Copper-clad laminate, resin-coated copper foil, and circuit board using the same

The copper-clad laminate and resin-coated copper foil address the challenges of transmission loss and heat resistance in high-frequency signal boards by incorporating a surface-treated copper foil and specialized resin composition, ensuring reduced loss and enhanced adhesion and heat resistance for reliable circuit performance.

JP7580069B2Active Publication Date: 2024-11-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021519493
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-15
Filing Date
2020-05-14
Publication Date
2024-11-11
Estimated Expiration
2040-05-14

AI Technical Summary

Technical Problem

Existing copper-clad laminates and copper foils used in high-frequency high-speed signal transmission boards face challenges in balancing transmission loss, conductor loss, adhesion, and heat resistance, particularly with the advent of 5G and WiGig technologies that require even higher frequency signals.

Method used

A copper-clad laminate and resin-coated copper foil design featuring a surface-treated copper foil with a finely roughened copper particle layer, a heat-resistant nickel treatment layer, a chromium rust-proofing layer, and a silane coupling agent layer, combined with a resin composition containing specific polymers and modified polyphenylene ether compounds to enhance adhesion and heat resistance while reducing transmission loss.

Benefits of technology

The solution provides a highly reliable circuit board with reduced transmission loss, excellent adhesion, and improved heat resistance, suitable for high-frequency signal transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580069000037
    Figure 0007580069000037
  • Figure 0007580069000038
    Figure 0007580069000038
  • Figure 0007580069000039
    Figure 0007580069000039
Patent Text Reader

Abstract

One aspect of the present invention pertains to a copper-clad laminated plate provided with: an insulation layer containing a cured product of a resin composition; and a surface-treated copper foil disposed on one surface or both surfaces of the insulation layer. The copper-clad laminated plate is characterized in that: the resin composition contains a polymer having a structural unit represented by formula (1) in the molecule (in the formula (1), Z represents an arylene group, R1-R3 each independently represent a hydrogen atom or an alkyl group, R4-R6 each independently represent a hydrogen atom or an alkyl group having 1-6 carbon atoms); and the surface-treated copper foil has a copper fine roughened particle treatment layer on at least one surface side of the copper foil, wherein the fine roughened particle treatment layer is formed from fine copper particles having a particle size of 40-200 nm, a heat resistant treatment layer containing nickel is provided on the fine roughened particle treatment layer, a rustproofing treatment layer containing at least chromium is provided on the heat resistant treatment layer, a silane coupling agent layer is provided on the rustproofing treatment layer, and the deposition amount of nickel in the heat resistant treatment layer is 30-60 mg / m2.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copper-clad laminate, a resin-coated copper foil, and a circuit board using the same. [Background technology]

[0002] Various metal foils, especially copper foil, are used as conductors in high-frequency, high-speed signal transmission boards, but in the future they will need to support 5G and WiGig (Wireless Gigabit), which use signals at even higher frequencies than currently available, and therefore there is a demand to further reduce the transmission loss of the boards.

[0003] To address this issue, it is necessary to improve the resin base material and copper foil that make up the board in order to reduce transmission loss. In other words, it is necessary to reduce the transmission loss caused by the dielectric of the resin base material and also reduce the conductor loss of the copper foil.

[0004] In the past, improvements on the copper foil side have been made to reduce conductor loss by reducing surface roughness, etc. However, reducing the surface roughness reduces adhesion to resin and heat resistance, which are essential basic properties of copper foil used in circuit boards, while increasing the surface roughness increases transmission loss, and it has been considered difficult to achieve both transmission properties and basic properties. This is thought to be because reducing the roughness reduces the adhesive area with the resin, making it difficult to obtain adhesion through the anchor effect, resulting in lower peel strength and poor heat resistance, while increasing the roughness increases the resistance of the current flowing through the copper foil surface, resulting in higher transmission loss.

[0005] In addition, it has been reported that in surface-treated copper foil for forming high-frequency signal transmission circuits, the roughening layer, which affects the transmission characteristics, is made of a non-conductive copper composite compound rather than the conventional metallic copper, thereby preventing the flow of electricity and reducing the conductive loss due to the roughening treatment (Patent Document 1).

[0006] It is also known that in surface-treated copper foil for printed wiring boards, the average height of the roughening particles in the silane coupling agent layer, which affects the transmission characteristics, is adjusted, and the amount of nickel in the nickel-containing metal treatment layer is adjusted (Patent Document 2).

[0007] On the other hand, from the viewpoint of resin substrates, it has been reported that low dielectric properties can be improved by using a resin containing a modified polyphenylene ether compound (Patent Document 3).

[0008] However, the technique described in Patent Document 1 does not include barrier treatment, chromate treatment, or the like, and therefore has a problem of inferior heat resistance in particular.

[0009] On the other hand, the technique described in Patent Document 2 has a problem in that since the amount of the metal treatment layer functioning as a barrier treatment layer is small, it is difficult to ensure heat resistance in a high temperature range (for example, 150° C. or higher).

[0010] Furthermore, in order to obtain better transmission characteristics for the resin substrate, currently, resins containing compounds having a lower dielectric tangent are being sought. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Patent No. 6110581 [Patent Document 2] Patent No. 6182584 [Patent Document 3] JP 2013-23517 A Summary of the Invention

[0012] The present invention has been made in consideration of the above circumstances, and has an object to provide a copper-clad laminate and a resin-coated copper foil that are capable of reducing transmission loss in high-speed signal transmission boards and have excellent adhesion and heat resistance, as well as a highly reliable circuit board using the same.

[0013] A copper-clad laminate according to one embodiment of the present invention is a copper-clad laminate comprising an insulating layer containing a cured product of a resin composition and a surface-treated copper foil on one or both sides of the insulating layer, wherein the resin composition contains a polymer having a structural unit represented by the following formula (1) in its molecule: [ka] (In formula (1), Z represents an arylene group, R1 to R3 each independently represent a hydrogen atom or an alkyl group, and R4 to R6 each independently represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.) and the surface-treated copper foil has a copper fine particle treatment layer on at least one side of the copper foil, the fine particle treatment layer being composed of fine copper particles having a particle diameter of 40 to 200 nm, a heat-resistant treatment layer containing nickel on the fine particle treatment layer, a rust-resistant treatment layer containing at least chromium on the heat-resistant treatment layer, a silane coupling agent layer on the rust-resistant treatment layer, and a nickel coating amount in the heat-resistant treatment layer of 30 to 60 mg / m 2 It is characterized in that:

[0014] A resin-coated copper foil according to another aspect of the present invention is a resin-coated copper foil comprising a resin layer containing a resin composition or a semi-cured product of the resin composition, and a surface-treated copper foil on one side of the resin layer, wherein the resin composition contains a polymer having a structural unit represented by the above formula (1) in the molecule, and the surface-treated copper foil has a copper fine particle treatment layer on at least one side of the copper foil, the fine particle treatment layer being composed of fine copper particles having a particle diameter of 40 to 200 nm, a heat-resistant treatment layer containing nickel on the fine particle treatment layer, a rust-proofing treatment layer containing at least chromium on the heat-resistant treatment layer, a silane coupling agent layer on the rust-proofing treatment layer, and a nickel coating amount in the heat-resistant treatment layer of 30 to 60 mg / m 2 It is characterized in that: [Brief description of the drawings]

[0015] [Figure 1]FIG. 1 is a schematic cross-sectional view showing the configuration of a surface-treated copper foil according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing the configuration of a metal-clad laminate according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing the configuration of a wiring board according to one embodiment of the present invention. [Figure 4] FIG. 4 is a schematic cross-sectional view showing the structure of a resin-coated copper foil according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The copper-clad laminate according to one aspect of the present invention is a copper-clad laminate comprising an insulating layer containing a cured product of a resin composition and a surface-treated copper foil on one or both sides of the insulating layer. The resin-coated copper foil according to another aspect of the present invention is a resin-coated copper foil comprising a resin layer containing a resin composition or a semi-cured product of the resin composition and a surface-treated copper foil on one side of the resin layer.

[0017] According to the present invention, it is possible to provide a copper-clad laminate and a resin-coated copper foil that are capable of reducing transmission loss in a high-speed signal transmission board and have excellent adhesion and heat resistance, and a highly reliable circuit board using the same.

[0018] The following is a detailed description of the configurations of the copper-clad laminate and the resin-coated copper foil according to the present embodiment. In the following description, the following reference numerals denote: 1 copper foil, 2 fine roughening particle treatment layer, 3 heat-resistant treatment layer, 4 rust-proofing treatment layer, 5 silane coupling agent layer, 11 copper-clad laminate, 12, 32 insulating layer, 13 surface-treated copper foil, 14 wiring, 21 wiring board, and 31 resin-coated copper foil.

[0019] <Copper-clad laminate> 2, the copper-clad laminate 11 of this embodiment is characterized by having an insulating layer 12 containing a cured product of a resin composition described below, and a copper foil (surface-treated copper foil) 13 described below on one or both sides of the insulating layer 12. With this configuration, it is possible to provide a highly reliable copper-clad laminate that has reduced transmission loss while having adhesion and heat resistance.

[0020] <Insulating layer> First, in this embodiment, the cured product of the resin composition refers to a state where the resin does not melt even when heated due to the progress of the curing reaction and crosslinking of the resin. Also, the semi-cured product of the resin composition refers to a state where the resin composition is partially cured to the extent that it can be further cured. That is, the semi-cured product is a resin composition in a semi-cured state (B stage). For example, when the resin composition is heated, the viscosity first gradually decreases, and then curing begins and the viscosity gradually increases. In such a case, the semi-cured state can be exemplified by a state between when the viscosity starts to increase and when it is completely cured.

[0021] The insulating layer of the copper-clad laminate of this embodiment contains a cured product of a resin composition described below. The insulating layer may further contain a glass substrate described below. The thickness of the insulating layer is not particularly limited, but is about 20 to 800 μm.

[0022] The resin composition constituting the insulating layer of the present embodiment is a resin composition characterized by containing a polymer having a structural unit represented by the following formula (1) in the molecule.

[0023] [ka] In formula (1), Z represents an arylene group. R1 to R3 are each independent. That is, R1 to R3 may be the same group or different groups. R1 to R3 represent a hydrogen atom or an alkyl group. R4 to R6 are each independent. That is, R4 to R6 may be the same group or different groups. R4 to R6 represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0024] The present inventors have conducted various investigations in order to provide a resin composition having superior heat resistance and low dielectric properties compared to conventional resin compositions, for example, the resin composition described in Patent Document 1. Specifically, the present inventors have focused on the above-mentioned polymer, i.e., a polymer having a structural unit represented by the following formula (1) in the molecule, and have found that a cured product obtained by curing this polymer has excellent heat resistance and low dielectric properties.

[0025] From the above, the resin composition is a resin composition that can give a cured product having low dielectric properties and high heat resistance.

[0026] (Polymer) The polymer is not particularly limited as long as it has a structural unit represented by the formula (1) in the molecule. In addition, the polymer may have a structural unit other than the structural unit represented by the formula (1) as long as it has a structural unit represented by the formula (1) in the molecule. In addition, the polymer may contain a repeating unit in which the structural unit represented by the formula (1) is repeatedly bonded, or may be a polymer in which a repeating unit in which the structural unit represented by the formula (1) is repeatedly bonded and a repeating unit in which a structural unit other than the structural unit represented by the formula (1) is repeatedly bonded are randomly bonded. That is, when it has a structural unit other than the structural unit represented by the formula (1), it may be a block copolymer or a random copolymer.

[0027] The arylene group in the formula (1) is not particularly limited. For example, the arylene group may be a monocyclic aromatic group such as a phenylene group, or a polycyclic aromatic group in which the aromatic ring is not a monocyclic ring but a polycyclic aromatic ring such as a naphthalene ring. The arylene group also includes a derivative in which the hydrogen atom bonded to the aromatic ring is replaced with a functional group such as an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group.

[0028] The alkyl group represented by R1 to R3 in the formula (1) is not particularly limited, and is preferably, for example, an alkyl group having 1 to 18 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a hexyl group, and a decyl group.

[0029] The alkyl group having 1 to 6 carbon atoms represented by R4 to R6 in the formula (1) is not particularly limited, and specific examples include a methyl group, an ethyl group, a propyl group, and a hexyl group.

[0030] The polymer preferably contains an aromatic polymer having a structural unit derived from a bifunctional aromatic compound having two carbon-carbon unsaturated double bonds bonded to an aromatic ring as the structural unit represented by the formula (1). The structural unit derived from the bifunctional aromatic compound is a structural unit obtained by polymerizing the bifunctional aromatic compound. In this specification, the aromatic polymer is also referred to as a divinyl aromatic polymer.

[0031] The bifunctional aromatic compound is not particularly limited as long as it is a bifunctional aromatic compound having two carbon-carbon unsaturated double bonds bonded to an aromatic ring. Examples of the bifunctional aromatic compound include m-divinylbenzene, p-divinylbenzene, 1,2-diisopropenylbenzene, 1,3-diisopropenylbenzene, 1,4-diisopropenylbenzene, 1,3-divinylnaphthalene, 1,8-divinylnaphthalene, 1,4-divinylnaphthalene, 1,5-divinylnaphthalene, 2,3-divinylnaphthalene, 2,7-divinylnaphthalene, and 2,6-divinylnaphthalene. , 4,4'-divinylbiphenyl, 4,3'-divinylbiphenyl, 4,2'-divinylbiphenyl, 3,2'-divinylbiphenyl, 3,3'-divinylbiphenyl, 2,2'-divinylbiphenyl, 2,4-divinylbiphenyl, 1,2-divinyl-3,4-dimethylbenzene, 1,3-divinyl-4,5,8-tributylnaphthalene, and 2,2'-divinyl-4-ethyl-4'-propylbiphenyl. These may be used alone or in combination of two or more. Among these, the bifunctional aromatic compound is preferably divinylbenzene such as m-divinylbenzene and p-divinylbenzene, and more preferably p-divinylbenzene.

