Non-aqueous electrolyte secondary battery
By using graphite particles with 1 to 5% internal porosity and optimizing the N/P ratio, the structural instability and capacity loss in lithium-transition metal composite oxide batteries are mitigated, resulting in enhanced durability and energy density.
Patent Information
- Application Number
- JP2021542649
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-04
- Filing Date
- 2020-07-28
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2040-07-28
AI Technical Summary
Lithium-transition metal composite oxides with high Ni content face structural instability and reduced battery capacity due to excessive Li extraction during charging, leading to poor charge/discharge cycle characteristics.
Incorporating graphite particles with 1 to 5% internal porosity as the negative electrode active material and setting the N/P ratio to 1.00 to 1.05, along with specific conditions on the maximum change in battery capacity, stabilizes the structure and enhances durability.
The solution significantly improves the battery's durability and energy density by suppressing capacity reduction and structural deterioration during charging and discharging.
Smart Images

Figure 0007580050000005 
Figure 0007580050000006 
Figure 0007580050000007
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a nonaqueous electrolyte secondary battery, and more particularly to a nonaqueous electrolyte secondary battery that uses a lithium transition metal composite oxide with a high Ni content as a positive electrode active material. [Background technology]
[0002] In recent years, lithium transition metal composite oxides with a high Ni content have been attracting attention as a positive electrode active material with high energy density. For example, Patent Document 1 describes a positive electrode active material having the general formula LiNi x Co y Al z O 2 A layered rock-salt structure lithium nickel composite oxide represented by (x+y+z=1, 0.05≦y≦0.4, 0.01≦z≦0.09) is used, and the active material density in the positive electrode is 2.3 to 3.0 g / cm 3 A non-aqueous electrolyte secondary battery is disclosed. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2001-216965 A Summary of the Invention
[0004] However, when a lithium transition metal composite oxide with a high Ni content is used as a positive electrode active material, the amount of Li extracted during charging is greater than that of a composite oxide with a low Ni content, making the layered structure of the composite oxide unstable and making it more likely that the battery capacity will decrease with charging and discharging. Note that the technology disclosed in Patent Document 1 cannot sufficiently suppress the structural deterioration of the composite oxide that accompanies the extraction of Li, and there is still room for improvement in the charge-discharge cycle characteristics (durability).
[0005] An object of the present disclosure is to improve the charge-discharge cycle characteristics of a non-aqueous electrolyte secondary battery that uses a lithium transition metal composite oxide with a high Ni content as a positive electrode active material.
[0006] A non-aqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a positive electrode, a negative electrode, and a non-aqueous electrolyte. The positive electrode contains 85 mol % of metal elements other than Li. End The negative electrode contains graphite particles having an internal porosity of 1 to 5%, and when the charge capacity of the positive electrode is P and the charge capacity of the negative electrode is N, an N / P ratio is 1.00 to 1.05, and a maximum change in battery capacity (Q) (dQ / dV(cf)) in the voltage range from a battery voltage of 4.0 V to an end-of-charge voltage and a maximum change in battery capacity (Q) (dQ / dV(cm)) in the battery voltage range from 3.8 V to 4.0 V satisfy the relationship of Formula 1.
[0007]
number
[0008] According to one aspect of the present disclosure, in a non-aqueous electrolyte secondary battery using a lithium transition metal composite oxide with a high Ni content, it is possible to suppress a capacity decrease accompanying charge and discharge. The non-aqueous electrolyte secondary battery according to the present disclosure has a high energy density and excellent cycle characteristics (durability). [Brief description of the drawings]
[0009] [Figure 1] 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment; [Figure 2A] FIG. 2 is a graph showing the relationship between battery voltage (V) and the change in battery capacity per unit volume (Q) (dQ / dV) calculated from a 0.05 It charging curve in the nonaqueous electrolyte secondary battery of the example. [Figure 2B] FIG. 2 is a diagram showing the relationship between battery voltage (V) and the amount of change (dQ / dV) in battery capacity per unit volume (Q) calculated from a 0.05 It charging curve in a nonaqueous electrolyte secondary battery of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] As mentioned above, lithium transition metal composite oxides with a high Ni content contribute to improving the energy density of batteries, but because a large amount of Li is extracted during charging, repeated charging and discharging causes the layered structure of the composite oxide to collapse and become unstable, which is thought to cause a decrease in battery capacity (durability). One method of suppressing the deterioration of the composite oxide is to lower the end-of-charge voltage, but in this case, deterioration of the negative electrode becomes an issue, and battery durability is not sufficiently improved.
