Method for producing partially coated electrode active material, and electrode active material
The partial coating of electrode active materials with metal alkoxides and ozone treatment addresses resistance buildup in lithium-ion batteries by creating a non-reactive surface, enhancing cycling stability and discharge performance.
Patent Information
- Application Number
- JP2020543016
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-02-09
- Filing Date
- 2019-01-31
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2039-01-31
AI Technical Summary
Existing methods for coating cathode active materials in lithium-ion batteries are inefficient in reducing resistance buildup during cycling, particularly when particle agglomeration occurs.
A method involving partial coating of electrode active materials with metal alkoxides or metal amides, followed by moisture treatment, and repeated cycles with ozone to create a non-uniform coating, ensuring at least 80% of particles are coated with 50% surface coverage, using specific chemical properties to prevent uncoated portions from reacting.
The method results in electrode active materials with low resistance buildup over 500 cycles, suitable for lithium-ion batteries, exhibiting improved discharge behavior and cycling stability.
Smart Images

Figure 0007580272000001 
Figure 0007580272000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a partially coated electrode active material, said method comprising the steps of: (a) General formula Li 1+x TM 1-x O 2 where T M is a combination of Ni, Co, and optionally Mn, and optionally at least one metal selected from Al, Ti, Mo, W, and Zr, x is in the range of 0 to 0.2, and at least 60 mol % of the transition metals in T M is Ni, the electrode active material having a residual moisture content in the range of 50 to 1,000 ppm; (b) treating the electrode active material with a metal alkoxide or a metal halide or a metal amide or an alkyl metal compound; (c) treating the material obtained in step (b) with moisture; (d) repeating the series of steps (b) and (c) two to four times; Including, In the final series of steps (b) and (c), the moisture is at least partially replaced by ozone. [Background technology]
[0002] Lithium-ion secondary batteries are modern devices for storing energy. Many applications have been considered, from small devices such as mobile phones and laptop computers to car batteries and other e-mobility batteries. Various battery components such as electrolytes, electrode materials and separators have important roles in the performance of the battery. Cathode materials have received particular attention. Several materials have been proposed, such as lithium iron phosphate, lithium cobalt oxide, and lithium nickel cobalt manganese oxide. Extensive research has been conducted, but the solutions found so far still leave room for improvement.
[0003] One problem with lithium-ion batteries is due to undesirable reactions at the surface of the cathode active material. Such reactions can be the decomposition of the electrolyte or the solvent or both. Therefore, attempts have been made to protect the surface without preventing lithium exchange during charging and discharging. Examples are attempts to coat the cathode active material with, for example, aluminum oxide or calcium oxide (see, for example, US 8,993,051).
[0004] However, the efficiency of the process can still be improved, especially in embodiments where the particles tend to agglomerate, and sometimes the efficiency can be improved both in terms of reaction time and percentage of coated particles. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] US 8,993,051 Summary of the Invention [Problem to be solved by the invention]
[0006] Accordingly, the present invention sought to provide a method for coating electrode active materials to reduce the tendency for resistance to build up during repeated cycling. [Means for solving the problem]
[0007] We have therefore found a method as defined at the outset, which hereinafter is also referred to as the inventive method or the method according to the (present) invention: The inventive method is a method for the production of a coated electrode active material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The term "partially coated" as used in the context of the present invention refers to coating at least 80% of the particles of a batch of particulate material, and at least 50%, for example 75-99.99%, preferably 80-90% of the surface of each particle.
[0009] The thickness of such coatings may be very thin, for example 0.1-5 nm. In other embodiments, the thickness may range from 6-15 nm. In further embodiments, the thickness of such coatings ranges from 16-50 nm. Thicknesses herein are the thicknesses per square meter of particle surface, assuming 100% conversion. 2 "Metal alkoxide" refers to an average thickness that is determined mathematically by calculating the amount of metal alkoxide or metal halide or metal amide or metal alkyl per layer.
[0010] Without wishing to be bound by any theory, it is believed that the uncoated portions of the particles do not react due to certain chemical properties of the particles, such as, but not limited to, density of chemically reactive groups such as hydroxyl groups, oxide moieties with chemical constraints, or adsorbed water.
[0011] In one embodiment of the present invention, the electrode active material has an average particle size (D50) in the range of 3 to 20 μm, preferably 5 to 16 μm. The average particle size can be determined, for example, by light scattering or laser diffraction or electroacoustic spectroscopy. The particles are usually composed of aggregates from primary particles, and the above particle size refers to the particle size of the secondary particles.
[0012] In one embodiment of the present invention, the electrode active material is 0.1 to 1.5 μm. 2 / g. The BET surface area can be determined by nitrogen adsorption after outgassing the sample at 200° C. for 30 minutes and beyond, according to DIN ISO 9277:2010.
[0013] The method of the present invention comprises three steps (a), (b) and (c), also referred to herein as step (a), step (b) and step (c).
[0014] Step (a) comprises reacting a compound of the general formula Li 1+x TM 1-x O 2 wherein TM is a combination of Ni, Co, optionally Mn, and optionally at least one metal selected from Al, Ti, Mo, W, and Zr, x is in the range of 0 to 0.2, and at least 60 mol % of the transition metals in TM is Ni, wherein the electrode active material has a residual moisture content in the range of 50 to 1,000 ppm.
[0015] TM is optionally in each case selected from at least one metal selected from Al, Ti, Zr, W and Mo, preferably selected from a combination of Mn and Ni, or a combination of Ni and Co, or a combination of Ni, Mn and Co, optionally in each case selected from at least one metal selected from Al, W, Ti and Zr. Preference is given to combinations of Ni and Co, and combinations of Ni, Mn and Co, optionally in each case selected from at least one metal selected from Al, W, Ti and Zr.
