Optical multilayers
The optical laminate with a retardation layer and gas barrier layer addresses the issue of performance degradation in retardation plates by reducing oxygen diffusion, ensuring stability under UV exposure and maintaining optical performance.
Patent Information
- Application Number
- JP2020070542
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-09
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2040-04-09
AI Technical Summary
Existing retardation plates in flat panel displays are prone to changes in retardation value due to light exposure, particularly under high-intensity ultraviolet rays, leading to deterioration in optical performance.
An optical laminate comprising a retardation layer and a gas barrier layer with low oxygen gas permeability, where the gas barrier layer is adjacent to the retardation layer, effectively suppressing oxygen diffusion and maintaining optical performance under harsh environments.
The optical laminate maintains high durability and stability of optical performance by preventing changes in retardation value even under high-intensity ultraviolet rays and harsh conditions.
Smart Images

Figure 0007580200000009 
Figure 0007580200000010 
Figure 0007580200000011
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical laminate, and particularly to an optical laminate including a retardation layer and a gas barrier layer adjacent to the retardation layer. [Background technology]
[0002] Retardation plates showing reverse wavelength dispersion are known as retardation plates used in flat panel displays (FPDs). Polymerizable liquid crystal compounds forming such retardation plates generally have a maximum absorption in the ultraviolet region, and it is known that the retardation value of a retardation plate formed from the polymerizable liquid crystal compound is easily changed due to exposure to light in the ultraviolet to visible light regions. Since the change in the retardation value in a retardation plate can cause a decrease in the optical performance of the retardation plate, retardation plates that are less likely to change in retardation value even when exposed to ultraviolet light or the like have been developed.
[0003] For example, Patent Document 1 discloses a technology for maintaining a balance of changes in retardation value in the entire retardation film by producing a retardation film using a polymerizable liquid crystal composition containing two or more polymerizable liquid crystal compounds, including a polymerizable liquid crystal compound whose retardation value changes in a positive direction when exposed to ultraviolet light and a polymerizable liquid crystal compound whose retardation value changes in a negative direction. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-003177 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, as disclosed in the above Patent Document 1, progress has been made in the development of retardation plates that are less susceptible to changes in retardation value due to exposure to light, but there remains a strong demand for optical laminates (retardation plates) that have high durability.
[0006] The present invention aims to provide a novel solution to the above-mentioned demands, different from Patent Document 1, that is, a means that can satisfy the above-mentioned demands without using two types of polymerizable liquid crystal compounds that cause corresponding changes in retardation value upon exposure to light, and aims to provide an optical laminate including a retardation layer that is unlikely to change in optical performance even when irradiated with high-intensity ultraviolet light and has high durability such that performance changes are unlikely to occur even under harsh environments. [Means for solving the problem]
[0007] The present invention provides the following preferred embodiments. [1] A retardation layer including a retardation-exhibiting layer composed of a cured product of a polymerizable liquid crystal composition including at least one polymerizable liquid crystal compound, and a gas barrier layer adjacent to at least one surface of the retardation layer, The gas barrier layer is 500 cm 3 / (m 2 An optical laminate having an oxygen gas permeability of less than 1000 nm (24h·atm). [2] The optical laminate according to [1] above, wherein the gas barrier layer contains a polymer having a crosslinked structure. [3] The optical laminate according to [2] above, wherein the crosslinked structure is derived from a hydrophobic crosslinking agent. [4] The optical laminate according to [3] above, wherein the hydrophobic crosslinking agent comprises at least one selected from the group consisting of an isocyanate-based crosslinking agent, a polyaldehyde-based crosslinking agent, and a metal compound-based crosslinking agent. [5] The optical laminate according to any one of the above [2] to [4], wherein the polymer comprises a polyvinyl alcohol-based resin. [6] The optical laminate according to any one of [1] to [5] above, wherein the gas barrier layer is disposed adjacent to both sides of the retardation layer. [7] The optical laminate according to any one of the above [1] to [6], wherein the gas barrier layer covers at least one side surface in the thickness direction of the retardation layer. [8] The optical laminate according to any one of the above [1] to [7], further comprising a polarizer layer. [9] The optical laminate according to [8], wherein the polarizer layer and the retardation layer are laminated via only the gas barrier layer adjacent to the retardation layer. Effect of the Invention
[0008] According to the present invention, it is possible to provide an optical laminate including a retardation layer, which is unlikely to undergo change in optical performance even when irradiated with high-intensity ultraviolet light, and has high durability such that performance changes are unlikely to occur even in harsh environments. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a layer structure of an optical laminate of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of a layer structure of an optical laminate of the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional view showing an example of a layer structure of an optical laminate of the present invention. [Figure 4] FIG. 1 is a schematic cross-sectional view showing an example of a layer structure of an optical laminate of the present invention. [Diagram 5] FIG. 1 is a schematic cross-sectional view showing an example of a layer structure of an optical laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, the embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.
[0011] The optical laminate of the present invention includes a retardation layer and a gas barrier layer adjacent to at least one surface of the retardation layer. Hereinafter, an example of the layer structure of the optical laminate of the present invention will be described with reference to Figures 1 and 2, but the optical laminate of the present invention is not limited to these embodiments.
[0012] 1 includes a retardation layer 1 and a gas barrier layer 2 adjacent to one surface of the retardation layer 1. In this optical laminate 11, the retardation layer 1 includes an alignment film 3 and a retardation-exhibiting layer 4 formed on the alignment film 3. In this specification, the term "retardation layer" refers to a structure consisting of an alignment film and a retardation-expressing layer formed on the alignment film when the retardation-expressing layer is formed on an alignment film, and refers to a structure consisting of the retardation-expressing layer when the retardation-expressing layer is formed without an alignment film.
[0013] The optical laminate of the present invention may be configured to include other layers having various functions that can be incorporated into image display devices and the like, in addition to the retardation layer and the gas barrier layer. Examples of the other layers include a (peelable) substrate, a polarizer layer, a cured resin layer such as a protective layer or a hard coat layer, a pressure-sensitive adhesive layer, and a front plate. In the optical laminate 11 shown in FIG. 1, the retardation layer 1 is formed on a peelable substrate 5. For example, after peeling off the peelable substrate 5, a second gas barrier layer 2 is formed on the alignment film 3 side of the retardation layer 1, thereby obtaining an optical laminate 11 having a gas barrier layer 2 on both sides of the retardation layer 1 as shown in FIG. 2. In addition, for example, as shown in FIG. 3, a polarizer layer 7 is laminated on the gas barrier layer 2 of the laminate having the layer structure shown in FIG. 1 and FIG. 2 via a pressure-sensitive adhesive layer 6, thereby obtaining an optical laminate 11 (elliptical polarizing plate) including the retardation layer 1 and the polarizer layer 7. After peeling off the peelable substrate 5, these optical laminates can be incorporated into image display devices and the like by, for example, bonding the retardation layer 1 to a display element or the like via a pressure-sensitive adhesive layer.
[0014] One of the reasons for the decrease in retardation value caused by light exposure of the retardation plate formed from the cured product of a polymerizable liquid crystal compound having a maximum absorption in the ultraviolet region is thought to be the generation of peroxide radicals in the liquid crystal cured product due to light exposure in an environment where oxygen is present.For example, the adhesive layer constituting the optical laminate generally has a high gas permeability, so when the optical laminate contains a pressure-sensitive adhesive layer as a layer constituting the optical laminate, gaseous oxygen is likely to penetrate from the pressure-sensitive adhesive layer into the optical laminate, and the oxygen that has penetrated into the optical laminate is likely to diffuse into the retardation layer.The optical laminate of the present invention has a gas barrier layer with low oxygen gas permeability on at least one side of the retardation layer, and is therefore a laminate that has excellent effect of suppressing the diffusion of oxygen into the retardation layer.
[0015] The optical laminate of the present invention includes a gas barrier layer adjacent to at least one surface of the retardation layer, and the gas barrier layer has a thickness of 500 cm 3 / (m 2 The gas barrier layer having an oxygen gas permeability of the above-mentioned upper limit or less is adjacent to the retardation layer, and thus, for example, an effect of suppressing the diffusion of oxygen that has entered from the pressure-sensitive adhesive layer constituting the optical laminate into the retardation layer can be obtained. From the viewpoint of obtaining a higher effect of suppressing the diffusion of oxygen gas, the oxygen gas permeability of the gas barrier layer adjacent to the retardation layer is preferably 300 cm 3 / (m 2 ·24h·atm) or less, preferably 200cm 3 / (m 2 ·24h·atm) or less, more preferably 150cm 3 / (m 2 ·24h·atm) or less, particularly preferably 100cm 3 / (m 2 The lower the oxygen gas permeability, the better the oxygen gas diffusion suppression effect. Therefore, in the present invention, the lower limit of the oxygen gas permeability is not particularly limited, and is not limited to 0 cm 3 / (m 2 ·24h·atm) may also be used. The oxygen gas permeability of the gas barrier layer can be measured by a differential pressure gas permeability measuring method in accordance with JIS K 7126-1. In detail, it can be measured according to the method described in the examples below.
[0016] In the present invention, the gas barrier layer may be provided on only one side of the retardation layer, or may be provided adjacent to both sides.Which side of the retardation layer the gas barrier layer is to be arranged on may be appropriately determined according to the type and arrangement of other layers constituting the optical laminate other than the retardation layer and the gas barrier layer, but it is preferable that the gas barrier layer is present on the side of the retardation layer on the side where the pressure-sensitive adhesive layer is present in the final optical laminate.In addition, when the retardation layer is composed of an alignment film and a retardation-expressing layer, it is preferable that the gas barrier layer is present on the side opposite to the alignment film of the retardation-expressing layer.When gas barrier layers are present on both sides of the retardation layer, the oxygen gas permeability of at least one of the gas barrier layers must be equal to or less than the upper limit, and it is preferable that the oxygen gas permeability of both gas barrier layers on both sides is equal to or less than the upper limit.
[0017] In one embodiment of the present invention, it is preferable that the gas barrier layer covers at least one side surface in the thickness direction of the retardation layer. A general optical laminate is often in the form of a rectangular sheet at the end, and in such an optical laminate, there are four sides in the thickness direction of the retardation layer. In the present invention, the gas barrier layer covers at least one side surface in the thickness direction of the retardation layer, for example, means a state in which at least one of the sides of such a retardation layer is at least partially covered with a gas barrier layer. By covering the side surface in the thickness direction of the retardation layer with a gas barrier layer, it is possible to reduce the area in which the retardation layer is in direct contact with the external environment (outside air), and it is possible to prevent oxygen and moisture in the air from entering the layer through the side surface in the thickness direction of the retardation layer. This makes it easier to effectively suppress the decrease in the retardation value of the retardation layer due to light exposure. In the optical laminate of the present invention, it is more preferable that the entire surface of at least one side surface in the thickness direction of the retardation layer is covered with a gas barrier layer, and it is even more preferable that the entire surface of all sides of the retardation layer is covered with a gas barrier layer.
[0018] In the present invention, the thickness of the gas barrier layer disposed adjacent to the retardation layer can be appropriately determined depending on the material constituting the gas barrier layer, the layer structure of the optical laminate, etc. The thickness of the gas barrier layer is preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more from the viewpoint of ensuring sufficient gas barrier properties. In addition, from the viewpoint of thinning the optical laminate, suppressing color unevenness due to interference, and imparting flexibility, it is preferably 50 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. When multiple gas barrier layers are present in the optical laminate of the present invention, the thicknesses of those gas barrier layers may be the same or different from each other, but it is preferable that all of the multiple gas barrier layers have a thickness within the above range. The thickness of the gas barrier layer can be measured by a thickness meter.
[0019] In the optical laminate of the present invention, the gas barrier layer disposed adjacent to the retardation layer is preferably a layer containing a polymer. The polymer material capable of forming the gas barrier layer is preferably a polymer having an oxygen gas permeability of 500 cm 3 / (m 2 The polymer material is not particularly limited as long as it can obtain a layer having a viscosity of 0.1-24h·atm or less, and a known polymer material can be used, but it is preferable to include a resin as the polymer material. In the present invention, the resin constituting the gas barrier layer may be either a thermoplastic resin or a thermosetting resin, and examples thereof include polyvinyl alcohol resin, polyester resin, polyolefin resin, polyamide resin, polyimide resin, polycarbonate resin, acrylic resin, and epoxy resin. These may be used alone or in combination of two or more. Among them, polyvinyl alcohol resin and epoxy resin are preferable as the polymer material, and polyvinyl alcohol resin is more preferable from the viewpoint of easily forming a gas barrier layer having a low oxygen gas permeability and excellent effect of suppressing the intrusion of oxygen gas into the retardation layer.
[0020] In one embodiment of the present invention, the gas barrier layer disposed adjacent to the retardation layer is formed from a resin composition containing a polyvinyl alcohol-based resin (hereinafter, also referred to as a "PVA-based resin composition"). In this specification, the polyvinyl alcohol resin refers to a resin containing 50% by mass or more of a structural unit derived from vinyl alcohol. The polyvinyl alcohol resin refers to a resin containing 50% by mass or more of a structural unit derived from vinyl alcohol. The polyvinyl alcohol resin can be obtained by saponifying a polyvinyl ester resin having a structural unit derived from a vinyl ester. Examples of the vinyl ester constituting the polyvinyl ester resin include vinyl acetate, vinyl butyrate, and vinyl propionate, and vinyl acetate is preferred.
[0021] The polyvinyl ester resin may be a homopolymer of a vinyl ester such as vinyl acetate, or may be a copolymer of the vinyl ester with another monomer copolymerizable therewith. Examples of other monomers that can be copolymerized with the vinyl ester include unsaturated carboxylic acids, unsaturated sulfonic acids, olefins, vinyl ethers, and acrylamides having an ammonium group.
[0022] The polyvinyl alcohol resin used in the gas barrier layer may be a partially saponified polyvinyl alcohol resin or a completely saponified polyvinyl alcohol resin. The degree of saponification of the polyvinyl alcohol resin is not particularly limited and may be appropriately determined, but is generally 70 mol% or more, preferably 80 mol% or more, more preferably 85 mol% or more, and even more preferably 90 mol% or more. When the degree of saponification of the polyvinyl alcohol resin is the above lower limit or more, the water resistance of the resulting gas barrier layer and the adhesion between the gas barrier layer and the adjacent layer are likely to be improved. The upper limit of the degree of saponification of the polyvinyl alcohol resin may be 100 mol% or less, and preferably 99.95 mol% or less. The degree of saponification of the polyvinyl alcohol resin can be measured in accordance with the method described in JIS K6726.
[0023] The method for saponifying the polyvinyl ester resin is not particularly limited, and any conventionally known method can be used. For example, the method includes saponification in an organic solvent such as alcohol in the presence of a catalyst.
[0024] The polyvinyl alcohol resin used in the gas barrier layer may be a homopolymer or a copolymer. By selecting the type of monomer constituting the copolymer with polyvinyl alcohol, various functions such as oxygen gas permeation inhibition, water resistance, and adhesion to adjacent layers can be imparted to the gas barrier layer. Examples of polyvinyl alcohol copolymers include ethylene-polyvinyl alcohol copolymers, acrylic acid, and methyl methacrylate-polyvinyl alcohol. The amount of vinyl alcohol units in the polyvinyl alcohol copolymer is preferably 80 to 98 mol%, more preferably 85 to 98 mol%.
[0025] The average degree of polymerization of polyvinyl alcohol is preferably 1000 to 10000, more preferably 1000 to 5000, and further preferably 1100 to 3000. Here, the average degree of polymerization means the number average degree of polymerization. When the average degree of polymerization is within this range, the stability of the physical properties of the aqueous solution containing the polyvinyl alcohol, and the oxygen gas barrier property and water resistance of the obtained cured film can be achieved at the same time. The average degree of polymerization of polyvinyl alcohol means the average degree of polymerization measured according to the description of JIS K6726.