[0032] The aromatic polymer may have not only the structural unit derived from the bifunctional aromatic compound but also other structural units. Examples of the other structural units include a structural unit derived from a monofunctional aromatic compound having one carbon-carbon unsaturated double bond bonded to an aromatic ring, a structural unit derived from a trifunctional aromatic compound having three carbon-carbon unsaturated double bonds bonded to an aromatic ring, a structural unit derived from an indene, and a structural unit derived from an acenaphthylene. The structural unit derived from the monofunctional aromatic compound is a structural unit obtained by polymerizing the monofunctional aromatic compound. The structural unit derived from the trifunctional aromatic compound is a structural unit obtained by polymerizing the trifunctional aromatic compound. The structural unit derived from the indenes is a structural unit obtained by polymerizing indenes. The structural unit derived from the acenaphthylene is a structural unit obtained by polymerizing acenaphthylene.

[0033] The monofunctional aromatic compound may have one carbon-carbon unsaturated double bond bonded to an aromatic ring, and the aromatic ring may have a group other than the carbon-carbon unsaturated double bond bonded.The monofunctional aromatic compound may, for example, be a monofunctional aromatic compound having one carbon-carbon unsaturated double bond bonded to an aromatic ring and no group other than the carbon-carbon unsaturated double bond bonded, or a monofunctional aromatic compound having one carbon-carbon unsaturated double bond bonded to an aromatic ring and further having an alkyl group such as an ethyl group bonded to the aromatic ring.

[0034] Examples of monofunctional aromatic compounds having one carbon-carbon unsaturated double bond bonded to an aromatic ring and no groups other than the carbon-carbon unsaturated double bond bonded include styrene, 2-vinylbiphenyl, 3-vinylbiphenyl, 4-vinylbiphenyl, 1-vinylnaphthalene, 2-vinylnaphthalene, and α-alkyl-substituted styrenes. Examples of α-alkyl-substituted styrenes include α-methylstyrene, α-ethylstyrene, α-propylstyrene, α-n-butylstyrene, α-isobutylstyrene, α-t-butylstyrene, α-n-pentylstyrene, α-2-methylbutylstyrene, α-3-methylbutyl-2-styrene, α-t-butylstyrene, α-t-butylstyrene, α-n-pentylstyrene, α-2-methylbutylstyrene, α-3-methylbutylstyrene, α-t-pentylstyrene, α-n-hexylstyrene, α-ethylstyrene, α-propylstyrene, α-n-butylstyrene, α-iso ...t-pentylstyrene, α-hexylstyrene, α-ethylstyrene, α-propylstyrene, α-n-butylstyrene, α-isobutylstyrene, α-t-butylstyrene, α-n-pentylstyrene, α-t-pentylstyrene, α-hexylstyrene, α-ethylstyrene, α-propylstyrene, α-n-butylstyrene, α-isobutylstyrene, α-t-butylstyrene, α-n-pentylstyrene, α-t-pentylstyrene, α-hexylstyrene, α-ethylstyrene, α-propyl Examples of such styrenes include styrene, α-2-methylpentylstyrene, α-3-methylpentylstyrene, α-1-methylpentylstyrene, α-2,2-dimethylbutylstyrene, α-2,3-dimethylbutylstyrene, α-2,4-dimethylbutylstyrene, α-3,3-dimethylbutylstyrene, α-3,4-dimethylbutylstyrene, α-4,4-dimethylbutylstyrene, α-2-ethylbutylstyrene, α-1-ethylbutylstyrene, α-cyclohexylstyrene, and α-cyclohexylstyrene. These may be used alone or in combination of two or more.

[0035] Examples of monofunctional aromatic compounds having one carbon-carbon unsaturated double bond bonded to an aromatic ring and further having an alkyl group bonded to the aromatic ring include nuclear alkyl-substituted aromatic compounds and alkoxy-substituted styrenes.

[0036] Examples of the nuclear alkyl-substituted aromatic compounds include ethyl vinyl aromatic compounds in which the alkyl group bonded to the aromatic ring is an ethyl group, nuclear alkyl-substituted styrenes in which an alkyl group is bonded to the styrene as the aromatic ring, and nuclear alkyl-substituted aromatic compounds other than the ethyl vinyl aromatic compounds and the nuclear alkyl-substituted styrenes (other nuclear alkyl-substituted aromatic compounds).

[0037] Examples of the ethylvinyl aromatic compounds include o-ethylvinylbenzene, m-ethylvinylbenzene, p-ethylvinylbenzene, 2-vinyl-2'-ethylbiphenyl, 2-vinyl-3'-ethylbiphenyl, 2-vinyl-4'-ethylbiphenyl, 3-vinyl-2'-ethylbiphenyl, 3-vinyl-3'-ethylbiphenyl, 3-vinyl-4'-ethylbiphenyl, 4-vinyl-2'-ethylbiphenyl, 4-vinyl-3'-ethylbiphenyl, 4-vinyl-4'-ethylbiphenyl, 1-vinyl-2-ethyl Examples of the ethylnaphthalene include naphthalene, 1-vinyl-3-ethylnaphthalene, 1-vinyl-4-ethylnaphthalene, 1-vinyl-5-ethylnaphthalene, 1-vinyl-6-ethylnaphthalene, 1-vinyl-7-ethylnaphthalene, 1-vinyl-8-ethylnaphthalene, 2-vinyl-1-ethylnaphthalene, 2-vinyl-3-ethylnaphthalene, 2-vinyl-4-ethylnaphthalene, 2-vinyl-5-ethylnaphthalene, 2-vinyl-6-ethylnaphthalene, 2-vinyl-7-ethylnaphthalene, and 2-vinyl-8-ethylnaphthalene.

[0038] Examples of the nuclear alkyl-substituted styrenes include m-methylstyrene, p-methylstyrene, m-propylstyrene, p-propylstyrene, mn-butylstyrene, pn-butylstyrene, mt-butylstyrene, pt-butylstyrene, mn-hexylstyrene, pn-hexylstyrene, m-cyclohexylstyrene, and p-cyclohexylstyrene.

[0039] Examples of the other nuclear alkyl-substituted aromatic compounds include 2-vinyl-2'-propylbiphenyl, 2-vinyl-3'-propylbiphenyl, 2-vinyl-4'-propylbiphenyl, 3-vinyl-2'-propylbiphenyl, 3-vinyl-3'-propylbiphenyl, 3-vinyl-4'-propylbiphenyl, 4-vinyl-2'-propylbiphenyl, 4-vinyl-3'-propylbiphenyl, 4-vinyl-4'-propylbiphenyl, 1-vinyl-2-propylnaphthalene, 1-vinyl-3-propylnaphthalene, and Examples of propylnaphthalene include 1-vinyl-4-propylnaphthalene, 1-vinyl-5-propylnaphthalene, 1-vinyl-6-propylnaphthalene, 1-vinyl-7-propylnaphthalene, 1-vinyl-8-propylnaphthalene, 2-vinyl-1-propylnaphthalene, 2-vinyl-3-propylnaphthalene, 2-vinyl-4-propylnaphthalene, 2-vinyl-5-propylnaphthalene, 2-vinyl-6-propylnaphthalene, 2-vinyl-7-propylnaphthalene, and 2-vinyl-8-propylnaphthalene.

[0040] Examples of the alkoxy-substituted styrene include o-ethoxystyrene, m-ethoxystyrene, p-ethoxystyrene, o-propoxystyrene, m-propoxystyrene, p-propoxystyrene, on-butoxystyrene, mn-butoxystyrene, pn-butoxystyrene, o-isobutoxystyrene, m-isobutoxystyrene, p-isobutoxystyrene, ot-butoxystyrene, mt-butoxystyrene, pt-butoxystyrene, on-pentoxystyrene, mn-pentoxystyrene, pn-pentoxystyrene, and α-methyl-o-butoxystyrene. , α-methyl-m-butoxystyrene, α-methyl-p-butoxystyrene, ot-pentoxystyrene, mt-pentoxystyrene, pt-pentoxystyrene, on-hexoxystyrene, mn-hexoxystyrene, pn-hexoxystyrene, α-methyl-o-pentoxystyrene, α-methyl-m-pentoxystyrene, α-methyl-p-pentoxystyrene, o-cyclohexoxystyrene, m-cyclohexoxystyrene, p-cyclohexoxystyrene, o-phenoxystyrene, m-phenoxystyrene, and p-phenoxystyrene.

[0041] The monofunctional aromatic compound may be one of the above-listed compounds or a combination of two or more of them. Among the above-listed compounds, styrene and p-ethylvinylbenzene are preferred as the monofunctional aromatic compound.

[0042] Examples of trifunctional aromatic compounds having three carbon-carbon unsaturated double bonds bonded to an aromatic ring include 1,2,4-trivinylbenzene, 1,3,5-trivinylbenzene, 1,2,4-triisopropenylbenzene, 1,3,5-triisopropenylbenzene, 1,3,5-trivinylnaphthalene, and 3,5,4'-trivinylbiphenyl. The trifunctional aromatic compounds may be used alone or in combination of two or more of the above-listed compounds.

[0043] Examples of the indenes include indene, alkyl-substituted indenes, and alkylcyindenes. Examples of the alkyl-substituted indenes include methylindene, ethylindene, propylindene, butylindene, t-butylindene, sec-butylindene, n-pentylindene, 2-methyl-butylindene, 3-methyl-butylindene, n-hexylindene, 2-methyl-pentylindene, 3-methyl-pentylindene, and 4-methyl-pentylindene. Examples of the alkoxyindenes include methoxyindene, ethoxyindene, butoxyindene, butoxyindene, t-butoxyindene, sec-butoxyindene, n-pentoxyindene, 2-methyl-butoxyindene, 3-methyl-butoxyindene, n-hexoxyindene, 2-methyl-pentoxyindene, 3-methyl-pentoxyindene, 4-methyl-pentoxyindene, etc. As the indenes, the above-exemplified compounds may be used alone or in combination of two or more kinds.

[0044] Examples of the acenaphthylenes include acenaphthylene, alkylacenaphthylenes, halogenated acenaphthylenes, and phenylacenaphthylenes. Examples of the alkylacenaphthylenes include 1-methylacenaphthylene, 3-methylacenaphthylene, 4-methylacenaphthylene, 5-methylacenaphthylene, 1-ethylacenaphthylene, 3-ethylacenaphthylene, 4-ethylacenaphthylene, and 5-ethylacenaphthylene. Examples of the halogenated acenaphthylenes include 1-chloroacenaphthylene, 3-chloroacenaphthylene, 4-chloroacenaphthylene, 5-chloroacenaphthylene, 1-bromoacenaphthylene, 3-bromoacenaphthylene, 4-bromoacenaphthylene, and 5-bromoacenaphthylene. Examples of the phenylacenaphthylenes include 1-phenylacenaphthylene, 3-phenylacenaphthylene, 4-phenylacenaphthylene, 5-phenylacenaphthylene, etc. As the acenaphthylenes, the above-exemplified compounds may be used alone or in combination of two or more kinds.

[0045] When the aromatic polymer has not only the structural unit derived from the bifunctional aromatic compound but also other structural units, it is a copolymer of the structural unit derived from the bifunctional aromatic compound and other structural units such as the structural unit derived from the monofunctional aromatic compound, etc. This copolymer may be a block copolymer or a random copolymer.

[0046] As described above, the polymer is not particularly limited as long as it is a polymer having a structural unit represented by the formula (1) in the molecule. The structural unit represented by the formula (1) preferably includes a structural unit represented by the following formula (2). That is, the polymer is preferably a polymer having a structural unit represented by the following formula (2) in the molecule.

[0047] [ka] In formula (2), R4 to R6 are the same as R4 to R6 in formula (1). Specifically, R4 to R6 each independently represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. R7 represents an arylene group having 6 to 12 carbon atoms.

[0048] The arylene group having 6 to 12 carbon atoms in the formula (2) is not particularly limited. Examples of the arylene group include monocyclic aromatic groups such as phenylene groups, and bicyclic aromatic groups in which the aromatic ring is not monocyclic but is bicyclic aromatic such as naphthalene rings. The arylene group also includes derivatives in which a hydrogen atom bonded to the aromatic ring is substituted with a functional group such as an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group.

[0049] The structural unit represented by the formula (2) preferably contains a structural unit represented by the following formula (3). That is, in the structural unit represented by the formula (2), R7 is preferably a phenylene group. Among the phenylene groups, a p-phenylene group is more preferable.

[0050] [ka] In formula (3), R4 to R6 are the same as R4 to R6 in formula (1). Specifically, R4 to R6 each independently represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0051] The polymer preferably includes a polymer further having a structural unit represented by the following formula (4) in the molecule. That is, the polymer preferably includes a structural unit derived from a monofunctional aromatic compound having one carbon-carbon unsaturated double bond bonded to an aromatic ring as the structural unit represented by the following formula (4). Therefore, the polymer is preferably a polymer having a structural unit represented by the above formula (1) and a structural unit represented by the following formula (4) in the molecule. That is, the polymer may have a structural unit other than the structural unit represented by the above formula (1) and the structural unit represented by the following formula (4) (structural units other than (1) and (4)) as long as the polymer has a structural unit represented by the above formula (1) and a structural unit represented by the following formula (4) in the molecule. The polymer may contain structural units other than the structural units (1) and (4), or may be a polymer, a block copolymer, or a random copolymer in which a repeating unit in which a structural unit represented by the formula (1) is repeatedly bonded, a repeating unit represented by the following formula (4), and a repeating unit in which a structural unit other than the structural units (1) and (4) is repeatedly bonded are randomly bonded.

[0052] [ka] In formula (4), R8~R 10 are independent of each other. That is, R8 to R 10 may be the same or different groups. 10 R represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. 11 represents an aryl group.

