequency power supply 132, a second matching circuit 133, a pressure reducing device 141, a gas flow control unit 150, a light measuring unit 161, a control unit 170, and a pressure gauge (not shown). The control unit 170 is connected to devices that need to be controlled, and performs the control required for plasma etching. In FIG. 1, the illustration of a part of the connection between the control unit 170 and the devices is omitted. Since known devices can be applied to the devices included in the apparatus 100, detailed explanations are omitted. In addition, as long as the method of the present invention can be implemented, these devices and configurations (including arrangement) can be changed.

[0053] The chamber 110 is a chamber capable of maintaining the inside in a reduced pressure state. The chamber 110 includes a gas inlet 110a, a gas exhaust port 110b, a dielectric window 111, and an observation window 112. The dielectric window 111 is formed of a dielectric material (e.g., aluminum nitride, alumina, quartz, etc.). A first electrode 121 is disposed adjacent to the dielectric window 111. The observation window 112 transmits light detected by the light measurement unit 161. The observation window 112 may be formed of quartz glass or the like.

[0054] The substrate 10 to be processed by the apparatus 100 is placed on the substrate stage 131. The substrate stage 131 is connected to a second high frequency power supply 132, and also functions as a second electrode for applying a bias voltage.

[0055] The pressure reducing device 141 is connected to the gas exhaust port 110b and reduces the pressure inside the chamber 110. A vacuum pump or the like is used for the pressure reducing device 141. The pressure reducing device 141 may include a pressure adjustment valve or the like. The apparatus 100 includes a pressure gauge for monitoring the pressure inside the chamber 110. The control unit 170 controls the pressure reducing device 141 based on the output of the pressure gauge to adjust the pressure inside the chamber 110.

[0056] A supply source 201 (e.g., a gas cylinder) of gas to be supplied to the chamber 110 is connected to the gas flow control unit 150. The control unit 170 controls the gas flow control unit 150 to adjust the flow rate of each gas. The gas flow control unit 150 includes a mass flow controller (MFC) disposed in a flow path of each gas to be supplied. The gas supplied from the supply source 201 is introduced into the chamber 110 through the gas flow control unit 150 and a gas inlet 110a. FIG. 1 shows an example of an apparatus in which three types of gas are used.

[0057] The light measurement unit 161 measures the intensity of light of a predetermined wavelength in the plasma in the chamber 110 through the observation window 112. The measurement result of the light measurement unit 161 is output to the control unit 170.

[0058] The chamber 110 includes a mechanism (e.g., an opening / closing mechanism) for loading and unloading the substrate 10 (not shown). When performing plasma etching using the apparatus 100, first, the substrate 10 is placed on the substrate stage 131. Next, the pressure inside the chamber 110 is reduced by the pressure reducing device 141, and a predetermined gas is introduced into the chamber 110 from the gas supply source 201. At this time, the pressure inside the chamber 110 is adjusted to a desired pressure as described above.

[0059] Next, a high frequency power is applied to the first electrode 121 by the first high frequency power supply 122 to generate plasma in the chamber 110. The substrate 10 is exposed to the generated plasma, and plasma etching or film formation is performed. At this time, a bias voltage is applied by the second high frequency power supply 132 as necessary.

[0060] (An example of a plasma etching method) An example of a plasma etching method according to the present disclosure will be described below. An example using the apparatus 100 shown in Fig. 1 will be described below, but an apparatus other than the apparatus 100 may be used. Also, an example in which the substrate 10 includes a silicon layer (silicon substrate) 11 and an element layer 12 will be described below, but another substrate may be used.

[0061] First, the substrate 10 is carried into the chamber 110 and placed on the substrate stage 131. A cross-sectional view of the substrate 10 is shown in Fig. 2A. The substrate 10 includes a silicon layer 11 and an element layer 12 disposed on the silicon layer 11. In other words, the substrate 10 includes the silicon layer 11 and the element layer 12 disposed on one main surface 10a side of the substrate 10.

[0062] The silicon layer 11 may be etched from the one main surface 10a side, or from the one main surface 10b side opposite to the one main surface 10a. In this example, an example of etching from the one main surface 10a side will be described. Furthermore, in this example, an example will be described in which the one main surface 10b of the substrate 10 is fixed to a holding sheet 31 for holding the substrate. The holding sheet 31 may be, for example, a dicing tape or a die attach film.

