Conductive polymer dispersion and method for producing same, coating composition, and conductive laminate and method for producing same
A conductive polymer dispersion is produced through polymerization and ion exchange, addressing stability issues with PEDOT-PSS in water-soluble solvents, ensuring high conductivity and uniformity without high-pressure treatments.
Patent Information
- Application Number
- JP2021099854
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-06-16
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2041-06-16
AI Technical Summary
Conductive polymer dispersions containing π-conjugated conductive polymers, such as PEDOT-PSS, suffer from poor dispersion stability when mixed with water-soluble organic solvents, leading to reduced conductivity and wettability over time.
A method for producing a conductive polymer dispersion by polymerizing thiophene compounds in the presence of a polyanion using hydrogen persulfate as an oxidizing agent, followed by an ion exchange step, results in a low-viscosity dispersion that maintains stability even when mixed with water-soluble organic solvents.
The method produces a conductive polymer dispersion with improved dispersibility and conductivity, allowing for the formation of a uniform conductive layer without the need for high-pressure dispersion treatments, and maintains stability over time.
Smart Images

Figure 0007580343000001 
Figure 0007580343000002 
Figure 0007580343000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive polymer dispersion containing a π-conjugated conductive polymer and a method for producing the same, a coating composition, and a conductive laminate and a method for producing the same. [Background technology]
[0002] A conductive polymer dispersion containing a conductive complex in which a π-conjugated conductive polymer is doped with a polyanion may be used as a paint or a component thereof for forming a conductive layer. For example, poly(3,4-ethylenedioxythiophene), a π-conjugated conductive polymer, is difficult to disperse in water, but by doping it with polystyrene sulfonic acid to form PEDOT-PSS, the dispersibility in water is improved. Patent Document 1 discloses a technique for improving the hydrophilicity of a conductive complex and improving its reactivity to epoxy compounds by dispersing the conductive complex in water and leaving it for 180 days or more. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-31013 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the method of Patent Document 1, the conductive complex is reacted with an epoxy compound, and then dissolved in an organic solvent to form a paint, thereby improving the wettability of the conductive complex to a hydrophobic film substrate. On the other hand, when the conductive complex is not hydrophobized by reaction with an epoxy compound, a water-soluble organic solvent such as alcohol is usually added to the conductive polymer dispersion to improve the wettability of the conductive complex to a substrate such as a film. However, the dispersion stability of the conductive complex in the paint to which the water-soluble organic solvent is added is not necessarily high, and the dispersibility may decrease several tens of hours after the addition of the water-soluble organic solvent. The conductivity of the conductive layer formed by applying the paint with reduced dispersibility also decreases. For this reason, it is required to maintain the dispersibility of the conductive complex in the paint after the paint is obtained by adding a water-soluble organic solvent to the conductive polymer dispersion that has been subjected to a dispersion treatment.
[0005] The present inventors have conducted extensive research into a method for obtaining a conductive polymer dispersion having improved dispersibility of a conductive complex by devising a method for synthesizing a conductive complex so as to obtain a conductive polymer dispersion having a low viscosity at the stage of preparing the conductive polymer dispersion prior to preparing a coating composition (paint), and a method for producing a conductive polymer dispersion in which the decrease in dispersibility of the conductive complex over time is suppressed even after a water-soluble organic solvent is added to form a coating composition, and have completed the present invention.
[0006] The present invention provides a conductive polymer dispersion having excellent dispersion stability even when coexisting with a water-soluble organic solvent, and a method for producing the same. Also provided are a coating composition containing the conductive polymer dispersion, and a conductive laminate using the conductive polymer dispersion or the coating composition, and a method for producing the same. [Means for solving the problem]
[0007] [1] A method for producing a conductive polymer dispersion containing water and a conductive complex comprising a polythiophene-based conductive polymer and a polyanion, the method comprising the steps of: polymerizing a thiophene-based compound in an aqueous solvent in the presence of a polyanion; and using a hydrogen persulfate compound as an oxidizing agent in the polymerization step. [2] The method for producing a conductive polymer dispersion according to [1], wherein the hydrogen persulfate compound is potassium hydrogen persulfate or a double salt of potassium hydrogen persulfate, potassium hydrogen sulfate, and potassium sulfate. [3] The method for producing a conductive polymer dispersion according to [1] or [2], wherein in the polymerization step, polymerization is carried out under conditions such that a sum of the solid content weights of the thiophene compound and the polyanion is 2 parts by mass or more when the weight of the aqueous solvent is 100 parts by mass. [4] The method for producing a conductive polymer dispersion according to any one of [1] to [3], wherein in the polymerization step, an added amount of the hydrogen persulfate compound is 10 parts by mass or more and 100 parts by mass or less when a weight of the thiophene compound is 10 parts by mass. [5] The method for producing a conductive polymer dispersion according to any one of [1] to [4], wherein the polythiophene-based conductive polymer is poly(3,4-ethylenedioxythiophene) or the polyanion is polystyrenesulfonic acid. [6] The method for producing the conductive polymer dispersion according to any one of [1] to [5], further comprising an ion exchange step of contacting the conductive polymer dispersion obtained in the polymerization step with at least one of a cation exchange resin and an anion exchange resin. [7] A conductive polymer dispersion containing a conductive complex containing a polythiophene-based conductive polymer and a polyanion, and water, wherein when the content of the conductive complex is 1 mass% relative to the total mass of the conductive polymer dispersion, the conductive polymer dispersion has a viscosity of 20 mPa s or less at 23°C. [8] A coating composition comprising the conductive polymer dispersion according to [7] and a water-soluble organic solvent. [9] A method for producing a conductive laminate, comprising applying the conductive polymer dispersion according to [7] or the coating composition according to [8] to at least a part of a surface of a substrate.