[0016] In a preferred embodiment, TM has the general formula (I): (Ni a Co b Mn c ) 1-d M d (I) (In the formula, a is in the range of 0.6 to 0.95, b is in the range of 0.025 to 0.2, c is in the range of 0.025 to 0.2, d is in the range of 0 to 0.1, M is Al; a+b+c=1) It is a combination of metals.
[0017] Li (1+x)[Ni 0.6 Co 0.2 Mn 0.2 ] (1-x) O 2 , Li (1+x) [Ni 0.7 Co 0.2 Mn 0.1 ] (1-x) O 2 and Li (1+x) [Ni 0.8 Co 0.1 Mn 0.1 ] (1-x) O 2 (wherein each x is defined as above) is particularly preferred.
[0018] The electrode active material is preferably provided as a free-flowing powder, without any additives such as conductive carbon or binders.
[0019] The electrode active material provided in step (a) has a residual water content in the range of 50 to 1,000 ppm, preferably 100 to 400 ppm. The residual water content can be determined by Karl Fischer titration.
[0020] In step (b), the electrode active material is treated with a metal alkoxide or a metal halide or a metal amide or an alkyl metal compound.
[0021] In one embodiment of the process of the present invention, step (b) is carried out at a temperature in the range of 15 to 1000° C., preferably 15 to 500° C., more preferably 20 to 350° C., even more preferably 50 to 150° C. In step (b), it is preferred to select a temperature at which the metal alkoxide or metal amide or alkyl metal compound, as the case may be, is in the gas phase.
[0022] In one embodiment of the invention, step (b) is carried out at atmospheric pressure, although step (b) may also be carried out at reduced or elevated pressure. For example, step (b) is carried out at a pressure ranging from 5 mbar to 1 bar above atmospheric pressure, preferably from 10 to 150 mbar above atmospheric pressure. In the context of the present invention, atmospheric pressure is ambient pressure, e.g. 1 atm or 1013 mbar at sea level. At different altitudes, the ambient pressure may be lower. In other embodiments, step (b) may be carried out at a pressure ranging from 150 mbar to 560 mbar above atmospheric pressure.
[0023] In a preferred embodiment of the present invention, the alkyl metal compound or metal alkoxide or metal amide is, respectively, Al(R 1 ) 3 , Al(R 1 ) 2 O.H., Al.R. 1 (OH) 2 , M 1 (R 1 ) 4-y H y , Al(OR 2 ) 3 , M 1 (OR 2 ) 4 , M 1 [NR 2 ] 2 ] 4 and methylalumoxane, wherein R 1 are the same or different, linear or branched C 1 ~C 8 -alkyl, R 2 are the same or different, linear or branched C 1 ~C 4 -alkyl, M 1 is Ti or Zr, with Ti being preferred.
[0024] Metal alkoxides are aluminum and transition metal C 1 ~C 4-alkoxides. Preferred transition metals are titanium and zirconium. Examples of alkoxides include methanolates, hereinafter also referred to as methoxides, ethanolates, hereinafter also referred to as ethoxides, propanolates, hereinafter also referred to as propoxides, and butanolates, hereinafter also referred to as butoxides. Particular examples of propoxides are n-propoxide and iso-propoxide. Particular examples of butoxides are n-butoxide, iso-butoxide, sec.-butoxide and tert.-butoxide. Combinations of alkoxides can also be used.
[0025] metal C 1 ~C 4 A preferred example of an -alkoxide is Ti[OCH(CH 3 ) 2 ] 4 , Ti(OC 4 H 9 ) 4 , Zn(OC 3 H 7 ) 2 , Zr(OC 4 H 9 ) 4 , Zr(OC 2 H 5 ) 4 , Al(OCH 3 ) 3 , Al(O.C. 2 H 5 ) 3 ,Al(OnC 3 H 7 ) 3 , Al(O-iso-C 3 H 7 ) 3 , Al(O-sec.-C 4 H 9 ) 3 , and Al(OC 2 H 5 )(O-sec.-C 4 H 9 ) 2 It is.
[0026] Examples of aluminum alkyl compounds are trimethylaluminum, triethylaluminum, triisobutylaluminum and methylalumoxane.
[0027] Metal amides are sometimes also called metal imides. An example of a metal amide is Ti[N(CH 3 ) 2 ] 4 It is.
[0028] Particularly preferred compounds are metal C 1 ~C 4 -alkoxides and metal alkyl compounds, and even more preferably trimethylaluminum.
[0029] In one embodiment of the present invention, the amount of metal alkoxide or metal amide or alkyl metal compound is in the range of 0.1 to 1 g per kg of electrode active material.
[0030] Preferably, the amount of metal alkoxide or metal amide or alkyl metal compound is calculated as 80 to 200% of a monolayer on the electrode active material per cycle.
[0031] In one embodiment of the invention, step (b) is carried out in a rotary kiln, a free-fall mixer, a continuous vibrating bed or a fluidized bed. Step (b) of the process of the invention, and step (c), which will be described in detail below, may be carried out in the same vessel or in different vessels.
[0032] In a preferred embodiment of the present invention, the duration of step (b) is in the range of 1 second to 2 hours, preferably 1 second to 10 minutes.
[0033] In a third step, also referred to in the context of the present invention as step (c), the material obtained in step (b) is treated with moisture.
[0034] In one embodiment of the present invention, step (c) is carried out at a temperature in the range of 50 to 250°C.
[0035] In one embodiment of the invention, step (c) is carried out in a rotary kiln, a free-fall mixer, a continuous vibrating bed or a fluidized bed.
[0036] In one embodiment of the present invention, step (c) is carried out at normal pressure, however, step (c) may be carried out at reduced or elevated pressure. For example, step (c) is carried out at a pressure ranging from 5 mbar to 1 bar above normal pressure, preferably from 10 to 250 mbar above normal pressure. In the context of the present invention, normal pressure is 1 atm or 1013 mbar. In another embodiment, step (c) may be carried out at a pressure ranging from 150 mbar to 560 mbar above normal pressure.