[0026] The polyvinyl alcohol resin used in the gas barrier layer is preferably modified. Examples of modified polyvinyl alcohol resins include acetoacetyl group-modified polyvinyl alcohol resins, carboxylic acid-modified polyvinyl alcohol resins, carbonyl group-modified polyvinyl alcohol resins, sulfonic acid-modified polyvinyl alcohol resins, hydrazide group-modified polyvinyl alcohol resins, thiol group-modified polyvinyl alcohol resins, alkyl group-modified polyvinyl alcohol resins, silyl group-modified polyvinyl alcohol resins, polyethylene glycol group-modified polyvinyl alcohol resins, ethylene oxide group-modified polyvinyl alcohol resins, urethane bond-modified polyvinyl alcohol resins, and phosphate ester group-modified polyvinyl alcohol resins. The use of such modified polyvinyl alcohol resins increases the number of options for crosslinking reactions by a crosslinking agent described later, making it easier to increase the crosslinking reactivity, and improving the water resistance of the gas barrier layer and the adhesion between the gas barrier layer and adjacent layers, which is preferable.
[0027] The polyvinyl alcohol-based resins may be used alone or in combination of two or more kinds. In addition, commercially available products may be used as the polyvinyl alcohol-based resin.
[0028] In the present invention, the gas barrier layer preferably contains a polymer having a crosslinked structure. By containing a polymer having a crosslinked structure, the gas barrier layer has a dense structure, which tends to improve the oxygen gas permeation suppression effect and tends to improve the adhesion between the gas barrier layer and the adjacent layer. When the gas barrier layer is formed from a PVA-based resin composition, a crosslinking agent that can be used to introduce a crosslinking structure into the polyvinyl alcohol-based polymer can be a compound known as a crosslinking agent for polyvinyl alcohol-based resins. Examples of such crosslinking agents include water-soluble additives and crosslinking agents such as ionic crosslinking agents such as glyoxylate salts and epoxy-based crosslinking agents, isocyanate-based crosslinking agents, polyaldehyde-based crosslinking agents such as glyoxal and glyoxal derivatives, and hydrophobic crosslinking agents such as zirconium chloride-based or titanium lactate-based metal compound-based crosslinking agents. Among them, from the viewpoint of imparting the gas barrier layer with high adhesion to adjacent layers as well as excellent water resistance, it is preferable that the crosslinking structure in the polymer constituting the gas barrier layer is derived from a hydrophobic crosslinking agent, and more preferably, it is derived from at least one crosslinking agent selected from the group consisting of isocyanate-based crosslinking agents, polyaldehyde-based crosslinking agents, and metal compound-based crosslinking agents. The crosslinking agents may be used alone or in combination of two or more.
[0029] As the crosslinking agent, a commercially available product can be used. Examples of the water-soluble crosslinking agent include "Safelink SPM-01" (manufactured by Mitsubishi Chemical Corporation) and "Sumirez Resin650" (manufactured by Taoka Chemical Co., Ltd.). Examples of the hydrophobic crosslinking agent include "Burnoc DNW-5000" (manufactured by DIC Corporation), "Orgatics ZB-400" (manufactured by Matsumoto Fine Chemical Co., Ltd.), and "Orgatics TC-310" (manufactured by Matsumoto Fine Chemical Co., Ltd.).
[0030] In the present invention, when a crosslinking agent is used to introduce a crosslinked structure into the polymer constituting the gas barrier layer, the amount of the crosslinking agent added may be appropriately determined depending on the type of the crosslinking agent used. The content of the crosslinking agent in the PVA resin composition is usually 0.1 to 100 parts by mass, preferably 1 to 50 parts by mass, and more preferably 10 to 30 parts by mass, relative to 100 parts by mass of the polyvinyl alcohol resin. When the content of the crosslinking agent is within the above range, the gas barrier layer becomes dense, the oxygen gas permeation suppression effect is easily improved, and the adhesion between the gas barrier layer and the layer adjacent thereto is easily improved. Furthermore, when a hydrophobic crosslinking agent is used, the resulting gas barrier layer can be given sufficiently high water resistance.
[0031] The PVA-based resin composition capable of forming a gas barrier layer is usually prepared as a solution in which a polyvinyl alcohol-based resin is dissolved in a solvent. The solvent in the PVA-based resin composition includes water, alcohol, a mixture of water and alcohol, and the like, and water is preferred. For example, the PVA-based resin composition is applied to the surface on which the gas barrier layer is to be formed, and the coating is dried and cured to obtain the gas barrier layer.
[0032] The solid content of the PVA resin obtained by adding a solvent to the polyvinyl alcohol resin or the crosslinking agent is preferably 2 to 50% by mass, more preferably 5 to 30% by mass, and even more preferably 5 to 15% by mass. When the solid content of the PVA resin composition is within the above range, the viscosity of the composition is low, and thus the coatability and handleability are improved. The "solid content" referred to here refers to the components remaining after removing the solvent such as water from the PVA resin composition.
[0033] The PVA-based resin composition may contain other components such as additives in addition to the polyvinyl alcohol-based resin, the crosslinking agent, and the solvent such as water. Examples of such other components include preservatives and leveling agents. When the composition for forming a gas barrier layer contains other components such as additives, the amount of such components is preferably 10% by mass or less, more preferably 5% by mass or less, based on the solid content of the composition for forming a gas barrier layer.
[0034] The method for forming a coating film of the PVA-based resin composition is not particularly limited, and examples thereof include known methods such as coating methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography.
[0035] The drying temperature and time for forming a gas barrier layer from a coating of a PVA-based resin composition are not particularly limited, and may be appropriately determined depending on the composition of the gas barrier layer-forming composition used. The drying process can be carried out, for example, by blowing hot air, and the temperature is usually within a range of 40 to 100° C., preferably 60 to 100° C. The drying time is usually 10 to 600 seconds.
[0036] In another embodiment of the present invention, the gas barrier layer disposed adjacent to the retardation layer is formed from a curable composition containing an active energy ray-curable resin (hereinafter also referred to as a "curable composition for forming a gas barrier layer"). Examples of the curable composition for forming the gas barrier layer include a cationic polymerizable curable composition containing an epoxy compound and a cationic polymerization initiator, a radically polymerizable curable composition containing an acrylic curing component and a radical polymerization initiator, a curable composition containing both a cationic polymerizable curing component such as an epoxy compound and a radically polymerizable curing component such as an acrylic compound, and further containing a cationic polymerization initiator and a radical polymerization initiator, and a curable composition that does not contain a polymerization initiator and is cured by irradiating with an electron beam, etc. Among them, from the viewpoints of durability against high-intensity ultraviolet light due to low oxygen gas permeability and water resistance, it is preferable that the gas barrier layer is a layer containing an epoxy resin, and it is preferable that the gas barrier layer is formed from a curable composition containing a cationic polymerizable epoxy compound that contains an epoxy compound.
[0037] Suitable epoxy compounds include hydrogenated epoxy compounds (glycidyl ethers of polyols having alicyclic rings) obtained by reacting epichlorohydrin with alicyclic polyols obtained by hydrogenating aromatic rings of aromatic polyols; aliphatic epoxy compounds such as polyglycidyl ethers of aliphatic polyhydric alcohols or their alkylene oxide adducts; and alicyclic epoxy compounds, which are epoxy compounds having one or more epoxy groups bonded to an alicyclic ring in the molecule. These may be used alone or in combination of two or more.
[0038] The curable composition for forming a gas barrier layer may be solvent-free, or the active ingredient may be diluted with a solvent. When the active ingredient is diluted with a solvent, examples of the solvent include volatile solvents such as toluene, xylene, methyl ethyl ketone, and methylene chloride. When the active ingredient is diluted with a solvent, the dilution ratio is preferably 2 to 40 times, more preferably 10 to 30 times. In this specification, the above-mentioned "active ingredient" means the solid content of the curable composition for forming a gas barrier layer, that is, all components excluding volatile components such as solvents from the curable composition for forming a gas barrier layer.
[0039] The content of the epoxy compound in the active ingredients of the curable composition for forming a gas barrier layer is preferably 70 to 99 mass %, more preferably 90 to 95 mass %.
[0040] When the curable composition for forming a gas barrier layer contains a cationic epoxy compound as a curable component, it preferably contains a photocationic polymerization initiator. Examples of the photocationic polymerization initiator include aromatic diazonium salts, onium salts such as aromatic iodonium salts and aromatic sulfonium salts, and iron-allene complexes.
[0041] The content of the cationic photopolymerization initiator in the curable composition for forming a gas barrier layer is preferably 0.1 to 30 parts by mass, more preferably 1 to 10 parts by mass, based on 100 parts by mass of the cationic epoxy compound.
[0042] The curable composition for forming a gas barrier layer may contain additives such as cationic polymerization accelerators such as oxetane and polyol, photosensitizers, ion trapping agents, antioxidants, chain transfer agents, tackifiers, thermoplastic resins, fillers, flow adjusters, plasticizers, defoamers, antistatic agents, leveling agents, and / or solvents, as necessary.
[0043] The gas barrier layer can be formed by applying the curable composition for forming the gas barrier layer to the surface on which the gas barrier layer is to be formed, and then curing the composition by irradiation with active energy rays. The method for applying the curable composition for forming the gas barrier layer can be the same as the method for applying the PVA-based resin composition.
[0044] Examples of light sources for active energy rays include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, halogen lamps, carbon arc lamps, tungsten lamps, gallium lamps, excimer lasers, LED light sources emitting light in the wavelength range of 380 to 440 nm, chemical lamps, black light lamps, microwave-excited mercury lamps, and metal halide lamps.
[0045] The UV irradiation intensity is usually 10 to 3,000 mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a polymerization initiator. The time for light irradiation is usually 0.1 seconds to 10 minutes, preferably 1 second to 5 minutes, more preferably 5 seconds to 3 minutes, and further preferably 10 seconds to 1 minute. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 to 3,000 mJ / cm. 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 It is.
[0046] In the present invention, when the gas barrier layer covers at least one side surface in the thickness direction of the retardation layer, the side surface in the thickness direction of the retardation layer can be covered with the gas barrier layer by, for example, a method in which the retardation layer to be covered with the gas barrier layer is immersed in a composition (solution) for forming a gas barrier layer, or the retardation layer and the release film are bonded via a composition (solution) for forming a gas barrier in such a manner that the side surface of the retardation layer is covered by the side surface of the release film.
[0047] In the optical laminate of the present invention, the retardation layer includes a retardation-exhibiting layer made of a cured product of a polymerizable liquid crystal composition (hereinafter also referred to as "polymerizable liquid crystal composition") containing at least one polymerizable liquid crystal compound. The polymerizable liquid crystal compound forming the retardation-exhibiting layer can be appropriately selected from conventionally known polymerizable liquid crystal compounds in the field of retardation films according to the desired optical properties.
[0048] The polymerizable liquid crystal compound is a liquid crystal compound having a polymerizable group. The polymerizable liquid crystal compound is generally a polymer (cured product) obtained by polymerizing the polymerizable liquid crystal compound alone in a state of being aligned in a specific direction, and includes a polymerizable liquid crystal compound exhibiting positive wavelength dispersion and a polymerizable liquid crystal compound exhibiting reverse wavelength dispersion. In the present invention, only one type of polymerizable liquid crystal compound may be used, or both types of polymerizable liquid crystal compounds may be mixed and used. The optical laminate of the present invention is excellent in the effect of reducing the amount of oxygen gas diffused into the retardation layer by disposing a gas barrier layer with low oxygen gas permeability adjacent to the retardation layer. For this reason, the effect of the present invention can be more significantly obtained when the retardation-exhibiting layer is formed from a polymerizable liquid crystal compound that generally has a maximum absorption in the ultraviolet region and is easily exposed to light in an environment where oxygen is present. Therefore, the retardation-exhibiting layer constituting the optical laminate of the present invention is preferably a cured product of a polymerizable liquid crystal composition containing a polymerizable liquid crystal compound exhibiting so-called reverse wavelength dispersion.
[0049] The polymerizable group refers to a group that can participate in a polymerization reaction. In the present invention, the polymerizable group of the polymerizable liquid crystal compound that forms the retardation layer is preferably a photopolymerizable group. The photopolymerizable group refers to a polymerizable group that can participate in a polymerization reaction by a reactive species generated from a photopolymerization initiator, such as an active radical or an acid. Examples of the photopolymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, a (meth)acryloyl group, an oxiranyl group, and an oxetanyl group. Among them, a (meth)acryloyl group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferable, and an acryloyl group is more preferable. The liquid crystal property exhibited by the polymerizable liquid crystal compound may be a thermotropic liquid crystal or a lyotropic liquid crystal, but a thermotropic liquid crystal is preferable in terms of the possibility of precise film thickness control. In addition, the phase order structure in the thermotropic liquid crystal may be a nematic liquid crystal, a smectic liquid crystal, or a discotic liquid crystal. The polymerizable liquid crystal compounds can be used alone or in combination of two or more kinds.
[0050] Polymerizable liquid crystal compounds having a so-called T-shaped or H-shaped molecular structure are likely to exhibit reverse wavelength dispersion when polymerized and cured, and polymerizable liquid crystal compounds having a T-shaped molecular structure tend to exhibit even stronger reverse wavelength dispersion.
[0051] The reverse wavelength dispersion is an optical property in which the in-plane retardation value at a short wavelength is larger than the in-plane retardation value at a long wavelength. Specifically, in the present invention, the polymerizable liquid crystal compound exhibiting the reverse wavelength dispersion is a polymerizable liquid crystal compound in which a polymer in an oriented state is represented by the following formula: Re(450) <Re(550)<Re(650) (Re(λ) represents the front retardation of the retarder at wavelength λ.) The compound satisfies the following formula: Furthermore, in the present invention, it is preferable that the polymerizable liquid crystal compound exhibiting reverse wavelength dispersion has a polymer in an oriented state that satisfies the following formulae (I) and (II). Re(450) / Re(550)≦1.0 (I) 1.0≦Re(650) / Re(550) (II) (In the formula, Re(λ) has the same meaning as above.)
[0052] The polymerizable liquid crystal compound exhibiting reverse wavelength dispersion is preferably a compound having the following characteristics (A) to (D). (A) A compound capable of forming a nematic phase or a smectic phase. (B) The polymerizable liquid crystal compound has π electrons in the long axis direction (a). (C) It has π electrons in a direction intersecting with the long axis direction (a) [intersecting direction (b)]. (D) The total number of π electrons present in the long axis direction (a) is N(πa), and the total number of molecular weights present in the long axis direction is N(Aa), where N(πa) is the total number of π electrons present in the long axis direction, and N(Aa) is the total number of molecular weights present in the long axis direction. The π electron density in the long axis direction (a) of a polymerizable liquid crystal compound is defined by the following formula (i): D(πa)=N(πa) / N(Aa) (i) The total number of π electrons present in the cross direction (b) is N(πb), and the total number of molecular weights present in the cross direction (b) is N(Ab), where N(πb) is the total number of π electrons present in the cross direction (b), and the π electron density in the cross direction (b) of the polymerizable liquid crystal compound is defined by the following formula (ii): D(πb)=N(πb) / N(Ab) (ii) and the formula (iii) 0≦[D(πa) / D(πb)]<1 (iii) [That is, the π electron density in the intersecting direction (b) is greater than the π electron density in the long axis direction (a)]. As described above, a polymerizable liquid crystal compound having π electrons on the long axis and in the direction intersecting therewith generally tends to have a T-shaped structure.