[0063] The substrate 10 is divided into streets St and a plurality of element areas EA defined by the streets St. By removing the portions of the substrate 10 corresponding to the streets St and dividing the substrate 10, a plurality of element chips each including an element layer 12 are obtained. The streets St are arranged, for example, in a lattice pattern.

[0064] The element layer 12 is a layer necessary for the element chip to function as an element. The element layer 12 includes at least one of a semiconductor portion, a conductive portion, an insulating portion, and the like. Examples of the semiconductor portion include a doped silicon layer and an undoped silicon layer. Examples of the conductive portion include a metal layer, and the like. Examples of the insulating portion include an insulating layer, and the like. There is no particular limitation on the configuration and material of the element layer 12, and they are selected according to the element chip to be manufactured. These configurations and materials may be publicly known configurations and materials.

[0065] A mask 15 is formed on one main surface 10a (the main surface exposed to plasma) of the substrate 10. The mask 15 has openings 15h in portions corresponding to the streets St. The openings 15h penetrate the mask 15, and the substrate 10 is exposed at the openings 15h. There is no particular limitation on the mask 15, and a known mask used in the Bosch process may be used. A mask having a predetermined opening 15h can be formed by a known method such as photolithography. The silicon layer 11 can also be etched from the side opposite to the side on which the element layer 12 is formed. In that case, the mask 15 is formed on the surface opposite to the element layer 12.

[0066] The aperture ratio varies depending on the size of the opening 15h. The aperture ratio is in the range described above. The width of the street St may be in the range of 5 μm to 200 μm, for example.

[0067] The substrate 10 is divided by digging deep into the portion of the opening 15h. First, the element layer 12 in the portion of the opening 15h is removed by plasma etching or the like to expose the silicon layer 11 in the portion of the opening 15h. FIG. 2A shows the substrate 10 after the element layer 12 in the portion of the opening 15h has been removed. There is no particular limitation on the method for removing the element layer 12, and the element layer 12 may be removed by a known method depending on the configuration of the element layer 12. Note that the substrate 10 from which the element layer 12 in the opening 15h has been removed may be prepared, and the substrate 10 may be processed in the apparatus 100.

[0068] Next, a part of the silicon layer 11 is etched until the silicon layer 11 is penetrated (etching step (E)). Specifically, the street St portion of the silicon layer 11 is removed by etching according to the following procedure. Main steps in the etching step (E) are shown in FIG.

[0069] (Silicon layer etching step) In the silicon layer etching step (etching steps (x) and (y)), as shown in FIG. 2B, a part of the silicon layer 11 (a part of the street St) is plasma-etched to form a recess 11v in the silicon layer 11 (step S501). The silicon layer etching step is performed in a state where an etching gas is introduced into the chamber 110. As the etching gas and etching conditions, the etching gas and etching conditions used for etching the silicon layer in the Bosch process may be applied. A preferred example of the etching gas includes a fluorine-containing gas. Examples of the fluorine-containing gas include CF4, CHF3, XeF2, XeF6, sulfur fluoride gas, and the like. Examples of the sulfur fluoride gas include sulfur hexafluoride gas (SF6), and the like. These gases may be used alone or in a mixture of two or more kinds, or may be diluted with a dilution gas. In the silicon layer etching step, the silicon layer 11 is etched approximately isotropically (isotropic etching).

[0070] 3, in this example, the silicon layer etching step (step S501) includes an etching step (y) (step S501a) and an etching step (x) (step S501b) in this order. Also, in this example, in the etching step (y), an end point of etching is detected.

[0071] As shown in FIG. 3, an etching step (step S501a) is performed by the etching step (y). In step S601, when it is determined that the recess 11v penetrates the silicon layer 11 and etching of the silicon layer 11 is completed (the end point is detected), the etching process (E) ends. If the end point is not detected, in step 602, it is determined whether the etching step (y) has been performed for a predetermined time. If the etching step (y) has not been performed for the predetermined time, the etching step (y) is continued. In step S601, it is determined whether the end point has been detected based on the light intensity of a predetermined wavelength measured by the light measurement unit 161.

[0072] As described above, the etching end point detection may be performed in both the etching step (x) and the etching step (y). In that case, steps S601 and S602 are performed after the etching step (x).

[0073] In the etching step (y), plasma is generated by applying a radio frequency power HPy smaller than the radio frequency power HPx applied in the etching step (x) to the plasma generating electrode (first electrode 121), thereby performing plasma etching. Therefore, in the etching step (y), the etching rate of the silicon layer 11 is slower than in the etching step (x).