[0011] Therefore, the present inventors conducted extensive research to solve the above problems and found that the durability of the battery can be significantly improved by using graphite particles having an internal porosity of 1 to 5% as the negative electrode active material, setting the ratio of the charge capacity P of the positive electrode to the charge capacity N of the negative electrode to 1.00 to 1.05, and satisfying the condition of the above formula 1. Hereinafter, one example of an embodiment of the nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail.
[0012] In the following, a cylindrical battery in which a wound electrode body 14 is housed in a cylindrical exterior can 16 with a bottom is exemplified, but the exterior can is not limited to a cylindrical exterior can, and may be, for example, a rectangular exterior can, or an exterior made of a laminate sheet including a metal layer and a resin layer. The electrode body may also be a laminated electrode body in which multiple positive electrodes and multiple negative electrodes are alternately laminated with separators interposed therebetween. In this specification, the expression "numerical value (A) to numerical value (B)" means that the value is equal to or greater than numerical value (A) and equal to or less than numerical value (B).
[0013] FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 according to an embodiment. As illustrated in FIG. 1, the nonaqueous electrolyte secondary battery 10 includes a wound electrode assembly 14, a nonaqueous electrolyte, and an exterior can 16 that accommodates the electrode assembly 14 and the electrolyte. The electrode assembly 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are wound in a spiral shape with the separator 13 interposed therebetween. The exterior can 16 is a cylindrical metal container with a bottom that is open on one axial side, and the opening of the exterior can 16 is closed by a sealing body 17. In the following description, for convenience of explanation, the sealing body 17 side of the battery is referred to as the top, and the bottom side of the exterior can 16 is referred to as the bottom.
[0014] The non-aqueous electrolyte includes a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixtures of two or more of these. The non-aqueous solvent may contain a halogen-substituted compound in which at least a portion of the hydrogen of these solvents is replaced with a halogen atom such as fluorine. The electrolyte salt may include, for example, LiPF 6 The electrolyte is not limited to a liquid electrolyte, and may be a solid electrolyte using a gel polymer or the like.
[0015] The positive electrode 11, the negative electrode 12, and the separator 13 constituting the electrode body 14 are all long strip-shaped bodies, and are alternately stacked in the radial direction of the electrode body 14 by being wound in a spiral shape. The negative electrode 12 is formed to be slightly larger than the positive electrode 11 in order to prevent lithium deposition. That is, the negative electrode 12 is formed to be longer than the positive electrode 11 in the longitudinal direction and the width direction (short direction). The two separators 13 are formed to be at least slightly larger than the positive electrode 11, and are arranged to sandwich the positive electrode 11, for example. The electrode body 14 has a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like.
[0016] Insulating plates 18 and 19 are disposed above and below the electrode body 14. In the example shown in Fig. 1, the positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and the negative electrode lead 21 passes outside the insulating plate 19 and extends toward the bottom side of the outer casing 16. The positive electrode lead 20 is connected to the lower surface of an internal terminal plate 23 of the sealing body 17 by welding or the like, and a cap 27, which is a top plate of the sealing body 17 and is electrically connected to the internal terminal plate 23, serves as a positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom inner surface of the outer casing 16 by welding or the like, and the outer casing 16 serves as a negative electrode terminal.
[0017] A gasket 28 is provided between the exterior can 16 and the sealing body 17 to ensure airtightness inside the battery. The exterior can 16 has a grooved portion 22 formed therein, with part of the side surface protruding inward, to support the sealing body 17. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior can 16, and supports the sealing body 17 on its upper surface. The sealing body 17 is fixed to the top of the exterior can 16 by the grooved portion 22 and the open end of the exterior can 16 which is crimped against the sealing body 17.
