Lithium secondary battery
By using specific cations and oxalate complex anions in the electrolyte, lithium secondary batteries achieve improved cycle characteristics and discharge capacity by stabilizing lithium metal deposition and suppressing dendrites, addressing the limitations of existing technologies.
Patent Information
- Application Number
- JP2021542650
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-30
- Filing Date
- 2020-07-28
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2040-07-28
AI Technical Summary
Lithium secondary batteries face limitations in capacity and cycle characteristics due to dendrite precipitation and increased side reactions, which degrade discharge capacity and stability.
Incorporating specific cations such as Na, K, Rb, Cs, Fr, Mg, Ca, Sr, Ba, and Al, along with oxalate complex anions in the non-aqueous electrolyte, stabilizing lithium metal deposition and suppressing dendrite formation through eutectoid deposition and film formation on the negative electrode.
Enhances cycle characteristics and discharge capacity by stabilizing lithium metal deposition, reducing dendrite formation, and improving the overall performance of lithium secondary batteries.
Smart Images

Figure 0007580051000003 
Figure 0007580051000001 
Figure 0007580051000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a lithium secondary battery that uses lithium metal as a negative electrode active material. [Background technology]
[0002] Non-aqueous electrolyte secondary batteries are used for applications such as ICT applications such as personal computers and smartphones, vehicle applications, and power storage applications. In these applications, non-aqueous electrolyte secondary batteries are required to have a higher capacity. Lithium ion batteries are known as high-capacity non-aqueous electrolyte secondary batteries. The capacity of lithium ion batteries can be increased by using, for example, an alloy active material such as graphite and a silicon compound as a negative electrode active material. However, the capacity of lithium ion batteries is reaching its limit.
[0003] Lithium secondary batteries are promising as non-aqueous electrolyte secondary batteries with a higher capacity than lithium ion batteries. In lithium secondary batteries, lithium metal is precipitated on the negative electrode during charging, and this lithium metal dissolves in the non-aqueous electrolyte during discharging. Lithium secondary batteries are sometimes called lithium metal secondary batteries.
[0004] In lithium batteries, lithium metal is deposited on the negative electrode during charging. At this time, the lithium metal can be deposited in the form of dendrites. However, when dendrites are formed, the specific surface area of the negative electrode increases, and side reactions tend to increase. As a result, the discharge capacity and cycle characteristics tend to decrease.
[0005] Non-Patent Document 1 describes that the addition of cesium ions or rubidium ions to the electrolyte suppresses the precipitation of dendrites. [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] Fei Ding, et al., “Dendrite-Free Lithium Deposition via Self-Healing Electrostatic Shield Mechanism”, J. Am. Chem. Soc., 2013, 135, p. 4450-4456 Summary of the Invention
[0007] However, even in Non-Patent Document 1, the effect of suppressing the precipitation of dendrites is insufficient, and there is a limit to the improvement in the cycle characteristics of lithium secondary batteries.
[0008] One aspect of the present disclosure relates to a lithium secondary battery including a positive electrode, a negative electrode, a lithium ion conductive non-aqueous electrolyte, and a separator disposed between the positive electrode and the negative electrode, in which lithium metal precipitates in the negative electrode during charging and the lithium metal dissolves in the non-aqueous electrolyte during discharging, the non-aqueous electrolyte including a cation and an anion, the cation including a lithium ion and at least one cation X selected from the group consisting of Na, K, Rb, Cs, Fr, Mg, Ca, Sr, Ba, and Al, and the anion including an oxalate complex anion Y.
[0009] In lithium secondary batteries, the cycle characteristics are improved. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a vertical cross-sectional view illustrating a lithium secondary battery according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] A lithium secondary battery according to an embodiment of the present disclosure includes a positive electrode, a negative electrode, a lithium ion conductive non-aqueous electrolyte, and a separator disposed between the positive electrode and the negative electrode. In the negative electrode, lithium metal is precipitated during charging, and the lithium metal is dissolved in the non-aqueous electrolyte during discharging. The non-aqueous electrolyte includes a cation and an anion. The cation includes a lithium ion and at least one cation X selected from the group consisting of Na, K, Rb, Cs, Fr, Mg, Ca, Sr, Ba, and Al. The anion includes an oxalate complex anion Y. The cation X is generally Na + , K + , Rb + , Cs + , Fr + , Mg 2+ , Ca 2+ , Sr 2+ , B.A. 2+ , Al 3+ etc.