[0053] In the formula (4), R to R10 The alkyl group having 1 to 6 carbon atoms represented by R4 to R6 in the formula (4) is not particularly limited, and may be the same as the alkyl group having 1 to 6 carbon atoms represented by R4 to R6 in the formula (1). 10 Specific examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, and a hexyl group.

[0054] The aryl group in the formula (4) is not particularly limited, and may be an unsubstituted aryl group, or an aryl group in which a hydrogen atom bonded to an aromatic ring is substituted with an alkyl group or the like. The unsubstituted aryl group may be a group in which one hydrogen atom is removed from an aromatic hydrocarbon having one aromatic ring, or a group in which one hydrogen atom is removed from an aromatic hydrocarbon having two or more independent aromatic rings (e.g., biphenyl, etc.). Examples of the aryl group in the formula (4) include an unsubstituted aryl group having 6 to 12 carbon atoms, and an arylene group having 6 to 18 carbon atoms in which a hydrogen atom of an aryl group having 6 to 12 carbon atoms is substituted with an alkyl group having 1 to 6 carbon atoms. Examples of the unsubstituted aryl group having 6 to 12 carbon atoms include a phenyl group, a naphthyl group, and a biphenylyl group. The aryl group in the formula (4), that is, R 11 More specifically, the aryl groups include those shown in Tables 1 and 2 below.

[0055] [Table 1]

[0056] [Table 2]

[0057] The weight average molecular weight of the polymer is preferably 1500 to 40000, more preferably 1500 to 35000. If the weight average molecular weight is too low, the heat resistance and the like tend to decrease. If the weight average molecular weight is too high, the moldability and the like tend to decrease. Therefore, if the weight average molecular weight of the resin composition is within the above range, the heat resistance and moldability are excellent. Here, the weight average molecular weight may be measured by a general molecular weight measurement method, and specifically, a value measured using gel permeation chromatography (GPC) and the like can be mentioned.

[0058] In the polymer, when the total of the structural units in the polymer is 100 mol%, the molar content of the structural unit represented by the formula (1) is preferably within the range of the above weight average molecular weight, specifically, preferably 2 to 95 mol%, more preferably 8 to 81 mol%. The molar content of the structural unit represented by the formula (2) and the molar content of the structural unit represented by the formula (3) are the same as the molar content of the structural unit represented by the formula (1), specifically, preferably 2 to 95 mol%, more preferably 8 to 81 mol%. In the case where the polymer has the structural unit represented by the formula (1) and the structural unit represented by the following formula (4) in the molecule, the molar content of the structural unit represented by the formula (1) is preferably 2 to 95 mol%, more preferably 8 to 81 mol%, and the molar content of the structural unit represented by the formula (4) is preferably 5 to 98 mol%, more preferably 19 to 92 mol%.

[0059] In the polymer, the average number of the structural units represented by the formula (1) is preferably within the range of the weight average molecular weight, specifically, preferably 1 to 160, more preferably 3 to 140. The average number of the structural units represented by the formula (2) and the average number of the structural units represented by the formula (3) are the same as the average number of the structural units represented by the formula (1), specifically, preferably 1 to 160, more preferably 3 to 140. In addition, when the polymer has a structural unit represented by the formula (1) and a structural unit represented by the following formula (4) in the molecule, the average number of the structural units represented by the formula (1) is preferably 1 to 160, more preferably 3 to 140, and the average number of the structural units represented by the formula (4) is preferably 2 to 350, more preferably 4 to 300.

[0060] A specific example of the polymer is a polymer containing a structural unit represented by the following formula (8) in the molecule and further containing at least one of a structural unit represented by the following formula (7) and a structural unit represented by the following formula (9). This polymer may be a block copolymer or a random copolymer.

[0061] [ka]

[0062] [ka]

[0063] [ka]

[0064] In a polymer containing a structural unit represented by the formula (8) in the molecule and further containing at least one of a structural unit represented by the formula (7) and a structural unit represented by the formula (9), the molar contents of the structural unit represented by the formula (7), the structural unit represented by the formula (8), and the structural unit represented by the formula (9) are preferably 0 to 92 mol%, 8 to 54 mol%, and 0 to 89 mol%, respectively. The average number of the structural units represented by the formula (7) is preferably 0 to 350, the average number of the structural units represented by the formula (8) is preferably 1 to 160, and the average number of the structural units represented by the formula (9) is preferably 0 to 270.

[0065] The equivalent of the vinyl group contained in the structural unit of the polymer represented by the formula (1) in which R1 to R3 are hydrogen atoms is preferably 250 to 1200, more preferably 300 to 1100. If the equivalent is too small, the vinyl group becomes too many, and the reactivity becomes too high, which may cause problems such as a decrease in the storage stability of the resin composition or a decrease in the flowability of the resin composition. If a resin composition having a too small equivalent is used, there may be a molding problem such as a molding defect such as the generation of voids during multilayer molding due to insufficient flowability, making it difficult to obtain a highly reliable wiring board. In addition, if the equivalent is too large, the vinyl group becomes too few, and the heat resistance of the cured product tends to be insufficient. Therefore, when the equivalent is within the above range, the heat resistance and moldability are excellent. The equivalent of the vinyl group contained in the structural unit represented by the formula (1) in which R1 to R3 are hydrogen atoms is the so-called vinyl equivalent.

[0066] (Modified PPE Compound) The resin composition of the present embodiment may further contain, in addition to the above polymer, a modified polyphenylene ether compound whose terminals have been modified with a group represented by the following formula (5) or (6).

[0067] [ka]

[0068] [ka]

[0069] This makes it possible to obtain a laminate having excellent low dielectric properties, such as a lower dielectric constant and a lower dielectric loss tangent, which is believed to be extremely useful as a variety of electronic materials.

[0070] In the formula (5), s represents an integer of 0 to 10. Z represents an arylene group. 12 ~R 14 are independent of each other. That is, R 12 ~R 14 may be the same or different groups. 12 ~R 14 represents a hydrogen atom or an alkyl group.

[0071] In addition, in the formula (6), when p is 0, it means that Z is directly bonded to the end of the polyphenylene ether.

[0072] The arylene group is not particularly limited. Examples of the arylene group include monocyclic aromatic groups such as phenylene groups, and polycyclic aromatic groups in which the aromatic ring is not monocyclic but is polycyclic aromatic such as naphthalene ring. The arylene group also includes derivatives in which a hydrogen atom bonded to the aromatic ring is substituted with a functional group such as an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group. The alkyl group is not particularly limited, and is preferably an alkyl group having 1 to 18 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a hexyl group, and a decyl group.

[0073] In formula (6), R 15represents a hydrogen atom or an alkyl group. The alkyl group is not particularly limited, and is preferably an alkyl group having 1 to 18 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a hexyl group, and a decyl group. Examples of the substituent represented by the formula (6) include an acrylate group and a methacrylate group.

[0074] Examples of the substituent containing a vinylbenzyl group include a substituent represented by the following formula (10).

[0075] [ka]

[0076] More specifically, examples of the group represented by the formula (10) include vinylbenzyl groups (ethenylbenzyl groups) such as p-ethenylbenzyl group and m-ethenylbenzyl group, vinylphenyl groups, acrylate groups, and methacrylate groups.

[0077] The modified polyphenylene ether compound has a polyphenylene ether chain in the molecule, and preferably has, for example, a repeating unit represented by the following formula (11) in the molecule.

[0078] [ka] In formula (11), t is an integer of 1 to 50. 16 ~R 19 are independent of each other. That is, R 16 ~R 19 may be the same or different groups. 16 ~R 19 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group, among which a hydrogen atom and an alkyl group are preferred.

[0079] R 16 ~R 19 Specific examples of the functional groups mentioned in the above include the following:

[0080] The alkyl group is not particularly limited, but is preferably, for example, an alkyl group having 1 to 18 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms. Specific examples include a methyl group, an ethyl group, a propyl group, a hexyl group, and a decyl group.

[0081] The alkenyl group is not particularly limited, but is preferably an alkenyl group having 2 to 18 carbon atoms, and more preferably an alkenyl group having 2 to 10 carbon atoms. Specific examples include a vinyl group, an allyl group, and a 3-butenyl group.

[0082] The alkynyl group is not particularly limited, but for example, an alkynyl group having 2 to 18 carbon atoms is preferable, and an alkynyl group having 2 to 10 carbon atoms is more preferable. Specific examples include an ethynyl group, a prop-2-yn-1-yl group (propargyl group), and the like.

[0083] The alkylcarbonyl group is not particularly limited as long as it is a carbonyl group substituted with an alkyl group, and is preferably, for example, an alkylcarbonyl group having 2 to 18 carbon atoms, and more preferably an alkylcarbonyl group having 2 to 10 carbon atoms. Specific examples include an acetyl group, a propionyl group, a butyryl group, an isobutyryl group, a pivaloyl group, a hexanoyl group, an octanoyl group, and a cyclohexylcarbonyl group.

[0084] The alkenylcarbonyl group is not particularly limited as long as it is a carbonyl group substituted with an alkenyl group, but for example, an alkenylcarbonyl group having 3 to 18 carbon atoms is preferable, and an alkenylcarbonyl group having 3 to 10 carbon atoms is more preferable. Specific examples include an acryloyl group, a methacryloyl group, and a crotonoyl group.

[0085] The alkynylcarbonyl group is not particularly limited as long as it is a carbonyl group substituted with an alkynyl group, but for example, an alkynylcarbonyl group having 3 to 18 carbon atoms is preferable, and an alkynylcarbonyl group having 3 to 10 carbon atoms is more preferable. Specific examples include a propioloyl group.

[0086] The weight average molecular weight (Mw) of the modified polyphenylene ether compound used in the present embodiment is not particularly limited. Specifically, it is preferably 500 to 5000, more preferably 800 to 4000, and further preferably 1000 to 3000. The weight average molecular weight may be measured by a general molecular weight measurement method, and specifically, it may be a value measured using gel permeation chromatography (GPC). In addition, when the modified polyphenylene ether compound has a repeating unit represented by the above formula (8) in the molecule, t is preferably a numerical value that causes the weight average molecular weight of the modified polyphenylene ether compound to be within such a range. Specifically, t is preferably 1 to 50.

[0087] When the weight average molecular weight of the modified polyphenylene ether compound is within such a range, it has the excellent low dielectric properties of polyphenylene ether, and not only is the heat resistance of the cured product excellent, but also the moldability is excellent. This is believed to be due to the following. When the weight average molecular weight of a normal polyphenylene ether is within such a range, it is a relatively low molecular weight, so the heat resistance of the cured product tends to decrease. In this respect, since the modified polyphenylene ether compound according to the present embodiment has one or more unsaturated double bonds at the terminal, it is believed that the heat resistance of the cured product is sufficiently high. In addition, when the weight average molecular weight of the modified polyphenylene ether compound is within such a range, it is a relatively low molecular weight, so it is believed that the moldability is also excellent. Therefore, it is believed that such a modified polyphenylene ether compound not only has excellent heat resistance of the cured product, but also has excellent moldability.

[0088] In addition, the average number of the substituents (number of terminal functional groups) at the molecular end per one molecule of the modified polyphenylene ether in the modified polyphenylene ether compound used in the present embodiment is not particularly limited. Specifically, it is preferably 1 to 5, more preferably 1 to 3, and even more preferably 1.5 to 3. If the number of terminal functional groups is too small, it tends to be difficult to obtain a cured product with sufficient heat resistance. If the number of terminal functional groups is too large, the reactivity becomes too high, and there is a risk of problems such as, for example, deterioration in the storage stability of the resin composition or deterioration in the fluidity of the resin composition. That is, when such a modified polyphenylene ether is used, there is a risk of moldability problems such as molding defects such as the generation of voids during multilayer molding due to insufficient fluidity, etc., and it is difficult to obtain a highly reliable printed wiring board.

[0089] The number of terminal functional groups of the modified polyphenylene ether compound may be a numerical value representing the average value of the above-mentioned substituents per molecule of all modified polyphenylene ether compounds present in 1 mole of the modified polyphenylene ether compound. The number of terminal functional groups can be measured, for example, by measuring the number of hydroxyl groups remaining in the obtained modified polyphenylene ether compound and calculating the reduction from the number of hydroxyl groups of the polyphenylene ether before modification. The reduction from the number of hydroxyl groups of the polyphenylene ether before modification is the number of terminal functional groups. The number of hydroxyl groups remaining in the modified polyphenylene ether compound can be measured by adding a quaternary ammonium salt (tetraethylammonium hydroxide) that associates with hydroxyl groups to a solution of the modified polyphenylene ether compound and measuring the UV absorbance of the mixed solution.

[0090] In addition, the intrinsic viscosity of the modified polyphenylene ether compound used in the present embodiment is not particularly limited. Specifically, it may be 0.03 to 0.12 dl / g, but is preferably 0.04 to 0.11 dl / g, and more preferably 0.06 to 0.095 dl / g. If the intrinsic viscosity is too low, the molecular weight tends to be low, and low dielectric properties such as low dielectric constant and low dielectric loss tangent tend to be difficult to obtain. If the intrinsic viscosity is too high, the viscosity is high, sufficient fluidity cannot be obtained, and the moldability of the cured product tends to decrease. Therefore, if the intrinsic viscosity of the modified polyphenylene ether compound is within the above range, excellent heat resistance and moldability of the cured product can be realized.

[0091] The intrinsic viscosity here is the intrinsic viscosity measured in methylene chloride at 25° C., and more specifically, for example, the value measured by a viscometer using a 0.18 g / 45 ml methylene chloride solution (liquid temperature 25° C.) As the viscometer, for example, the AVS500 Visco System manufactured by Schott Corporation can be mentioned.

[0092] More specific examples of the modified polyphenylene ether compound include a modified polyphenylene ether compound represented by the following formula (12) and a modified polyphenylene ether compound represented by the following formula (13). As the modified polyphenylene ether compound, these modified polyphenylene ether compounds may be used alone or these two types of modified polyphenylene ether compounds may be used in combination.