[10] A conductive laminate comprising a substrate and a conductive layer formed on at least a portion of the surface of the substrate, the conductive layer being a cured layer of the conductive polymer dispersion according to [7] or the coating composition according to [8]. Effect of the Invention
[0008] According to the method for producing a conductive polymer dispersion of the present invention, a conductive polymer dispersion having a low viscosity can be produced without carrying out a high-pressure dispersion treatment using a high-pressure homogenizer or the like. The conductive polymer dispersion of the present invention exhibits a significantly lower viscosity than conventional products, and also exhibits excellent storage stability when mixed with a water-soluble organic solvent to form a coating composition. In the conductive laminate of the present invention, the conductive layer has excellent appearance. According to the method for producing a conductive laminate of the present invention, the above-mentioned conductive laminate can be easily produced.
[0009] This invention is believed to contribute to SDGs Goal 12, "Responsible Consumption and Production."
[0010] In this specification and claims, the lower limit and upper limit of a numerical range indicated with "to" are included in the numerical range. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] ≪Conductive polymer dispersion liquid≫ A first aspect of the present invention is a conductive polymer dispersion comprising water and a conductive complex containing a π-conjugated conductive polymer and a polyanion, wherein when the content of the conductive complex is 1 mass % relative to the total mass of the conductive polymer dispersion, the conductive polymer dispersion has a viscosity of 20 mPa s or less at 23°C.
[0012] [Conductive composite] The conductive complex contained in the conductive polymer dispersion of this embodiment contains a polythiophene-based conductive polymer and a polyanion. The polyanion in the conductive complex is doped into the polythiophene-based conductive polymer to form a conductive complex having electrical conductivity.
[0013] (Polythiophene-based conductive polymer) The main chain of the polythiophene-based conductive polymer constitutes a π-conjugated system by polymerization of a thiophene-based compound. Polythiophene-based conductive polymers include polythiophene, poly(3-methylthiophene), poly(3-ethylthiophene), poly(3-propylthiophene), poly(3-butylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3-bromothiophene), poly(3-chlorothiophene), and poly(3-iodothiophene). thiophene), poly(3-cyanothiophene), poly(3-phenylthiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), oxythiophene), poly(3-octadecyloxythiophene), poly(3,4-dihydroxythiophene), poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-di dodecyloxythiophene), poly(3,4-ethylenedioxythiophene), poly(3,4-propylenedioxythiophene), poly(3,4-butylenedioxythiophene), poly(3-methyl-4-methoxythiophene), poly(3-methyl-4-ethoxythiophene), poly(3-carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4-carboxyethylthiophene), and poly(3-methyl-4-carboxybutylthiophene). Among these polythiophene-based conductive polymers, poly(3,4-ethylenedioxythiophene) is particularly preferred because of its excellent conductivity, transparency, and heat resistance. The polythiophene-based conductive polymer contained in the conductive composite may be of one type or of two or more types.
[0014] (Polyanion) A polyanion is a polymer having two or more monomer units each having an anionic group in the molecule. The anionic group of the polyanion functions as a dopant for a polythiophene-based conductive polymer, improving the conductivity of the polythiophene-based conductive polymer. The anion group of the polyanion is preferably a sulfo group or a carboxy group. Specific examples of such polyanions include polymers having a sulfo group, such as polystyrene sulfonic acid, polyvinyl sulfonic acid, polyallyl sulfonic acid, polyacrylic acid esters having a sulfo group, polymethacrylic acid esters having a sulfo group (for example, poly(4-sulfobutyl methacrylate, polysulfoethyl methacrylate, polymethacryloyloxybenzenesulfonic acid), poly(2-acrylamido-2-methylpropanesulfonic acid), and polyisoprene sulfonic acid; and polymers having a carboxy group, such as polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacrylic acid, polymethacrylic acid, poly(2-acrylamido-2-methylpropanecarboxylic acid), and polyisoprene carboxylic acid. The polyanion may be a homopolymer in which a single monomer is polymerized, or a copolymer in which two or more monomers are polymerized. Among these polyanions, polymers having a sulfo group are preferred, and polystyrene sulfonic acid is more preferred, since they can provide higher electrical conductivity. The polyanions may be used alone or in combination of two or more kinds.