[0012] In lithium secondary batteries, lithium metal is repeatedly deposited and dissolved at the negative electrode during charging and discharging. In lithium secondary batteries, lithium metal is almost always present at the negative electrode. Therefore, in lithium secondary batteries, there are more opportunities for contact between lithium metal and the non-aqueous electrolyte than in lithium ion batteries, and side reactions between the two tend to become more pronounced.
[0013] In addition, lithium metal is more likely to precipitate in a dendrite-like shape in lithium secondary batteries than in lithium ion batteries. When lithium metal precipitates in a dendrite-like shape, the specific surface area of the lithium metal increases. This further increases side reactions between the lithium metal and the electrolyte. As a result, the discharge capacity decreases significantly, and cycle characteristics tend to decrease significantly.
[0014] In the lithium secondary battery of this embodiment, during charging, the cation X contained in the electrolyte is preferentially co-precipitated with the lithium ions, and an alloy containing lithium and the cation X is precipitated on the negative electrode. This type of co-precipitation is considered to proceed more stably than when only the lithium ions receive electrons and precipitate.
[0015] In addition, the oxalate complex anion Y contained in the electrolyte has the effect of stabilizing the lithium ion and the cation X, and is considered to play a role in preventing the localized co-deposition of the lithium ion and the cation X. As a result, it is considered that the precipitation of dendrites is suppressed, and the cycle characteristics are significantly improved. It is considered that the stabilization of the cation is influenced by the fact that the oxalate complex anion Y is easily coordinated to include the cation.
[0016] Furthermore, when the oxalate complex anion Y is decomposed at the negative electrode, a stable coating is formed on the surface of the negative electrode. It is believed that the oxalate complex anion Y decomposes preferentially over other components contained in the electrolyte, forming a uniform and flexible coating on the surface of the negative electrode. It is also believed that the initiation points of lithium metal deposition become uniform and the co-deposition of lithium ions and cations X is further facilitated by incorporating lithium ions and cations X, which have different ionic radii, into such a coating. As a result, the deposition of dendrites is further suppressed.
[0017] The oxalate complex anion Y may be, for example, B(C 2 O 4 ) 2 - , B.F. 2 (C 2 O 4 ) - , P(C 2 O 4 ) 3 - , P.F. 2 (C 2 O 4 ) 2 - and P.F. 4 (C 2 O 4 ) - At least one selected from the group consisting of the following may be used. These are considered to have a large effect of stably advancing the co-deposition of lithium ions and cations X. Among them, fluorine-containing oxalate complex anion Y is considered to have a large effect.
[0018] The cation X and the oxalate complex anion Y may be contained in the non-aqueous electrolyte as their salts, or a salt of the cation X with another anion and a lithium salt of the oxalate complex anion Y may be contained in the non-aqueous electrolyte.
[0019] The configuration of the lithium secondary battery will be described in more detail below.
[0020] [Negative electrode] The negative electrode usually includes a negative electrode current collector. For example, a metal foil can be used as the negative electrode current collector. The negative electrode has a layer containing lithium metal (lithium metal layer or lithium alloy layer) at least during charging. The open circuit potential of the negative electrode during full charging is, for example, 0 V or more and 70 mV or less with respect to lithium metal.
[0021] The fully charged state refers to a state in which the battery is charged to a state of charge (SOC) of 0.98×C or more, where C is the rated capacity of the battery. The open circuit potential of the negative electrode at the fully charged state may be measured by disassembling a fully charged battery under an argon atmosphere, removing the negative electrode, assembling a cell with lithium metal as the counter electrode, and then measuring the potential. The nonaqueous electrolyte of the cell may have the same composition as the nonaqueous electrolyte in the disassembled battery, and for example, the electrolyte used in Example 1 described later may be used as a model electrolyte.