[0093] [ka]

[0094] [ka]

[0095] In formula (12) and formula (13), R 20 ~R 27 And R 28 ~R 35are each independently a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group. X1 and X2 are each independently a group represented by the above formula (5) or (6). A and B are each a repeating unit represented by the following formula (14) and formula (15), respectively. In addition, in formula (13), Y is a linear, branched, or cyclic hydrocarbon having 20 or less carbon atoms.

[0096] [ka]

[0097] [ka]

[0098] In the formulas (14) and (15), m and n each represent an integer of 0 to 20. 36 ~R 39 And R 40 ~R 43 each independently represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group.

[0099] The modified polyphenylene ether compound represented by the formula (12) and the modified polyphenylene ether compound represented by the formula (13) are not particularly limited as long as they satisfy the above-mentioned constitution. 20 ~R 27 And R 28 ~R 35 are independent of each other as described above. That is, R 20 ~R 27 And R 28 ~R 35 may be the same or different groups. 20 ~R 27 And R 28 ~R 35represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group, among which a hydrogen atom and an alkyl group are preferred.

[0100] In addition, in the formula (14) and the formula (15), m and n each preferably represent 0 to 20 as described above. Furthermore, it is preferable that m and n represent a numerical value such that the sum of m and n is 1 to 30. Therefore, it is more preferable that m represents 0 to 20, n represents 0 to 20, and the sum of m and n represents 1 to 30. In addition, R 36 ~R 39 And R 40 ~R 43 are independent of each other. That is, R 36 ~R 39 And R 40 ~R 43 may be the same or different groups. 36 ~R 39 And R 40 ~R 43 represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group, or an alkynylcarbonyl group, among which a hydrogen atom and an alkyl group are preferred.

[0101] R 20 ~R 43 is R in the above formula (11). 16 ~R 19 is the same as:

[0102] In the formula (13), as described above, Y is a linear, branched, or cyclic hydrocarbon having a carbon number of 20 or less. Examples of Y include a group represented by the following formula (16).

[0103] [ka]

[0104] In the formula (16), R44 and R 45 are each independently a hydrogen atom or an alkyl group. Examples of the alkyl group include a methyl group. Examples of the group represented by formula (16) include a methylene group, a methylmethylene group, and a dimethylmethylene group, and among these, a dimethylmethylene group is preferred.

[0105] In the formula (12) and the formula (13), X1 and X2 are each independently a group represented by the formula (5) or the formula (6). In the modified polyphenylene ether compound represented by the formula (12) and the modified polyphenylene ether compound represented by the formula (13), X1 and X2 may be the same or different substituents.

[0106] More specific examples of the modified polyphenylene ether compound represented by the formula (12) include modified polyphenylene ether compounds represented by the following formula (17).

[0107] [ka]

[0108] More specific examples of the modified polyphenylene ether compound represented by the formula (13) include a modified polyphenylene ether compound represented by the following formula (18) and a modified polyphenylene ether compound represented by the following formula (19).

[0109] [ka]

[0110] [ka]

[0111] In the above formulas (17) to (19), m and n are the same as m and n in the above formulas (14) and (15). 12 ~R 14 and s is R in the above formula (5). 12 ~R 14 In the above formula (18) and the above formula (19), Y is the same as Y in the above formula (13). In the above formula (19), R 15 is R in the above formula (6). 15 is the same as:

[0112] In the modified polyphenylene ether compound used in the present embodiment, the average number of the substituents (number of terminal functional groups) at the molecular terminals per one modified polyphenylene ether molecule may be within the above-mentioned range. For example, in the case of the modified polyphenylene ether compounds represented by the above formulas (17) to (19), specifically, the average number is preferably 1 to 2, and more preferably 1.5 to 2.

[0113] The method for synthesizing the modified polyphenylene ether compound used in the present embodiment is not particularly limited as long as it is possible to synthesize a modified polyphenylene ether compound terminally modified with a group (hereinafter also referred to as a substituent) represented by the formula (5) or (6).Specific examples include a method of reacting a polyphenylene ether with a compound in which the substituent and a halogen atom are bonded.

[0114] Examples of the compound in which the substituent and the halogen atom are bonded include compounds in which the substituents represented by the formulas (5) to (6) are bonded to the halogen atom. Specific examples of the halogen atom include chlorine, bromine, iodine, and fluorine atoms, and among these, chlorine is preferred. More specific examples of the compound in which the substituent and the halogen atom are bonded to the halogen atom include chloromethylstyrenes such as o-chloromethylstyrene, p-chloromethylstyrene, and m-chloromethylstyrene.

[0115] The raw material polyphenylene ether is not particularly limited as long as it can finally synthesize a predetermined modified polyphenylene ether compound. Specifically, polyphenylene ethers composed of 2,6-dimethylphenol and at least one of a bifunctional phenol and a trifunctional phenol, and poly(2,6-dimethyl-1,4-phenylene oxide) and the like, which are mainly composed of polyphenylene ether, can be mentioned. In addition, the bifunctional phenol is a phenolic compound having two phenolic hydroxyl groups in the molecule, for example, tetramethylbisphenol A, etc. In addition, the trifunctional phenol is a phenolic compound having three phenolic hydroxyl groups in the molecule. In particular, the polyphenylene ether compound of the present embodiment preferably contains a structure derived from 2,6-dimethylphenol and a bifunctional phenol.

[0116] The synthesis method of the modified polyphenylene ether compound includes the above-mentioned method. Specifically, the above-mentioned polyphenylene ether and the compound in which the substituent and the halogen atom are bonded are dissolved in a solvent and stirred. By doing so, the polyphenylene ether reacts with the compound in which the substituent and the halogen atom are bonded, and the modified polyphenylene ether compound used in the present embodiment is obtained.

[0117] The reaction is preferably carried out in the presence of an alkali metal hydroxide. By doing so, it is believed that the reaction proceeds favorably. This is believed to be because the alkali metal hydroxide functions as a dehydrohalogenation agent, specifically, a dehydrochlorination agent. That is, it is believed that the alkali metal hydroxide removes hydrogen halide from the phenol group of the polyphenylene ether and the compound in which the substituent and the halogen atom are bonded, and thereby the substituent is bonded to the oxygen atom of the phenol group instead of the hydrogen atom of the phenol group of the polyphenylene ether.

[0118] The alkali metal hydroxide is not particularly limited as long as it can act as a dehalogenating agent, and examples thereof include sodium hydroxide, etc. The alkali metal hydroxide is usually used in the form of an aqueous solution, specifically, an aqueous sodium hydroxide solution.

[0119] The reaction conditions such as reaction time and reaction temperature vary depending on the compound to which the substituent and the halogen atom are bonded, and are not particularly limited as long as the reaction proceeds favorably under the conditions. Specifically, the reaction temperature is preferably room temperature to 100°C, more preferably 30 to 100°C. The reaction time is preferably 0.5 to 20 hours, more preferably 0.5 to 10 hours.

[0120] The solvent used in the reaction is not particularly limited as long as it can dissolve the polyphenylene ether and the compound having the substituent and the halogen atom bonded thereto and does not inhibit the reaction between the polyphenylene ether and the compound having the substituent and the halogen atom bonded thereto. Specific examples thereof include toluene.

[0121] The above reaction is preferably carried out in the presence of not only an alkali metal hydroxide but also a phase transfer catalyst. That is, the above reaction is preferably carried out in the presence of an alkali metal hydroxide and a phase transfer catalyst. It is believed that the above reaction proceeds more favorably by doing so. This is believed to be due to the following. It is believed that the phase transfer catalyst is a catalyst that has the function of incorporating an alkali metal hydroxide, is soluble in both a polar solvent phase such as water and a non-polar solvent phase such as an organic solvent, and can move between these phases. Specifically, when an aqueous sodium hydroxide solution is used as the alkali metal hydroxide and an organic solvent such as toluene, which is not compatible with water, is used as the solvent, even if the aqueous sodium hydroxide solution is dropped into the solvent being used for the reaction, the solvent and the aqueous sodium hydroxide solution are separated, and it is believed that the sodium hydroxide is unlikely to move to the solvent. In that case, it is believed that the aqueous sodium hydroxide solution added as the alkali metal hydroxide is unlikely to contribute to promoting the reaction. On the other hand, when the reaction is carried out in the presence of an alkali metal hydroxide and a phase transfer catalyst, the alkali metal hydroxide is transferred to the solvent while being incorporated in the phase transfer catalyst, and the aqueous sodium hydroxide solution is likely to contribute to promoting the reaction. Therefore, when the reaction is carried out in the presence of an alkali metal hydroxide and a phase transfer catalyst, the reaction is believed to proceed more favorably.

[0122] The phase transfer catalyst is not particularly limited, but examples thereof include quaternary ammonium salts such as tetra-n-butylammonium bromide.

[0123] The resin composition used in the present embodiment preferably contains, in addition to the above polymer, the modified polyphenylene ether compound obtained as described above.

[0124] The resin composition of the present embodiment may contain a thermosetting resin other than the polymer or polyphenylene ether compound as described above. Examples of other usable thermosetting resins include epoxy resins, phenolic resins, amine resins, unsaturated polyester resins, and thermosetting polyimide resins.

[0125] (Other Ingredients) The resin composition according to the present embodiment may contain components other than the polymer (other components) as necessary, within a range that does not impair the effects of the present invention. The other components contained in the resin composition according to the present embodiment may further contain additives such as, for example, a curing agent, a silane coupling agent, a flame retardant, an initiator, an antifoaming agent, an antioxidant, a heat stabilizer, an antistatic agent, an ultraviolet absorber, a dye or pigment, a lubricant, and an inorganic filler. In addition to the polymer, the resin composition may contain resins such as polyphenylene ether, an epoxy resin, an unsaturated polyester resin, and a thermosetting polyimide resin.

[0126] In particular, the curing agent is not particularly limited as long as it is a curing agent (crosslinking type crosslinking agent) that can react with the polymer and, if necessary, the modified polyphenylene ether compound to crosslink the polymer and the curing agent and cure the resin composition. Examples of the crosslinking type curing agent include a compound having two or more unsaturated double bonds in the molecule, an alkenyl isocyanurate compound, styrene, a styrene derivative, an allyl compound having at least one allyl group in the molecule, a polyfunctional maleimide compound having at least two maleimide groups in the molecule, a modified maleimide compound, and an acenaphthylene compound having an acenaphthylene structure in the molecule.

[0127] In addition, the compound having two or more unsaturated double bonds in the molecule includes a polyfunctional methacrylate compound having two or more methacryloyl groups in the molecule, a polyfunctional acrylate compound having two or more acryloyl groups in the molecule, and a polyfunctional vinyl compound having two or more vinyl groups in the molecule. Examples of the polyfunctional vinyl compound include divinylbenzene and polybutadiene. The alkenyl isocyanurate compound may be any compound having an isocyanurate structure and an alkenyl group in the molecule, and examples of the alkenyl isocyanurate compound include triallyl isocyanurate (TAIC) and other trialkenyl isocyanurate compounds.

[0128] Examples of the styrene derivative include bromostyrene such as dibromostyrene, etc. Examples of the modified maleimide compound include modified maleimide compounds in which a part of the molecule is modified with an amine, modified maleimide compounds in which a part of the molecule is modified with silicone, and modified maleimide compounds in which a part of the molecule is modified with an amine and silicone.

[0129] The allyl compound may be a monofunctional allyl compound having one allyl group in the molecule, or a polyfunctional allyl compound having two or more allyl groups in the molecule. An example of the polyfunctional allyl compound is diallyl phthalate (DAP).

[0130] The polyfunctional maleimide compound having at least two maleimide groups in the molecule is not particularly limited, and examples of the polyfunctional maleimide compound include phenylene bismaleimides such as 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, and m-phenylene bismaleimide, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1,6'-bismaleimide-(2,2,4-trimethyl)hexane, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenylsulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene, and maleimide compounds having a biphenyl structure. Examples of the modified maleimide compound include modified maleimide compounds having a maleimide group in the molecule, a part of which is modified with an amine compound, modified maleimide compounds having a part of which is modified with a silicone compound, and modified maleimide compounds having a part of which is amine-modified and silicone-modified with an amine compound and a silicone compound.

[0131] Examples of the acenaphthylene compound include acenaphthylene, alkylacenaphthylenes, halogenated acenaphthylenes, and phenylacenaphthylenes. Examples of the alkylacenaphthylenes include 1-methylacenaphthylene, 3-methylacenaphthylene, 4-methylacenaphthylene, 5-methylacenaphthylene, 1-ethylacenaphthylene, 3-ethylacenaphthylene, 4-ethylacenaphthylene, and 5-ethylacenaphthylene. Examples of the halogenated acenaphthylenes include 1-chloroacenaphthylene, 3-chloroacenaphthylene, 4-chloroacenaphthylene, 5-chloroacenaphthylene, 1-bromoacenaphthylene, 3-bromoacenaphthylene, 4-bromoacenaphthylene, and 5-bromoacenaphthylene. Examples of the phenylacenaphthylenes include 1-phenylacenaphthylene, 3-phenylacenaphthylene, 4-phenylacenaphthylene, 5-phenylacenaphthylene, etc. The acenaphthylene compound may be a monofunctional acenaphthylene compound having one acenaphthylene structure in the molecule as described above, or a polyfunctional acenaphthylene compound having two or more acenaphthylene structures in the molecule.

[0132] Among these, the alkenyl isocyanurate compound, the polyfunctional acrylate compound, the polyfunctional methacrylate compound, and the polyfunctional vinyl compound are preferred in that they can further increase the heat resistance of the cured product of the resin composition. This is believed to be due to the fact that the crosslinking of the resin composition is more suitably formed by the curing reaction by using these crosslinking curing agents. In addition, the crosslinking curing agent may be used alone or in combination of two or more types. In addition, as the crosslinking curing agent, not only the crosslinking curing agents exemplified above, such as a compound having two or more unsaturated double bonds in the molecule, but also a compound having one unsaturated double bond in the molecule may be used in combination. Examples of the compound having one unsaturated double bond in the molecule include a monovinyl compound having one vinyl group in the molecule.