[0018] The sealing body 17 has a structure in which an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are laminated in this order from the electrode body 14 side. Each member constituting the sealing body 17 has, for example, a disk shape or a ring shape, and each member except the insulating member 25 is electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks so as to push the upper valve body 26 toward the cap 27, thereby cutting off the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0019] The positive electrode 11, negative electrode 12, and separator 13 that constitute the electrode assembly 14 will be described in detail below, in particular the positive electrode active material that constitutes the positive electrode 11 and the negative electrode active material that constitutes the negative electrode 12. Additionally, charging control of the battery will be described in detail.
[0020] [Positive electrode] The positive electrode 11 has a positive electrode core and a positive electrode composite layer provided on the surface of the positive electrode core. For the positive electrode core, a foil of a metal such as aluminum that is stable in the potential range of the positive electrode 11, a film with the metal disposed on the surface layer, or the like can be used. The positive electrode composite layer contains a positive electrode active material, a binder, and a conductive material, and is preferably provided on both sides of the positive electrode core except for the part to which the positive electrode lead 20 is connected. The positive electrode 11 can be produced, for example, by applying a positive electrode composite slurry containing a positive electrode active material, a binder, a conductive material, and the like to the surface of the positive electrode core, drying the coating, and then compressing it to form a positive electrode composite layer on both sides of the positive electrode core.
[0021] Examples of the conductive material contained in the positive electrode mixture layer include carbon materials such as carbon black, acetylene black, ketjen black, and graphite. Examples of the binder contained in the positive electrode mixture layer include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, and polyolefin. These resins may be used in combination with cellulose derivatives such as carboxymethylcellulose (CMC) or its salt, and polyethylene oxide (PEO).
[0022] The positive electrode 11 is 85 mol % based on the total number of moles of metal elements excluding Li. End The lithium transition metal composite oxide includes a lithium transition metal composite oxide containing Ni. Hereinafter, for convenience of explanation, the lithium transition metal composite oxide is referred to as "composite oxide (Z)". The composite oxide (Z) functions as a positive electrode active material. The composite oxide (Z) has a layered structure, for example, a layered structure belonging to the space group R-3m, or a layered structure belonging to the space group C2 / m. The positive electrode active material may be mainly composed of the composite oxide (Z) and substantially composed of only the composite oxide (Z). Note that the positive electrode active material may contain a composite oxide other than the composite oxide (Z) or other compounds within a range that does not impair the object of the present disclosure.
[0023] As described above, the composite oxide (Z) is 85 mol% based on the total number of moles of metal elements excluding Li. End The Ni content is 85 mol % or more, whereby a battery with high energy density can be obtained. The Ni content may be 86 mol % or more, or 90 mol % or more, based on the total number of moles of metal elements excluding Li. The upper limit of the Ni content is not particularly limited, but is preferably 97 mol %, more preferably 95 mol %, based on the total number of moles of metal elements excluding Li.
[0024] The composite oxide (Z) may contain a metal element other than Li and Ni. Examples of the metal element include Co, Mn, Al, Zr, B, Mg, Fe, Cu, Zn, Sn, Na, K, Ba, Sr, Ca, W, Mo, Si, Nb, Sr, etc. The composite oxide (Z) preferably contains Al in addition to at least Li and Ni, and more preferably further contains at least one selected from Mn and Nb. Al does not change its oxidation number during charging and discharging, and stabilizes the layered structure of the composite oxide (Z). Similarly, Nb also stabilizes the layered structure of the composite oxide (Z) and contributes to improving the durability of the battery.
[0025] When the composite oxide (Z) contains Al, the content of Al is preferably 0.5 to 8.0 mol % and more preferably 1.0 to 5.0 mol % based on the total number of moles of metal elements excluding Li. When the composite oxide (Z) contains Mn, the content of Mn is preferably 10 mol % or less based on the total number of moles of metal elements excluding Li. When the composite oxide (Z) contains Nb, the content of Nb is preferably 1.0 mol % or less based on the total number of moles of metal elements excluding Li. The composite oxide (Z) may contain Co. The content of Co is preferably 10 mol % or less and may be 3 mol % or less based on the total number of moles of transition metal elements.