[0015] The weight average molecular weight Mw of the polyanion is preferably 20,000 or more and 1,000,000 or less, and more preferably 50,000 or more and 800,000 or less. When the weight average molecular weight Mw is within the above preferred range, the dispersion stability of the conductive composite in the conductive polymer dispersion of this embodiment and in the coating material of the second embodiment described below is further improved. The weight average molecular weight Mw is an average molecular weight based on mass measured by gel filtration chromatography and calculated as pullulan.
[0016] In the polyanion doped into the polythiophene conductive polymer, some of the anion groups are not doped into the polythiophene conductive polymer and have excess anion groups that are not involved in the doping. Since these excess anion groups are hydrophilic groups, the conductive composite has high water dispersibility and low organic solvent dispersibility. When the number of all anionic groups in the polyanion is taken as 100 mol %, the excess anionic groups are preferably from 30 mol % to 90 mol %, more preferably from 45 mol % to 75 mol %.
[0017] The content of the polyanion in the conductive complex is preferably in the range of 1 part by mass to 1000 parts by mass, more preferably 10 parts by mass to 700 parts by mass, and even more preferably 100 parts by mass to 500 parts by mass, per 100 parts by mass of the polythiophene-based conductive polymer. If the content of the polyanion is equal to or higher than the lower limit, the doping effect on the polythiophene-based conductive polymer tends to be stronger, and the conductivity becomes higher. On the other hand, if the content of the polyanion is equal to or lower than the upper limit, the polythiophene-based conductive polymer can be sufficiently contained, so that sufficient conductivity can be ensured.
[0018] The content of the conductive complex relative to the total mass of the conductive polymer dispersion of this embodiment is preferably from 0.01 to 5.0 mass%, more preferably from 1.0 to 4.0 mass%, and even more preferably from 2.0 to 3.0 mass%. When the content is at least as high as the lower limit of the above range, the conductivity of the conductive layer formed by applying the conductive polymer dispersion can be further improved. When it is equal to or less than the upper limit of the above range, the dispersibility of the conductive complex in the conductive polymer dispersion can be improved, and a uniform conductive layer can be formed.
[0019] The viscosity of the conductive polymer dispersion of this embodiment at 23° C. is 20 mPa s or less, preferably 15 mPa s or less, more preferably 10 mPa s or less, and even more preferably 5 mPa s or less, when the concentration of the conductive complex relative to the total mass of the conductive polymer dispersion is adjusted to 1.0 mass %. There is no particular restriction on the lower limit of the viscosity, and a guideline is 0.1 mPa s or more. Within the above preferred range, it is easy to bring the conductive polymer dispersion into contact with an ion exchange resin, and it is also easy to separate the ion exchange resin after contact. Furthermore, the above low viscosity correlates with high dispersibility of the conductive complex in the conductive polymer dispersion. The conductive polymer dispersion having the above low viscosity does not require high-pressure dispersion treatment using a high-pressure homogenizer or the like, and the conductive layer formed by coating the substrate has excellent conductivity and transparency. In measuring the viscosity, the conductive polymer dispersion preferably contains only ion-exchanged water as a dispersion medium, and preferably does not contain any additives other than the conductive complex. The viscosity was measured at 23° C. using a tuning fork vibration viscometer in accordance with JIS Z8803:2011 (viscosity measurement method using a vibration viscometer).
[0020] <Coating composition (paint)> A second aspect of the present invention is a coating composition comprising the conductive polymer dispersion of the first aspect and a water-soluble organic solvent. In the coating composition of this aspect, the conductive complex is in a dispersed state.
[0021] The coating composition of this embodiment contains water and a water-soluble organic solvent. The mixture of water and the water-soluble organic solvent is sometimes called an aqueous dispersion medium.
[0022] A water-soluble organic solvent is an organic solvent that dissolves in an amount of 1 g or more in 100 g of water at 20°C. Examples of the water-soluble organic solvent include alcohol-based solvents, ether-based solvents, ketone-based solvents, nitrogen atom-containing solvents, and ester-based solvents. Examples of alcohol-based solvents include methanol, ethanol, 1-propanol, 2-propanol (isopropanol), 2-methyl-2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, allyl alcohol, ethylene glycol, propylene glycol, propylene glycol monomethyl ether, and ethylene glycol monomethyl ether. Examples of the ether solvent include diethyl ether, dimethyl ether, propylene glycol dialkyl ether, and diethylene glycol diethyl ether. Examples of the ketone solvent include diethyl ketone, methyl propyl ketone, methyl butyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, methyl amyl ketone, diisopropyl ketone, methyl ethyl ketone, acetone, and diacetone alcohol. Examples of the nitrogen atom-containing solvent include N-methylpyrrolidone, dimethylacetamide, and dimethylformamide. The water-soluble organic solvent may be contained alone or in combination of two or more kinds. In order to improve the applicability of the coating composition of this embodiment to a substrate, the water-soluble organic solvent is preferably an alcohol-based solvent or a ketone-based solvent, and more preferably an alcohol-based solvent.
[0023] The content of the water-soluble organic solvent relative to the total mass of the aqueous dispersion medium is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more. The content of the water-soluble organic solvent is preferably 90% by mass or less. When the content is within the above preferred range, the wettability to the substrate can be improved while suppressing deterioration over time of the dispersion stability of the conductive composite in the coating composition of this embodiment.