[0133] The polyfunctional acrylate compound includes a polyfunctional acrylate compound having two or more acryloyl groups in the molecule, such as tricyclodecane dimethanol diacrylate.

[0134] Examples of the polyfunctional methacrylate compound include a compound having a polyphenylene ether structure and two or more methacryloyl groups in the molecule, tricyclodecane dimethanol dimethacrylate, etc. Examples of the compound having a polyphenylene ether structure and two or more methacryloyl groups in the molecule include a methacryl-modified polyphenylene ether compound in which a terminal hydroxyl group of polyphenylene ether is modified with a methacryl group, etc.

[0135] The curing agent may be used alone or in combination of two or more kinds.

[0136] The curing agent preferably has a weight average molecular weight of 100 to 5000, more preferably 100 to 4000, and even more preferably 100 to 3000. If the weight average molecular weight of the curing agent is too low, the curing agent may be easily volatilized from the compounding components of the resin composition. If the weight average molecular weight of the curing agent is too high, the viscosity of the varnish of the resin composition and the melt viscosity during heat molding may be too high. Therefore, if the weight average molecular weight of the curing agent is within such a range, a resin composition having excellent heat resistance of the cured product can be obtained. This is considered to be because the resin composition of this embodiment can be suitably cured by the reaction with the polymer or modified polyphenylene ether compound. Here, the weight average molecular weight may be measured by a general molecular weight measurement method, and specifically, a value measured using gel permeation chromatography (GPC) may be mentioned.

[0137] In addition, the resin composition according to the present embodiment may contain a silane coupling agent, as described above. The silane coupling agent may be contained in the resin composition, or may be contained in the inorganic filler contained in the resin composition as a silane coupling agent that has been surface-treated in advance. Among these, the silane coupling agent is preferably contained in the inorganic filler as a silane coupling agent that has been surface-treated in advance, and it is more preferable to contain the silane coupling agent in the inorganic filler as a silane coupling agent that has been surface-treated in advance, and further to contain the silane coupling agent in the resin composition. In addition, in the case of a prepreg, the prepreg may contain the silane coupling agent in the fibrous base material as a silane coupling agent that has been surface-treated in advance.

[0138] Examples of the silane coupling agent include silane coupling agents having at least one functional group selected from the group consisting of vinyl, styryl, methacryloyl, acryloyl, and phenylamino groups. That is, the silane coupling agent includes compounds having at least one reactive functional group selected from vinyl, styryl, methacryloyl, acryloyl, and phenylamino groups, and further having hydrolyzable groups such as methoxy and ethoxy groups.

[0139] The silane coupling agent includes, for example, vinyl triethoxysilane and vinyl trimethoxysilane, which have a vinyl group. The silane coupling agent includes, for example, p-styryl trimethoxysilane and p-styryl triethoxysilane, which have a styryl group. The silane coupling agent includes, for example, 3-methacryloxypropyl trimethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl triethoxysilane, 3-methacryloxypropyl methyl diethoxysilane, and 3-methacryloxypropyl ethyl diethoxysilane, which have a methacryloyl group. The silane coupling agent includes, for example, 3-acryloxypropyl trimethoxysilane and 3-acryloxypropyl triethoxysilane, which have an acryloyl group. Examples of the silane coupling agent include those having a phenylamino group, such as N-phenyl-3-aminopropyltrimethoxysilane and N-phenyl-3-aminopropyltriethoxysilane.

[0140] The resin composition according to the present embodiment may contain a flame retardant as described above. By containing a flame retardant, the flame retardancy of the cured product of the resin composition can be improved. The flame retardant is not particularly limited. Specifically, in fields where halogen-based flame retardants such as bromine-based flame retardants are used, for example, ethylene dipentabromobenzene, ethylene bistetrabromoimide, decabromodiphenyl oxide, and tetradecabromodiphenoxybenzene having a melting point of 300° C. or more are preferred. It is considered that the use of a halogen-based flame retardant can suppress the elimination of halogen at high temperatures and suppress the decrease in heat resistance. In addition, in fields where halogen-free is required, phosphate-based flame retardants, phosphazene-based flame retardants, bisdiphenylphosphine oxide-based flame retardants, and phosphinate-based flame retardants can be mentioned. A specific example of a phosphate-based flame retardant is a condensed phosphate ester of dixylenyl phosphate. A specific example of a phosphazene-based flame retardant is phenoxyphosphazene. A specific example of the bisdiphenylphosphine oxide flame retardant is xylylenebisdiphenylphosphine oxide. A specific example of the phosphinate flame retardant is a metal phosphinate of an aluminum salt of dialkylphosphinic acid. As the flame retardant, each of the flame retardants exemplified above may be used alone or in combination of two or more.

[0141] The resin composition according to the present embodiment may contain an initiator (reaction initiator) as described above. The resin composition may proceed with the curing reaction even if it is composed of only the polymer. However, depending on the process conditions, it may be difficult to raise the temperature to a level where the curing proceeds, so a reaction initiator may be added. The reaction initiator is not particularly limited as long as it can promote the curing reaction between the polymer and, as necessary, the modified polyphenylene ether compound. Specifically, examples of the reaction initiator include oxidizing agents such as α,α'-di(t-butylperoxy)diisopropylbenzene, 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne, benzoyl peroxide, 3,3',5,5'-tetramethyl-1,4-diphenoquinone, chloranil, 2,4,6-tri-t-butylphenoxyl, t-butylperoxyisopropyl monocarbonate, and azobisisobutyronitrile. In addition, a carboxylate metal salt or the like may be used in combination as necessary. By doing so, the curing reaction can be further promoted. Among these, α,α'-di(t-butylperoxy)diisopropylbenzene is preferably used. Since α,α'-di(t-butylperoxy)diisopropylbenzene has a relatively high reaction initiation temperature, it can suppress the promotion of the curing reaction at the time when curing is not required, such as when drying the prepreg, and can suppress the deterioration of the storage stability of the resin composition. Furthermore, since α,α'-di(t-butylperoxy)diisopropylbenzene has low volatility, it does not volatilize during drying or storage of the prepreg, and has good stability. Moreover, the reaction initiator may be used alone or in combination of two or more kinds.

[0142] As described above, the resin composition according to the present embodiment may contain a filler such as an inorganic filler. Examples of the filler include those added to enhance the heat resistance and flame retardancy of the cured product of the resin composition, and are not particularly limited. In addition, by including a filler, the heat resistance and flame retardancy can be further enhanced. Specific examples of the filler include silica such as spherical silica, metal oxides such as alumina, titanium oxide, and mica, metal hydroxides such as aluminum hydroxide and magnesium hydroxide, talc, aluminum borate, barium sulfate, and calcium carbonate. Among these, silica, mica, and talc are preferable, and spherical silica is more preferable. In addition, the filler may be used alone or in combination of two or more. In addition, the filler may be used as it is, or may be surface-treated with the silane coupling agent. In addition, when a filler is included, its content (filler content) is preferably 30 to 270 mass% and more preferably 50 to 250 mass% relative to the resin composition.

[0143] The content ratio of the polymer in the resin composition of the present embodiment is not particularly limited as long as it is a ratio that can form a cured product that can become an insulating layer. For example, the content is preferably about 30 to 95 parts by mass, more preferably 40 to 90 parts by mass, and even more preferably 50 to 90 parts by mass, relative to the total amount (100 parts by mass) of the resin composition.

[0144] When the resin composition of the present embodiment further contains a modified polyphenylene ether compound, the content thereof is preferably about 5 to 30 parts by mass, more preferably 5 to 20 parts by mass, and further preferably 10 to 20 parts by mass, relative to the total amount (100 parts by mass) of the resin composition.

[0145] When a curing agent is further included, the content ratio of the curing agent relative to the total amount (100 parts by mass) of the resin composition is preferably about 5 to 70 parts by mass, more preferably 10 to 70 parts by mass, and further preferably 10 to 50 parts by mass.

[0146] When a copper-clad laminate is produced, the resin composition as described above is usually prepared in the form of a varnish and is often used as a resin varnish. Such a resin varnish is prepared, for example, as follows.

[0147] First, the polymer, and if necessary, each component that can be dissolved in an organic solvent, such as a modified polyphenylene ether compound, a curing agent, and various additives, are put into an organic solvent and dissolved. At this time, heating may be performed if necessary. Then, if necessary, a component that is not soluble in an organic solvent, an inorganic filler, etc. are added, and the mixture is dispersed until a predetermined dispersion state is reached using a ball mill, a bead mill, a planetary mixer, a roll mill, etc., to prepare a varnish-like resin composition. The organic solvent used here is not particularly limited as long as it dissolves the polymer, the curing agent, etc. and does not inhibit the curing reaction. Specific examples include toluene, cyclohexanone, methyl ethyl ketone, and propylene glycol monomethyl ether acetate. These may be used alone or in combination of two or more.

[0148] In addition to the cured product of the resin composition, the insulating layer of the present embodiment preferably further contains a glass substrate, which has the advantages of suppressing processing troubles (such as cracks), reducing dimensional changes, reducing linear expansion, and suppressing warpage.

[0149] When the insulating layer of the present embodiment includes a glass substrate, the insulating layer may be used as a prepreg obtained by impregnating the glass substrate with the above-mentioned resin composition. As a method for producing such a prepreg, for example, a method of impregnating a glass substrate with the above-mentioned resin varnish (a resin composition prepared in a varnish form) and then drying the glass substrate may be mentioned.

[0150] The resin varnish is impregnated into the glass substrate by immersion, coating, etc. This impregnation can be repeated multiple times as necessary. In addition, it is also possible to repeat the impregnation using multiple resin varnishes with different compositions and concentrations to adjust the final composition and resin amount to the desired one.

[0151] The glass substrate impregnated with the resin varnish is heated under the desired heating conditions of 80 to 170° C. for 1 to 10 minutes to obtain a resin layer (A stage) containing the resin composition before curing or a resin layer in a semi-cured state (B stage). After applying the resin varnish (impregnating the resin varnish in the case of a prepreg), the organic solvent can be volatilized from the varnish by heating, thereby reducing or removing the organic solvent.

[0152] (Surface-treated copper foil) The surface-treated copper foil according to the present embodiment is a surface-treated copper foil having a copper fine particle treatment layer 2 on at least one side of a copper foil 1 as shown in FIG. 1, the fine rough particle treatment layer 2 being composed of fine copper particles having a particle diameter of 40 to 200 nm, a heat-resistant treatment layer 3 containing nickel on the fine rough particle treatment layer 2, a rust-resistant treatment layer 4 containing at least chromium on the heat-resistant treatment layer 3, a silane coupling agent treatment layer 5 on the rust-resistant treatment layer, and a nickel deposition amount in the heat-resistant treatment layer of 30 to 60 mg / m 2 It is characterized in that:

[0153] With this configuration, a fine-roughening particle treatment layer composed of fine roughening particles is provided on the surface of the untreated copper foil, thereby improving adhesion to the resin substrate. Furthermore, by adjusting the size of the fine roughening particles and, in particular, the amount of nickel deposited in the heat-resistant treatment layer, it is possible to achieve both transmission characteristics and basic characteristics (adhesion to the resin substrate and heat resistance).

[0154] First, each component of the surface-treated copper foil of this embodiment will be specifically described below.

[0155] (copper foil) Conventionally, the copper foil used for rigid boards and the like was generally electrolytic copper foil, and the copper foil used for flexible boards and the like was generally rolled copper foil, but in recent years, with the rise of the flexible board market in particular, electrolytic copper foils having properties comparable to those of rolled copper foil have been developed, and currently, rolled copper foils and electrolytic copper foils are used regardless of the type of board. Therefore, the untreated copper foil used in this embodiment is not limited to rolled copper foil or electrolytic copper foil, and any copper foil may be used.

[0156] (Fine roughening particle treatment layer) The fine roughening particle treated layer is a first surface treatment layer formed on the untreated copper foil, and is provided to increase the surface area and improve the peel strength from the resin substrate, and is composed of fine copper particles having a particle diameter of 40 to 200 nm.

[0157] In this embodiment, the particle diameter is used in the following sense. That is, a field emission scanning electron microscope FE-SEM (JSM-7800F manufactured by JEOL Ltd.) is used to observe at a magnification of 80,000 times while tilting the sample stage by 40 degrees, and the height of the observed copper particles is taken as the particle diameter value. The particle diameter of the fine copper particles in the fine roughening particle treatment layer of this embodiment is a maximum value of 200 nm and a minimum value of 40 nm in the range observed and measured by the above method.

[0158] In this embodiment, the fine copper particle treatment layer does not exclude copper particles having a particle diameter of more than 200 nm or less than 40 nm. However, if there are many particles having a particle diameter of more than 200 nm, the transmission loss may increase, and if there are many particles having a particle diameter of less than 40 nm, sufficient adhesion may not be ensured, and neither of these cases is preferable. For example, the fine copper particle treatment layer in this embodiment preferably contains 90% or more copper particles having a particle diameter of 40 to 200 nm, and more preferably contains 95% or more copper particles having a particle diameter of 40 to 200 nm.

[0159] The fine roughening particle treatment layer can be formed by electrolytic plating.

[0160] The particle diameter of the fine copper particles of this embodiment is strongly influenced by the plating bath composition as well as the electrolytic current density. For example, when the electrolytic current density is high, the particle diameter of the roughening particles tends to be small, and conversely, when the electrolytic current density is low, the particle diameter of the roughening particles tends to be large. Therefore, in order to obtain roughening particles with a desired particle diameter, the electrolytic current density must be appropriately set.

[0161] Examples of bath compositions and electrolysis conditions for forming a copper layer treated with fine roughening particles are given below, but the present invention is not limited to these.