[0053] In the above features (A) to (D), the long axis direction (a) and the number of π electrons N are defined as follows. The long axis direction (a) is, for example, in the case of a compound having a rod-like structure, the long axis direction of the rod. The number of π electrons present in the long axis direction (a), N(πa), does not include the π electrons lost due to the polymerization reaction. The number of π electrons present along the long axis (a), N(πa), is the total number of π electrons on the long axis and those conjugated with it, and includes, for example, the number of π electrons present in rings present along the long axis (a) that satisfy Hückel's rule. The number of π electrons present in the intersecting direction (b), N(πb), does not include the π electrons lost due to the polymerization reaction. A polymerizable liquid crystal compound that satisfies the above conditions has a mesogenic structure in the long axis direction, and this mesogenic structure allows the compound to exhibit a liquid crystal phase (nematic phase, smectic phase).
[0054] A nematic phase or a smectic phase can be formed by heating the polymerizable liquid crystal compound satisfying the above (A) to (D) to a temperature equal to or higher than the phase transition temperature. In the nematic phase or the smectic phase formed by the orientation of the polymerizable liquid crystal compound, the long axis directions of the polymerizable liquid crystal compound are usually aligned so as to be parallel to each other, and the long axis direction is the orientation direction of the nematic phase or the smectic phase. When such a polymerizable liquid crystal compound is made into a film and polymerized in the nematic phase or the smectic phase state, a polymer film can be formed that is made of a polymer that is polymerized in a state of being aligned in the long axis direction (a). This polymer film absorbs ultraviolet light by the π electrons in the long axis direction (a) and the π electrons in the cross direction (b). Here, the maximum absorption wavelength of ultraviolet light absorbed by the π electrons in the cross direction (b) is defined as λbmax. λbmax is usually 300 nm to 400 nm. The π electron density satisfies the above formula (iii), and the π electron density in the cross direction (b) is greater than the π electron density in the long axis direction (a), resulting in a polymer film in which the absorption of linearly polarized ultraviolet light (wavelength λbmax) having a vibration plane in the cross direction (b) is greater than the absorption of linearly polarized ultraviolet light (wavelength λbmax) having a vibration plane in the long axis direction (a). The ratio (the ratio of the absorbance in the cross direction (b) of linearly polarized ultraviolet light / the absorbance in the long axis direction (a)) is, for example, greater than 1.0, preferably 1.2 or more, and usually 30 or less, for example 10 or less.
[0055] Generally, the polymerizable liquid crystal compound having the above characteristics is often one that exhibits reverse wavelength dispersion in the birefringence of the polymer when polymerized in a state aligned in one direction. Specific examples of such polymerizable liquid crystal compounds include those represented by the following formula (1): [ka] When the polymerizable liquid crystal compound has a structure represented by the above formula (1), it is possible to obtain a polymerizable liquid crystal composition that exhibits reverse wavelength dispersion, is capable of uniform polarization conversion in a wide wavelength range, and can provide good display characteristics when used in a display device.
[0056] In formula (1), Ar a is a divalent aromatic group which may have a substituent. L 1a , L 2a , B 1a and B. 2a are each independently a single bond or a divalent linking group, an alkylene group having 1 to 4 carbon atoms, -COO-, -OCO-, -O-, -S-, -ROR-, -RCOOR-, -ROCOR-, ROC=OOR-, -N=N-, -CR'=CR'-, or -C≡C-. Here, each R independently represents a single bond or an alkylene group having 1 to 4 carbon atoms, and each R' independently represents an alkyl group having 1 to 4 carbon atoms or a hydrogen atom. G 1a and G 2a each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group, a hydrogen atom contained in the alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. E 1a and E 2aeach independently represents an alkanediyl group having 1 to 17 carbon atoms. Here, a hydrogen atom contained in the alkanediyl group may be substituted with a halogen atom, and —CH 2 - may be substituted by -O-, -S- or -Si-. P 1a and P 2a each independently represents a hydrogen atom or a polymerizable group; P 1a and P 2a At least one of the groups is a polymerizable group. k a and l a each independently represents an integer of 0 to 3, and 1≦k a +l a Here, 2≦k a +l a If B 1a and B. 2a , G 1a and G 2a may be the same as or different from each other.
[0057] L 1a and L 2a are each independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -ROR-, -RCOOR-, -ROCOR-, -ROC=OOR-, -N=N-, -CR'=CR'-, or -C≡C-. Here, R is each independently a single bond or an alkylene group having 1 to 4 carbon atoms, and R' is each independently an alkyl group having 1 to 4 carbon atoms or a hydrogen atom. 1a and L 2a are each independently preferably a single bond, -OR''-, or -CH 2 -, -CH 2 CH 2 -, -COOR''-, or -OCOR''-, where R'' is independently a single bond, -CH 2 -, -CH 2 CH 2 - represents either 1a and L 2a are each independently preferably a single bond, -O-, or -CH2 CH 2 -, -COO-, -COOCH 2 CH 2 - or -OCO-. 1a and L 2a may be the same or different from each other, but from the viewpoint of facilitating the production of the polymerizable liquid crystal compound and reducing the production cost, L 1a and L 2a are preferably the same as each other. 1a and L 2a are identical to each other, Ar a L when viewed from the center 1a and L 2a This means that the structures of B are identical to each other. 1a and B 2a , G 1a and G 2a , E 1a and E 2a , P 1a and P 2a The same is true for the relationship in
[0058] B 1a and B. 2a are each independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -ROR-, -RCOOR-, -ROCOR-, or -ROC=OOR-. Here, R is each independently a single bond or an alkylene group having 1 to 4 carbon atoms. B 1a and B. 2a are each independently preferably a single bond, -OR''-, or -CH 2 -, -CH 2 CH 2 -, -COOR''-, or -OCOR''-. where R'' is independently a single bond, -CH 2 -, -CH 2 CH 2 - represents either 1a and B. 2a are each independently preferably a single bond, -O-, or -CH 2 CH 2 -, -COO-, -COOCH2 CH 2 -, -OCO- or -OCOCH 2 CH 2 In formula (1), B 1a and B. 2a may be the same or different from each other, but from the viewpoint of facilitating the production of the polymerizable liquid crystal compound and reducing the production cost, B 1a and B 2a are preferably identical to each other.
[0059] G 1a and G 2a are each independently preferably a 1,4-phenylenediyl group which may be substituted with at least one substituent selected from the group consisting of halogen atoms and alkyl groups having 1 to 4 carbon atoms, or a 1,4-cyclohexanediyl group which may be substituted with at least one substituent selected from the group consisting of halogen atoms and alkyl groups having 1 to 4 carbon atoms, more preferably a 1,4-phenylenediyl group substituted with a methyl group, an unsubstituted 1,4-phenylenediyl group, or an unsubstituted 1,4-trans-cyclohexanediyl group, and particularly preferably an unsubstituted 1,4-phenylenediyl group or an unsubstituted 1,4-trans-cyclohexanediyl group. 1a and G 2a may be the same or different from each other, but from the viewpoint of facilitating the production of the polymerizable liquid crystal compound and reducing the production cost, G 1a and G 2a are preferably identical to each other. 1a and G 2a When a plurality of L are present, it is preferable that at least one of them is a divalent alicyclic hydrocarbon group. 1a or L 2a G binds to 1a and G 2a At least one of the groups is preferably a divalent alicyclic hydrocarbon group. In particular, L 1a or L 2a G binds to 1a and G 2aIt is more preferable that each of the above is a 1,4-trans-cyclohexanediyl group.
[0060] E 1a and E 2a are each independently preferably an alkanediyl group having 1 to 17 carbon atoms, and more preferably an alkanediyl group having 4 to 12 carbon atoms. 1a and E 2a may be the same or different from each other, but from the viewpoint of facilitating the production of the polymerizable liquid crystal compound and reducing the production cost, E 1a and E 2a are preferably identical to each other.
[0061] k a and l a From the viewpoint of inverse wavelength dispersion, 2≦k a +l a The range of ≦6 is preferred, and k a +l a = 4 is preferable, and k a =2 and l a It is more preferable that =2.
[0062] P 1a or P 2a Examples of the polymerizable group represented by the formula (1) include an epoxy group, a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among these, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferred, and an acryloyloxy group is more preferred. In the formula (1), P 1a and P 2a may be the same or different from each other, but from the viewpoint of facilitating the production of the polymerizable liquid crystal compound and reducing the production cost, E 1a and E 2a are preferably identical to each other.
[0063] From the viewpoint of facilitating the production of polymerizable liquid crystal compounds and reducing the production cost, L 1a =L 2a And G 1a =G 2a And B 1a =B 2a And E 1a =E 2a And P 1a =P 2a Katsuk a =l a It is more preferable that:
[0064] Ar a is a divalent aromatic group which may have a substituent. In the present invention, the aromatic group refers to a group having a planar ring structure, the number of π electrons of which is [4n+2] (n represents an integer) according to the Huckel rule, and when a ring structure is formed by including heteroatoms such as -N= or -S-, the aromatic group satisfies the Huckel rule including the non-covalent bond electron pairs on these heteroatoms and has aromaticity.
[0065] Ar a The optionally substituted aromatic group represented by the following formula (I) preferably has an optionally substituted aromatic hydrocarbon ring or an optionally substituted aromatic heterocycle. Examples of the aromatic hydrocarbon ring include a benzene ring, a naphthalene ring, and an anthracene ring, and examples of the aromatic heterocycle include a furan ring, a benzofuran ring, a pyrrole ring, an indole ring, a thiophene ring, a benzothiophene ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, a triazole ring, a triazine ring, a pyrroline ring, an imidazole ring, a pyrazole ring, a thiazole ring, a benzothiazole ring, a thienothiazole ring, an oxazole ring, a benzoxazole ring, and a phenanthroline ring. a When a nitrogen atom is contained, the nitrogen atom preferably has π electrons.
[0066] Among them, Ar aPreferably, Ar has an aromatic heterocycle containing at least two heteroatoms selected from the group consisting of nitrogen atoms, oxygen atoms, and sulfur atoms, more preferably has a thiazole ring or a benzothiazole ring, and further preferably has a benzothiazole ring. a has an aromatic heterocycle containing at least two heteroatoms selected from the group consisting of nitrogen atoms, oxygen atoms, and sulfur atoms, the aromatic heterocycle is 1a and L 2b may be directly bonded to form a divalent aromatic group, and L 1a and L 2b The aromatic heterocycle may be included as a substituent of a divalent aromatic group directly bonded to the aromatic heterocycle. a It is preferred that the entire group is sterically configured in a direction approximately perpendicular to the molecular orientation direction.
[0067] In formula (1), Ar a The total number of π electrons contained in the divalent aromatic group represented by N π is preferably 12 or more, more preferably 13 or more, and even more preferably 16 or more. Also, it is preferably 32 or less, more preferably 30 or less, even more preferably 28 or less, and particularly preferably 24 or less.
[0068] Ar a Examples of the aromatic group represented by the formula include groups represented by the following formulae (Ar-1) to (Ar-22). [ka]
[0069] In formulae (Ar-1) to (Ar-22), * represents a linking portion, Z 0 , Z 1 and Z 2each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, an alkylsulfinyl group having 1 to 12 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, a carboxyl group, a fluoroalkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkylthio group having 1 to 12 carbon atoms, an N-alkylamino group having 1 to 12 carbon atoms, an N,N-dialkylamino group having 2 to 12 carbon atoms, an N-alkylsulfamoyl group having 1 to 12 carbon atoms, or an N,N-dialkylsulfamoyl group having 2 to 12 carbon atoms.
[0070] Q 1 and Q 2 are each independently -CR 2’ R 3’ -, -S-, -NH-, -NR 2’ -, -CO- or -O-; R 2’ and R 3’ each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0071] J 1 and J. 2 each independently represents a carbon atom or a nitrogen atom.
[0072] Y 1 , Y 2 and Y 3 each independently represents an optionally substituted aromatic hydrocarbon group or an optionally substituted aromatic heterocyclic group.
[0073] W 1 and W 2 each independently represents a hydrogen atom, a cyano group, a methyl group or a halogen atom; and m represents an integer of 0 to 6.
[0074] Y 1 , Y 2 and Y 3Examples of the aromatic hydrocarbon group in the formula (I) include aromatic hydrocarbon groups having 6 to 20 carbon atoms, such as a phenyl group, a naphthyl group, an anthryl group, a phenanthryl group, and a biphenyl group, of which a phenyl group and a naphthyl group are preferred, and a phenyl group is more preferred. Examples of the aromatic heterocyclic group in the formula (I) include aromatic heterocyclic groups having 4 to 20 carbon atoms and containing at least one heteroatom, such as a nitrogen atom, an oxygen atom, or a sulfur atom, such as a furyl group, a pyrrolyl group, a thienyl group, a pyridinyl group, a thiazolyl group, and a benzothiazolyl group, of which a furyl group, a thienyl group, a pyridinyl group, a thiazolyl group, and a benzothiazolyl group are preferred.
[0075] Y 1 , Y 2 and Y 3 may each independently be an optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group. The polycyclic aromatic hydrocarbon group refers to a condensed polycyclic aromatic hydrocarbon group or a group derived from an aromatic ring assembly. The polycyclic aromatic heterocyclic group refers to a condensed polycyclic aromatic heterocyclic group or a group derived from an aromatic ring assembly.
[0076] Z 0 , Z 1 and Z 2 are each preferably independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, or an alkoxy group having 1 to 12 carbon atoms; Z 0 is more preferably a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a cyano group; Z 1 and Z 2 is more preferably a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group, or a cyano group.
[0077] Q 1 and Q 2 -NH-, -S-, -NR 2’ -, -O- are preferred, R 2’ is preferably a hydrogen atom, and among these, -S-, -O-, and -NH- are particularly preferable.
[0078] In formulas (Ar-16) to (Ar-22), Y 1 is the nitrogen atom to which it is bonded and Z0 and may form an aromatic heterocyclic group. Examples of the aromatic heterocyclic group include those mentioned above as aromatic heterocyclic rings that Ar may have, such as a pyrrole ring, an imidazole ring, a pyrroline ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, an indole ring, a quinoline ring, an isoquinoline ring, a purine ring, and a pyrrolidine ring. This aromatic heterocyclic group may have a substituent. In addition, Y 1 is the nitrogen atom to which it is bonded and Z 0 In addition, it may be the above-mentioned optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group, for example, a benzofuran ring, a benzothiazole ring, a benzoxazole ring, etc.
[0079] Among the formulae (Ar-1) to (Ar-22), the formulae (Ar-6) and (Ar-7) are preferred from the viewpoint of molecular stability. Among them, the divalent aromatic group represented by the following formula (1-1-A) is more preferred.
[0080] [ka] [In the formula, Q 1 , Y 1 , Z 1 and Z 2 has the same meaning as above.
[0081] Ar a Examples of the aromatic group represented by the formula include a group represented by the following formula (Ar-23). [ka]
[0082] In formula (Ar-23), *, Z 1 , Z 2 , Q 1 and Q 2 has the same meaning as above, and U 1represents a nonmetallic atom of Groups 14 to 16 which may have a substituent bonded thereto. Examples of nonmetallic atoms of Groups 14 to 16 include carbon atoms, nitrogen atoms, oxygen atoms, and sulfur atoms, and preferred examples include =O, =S, =NR', and =C(R')R'. Examples of the substituent R' include a hydrogen atom, a halogen atom, an alkyl group, a halogenated alkyl group, an alkenyl group, an aryl group, a cyano group, an amino group, a nitro group, a nitroso group, a carboxy group, an alkylsulfinyl group having 1 to 6 carbon atoms, an alkylsulfonyl group having 1 to 6 carbon atoms, a fluoroalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkylsulfanyl group having 1 to 6 carbon atoms, an N-alkylamino group having 1 to 6 carbon atoms, an N,N-dialkylamino group having 2 to 12 carbon atoms, an N-alkylsulfamoyl group having 1 to 6 carbon atoms, and a dialkylsulfamoyl group having 2 to 12 carbon atoms. When the non-metallic atom is a carbon atom (C), the two R' may be the same or different.