[0024] The water content relative to the total mass of the aqueous dispersion medium is preferably 70 mass% or less, more preferably 60 mass% or less, and even more preferably 50 mass% or less. From the viewpoint of improving the dispersibility of the conductive composite, the water content is preferably 10 mass% or more. When the content is within the above preferred range, the wettability to the substrate can be improved while suppressing deterioration over time of the dispersion stability of the conductive composite in the coating composition of this embodiment.
[0025] The content of the conductive complex relative to the total mass of the coating composition of this embodiment is, for example, preferably 0.01 mass% or more and 4 mass% or less, more preferably 0.1 mass% or more and 3 mass% or less, even more preferably 0.2 mass% or more and 2 mass% or less, and particularly preferably 0.3 mass% or more and 1 mass% or less. When the content is within the above preferred range, a decrease in the dispersion stability of the conductive composite in the coating composition of this embodiment can be suppressed, and a conductive layer with good conductivity can be formed by applying the composition to a substrate.
[0026] <Binder components> The coating composition of this embodiment may contain a binder component. The binder component is a resin other than the polythiophene-based conductive polymer and the polyanion or a precursor thereof, and is a thermoplastic resin, or a curable monomer or oligomer that is cured when the conductive layer is formed. The thermoplastic resin becomes the binder resin as it is, and the curable monomer or oligomer becomes the resin formed by curing becomes the binder resin. The binder component may be one type only, or two or more types may be included.
[0027] Specific examples of binder resins derived from binder components include acrylic resins (acrylic compounds), polyester resins, polyurethane resins, polyimide resins, polyether resins, melamine resins, and silicones. The binder resin contained in the coating composition of this embodiment is preferably a water-dispersible resin, more preferably a water-dispersible emulsion resin. The water-dispersible resin is an emulsion resin or a water-soluble resin.
[0028] Specific examples of water-dispersible emulsion resins include acrylic resins (acrylic compounds), polyester resins, polyurethane resins, polyimide resins, melamine resins, etc., which are emulsionized with an emulsifier. Among them, polyester emulsions are preferred because the strength of the coating film formed by applying the coating composition of this embodiment to a substrate is high. In particular, polyester emulsions are preferred because the adhesion of the coating film to the substrate is high when the composition is applied to a polyester film substrate.
[0029] Specific examples of the water-soluble resin include acrylic resin (acrylic compound), polyester resin, polyurethane resin, polyimide resin, and melamine resin, which have an acid group such as a carboxy group or a sulfo group or a salt thereof. Here, the water-soluble resin is preferably one that dissolves in an amount of 1 g or more, preferably 5 g or more, and more preferably 10 g or more in 100 g of distilled water at 25° C.
[0030] The acid group, such as a carboxy group or a sulfo group, contained in the water-dispersible resin may form a salt with a cation, such as a sodium ion or a potassium ion.
[0031] The curable monomer or oligomer may be a thermosetting monomer or oligomer, or a photocurable monomer or oligomer. Here, the oligomer refers to a polymer having a mass average molecular weight of less than 10,000. Note that a polymer having a mass average molecular weight of more than 10,000 does not have curability. Examples of the curable monomer include an acrylic monomer (acrylic compound), an epoxy monomer, an organosiloxane, etc. Examples of the curable oligomer include an acrylic oligomer (acrylic compound), an epoxy oligomer, a silicone oligomer (curable silicone), etc. When an acrylic monomer or an acrylic oligomer is used as the binder component, it can be easily cured by heating or light irradiation. When an organosiloxane or a silicone oligomer is used as the binder component, it is possible to impart releasability (non-adhesiveness) to the conductive layer.
[0032] When the composition contains a curable monomer or oligomer, it is preferable to further contain a curing catalyst. For example, when the composition contains a thermosetting monomer or oligomer, it is preferable to contain a thermal polymerization initiator that generates radicals by heating, and when the composition contains a photocurable monomer or oligomer, it is preferable to contain a photopolymerization initiator that generates radicals by light irradiation. In addition, when the composition contains an organosiloxane or silicone oligomer, it is preferable to contain a platinum catalyst for curing.
[0033] The content of the binder component in the coating composition of this embodiment is preferably 100 parts by mass or more and 20,000 parts by mass or less, and more preferably 100 parts by mass or more and 5,000 parts by mass or less, relative to 100 parts by mass of the conductive composite. When the content is equal to or greater than the lower limit of the above range, the film-forming properties and film strength can be improved when the coating composition of this embodiment is applied to a substrate. When the content is equal to or less than the upper limit of the above range, a decrease in electrical conductivity due to a decrease in the content ratio of the conductive complex can be suppressed.