[0026] An example of a suitable composite oxide (Z) is represented by the general formula Li a Ni b Co c Al d Mn e Nb f O g (wherein, 0.8≦a≦1.2, 0.85≦b<1, 0≦c≦0.03, 0≦d≦0.08, 0≦e≦0.10, 0≦f≦0.01, 1≦g≦2). The contents of the elements constituting the composite oxide (Z) can be measured by an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), or the like.
[0027] The complex oxide (Z) is, for example, a secondary particle formed by agglomeration of a plurality of primary particles. The particle size of the primary particles is generally 0.05 μm to 1 μm. The volume-based median diameter (D50) of the complex oxide (Z) is, for example, 3 μm to 30 μm, preferably 5 μm to 25 μm. D50 means the particle size at which the cumulative frequency is 50% from the smallest particle size in the volume-based particle size distribution, and is also called the median diameter. The particle size distribution of the complex oxide (Z) can be measured using a laser diffraction type particle size distribution measuring device (for example, MT3000II manufactured by Microtrack Bell Co., Ltd.) using water as a dispersion medium.
[0028] [Negative electrode] The negative electrode 12 has a negative electrode core and a negative electrode composite layer provided on the surface of the negative electrode core. For the negative electrode core, a foil of a metal such as copper that is stable in the potential range of the negative electrode 12, a film with the metal disposed on the surface layer, or the like can be used. The negative electrode composite layer contains a negative electrode active material and a binder, and is preferably provided on both sides of the negative electrode core except for the part to which the negative electrode lead 21 is connected. The negative electrode 12 can be produced, for example, by applying a negative electrode composite slurry containing a negative electrode active material and a binder to the surface of the negative electrode core, drying the coating, and then compressing it to form a negative electrode composite layer on both sides of the negative electrode core.
[0029] The binder contained in the negative electrode mixture layer may be, as in the case of the positive electrode 11, a fluororesin, PAN, polyimide, acrylic resin, polyolefin, or the like, but it is preferable to use styrene-butadiene rubber (SBR). The negative electrode mixture layer preferably further contains CMC or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), or the like. Among them, it is preferable to use SBR in combination with CMC or a salt thereof, or PAA or a salt thereof.
[0030] The negative electrode 12 includes graphite particles having an internal porosity of 1 to 5%. Hereinafter, for convenience of explanation, the graphite particles are referred to as "graphite particles (G)". The graphite particles (G) function as a negative electrode active material. The internal void means a closed void that is not connected from the inside of the particle to the particle surface, and is distinguished from an external void that is connected from the inside of the particle to the particle surface. The negative electrode active material may be mainly composed of the graphite particles (G) and substantially composed of only the graphite particles (G). The negative electrode active material may include graphite particles having an internal porosity of less than 1% or more than 5%, or a compound other than graphite, such as a Si-containing compound, within a range that does not impair the object of the present disclosure.
[0031] The graphite particles (G) may be either natural graphite or artificial graphite, but are preferably artificial graphite from the viewpoint of adjusting the internal porosity. The graphite particles 30 have a D50 of, for example, 5 μm to 30 μm, and preferably 10 μm to 25 μm. The D50 is measured in the same manner as the D50 of the composite oxide (Z).
[0032] The internal porosity of the graphite particles (G) is 1 to 5% as described above, more preferably 1.5% to 4.5%, and more preferably 2.0 to 4.0%. By using graphite particles with an internal porosity within this range, material deterioration of the positive and negative electrodes accompanying charge and discharge is suppressed. The negative electrode 12 contains graphite particles with a particle size (diameter of the circumscribed circle of the particle in a scanning electron microscope (SEM) image) of 5 μm to 50 μm, and 50% or more, preferably 80% or more, or substantially all of the particles have an internal porosity of 1 to 5%. In other words, at least 50% of the graphite particles with a particle size of 5 μm to 50 μm contained in the negative electrode 12 are graphite particles (G).