[0037] Steps (b) and (c) may be carried out at the same or different pressures, preferably at the same pressure.
[0038] For example, said moisture may be introduced by treating the material obtained according to step (b) with a moisture-saturated inert gas, for example moisture-saturated nitrogen, or a moisture-saturated noble gas, for example argon. In step (c), saturation refers to normal conditions or reaction conditions.
[0039] In a preferred embodiment of the present invention, the duration of step (c) ranges from 10 seconds to 2 hours, preferably from 1 second to 10 minutes.
[0040] In one embodiment of the present invention, between steps (b) and (c), the reactor in which the process of the present invention is carried out is flushed or purged with an inert gas, for example with dry nitrogen or with dry argon. Suitable flush or purge times are between 1 second and 30 minutes, preferably between 1 second and 10 minutes. The amount of inert gas is preferably sufficient to exchange the reactor contents by 1 to 15 times. Such flush or purge makes it possible to avoid the generation of by-products such as separate particles of the reaction products of the metal alkoxide or metal amide or alkyl metal compound with water, respectively. In the case of the combination of trimethylaluminum and water, such by-products are methane and alumina, or trimethylaluminum not deposited on the particulate material, the latter being an undesirable by-product. The flush may be carried out after step (c) and thus before another step (b). In this specification, "dry" refers to a water content of less than 10 ppm by weight, for example 3 to 5 ppm.
[0041] In one embodiment of the invention, each flash step between (b) and (c) has a duration in the range of 1 second to 10 minutes.
[0042] In one embodiment of the invention, between steps (b) and (c), the reactor is evacuated. Said evacuation may be carried out after step (c) and thus before another step (b). Evacuation in this context includes any pressure drop, for example from 10 to 1,000 mbar (absolute), preferably from 10 to 500 mbar (absolute).
[0043] Each step (b) and (c) may be carried out in a fixed bed reactor, a fluidized bed reactor, a forced flow reactor or mixer, such as a forced mixer or a free-fall mixer. An example of a fluidized bed reactor is a spouted bed reactor. Examples of forced mixers are ploughshare mixers, paddle mixers and shovel mixers. Plowshare mixers are preferred. The preferred ploughshare mixers are installed horizontally, the term horizontal referring to the axis around which the mixing elements rotate. Preferably, the process of the present invention is carried out with a shovel mixing tool, a paddle mixing tool, a Becker blade mixing tool and most preferably with a ploughshare mixer according to the hurling and whirling principle. Free-fall mixers use gravity to achieve mixing. In a preferred embodiment, steps (b) and (c) of the process of the present invention are carried out in a drum or pipe-like vessel rotating about its horizontal axis. In a more preferred embodiment, steps (b) and (c) of the process of the present invention are carried out in a rotating vessel equipped with baffles.
[0044] In one embodiment of the invention, the rotating vessel comprises baffles in the range of 2 to 100, preferably in the range of 2 to 20. Preferably, such baffles are mounted flush against the vessel wall.
[0045] In one embodiment of the present invention, such baffles are arranged axisymmetrically along the rotating vessel, drum, or pipe, with an angle between them and the wall of the rotating vessel ranging from 5 to 45°, preferably from 10 to 20°. With such an arrangement, they can transport the coated cathode active material very efficiently through the rotating vessel.
[0046] In one embodiment of the present invention, the baffle extends into the rotating vessel within a range of 10 to 30% of the diameter.
[0047] In one embodiment of the present invention, the baffle covers a range of 10-100%, preferably 30-80%, of the total length of the rotating vessel, where the term length is taken parallel to the axis of rotation.
[0048] In a preferred embodiment of the invention, the method of the invention comprises the step of removing the coated material from the container or containers respectively by air convection, for example at 20-100 m / s.
[0049] In one embodiment of the invention, the exhaust gas is treated with water at a pressure above 1 bar, even more preferably at a pressure higher than the pressure in the reactor in which steps (b) and (c) are carried out, for example at a pressure in the range of 1.010 to 2.1 bar, preferably in the range of 1.005 to 1.150 bar. The high pressure is advantageous to compensate for the pressure loss in the exhaust line.
[0050] Step (d) involves repeating the sequence of steps (b) and (c) two to four times, where in the last sequence of steps (b) and (c) moisture is at least partially replaced by ozone. Said latter step is hereinafter referred to as step (c). * ) is also called.
[0051] Repeating may include repeating a sequence of steps (b) and (c) each time under the exact same conditions or under modified conditions, while still falling within the above definition. For example, each step (b) may be performed under the exact same conditions, or for example, each step (b) may be performed under different temperature conditions or for different durations, e.g., at 120°C, then 10°C and 160°C, each for 1 second to 1 hour.
[0052] Process (c * In step (c), ozone at least partially replaces moisture. * It is preferred that no humidity is applied in step (c) and that the humidity is completely replaced by ozone. Ozone may be generated from oxygen under conditions known per se, and therefore step (c) * ), ozone is usually applied in the presence of oxygen.
[0053] During the application of ozone, step (c * ) preferably no nitrogen is present.
[0054] In one embodiment of the present invention, step (c * In another embodiment of the present invention, step (c * ) is carried out at a pressure in the range of 5 mbar to 1 bar higher than normal pressure, preferably in the range of 10 to 250 mbar higher than normal pressure. * Step (c) is carried out at a pressure lower than normal pressure, for example, at a pressure lower than normal pressure by 100 to 900 mbar, preferably lower by 100 to 500 mbar. * ) may be carried out at a temperature of 20 to 300°C, preferably 100 to 300°C, and more preferably 150 to 250°C.