[0022] The metal constituting the negative electrode current collector is preferably a metal that does not react with lithium metal, and examples thereof include copper (Cu), nickel (Ni), iron (Fe), and alloys containing these metal elements. As the alloy, copper alloys, stainless steel (SUS), and the like are preferable. Among them, copper and / or copper alloys are preferable because of their excellent electrical conductivity. The copper content in the negative electrode current collector is preferably 50 mass% or more, and may be 80 mass% or more. The thickness of the negative electrode current collector is not particularly limited, and is, for example, 5 μm to 20 μm.
[0023] The negative electrode may include a negative electrode current collector and a plurality of layers laminated on the negative electrode current collector. The plurality of layers may include, for example, a first layer and a second layer. The first layer includes a material capable of absorbing lithium ions, and the second layer includes lithium metal. In this case, the first layer is disposed closer to the negative electrode current collector than the second layer. The first layer helps to deposit lithium ions uniformly on the negative electrode current collector at the beginning of charging with the negative electrode current collector.
[0024] The material capable of absorbing lithium ions contained in the first layer may be, for example, a material that can be used as a negative electrode active material of a lithium ion battery. Specifically, a carbon material capable of electrochemically absorbing and releasing lithium ions, a metal that alloys with lithium, a metal compound, etc. may be used. Also, a film of a metal that alloys with lithium may be formed as the first layer. Specific examples of metals that form the metal film include, for example, aluminum, zinc, silicon, and tin.
[0025] [Positive electrode] The positive electrode comprises a positive electrode mixture layer containing a positive electrode active material and a positive electrode current collector. The positive electrode mixture layer can be formed by applying a positive electrode slurry, in which a positive electrode mixture containing a positive electrode active material, a binder, a conductive agent, etc. is dispersed in a dispersion medium, to the surface of the positive electrode current collector and drying it. The coating film after drying may be rolled as necessary. The positive electrode mixture layer may be formed on one surface of the positive electrode current collector or on both surfaces.
[0026] When the positive electrode active material contains a composite oxide containing lithium and a transition metal, the total amount of lithium contained in the positive electrode and the negative electrode M Li and the amount of transition metal in the positive electrode, M TM Molar ratio to: M Li / M TM may be 1.1 or less. In other words, in a lithium secondary battery (lithium metal secondary battery), most (or all) of the lithium involved in charging and discharging is derived from the composite oxide containing lithium and a transition metal, which is the positive electrode active material.
[0027] Here, the total amount of lithium contained in the positive electrode and the negative electrode M LiIt refers to the total amount of lithium possessed by the positive electrode active material layer per unit area and the negative electrode per unit area facing it (more specifically, the total of the first layer and the second layer). Also, the amount M of the transition metal possessed by the positive electrode TM It refers to the amount of transition metal possessed by the positive electrode active material layer per unit area described above.
[0028] The molar ratio of lithium to transition metal contained in the composite oxide: lithium / transition metal may be, for example, 0.9 to 1.1.
[0029] Examples of such positive electrode active materials include layered rock salt type composite oxides. Specifically, as the positive electrode active material, for example, Li a CoO 2 、Li a NiO 2 、Li a MnO 2 、Li a Co b Ni 1-b O 2 、Li a Co b M 1-b O c (M is at least one selected from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B), Li a Ni b M 1-b O c (M is at least one selected from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Co, Cu, Zn, Al, Cr, Pb, Sb, and B), LiMPO 4、 (M is at least one selected from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B) may be mentioned. Here, 0 < a ≤ 1.1, 0 ≤ b ≤ 0.9, and 2 ≤ c ≤ 2.3. Note that the a value indicating the molar ratio of lithium increases and decreases during charge and discharge.
[0030] Among them, a layered rock salt type composite oxide containing nickel element is preferable. Such a composite oxide is Li a Ni x M 1-x O2 (M is at least one selected from the group consisting of Mn, Co, and Al, and satisfies 0 < a ≤ 1.1 and 0.3 ≤ x ≤ 1). From the viewpoint of increasing the capacity, it is preferable to satisfy 0.85 ≤ x ≤ 1. Further, from the viewpoint of the stability of the crystal structure, lithium-nickel-cobalt-aluminum composite oxide (NCA) containing Co and Al as M: Li a Ni x Co y Al z O 2 (0 < a ≤ 1.1, 0.85 ≤ x < 1, 0 < y < 0.15, 0 < z ≤ 0.1, x + y + z = 1) is more preferable. Specific examples of NCA include LiNi 0.8 Co 0.15 Al 0.05 O 2 , LiNi 0.8 Co 0.18 Al 0.02 O 2 , LiNi 0.9 Co 0.05 Al 0.05 O 2 etc.