[0033] In this specification, the internal porosity of a graphite particle means the ratio of the area of the internal voids of the graphite particle to the cross-sectional area of the graphite particle. The method for measuring the internal porosity of a graphite particle is as follows. (1) Using an ion milling device (for example, IM4000PLUS manufactured by Hitachi High-Technologies Corporation) or the like, a cross section of the negative electrode mixture layer is exposed. (2) A backscattered electron image of the cross section of the exposed negative electrode composite layer is taken using a scanning electron microscope (SEM). The magnification for taking the backscattered electron image is 3000 to 5000 times. (3) The SEM image of the cross section of the negative electrode composite layer is imported into a computer and binarized using image analysis software (e.g., ImageJ, manufactured by the National Institutes of Health, USA) to obtain a binarized image in which the particle cross sections in the cross-sectional image are colored black and voids present in the particle cross sections are colored white. (4) From the binarized image, graphite particles having a particle size of 5 μm to 50 μm are selected, and the area of the cross section of the graphite particle and the area of the internal voids present in the cross section of the graphite particle are calculated.
[0034] It should be noted that, among the voids present in the cross section of a graphite particle, those with a width of 3 μm or less may be regarded as internal voids, since it may be difficult to distinguish between internal and external voids in image analysis. The internal porosity of a graphite particle is the average value of 10 particles.
[0035] The graphite particles (G) have a pore size of 2 nm or less, as determined from the nitrogen adsorption isotherm using the density functional theory (DFT) method, and the volume per mass of the pores is 0.3 mm 3 / g or less. In this case, it is considered that side reactions with the electrolyte are suppressed and the durability of the battery is further improved. The volume of the graphite particles (G) is 0.2 mm 3 / g or less is more preferable, and 0.1 mm 3 The lower limit of the volume is not particularly limited and may be below the detection limit, but is preferably 0.005 mm 3 / g or more.
[0036] The volume of the graphite particles (G) may be determined by a known method using the DFT method from the nitrogen adsorption isotherm of the graphite particles (G), for example, using a specific surface area measuring device (autosorb iQ-MP, manufactured by Quantachrome Instruments Co., Ltd.). Specifically, adsorption isotherms corresponding to the pore sizes of various pores are calculated in advance by simulation, and then the adsorption isotherm of the graphite particles is obtained using nitrogen gas, and the obtained adsorption isotherm is analyzed and superimposed on the adsorption isotherm calculated by simulation. As a result, the volume per mass of each pore is calculated, and the volume per mass of pores with a pore size of 2 nm or less can be determined based on the calculation result.
[0037] Graphite particles (G) have a BET specific surface area of 0.3 m 2 / g or more, and 0.5m 2 / g or more. In this case, the edge faces of the graphite crystals where lithium ions are inserted and removed during charging and discharging are exposed, which is considered to improve the load characteristics (rate characteristics). Although there is no particular upper limit for the BET specific surface area of the graphite particles (G), from the viewpoint of suppressing side reactions with the electrolyte, it is preferable that the upper limit is 2 m 2 / g or less is preferable, and 1.5m 2 The BET specific surface area of the graphite particles (G) is measured by a BET method using a conventionally known specific surface area measuring device (for example, Macsorb (registered trademark) HM model-1201 manufactured by Mountech Co., Ltd.).
[0038] The graphite particles (G) can be produced, for example, by crushing the main raw material coke (precursor) to a predetermined size, agglomerating the crushed product using a binder, calcining the product in that state to graphitize it, and sieving it. The temperature of the heat treatment may be within the temperature range of conventional graphitization treatment, for example, 1800°C to 3000°C. Here, the internal porosity can be adjusted to 1 to 5% by controlling the particle size of the precursor after crushing or the particle size of the precursor in an aggregated state. For example, the D50 of the precursor after crushing is preferably 12 μm to 20 μm. A ball mill, a hammer mill, a pin mill, a jet mill, or the like can be used to crush the precursor.
[0039] In addition to the graphite particles according to the present embodiment, the negative electrode mixture layer may further include, as the negative electrode active material, lithium alloys such as metallic lithium, lithium-aluminum alloys, lithium-lead alloys, lithium-silicon alloys, and lithium-tin alloys; graphite other than graphite particles having a pore volume of 2 nm or less within the above range; carbon materials such as coke and organic sintered bodies; SnO 2 , SnO, TiO 2 From the viewpoint of suppressing the expansion and contraction of the negative electrode mixture layer during charge / discharge cycles and preventing the destruction of the coating film formed on the negative electrode active material, the graphite particles according to this embodiment are preferably 50 mass % or more, and more preferably 75 mass % or more of the total amount of the negative electrode active material.