[0055] In one embodiment of the present invention, step (c * The duration of the ) is in the range of 1 second to 2 hours, preferably 1 second to 10 minutes.
[0056] Process (c * (c) may be carried out in the same type of vessel as step (c). * ) are carried out in the same vessel.
[0057] A particulate electrode active material is obtained.
[0058] In one embodiment of the present invention, a series of steps (b) and (c) * In another embodiment, the sequence of steps (b) and (c) is carried out only once. * ) is performed 2 to 5 times.
[0059] In one embodiment of the present invention, step (c * After step (c), a post-treatment, for example a thermal post-treatment (e), is carried out. Such a thermal post-treatment (e) may be carried out in the following manner: * ), the particulate electrode active material obtained thereafter may be treated at a temperature in the range of 150 to 800°C, preferably 150 to 400°C, and preferably 180 to 350°C, for a period in a certain range, for example, 10 minutes to 2 hours.
[0060] A further aspect of the present invention relates to a particulate electrode active material, hereinafter also referred to as the inventive electrode active material. The electrode material of the present invention has the general formula Li 1+x TM 1-x O 2 wherein TM is a combination of Ni, Co, optionally Mn, and optionally at least one metal selected from Al, Ti, Mo, W, and Zr, x is in the range of 0-0.2, and at least 60 mol % of the transition metals in TM is Ni, and the outer surface of the particles is non-uniformly coated with an acidic oxide selected from acidic aluminum oxyhydroxide, acidic alumina, acidic titania, and acidic zirconia. Acidic aluminum oxyhydroxide and acidic alumina are preferred.
[0061] Non-uniform coatings can be mapped with X-ray photoelectron spectroscopy ("XPS") or transmission electron microscopy using energy dispersive X-ray spectroscopy ("TEM-EDX").
[0062] TM is already defined above.
[0063] In one embodiment of the present invention, the electrode active material of the present invention has an average particle size (D50) in the range of 3 to 20 μm, preferably 5 to 16 μm. The average particle size can be determined, for example, by light scattering or laser diffraction or electroacoustic spectroscopy. The particles are usually composed of aggregates from primary particles, and the above particle size refers to the particle size of the secondary particles.
[0064] In one embodiment of the present invention, the electrode active material of the present invention is 0.1 to 1.5 μm 2 / g. The BET surface area can be determined by nitrogen adsorption after outgassing the sample at 200° C. for 30 minutes and beyond, according to DIN ISO 9277:2010.
[0065] Preferably, the TM in the particulate material of the present invention is Ni 0.6 Co 0.2 Mn 0.2, Ni 0.7 Co 0.2 Mn 0.1 and Ni 0.8 Co 0.1 Mn 0.1 wherein the acidic oxide is selected from acidic aluminum oxyhydroxide and acidic alumina.
[0066] In one embodiment of the present invention, the electrode active material of the present invention has an average particle size (D50) in the range of 3 to 20 μm, preferably 5 to 16 μm. The average particle size can be determined, for example, by light scattering or laser diffraction or electroacoustic spectroscopy. The particles are usually composed of aggregates from primary particles, and the above particle size refers to the particle size of the secondary particles.
[0067] In one embodiment of the invention, the non-uniform coating has an average thickness in the range of 0.2 to 2 nm, preferably 0.3 to 0.8 nm.
[0068] The electrode active materials of the present invention are highly suitable for use as cathodes in lithium ion batteries. They exhibit low resistance build-up caused by repeated cycling, for example, over 500 cycles.
[0069] A further aspect of the present invention relates to electrodes comprising at least one electrode active material according to the present invention. They are particularly useful for lithium-ion batteries. Lithium-ion batteries comprising at least one electrode according to the present invention show good discharge behavior. An electrode comprising at least one electrode active material according to the present invention is hereinafter also referred to as the cathode of the present invention or the cathode of the present invention.
[0070] The cathodes according to the present invention may include additional components. They may include a current collector, such as, but not limited to, aluminum foil. They may further include conductive carbon and a binder.
[0071] Suitable binders are preferably selected from organic (co)polymers. Suitable (co)polymers, i.e. homopolymers or copolymers, can be selected from (co)polymers obtainable, for example, by anionic (co)polymerization, catalytic (co)polymerization or free radical (co)polymerization, in particular from polyethylene, polyacrylonitrile, polybutadiene, polystyrene and copolymers of at least two comonomers selected from ethylene, propylene, styrene, (meth)acrylonitrile and 1,3-butadiene. Polypropylene is also suitable. Polyisoprene and polyacrylates are furthermore suitable. Polyacrylonitrile is particularly preferred.
[0072] In the context of the present invention, polyacrylonitrile is understood to mean not only polyacrylonitrile homopolymers but also copolymers of acrylonitrile with 1,3-butadiene or with styrene. Polyacrylonitrile homopolymers are preferred.
[0073] In the context of the present invention, polyethylene refers not only to homopolyethylenes, but also to polyethylenes containing at least 50 mol % copolymerized ethylene and up to 50 mol % of at least one further comonomer, such as α-olefins, such as propylene, butylene (1-butene), 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-pentene, and also isobutene, vinyl aromatics, such as styrene, and also (meth)acrylic acid, vinyl acetate, vinyl propionate, C 10 copolymers of (meth)acrylic acid. 1 ~C 10 -alkyl esters, in particular methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, 2-ethylhexyl acrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, and also copolymers of ethylene with maleic acid, maleic anhydride and itaconic anhydride. The polyethylene may be HDPE or LDPE.
[0074] In the context of the present invention, polypropylene is understood to mean not only homopolypropylene but also copolymers of propylene with at least 50 mol % copolymerized propylene and up to 50 mol % of at least one further comonomer, such as ethylene, and α-olefins, such as butylene, 1-hexene, 1-octene, 1-decene, 1-dodecene and 1-pentene. The polypropylene is preferably isotactic polypropylene or essentially isotactic polypropylene.