[0083] In the present invention, examples of the polymerizable liquid crystal compound (1) include compounds described in JP-A-2019-003177 and the like.
[0084] In the polymerizable liquid crystal compound (1), the polymer in the oriented state of the polymerizable liquid crystal compound exhibits reverse wavelength dispersion, and when the polymerizable liquid crystal compound is alone oriented, it has a wavelength dispersion of 500 mJ / cm 2 The retardation value [R(A,500,450)] at a wavelength of 450 nm measured after irradiation with ultraviolet light of 3000 mJ / cm 2 A polymerizable liquid crystal compound (A) in which the retardation value [R(A,3000,450)] (hereinafter also referred to as "ΔRe(450)") at a wavelength of 450 nm changes in the positive direction when measured after irradiation with ultraviolet light of 500 mJ / cm. A polymer in the aligned state of the polymerizable liquid crystal compound exhibits reverse wavelength dispersion, and the polymerizable liquid crystal compound is oriented alone. 2 The retardation value [R(A,500,450)] at a wavelength of 450 nm measured after irradiation with ultraviolet light of 3000 mJ / cm2 The liquid crystal composition contains a polymerizable liquid crystal compound (B) whose retardation value [R(A, 3000, 450)] at a wavelength of 450 nm measured after irradiation with ultraviolet light of 100 nm changes in the negative direction.
[0085] In this specification, the term "change in retardation value in the positive direction" means that the retardation value is changed by 500 mJ / cm when the target polymerizable liquid crystal compound is aligned alone. 2 The retardation value [R(A,500,450)] at a wavelength of 450 nm measured after irradiation with ultraviolet light of 3000 mJ / cm 2 This means that the retardation value [R(A,3000,450)] at a wavelength of 450 nm measured after irradiation with ultraviolet light of 100 nm becomes larger. On the other hand, the retardation value "changes in the negative direction" means that the retardation value [R(A,3000,450)] becomes smaller than the retardation value [R(A,500,450)]. In this specification, when the change in ΔRe(450) is 1.5 nm or less, preferably 1 nm or less, more preferably 0.5 nm or less in absolute value, the polymerizable liquid crystal compound is considered to be a compound having a property that the retardation value does not change under the above-mentioned specific ultraviolet irradiation conditions.
[0086] In the present invention, the retardation value [R(A,500,450)] of the polymerizable liquid crystal compound is determined by applying a solution containing a polymerizable liquid crystal compound to which a predetermined amount of a polymerization initiator and a solvent has been added onto an alignment film, and then irradiating the liquid crystal compound with ultraviolet light having a wavelength of 365 nm with an integrated light intensity of 500 mJ / cm at a wavelength of 365 nm. 2 The retardation value of the polymerizable liquid crystal compound [R(A,3000,450)] is a value obtained by measuring the in-plane retardation value of the cured liquid crystal layer obtained by irradiating the cured liquid crystal layer with the light having a wavelength of 450 nm so that the retardation value [R(A,500,450)] is 2500 mJ / cm 2 by further irradiating the cured liquid crystal layer with the ultraviolet light having a wavelength of 365 nm so that the accumulated light amount at the wavelength of 365 nm is 2500 mJ / cm 2 . 2 (That is, the cumulative amount of light at the time of irradiation at a wavelength of 365 nm is 3000 mJ / cm, including the ultraviolet light irradiated during the preparation of the liquid crystal cured layer. 2The retardation value is a value obtained by measuring the inner surface retardation value of the cured liquid crystal layer with respect to light having a wavelength of 450 nm after irradiation so as to obtain a retardation value of 450 nm.
[0087] Polymerizable liquid crystal compounds, particularly polymerizable liquid crystal compounds that exhibit reverse wavelength dispersion and have a maximum absorption in the ultraviolet region of 250 to 400 nm, may have their optical properties changed by irradiation with ultraviolet light. Whether ΔRe(450) changes in the positive or negative direction when the polymerizable liquid crystal compound is irradiated with ultraviolet light under the above-mentioned specific conditions is usually determined by the molecular structure of the polymerizable liquid crystal compound. In particular, in the polymerizable liquid crystal compound represented by the above formula (1), Ar a It is believed that this is determined by the molecular structure of the material.
[0088] Although not necessarily limited, Ar a When the aromatic group represented by the formula (1) is composed of a nitrogen atom, a sulfur atom, an oxygen atom, a carbon atom, and a hydrogen atom, the retardation value under the above ultraviolet irradiation conditions tends to change in the positive direction. a In the case where the aromatic group represented by the formula (1-1-A) is a divalent aromatic group composed of a nitrogen atom, a sulfur atom, an oxygen atom, a carbon atom and a hydrogen atom, the polymerizable liquid crystal compound is often a compound in which the retardation value changes in the positive direction under the above ultraviolet irradiation conditions. More specifically, the polymerizable liquid crystal compound (A) in which the retardation value changes in the positive direction under the above ultraviolet irradiation conditions is, for example, 1 is -S- and Y 1 is an aromatic group having a polycyclic aromatic heterocycle having an alkenyl structure. When the compound has an alkenyl structure, it undergoes photooxidation, and the alkenyl moiety tends to be oxidized, increasing the retardation value (changing in the positive direction).
[0089] On the other hand, although not necessarily limited, Ar a When the aromatic group represented by the formula (1) is composed of a nitrogen atom, a sulfur atom, a carbon atom, and a hydrogen atom, the retardation value under the above ultraviolet irradiation conditions tends to change in the negative direction.a When the aromatic group represented by the formula (1-1-A) is a divalent aromatic group composed of a nitrogen atom, a sulfur atom, a carbon atom and a hydrogen atom, the polymerizable liquid crystal compound is often a compound whose retardation value changes in the negative direction under the above-mentioned ultraviolet irradiation conditions. More specifically, the polymerizable liquid crystal compound (B) whose retardation value changes in the negative direction under the above-mentioned ultraviolet irradiation conditions is, for example, 1 is -S- and Y 1 is an aromatic group having a polycyclic aromatic heterocycle not having an alkenyl structure, and Y 1 is an aromatic group having no alkenyl structure and having a polycyclic aromatic heterocycle containing two heteroatoms, in particular Y 1 does not have an alkenyl structure, is a condensed ring of a five-membered ring and a six-membered ring, and has a polycyclic aromatic heterocycle containing two heteroatoms in the five-membered ring portion.
[0090] When the polymerizable liquid crystal composition contains a polymerizable liquid crystal compound whose ΔRe(450) changes in the positive direction upon ultraviolet irradiation and a polymerizable liquid crystal compound whose ΔRe(450) changes in the negative direction, the changes in the optical properties of the individual polymerizable liquid crystal compounds upon ultraviolet irradiation are offset, and the change in the optical properties of the polymerizable liquid crystal composition upon ultraviolet irradiation can be suppressed. However, in the optical film of the present invention, the gas barrier layer disposed adjacent to the retardation layer can suppress the generation of peroxide radicals caused by exposure to light in the presence of oxygen. Therefore, even when the optical film contains only one of the polymerizable liquid crystal compound (A) whose ΔRe(450) changes in the positive direction and the polymerizable liquid crystal compound (B) whose ΔRe(450) changes in the negative direction, the change in the retardation value in the retardation layer can be suppressed, and an optical laminate with excellent durability can be provided.
[0091] In the present invention, the polymerizable liquid crystal composition forming the retardation layer may be a polymerizable liquid crystal compound, which may be used alone or in combination. Examples of the polymerizable compound other than the polymerizable liquid crystal compound (1) include polymerizable liquid crystal compounds that do not have light absorption in the ultraviolet region and do not change retardation value under the above ultraviolet irradiation conditions. Although not necessarily limited, specific examples thereof include many polymerizable liquid crystal compounds that show positive wavelength dispersion, and for example, compounds having a polymerizable group among the compounds described in "3.8.6 Network (completely cross-linked type)" and "6.5.1 Liquid crystal material b. Polymerizable nematic liquid crystal material" in Liquid Crystal Handbook (edited by Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 2000) can be used. In addition, commercially available products may be used as these polymerizable liquid crystal compounds.
[0092] In the present invention, the polymerizable liquid crystal composition forming the retardation layer preferably contains a polymerizable liquid crystal compound (1). The content thereof is preferably 60 parts by mass or more, more preferably 70 parts by mass or more, and even more preferably 80 parts by mass or more, based on 100 parts by mass of the total amount of the polymerizable liquid crystal compounds contained in the polymerizable liquid crystal composition. All of the polymerizable liquid crystal compounds contained in the polymerizable liquid crystal composition may be the polymerizable liquid crystal compound (1).
[0093] The content of the polymerizable liquid crystal compound in the polymerizable liquid crystal composition is, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, more preferably 85 to 98 parts by mass, and even more preferably 90 to 95 parts by mass, based on 100 parts by mass of the solid content of the polymerizable liquid crystal composition. If the content of the polymerizable liquid crystal compound is within the above range, it is advantageous in terms of the alignment of the obtained retardation-exhibiting layer. In this specification, the solid content of the polymerizable liquid crystal composition means all components excluding volatile components such as organic solvents from the polymerizable liquid crystal composition.
[0094] In the present invention, the polymerizable liquid crystal composition forming the retardation layer preferably contains a polymerization initiator. The polymerization initiator is a compound that generates reactive species by the contribution of heat or light and can initiate a polymerization reaction of the polymerizable liquid crystal or the like. Examples of the reactive species include active species such as radicals, cations, and anions. Among them, a photopolymerization initiator that generates radicals by light irradiation is preferred from the viewpoint of easy reaction control.
[0095] Examples of photopolymerization initiators include benzoin compounds, benzophenone compounds, benzyl ketal compounds, α-hydroxyketone compounds, α-aminoketone compounds, triazine compounds, iodonium salts, and sulfonium salts.Specific examples include Irgacure (registered trademark) 907, Irgacure 184, Irgacure 651, Irgacure 819, Irgacure 250, Irgacure 369, Irgacure 379, Irgacure 127, Irgacure 2959, Irgacure 754, Irgacure 379EG (all manufactured by BASF Japan Ltd.), Seikuol BZ, Seikuol Z, Seikuol BEE (all manufactured by Seiko Chemical Co., Ltd.), Kayacure (registered trademark) Examples of suitable antibacterial agents include ADEKA CURE BP100 (manufactured by Nippon Kayaku Co., Ltd.), Kayacure UVI-6992 (manufactured by Dow), ADEKA OPTOMER SP-152, ADEKA OPTOMER SP-170, ADEKA OPTOMER N-1717, ADEKA OPTOMER N-1919, ADEKA ARCLES NCI-831, ADEKA ARCLES NCI-930 (all manufactured by ADEKA Corporation), TAZ-A, TAZ-PP (all manufactured by Nippon SiberHegner AG) and TAZ-104 (manufactured by Sanwa Chemical Co., Ltd.). In the present invention, the polymerizable liquid crystal composition preferably contains at least one type of photopolymerization initiator, and more preferably contains one or two types of photopolymerization initiators.
[0096] The photopolymerization initiator can fully utilize the energy emitted from the light source and has excellent productivity, so that the maximum absorption wavelength is preferably 300 nm to 400 nm, and more preferably 300 nm to 380 nm, and among them, an α-acetophenone-based polymerization initiator or an oxime-based photopolymerization initiator is preferable.
[0097] Examples of α-acetophenone compounds include 2-methyl-2-morpholino-1-(4-methylsulfanylphenyl)propan-1-one, 2-dimethylamino-1-(4-morpholinophenyl)-2-benzylbutan-1-one, and 2-dimethylamino-1-(4-morpholinophenyl)-2-(4-methylphenylmethyl)butan-1-one, and more preferably 2-methyl-2-morpholino-1-(4-methylsulfanylphenyl)propan-1-one and 2-dimethylamino-1-(4-morpholinophenyl)-2-benzylbutan-1-one. Examples of commercially available α-acetophenone compounds include Irgacure 369, 379EG, and 907 (all manufactured by BASF Japan Co., Ltd.) and Seikuol BEE (manufactured by Seiko Chemical Co., Ltd.).
[0098] The oxime-based photopolymerization initiator generates methyl radicals by irradiation with light. The methyl radicals allow the polymerization of the polymerizable liquid crystal compound to proceed favorably in the deep part of the liquid crystal cured layer (retardation layer) to be formed. In addition, from the viewpoint of more efficiently proceeding the polymerization reaction in the deep part of the liquid crystal cured layer to be formed, it is preferable to use a photopolymerization initiator that can efficiently utilize ultraviolet light with a wavelength of 350 nm or more. As photopolymerization initiators that can efficiently utilize ultraviolet light with a wavelength of 350 nm or more, triazine compounds and oxime ester type carbazole compounds are preferable, and from the viewpoint of sensitivity, oxime ester type carbazole compounds are more preferable. Examples of oxime ester type carbazole compounds include 1,2-octanedione, 1-[4-(phenylthio)-2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime), and the like. Commercially available oxime ester carbazole compounds include Irgacure OXE-01, Irgacure OXE-02, Irgacure OXE-03 (all manufactured by BASF Japan Ltd.), ADEKA Optomer N-1919, ADEKA Arcles NCI-831 (all manufactured by ADEKA Corporation), and the like.
[0099] The amount of the photopolymerization initiator added is usually 0.1 to 30 parts by mass, preferably 1 to 20 parts by mass, and more preferably 1 to 15 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. Within the above range, the reaction of the polymerizable group proceeds sufficiently, and the alignment of the polymerizable liquid crystal compound is unlikely to be disturbed.
[0100] By blending a polymerization inhibitor, the polymerization reaction of the polymerizable liquid crystal compound can be controlled. Examples of the polymerization inhibitor include hydroquinones having a substituent such as hydroquinone and alkyl ether; catechols having a substituent such as alkyl ether, such as butylcatechol; radical scavengers such as pyrogallols and 2,2,6,6-tetramethyl-1-piperidinyloxy radical; thiophenols; β-naphthylamines and β-naphthols. The content of the polymerization inhibitor is usually 0.01 to 10 parts by mass, preferably 0.1 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound in order to polymerize the polymerizable liquid crystal compound without disturbing the orientation of the polymerizable liquid crystal compound.
[0101] Furthermore, the photopolymerization initiator can be made highly sensitive by using a sensitizer. Examples of the photosensitizer include xanthones such as xanthone and thioxanthone; anthracenes having anthracene and alkyl ether as a substituent; phenothiazine; and rubrene. Examples of the photosensitizer include xanthones such as xanthone and thioxanthone; anthracenes having anthracene and alkyl ether as a substituent; phenothiazine; and rubrene. The content of the photosensitizer is usually 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound.