[0040] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. The material of the separator 13 is preferably a polyolefin such as polyethylene or polypropylene, or cellulose. The separator 13 may have either a single-layer structure or a laminated structure. A heat-resistant layer or the like may be formed on the surface of the separator.
[0041] [Charging capacity / charging control] The nonaqueous electrolyte secondary battery 10 satisfies an N / P ratio of 1.00 to 1.05, where P is the charge capacity of the positive electrode 11 and N is the charge capacity of the negative electrode 12. In this case, the energy density of the battery can be increased while suppressing the deposition of Li in the negative electrode 12. The N / P ratio varies depending on the composition, physical properties, mass ratio, etc. of the positive electrode active material and the negative electrode active material. For this reason, it is necessary to adjust the composition, physical properties, mass ratio, etc. of each active material using the composite oxide (Z) and graphite particles (G) so as to satisfy the above N / P ratio.
[0042] In the nonaqueous electrolyte secondary battery 10, the maximum change in battery capacity (dQ / dV(cf)) in the battery voltage range from 4.0 V to the end-of-charge voltage and the maximum change in battery capacity (dQ / dV(cm)) in the battery voltage range from 3.8 V to 4.0 V satisfy the relationship of Formula 1.
[0043]
number
[0044] dQ / dV means the amount of change in battery capacity Q per unit voltage, and is calculated from the charging curve of the nonaqueous electrolyte secondary battery 10. By using a composite oxide (Z) as the positive electrode active material and graphite particles (G) as the negative electrode active material, adjusting the N / P ratio to 1.00 to 1.05, and satisfying the relationship of formula 1, the durability of the battery is significantly improved.
[0045] Charge control of the nonaqueous electrolyte secondary battery 10, particularly the charge cut-off voltage, is important in satisfying the relationship of formula 1. As long as the relationship of formula 1 is satisfied, the charge cut-off voltage is not particularly limited, but is preferably set to 4.15 V or less, for example, in the range of 4.00 to 4.15 V. Even if the charge cut-off voltage is set to 4.15 V or less, the intensity ratio (cf / cm) varies greatly depending on the composition, physical properties, mass ratio, etc. of the positive electrode active material and the negative electrode active material. For this reason, it is necessary to adjust the composition, physical properties, mass ratio, etc. of each active material using the composite oxide (Z) and graphite particles (G) so as to satisfy the relationship of formula 1.
[0046] 2A and 2B are diagrams showing the relationship between the battery voltage (V) and dQ / dV in the nonaqueous electrolyte secondary batteries of Example 1 and Comparative Example 2 described later. As shown in FIGS. 2A and 2B, in the nonaqueous electrolyte secondary battery 10, for example, a peak of dQ / dV appears in a voltage range exceeding 4.0V and in a voltage range of 3.8V to 4.0V. In this case, the peak top value in the voltage range of 3.8V to 4.0V is (dQ / dV(cm)). The end-of-charge voltage is set so that (dQ / dV(cf)) is equal to or less than (dQ / dV(cm)) and the relationship of Equation 1 is satisfied.
[0047] The nonaqueous electrolyte secondary battery 10 having the above configuration constitutes a battery system together with, for example, a charge control device configured to control charging of the battery. The nonaqueous electrolyte secondary battery 10 is connected to a load and supplies stored power to the load. The battery system may include an assembled battery (also called a battery pack or a battery module) in which a plurality of nonaqueous electrolyte secondary batteries 10 are connected in series, parallel, or series-parallel. The charge control device may be incorporated in the battery module, or may be configured as a part of a control device for a device or facility such as a vehicle in which the nonaqueous electrolyte secondary battery 10 is mounted.
[0048] The charge control device determines the charging conditions of the battery based on the charging state of the battery acquired from the battery monitoring unit, for example. The charge control device may have a rectifier circuit and convert AC power from a power source into a predetermined DC power to supply to the nonaqueous electrolyte secondary battery 10. The charge control device is configured with a computer including a processor, a memory, an input / output interface, and the like. The processor is configured with, for example, a CPU or a GPU, and performs charging control by reading and executing a processing program. The memory includes a nonvolatile memory such as a ROM, HDD, SSD, and the like, and a volatile memory such as a RAM. The processing program is stored in the nonvolatile memory.