[0075] In the context of the present invention, polystyrene refers to homopolymers of styrene as well as acrylonitrile, 1,3-butadiene, (meth)acrylic acid, C 2 styrene, 1,3-butadiene, (meth)acrylic acid, 1 ~C 10 -alkyl esters, divinylbenzene, in particular 1,3-divinylbenzene, 1,2-diphenylethylene and α-methylstyrene copolymers are also understood to mean.
[0076] Another preferred binder is polybutadiene.
[0077] Other suitable binders are selected from polyethylene oxide (PEO), cellulose, carboxymethyl cellulose, polyimides and polyvinyl alcohol.
[0078] In one embodiment of the invention, the binder has an average molecular weight M ranging from 50,000 g / mol to 1,000,000 g / mol, preferably up to 500,000 g / mol. W The (co)polymers are selected from those having the formula:
[0079] The binder may be a crosslinked or non-crosslinked (co)polymer.
[0080] In a particularly preferred embodiment of the present invention, the binder is selected from halogenated (co)polymers, in particular fluorinated (co)polymers.Halogenated or fluorinated (co)polymers are understood to mean (co)polymers that contain at least one (co)polymerized (co)monomer with at least one halogen atom or at least one fluorine atom per molecule, more preferably at least two halogen atoms or at least two fluorine atoms per molecule.Examples include polyvinyl chloride, polyvinylidene chloride, polytetrafluoroethylene, polyvinylidene fluoride (PVdF), tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), vinylidene fluoride-tetrafluoroethylene copolymer, perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, and ethylene-chlorofluoroethylene copolymer.
[0081] Suitable binders are especially polyvinyl alcohol and halogenated (co)polymers, such as polyvinyl chloride or polyvinylidene chloride, in particular fluorinated (co)polymers, such as polyvinyl fluoride and especially polyvinylidene fluoride and polytetrafluoroethylene.
[0082] The cathode of the present invention may contain 1 to 15% by weight of binder(s) relative to the electrode active material. In other embodiments, the cathode of the present invention may contain 0.1% to less than 1% by weight of binder(s).
[0083] A further aspect of the invention is a battery containing at least one cathode comprising the electrode active material of the invention, carbon and a binder, at least one anode, and at least one electrolyte.
[0084] The cathode embodiments of the present invention have already been described in detail above.
[0085] The anode is made of at least one anode active material, such as carbon (graphite), TiO 2 , lithium titanium oxide, silicon, lithium or tin. The anode may further contain a current collector, for example a metal foil, such as copper foil.
[0086] The electrolyte may include at least one non-aqueous solvent, at least one electrolyte salt, and optionally, additives.
[0087] The non-aqueous solvent for the electrolyte may be liquid or solid at room temperature and is preferably selected from polymers, cyclic or acyclic ethers, cyclic and acyclic acetals, and cyclic or acyclic organic carbonates.
[0088] Examples of suitable polymers are in particular polyalkylene glycols, preferably poly-C 1 ~C 4 -alkylene glycols, and in particular polyethylene glycols, where the polyethylene glycols are those containing up to 20 mol % of one or more C 1 ~C 4 The polyalkylene glycol may preferably be a polyalkylene glycol having two methyl or ethyl end caps.
[0089] The molecular weight M of suitable polyalkylene glycols and particularly suitable polyethylene glycols W may be at least 400 g / mol.
[0090] The molecular weight M of suitable polyalkylene glycols and particularly suitable polyethylene glycols W can be up to 5,000,000 g / mol, preferably up to 2,000,000 g / mol.
[0091] Examples of suitable acyclic ethers are, for example, diisopropyl ether, di-n-butyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, preferably 1,2-dimethoxyethane.
[0092] Examples of suitable cyclic ethers are tetrahydrofuran and 1,4-dioxane.
[0093] Examples of suitable acyclic acetals are, for example, dimethoxymethane, diethoxymethane, 1,1-dimethoxyethane and 1,1-diethoxyethane.
[0094] An example of a suitable cyclic acetal is 1,3-dioxane, and especially 1,3-dioxolane.
[0095] Examples of suitable acyclic organic carbonates are dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate.
[0096] Examples of suitable cyclic organic carbonates are those represented by the general formulas (III) and (IV): [ka] (In the formula, R 1 , R 2 and R 3 can be the same or different, hydrogen and C 1 ~C 4 -alkyl, for example selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl, preferably R 2 and R 3 (Both cannot be tert-butyl) It is a compound of the formula:
[0097] In a particularly preferred embodiment, R 1 is methyl, R 2 and R 3 are each hydrogen or R 1 , R 2 and R 3are hydrogen.
[0098] Another preferred cyclic organic carbonate is vinylene carbonate of formula (V).
[0099] [ka]
[0100] Preferably, the solvent or solvents are used in an aqueous state, ie with a water content in the range of 1 ppm to 0.1% by weight, which can be determined, for example, by Karl Fischer titration.
[0101] The electrolyte (C) further comprises at least one electrolyte salt. Suitable electrolyte salts are in particular lithium salts. Examples of suitable lithium salts include LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 , LiCF 3 SO 3 , LiC(C n F 2n+1 SO 2 ) 3 , lithium imide, e.g. LiN(C n F 2n+1 SO 2 ) 2 (wherein n is an integer ranging from 1 to 20), LiN(SO 2 F) 2 , Li 2 SiF 6 , LiSbF 6 , LiAlCl 4 and the general formula (C n F 2n+1 SO 2 ) t It is the salt of YLi. where t=1 when Y is selected from oxygen and sulfur; when Y is selected from nitrogen and phosphorus, t=2; When Y is selected from carbon and silicon, t=3).