[0102] Furthermore, the polymerizable liquid crystal composition may contain a leveling agent. The leveling agent is an additive that has the function of adjusting the fluidity of the polymerizable liquid crystal composition and making the film obtained by applying the composition flatter, and examples of the leveling agent include silicone-based, polyacrylate-based and perfluoroalkyl-based leveling agents. Specifically, DC3PA, SH7PA, DC11PA, SH28PA, SH29PA, SH30PA, ST80PA, ST86PA, SH8400, SH8700, FZ2123 (all manufactured by Dow Corning Toray Co., Ltd.), KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, KF6001 (all manufactured by Shin-Etsu Chemical Co., Ltd.), TSF400, TSF401, TSF410, TSF4300, TSF4440, TSF4445, TSF-4446, TSF4452, TSF4460 (all manufactured by Momentive Performance Materials Co., Ltd.) Japan LLC), Fluorinert (registered trademark) FC-72, FC-40, FC-43, FC-3283 (all manufactured by Sumitomo 3M Limited), Megafac (registered trademark) R-08, R-30, R-90, F-410, F-411, F-443, F-445, F-470, F-477, F-479, F-482, F-483 (all manufactured by DIC Corporation), F-top (trade name) EF301, EF303, EF351, EF352 (all manufactured by Mitsubishi Materials Electronics Co., Ltd.), Surflon (registered trademark) S-381, S-382, S-383, S-393, SC-101, SC-105, KH-40, SA-100 (all manufactured by AGC Seimi Chemical Co., Ltd.), trade names E1830, E5844 (manufactured by Daikin Fine Chemical Research Institute Co., Ltd.), BM-1000, BM-1100, BYK-352, BYK-353 and BYK-361N (all trade names: manufactured by BM Chemie Co., Ltd.), etc. Among them, polyacrylate-based leveling agents and perfluoroalkyl-based leveling agents are preferred.
[0103] The content of the leveling agent in the polymerizable liquid crystal composition is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, based on 100 parts by mass of the polymerizable liquid crystal compound. When the content of the leveling agent is within the above range, the polymerizable liquid crystal compound is easily aligned horizontally, and the obtained retardation-exhibiting layer tends to be smoother, which is preferable. The polymerizable liquid crystal composition may contain two or more types of leveling agents.
[0104] In one embodiment of the present invention, the retardation-exhibiting layer has optical properties represented by the following formulas (I), (II) and (III). The retardation-exhibiting layer is usually a cured product obtained by curing a polymerizable liquid crystal compound in a state where the polymerizable liquid crystal compound is aligned in the horizontal direction relative to the plane of the retardation-exhibiting layer. Re(450) / Re(550)≦1.00 (I) 1.00≦Re(650) / Re(550) (II) 100nm≦Re(550)≦180nm (III) (In the formula, Re(λ) represents an in-plane retardation value of the retardation layer at a wavelength of λ nm, and Re=(nx(λ)-ny(λ))×d (d represents the thickness of the retardation layer, nx represents the principal refractive index at a wavelength of λ nm in a direction parallel to the plane of the retardation layer in the index ellipsoid formed by the retardation layer, and ny represents the refractive index at a wavelength of λ nm in a direction parallel to the plane of the retardation layer and perpendicular to the direction of nx in the index ellipsoid formed by the retardation layer).)
[0105] When the retardation layer satisfies the formulas (I) and (II), the retardation layer exhibits the so-called reverse wavelength dispersion, in which the in-plane retardation value at a short wavelength is smaller than the in-plane retardation value at a long wavelength. Since the reverse wavelength dispersion is improved and the optical properties of the retardation layer are further improved, Re(450) / Re(550) is preferably 0.70 or more, more preferably 0.78 or more, and also preferably 0.92 or less, more preferably 0.90 or less, even more preferably 0.88 or less, particularly preferably 0.87 or less, and even more particularly preferably 0.86 or less. In addition, Re(650) / Re(550) is preferably 1.0 or more, more preferably 1.01 or more, and even more preferably 1.02 or more.
[0106] The in-plane retardation value can be adjusted by the thickness d of the retardation-exhibiting layer. Since the in-plane retardation value is determined by the above formula Re(λ)=(nx(λ)-ny(λ))×d, a desired in-plane retardation value (Re(λ): in-plane retardation value of the retardation-exhibiting layer at wavelength λ(nm)) can be obtained by adjusting the three-dimensional refractive index and the film thickness d.
[0107] In addition, when the retardation layer satisfies formula (III), when an optical laminate (elliptically polarizing plate) including the retardation layer is applied to an organic EL display device, the effect of improving the front reflection hue (the effect of suppressing coloration) is excellent. A more preferable range of the in-plane retardation value is 120 nm≦Re(550)≦170 nm, and an even more preferable range is 130 nm≦Re(550)≦150 nm.
[0108] In the present invention, the retardation layer is, for example, forming a coating film of a polymerizable liquid crystal composition on a supporting substrate or an alignment film, drying the coating film, and aligning a polymerizable liquid crystal compound in the polymerizable liquid crystal composition; and A process of polymerizing the polymerizable liquid crystal compound while maintaining the alignment state, and forming a retardation layer which is a liquid crystal cured layer. The composition can be produced by a method comprising the steps of:
[0109] A coating film of the polymerizable liquid crystal composition can be formed by applying the polymerizable liquid crystal composition onto a supporting substrate or onto an alignment film described below. The viscosity of the polymerizable liquid crystal composition is preferably adjusted to, for example, 10 mPa·s or less, preferably about 0.1 to 7 mPa·s, so as to facilitate application. The viscosity of the polymerizable liquid crystal composition can be adjusted by the content of the solvent.
[0110] The solvent is preferably one capable of dissolving the polymerizable liquid crystal compound, and is preferably one that is inactive in the polymerization reaction of the polymerizable liquid crystal compound. Examples of the solvent include alcohol solvents such as water, methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorine-containing solvents such as chloroform and chlorobenzene; and amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone. These solvents may be used alone or in combination of two or more. Among these, alcohol solvents, ester solvents, ketone solvents, chlorine-containing solvents, amide solvents and aromatic hydrocarbon solvents are preferred.
[0111] The content of the solvent in 100 parts by mass of the polymerizable liquid crystal composition is preferably 50 to 98 parts by mass, more preferably 70 to 95 parts by mass. Therefore, the solid content concentration in the polymerizable liquid crystal composition is preferably 2 to 50% by mass, more preferably 5 to 30%, and even more preferably 5 to 15%. When the solid content of the polymerizable liquid crystal composition is equal to or less than the upper limit, the viscosity of the polymerizable liquid crystal composition is low, so that the thickness of the retardation-exhibiting layer obtained by applying the composition becomes approximately uniform, and unevenness tends to be less likely to occur. In addition, when the solid content is equal to or more than the lower limit, the retardation layer does not become too thin, and the birefringence required for optical compensation of the liquid crystal panel tends to be given. The solid content can be appropriately determined in consideration of the thickness of the retardation-exhibiting layer to be manufactured.
[0112] The supporting substrate can be glass substrate and film substrate, and from the viewpoint of processability, film substrate is preferred.The resin constituting the film substrate can be, for example, polyolefin such as polyethylene, polypropylene, norbornene polymer, cyclic olefin resin, polyvinyl alcohol, polyethylene terephthalate, polymethacrylic acid ester, polyacrylic acid ester, cellulose ester such as triacetyl cellulose, diacetyl cellulose and cellulose acetate propionate, polyethylene naphthalate, polycarbonate, polysulfone, polyether sulfone, polyether ketone, polyphenylene sulfide and polyphenylene oxide, and other plastics.
[0113] Commercially available products may be used as the support substrate. Examples of commercially available cellulose ester substrates include "FUJITAC FILM" (manufactured by Fuji Photo Film Co., Ltd.), "KC8UX2M", "KC8UY" and "KC4UY" (all manufactured by Konica Minolta Opto, Inc.). Examples of commercially available cyclic olefin resins include "Topas" (registered trademark) (manufactured by Ticona, Germany), "Arton" (registered trademark) (manufactured by JSR Corporation), "ZEONOR" (registered trademark), "ZEONEX" (registered trademark) (all manufactured by Zeon Corporation), and "Apel" (registered trademark) (manufactured by Mitsui Chemicals, Inc.). Such cyclic olefin resins can be formed into a film by known means such as a solvent casting method or a melt extrusion method to form a substrate. Commercially available cyclic olefin resin substrates can also be used. Examples of commercially available cyclic olefin resin substrates include "S-Cina" (registered trademark), "SCA40" (registered trademark) (all manufactured by Sekisui Chemical Co., Ltd.), "ZEONOR Film" (registered trademark) (manufactured by Optes Co., Ltd.), and "Arton Film" (registered trademark) (manufactured by JSR Corporation).
[0114] The thickness of the substrate is preferably thin in terms of the mass that can be practically handled, but if it is too thin, the strength decreases and the processability tends to be poor. The thickness of the substrate is usually 5 μm to 300 μm, preferably 20 μm to 200 μm. In addition, by peeling off the substrate and transferring only the retardation layer, a further thinning effect can be obtained.
[0115] Examples of a method for applying the polymerizable liquid crystal composition to a substrate or the like include known methods such as application methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography.
[0116] Next, the solvent is removed by drying or the like to form a dried coating film. Examples of drying methods include natural drying, ventilation drying, heat drying, and reduced pressure drying. In this case, by heating the coating film obtained from the polymerizable liquid crystal composition, the solvent can be dried and removed from the coating film, and the polymerizable liquid crystal compound can be aligned in a desired direction (for example, horizontal direction) relative to the coating film plane. The heating temperature of the coating film can be appropriately determined in consideration of the materials of the polymerizable liquid crystal compound used and the substrate on which the coating film is formed, but in order to phase-transition the polymerizable liquid crystal compound to a liquid crystal phase state, it is usually necessary that the temperature is equal to or higher than the liquid crystal phase transition temperature. In order to make the polymerizable liquid crystal compound have a desired alignment state while removing the solvent contained in the polymerizable liquid crystal composition, the composition can be heated to a temperature equal to or higher than the liquid crystal phase transition temperature (smectic phase transition temperature or nematic phase transition temperature) of the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition. The liquid crystal phase transition temperature can be measured using, for example, a polarizing microscope equipped with a temperature control stage, a differential scanning calorimeter (DSC), a thermogravimetric differential thermal analyzer (TG-DTA), etc. When two or more polymerizable liquid crystal compounds are used in combination, the phase transition temperature means a temperature measured in the same manner as when one type of polymerizable liquid crystal compound is used, using a mixture of polymerizable liquid crystal compounds in which all polymerizable liquid crystal compounds constituting the polymerizable liquid crystal composition are mixed in the same ratio as the composition in the polymerizable liquid crystal composition. It is also known that the liquid crystal phase transition temperature of a polymerizable liquid crystal compound in a polymerizable liquid crystal composition may be generally lower than the liquid crystal phase transition temperature of the polymerizable liquid crystal compound alone.
[0117] The heating time can be appropriately determined depending on the heating temperature, the type of polymerizable liquid crystal compound used, the type and boiling point of the solvent, and the amount thereof, but is usually 15 seconds to 10 minutes, and preferably 0.5 to 5 minutes.
[0118] The removal of the solvent from the coating film may be performed simultaneously with or separately from the heating of the polymerizable liquid crystal compound to a temperature equal to or higher than the liquid crystal phase transition temperature, but is preferably performed simultaneously from the viewpoint of improving productivity. Before heating the polymerizable liquid crystal compound to a temperature equal to or higher than the liquid crystal phase transition temperature, a preliminary drying step may be provided to adequately remove the solvent in the coating film obtained from the polymerizable liquid crystal composition under conditions in which the polymerizable liquid crystal compound contained in the coating film is not polymerized. Examples of the drying method in the preliminary drying step include natural drying, ventilation drying, heat drying, and reduced pressure drying, and the drying temperature (heating temperature) in the drying step can be appropriately determined depending on the type of polymerizable liquid crystal compound used, the type of solvent, its boiling point, and its amount, etc.
[0119] Next, in the obtained dried coating film, the polymerizable liquid crystal compound is polymerized while maintaining the orientation state of the polymerizable liquid crystal compound, thereby forming a retardation-exhibiting layer that is a polymer of the polymerizable liquid crystal compound that exists in a desired orientation state. As a polymerization method, a photopolymerization method is usually used. In photopolymerization, the light to be irradiated to the dried coating film is appropriately selected according to the type of photopolymerization initiator contained in the dried coating film, the type of polymerizable liquid crystal compound (particularly, the type of polymerizable group possessed by the polymerizable liquid crystal compound) and the amount thereof. Specific examples thereof include one or more types of light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α-rays, β-rays and γ-rays, and active electron beams. Among them, ultraviolet light is preferred in terms of ease of controlling the progress of the polymerization reaction and the fact that photopolymerization devices widely used in this field can be used, and it is preferable to select the types of polymerizable liquid crystal compound and photopolymerization initiator contained in the polymerizable liquid crystal composition so that they can be photopolymerized by ultraviolet light.
[0120] In addition, during polymerization, the polymerization temperature can be controlled by irradiating light while cooling the dried coating film with an appropriate cooling means. By adopting such a cooling means, the polymerization of the polymerizable liquid crystal compound can be carried out at a lower temperature, and even if a substrate having a relatively low heat resistance is used, a retardation-exhibiting layer can be appropriately formed. In addition, it is also possible to promote the polymerization reaction by increasing the polymerization temperature within a range in which no problems due to heat during light irradiation (such as deformation of the substrate due to heat) occur. During photopolymerization, a patterned cured film can also be obtained by performing masking or development.
[0121] Examples of the light source of the active energy rays include the same as those exemplified above as the light source of the active energy rays that can be used when curing the curable composition for forming a gas barrier layer. The ultraviolet irradiation intensity is usually 10 to 3,000 mW / cm. 2 The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a photopolymerization initiator. The time for light irradiation is usually 0.1 seconds to 10 minutes, preferably 0.1 seconds to 5 minutes, more preferably 0.1 seconds to 3 minutes, and further preferably 0.1 seconds to 1 minute. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 to 3,000 mJ / cm. 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 It is.
[0122] The thickness of the retardation-exhibiting layer can be appropriately selected depending on the use of the optical laminate, the display device to which it is applied, etc., and is preferably 0.1 to 10 μm, more preferably 0.2 to 5 μm, and further preferably 0.2 to 3 μm.
[0123] The coating film of the polymerizable liquid crystal composition may be formed on an alignment film. The alignment film has an alignment regulating force that aligns the polymerizable liquid crystal compound in a desired direction. For example, when preparing a retardation-expressing layer that satisfies the above formulas (I) to (III) from the polymerizable liquid crystal composition, it is preferable to use a horizontal alignment film that has an alignment regulating force that aligns the polymerizable liquid crystal compound in the horizontal direction. The alignment regulating force can be arbitrarily adjusted by the type of alignment film, the surface state, the rubbing conditions, etc., and when the alignment film is formed from a photoalignable polymer, it can be arbitrarily adjusted by the polarized light irradiation conditions, etc.
[0124] The alignment film is preferably one that has solvent resistance that does not dissolve the polymerizable liquid crystal composition when applied, and also has heat resistance in a heat treatment for removing the solvent or for orienting the polymerizable liquid crystal compound. Examples of the alignment film include an alignment film containing an alignment polymer, a photoalignment film, a groove alignment film having a concave-convex pattern or a plurality of grooves on the surface, and a stretched film stretched in the alignment direction, and the like, and a photoalignment film is preferred from the viewpoint of the accuracy of the alignment angle and the quality.
[0125] Examples of the oriented polymer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and polyamic acids, which are hydrolyzates thereof, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among them, polyvinyl alcohol is preferred. The oriented polymers can be used alone or in combination of two or more kinds.
[0126] An alignment film containing an alignment polymer is usually obtained by applying a composition in which an alignment polymer is dissolved in a solvent (hereinafter, sometimes referred to as an "alignment polymer composition") to a substrate and removing the solvent, or by applying an alignment polymer composition to a substrate, removing the solvent, and rubbing (rubbing method). Examples of the solvent include the same solvents as those exemplified above as solvents that can be used in the polymerizable liquid crystal composition.