[0031] Examples of the binder include resin materials such as fluororesins such as PTFE and PVdF; polyolefin resins such as polyethylene and polypropylene; polyamide resins such as aramid resins; polyimide resins such as polyimide and polyamideimide; acrylic resins such as polyacrylic acid, methyl polyacrylate, and ethylene-acrylic acid copolymer; vinyl resins such as PAN and polyvinyl acetate; polyvinylpyrrolidone; polyethersulfone; rubber-like materials such as styrene-butadiene copolymer rubber (SBR), etc. These may be used alone or in combination of two or more.
[0032] Examples of conductive agents include graphite such as natural graphite and artificial graphite, carbon blacks such as acetylene black, conductive fibers such as carbon fiber and metal fiber, carbon fluoride, metal powders such as aluminum, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and organic conductive materials such as phenylene derivatives. These may be used alone or in combination of two or more.
[0033] The shape and thickness of the positive electrode current collector can be selected from the shape and range corresponding to those of the negative electrode current collector. Examples of the material of the positive electrode current collector include stainless steel, aluminum (Al), aluminum alloy, and titanium.
[0034] [Non-aqueous electrolyte] The non-aqueous electrolyte has lithium ion conductivity and contains cations and anions, where the cations include lithium ions and a cation X, and the anions include an oxalate complex anion Y.
[0035] The non-aqueous electrolyte may be an electrolytic solution containing a solvent (i.e., liquid), a gel, or a solid. A gel non-aqueous electrolyte includes a liquid non-aqueous electrolyte (electrolytic solution) and a matrix polymer. As the matrix polymer, for example, a polymer material that absorbs a non-aqueous solvent and gels is used. Examples of such polymer materials include fluororesin, acrylic resin, and / or polyether resin.
[0036] The electrolyte will now be described in further detail by way of example.
[0037] The electrolyte solution can be prepared, for example, by dissolving a lithium salt and an oxalate complex salt in a solvent. The lithium salt may be used alone or in combination of two or more. The oxalate complex salt may be used alone or in combination of two or more. In this case, a part of the lithium salt may be an oxalate complex salt, and at least a part of the oxalate complex salt may be a salt of a cation X.
[0038] Examples of lithium salts include lithium salts of chlorine-containing acids (LiClO 4 , LiAlCl 4 , LiB 10 Cl 10 etc.), lithium salts of fluorine-containing acids (LiPF 6 , LiPF 2 O 2 , LiBF 4 , LiSbF 6 , LiAsF 6 , LiCF 3 SO 3 , LiCF 3 CO 2 etc.), lithium halides (LiCl, LiBr, LiI, etc.), etc. can be used.
[0039] The lithium salt may be a lithium salt of a fluorine-containing acid imide. Such a salt contains a fluorine-containing imide anion. Examples of the fluorine-containing imide anion include bis(fluorosulfonyl)imide anion (N(SO 2 F) 2 - ) (also called FSI), bis(trifluoromethylsulfonyl)imide anion (N(SO 2 CF 3 ) 2 - ) (also known as TFSI), bis(perfluoroethylsulfonyl)imide anion (N(SO 2 C 2 F 5 ) 2 - ) etc.
[0040] Examples of the solvent include cyclic carbonates, chain carbonates, cyclic carboxylates, and chain carboxylates. Examples of the cyclic carbonates include propylene carbonate (PC), ethylene carbonate (EC), vinylene carbonate (VC), fluoroethylene carbonate (FEC), and vinylethylene carbonate (VEC). Examples of the chain carbonates include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Examples of the cyclic carboxylates include γ-butyrolactone (GBL), and γ-valerolactone (GVL). Examples of the chain carboxylates include methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP). The solvent may be used alone or in combination of two or more.
[0041] Other examples of the solvent include cyclic ethers, chain ethers, nitriles such as acetonitrile, and amides such as dimethylformamide.
[0042] Examples of cyclic ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, crown ethers, and the like.