[0102] The preferred electrolyte salt is LiC(CF 3 SO 2 ) 3 , LiN(CF 3 SO 2 ) 2 , LiPF 6 , LiBF 4 , LiClO 4 Particularly preferably, LiPF 6 and LiN(CF 3 SO 2 ) 2 It is.
[0103] In one embodiment of the present invention, the battery according to the present invention comprises one or more separators by which the electrodes are mechanically separated.Suitable separators are polymer films, especially porous polymer films, that are unreactive towards metallic lithium.Particularly suitable materials for the separators are polyolefins, especially film-forming porous polyethylene and film-forming porous polypropylene.
[0104] A separator made of polyolefin, particularly polyethylene or polypropylene, may have a porosity in the range of 35 to 45%. A suitable pore size is, for example, in the range of 30 to 500 nm.
[0105] In another embodiment of the present invention, the separator can be selected from PET nonwoven fabrics filled with inorganic particles. Such separators can have a porosity in the range of 40-55%. Suitable pore sizes are, for example, in the range of 80-750 nm.
[0106] The battery according to the invention further comprises a housing which may have any shape, for example a cube or the shape of a cylindrical disk or a cylindrical can. In one variant, a metal foil configured as a pouch is used as the housing.
[0107] The battery according to the invention exhibits, for example, good discharge behavior at low temperatures (below 0° C., e.g. even below −10° C.), very good discharge and cycling behavior, especially with respect to capacity loss, at high temperatures (above 45° C., e.g. up to 60° C.), good safety behavior at high temperatures, such as above 60° C. Preferably, the cycling stability and the C-rate capacity behavior are also improved or are at least the same, although the Li content is lower.
[0108] The battery according to the present invention may comprise two or more electrochemical cells that are combined with each other, for example, connected in series or connected in parallel. A series connection is preferred. In the battery according to the present invention, at least one electrochemical cell contains at least one cathode according to the present invention. Preferably, in the electrochemical cell according to the present invention, the majority of the electrochemical cells contain the cathode according to the present invention. Even more preferably, in the battery according to the present invention, all the electrochemical cells contain the cathode according to the present invention.
[0109] The present invention further provides a method for using the battery according to the present invention in equipment, especially mobile equipment.Examples of mobile equipment are vehicles, such as automobiles, bicycles, aircraft, or water vehicles, such as boats or ships.Other examples of mobile equipment are manually operated, such as computers, especially laptops, phones, or powered hand tools, for example in the construction sector, especially drills, battery-powered drivers, or battery-powered staplers.
[0110] The present invention is further illustrated by the examples. EXAMPLES
[0111] sccm: standard cubic centimeters per minute, cubic centimeters under standard conditions I. Cathode Active Material I.1. Preparation of cathode active material precursor A stirred tank reactor was filled with deionized water. Precipitation of mixed transition metal hydroxide precursor was initiated by simultaneously feeding the aqueous transition metal solution and the alkaline precipitant at a flow rate ratio of 1.9 with a total flow rate of 8 hours residence time. The aqueous transition metal solution contained Ni, Co and Mn as their respective sulfates in a molar ratio of 6:2:2 with a total transition metal concentration of 1.65 mol / kg. The alkaline precipitant consisted of 25% by weight sodium hydroxide solution and 25% by weight ammonia solution in a mass ratio of 25. The pH value was maintained at 11.9 by separately feeding the aqueous sodium hydroxide solution. After the particle size was stabilized, the resulting suspension was continuously removed from the stirred vessel. The resulting suspension was filtered, washed with distilled water, dried in air at 120°C and sieved to obtain the mixed transition metal (TM) oxyhydroxide precursor.
[0112] I.2. Preparation of Cathode Active Material C-CAM.1 (comparison): The mixed transition metal oxyhydroxide precursor obtained according to I.1 was treated with Al 2 O 3 (average particle size 6 nm) and LiOH monohydrate to obtain a concentration of 0.3 mol % Al relative to Ni+Co+Mn+Al and a Li / (TM+Al) molar ratio of 1.03. The mixture was heated to 885° C. and kept in a forced flow of oxygen for 8 hours to obtain the electrode active material C-CAM 1.
[0113] The D50 determined using the technique of laser diffraction on a Mastersize 3000 machine from Malvern Instruments was 9.5 μm. The Al content was determined by ICP analysis and corresponded to 820 ppm. The residual moisture determined at 250° C. was 300 ppm.
[0114] C-CAM.2 (comparison): 100 g of C-CAM.1 was placed in a fluidized bed reactor equipped with an external heating jacket and fluidized at an average pressure of 130 mbar. The fluidized bed reactor was heated to 180° C. and maintained at 180° C. for 3 hours. Trimethylaluminum (TMA) in gaseous state was introduced into the fluidized bed reactor through a filter plate by opening a valve to a precursor reservoir containing TMA in liquid state and maintained at 50° C. The TMA was diluted with nitrogen as carrier gas. TMA and N 2 The gas flow rate was 10 sccm. After a reaction period of 210 seconds, the unreacted TMA was removed by nitrogen flow and the reactor was purged with nitrogen at a flow rate of 30 sccm for 15 minutes. Then, water in gaseous state was introduced into the fluidized bed reactor (flow rate: 10 sccm) by opening a valve to a reservoir containing liquid water maintained at 24°C. After a reaction period of 120 seconds, the unreacted TMA was removed by nitrogen flow and the reactor was purged with nitrogen at 30 sccm for 15 minutes. The above sequence was repeated three times. The reactor was cooled to 25°C and the material was discharged. The obtained C-CAM.2 showed the following characteristics: D50 = 10.6 μm, determined using the technique of laser diffraction on a Mastersize 3000 machine from Malvern Instruments. The Al content determined by inductively coupled plasma-optical emission spectroscopy (ICP-OES) via quantification against a standard solution using a PE-Optima 3300 RL instrument (standard detection limit 3 ppm): 260 ppm. The residual moisture determined at 250° C. was 120 ppm.