[0127] The concentration of the oriented polymer in the oriented polymer composition may be within a range in which the oriented polymer material can be completely dissolved in the solvent, and is preferably 0.1 to 20% in terms of solid content relative to the solution, and more preferably about 0.1 to 10%.
[0128] As the oriented polymer composition, a commercially available alignment film material may be used as it is. Examples of commercially available alignment film materials include Sunever (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark, manufactured by JSR Corporation).
[0129] The method for applying the alignable polymer composition to the substrate may be the same as the method exemplified for applying the polymerizable liquid crystal composition to the supporting substrate.
[0130] Methods for removing the solvent contained in the orientable polymer composition include natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0131] In order to impart an orientation control force to the orientation film, a rubbing treatment can be performed as necessary (rubbing method). A method for imparting an orientation control force by the rubbing method includes a method in which an orientation polymer composition is applied to a substrate and annealed to bring an orientation polymer film formed on the substrate surface into contact with a rotating rubbing roll wrapped with a rubbing cloth. If masking is performed during the rubbing treatment, multiple regions (patterns) with different orientation directions can also be formed on the orientation film.
[0132] A photo-alignment film is usually obtained by applying a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter also referred to as a "photo-alignment film forming composition") to a substrate, removing the solvent, and then irradiating the substrate with polarized light (preferably polarized UV). Photo-alignment films are also advantageous in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the irradiated polarized light.
[0133] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it includes groups involved in photoreactions that induce molecular alignment or are the origin of liquid crystal alignment ability, such as isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction, caused by irradiation with light. Among them, groups involved in dimerization reaction or photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group, a group having an unsaturated bond, particularly a double bond, is preferred, and a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) is particularly preferred.
[0134] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazole groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having an azoxybenzene structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have substituents such as alkyl groups, alkoxy groups, aryl groups, allyloxy groups, cyano groups, alkoxycarbonyl groups, hydroxyl groups, sulfonic acid groups, and halogenated alkyl groups.
[0135] Among them, photoreactive groups involved in photodimerization are preferred, and cinnamoyl and chalcone groups are preferred because the amount of polarized light irradiation required for photoalignment is relatively small and a photoalignment film having excellent thermal stability and stability over time is easily obtained. As the polymer having a photoreactive group, one having a cinnamoyl group such that the terminal of the polymer side chain has a cinnamic acid structure is particularly preferred.
[0136] A photo-alignment layer can be formed on a substrate by applying the composition for forming a photo-alignment film on the substrate. The solvent contained in the composition can be the same as the solvents exemplified above as the solvents usable for the polymerizable liquid crystal composition, and can be appropriately selected depending on the solubility of the polymer or monomer having a photoreactive group.
[0137] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately adjusted depending on the type of polymer or monomer and the thickness of the intended photo-alignment film, but is preferably at least 0.2% by mass, more preferably in the range of 0.3 to 10% by mass, based on the mass of the composition for forming a photo-alignment film. The composition for forming a photo-alignment film may contain a polymer material such as polyvinyl alcohol or polyimide, or a photosensitizer, within a range that does not significantly impair the properties of the photo-alignment film.
[0138] The method of applying the composition for forming a photo-alignment film to a substrate may be the same as the method of applying the oriented polymer composition to a substrate. Examples of the method of removing the solvent from the applied composition for forming a photo-alignment film include natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0139] The polarized light may be irradiated by directly irradiating the polarized UV light onto the composition for forming a photo-aligned film coated on the substrate after removing the solvent, or by irradiating the polarized light from the substrate side and transmitting the polarized light. In addition, it is particularly preferable that the polarized light is substantially parallel light. The wavelength of the polarized light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength of 250 to 400 nm is particularly preferable. Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferable. Among these, high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are preferable because they have a high emission intensity of ultraviolet light with a wavelength of 313 nm. The light from the light source can be irradiated by passing through an appropriate polarizer to irradiate the polarized UV light. As such a polarizer, a polarizing filter, a polarizing prism such as a Glan-Thompson or Glan-Taylor type polarizer, or a wire grid type polarizer can be used.
[0140] If masking is performed during rubbing or polarized light irradiation, a plurality of regions (patterns) in which the liquid crystal alignment directions are different can be formed.
[0141] A groove alignment film is a film that has a concave-convex pattern or multiple grooves on the film surface. When a polymerizable liquid crystal compound is applied to a film with multiple equally spaced linear grooves, the liquid crystal molecules are aligned in the direction along the grooves.
[0142] Methods for obtaining a groove alignment film include a method in which the surface of a photosensitive polyimide film is exposed to light through an exposure mask having slits in a pattern shape, followed by development and rinsing to form an uneven pattern; a method in which a layer of uncured UV-curable resin is formed on a plate-shaped master having grooves on its surface, the formed resin layer is transferred to a substrate and then cured; and a method in which a roll-shaped master having multiple grooves is pressed against an uncured UV-curable resin film formed on a substrate to form unevenness, followed by curing.
[0143] The thickness of the alignment film (alignment film containing an alignment polymer or photoalignment film) is usually in the range of 10 to 10,000 nm, preferably in the range of 10 to 1000 nm, more preferably 10 to 500 nm or less, even more preferably 10 to 300 nm, and particularly preferably 50 to 250 nm.
[0144] In this specification, the optical laminate means a laminate having various optical properties that includes an optically functional layer (for example, a layer that functions to improve the visibility of an image) and can be incorporated into an image display device such as an organic electroluminescence display device. The optical laminate of the present invention may include a retardation layer and a gas barrier layer adjacent to the retardation layer, and may be composed of only a retardation layer and a gas barrier layer, or may include other layers such as a polarizer layer in addition to the retardation layer and the gas barrier layer. The optical laminate of the present invention may also be composed of a substrate layer that can be peeled off when incorporated into an image display device or the like.
[0145] When the optical laminate of the present invention includes a polarizer layer in addition to the retardation layer and the gas barrier layer, the optical laminate can function as an elliptical polarizing plate. The polarizer layer is a layer having a polarizing function including at least a linear polarizer, and may further include a thermoplastic resin film etc. that is attached to at least one surface of the linear polarizer. A linear polarizer is an optical element that has the property of transmitting linearly polarized light having a vibration plane perpendicular to the absorption axis when unpolarized light is incident.
[0146] The linear polarizer may be, for example, an oriented polyvinyl alcohol-based resin film to which a dichroic dye such as iodine is adsorbed and oriented. The linear polarizer may be a single-layer polyvinyl alcohol-based resin film (a polyvinyl alcohol resin film in which polyvinyl alcohol molecules contained in the polyvinyl alcohol resin film are oriented) to which a dichroic dye is adsorbed and oriented, or a laminated film of two or more layers in which a polyvinyl alcohol-based resin layer to which a dichroic dye is adsorbed and oriented is provided on a substrate film.
[0147] Such a linear polarizer can be produced by a method known in the art, such as a method including a step of uniaxially stretching a polyvinyl alcohol-based resin film, a step of dyeing the polyvinyl alcohol-based resin film with a dichroic dye to adsorb the dichroic dye, a step of treating the polyvinyl alcohol-based resin film with the adsorbed dichroic dye with an aqueous boric acid solution, and a step of washing with water after the treatment with the aqueous boric acid solution.
[0148] The thickness of the linear polarizer formed by adsorbing and aligning a dichroic dye on a single-layer polyvinyl alcohol resin film is preferably 20 μm or less, more preferably 15 μm or less, and further preferably 10 μm or less.
[0149] When the polarizer layer has a structure in which a thermoplastic resin film or the like is laminated on at least one surface of a linear polarizer, the linear polarizer and the thermoplastic resin film can be attached to each other with an adhesive, etc. As the thermoplastic resin film, a film similar to the resin film exemplified as the support substrate usable for forming the retardation layer can be preferably used.
[0150] When the optical laminate of the present invention contains a polarizer layer, it is preferable that the polarizer layer and the gas barrier layer and / or the retardation layer are laminated so that the angle between the slow axis (optical axis) of the retardation-exhibiting layer and the absorption axis of the polarizer layer is 45±5°.
[0151] As shown in FIG. 4, in one embodiment of the present invention, the retardation layer 1 and the polarizer layer 7 are laminated only through the gas barrier layer 2 adjacent to the retardation layer 1. That is, in this embodiment, there is no adhesive layer between the gas barrier layer adjacent to the retardation layer and the polarizer layer for bonding them. Many adhesive layers, particularly adhesive layers, are prone to infiltrate gaseous oxygen gas and moisture, and when an adhesive layer is present near the retardation layer, oxygen gas and moisture are likely to diffuse into the retardation layer. When the retardation layer and the polarizer layer are laminated only through the gas barrier layer, the amount of oxygen gas and moisture that penetrates into the optical laminate can be reduced, and the gas barrier layer can suppress the diffusion of oxygen gas and / or moisture, so that it is expected that the optical laminate can be given higher durability.
[0152] In another embodiment of the present invention, the polarizer layer and the gas barrier layer and / or the retardation layer can be laminated via, for example, a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer for bonding the polarizer layer and the gas barrier layer and / or the retardation layer is preferably formed from a pressure-sensitive adhesive. The pressure-sensitive adhesive may be any layer that can function as a layer for bonding layers such as the gas barrier layer and the polarizer layer, and a known pressure-sensitive adhesive composition may be used.
[0153] For example, the pressure-sensitive adhesive composition may be a pressure-sensitive adhesive composition mainly composed of a resin such as a (meth)acrylic, rubber, urethane, ester, silicone, or polyvinyl ether resin. Among these, a pressure-sensitive adhesive composition having a (meth)acrylic resin as a base polymer, which is excellent in transparency, weather resistance, heat resistance, etc., is preferred.
[0154] As the (meth)acrylic resin (base polymer) used in the pressure-sensitive adhesive composition, for example, a polymer or copolymer containing one or more (meth)acrylic acid esters as monomers, such as butyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, is preferably used. It is preferable to copolymerize a polar monomer into the base polymer. Examples of the polar monomer include monomers having a carboxyl group, a hydroxyl group, an amide group, an amino group, an epoxy group, and the like, such as (meth)acrylic acid, 2-hydroxypropyl (meth)acrylate, hydroxyethyl (meth)acrylate, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, and glycidyl (meth)acrylate. Adhesives containing such copolymers are preferred because they have excellent adhesive properties and can be removed relatively easily after application to a substrate without leaving any adhesive residue on the substrate.
[0155] The adhesive composition may contain only the base polymer, but may also contain a crosslinking agent. Examples of the crosslinking agent include divalent or higher metal ions that form carboxylate metal salts with carboxyl groups, polyamine compounds that form amide bonds with carboxyl groups, polyepoxy compounds or polyols that form ester bonds with carboxyl groups, and polyisocyanate compounds that form amide bonds with carboxyl groups.
[0156] The pressure-sensitive adhesive composition may contain a solvent as necessary. Examples of the solvent include those exemplified as solvents that can be used in the polymerizable liquid crystal composition and the like.
[0157] The thickness of the adhesive layer can be appropriately determined depending on the layer structure of the optical laminate. Since the optical laminate of the present invention has a gas barrier layer adjacent to the retardation layer, even when oxygen gas or moisture penetrates into the optical laminate from the adhesive layer, the effect of suppressing the change in the retardation value in the retardation layer is excellent. Therefore, even if the thickness of the adhesive layer into which oxygen gas or moisture easily penetrates is relatively large, an optical laminate having excellent durability can be provided. Therefore, the thickness of the adhesive layer in the optical laminate of the present invention may be, for example, 1 μm or more and 100 μm or less. From the viewpoint of thinning the optical laminate, it is preferably 25 μm or less, more preferably 20 μm or less, and even more preferably 15 μm or less. When the optical laminate of the present invention contains multiple adhesive layers, it is preferable that the thickness of at least the adhesive layer provided adjacent to or close to the retardation layer and / or the gas barrier layer is within the above range, and it is more preferable that the thicknesses of all the adhesive layers included in the optical laminate of the present invention are within the above range.
[0158] In one embodiment of the present invention, the optical laminate of the present invention includes a front plate, as shown in Fig. 5. In Fig. 5, a front plate 8 is attached to a polarizer layer 7 via an adhesive layer 9. The front plate may be, for example, a thermoplastic resin film. Examples of resins constituting the thermoplastic resin film include polyolefin resins such as polyethylene and polypropylene; cyclic polyolefin resins such as norbornene polymers; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; (meth)acrylic acid resins such as poly(methyl meth)acrylate; cellulose ester resins such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; vinyl alcohol resins such as polyvinyl alcohol and polyvinyl acetate; polycarbonate resins; polystyrene resins; polyarylate resins; polysulfone resins; polyethersulfone resins; polyamide resins; polyimide resins; polyether ketone resins; polyphenylene sulfide resins; polyphenylene oxide resins; and resin films composed of mixtures, copolymers, and the like thereof. Of the above resins, it is preferable to use any one of cyclic polyolefin resins, polyester resins, cellulose ester resins, and (meth)acrylic acid resins, or mixtures thereof. The thermoplastic resin film may be a single layer made of one or a mixture of two or more of the above-mentioned resin materials, or may have a multi-layer structure of two or more layers. When the film has a multi-layer structure, the resins constituting each layer may be the same or different.
[0159] In addition to the resin material, the thermoplastic resin film may contain any additives, such as ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, coloring inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants.
[0160] The thickness of the thermoplastic resin film used as the front panel is, from the viewpoint of thinning and flexibility of the optical laminate, and from the viewpoint of durability of the optical laminate, preferably from 2 μm to 300 μm, more preferably from 5 μm to 200 μm, even more preferably from 5 μm to 100 μm, particularly preferably from 5 μm to 50 μm, and especially preferably from 5 μm to 30 μm.
[0161] The adhesive layer for bonding the front plate to the polarizer layer etc. is preferably formed from an adhesive, particularly an aqueous adhesive. Any aqueous adhesive can be used as the aqueous adhesive as long as it can function as a layer for adhering and holding the front plate to the polarizer layer etc., and a known aqueous adhesive composition can be used. For example, the water-based adhesive composition is an adhesive mainly composed of a water-soluble resin or a water-dispersible resin. Examples of the water-soluble resin or the water-dispersible resin include (meth)acrylic resins; polyvinyl alcohol resins; polyvinyl acetal resins; ethylene-vinyl alcohol copolymer resins; polyvinylpyrrolidone resins; polyamidoamine resins; epoxy resins; melamine resins; urea resins; polyamide resins; polyester resins; polyurethane resins; cellulose resins such as methyl cellulose, hydroethyl cellulose, and carboxymethyl cellulose; polysaccharides such as sodium alginate and starch. Among these, (meth)acrylic resins; hydroxyl-containing resins such as polyvinyl alcohol resins and polyvinyl acetal resins are preferred, and polyvinyl alcohol resins are more preferred.
[0162] The content of the water-soluble resin or water-dispersible resin in the aqueous adhesive composition may be appropriately determined depending on factors such as the type of resin used, but is typically 1 to 10 parts by mass, and preferably 1 to 5 parts by mass, per 100 parts by mass of water.
[0163] The thickness of the adhesive layer formed from the aqueous adhesive composition is usually 0.02 to 5 μm, preferably 0.05 to 2 μm, and more preferably 0.1 to 1 μm. If the adhesive layer formed from the dry-solidifying adhesive is too thick, the appearance is likely to be poor.