[0074] If it is determined in step S601 that the end point has not been detected and if it is determined in step S602 that the etching step (y) has been performed for a predetermined time, then the etching step (x) is performed for a predetermined time (step S501b).

[0075] (Protective film formation step) Next, as shown in FIG. 2C, a protective film 21 is formed on the inside (inner surface) of the recess 11v (protective film forming step: step S502). The protective film 21 is formed so as to cover the surface of the silicon layer 11 exposed in the recess 11v. As shown in FIG. 2C, the protective film 21 may cover the end face of the element layer 12 exposed below the opening 15h. This makes it possible to protect the element layer 12. Furthermore, the protective film 21 may cover the end face of the mask 15 exposed in the opening 15h. The protective film 21 may cover the surface of the mask 15.

[0076] The protective film 21 can be formed by generating plasma in a state where a protective film forming gas (gas for forming a protective film) is introduced into the chamber 110. The protective film may be formed under the same conditions as those for forming a protective film in the known Bosch process.

[0077] The protective film forming gas may be a known gas used for forming a protective film in the Bosch process or the like. The protective film forming gas preferably contains a fluorocarbon. Examples of the fluorocarbon include fluorinated alicyclic hydrocarbons such as octafluorocyclobutane (C4F8) and octafluorocyclopentene (C5F8), difluoromethane (CH2F2), and the like. The protective film forming gas may be used alone or in combination of two or more.

[0078] (Protection film etching step) 2D, the protective film 21 present at the bottom of the recess 11v is removed by plasma etching to form a through hole 21h in the protective film 21 (protective film etching step: step S503). By this etching, the silicon layer 11 is exposed at the bottom of the recess 11v.

[0079] The protective film can be etched by generating plasma in a state where an etching gas for etching the protective film is introduced into the chamber 110. The protective film may be etched under the same conditions as those for etching the protective film in the known Bosch process.

[0080] The etching of the protective film 21 is usually performed in a state where a bias voltage is applied to the second electrode (substrate stage 131). That is, the etching of the protective film 21 is usually performed by anisotropic etching, whereby the protective film 21 present at the bottom of the recess 11v is selectively removed.

[0081] The etching gas may be any known etching gas used for etching a protective film in the Bosch process, etc. Specifically, the etching gas exemplified in the description of the silicon layer etching step may be used.

[0082] In this manner, a group of steps consisting of a silicon layer etching step, a protective film forming step, and a protective film etching step is performed. After one group of steps is completed, the group of steps is repeatedly performed until it is determined that the removal of the silicon layer 11 is completed. Specifically, after the process of FIG. 2D, a silicon layer etching step is performed to deepen the recess 11v as shown in FIG. 2E. Next, a protective film forming step and a protective film etching step are performed to obtain the substrate 10 in the state shown in FIG. 2F.

[0083] By repeatedly performing the steps, the recesses 11v penetrate the silicon layer 11 to form through-grooves 11h, as shown in Fig. 2G. As a result, the substrate 10 is divided into individual element chips 10x. In one example, the etching ends when the recesses 11v penetrate the silicon layer 11 to form substantially vertical through-grooves 11h.

[0084] Thereafter, if necessary, the mask 15 is removed by plasma ashing or the like. Then, the element chips 10x are separated from the holding sheet 31. In this manner, a plurality of element chips 10x are manufactured.

[0085] In this example, it is determined whether the recess 11v penetrates the silicon layer 11 based on the emission intensity of the plasma in the silicon layer etching step. If the recess 11v does not penetrate the silicon layer 11, a product containing Si (Si-containing product) is generated by etching the silicon layer. Examples of the Si-containing product include Si and SiF x (X is a natural number from 1 to 4). Si and SiF x The Si-containing products such as SiF are excited in the plasma and emit light. By measuring the intensity of these emitted lights, the amount of products containing Si generated by etching can be estimated. In other words, by measuring the intensity of the light emitted at a predetermined wavelength in the plasma (light emitted by the Si-containing products), it is possible to determine whether the recess 11v has penetrated the silicon layer 11. SiF excited in the plasma x(Silicon fluoride radical) has an emission peak in the range of 435 to 445 nm. Therefore, the emission intensity in this wavelength range (for example, the emission intensity at the peak wavelength of any emission peak present in this wavelength range) may be measured. Hereinafter, the wavelength of the emission intensity measured to detect the end point of etching may be referred to as the "measurement wavelength λ".