[0115] CAM.3 (Invention): The preparation of C-CAM.2 was repeated as above, but without the fourth water treatment step. Instead, the fluidized bed reactor was 2 8% by weight O in the stream 3 After opening the dosing valve, the O 3 / O 2 The mixture was introduced into a fluidized bed reactor for 30 min and N 2 was continued at 10 sccm. * .3).
[0116] After the fourth cycle was completed, the reactor was gassed with 30 sccm of N 2 The mixture was purged for 1500 seconds.
[0117] Elemental analysis of the aluminum content was performed by ICP-OES using a PE-Optima 3300 RL machine (typical detection limit 3 ppm). After coating, an absorption of 280 ppm Al was detected. Residual moisture determined at 250 °C was 110 ppm. C-CAM.3 was acidified with Al. 2 O 3 The mixture was partially coated with .
[0118] CAM.4 (Invention): The preparation of C-CAM.2 was repeated as above, but without the fourth water treatment step. Instead, the fluidized bed reactor was 2 8% by weight O in the stream 3 After opening the dosing valve, the O 3 / O 2 The mixture was introduced into a fluidized bed reactor for 30 min and N 2 was continued to flow at 10 sccm (step c * .4).
[0119] After the fourth cycle was completed, the reactor was gassed with 30 sccm of N 2 The series of TMA-treatments and steps (C * .4) was repeated three times.
[0120] Elemental analysis of the aluminum content was performed by ICP-OES using a PE-Optima 3300 RL machine (typical detection limit 3 ppm) and quantification against standard solutions. After coating, an absorption of 280 ppm Al was detected. Residual moisture determined at 250 °C was 110 ppm. C-CAM.4 was acidified with Al. 2 O 3 The mixture was partially coated with .
[0121] II Electrochemical Cell II.1. Preparation of electrodes for electrochemical testing Positive electrodes for electrochemical cycling experiments in single-layer pouch cells were prepared by coating slurries containing 94% by weight of cathode active material (94% by weight), 1% by weight of activated carbon (Super C65 L purchased from Imerys), 2% by weight of graphite (SFG6L from Imerys) and 3% by weight of polyvinylidene fluoride (PVdF) binder suspended in N-methyl-2-pyrrolidinone (NMP) onto aluminum foil (thickness = 20 μm) using a continuous doctor knife coating system, followed by drying (Mathis, KTF-S). Typically, all slurries were prepared based on at least 30 g of cathode active material, and the amount of NMP used was such that the total solids (CAM + Super C65 L + SFG6L + PVdF) was about 65%. Before cell assembly, the electrode tapes were dried in a hot air chamber at 120 °C for 16 h and finally pressed using a roll calendar.
[0122] II.2. Electrochemical Tests in Half Cells Electrochemical testing of the cathode active materials (C-CAM.1, C-CAM.2, CAM.3, and CAM.4) was performed in coin half cells (vs. Li metal as anode material, upper cut-off voltage 4.3 V vs. Li / Li + 1M LiPF in EC:EMC wt% (EC=ethylene carbonate, EMC=ethyl methyl carbonate) as electrolyte 6 , GF / D glass fiber separator (Whatman, and CR2032 from Hohsen Corp.) to obtain the first cycle discharge capacity.
[0123] The half-cells of the invention based on CAM.3 or CAM.4 outperformed the comparative half-cells based on C-CAM.1 or C-CAM.2.
[0124] III. Evaluation of electrochemical cells (single-layer pouch cells) A commercially available graphite coated tape from Elexcel Corporation Ltd. was used as the negative electrode. A single-layer pouch cell was fabricated using the positive electrode containing the above cathode active material, the negative electrode composite electrode, and a polypropylene separator (Celgard 2500 separator). Then, in an argon-filled glove box with oxygen and water levels below 1.0 ppm, 1 M LiPF in electrolyte (3:7 wt.% EC:DEC and 2 wt.% VC (DEC=diethyl carbonate, VC=vinylene carbonate) was added to the cell. 6 ) and subjected them to electrochemical testing in a Maccor 4000 battery test system.
[0125] III.1. Formation at 25°C The pouch cells prepared containing the above cathodes and graphite anodes were charged at a constant current of 0.1 C to a voltage of 4.25 V (CC charge). After degassing the cells, they were discharged at 0.1 C (3.0 V cutoff) (cycle 1). Immediately after, the cells were charged at a constant current of 0.1 C at 25° C. to a voltage of 4.25 V (CC) and discharged at 0.1 C (3.0 V cutoff) (cycle 2). The cells were then charged at a constant current of 0.5 C to a voltage of 4.25 V, charged at 4.25 V (CCCV) for 60 minutes or until the current was less than 0.02 C, and then the cells were discharged at a constant current of 0.5 C to a discharge voltage of 3 V (4 times, cycles 3-7). The cell was further cycled using the same charging conditions as in cycle 3, but with discharge voltages of 1C (twice, cycles 7-8), 2C (twice, cycles 9-10), and 3C (twice, cycles 11-12). Finally, the cell was charged and discharged 10 times following the same procedure used in cycle 3.
[0126] III.2. Evaluation of Pouch Cell Cycling at 45°C (cycling) and 25°C (resistance measurement) using 4.25V as the upper cut-off voltage Once the cell was formed as described above, it was charged at 25° C. at a constant current of 0.2 C to a voltage of 4.25 V, charged at 4.25 V (CCCV) for 60 minutes or until the current was less than 0.02 C, and then the cell was discharged at a constant current of 0.2 C to a discharge voltage of 3 V. This procedure was repeated once, and the discharge capacity was taken as the reference capacity for the next cycle. In this cycle, the cell was charged at a constant current of 0.2 C to 75% of the pre-determined reference capacity (75% state of charge = 75% SoC). Immediately after, a current pulse of 2.5 C was applied for 30 seconds to determine the cell resistance (cell resistance measurement). The cell was then discharged at a constant current of 0.2 C to 50% and 25% SoC, and the cell resistance measurement was repeated at each of these SoC values. The cell was then further discharged at a constant current of 0.2 C to 3.0 V.