[0164] The present invention can provide a display device including the optical laminate of the present invention as one of the embodiments. In this specification, the display device is a device having a display mechanism, and includes a light-emitting element or a light-emitting device as a light source. Examples of the display device include a liquid crystal display device, an organic electroluminescence (EL) display device, an inorganic electroluminescence (EL) display device, a touch panel display device, an electron emission display device (field emission display device (FED, etc.), surface field emission display device (SED)), electronic paper (display device using electronic ink or electrophoretic element), a plasma display device, a projection type display device (a grating light valve (GLV) display device, a display device having a digital micromirror device (DMD), etc.), and a piezoelectric ceramic display. The liquid crystal display device includes any of a transmissive liquid crystal display device, a semi-transmissive liquid crystal display device, a reflective liquid crystal display device, a direct-view liquid crystal display device, and a projection type liquid crystal display device. These display devices may be display devices that display two-dimensional images, or stereoscopic display devices that display three-dimensional images. EXAMPLES
[0165] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.
[0166] 1. Preparation of optical laminate (1) Preparation of laminate 1 including polarizer layer The first laminate was prepared using the following components.
[0167] <Front plate> As the front panel, a saponified triacetyl cellulose-based resin film (Konica Minolta, Inc., "KC2UA") having a thickness of 25 μm was used.
[0168] <Release base material> As the release substrate A, a 40 μm-thick triacetyl cellulose-based resin film (manufactured by Konica Minolta, Inc., "KC4UY") that had not been subjected to a saponification treatment was used. As the release substrate B, a 25 μm-thick triacetyl cellulose-based resin film (manufactured by Konica Minolta, Inc., "KC2UA") that had not been subjected to a saponification treatment was used. As the release substrate C, a cycloolefin resin film (manufactured by Zeon Corporation, "ZF-14-50") having a thickness of 50 μm and not subjected to a corona treatment was used. As release substrate D, a cycloolefin resin film (manufactured by Zeon Corporation, "ZF-14-23") having a thickness of 23 μm and not subjected to corona treatment was used.
[0169] <Water-based adhesive layer> The following composition liquid A and composition liquid B were mixed at room temperature in a mass ratio of 1:1 and stirred for 30 minutes to prepare a water-based adhesive layer-forming composition. Composition solution A: An acetoacetyl-modified polyvinyl alcohol resin with a saponification degree of 99.2 mol% (Mitsubishi Chemical Corporation, "GOHSENOL Z200") was dissolved in water (distilled water) to prepare a PVA aqueous solution with a solid content of 8 mass%. The prepared 8 mass% PVA solution and a 40% glyoxal aqueous solution were mixed in a mass ratio of 3.0:0.7, and the total solid content was adjusted to 3 parts per 100 parts of water to prepare composition solution A. Composition solution B: An acetoacetyl-modified polyvinyl alcohol resin with a saponification degree of 99.2 mol% (Mitsubishi Chemical Corporation, "GOHSENOL Z200") was dissolved in water (distilled water) to prepare a PVA aqueous solution with a solid content of 8 mass%. The prepared 8 mass% PVA solution and zinc chloride were mixed in a mass ratio of 3.0:0.09, and the total solid content was adjusted to 3 parts per 100 parts of water to prepare composition solution B.
[0170] <Polarizer layer> As a polarizer layer, a linear polarizer (thickness: 8 μm) was prepared, which was a uniaxially stretched film obtained by adsorbing iodine to a polyvinyl alcohol-based resin film and orienting it.
[0171] Preparation of the first laminate A front plate was laminated on one surface of the polarizer layer via a composition for forming an aqueous adhesive layer, and a release substrate A was laminated on the other surface of the polarizer layer via pure water. The laminate was passed between a pair of laminating rolls and then dried at 85°C for 3 minutes to obtain a laminate 1 having a layer structure of front plate / aqueous adhesive layer / polarizer layer / release substrate A. No adhesive was interposed between the polarizer layer and release substrate A, and release substrate A was peelably laminated on the polarizer layer. By peeling release substrate A from laminate 1, a first laminate having a layer structure of front plate / aqueous adhesive layer / polarizer layer is obtained.
[0172] (2) Preparation of a laminate including a retardation layer <Retardation layer> The retardation layer is composed of the following photoalignment film and a retardation-exhibiting layer, which are formed releasably on the following retardation layer base material.
[0173] (i) Preparation of composition for forming photo-alignment film 5 parts of a photo-alignment material (weight average molecular weight: 30,000) having the following structure was mixed with 95 parts of cyclopentanone (solvent). The resulting mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a photo-alignment film.
[0174] [ka]
[0175] (ii) Preparation of Retardation Layer-Forming Composition To form a retardation layer, the following polymerizable liquid crystal compound α and polymerizable liquid crystal compound β were used. Polymerizable liquid crystal compound α was produced by the method described in JP-A-2010-31223. Polymerizable liquid crystal compound β was produced according to the method described in JP-A-2009-173893. The molecular structures of each compound are shown below. The polymerizable liquid crystal compound α is 500 mJ / cm when aligned alone. 2 The retardation value at a wavelength of 450 nm [R(A,500,450)] measured after irradiation with ultraviolet light of 3000 mJ / cm2 in a single oriented state 2The retardation value [R(A,3000,450)] at a wavelength of 450 nm measured after irradiation with ultraviolet light of 500 mJ / cm 2 at a wavelength of 550 nm changes in the positive direction. 2 The retardation value [R(A,500,550)] measured after irradiation with ultraviolet light of 3000 mJ / cm2 in a single oriented state 2 The phase difference value [R(A, 3000, 550)] measured after irradiation with ultraviolet light also changes in the positive direction. The polymerizable liquid crystal compound β is a polymerizable liquid crystal compound having a property that the retardation value does not change under the above-mentioned specific ultraviolet irradiation conditions.
[0176] [Polymerizable liquid crystal compound α] [ka] [Polymerizable liquid crystal compound β] [ka]
[0177] Polymerizable liquid crystal compound α and polymerizable liquid crystal compound β were mixed in a mass ratio of 87:13. 1.0 part of a leveling agent (manufactured by DIC Corporation, "Megafac F-556") and 6 parts of a polymerization initiator, 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (manufactured by IGM Resins BV, "Omnirad 369"), were added to 100 parts of the resulting mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration was 13%, and the mixture was stirred at 80°C for 1 hour to obtain a composition for forming a retardation layer.
[0178] (iii) Preparation of retardation layer substrate A cycloolefin resin film (ZF-14-50, manufactured by Zeon Corporation) having a thickness of 50 μm was subjected to a corona treatment to prepare a retardation layer substrate. The corona treatment was performed using TEC-4AX manufactured by Ushio Inc. The corona treatment was performed once under the conditions of an output of 0.78 kW and a treatment speed of 10 m / min.
[0179] (iv) Formation of photo-alignment film The composition for forming a photoalignment film was applied to the retardation layer base material fixed on the glass substrate using a wire bar coater (Orihara Manufacturing Co., Ltd., "G-7 type coating device") and dried for 1 minute at 80°C. The coating film was irradiated with a polarized UV irradiation device (Ushio Inc., "SPOT CURE SP-9") with an integrated light amount of 100 mJ / cm at a wavelength of 313 nm. 2 Polarized UV exposure was performed at an axial angle of 45° so that the thickness of the resulting photo-alignment film was 100 nm when measured with an optical thickness meter (manufactured by Filmetrics, Inc., "F20").
[0180] (v) Formation of phase difference layer The composition for forming a retardation layer was applied onto the photo-alignment film using a wire bar coater (Orihara Manufacturing Co., Ltd., "G-7 type coating device") and dried for 1 minute at 120° C. The coating film was irradiated with ultraviolet light (under a nitrogen atmosphere, cumulative light amount at a wavelength of 365 nm: 500 mJ / cm ) using a high-pressure mercury lamp (Ushio Inc., "Uniquer VB-15201BY-A"). 2 ) to form a retardation-exhibiting layer. Subsequently, a pressure-sensitive adhesive layer was laminated on the retardation-exhibiting layer, and a laminate having a layer structure of retardation-exhibiting layer / photoalignment film / retardation layer base material was attached to glass via the pressure-sensitive adhesive layer. As the pressure-sensitive adhesive layer, a pressure-sensitive adhesive laminate was prepared having a light release non-carrier film (hereinafter also simply referred to as "light release NCF") laminated on one side of a (meth)acrylic pressure-sensitive adhesive layer (thickness: 15 μm) and a heavy release non-carrier film (hereinafter also simply referred to as "heavy release NCF") laminated on the other side. The optical laminate including the pressure-sensitive adhesive layer is obtained by peeling off the light release NCF and transferring the exposed surface to an adhesion layer (retardation layer). Next, the retardation layer base material was peeled off to obtain a sample for measuring retardation. The retardation at a wavelength of 550 nm was measured with a retardation measuring device (manufactured by Oji Scientific Instruments, "KOBRA-WPR") and found to be 142 nm.
[0181] (3) Preparation of gas barrier layer and measurement of oxygen permeability Gas barrier layers 1 to 3 were produced as follows. (i) Preparation of the composition for forming a gas barrier layer <Gas Barrier 1 Forming Composition (Non-hydrophobic Crosslinked PVA Resin Composition)> An acetoacetyl-modified polyvinyl alcohol resin (Mitsubishi Chemical's Gohsenol Z200) with a saponification degree of 99.2 mol% was dissolved in water (distilled water) to prepare a PVA aqueous solution with a solid content of 8 mass%. The 8 mass% PVA solution prepared was mixed with 10 mass% sodium glyoxylate (Mitsubishi Chemical's "Safelink SPM-01") as a crosslinking agent in a mass ratio of 3.0:0.3, and the total solid content was adjusted to 3 parts per 100 parts of water to prepare a composition for forming gas barrier 1.
[0182] <Gas barrier 2 forming composition (hydrophobic cross-linked PVA resin composition)> An acetoacetyl-modified polyvinyl alcohol resin with a saponification degree of 99.2 mol% (Mitsubishi Chemical Corporation, "GOHSENOL Z200") was dissolved in water (distilled water) to prepare a PVA aqueous solution with a solid content of 8 mass%. The prepared 8 mass% PVA solution was mixed with a 40% aqueous solution of glyoxal as a crosslinking agent in a mass ratio of 3.0:0.7, and the total solid content was adjusted to 3 parts per 100 parts of water, to obtain a PVA resin composition A. Separately, an acetoacetyl-modified polyvinyl alcohol resin with a saponification degree of 99.2 mol% (Mitsubishi Chemical Corporation, "GOHSENOL Z200") was dissolved in water (distilled water) to prepare a PVA aqueous solution with a solid content of 8 mass%. The prepared 8 mass% PVA solution was mixed with zinc chloride in a mass ratio of 3.0:0.09, and the total solid content was adjusted to 3 parts per 100 parts of water to obtain a PVA resin composition B. The PVA resin compositions A and B prepared above were mixed at room temperature in a mass ratio of 1:1 and stirred for 30 minutes to prepare a composition for forming a gas barrier 2.
[0183] <Gas barrier 3 forming composition> As a composition for forming a gas barrier 3, a composition for forming a gas barrier 3 containing an epoxy-based polymerizable compound, a polymerization initiator, a photosensitizer, and a leveling agent, but not containing a solvent, was prepared.
[0184] (ii) Measurement method for oxygen gas permeability <Method for measuring oxygen gas permeability> The gas permeability of oxygen gas was measured using a differential pressure gas permeability measuring device (GTR-30AS, manufactured by GTR Tech Co., Ltd.) in accordance with JIS K 7126-1 (differential pressure method). The measurement conditions are as follows. In the following, unless otherwise specified, the gas permeability of oxygen gas is simply referred to as "oxygen permeability". Measurement conditions ·Measurement temperature: 30℃ ·Transmission area: 15.2cm 2 Permeation gas: Ultra-high purity oxygen gas Gas supply pressure: 2kgf / cm 2 (223cmHg) Gas permeation direction of laminate: from the coated surface to the substrate surface Gas permeation times: 0 minutes, 15 minutes and 30 minutes
[0185] <Calculation of oxygen permeability of each layer of laminate> The oxygen permeability of each layer was calculated from the oxygen permeability of the two-layer laminate using the following formula (X). (TA) -1 + (TB) -1 = (TAB) -1 (X) [In the formula, the oxygen permeability of the A layer is TA, the oxygen permeability of the B layer is TB, and the oxygen permeability of the laminate of the A layer and the B layer is TAB.]
[0186] (ii) Preparation of gas barrier layers 1 to 3 and measurement of oxygen permeability of each layer A 25 μm-thick triacetyl cellulose-based resin film (Konica Minolta, Inc.'s "KC2UA") was used as a substrate for producing the gas barrier layers 1 to 3. The oxygen permeability of the substrate was 1600 cm 3 / (m 2 ·24h·atm).
[0187] <Gas barrier layer 1> A gas barrier 1-forming composition was dropped between a saponified 25 μm-thick triacetyl cellulose-based resin film (Konica Minolta, Inc., "KC2UA") substrate and a release substrate A, and the substrate was passed through a pair of laminating rolls and then dried at 80° C. for 3 minutes to obtain a laminate having a layer structure of a 25 μm-thick triacetyl cellulose-based resin film substrate / gas barrier layer 1 / release substrate A. The release substrate A of the laminate was peeled off to obtain a laminate consisting of a 25 μm-thick triacetyl cellulose-based resin film substrate / gas barrier layer 1, and the oxygen permeability of the laminate was 100 cm 3 / (m 2 From the measured value and the value calculated by formula (X), the oxygen permeability of the gas barrier layer 1 was found to be less than 100 cm 3 / (m 2 ·24h·atm). The thickness of the gas barrier layer 1 was measured by cross-sectional length measurement using a scanning electron microscope (manufactured by JEOL Ltd., "JSM-7500F"), and was found to be 0.1 μm at the thinnest part and 0.2 μm at the thickest part.
[0188] <Gas barrier layer 2> A laminate having a layer structure of a 25 μm-thick triacetyl cellulose-based resin film substrate / gas barrier layer 2 / release substrate A was formed in the same manner as in gas barrier layer 1, except that the composition for forming gas barrier 2 was used instead of the composition for forming gas barrier 1, and the oxygen permeability was measured. The oxygen permeability of gas barrier layer 2 was 3 / (m 2The thickness of the gas barrier layer 2 was measured by cross-sectional length measurement using a scanning electron microscope (manufactured by JEOL Ltd., "JSM-7500F"), and was found to be 0.1 μm at its thinnest point and 0.2 μm at its thickest point.
[0189] <Gas Barrier 3> A composition for forming a gas barrier 3 is dropped between a corona-treated 25 μm-thick triacetyl cellulose-based resin film (Konica Minolta, Inc.'s "KC2UA") substrate and a release substrate C, and the substrate is passed between a pair of laminating rolls. The composition is then irradiated with ultraviolet light (using a deuterium lamp manufactured by Heraeus K.K.) at an integrated light dose of 400 mJ / cm. 2 The laminate was irradiated with ultraviolet light so that the ultraviolet ray concentration reached 1000 nm (UVB). As a result, a laminate having a layer structure of 25 μm-thick triacetyl cellulose-based resin film substrate / gas barrier layer 3 / releasable substrate C was obtained. The release substrate C was peeled off from the laminate, and the resulting laminate of 25 μm-thick triacetyl cellulose-based resin film substrate / gas barrier layer 3 had an oxygen permeability of 750 cm 3 / (m 2 From the measured value and the value calculated by formula (X), the oxygen permeability of the gas barrier layer 3 was 1400 cm 3 / (m 2 ·24h·atm). The thickness of the gas barrier layer 3 was measured using a scanning electron microscope ("F20" manufactured by Filmetrics Inc.) and was found to be 2.5 μm.