[0086] When the recess 11v penetrates the silicon layer 11 and reaches the one main surface 10b of the substrate 10, the amount of the silicon layer 11 etched per unit time decreases, and the emission intensity of the Si-containing product decreases. If etching is continued thereafter, a roughly vertical through groove 11h is formed. If etching is continued after the through groove 11h is formed, the sidewall of the silicon layer 11 at the bottom of the through groove 11h is etched (see FIG. 2G), and the emission intensity of the Si-containing product may increase again. By monitoring this change in emission intensity, the end point of etching can be appropriately determined. As described above, the type of change in emission intensity that indicates the end point of etching may be determined depending on the structure of the substrate 10 and the etching conditions.

[0087] If the silicon layer 11 is etched beyond the end point of the etching, the side surface of the bottom of the through groove 11h is etched, resulting in a shape abnormality called a notch 11n, as shown in FIG. 2G. If the notch 11n becomes too large, it may be undesirable for the device chip. Furthermore, continuing the etching after the through groove 11h is formed will result in a time loss. Therefore, it is important to appropriately determine the end point of the etching.

[0088] The silicon layer etching step includes an etching step (y) and an etching step (x). In the etching step (y), the etching rate of the silicon layer 11 is slow, so that the notching 11n can be prevented from becoming too large. In addition, in the etching step (y), the ratio of the emission intensity of the Si-containing product at the measurement wavelength λ to the emission intensity (noise emission intensity) derived from a substance other than the Si-containing product at the measurement wavelength λ becomes large. Therefore, in the etching step (y), the end point of etching can be easily determined appropriately. These effects can be obtained regardless of the order of the etching step (x) and the etching step (y). Also, in the protective film etching step, the silicon layer 11 is etched after the protective film 21 is etched. Therefore, even when the protective film etching step includes the etching step (x) and the etching step (y), the above effects can be obtained.

[0089] An example in which the end point of etching was determined by measuring the emission intensity at a wavelength of 440 nm will be described below. In this example, a silicon layer (silicon substrate) was etched by a silicon layer etching step including an etching step (x) and an etching step (y).

[0090] In this example, a 6-inch diameter silicon substrate (450 μm thick) was divided by an etching method (EM). The opening width (width of street St) was 30 μm, and the opening ratio was 0.5%. Photoresist was used as the mask. In the silicon layer etching step, SF6 (flow rate 600 sccm) was used as the etching gas. The pressure in the chamber during etching was 15 Pa. The power applied to the first electrode to generate plasma was 4800 W in the etching step (x) and 2400 W in the etching step (y). The power applied to the second electrode in the silicon layer etching step was 20 W. The time for the etching step (x) was 2.2 seconds, and the time for the etching step (y) was 7.0 seconds.

[0091] FIG. 4 shows the results of measuring the emission intensity at 440 nm in the silicon layer etching step. One cycle in FIG. 4 consists of one etching step (x) and one etching step (y). A protective film forming step and a protective film etching step are performed between these cycles. A point in the graph in FIG. 4 indicates the value of the emission intensity derived from the Si-containing product in the etching step (y). The value of the emission intensity derived from the Si-containing product is the value obtained by analytically subtracting the emission intensity (noise emission intensity) derived from substances other than the Si-containing product at a wavelength of 440 nm from the emission intensity at a wavelength of 440 nm. Note that since the etching rate varies depending on the location on the substrate, the timing at which the recess penetrates the silicon substrate varies. Therefore, the emission intensity measured reflects this variation.

[0092] The emission intensity at 440 nm is almost constant up to the 6th cycle, but decreases after the 7th cycle. This is believed to be because at least some of the recesses 11v reach the one main surface 10b. Thereafter, the emission intensity increases from the 15th cycle. This is believed to be because at least some of the side surfaces of the through grooves 11h start to be etched. In the example shown in FIG. 4, it is possible to determine that the etching has ended at the time of the 15th cycle. Thus, according to the method of the present disclosure, it is easy to accurately determine the etching end point. [Industrial Applicability]

[0093] The present disclosure can be used in a plasma etching method, a plasma etching apparatus, and a method for manufacturing element chips. [Explanation of symbols]

[0094] 10: Substrate 10x: Element chip 11: Silicon layer 11h: Through groove 11v : Recess 12: Element layer 15: Mask 15h: opening 21:Protective film 100: Equipment 110: Chamber 110a: Gas inlet 141: Pressure reducing device 150: Gas flow control section 161: Light measurement unit 170: Control section