[0049] The battery system may include a battery monitoring unit. The battery monitoring unit detects, for example, the charging current supplied to the nonaqueous electrolyte secondary battery 10 and the battery voltage. The charge control device estimates the state of charge (SOC) from the battery voltage acquired by the battery monitoring unit, and executes charge control based on the SOC. The SOC can also be estimated from the charge / discharge current and the charge / discharge time. A conventionally known method can be used to estimate the SOC. EXAMPLES
[0050] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0051] <Example 1> [Preparation of positive electrode] As the positive electrode active material, LiNi 0.91 Co 0.045 Al 0.045 O 2 A lithium transition metal composite oxide represented by the formula (1) was used. The positive electrode active material, acetylene black, and polyvinylidene fluoride were mixed in a solid content mass ratio of 98:1:1, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode composite slurry. The slurry was applied to both sides of a positive electrode core made of aluminum foil by a doctor blade method, and after drying the coating, the coating was compressed with a roller and cut into a predetermined electrode size to prepare a positive electrode in which a positive electrode composite layer was formed on both sides of the positive electrode core. In addition, an exposed portion in which the core surface was exposed was provided in a part of the positive electrode, and an aluminum positive electrode lead was attached.
[0052] [Preparation of graphite particles] Coke and pitch binder were crushed and mixed, then calcined at 1000℃, and then graphitized at 3000℃. 2 The powder was pulverized in a ball mill under atmospheric pressure, and the resulting powder was classified to obtain graphite particles G1 having a D50 of 16 μm and an internal porosity of 2%, as measured by the above method. The BET specific surface area of the graphite particles G1 was 0.5 m 2 / g, and the volume per mass of pores with a pore diameter of 2 nm or less determined by the DFT method is 0.1 mm 3 / g.
[0053] [Preparation of negative electrode] Graphite particles G1 were used as the negative electrode active material. The negative electrode active material, sodium carboxymethylcellulose (CMC-Na), and styrene-butadiene rubber (SBR) were mixed in an aqueous solution at a solid content mass ratio of 98:1:1 to prepare a negative electrode composite slurry. The slurry was applied to both sides of a negative electrode core made of copper foil, the coating film was dried, and then the coating film was compressed using a roller and cut into a predetermined electrode size to prepare a negative electrode in which a negative electrode composite layer was formed on both sides of the negative electrode core. In addition, an exposed portion in which the surface of the negative electrode core was exposed was provided in a part of the negative electrode, and a nickel negative electrode lead was attached to the exposed portion.
[0054] [Preparation of non-aqueous electrolyte] LiPF was dissolved in a mixed solvent of ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) in a volume ratio of 3:3:4. 6 was dissolved in the solution at a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte solution.
[0055] [Preparation of non-aqueous electrolyte secondary battery] The positive electrode and the negative electrode were spirally wound with a polyethylene separator between them to produce a wound electrode body. Insulating plates were placed on the top and bottom of the electrode body, the negative electrode lead was welded to the inner bottom surface of the outer can, and the positive electrode lead was welded to a sealing member, and the electrode body was housed in the outer can. Thereafter, a nonaqueous electrolyte was injected into the outer can, and the opening of the outer can was sealed with a sealing member via a gasket to produce a cylindrical nonaqueous electrolyte secondary battery.
[0056] In the nonaqueous electrolyte secondary battery of Example 1, the N / P ratio was set to 1.04, the end-of-charge voltage was set to 4.1 V, and the intensity ratio (cf / cm) was set to 0.97.
[0057] <Comparative Example 1> A nonaqueous electrolyte secondary battery was produced in the same manner as in Example 1, except that graphite particles G2 produced by the following method were used instead of graphite particles G1.
[0058] [Preparation of graphite particles] Coke and pitch binder were pulverized and mixed, then calcined at 1000°C, and then graphitized at 3000°C. The mixture was pulverized in a roller mill under an inert atmosphere, and the resulting powder was classified to obtain graphite particles G2 with a D50 of 17 μm and an internal porosity of 18%. The BET specific surface area of the graphite particles G2 was 0.3 m 2 / g, and the volume per mass of pores with a pore diameter of 2 nm or less determined by the DFT method is 1.5 mm 3 / g.