[0043] Examples of chain ethers include 1,2-dimethoxyethane, dimethyl ether, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0044] The contents of the lithium salt, the cation X, and the oxalate complex anion Y in the electrolyte solution can be measured, for example, by using NMR, ion chromatography, or the like.
[0045] The concentration of lithium ions in the electrolyte may be, for example, 0.5 mol / L or more and 3.5 mol / L or less, 1 mol / L or more and 2 mol / L or less, or 1 mol / L or more and 1.5 mol / L or less. By setting the lithium ion concentration within the above range, an electrolyte having excellent ion conductivity and appropriate viscosity can be obtained. The oxalate complex anion Y can also be added to the electrolyte in the form of a lithium salt.
[0046] The concentration of the cation X in the electrolyte may be, for example, 0.01 mol / L or more and 0.5 mol / L or less, or 0.05 mol / L or more or 0.1 mol / L or more. In this case, a sufficient effect of improving the capacity retention rate can be obtained. In addition, sufficient lithium ion conductivity can be obtained.
[0047] The concentration of the oxalate complex anion Y in the electrolyte may be, for example, 0.5 mol / L or less. In this case, gas generation due to decomposition of the oxalate complex anion Y is significantly suppressed, and an electrolyte having excellent ion conductivity and appropriate viscosity is easily obtained. In order to more significantly improve the cycle characteristics, the concentration of the oxalate complex anion Y in the electrolyte may be, for example, 0.01 mol / L or more.
[0048] In order to obtain an electrolyte solution having better lithium ion conductivity, for example, the electrolyte solution may contain LiPF 6 In the case where the electrolyte contains 6 - The ratio of the molar content of the oxalate complex anion Y to the molar content of the ions may be 0.1 or more and 0.5 or less.
[0049] [Separator] A separator is interposed between the positive electrode and the negative electrode. The separator has high ion permeability and has appropriate mechanical strength and insulation properties. As the separator, a microporous thin film, a woven fabric, a nonwoven fabric, etc. can be used. As the material of the separator, polyolefin such as polypropylene and polyethylene is preferable.
[0050] [Lithium secondary battery] FIG. 3 is a vertical sectional view of an example of a cylindrical lithium secondary battery according to one embodiment of the present invention.
[0051] The lithium secondary battery 100 is a wound type battery including a wound electrode group 40 and a non-aqueous electrolyte (not shown). The wound electrode group 40 includes a strip-shaped positive electrode 10, a strip-shaped negative electrode 20, and a separator 30. A positive electrode lead 13 is connected to the positive electrode 10, and a negative electrode lead 23 is connected to the negative electrode 20.
[0052] The positive electrode lead 13 has one end connected to the positive electrode 10 in the length direction, and the other end connected to the sealing plate 90. The sealing plate 90 is provided with a positive electrode terminal 15. The negative electrode lead 23 has one end connected to the negative electrode 20, and the other end connected to the bottom of the battery case 70, which serves as the negative electrode terminal. The battery case 70 is a cylindrical battery can with a bottom, one end in the length direction is open, and the bottom of the other end serves as the negative electrode terminal. The battery case (battery can) 70 is made of metal, for example, iron. The inner surface of the iron battery case 70 is usually nickel-plated. An upper insulating ring 80 and a lower insulating ring 60, which are made of resin, are arranged above and below the wound electrode group 40, respectively.
[0053] In the illustrated example, a cylindrical lithium secondary battery having a wound electrode group has been described, but the present embodiment is not limited to this case and can be applied to other types of lithium secondary battery. The shape of the lithium secondary battery can be appropriately selected from various shapes such as a cylindrical shape, a coin shape, a square shape, a sheet shape, and a flat shape depending on the application. The shape of the electrode group is not particularly limited, and may be a laminated type. In addition, the configuration of the lithium secondary battery other than the negative electrode may be a known one without any particular limitation.
[0054] The present invention will be specifically described below based on examples and comparative examples, but the present invention is not limited to the following examples.
[0055] [Example 1] (1) Preparation of the positive electrode The positive electrode active material is a lithium-containing composite oxide (LiNi 0.9 Co 0.05 Al 0.05 O 2 ), acetylene black, polyvinylidene fluoride, and N-methyl-2-pyrrolidone (NMP) were mixed in a predetermined mass ratio to prepare a positive electrode slurry. Next, the positive electrode slurry was applied to the surface of an aluminum foil serving as a positive electrode current collector, and the coating was dried and then rolled to form a positive electrode mixture layer on both sides of the aluminum foil.