[0034] (Other additives) The coating composition and the conductive polymer dispersion may contain other known additives. Examples of the additives that can be used include surfactants, inorganic conductive agents, antifoaming agents, coupling agents, antioxidants, and ultraviolet absorbing agents. The surfactant may be a nonionic, anionic or cationic surfactant, with the nonionic surfactant being preferred from the standpoint of storage stability. A polymer surfactant such as polyvinylpyrrolidone may also be added. Examples of the inorganic conductive agent include metal ions, conductive carbon, etc. Metal ions can be generated by dissolving a metal salt in water. The antifoaming agent includes silicone resin, polydimethylsiloxane, silicone oil, and the like. The coupling agent may be a silane coupling agent having a vinyl group or an amino group. Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, oxanilide-based ultraviolet absorbers, hindered amine-based ultraviolet absorbers, and benzoate-based ultraviolet absorbers. When the above-mentioned additives are contained, the content ratio is appropriately determined depending on the type of additive, but can be, for example, in the range of 0.001 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the conductive composite.
[0035] The coating composition of this embodiment can be produced by appropriately adding water, a water-soluble organic solvent, a binder component, other additives, and the like to the conductive polymer dispersion of the first embodiment and mixing them in a conventional manner.
[0036] <Method for producing conductive polymer dispersion> A third aspect of the present invention is a method for producing a conductive polymer dispersion containing water and a conductive complex containing a polythiophene-based conductive polymer and a polyanion, the method including a polymerization step of polymerizing a thiophene-based compound in an aqueous solvent in the presence of a polyanion, and a hydrogen persulfate compound is used as an oxidizing agent in the polymerization step.
[0037] An aqueous solution (reaction solution) containing a thiophene-based compound as a monomer and a polyanion at an arbitrary content ratio is prepared, and the thiophene-based compound is polymerized by the action of a hydrogen persulfate compound to form a polythiophene-based conductive polymer. In the reaction solution, the polythiophene-based conductive polymer is naturally doped with the polyanion, and a conductive complex consisting of the polythiophene-based conductive polymer and the polyanion is formed. The content ratio (mass basis) of the polythiophene-based conductive polymer:polyanion contained in the formed conductive complex is the same as the content ratio of the thiophene-based compound contained in the reaction solution immediately before the start of polymerization to the content of the polyanion. In other words, the content ratio of the monomer and polyanion blended in the reaction solution is reflected in the content ratio of the polythiophene-based conductive polymer and the polyanion in the formed conductive complex.
[0038] The content ratio of the thiophene compound to the polyanion in the reaction solution immediately before the start of polymerization is preferably from (1:2) to (1:5) by mass, more preferably from (1:2) to (1:4.5), and even more preferably from (1:3) to (1:4). When the content is within the above range, the conductive polymer dispersion liquid of the first embodiment described above can be easily formed.
[0039] In the polymerization step, it is desirable to carry out the polymerization under conditions in which the sum of the solid weights of the thiophene compound and the polyanion is preferably 2 parts by mass or more, more preferably 3 parts by mass or more, and even more preferably 3.5 parts by mass or more, when the weight of the aqueous solvent is 100 parts by mass. The upper limit of the sum is, for example, 7 parts by mass. When polymerization is carried out within the above preferred range, there is an advantage that the resulting conductive polymer has good electrical conductivity.
[0040] The hydrogen persulfate compound, which is the oxidizing agent, is, for example, a compound containing the general formula: MHSO5 (M represents any alkali metal such as Na or K), and may be a double salt. The hydrogen persulfate compound is preferably potassium hydrogen persulfate (also known as potassium monopersulfate or potassium peroxymonosulfate) or a double salt of potassium hydrogen persulfate, potassium hydrogen sulfate, and potassium sulfate (chemical formula: 2KHSO5·KHSO4·K2SO4). The above suitable compounds make it easier to form a low-viscosity, highly dispersed conductive polymer dispersion.
[0041] In the reaction liquid, when the weight of the thiophene compound is 10 parts by mass, the total amount of the hydrogen persulfate compounds added is preferably 10 parts by mass or more and 100 parts by mass or less, more preferably 20 parts by mass or more and 80 parts by mass or less, and even more preferably 30 parts by mass or more and 70 parts by mass or less. When the amount is in the above preferred range, a conductive polymer dispersion liquid with low viscosity and high dispersion can be more easily formed.
[0042] A catalyst may be added to the reaction solution. The catalyst is not particularly limited as long as it promotes the polymerization of the thiophene compound, and examples of the catalyst include transition metal compounds such as ferric chloride, ferric sulfate, ferric nitrate, and cupric chloride. Among them, it is preferable to use a catalyst containing iron, since the polymerization proceeds stably at room temperature.
[0043] The content of the catalyst added to the reaction liquid is, for example, preferably 0.001% by mass or more and 2% by mass or less, more preferably 0.005% by mass or more and 1% by mass or less, and even more preferably 0.01% by mass or more and 0.5% by mass or less, relative to the total mass of the reaction liquid. When the amount is within the above range, the polymerization reaction can proceed stably, so that the formation of a complex with the polyanion present in the reaction system proceeds stably, and a conductive complex with good conductivity can be easily obtained.
[0044] The explanation of the polyanion contained in the reaction solution is the same as that of the polyanion in the first embodiment, and therefore a duplicated explanation will be omitted.