Claims

1. A plasma etching method for etching a substrate including a silicon layer by plasma etching using plasma, comprising the steps of: etching a portion of the silicon layer until the silicon layer is penetrated; The etching step includes: a silicon layer etching step of plasma etching the portion of the silicon layer to form a recess in the silicon layer; a protective film forming step of forming a protective film on the inside of the recess; a protective film etching step of removing the protective film present at the bottom of the recess by plasma etching; and At least one step selected from the group consisting of the silicon layer etching step and the protective film etching step is an etching step (x) of generating the plasma by high frequency power and performing plasma etching; and an etching step (y) of generating the plasma by using a radio frequency power smaller than the radio frequency power applied in the etching step (x), and performing plasma etching; a determination as to whether the recess has penetrated the silicon layer and etching of the silicon layer has been completed is made based on an emission intensity of the plasma in the etching step (y).

2. 2. The plasma etching method according to claim 1, wherein the etching step (x) is performed after the etching step (y) if it is not determined that etching of the silicon layer is completed in the etching step (y).

3. 3. The plasma etching method according to claim 1, wherein the at least one step includes the silicon layer etching step.

4. In the silicon layer etching step, 6 An etching gas containing a gas is used, The determination is performed by determining whether the amount of Si and / or SiF in the plasma is large. x The plasma etching method according to claim 3, wherein the plasma etching method is performed based on the emission intensity of

5. 5. The plasma etching method according to claim 1, wherein the recess has an opening ratio of 1% or less.

6. 1. A plasma etching apparatus comprising: a chamber having a gas inlet in which a substrate is disposed; an electrode for generating a plasma within the chamber; a light measuring unit for measuring the emission intensity of the plasma; a control unit; the control unit executes an etching step of etching a portion of the silicon layer until the silicon layer is penetrated when etching a substrate including a silicon layer by plasma etching using the plasma; The etching step includes: a silicon layer etching step of plasma etching the portion of the silicon layer to form a recess in the silicon layer; a protective film forming step of forming a protective film on the inside of the recess; a protective film etching step of removing the protective film present at the bottom of the recess by plasma etching; and At least one step selected from the group consisting of the silicon layer etching step and the protective film etching step is an etching step (x) of generating the plasma by high frequency power and performing plasma etching; and an etching step (y) of generating the plasma by using a radio frequency power smaller than the radio frequency power applied in the etching step (x), and performing plasma etching; The control unit determines whether or not the recess has penetrated the silicon layer and etching of the silicon layer has been completed based on the emission intensity of the plasma in the etching step (y).

7. A method for manufacturing a component chip using a substrate including a silicon layer, comprising the steps of: an etching step of etching a portion of the silicon layer by plasma etching using a plasma until the silicon layer is penetrated; The etching step includes: a silicon layer etching step of plasma etching the portion of the silicon layer to form a recess in the silicon layer; a protective film forming step of forming a protective film on the inside of the recess; a protective film etching step of removing the protective film present at the bottom of the recess by plasma etching; and At least one step selected from the group consisting of the silicon layer etching step and the protective film etching step is an etching step (x) of generating the plasma by high frequency power and performing plasma etching; and an etching step (y) of generating the plasma by using a radio frequency power smaller than the radio frequency power to perform plasma etching, a determination as to whether or not the recess has penetrated the silicon layer and etching of the silicon layer has been completed is made based on the emission intensity of the plasma in the etching step (y).

8. 8. The method according to claim 7, wherein the etching step (x) is performed after the etching step (y) if it is not determined that etching of the silicon layer is completed in the etching step (y).

9. The method of claim 7 or 8, wherein the at least one step includes the silicon layer etching step.

10. In the silicon layer etching step, 6 An etching gas containing a gas is used, The determination is performed by determining whether the amount of Si and / or SiF in the plasma is large. x The method according to claim 9, wherein the method is carried out based on the luminescence intensity of

11. The method according to any one of claims 7 to 10, wherein the opening ratio of the recess is 1% or less.

Citation Information

Patent Citations

  • Anisotropic plasma etching method for semiconductors

    JP2002543611A

  • Endpoint detection in time division multiplexed etch processes

    JP2006518913A

  • Envelope Follower Endpoint Detection in Time Division Multiplexing Processes

    JP2007501532A

  • Plasma etching method and plasma etching apparatus capable of detecting end point

    JP2008053678A

  • Semiconductor device manufacturing method

    JP2013084695A