[0127] Following the above cell resistance measurements, the cells were transferred to a climate chamber maintained at a constant temperature of 45°C. After an equilibration time of 12 hours, the cells were charged at a constant current of 1C to a voltage of 4.25V, charged at 4.25V (CCCV) for 60 minutes or until the current was less than 0.02C, and then the cells were discharged at a constant current of 1C to a discharge voltage of 3V (100 times). The entire sequence of steps above (resistance measurements at various SoC values at 25°C and 1C cycling at 45°C) was repeated at least five times. The results after 500 cycles at 1C and 45°C from the different examples are shown in Table 2 and expressed as a percentage of the values obtained at the beginning of the procedure.
[0128] The pouch cells of the present invention based on CAM.3 or CAM.4 outperformed the comparative pouch cells based on C-CAM.1 or C-CAM.2.
Claims
1. 1. A method for producing a partially coated electrode active material, the method comprising the steps of: (a) General formula Li 1+x T.M. 1-x O 2 providing an electrode active material according to the formula: wherein TM is a combination of Ni, Co, optionally Mn, and optionally at least one metal selected from Al, Ti, Mo, W, and Zr, x is in the range of 0 to 0.2, and at least 60 mole % of the transition metals in TM is Ni, said electrode active material having a residual moisture content in the range of 50 to 1,000 ppm; (b) treating the electrode active material with a metal alkoxide, metal halide, metal amide, or alkyl metal compound having at least one metal species selected from the group consisting of Ti, Zn, Zr, and Al; (c) treating the material obtained in step (b) with moisture; (d) repeating the series of steps (b) and (c) two to four times; Including, A method wherein in the final series of steps (b) and (c) the moisture is at least partially replaced by ozone.
2. TM is a compound represented by the general formula (I): (Ni a Co b Mn c ) 1-d M d (I) (wherein a is in the range of 0.6 to 0.95; b is in the range of 0.025 to 0.2; c is in the range of 0.025 to 0.2; d is in the range of 0 to 0.1; M is Al; a + b + c = 1) The method of claim 1, wherein the metal combination is
3. 3. The process according to claim 1 or 2, wherein step (b) is carried out in a rotary kiln, a free-fall mixer, a continuous vibrating bed or a fluidized bed.
4. 4. The process according to claim 1, wherein the alkylmetal compound in step (c) is selected from trimethylaluminum and triethylaluminum.
5. 5. The method of any one of claims 1 to 4, wherein each flush step between (b) and (c) has a duration in the range of 30 seconds to 1 hour.
6. 6. The process according to any one of claims 1 to 5, wherein steps (b) to (c) and (d) are carried out in a free-fall mixer.
7. The process according to any one of claims 1 to 5, wherein steps (b) to (c) and (d) are carried out in a fluidized bed.
8. TM is Ni 0.6 Co 0.2 Mn 0.2 , Ni 0.7 Co 0.2 Mn 0.1 , Ni 0.8 Co 0.1 Mn 0.1 and Ni 0.85 Co 0.1 Mn 0.05 The method according to any one of claims 1 to 7, wherein the compound is selected from the group consisting of
9. 9. The method according to any one of claims 1 to 8, wherein in the last series of steps (b) and (c) moisture is completely replaced by ozone.
10. 10. The method according to any one of claims 1 to 9, wherein the thickness of the layer formed by coating is in the range of 0.1 to 5 nm, said layer thickness representing an average thickness determined mathematically by calculating the amount of metal alkoxide or metal halide or metal amide or metal alkyl, respectively, per particle surface, assuming 100% conversion.
11. General formula Li 1+x T.M. 1-x O 2 wherein TM is a combination of Ni, Co, and further Mn, and optionally at least one metal selected from Al, Ti, Mo, W, and Zr, x is in the range of 0 to 0.2, and at least 60 mol % of the transition metals in TM is Ni, wherein an outer surface of the particulate electrode active material is coated with an acidic oxide selected from acidic aluminum oxyhydroxide and acidic alumina; A particulate electrode active material, wherein the thickness of the layer formed by coating on the outer surface of the particulate electrode active material is in the range of 0.1 to 5 nm, the thickness of the layer represents an average thickness determined mathematically by calculating the amount of acid aluminum oxyhydroxide and acid alumina per particle surface, respectively, assuming 100% conversion, and the surface of each particulate electrode active material is coated in the range of 50% to 99.99%.
12. TM is Ni 0.6 Co 0.2 Mn 0.2 , Ni 0.7 Co 0.2 Mn 0.1 and Ni 0.8 Co 0.1 Mn 0.1 12. The particulate electrode active material of claim 11, wherein the acidic oxide is selected from acidic aluminum oxyhydroxide and acidic alumina.
13. 13. Use of a particulate electrode active material according to claim 11 or 12 in or for the manufacture of a lithium ion battery.
Citation Information
Patent Citations
Method of producing cathode active material
JP2014222583A
Positive electrode active material, positive electrode for lithium ion secondary battery, and lithium ion secondary battery
JP2016136464A
Surface-modified cathode materials with an aqueous alumina sol and a method for preparing the same
KR100813014B1
Method for covering particles, especially a battery electrode material particles, and particles obtained with such method and a battery comprising such particle
US8993051B2
Nonaqueous electrolyte secondary battery and method for manufacturing same
WO2017159267A1