[0045] Specific examples of the thiophene-based compound contained in the reaction liquid include compounds that form the monomer units of the polythiophene-based conductive polymer of the first embodiment.
[0046] The conductive polymer dispersion of the first embodiment can be obtained by the above method. Since the conductive composite formed after the polymerization reaction has excellent dispersibility, there is no need for high-pressure dispersion treatment using a high-pressure homogenizer or dispersion treatment using a high-output dispersion device for reducing the diameter of fine particles.
[0047] Before using the conductive polymer dispersion, the catalyst and oxidizing agent added to the reaction liquid may be removed. Examples of the removal method include a method of contacting the conductive polymer dispersion with an ion exchange resin to adsorb the catalyst and oxidizing agent to the ion exchange resin, and a method of ultrafiltrating the conductive polymer dispersion to remove the catalyst and oxidizing agent while replacing the dispersion medium. Among these, the method of using an ion exchange resin is preferable because it is simple. It is preferable to use a cation exchange resin and an anion exchange resin in combination as the ion exchange resin.
[0048] <Conductive laminate> A third aspect of the present invention is a conductive laminate comprising a substrate and a conductive layer formed on at least a partial surface of the substrate, the conductive layer being a cured layer of the conductive polymer dispersion of the first aspect or the coating composition of the second aspect.
[0049] [Conductive layer] The conductive layer may be formed over the entire surface of any surface of the substrate, or over a portion of the entire surface. In the conductive film, it is preferable that a conductive layer of substantially uniform thickness is formed over substantially the entire surface of one surface or the other surface of the film substrate. When a conductive layer is formed only over a portion of the surface of the substrate, the conductive layer may be, for example, a fine conductive pattern such as a circuit or an electrode, or the conductive layer may be provided on the same surface and the conductive layer may be not provided on the same surface and may be roughly divided.
[0050] The average thickness of the conductive layer is, for example, preferably 10 nm or more and 100 μm or less, more preferably 20 nm or more and 50 μm or less, and even more preferably 30 nm or more and 30 μm or less. When the average thickness of the conductive layer is equal to or greater than the lower limit, high conductivity can be exhibited, and when the average thickness is equal to or less than the upper limit, the adhesion of the conductive layer to the substrate is further improved.
[0051] [Base material] The substrate may be a substrate made of an insulating material or a substrate made of a conductive material. The shape of the substrate is not particularly limited, and examples thereof include a shape mainly having a flat surface, such as a film or a substrate. Examples of insulating materials include glass, synthetic resin, and ceramics. The conductive material may be a metal, a conductive metal oxide, carbon, or the like.
[0052] (Film substrate) When a film substrate is used as the substrate, the conductive laminate becomes a conductive film. The film substrate may be, for example, a plastic film made of a synthetic resin, such as ethylene-methyl methacrylate copolymer resin, ethylene-vinyl acetate copolymer resin, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyacrylate, polycarbonate, polyvinylidene fluoride, polyarylate, styrene-based elastomer, polyester-based elastomer, polyethersulfone, polyetherimide, polyetheretherketone, polyphenylene sulfide, polyimide, cellulose triacetate, and cellulose acetate propionate. From the viewpoint of improving the adhesion between the film substrate and the conductive layer, the synthetic resin for the film substrate is preferably a polyester resin, and among these, polyethylene terephthalate is preferable.
[0053] The synthetic resin for the film substrate may be either amorphous or crystalline. The film substrate may be either unstretched or stretched. The film substrate may be subjected to a surface treatment such as a corona discharge treatment, a plasma treatment, or a flame treatment in order to further improve the adhesion of the conductive layer.
[0054] The average thickness of the film substrate is preferably 5 μm to 500 μm, more preferably 20 μm to 200 μm. If the average thickness of the film substrate is equal to or more than the lower limit, the film is less likely to break, and if the average thickness is equal to or less than the upper limit, the film can have sufficient flexibility. The average thickness of the film substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.
[0055] (Glass substrate) Examples of the glass substrate include an alkali-free glass substrate, a soda-lime glass substrate, a borosilicate glass substrate, and a quartz glass substrate. If the substrate contains an alkali component, the conductivity of the conductive layer tends to decrease, so among the above glass substrates, an alkali-free glass is preferred. Here, the alkali-free glass refers to a glass composition in which the content of the alkali component is 0.1 mass% or less with respect to the total mass of the glass composition.
[0056] The average thickness of the glass substrate is preferably from 100 μm to 3000 μm, more preferably from 100 μm to 1000 μm. If the average thickness of the glass substrate is equal to or more than the lower limit, the substrate is less likely to break, and if the average thickness is equal to or less than the upper limit, the substrate can contribute to a thinner conductive laminate. The average thickness of the glass substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.
[0057] <Method for manufacturing conductive laminate> A fourth aspect of the present invention is a method for producing a conductive laminate, the method comprising applying the conductive polymer dispersion of the first aspect or the coating composition of the second aspect to at least a part of the surface of a substrate to form a conductive layer. The conductive laminate of the third aspect can be produced by the production method of this aspect.