[0162] (Bath composition) Copper sulfate pentahydrate: 10 to 70 g / L (particularly preferably 30 to 50 g / L) Pentasodium diethylenetriaminepentaacetic acid (DTPA·5Na): 50 to 150 g / L (particularly preferably 80 to 120 g / L) pH: 3.0 to 6.0 (particularly preferably 3.5 to 5.5) pH is adjusted using sulfuric acid and sodium hydroxide

[0163] (Electrolysis conditions) Current density: 0.5~10.0A / dm 2 (Particularly preferably 1.0 to 6.0 A / dm 2 ) Electrical capacity: 10~130A·sec / dm 2 (Especially preferably 30 to 110 A·sec / dm 2 ) Liquid temperature: 25 to 50°C (particularly preferably 30 to 45°C) Anode: copper plate.

[0164] The appropriate concentration of DTPA·5Na is 50 to 150 g / L, but if it is outside this range and is less than 50 g / L, it is difficult to obtain sufficient fineness and the roughening particles become coarse. If it exceeds 150 g / L, the current efficiency will decrease, the amount of deposition in the roughening treatment will decrease dramatically, and the voltage will also increase, making it uneconomical.

[0165] The amount of electricity is 10 to 130 A·sec / dm 2In this range, copper particles with a particle size of 40 to 200 nm can be obtained, and there is an advantage that adhesion to the resin can be easily ensured. On the other hand, the quantity of electricity is 10 A sec / dm 2 If it is less than 130A·sec / dm, the number of copper particles less than 40nm will increase, and adhesion may decrease. 2 If the amount is larger, the particle shape tends to become dendritic and the particle size tends to become coarse, resulting in problems such as reduced adhesion to untreated copper foil, increased powder falling, and increased surface roughness of the laminate surface.

[0166] (Heat-resistant layer) The heat-resistant layer is a heat-resistant and rust-preventive layer provided to protect the copper foil, including the fine roughening particle treatment layer, from stress such as chemicals and heat, and is sometimes called a barrier treatment layer. The heat-resistant layer of this embodiment contains nickel or nickel and phosphorus, and the nickel coating amount in the heat-resistant layer is 30 to 60 mg / m 2 It is.

[0167] The amount of nickel deposited is 30 to 60 mg / m 2 This allows both the transmission characteristics and the basic characteristics to be achieved. 2 If the thickness is less than 60 mg / m, the heat resistance decreases, and for example, swelling occurs at the interface between the resin and the copper foil, which may result in a decrease in adhesion. 2 If the amount exceeds this range, the transmission loss may increase. A more preferable range for the amount of nickel coating is 40 to 50 mg / m 2 It is.

[0168] In this embodiment, the "adhesion amount" refers to the mass of nickel deposited per unit area on the fine roughening particle treatment layer side of the copper foil by plating (for example, electrolytic plating). The adhesion amount can be measured by dissolving and diluting the treated copper foil with nitric acid or the like, and analyzing the nickel concentration using an ICP emission spectrometer.

[0169] The heat-resistant layer of the present embodiment is preferably made of nickel (Ni) or nickel (Ni) and phosphorus (P).

[0170] The heat-resistant layer of this embodiment is a second surface treatment layer formed after the fine roughening particle treatment layer is formed, and can be formed by electrolytic plating. The nickel deposition amount can be adjusted by adjusting the current conditions when the electrolytic plating is performed.

[0171] Examples of bath compositions and electrolysis conditions for forming the heat-resistant layer of this embodiment composed of nickel and phosphorus are given below, but the present invention is not limited to these.

[0172] (Bath composition) Nickel sulfate hexahydrate 10-100g / L (preferably 20-60g / L) Sodium acetate trihydrate: 2-40g / L (preferably 5-30g / L) Sodium hypophosphite monohydrate 0.1 to 10 g / L (particularly preferably 1.0 to 6.0 g / L) pH 3.0 to 5.5 (particularly preferably 3.5 to 5.0)

[0173] (Electrolysis conditions) Current density: 0.5~3.5A / dm 2 (Especially preferably 1.0 to 2.0 A / dm 2 ) Electrical capacity: 1.8~2.7A·sec / dm 2 (2.0 to 2.5 A·sec / dm is especially preferable. 2 ) Liquid temperature: 25 to 50°C (particularly preferably 30 to 40°C) Anode: An insoluble electrode such as platinum group oxide coated titanium.

[0174] Nickel sulfate hexahydrate, nickel chloride hexahydrate, nickel acetate tetrahydrate, etc. can be used as a nickel ion source. Sodium phosphite, sodium hypophosphite, nickel phosphite, etc. can be used as a phosphorus ion source. Sodium sulfate may also be added to impart electrical conductivity.

[0175] (Anti-rust treatment layer) The rust-proofing layer is a layer provided to prevent oxidation during heating or storage. The rust-proofing layer of this embodiment contains at least chromium (Cr) and is sometimes called a chromate-treated layer. It may further contain zinc (Zn).

[0176] The rust-proofing layer of this embodiment is a third surface treatment layer formed after the formation of the heat-resistant layer, and can be formed by electrolytic plating.

[0177] The bath composition for forming the rust-proofing layer of this embodiment may be a known one, and examples of such bath compositions include hexavalent chromium, such as chromic acid, sodium dichromate, and potassium dichromate. The chromium precipitated after the rust-proofing layer is a mixture of Cr(OH)3 and Cr2O3, and there is no hexavalent chromium, which is harmful to the human body, but it precipitates in the form of trivalent chromium. The chromic acid solution may be either alkaline or acidic.

[0178] In addition, an alkaline zinc chromate solution containing zinc ions and hexavalent chromium ions as described in Japanese Patent Publication No. 15950 / 1983 may be used as the alkaline chromic acid solution. By using this chromic acid solution, it is possible to improve the rust prevention properties more than a rust prevention treatment layer made from a chromic acid solution alone.

[0179] The electrolytic bath and electrolytic conditions for applying the rust-proofing layer of this embodiment include, for example, the bath composition and conditions shown below, but are not particularly limited thereto.

[0180] (Bath composition) Sodium dichromate: 2.5 to 60 g / L (particularly preferably 5 to 30 g / L) Zinc ion: 0.25 to 16 g / L (particularly preferably 0.5 to 8 g / L) Sodium hydroxide: 10 to 180 g / L (particularly preferably 20 to 90 g / L)

[0181] (Electrolysis conditions) Current density: 1.5~8.0A / dm 2 (Especially preferably 3.0 to 4.0 A / dm 2 ) Electrical capacity: 4.5~6.5A·sec / dm 2 (5.0 to 6.0 A·sec / dm is especially preferable. 2 ) Liquid temperature: 25 to 50°C (particularly preferably 30 to 40°C) Anode: An insoluble electrode such as platinum group oxide coated titanium.

[0182] (Silane coupling agent treated layer) The silane coupling agent treatment layer of this embodiment is the fourth surface treatment layer formed after forming the above-mentioned rust-proofing treatment layer, and is a layer provided to further improve adhesion with resin substrate.Furthermore, by providing the silane coupling agent treatment layer, not only can it improve peel strength, but also can suppress the deterioration of peel strength after severe test, and further improve rust prevention, and become a copper foil for circuit board with excellent versatility.

[0183] The silane coupling agent-treated layer of this embodiment can be formed by adding an appropriate amount of silane coupling agent to water or the like, applying the aqueous solution by immersion treatment or spray treatment, and then washing with water and drying. The silane coupling agent can be selected from a wide variety of groups, including epoxy groups, amino groups, mercapto groups, vinyl groups, methacryloxy groups, and styryl groups. However, each group has different characteristics and is compatible with the substrate, so it is necessary to select and use the appropriate one.

[0184] The bath for forming the silane coupling agent treatment layer may have the following composition and conditions, but is not limited thereto.

[0185] (Bath composition, conditions) γ-aminopropyltriethoxysilane: 1 to 5 mL / L (particularly preferably 2 to 4 mL / L) Liquid temperature: 25 to 35°C (particularly preferably 28 to 32°C) Immersion time: 15 seconds.

[0186] (Method of manufacturing copper-clad laminate) The copper-clad laminate of this embodiment can be produced, for example, by stacking one or more prepregs containing the resin composition as described above, and then stacking the above-mentioned copper foil on both or just one of the top and bottom surfaces of the prepreg such that the silane coupling agent layer is in contact with the prepreg, and then heating and press-molding the resulting laminate to form an integrated laminate having copper foil clad on both sides or just one side.

[0187] The heating and pressing conditions can be appropriately set depending on the thickness of the laminate to be produced, the type of resin composition, etc., but can be, for example, a temperature of 170 to 220° C., a pressure of 1.5 to 5.0 MPa, and a time of 60 to 150 minutes.

[0188] <Resin-coated copper foil> As described above, the resin-coated copper foil 31 of this embodiment has a configuration in which a resin layer 32 containing a resin composition or a semi-cured product of the resin composition and a copper foil 13 provided on one side of the resin layer are laminated (see FIG. 4). That is, the resin-coated copper foil of this embodiment may be a resin-coated copper foil comprising a resin layer containing a resin composition before curing (A-stage resin composition) and a copper foil, or a resin layer containing a semi-cured product of a resin composition (B-stage resin composition) and a copper foil.

[0189] The resin composition used in the resin layer and the copper foil may be the same as those described above for the copper-clad laminate.

[0190] In the resin-coated copper foil of the present embodiment, the resin composition or the semi-cured product thereof may be obtained by drying or heating the resin composition.

[0191] Examples of a method for producing a resin-coated copper foil include a method in which the resin varnish obtained above is applied to the surface of a copper foil on which a silane coupling agent layer has been formed, and then the resin composition is semi-cured by drying.

[0192] Since the resin layer of resin-coated copper foil does not usually contain a glass substrate, the resin varnish is applied to the copper foil by coating, etc., which can be repeated multiple times as necessary. In this case, it is also possible to repeatedly coat multiple resin varnishes with different compositions and concentrations to adjust the final composition (content ratio) and resin amount to the desired one.

[0193] When the resin varnish is applied and then semi-cured, it is heated under desired heating conditions, for example, at 80 to 170° C. for 1 to 10 minutes to obtain a resin layer containing the resin composition before curing (A stage) or a resin layer in a semi-cured state (B stage). After applying the resin varnish (impregnating the resin varnish in the case of a prepreg), the organic solvent can be volatilized from the varnish by heating, thereby reducing or removing the organic solvent.

[0194] The resin-coated copper foil of this embodiment has the same effects and advantages as the above-mentioned copper-clad laminate.

[0195] <Circuit board> The copper-clad laminate and resin-coated copper foil of this embodiment can be used as a circuit board 21 having a conductor pattern on the surface as a circuit 14, as shown in Fig. 3, by forming a circuit by etching the copper foil on the surface. In addition to the above-mentioned methods, examples of the circuit formation method include circuit formation by a semi-additive process (SAP) or a modified semi-additive process (MSAP). The circuit board obtained by using the copper-clad laminate and resin-coated copper foil of this embodiment is a highly reliable circuit board that has heat resistance and reduced transmission loss.

[0196] As described above, this specification discloses various aspects of the technology, the main technologies of which are summarized below.

[0197] A copper-clad laminate according to one embodiment of the present invention is a copper-clad laminate comprising an insulating layer containing a cured product of a resin composition and a surface-treated copper foil on one or both sides of the insulating layer, wherein the resin composition contains a polymer having a structural unit represented by the following formula (1) in its molecule: [ka] (In formula (1), Z represents an arylene group, R1 to R3 each independently represent a hydrogen atom or an alkyl group, and R4 to R6 each independently represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.) and the surface-treated copper foil has a copper fine particle treatment layer on at least one side of the copper foil, the fine particle treatment layer being composed of fine copper particles having a particle diameter of 40 to 200 nm, a heat-resistant treatment layer containing nickel on the fine particle treatment layer, a rust-resistant treatment layer containing at least chromium on the heat-resistant treatment layer, a silane coupling agent layer on the rust-resistant treatment layer, and a nickel coating amount in the heat-resistant treatment layer of 30 to 60 mg / m 2 It is characterized in that:

[0198] With this configuration, it is possible to reduce the transmission loss of a high-speed signal transmission board, and to provide a copper-clad laminate that is excellent in adhesion and heat resistance.

[0199] In the resin composition, the structural unit represented by formula (1) preferably contains a structural unit represented by formula (2) below.

[0200] [ka] In formula (2), R4 to R6 each independently represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and R7 represents an arylene group having 6 to 12 carbon atoms.

[0201] This configuration results in a copper clad laminate having an insulating layer with lower dielectric properties and higher heat resistance.

[0202] In the resin composition, the structural unit represented by formula (2) preferably contains a structural unit represented by formula (3) below.

[0203] [ka] In formula (3), R4 to R6 each independently represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0204] This configuration results in a copper clad laminate having an insulating layer with lower dielectric properties and higher heat resistance.

[0205] In the resin composition, the polymer preferably further includes a polymer having a structural unit represented by the following formula (4) in the molecule.

[0206] [ka] In formula (4), R8~R 10 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; R 11 represents an aryl group.

[0207] This configuration results in a copper clad laminate having an insulating layer with lower dielectric properties and higher heat resistance.

[0208] In the resin composition, the aryl group in the structural unit represented by formula (4) preferably contains an aryl group having an alkyl group having 1 to 6 carbon atoms.

[0209] This configuration results in a copper clad laminate having an insulating layer with lower dielectric properties and higher heat resistance.

[0210] In the resin composition, the polymer preferably has a weight average molecular weight of 1,500 to 40,000.

[0211] This configuration results in a copper clad laminate having an insulating layer with lower dielectric properties and higher heat resistance.

[0212] In the resin composition, the polymer preferably has an equivalent weight of the vinyl group contained in the structural unit represented by formula (1) in which R1 to R3 are hydrogen atoms, of 250 to 1,200.

[0213] According to this configuration, a copper-clad laminate having an insulating layer with lower dielectric properties, higher heat resistance, and excellent formability can be obtained.