[0056] (2) Preparation of the negative electrode An electrolytic copper foil (thickness: 10 μm) was cut to a predetermined electrode size to obtain a negative electrode current collector.
[0057] (3) Preparation of electrolyte A mixture of fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), and dimethyl ether (DME) in a volume ratio of 4:1:15 was added to the lithium salt LiPF 6 , and cesium difluorooxalatoborate (CsBF) as a salt of cation X and oxalate complex anion Y. 2 (C 2 O 4 )) (referred to as CsFOB in Table 1) was added to prepare the electrolyte. 6 The concentration of CsBF in the electrolyte was 1.0 mol / L. 2 (C 2 O 4 The concentration of was 0.1 mol / liter.
[0058] (4) Battery construction A lead tab was attached to each electrode, and the positive and negative electrodes were spirally wound with a separator between them so that the leads were located at the outermost periphery to prepare an electrode group. The electrode group was inserted into an exterior body made of a laminate film with an aluminum foil barrier layer, and vacuum dried at 105°C for 2 hours. An electrolyte was then poured in, and the opening of the exterior body was sealed to obtain a battery A1.
[0059] [Example 2] In preparing the electrolyte, CsBF 2 (C 2 O 4 ) instead of magnesium difluorooxalate borate (Mg(BF 2 (C 2 O 4 )) 2 ) (Table 1 shows MgFOB 2 The electrolyte used was Mg(BF 2 (C 2 O 4 )) 2The concentration of was 0.1 mol / L. Except for this, the same procedure as in Example 1 was carried out to obtain a battery A2.
[0060] [Comparative Example 1] In preparing the electrolyte, CsBF 2 (C 2 O 4 ) instead of CsPF 6 CsPF in the electrolyte 6 The concentration of was 0.1 mol / L. Except for this, the same procedure as in Example 1 was carried out to obtain a battery B1.
[0061] [Comparative Example 2] In preparing the electrolyte, CsBF 2 (C 2 O 4 ) instead of Mg(N(SO 2 CF 3 ) 2 ) 2 (Table 1 shows MgTFSI 2 The electrolyte solution (N(SO 2 CF 3 ) 2 ) 2 The concentration of was 0.1 mol / L. Except for this, the same procedure as in Example 1 was carried out to obtain a battery B2.
[0062] [Comparative Example 3] In preparing the electrolyte, CsBF 2 (C 2 O 4 ) was not used. Except for this, the same procedures as in Example 1 were carried out to obtain a battery B3.
[0063] [Rating 1] A charge / discharge test was carried out on the obtained batteries A1, A2, and B1 to B3.
[0064] In the charge / discharge test, the battery was charged under the following conditions in a thermostatic chamber at 25°C, then rested for 20 minutes and discharged under the following conditions. This charge / discharge cycle was counted as one cycle, and the charge / discharge test was performed for 50 cycles. The capacity retention rate (%) was calculated by dividing the discharge capacity at the 50th cycle by the discharge capacity at the 1st cycle. The evaluation results are shown in Table 1.
[0065] (Charging) The battery was charged at a constant current of 0.3 It until the battery voltage reached 4.1 V, and then charged at a constant voltage of 4.1 V until the current value reached 0.02 It.
[0066] (Discharge) The battery was discharged at a constant current of 0.3 It until the battery voltage reached 2.85 V.
[0067] [Table 1]
[0068] It can be seen from Table 1 that the capacity retention rate is significantly improved when the electrolyte contains both the cation X and the oxalate complex anion Y. On the other hand, the capacity retention rate of batteries B1 and B2, in which only the cation X is contained in the electrolyte, is lower than that of battery B3, which does not contain the cation X.
[0069] [Reference example 1] A negative electrode slurry was prepared by mixing graphite, sodium carboxymethylcellulose (CMC-Na), styrene-butadiene rubber (SBR), and water in a predetermined mass ratio as the negative electrode active material. The negative electrode slurry was then applied to the surface of a copper foil, which was a negative electrode current collector, and the coating was dried and then rolled to form a negative electrode mixture layer on both sides of the copper foil.