[0058] Examples of a method for applying (coating) the conductive polymer dispersion or coating composition to any surface of a substrate include a method using a coater such as a gravure coater, a roll coater, a curtain flow coater, a spin coater, a bar coater, a reverse coater, a kiss coater, a fountain coater, a rod coater, an air doctor coater, a knife coater, a blade coater, a cast coater, or a screen coater; a method using a sprayer such as an air spray, an airless spray, or a rotor dampening; and an immersion method such as dipping.
[0059] The amount of conductive polymer dispersion or coating composition applied to the substrate is not particularly limited, but taking into consideration uniform and even application, conductivity, and film strength, it is preferable to apply the conductive polymer dispersion or coating composition in an amount of 0.01 g / m2 or less in terms of solid content. 2 More than 10.0g / m 2 The following ranges are preferred:
[0060] A coating film made of a conductive polymer dispersion or a coating composition applied onto a substrate is dried to remove at least a portion of the dispersion medium, and then cured to form a conductive layer. Methods for drying the coating film include heat drying, vacuum drying, etc. Examples of heat drying that can be used include hot air heating and infrared heating. When applying heat drying, the heating temperature is appropriately set depending on the dispersion medium used, but is usually within the range of 50° C. to 200° C. Here, the heating temperature is the set temperature of the drying device. A suitable drying time within the above heating temperature range is preferably 0.5 minutes to 30 minutes, more preferably 1 minute to 15 minutes. EXAMPLES
[0061] [Preparation of polyanions] As a raw material, an aqueous solution (concentration: 25-30%) of poly(sodium 4-styrenesulfonate) having a weight average molecular weight of 70,000 to 200,000 manufactured by Sigma-Aldrich Corporation or a powder having a weight average molecular weight of 800,000 was used. First, ion-exchanged water was added to a powder or aqueous solution of poly(sodium 4-styrenesulfonate) to adjust it to a uniform aqueous solution with a solid concentration of 15 wt%, and cation-exchange resin was added until the pH became less than 1. After that, the cation-exchange resin was filtered off using a stainless steel mesh filter, and the solid concentration was adjusted to 10 wt% with ion-exchanged water to obtain an aqueous solution of polystyrenesulfonic acid (PSS). The weight-average molecular weight of PSS was measured using a high performance liquid gel filtration chromatography system with pullulan as the standard substance.
[0062] [Preparation of thiophene compounds] Commercially available 3,4-ethylenedioxythiophene (Tokyo Chemical Industry Co., Ltd.) was purchased and purified by vacuum distillation before use in the reaction.
[0063] [Example 1] 360g of ion-exchanged water for dilution and 1.0g of ferric sulfate (Tokyo Chemical Industry Co., Ltd.) were added to 137g of poly(4-styrenesulfonic acid) aqueous solution with a solid content concentration of 10wt% and a weight average molecular weight of 200,000, and the solution was bubbled with nitrogen at a flow rate of 1L per minute for 10 minutes, stirred under a nitrogen atmosphere, and maintained at 25°C. 3.5g of 3,4-ethylenedioxythiophene, which had been distilled and purified, was added to this aqueous solution. Next, 15.3g of oxone (a triple salt of potassium hydrogen persulfate, potassium sulfate, and potassium hydrogen sulfate, chemical formula 2KHSO5·KHSO4·K2SO4, Fujifilm Wako Pure Chemical Industries, Ltd.), a persulfate compound, was added as an oxidizing agent, and the mixture was stirred and reacted at 25°C for 30 minutes under a nitrogen atmosphere to synthesize PEDOT-PSS. In this reaction, the sum of the solid weights of the thiophene compound and the polyanion was 3.6 parts by mass when the weight of the water solvent was 100 parts by mass. 60 g of cation exchange resin and 60 g of anion exchange resin were added to the reaction solution, stirred for 5 minutes, and then allowed to stand for 2 hours. The ion exchange resin was filtered off using a stainless steel mesh filter to obtain a conductive polymer dispersion containing an aqueous dispersion medium and PEDOT-PSS with a solid content concentration of 2.7 wt%.
[0064] [Example 2] A conductive polymer dispersion was obtained in the same manner as in Example 1, except that 137 g of an aqueous poly(4-styrenesulfonic acid) solution having a solid content concentration of 10 wt% and a weight average molecular weight of 800,000 was used and the amount of ion-exchanged water for dilution was changed to 565 g. When the weight of the water solvent during the reaction was taken as 100 parts by mass, the sum of the solid content weights of the thiophene compound and polyanion was 2.5 parts by mass, and the solid content concentration of the conductive polymer dispersion was 2.1 wt%.
[0065] [Example 3] A conductive polymer dispersion was obtained in the same manner as in Example 1, except that 81 g of an aqueous poly(4-styrenesulfonic acid) solution with a solid content concentration of 10 wt% and a weight average molecular weight of 200,000 was used, the amount of ion-exchanged water for dilution was changed to 159 g, and the reaction temperature was changed to 10° C. When the weight of the aqueous solvent during the reaction was taken as 100 parts by mass, the sum of the solid content weights of the thiophene compound and polyanion was 5.0 parts by mass, and the solid content concentration of the conductive polymer dispersion was 3.6 wt%.