[0214] In the copper-clad laminate, the resin composition preferably contains a modified polyphenylene ether compound terminally modified with a group represented by the above formula (5) or (6), thereby obtaining even more excellent low dielectric properties.

[0215] In the surface-treated copper foil, the heat-resistant layer is preferably made of nickel or nickel and phosphorus, which makes it possible to more reliably obtain the above-mentioned effects.

[0216] A resin-coated copper foil according to a further aspect of the present invention is characterized by comprising a resin layer containing the resin composition or a semi-cured product of the resin composition as described above, and the above-mentioned surface-treated copper foil on one side of the resin layer.

[0217] Furthermore, the present invention also includes a circuit board comprising the above-mentioned copper-clad laminate or the above-mentioned resin-coated copper foil and having a conductor pattern on its surface as a circuit.

[0218] The present invention also provides a resin composition for forming an insulating layer in a copper-clad laminate comprising an insulating layer containing a cured product of a resin composition and a surface-treated copper foil on one or both sides of the insulating layer, the resin composition comprising a polymer having a structural unit represented by the following formula (1) in a molecule: [ka] (In formula (1), Z represents an arylene group, R1 to R3 each independently represent a hydrogen atom or an alkyl group, and R4 to R6 each independently represent a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.) and, The surface-treated copper foil has a copper fine particle treatment layer on at least one side of the copper foil, the fine particle treatment layer being composed of fine copper particles having a particle diameter of 40 to 200 nm, and has a heat-resistant layer containing nickel on the fine particle treatment layer; A rust-proofing layer containing at least chromium is provided on the heat-resistant layer, a silane coupling agent layer is provided on the rust-proofing layer, and the amount of nickel deposited in the heat-resistant layer is 30 to 60 mg / m 2 The present invention also includes a resin composition comprising:

[0219] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples. EXAMPLES

[0220] First, in the present examples, each component used in preparing the resin composition will be described.

[0221] Modified PPE1 Polyphenylene ether and chloromethylstyrene were reacted to obtain modified polyphenylene ether 1 (modified PPE1).

[0222] Specifically, first, 200 g of polyphenylene ether (polyphenylene ether, SA90 manufactured by SABIC Innovative Plastics, 2 terminal hydroxyl groups, weight average molecular weight Mw1700), 30 g of a mixture of p-chloromethylstyrene and m-chloromethylstyrene in a mass ratio of 50:50 (chloromethylstyrene: CMS manufactured by Tokyo Chemical Industry Co., Ltd.), 1.227 g of tetra-n-butylammonium bromide as a phase transfer catalyst, and 400 g of toluene were charged and stirred in a 1-liter three-neck flask equipped with a temperature controller, a stirrer, a cooling device, and a dropping funnel. Then, the mixture was stirred until the polyphenylene ether, chloromethylstyrene, and tetra-n-butylammonium bromide were dissolved in toluene. At that time, the mixture was gradually heated until the liquid temperature reached 75°C. Then, an aqueous sodium hydroxide solution (20 g sodium hydroxide / 20 g water) was dropped into the solution as an alkali metal hydroxide over 20 minutes. After that, the mixture was further stirred at 75°C for 4 hours. Next, the contents of the flask were neutralized with 10% by mass of hydrochloric acid, and then a large amount of methanol was added. This caused a precipitate to form in the liquid in the flask. In other words, the product contained in the reaction liquid in the flask was reprecipitated. Then, this precipitate was removed by filtration, washed three times with a mixture of methanol and water in a mass ratio of 80:20, and then dried under reduced pressure at 80°C for 3 hours. Thus, a vinylbenzene-terminated PPE (modified PPE1) with a weight average molecular weight (Mw) of 2300 was obtained.

[0223] The obtained solid is 1 The solid was analyzed by H-NMR (400 MHz, CDCl3, TMS). As a result of measuring the NMR, a peak derived from ethenylbenzyl was confirmed at 5 to 7 ppm. This confirmed that the solid obtained was an ethenylbenzyl-modified polyphenylene ether.

[0224] Modified PPE2 The polyphenylene ether was synthesized in the same manner as in the synthesis of modified PPE1, except that the polyphenylene ether described below was used and the conditions described below were used.

[0225] The polyphenylene ether used was SA120 (intrinsic viscosity (IV) 0.125 dl / g, number of terminal hydroxyl groups 1, weight average molecular weight Mw 3100) manufactured by SABIC Innovative Plastics.

[0226] Next, the reaction of polyphenylene ether with chloromethylstyrene was carried out in a manner similar to that of modified PPE1, using 200 g of the polyphenylene ether (SA120), 15 g of CMS, and 0.92 g of phase transfer catalyst (tetra-n-butylammonium bromide), and using an aqueous sodium hydroxide solution (10 g sodium hydroxide / 10 g water) instead of an aqueous sodium hydroxide solution (20 g sodium hydroxide / 20 g water), to obtain a terminal vinylbenzene-modified PPE (modified PPE2) with a weight average molecular weight (Mw) of 3,300.

[0227] The resulting solid is then 1 The solid was analyzed by H-NMR (400 MHz, CDCl3, TMS). As a result of measuring the NMR, a peak derived from ethenylbenzyl was confirmed at 5 to 7 ppm. This confirmed that the solid obtained was an ethenylbenzyl-modified polyphenylene ether.

[0228] ·SA9000: SA9000 manufactured by SABIC Innovative Plastics (terminal methacrylic group modified PPE, weight average molecular weight (Mw) 2000)

[0229] SA90: SA90 manufactured by SABIC Innovative Plastics (unmodified PPE, weight average molecular weight (Mw) 1700)

[0230] Polymer 1: A polymer obtained by the following method.

[0231] 2.9 mol (377 g) of divinylbenzene, 1.7 mol (224.4 g) of ethylvinylbenzene, 10.4 mol (1081.6 g) of styrene, and 15 mol (1532 g) of n-propyl acetate were charged into a 5.0 L reactor and stirred. The mixture obtained by this stirring was heated to 70° C., and then 600 mmol of boron trifluoride diethyl ether complex was added. The mixture was further stirred at 70° C. for 4 hours to react divinylbenzene, ethylvinylbenzene, and styrene. Then, a saturated aqueous solution of sodium bicarbonate was added to the reaction solution in the reactor to stop the reaction. The organic layer separated by the addition was washed three times with pure water. The washed organic layer was subjected to reduced pressure devolatilization at 60° C. to obtain polymer 1.

[0232] The obtained polymer 1 was a polymer having a structural unit represented by the above formula (1) in the molecule [an aromatic polymer having a structural unit derived from a bifunctional aromatic compound in which two carbon-carbon unsaturated double bonds are bonded to an aromatic ring, a compound having structural units represented by the above formulas (5) to (7), weight average molecular weight Mw: 26,300, vinyl equivalent (equivalent of vinyl group contained in the structural unit represented by the above formula (1) in which R1 to R3 are hydrogen atoms): 510].

[0233] Polymer 2: A polymer obtained by the following method.

[0234] 3.6 mol (468 g) of divinylbenzene, 2.2 mol (290.4 g) of ethylvinylbenzene, 9.2 mol (956.8 g) of styrene, and 15 mol (1532 g) of n-propyl acetate were charged into a 5.0 L reactor and stirred. The mixture obtained by this stirring was heated to 70° C., and then 600 mmol of boron trifluoride diethyl ether complex was added. The mixture was further stirred at 70° C. for 4 hours to react divinylbenzene, ethylvinylbenzene, and styrene. Then, a saturated aqueous sodium bicarbonate solution was added to the reaction solution in the reactor to stop the reaction. The organic layer separated by the addition was washed three times with pure water. The washed organic layer was subjected to reduced pressure devolatilization at 60° C. to obtain polymer 2.

[0235] The obtained polymer 2 was a polymer having a structural unit represented by the above formula (1) in the molecule [an aromatic polymer having a structural unit derived from a bifunctional aromatic compound in which two carbon-carbon unsaturated double bonds are bonded to an aromatic ring, a compound having structural units represented by the above formulas (5) to (7), weight average molecular weight Mw: 31,100, vinyl equivalent (equivalent of vinyl group contained in the structural unit represented by the above formula (1) in which R1 to R3 are hydrogen atoms): 380].

[0236] Polymer 3: A polymer obtained by the following method.

[0237] 3.9 mol (507 g) of divinylbenzene, 2.3 mol (303.6 g) of ethylvinylbenzene, 8.8 mol (915.2 g) of styrene, and 15 mol (1532 g) of n-propyl acetate were charged into a 5.0 L reactor and stirred. The mixture obtained by this stirring was heated to 70° C., and then 600 mmol of boron trifluoride diethyl ether complex was added. The mixture was further stirred at 70° C. for 4 hours to react divinylbenzene, ethylvinylbenzene, and styrene. Then, a saturated aqueous sodium bicarbonate solution was added to the reaction solution in the reactor to stop the reaction. The organic layer separated by the addition was washed three times with pure water. The washed organic layer was subjected to reduced pressure devolatilization at 60° C. to obtain polymer 3.

[0238] The obtained polymer 3 was a polymer having a structural unit represented by the above formula (1) in the molecule [an aromatic polymer having a structural unit derived from a bifunctional aromatic compound in which two carbon-carbon unsaturated double bonds are bonded to an aromatic ring, a compound having structural units represented by the above formulas (5) to (7), weight average molecular weight Mw: 39,500, vinyl equivalent (equivalent of vinyl group contained in the structural unit represented by the above formula (1) in which R1 to R3 are hydrogen atoms): 320].

[0239] The vinyl equivalent of the vinyl group contained in the structural unit of polymers 1 to 3 represented by the formula (1) and in which R1 to R3 are hydrogen atoms (vinyl equivalent) was calculated by iodine value measurement by the Wiess method. Specifically, the compound to be measured was first dissolved in chloroform to a concentration of 0.3 g / 35 mL to 0.3 g / 25 mL. An excess amount of iodine chloride was added to the double bonds present in this solution. By doing so, the double bonds react with iodine chloride, and after this reaction has sufficiently progressed, a 20% by mass aqueous potassium iodide solution was added to the solution after the reaction, and the iodine content remaining in the solution after the reaction was reduced to I3 - This I3 was extracted into the aqueous phase. - The aqueous phase into which was extracted was titrated with an aqueous sodium thiosulfate solution (0.1 mol / L sodium thiosulfate standard solution) to calculate the iodine value. The following formula was used to calculate the iodine value.

[0240] Iodine value = [(BA) x F x 1.269] / mass of compound (g) In the above formula, B represents the titer (cc) of 0.1 mol / L sodium thiosulfate standard solution required for the blank test, A represents the titer (cc) of 0.1 mol / L sodium thiosulfate standard solution required for neutralization, and F represents the titer of sodium thiosulfate.

[0241] Hardener 1: TAIC (triallyl isocyanurate, manufactured by Nippon Kasei Chemical Co., Ltd.)

[0242] Hardener 2: Acenaphthylene (manufactured by JFE Chemical Corporation)

[0243] Hardener 3: Dibromostyrene (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0244] Reaction initiator: Perbutyl P: 1,3-di(t-butylperoxyisopropyl)benzene (Perbutyl P manufactured by NOF Corporation)

[0245] <Creating surface-treated copper foil> (Surface-treated copper foil 1) As a pretreatment, a copper plate was used as the cathode and the above untreated copper foil was used as the anode in a 100 g / L sulfuric acid aqueous solution, and the current density was 5 A / dm 2 The untreated copper foil surface was electrolyzed at 0.5 V for 6 seconds to remove the oxide layer and activate the surface.

[0246] Next, a copper fine roughening particle treated layer was formed on the laminate surface side of the untreated copper foil by treating with the bath composition and electrolysis conditions shown below.

[0247] (Bath composition) Copper sulfate pentahydrate 35g / L Pentasodium diethylenetriaminepentaacetate 100g / L pH 4.8

[0248] (Electrolysis conditions) Current density: 6A / dm 2 Electrical capacity: 50A·sec / dm 2 Liquid temperature: 30℃ Electrode: copper plate

[0249] The obtained fine rough particle treated layer was observed at a magnification of 80,000 times using a field emission scanning electron microscope FE-SEM (JSM-7800F manufactured by JEOL Ltd.) with the sample stage tilted at 40°. The height of the observed copper particles was taken as the particle diameter value, and the particle diameter of the rough particles in the fine rough particle treated layer was a minimum of 40 nm and a maximum of 200 nm.

[0250] Next, after washing with water, a heat-resistant treatment layer, which is a second surface treatment layer, was formed by treatment with the bath composition and electrolysis conditions shown below.

[0251] (Bath composition) Nickel sulfate hexahydrate 30g / L Sodium acetate trihydrate 10g / L Sodium hypophosphite monohydrate 2.0g / L

[0252] (Electrolysis conditions) Current density: 1.6A / dm 2 Electrical capacity: 2.7A·sec / dm 2 pH 4.5 Liquid temperature: 32℃ Anode: platinum group oxide coated titanium plate

[0253] The nickel deposition amount in the obtained heat-resistant layer was measured by dissolving and diluting the treated copper foil with nitric acid and analyzing the nickel concentration with an ICP emission spectrometer. As a result, the nickel deposition amount was 56 mg / m 2 It was.

[0254] Next, after rinsing with water, a rust-proofing layer which would become the third surface treatment layer was treated with the electrolytic bath composition, pH and electrolysis conditions shown below.

[0255] (Bath composition) Sodium dichromate: 10g / L Zinc ion: 1.0g / L Sodium hydroxide: 40g / L Liquid temperature: 30℃

[0256] (Electrolysis conditions) Current density: 4A / dm 2 Electrical capacity: 5.5A·sec / dm 2 Anode: platinum group oxide coated titanium plate

[0257] Next, after washing with water, a silane coupling agent treatment layer, which would be the fourth surface treatment layer, was formed by treatment with the bath composition, liquid temperature and immersion time shown below, thereby obtaining the surface-treated copper foil of Example 1.