[0190] <Adhesive layer> A 15 μm thick acrylic adhesive layer was laminated on a 25 μm thick triacetyl cellulose resin film (Konica Minolta, Inc., "KC2UA") substrate, and the oxygen permeability of the 25 μm thick triacetyl cellulose resin film / adhesive layer laminate was measured. The oxygen permeability was 1600 cm 3 / (m 2 From the measured value and the value calculated from formula (X), the oxygen permeability of the pressure-sensitive adhesive layer was a value exceeding the upper limit of measurement.
[0191] (4) Preparation of laminates and environmental test samples of the examples and comparative examples (i) Example 1 <Preparation of second laminate> A release substrate A was laminated on the retardation layer surface of the retardation layer (structure of retardation layer substrate / photo-alignment film / retardation layer) formed on the retardation layer substrate via a gas barrier 2 forming composition, passed between a pair of laminating rolls, and dried at 80°C for 3 minutes to obtain a laminate consisting of release substrate A / gas barrier layer 2 / retardation layer / retardation layer substrate. The sample width of the retardation layer was the same as the sample width of release substrate A, and release substrate A was peelably laminated on the gas barrier layer 2. The release substrate A was peeled off from the laminate, and the adhesive layer surface of the laminate consisting of heavy release NCF / adhesive layer was closely laminated on the gas barrier layer 2 surface to obtain a laminate 2 having a layer structure consisting of heavy release NCF / adhesive layer / gas barrier layer 2 / retardation layer / retardation layer substrate. By peeling off the heavy peel NCF of the laminate 2, a second laminate (without a gas barrier layer on the light-emitting part (glass plate) side) consisting of an adhesive layer / gas barrier layer 2 / retardation layer and a laminate consisting of a retardation layer base material can be obtained.
[0192] <Preparation of environmental test samples> The polarizer layer side of the first laminate and the adhesive layer side of the laminate of the second laminate and the retardation layer substrate were closely laminated to obtain a laminate consisting of a front plate / water-based adhesive layer / polarizer layer / adhesive layer / gas barrier layer 2 / retardation layer and a retardation layer substrate. Next, the retardation layer substrate of the laminate was peeled off and the exposed surface was closely laminated with a glass plate having a thickness of 0.7 mm via an adhesive layer to obtain an environmental test sample. The environmental test sample was made of the third laminate / adhesive layer / glass plate, and each side of the third laminate was located 10 mm inside each side of the glass plate. The size of the glass plate was 50 mm x 50 mm. The adhesive layer for bonding the laminate and the glass plate was the same as the adhesive layer for bonding the first laminate and the second laminate.
[0193] (ii) Example 2 <Preparation of second laminate> A release substrate A was laminated on the retardation layer surface of the retardation layer (structure of retardation layer substrate / photo-alignment film / retardation layer) formed on the retardation layer substrate via a gas barrier 2 forming composition, passed between a pair of laminating rolls, and then dried at 80 ° C for 3 minutes to obtain a laminate consisting of release substrate A / gas barrier layer 2 / retardation layer / retardation layer substrate. Next, a release substrate B was laminated on the exposed surface by peeling the retardation layer substrate from the laminate via a gas barrier 2 forming composition, passed between a pair of laminating rolls, and then dried at 80 ° C for 3 minutes to obtain a laminate consisting of release substrate A / gas barrier layer 2 / retardation layer / gas barrier layer 2 / release substrate B. The two release substrates are each peelably laminated on the gas barrier layer 2, and the release substrate A can be peeled off before the release substrate B. The adhesive layer surface of a laminate consisting of heavy release NCF / adhesive layer was closely laminated to the surface of gas barrier layer 2 exposed by peeling off release substrate A of the laminate, thereby obtaining a laminate having a layer structure consisting of heavy release NCF / adhesive layer / gas barrier layer 2 / retardation layer / gas barrier layer 2 / release substrate B. The heavy release NCF of the laminate was peeled off to obtain a laminate consisting of a second laminate (double-sided gas barrier layer) consisting of adhesive layer / gas barrier layer 2 / retardation layer / gas barrier layer 2 and release substrate B.
[0194] <Preparation of environmental test samples> The polarizer layer side of the first laminate and the adhesive layer side of the laminate of the second laminate and the release substrate B were laminated in close contact to obtain a laminate consisting of a third laminate consisting of a front plate / aqueous adhesive layer / polarizer layer / adhesive layer / gas barrier layer 2 / retardation layer / gas barrier layer 2 and the release substrate B. Next, the release substrate B of the laminate was peeled off and the exposed surface was laminated in close contact with a glass plate having a thickness of 0.7 mm via the same adhesive layer as used in Example 1 to obtain an environmental test sample. The environmental test sample was made of the third laminate / adhesive layer / glass plate, and each side of the third laminate was located 10 mm inward from each side of the glass plate. The size of the glass plate was 50 mm x 50 mm.
[0195] (iii) Example 3 <Preparation of second laminate> A second laminate was obtained in the same manner as in Example 2, except that when laminating release substrate A on the retardation-expressing layer surface of the retardation layer via a gas barrier 2-forming composition, the sample width of the retardation layer was narrowed by 10 mm compared with the sample width of release substrate A, and gas barrier layer 2 was formed also on all ends of the retardation layer in the thickness direction.
[0196] <Preparation of environmental test samples> An environmental test sample was obtained in the same manner as in Example 2.
[0197] (iv) Example 4 The retardation layer surface of the retardation layer and the polarizer layer surface of the first laminate were laminated via a gas barrier 2 forming composition, passed between a pair of laminating rolls, and then dried at 80°C for 3 minutes to obtain a laminate consisting of a front plate / water-based adhesive layer / polarizer layer / gas barrier layer 2 / retardation layer (no adhesive layer and no gas barrier layer on the light-emitting part (glass plate) side) and a retardation layer substrate. The retardation layer substrate was peeled off from the laminate, and the exposed surface was adhered to a glass plate having a thickness of 0.7 mm via the same adhesive layer as used in Example 1 to obtain an environmental test sample. The environmental test sample was made of a third laminate / adhesive layer / glass plate, and was prepared so that each side of the third laminate was located 10 mm inside each side of the glass plate. The size of the glass plate was 50 mm x 50 mm.
[0198] (v) implementation example 5 <Preparation of second laminate> A second laminate (without a gas barrier layer on the light-emitting portion (glass plate) side) was obtained in the same manner as in Example 1, except that a gas barrier 1 forming composition was used as the gas barrier forming composition.
[0199] <Preparation of environmental test samples> An environmental test sample was obtained in the same manner as in Example 1.
[0200] (vi) Comparative example 1 The polarizer layer surface of the first laminate and the retardation layer surface of the retardation layer were laminated via an adhesive layer to obtain a third laminate consisting of a front plate / water-based adhesive layer / polarizer layer / adhesive layer / retardation layer and a laminate consisting of a retardation layer base material. The retardation layer base material was peeled off from the laminate, and the exposed surface was adhered to a glass plate having a thickness of 0.7 mm via the same adhesive layer as in Example 1 to obtain an environmental test sample.
[0201] (vii) Comparative example 2 <Preparation of second laminate> A release substrate C is laminated on the retardation layer surface of the retardation layer via a gas barrier 3-forming composition, and the laminate is passed between a pair of laminating rolls. Then, an ultraviolet ray irradiation device (a deuterium lamp manufactured by Heraeus K.K.) is used to irradiate the laminate with an integrated light amount of 400 mJ / cm 2 . 2 The laminate was irradiated with ultraviolet light so that the wavelength was 1000 nm (UVB), and a laminate consisting of a release substrate C / gas barrier layer 3 / retardation layer / retardation layer substrate was obtained. The release substrate C was peeled off from the laminate, and the adhesive layer surface of a laminate consisting of a heavy release NCF / adhesive layer was closely laminated on the gas barrier layer 3 surface to obtain a laminate having a layer structure consisting of heavy release NCF / adhesive layer / gas barrier layer 3 / retardation layer / retardation layer substrate. The heavy release NCF of the laminate was peeled off, and a laminate consisting of a second laminate (without a gas barrier layer on the light-emitting portion (glass plate) side) consisting of an adhesive layer / gas barrier layer 3 / retardation layer and a retardation layer substrate was obtained.
[0202] <Preparation of environmental test samples> An environmental test sample was obtained in the same manner as in Example 1.
[0203] (viii) Comparative example 3 <Preparation of second laminate> A release substrate C is laminated on the retardation layer surface of the retardation layer via a gas barrier 3-forming composition, and the laminate is passed between a pair of laminating rolls. Then, an ultraviolet ray irradiation device (a deuterium lamp manufactured by Heraeus K.K.) is used to irradiate the laminate with an integrated light amount of 400 mJ / cm 2 . 2The laminate was then irradiated with ultraviolet light so that the wavelength was 1000 nm (UVB), and a laminate consisting of a release substrate C / gas barrier layer 3 / retardation layer / retardation layer substrate was obtained. Next, the retardation layer substrate was peeled off from the laminate, and a release substrate D was laminated on the exposed surface via a gas barrier 3-forming composition. The laminate was then passed through a pair of laminating rolls, and the integrated light amount was 400 mJ / cm2. 2 The laminate was irradiated with ultraviolet light so that the wavelength was 1000 nm (UVB), and a laminate consisting of release substrate C / gas barrier layer 3 / retardation layer / gas barrier layer 3 / release substrate D was obtained. The two release substrates were each peelably laminated on the gas barrier layer 3, and the release substrate C could be peeled off before the release substrate D. The release substrate C was peeled off and the gas barrier layer 3 surface of the laminate was exposed. The adhesive layer surface of the laminate consisting of the heavy release NCF / adhesive layer was closely laminated on the gas barrier layer 3 surface of the laminate, which was exposed by peeling off the release substrate C, to obtain a laminate having a layer structure consisting of the heavy release NCF / adhesive layer / gas barrier layer 3 / retardation layer / gas barrier layer 3 / release substrate D. The heavy release NCF of the laminate was peeled off, and a laminate consisting of the adhesive layer / gas barrier layer 3 / retardation layer / gas barrier layer 3 and the release substrate D was obtained.
[0204] <Preparation of environmental test samples> The polarizer layer side of the first laminate and the pressure-sensitive adhesive layer side of the laminate of the second laminate and release substrate D were closely laminated to obtain a laminate consisting of a third laminate consisting of a front plate / aqueous adhesive layer / polarizer layer / pressure-sensitive adhesive layer / gas barrier layer 3 / retardation layer / gas barrier layer 3 and release substrate D. Next, release substrate D of the laminate was peeled off, and the exposed surface was closely laminated to a glass plate having a thickness of 0.7 mm via the same pressure-sensitive adhesive layer as used in Example 1 to obtain an environmental test sample.
[0205] (5) Environmental test methods and evaluation of results The above environmental test samples were used in Examples 1 to 5、 The embodiments of Comparative Examples 1 to 3 were produced and subjected to environmental test durability evaluation. The environmental tests included a light exposure test and a warm water immersion test. The results are shown in Table 1. (i) <Light exposure test method> The light exposure durability was evaluated by carrying out a deterioration test using the following equipment and method: The light source consisted of a xenon arc lamp, quartz glass, and a daylight filter, and the temperature inside the test chamber was adjusted so as not to exceed 45°C. Measurement device: ATLAS Suntest XLS+ (manufactured by Ametech Co., Ltd.) Conditions: 267W / m with irradiation energy in the 300nm to 800nm wavelength range 2 ×300 hours
[0206] (ii) <Evaluation of light exposure durability 1: Change in central retardation> The retardation R0 (nm) at a wavelength of 550 nm was measured at the same location in the center of the surface of the environmental test sample before and after the light exposure durability test using a phase difference measuring device (KOBRA-WPR, manufactured by Oji Scientific Instruments Co., Ltd.) to determine the amount of change before and after the light exposure durability test. No clearly visible change in reflected color was observed in samples with an R0 change of less than about 1 nm, but a noticeable change in reflected color occurred in samples with an R0 change of more than 2 nm, resulting in a significant decrease in the black display ability.
[0207] (iii) <Evaluation of light exposure durability 2: Change in edge reflection color> Aluminum foil ("My Foil" manufactured by UACJ Foil Corporation) was attached to the glass surface of the environmental test sample via an adhesive layer, and the length of the edge color change of the sample was measured before and after the light exposure durability test. The length of the edge color change must be less than 3 mm, since there is a risk that the color change of the image display device will extend beyond the non-visible part that covers the side of the image display device of the smartphone or television.
[0208] (iv) <Hot water immersion test method> The environmental test sample was immersed in pure water at 60°C for 10 hours, and the changes before and after immersion were observed.
[0209] (v) <Evaluation of hot water immersion durability> When water immersion caused moisture to penetrate from the edge of the gas barrier layer to the in-plane center, and spot-like lifting or peeling was observed between the gas barrier layer and the retardation layer, it was marked as X. On the other hand, when a transmission color change of less than 0.5 mm was observed at the edge of the polarizer layer, moisture did not penetrate to the center of the polarizer, and no lifting or peeling was observed, it was marked as O.
[0210] [Table 1] [Explanation of symbols]
[0211] 1: Retardation layer 2: Gas barrier layer 3: Alignment film 4: Phase contrast layer 5: Peelable substrate 6: Adhesive layer 7: Polarizer layer 8: Front plate 9: Adhesive layer 11: Optical laminate
Claims
1. A retardation layer including a retardation-exhibiting layer formed of a cured product of a polymerizable liquid crystal composition including at least one polymerizable liquid crystal compound, a gas barrier layer adjacent to at least one surface of the retardation layer, and a polarizer layer, the polarizer layer and the retardation layer are laminated with only a gas barrier layer adjacent to the retardation layer interposed therebetween, The retardation-exhibiting layer is represented by the following formula (I), formula (II) and formula (III): Re(450) / Re(550)≦1.00 (I) 1.00≦Re(650) / Re(550) (II) 100nm≦Re(550)≦180nm (III) [wherein Re(λ) represents an in-plane retardation value of the retardation-exhibiting layer at a wavelength of λ nm, Re(550) represents an in-plane retardation value of the retardation-exhibiting layer at a wavelength of 550 nm, and Re=(nx(550)-ny(550))×d (wherein d represents a thickness of the retardation-exhibiting layer, nx represents a principal refractive index at a wavelength of 550 nm in a direction parallel to the plane of the retardation-exhibiting layer in an index ellipsoid formed by the retardation-exhibiting layer, and ny represents a refractive index at a wavelength of 550 nm in a direction parallel to the plane of the retardation-exhibiting layer and perpendicular to the direction of nx in an index ellipsoid formed by the retardation-exhibiting layer), the gas barrier layer contains a polymer having a crosslinked structure derived from a hydrophobic crosslinking agent, The gas barrier layer is 500 cm 3 / (m 2 An optical laminate having an oxygen gas permeability of 24 h atm or less.
2. 2. The optical laminate according to claim 1, wherein the hydrophobic crosslinking agent comprises at least one selected from the group consisting of an isocyanate-based crosslinking agent, a polyaldehyde-based crosslinking agent, and a metal compound-based crosslinking agent.
3. The optical laminate according to claim 1 or 2, wherein the polymer comprises a polyvinyl alcohol-based resin.
4. The optical laminate according to any one of claims 1 to 3, wherein the gas barrier layer is disposed adjacent to both sides of the retardation layer.
5. The optical laminate according to any one of claims 1 to 4, wherein the gas barrier layer covers at least one side surface in the thickness direction of the retardation layer.
Citation Information
Patent Citations
Substrate for display device and manufacturing method therefor
JP2003195271A
Water-based curable resin composition and laminate comprising cured film thereof
JP2005162892A
Polarizing plate and projection type liquid crystal display device using the same
JP2010117537A
Dichroic dye composition, light-absorbable anisotropic film, and polarizing element
JP2010150513A
Reversible thermosensitive recording material
JP2013173357A