[0059] <Comparative Example 2> A nonaqueous electrolyte secondary battery was fabricated having the same configuration as in Example 1, except that the N / P ratio was set to 1.04, the end-of-charge voltage was set to 4.3 V, and the intensity ratio (cf / cm) was set to 1.86.
[0060] [Evaluation of capacity retention rate (durability) after cycle testing] Each of the batteries in the examples and comparative examples was charged at a constant current of 0.5 It in a temperature environment of 45° C. up to the end-of-charge voltage, and then charged at a constant voltage until the current value at the end-of-charge voltage was 1 / 50 It. Thereafter, constant-current discharge was performed at a constant current of 0.5 It until the battery voltage reached 3.0 V. This charge / discharge cycle was repeated 800 cycles. The discharge capacity at the first cycle and the discharge capacity at the 800th cycle of the cycle test were obtained, and the capacity retention rate was calculated by the following formula. The evaluation results are shown in Table 1 together with the composition of the lithium transition metal composite oxide, the internal porosity of the graphite particles, and the intensity ratio (cf / cm).
[0061] Capacity retention rate (%) = (800th cycle discharge capacity ÷ 1st cycle discharge capacity) × 100 2A and 2B show the relationship between the battery voltage (V) and the change in battery capacity (Q) per unit volume (dQ / dV) calculated from the 0.05 It charging curves of each of the batteries of Example 1 and Comparative Example 2.
[0062] [Table 1]
[0063] As is clear from the results shown in Table 1, the batteries of the examples have higher capacity retention rates after cycle testing and are superior in charge-discharge cycle characteristics (durability) compared to the batteries of the comparative examples. When graphite particles with an internal porosity of more than 5% are used (Comparative Example 1), it is difficult to ensure good durability, and in particular, when the strength ratio (cf / cm) exceeds 1 (Comparative Example 2), durability is significantly reduced. [Explanation of symbols]
[0064] 10 Nonaqueous electrolyte secondary battery 11 Positive electrode 12 Negative electrode 13 Separator 14 Electrode body 16 Outer can 17 Sealing body 18,19 Insulating plate 20 Positive lead 21 Negative lead 22 Grooved part 23 Internal terminal board 24 Lower valve body 25 Insulating materials 26 Upper valve 27 Cap 28 Gasket
Claims
1. A non-aqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte, The positive electrode contains a lithium transition metal composite oxide containing 85 mol % or more of Ni based on the total number of moles of metal elements excluding Li, the negative electrode comprises graphite particles having an internal porosity of 1 to 5%; When the charge capacity of the positive electrode is P and the charge capacity of the negative electrode is N, the N / P ratio is 1.00 to 1.05; The maximum change in battery capacity (Q) (dQ / dV (cf)) in the voltage range from the battery voltage of 4.0 V to the end-of-charge voltage, and the maximum change in battery capacity (Q) (dQ / dV (cm)) in the voltage range from the battery voltage of 3.8 V to 4.0 V, [0010] A non-aqueous electrolyte secondary battery that satisfies the above relationship.
2. The graphite particles have a pore volume per mass of 0.3 mm2 having a pore diameter of 2 nm or less as determined by a DFT method from a nitrogen adsorption isotherm. 3 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the capacitance is 0.1 to 0.5 μm.
3. The BET specific surface area of the graphite particles is 0.5 m 2 3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the molecular weight of the nonaqueous electrolyte is 1 / g or more.
4. 4. The nonaqueous electrolyte secondary battery according to claim 1, wherein the end-of-charge voltage is 4.15 V or less.
Citation Information
Patent Citations
Positive electrode for lithium secondary battery
JP2001216965A
Electrode for lithium ion secondary battery, electrode group for lithium ion secondary battery using the electrode and lithium ion secondary battery using the electrode group
JP2011165388A
Composite particles, methods for manufacturing the same, and articles containing the same
JP2014505992A
Nonaqueous electrolytic solution and secondary battery of the nonaqueous electrolytic solution
JP2019033074A