[0258] (Bath composition) γ-Aminopropyltriethoxysilane 2mL / L Liquid temperature: 30℃ Immersion time: 15 seconds

[0259] (Surface-treated copper foil 2) Surface-treated copper foil 2 was obtained in the same manner as surface-treated copper foil 1, except that the second heat-resistant layer was formed by treatment with the bath composition and electrolysis conditions shown below. The nickel coating weight of the obtained heat-resistant layer was 32 mg / m 2 It was.

[0260] (Bath composition) Nickel sulfate hexahydrate 30g / L Sodium acetate trihydrate 10g / L Sodium hypophosphite monohydrate 2.0g / L pH 4.5

[0261] (Electrolysis conditions) Current density: 1.0A / dm 2 Electrical capacity: 1.8A·sec / dm 2 Liquid temperature: 32℃ Electrode: platinum group oxide coated titanium plate

[0262] (Surface-treated copper foil 3) Surface-treated copper foil 3 was obtained in the same manner as surface-treated copper foil 1, except that the second heat-resistant layer was not provided. The nickel coating amount of the obtained surface-treated copper foil 3 was 0 mg / m 2 It was.

[0263] (Surface-treated copper foil 4) Surface-treated copper foil 4 was obtained in the same manner as surface-treated copper foil 1, except that the second heat-resistant layer was formed by treatment under the bath composition and electrolysis conditions shown below. The nickel coating weight of the obtained heat-resistant layer was 82 mg / m 2 It was.

[0264] (Bath composition) Nickel sulfate hexahydrate 30g / L Sodium acetate trihydrate 10g / L Sodium hypophosphite monohydrate 2.0g / L

[0265] (Electrolysis conditions) Current density: 2.1A / dm 2 Electrical capacity: 3.6A·sec / dm 2 pH 4.5 Liquid temperature: 32℃ Anode: platinum group oxide coated titanium plate

[0266] (Surface-treated copper foil 5) "T4X-SV" manufactured by Fukuda Metal Foil & Powder Co., Ltd. was used as the surface-treated copper foil 5. The nickel coating amount in the heat-resistant layer of this surface-treated copper foil was 106 mg / m 2 It was.

[0267] (Surface-treated copper foil 6) Surface-treated copper foil 6 was obtained in the same manner as surface-treated copper foil 1, except that the first fine rough particle treated layer was formed by treatment with the bath composition and electrolysis conditions shown below. The particle diameter of the rough particles in the obtained fine rough particle treated layer was a minimum of 700 nm and a maximum of 1400 nm. The nickel coating weight in the obtained heat-resistant layer was 32 mg / m 2 It was.

[0268] (Bath composition) Bath (1) Copper sulfate pentahydrate 47g / L Sulfuric acid 100g / L Bath (2) Copper sulfate pentahydrate 200g / L Sulfuric acid 100g / L

[0269] (Electrolysis conditions) Current density in bath (1) is 50A / dm 2 , Electric charge 130A·sec / dm 2 After electrolysis under electrolysis conditions of a liquid temperature of 30°C to deposit fine copper particles, the solution was further electrolyzed in bath (2) at a current density of 5A / dm 2 , electric charge 400A·sec / dm 2 The electrolysis was performed under electrolysis conditions of a solution temperature of 40° C., thereby forming a fine roughening particle treatment layer.

[0270] (Surface-treated copper foil 7) A second heat-resistant layer was formed by electrolysis under the bath composition and electrolytic conditions shown below. Except for not forming an anticorrosive layer, the surface-treated copper foil 7 was obtained in the same manner as the surface-treated copper foil 1. The nickel coating weight of the obtained heat-resistant layer was 42 mg / m 2 It was.

[0271] (Bath composition) Nickel sulfate hexahydrate 30g / L Sodium acetate trihydrate 10g / L Sodium hypophosphite monohydrate 2.0g / L

[0272] (Electrolysis conditions) Current density: 1.3A / dm 2 Electrical capacity: 2.3A·sec / dm 2 pH 4.5 Liquid temperature: 32℃ Anode: platinum group oxide coated titanium plate

[0273] <Preparation of copper-clad laminates in Examples 1 to 12 and Comparative Examples 1 to 8> First, the above components other than the initiator were added to toluene and mixed in the compositions (parts by mass) shown in Tables 1 and 2 so that the solid content concentration was 65% by mass. The mixture was stirred for 60 minutes. Then, the initiator 1,3-bis(butylperoxyisopropyl)benzene (Perbutyl P manufactured by NOF Corporation) was added in the blending ratio shown in Table 1 to obtain a varnish-like resin composition (resin varnish) for each of the examples and comparative examples. The following evaluation boards were produced using this resin varnish.

[0274] (Heat resistance evaluation board) The resin varnishes obtained in the examples and comparative examples were each impregnated into a glass substrate (#2116 type, "L glass" (manufactured by Asahi Kasei Corporation, relative dielectric constant 4.6) and then heated and dried at 130°C for approximately 3 to 8 minutes to obtain a prepreg. At that time, the content of resin components such as polyphenylene ether and crosslinking agent (resin content) was adjusted to approximately 50 mass%.

[0275] Six sheets of each prepreg were then stacked together, and copper foil as shown in Table 1 was placed on both sides of each prepreg. The laminate was then heated and pressed at 200°C for 2 hours at a pressure of 3 MPa to obtain a copper-clad laminate for evaluation having a thickness of 750 μm.

[0276] [Oven heat resistance test] Using the obtained copper foil-clad laminate, test pieces were made according to JIS C 6481 and treated for one hour in thermostatic chambers equipped with air circulation devices set at 250℃, 260℃, 280℃, and 300℃. Test pieces that showed no abnormalities out of five were judged as "PASS", and those that showed "blistering" or "peeling" in one or more of the five test pieces were judged as "NG". In this test, samples that were rated "PASS" at 280℃ were deemed to have passed the test.

[0277] [Glass transition temperature (Tg)] The outer copper foil of the copper-clad laminate was entirely etched, and the Tg of the obtained sample was measured using a viscoelasticity spectrometer "DMS6100" manufactured by Seiko Instruments Inc. At this time, dynamic viscoelasticity measurement (DMA) was performed in a three-point bending mode at a frequency of 10 Hz, and the temperature at which tan δ was maximized when the temperature was raised from room temperature to 320°C at a heating rate of 5°C / min was defined as Tg.

[0278] (Transmission characteristic evaluation board) The resin varnishes obtained in the examples and comparative examples were each impregnated into a glass substrate (#1078 type, "L glass" (manufactured by Asahi Kasei Corporation, relative dielectric constant 4.6) and then heated and dried at 130°C for about 3 to 8 minutes to obtain a prepreg. At that time, the content of resin components such as polyphenylene ether and crosslinking agent (resin content) was adjusted to about 60 mass%.

[0279] Two sheets of each prepreg were then stacked together, and copper foil as shown in Table 1 was placed on both sides of each prepreg. The laminate was then heated and pressed at 200°C for 2 hours at a pressure of 3 MPa to obtain a copper-clad laminate for evaluation having a thickness of 150 μm.

[0280] [Transmission loss evaluation test] One side of the obtained double-sided board was processed to a line width of 100 to 200 μm, and then two more prepregs were laminated to sandwich the processed surface to produce a three-layer board. The line width was adjusted so that the characteristic impedance of the circuit after finishing was 50 Ω.

[0281] The transmission characteristics of the obtained laminate were evaluated by measuring the transmission loss using a network analyzer (N5230A manufactured by Keysight Technologies, Inc.) at a frequency of 20 GHz.

[0282] The test results are shown in Tables 3 and 4.

[0283] [Table 3]

[0284] [Table 4]

[0285] As is clear from the results in Table 3, it was confirmed that the laminate using the surface-treated copper foil and resin composition of the present invention has excellent heat resistance and also has very excellent transmission characteristics.

[0286] It was also found that a higher Tg could be obtained when a resin composition containing the polymer of the present invention in combination with a modified polyphenylene ether compound was used.

[0287] In contrast, in Comparative Examples 1 to 3 in which the resin composition of the present invention was not used, the transmission loss was inferior to that of the Examples. In Comparative Example 4 in which the amount of nickel attached in the heat-resistant treatment layer of the surface-treated copper foil was 0, heat resistance could not be obtained. On the other hand, in Comparative Examples 5 and 6 in which the amount of nickel attached in the heat-resistant treatment layer was excessive, the transmission characteristics were insufficient.

[0288] In addition, in Comparative Example 7, in which the copper particles in the fine roughening particle treatment layer were large, the transmission characteristics were poor and the heat resistance was not sufficient. In Comparative Example 8, in which no rust-proofing layer was formed, sufficient heat resistance could not be obtained.

[0289] This application is based on Japanese Patent Application No. 2019-092354, filed on May 15, 2019, the contents of which are incorporated herein by reference.

[0290] In order to express the present invention, the present invention has been described appropriately and sufficiently through the embodiments with reference to specific examples and drawings, etc., but it should be recognized that those skilled in the art can easily change and / or improve the above-mentioned embodiments. Therefore, unless the changes or improvements made by those skilled in the art are at a level that departs from the scope of the claims described in the claims, the changes or improvements are interpreted as being included in the scope of the claims. [Industrial Applicability]

[0291] The present invention has wide industrial applicability in technical fields such as electronic materials and electronic devices.

Claims

1. A copper-clad laminate comprising an insulating layer containing a cured product of a resin composition and a surface-treated copper foil on one or both sides of the insulating layer, The resin composition contains a polymer having a structural unit represented by the following formula (1) in the molecule: 【Chemistry 1】 (In formula (1), Z represents an arylene group, R 1 ~R 3 each independently represents a hydrogen atom or an alkyl group; R 4 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. and, The surface-treated copper foil comprises a copper foil, a copper fine roughening particle treatment layer, a heat-resistant treatment layer containing nickel, a rust-proofing treatment layer containing at least chromium, and a silane coupling agent treatment layer; The copper foil has a copper fine particle treated layer on at least one side thereof, The fine roughening particle treatment layer is composed of fine copper particles having a particle diameter of 40 to 200 nm, The heat-resistant treatment layer is provided on the fine roughening particle treatment layer, The rust-proofing layer is provided on the heat-resistant layer, The silane coupling agent treatment layer is provided on the rust-proofing treatment layer, and The amount of nickel deposited in the heat-resistant layer is 30 to 60 mg / m 2 Characterized in that Copper clad laminate.

2. The copper-clad laminate according to claim 1 , wherein the structural unit represented by the formula (1) includes a structural unit represented by the following formula (2): 【Chemistry 2】 (In formula (2), R 4 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; R 7 represents an arylene group having 6 to 12 carbon atoms.

3. The copper-clad laminate according to claim 2, wherein the structural unit represented by the formula (2) includes a structural unit represented by the following formula (3): 【Chemistry 3】 (In formula (3), R 4 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

4. The copper-clad laminate according to any one of claims 1 to 3, wherein the polymer further comprises a polymer having a structural unit represented by the following formula (4) in the molecule: 【Chemistry 4】 (In formula (4), R 8 ~R 10 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; R 11 represents an aryl group.

5. The copper-clad laminate according to claim 4, wherein the aryl group in the structural unit represented by the formula (4) includes an aryl group having an alkyl group having 1 to 6 carbon atoms.

6. The copper-clad laminate according to any one of claims 1 to 5, wherein the weight average molecular weight of the polymer is 1,500 to 40,000.

7. The polymer is represented by the formula (1), and R 1 ~R 3 The copper-clad laminate according to any one of claims 1 to 6, wherein the equivalent weight of the vinyl group contained in the structural unit in which is a hydrogen atom is 250 to 1,200.

8. The copper-clad laminate according to any one of claims 1 to 7, wherein the resin composition further contains a modified polyphenylene ether compound whose terminals are modified with the following formula (5) or (6): 【Chemistry 5】 (In formula (5), s represents an integer of 0 to 10. Z represents an arylene group. R 12 ~R 14 each independently represents a hydrogen atom or an alkyl group. 【Chemistry 6】 (In formula (6), R 15 represents a hydrogen atom or an alkyl group)

9. A resin-coated copper foil comprising a resin layer containing a resin composition or a semi-cured product of the resin composition, and a surface-treated copper foil on one side of the resin layer, The resin composition contains a polymer having a structural unit represented by the following formula (1) in the molecule: 【Chemistry 7】 (In formula (1), Z represents an arylene group, R 1 ~R 3 each independently represents a hydrogen atom or an alkyl group; R 4 ~R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. and, The surface-treated copper foil comprises a copper foil, a copper fine roughening particle treatment layer, a heat-resistant treatment layer containing nickel, a rust-proofing treatment layer containing at least chromium, and a silane coupling agent treatment layer; The copper foil has a copper fine particle treated layer on at least one side thereof, The fine roughening particle treatment layer is composed of fine copper particles having a particle diameter of 40 to 200 nm, The heat-resistant treatment layer is provided on the fine roughening particle treatment layer, The rust-proofing layer is provided on the heat-resistant layer, The silane coupling agent treatment layer is provided on the rust-proofing treatment layer, and The amount of nickel deposited in the heat-resistant layer is 30 to 60 mg / m 2 Characterized in that Resin-coated copper foil.

10. A circuit board using the copper-clad laminate according to any one of claims 1 to 8 or the resin-coated copper foil according to claim 9, the circuit board having a conductor pattern as a circuit on the surface.

Citation Information

Patent Citations

  • Novel azetidinone derivative and its salt

    JP1986010581A

  • Video signal processing circuit

    JP1986082584A

  • Copper foil for high frequency printed wiring board and its production method

    JP2006210689A

  • Polyphenylene ether resin composition, resin varnish, prepreg, metal-clad laminate, and printed wiring board

    JP2013023517A

  • Soluble polyfunctional vinyl aromatic copolymer, method for producing the same, curable resin composition, and cured product of the same