[0070] A battery R1 was obtained in the same manner as in Example 1, except that the above negative electrode was used.
[0071] [Reference example 2] A battery R2 in which the electrolyte did not contain either the cation X or the oxalate complex anion Y was obtained in the same manner as in Comparative Example 3, except that the negative electrode of Reference Example 1 was used.
[0072] [Rating 2] The resulting batteries R1 and R2 were subjected to a charge / discharge test in the same manner as in Evaluation 1. The evaluation results are shown in Table 2.
[0073] [Table 2]
[0074] In Table 2, no clear difference in the capacity retention rate was observed between batteries R1 and R2. From this, it can be understood that the synergistic effect of the electrolyte containing both cation X and oxalate complex anion Y is an effect specific to lithium secondary batteries, in which lithium metal precipitates at the negative electrode during charging and dissolves in the electrolyte during discharging. [Industrial Applicability]
[0075] Since the lithium secondary battery according to the present invention has excellent cycle characteristics, it can be used in electronic devices such as mobile phones, smartphones, and tablet terminals, electric vehicles including hybrids and plug-in hybrids, and home storage batteries combined with solar cells. [Explanation of symbols]
[0076] 10 positive electrode 13 Positive lead 15 Positive terminal 20 negative electrode 23 Negative lead 30 Separator 40 Wound electrode group 60 Lower insulation ring 70 Battery case 80 Upper insulation ring 90 Sealing plate 100 Lithium secondary battery
Claims
1. A battery comprising a positive electrode, a negative electrode, a lithium ion conductive non-aqueous electrolyte, and a separator disposed between the positive electrode and the negative electrode; In the negative electrode, lithium metal is precipitated during charging, and the lithium metal is dissolved in the non-aqueous electrolyte during discharging, The non-aqueous electrolyte contains a cation and an anion, The cation comprises a lithium ion and at least one cation X selected from the group consisting of Na, K, Rb, Cs, Fr, Mg, Ca, Sr, Ba and Al; the anion comprises an oxalate complex anion Y; The oxalate complex anion Y contains fluorine, A lithium secondary battery, wherein the concentration of the oxalate complex anion Y in the non-aqueous electrolyte is 0.5 mol / L or less.
2. The oxalate complex anion Y is BF 2 (C 2 O 4 ) - , P.F. 2 (C 2 O 4 ) 2 - , and P.F. 4 (C 2 O 4 ) - 2. The lithium secondary battery according to claim 1, wherein the lithium secondary battery is at least one selected from the group consisting of:
3. The non-aqueous electrolyte contains PF 6 − ions, 3. The lithium secondary battery according to claim 1, wherein a ratio of a molar content of the oxalate complex anion Y in the non-aqueous electrolyte to a molar content of the PF 6 − ion in the non-aqueous electrolyte is 0.1 or more and 0.5 or less.
4. 4. The lithium secondary battery according to claim 1, wherein the concentration of the fluorine-containing oxalate complex anion Y in the non-aqueous electrolyte is 0.01 mol / L or more and 0.5 mol / L or less.
5. 5. The lithium secondary battery according to claim 1, wherein the concentration of the cation X in the non-aqueous electrolyte is 0.01 mol / L or more and 0.5 mol / L or less.
6. 6. The lithium secondary battery according to claim 1, wherein a concentration of the lithium ions in the non-aqueous electrolyte is 0.5 mol / liter or more and 3.5 mol / liter or less.
7. The positive electrode includes a positive electrode mixture layer including a positive electrode active material and a positive electrode current collector, The positive electrode active material includes a composite oxide including lithium and a transition metal, The total amount of lithium contained in the positive electrode and the negative electrode M Li and the amount M of the transition metal contained in the positive electrode. TM Molar ratio with: M Li / M TM The lithium secondary battery according to any one of claims 1 to 6, wherein is 1.1 or less.
Citation Information
Patent Citations
Lithium-ion secondary battery
JP2008282617A
Lithium ion secondary battery
JP2008305574A
Method for manufacturing nonaqueous electrolyte secondary battery
JP2014143061A
Additives for galvanic cells
JP2015534711A
Electrolyte for nonaqueous secondary battery, electrolyte solution using the same, and battery
JP2018133146A