[0066] [Example 4] A conductive polymer dispersion was obtained in the same manner as in Example 1, except that 81 g of an aqueous poly(4-styrenesulfonic acid) solution with a solid content concentration of 10 wt% and a weight average molecular weight of 70,000 was used, the amount of ion-exchanged water for dilution was changed to 307 g, and 7.7 g of oxone and 3.0 g of sodium persulfate were used as the oxidizing agents. When the weight of the aqueous solvent during the reaction was taken as 100 parts by mass, the sum of the solid content weights of the thiophene compound and polyanion was 3.1 parts by mass, and the solid content concentration of the conductive polymer dispersion was 2.2 wt%.
[0067] [Example 5] A conductive polymer dispersion was obtained in the same manner as in Example 1, except that the amount of ion-exchanged water for dilution was changed to 1440 g, the reaction time was changed to 90 minutes, and a step of vacuum concentration was added after filtering out the ion-exchange resin. When the weight of the water solvent during the reaction was taken as 100 parts by mass, the sum of the solid weights of the thiophene compound and polyanion was 1.1 parts by mass, and the solid concentration of the conductive polymer dispersion was 2.0 wt%.
[0068] [Comparative Example 1] Except for using 3.0 g of sodium persulfate as the oxidizing agent, a conductive polymer dispersion was obtained in the same manner as in Example 1. When the weight of the aqueous solvent during the reaction was taken as 100 parts by mass, the sum of the solid content weights of the thiophene compound and the polyanion was 3.6 parts by mass, and the solid content concentration of the conductive polymer dispersion was 2.6 wt%.
[0069] [Comparative Example 2] The conductive polymer dispersion obtained in Comparative Example 1 was subjected to a dispersion treatment using a high-pressure wet-type atomizer to obtain a conductive polymer dispersion with a reduced viscosity.
[0070] [Comparative Example 3] The reaction was carried out in the same manner as in Example 2, except that 3.0 g of sodium persulfate was used as the oxidizing agent, but the reaction solution became highly viscous and gelled. The ion exchange step could not be carried out, and a conductive polymer dispersion could not be obtained.
[0071] <Evaluation of Viscosity> The viscosity at 23°C of the conductive polymer dispersions obtained in Examples 1 to 5 and Comparative Examples 1 and 2 was measured using a vibration viscometer. Furthermore, the viscosity was also measured in the same manner when ion-exchanged water was added to adjust the solid content concentration to 1 wt%. The results are shown in Table 1. The above viscosity is a value measured at 23° C. using a tuning fork vibration viscometer in accordance with JIS Z8803:2011 (viscosity measurement method using a vibration viscometer).
[0072] [Table 1]
[0073] <Evaluation of electrical conductivity> The conductive polymer dispersions obtained in Examples 1 to 5 and Comparative Examples 1 to 2 were adjusted with ion-exchanged water so that the solid content concentration was 1 wt%. 0.01 g of an acetylene-based surfactant (Surfynol 420, manufactured by Nissin Chemical Industry Co., Ltd.) and 50 g of methanol were added to 50 g of this conductive polymer dispersion and thoroughly mixed to obtain a coating composition (paint). This paint was applied to a polyethylene terephthalate film (Lumirror T60, manufactured by Toray Industries, Inc.) using a bar coater with a wet film thickness of 16 μm, and heated and dried at a drying temperature of 100° C. for 1 minute to obtain a conductive film. The surface resistance value of the obtained conductive film was measured using a resistivity meter (Hiresta, manufactured by Nitto Seiko Analytech Co., Ltd.) under the condition of an applied voltage of 10 V. In addition, the appearance of the conductive film was visually evaluated. The results are shown in Table 2.
[0074] [Table 2]
[0075] <Evaluation of dispersion stability> The conductive polymer dispersions obtained in Examples 1 to 5 and Comparative Examples 1 and 2 were each adjusted with ion-exchanged water so that the solid content concentration was 1 wt%. 50 g of this conductive polymer dispersion was added to and mixed with 50 g of 2-propanol to obtain a coating composition (paint). When the state of the paint was observed after storage at 40°C for 10 days, the paints of Examples 1 to 5 showed no change even after storage and had high dispersion stability. On the other hand, the paints of Comparative Examples 1 to 2 solidified into a gel and had low dispersion stability.
Claims
1. A method for producing a conductive polymer dispersion containing a conductive complex including a polythiophene-based conductive polymer and a polyanion, and water, the method comprising the steps of: polymerizing a thiophene-based compound in an aqueous solvent in the presence of a polyanion; The method for producing a conductive polymer dispersion, wherein a hydrogen persulfate compound is used as an oxidizing agent in the polymerization step.
2. 2. The method for producing a conductive polymer dispersion according to claim 1, wherein the hydrogen persulfate compound is potassium hydrogen persulfate or a double salt composed of potassium hydrogen persulfate, potassium hydrogen sulfate, and potassium sulfate.
3. 3. The method for producing a conductive polymer dispersion according to claim 1, wherein in the polymerization step, polymerization is performed under conditions such that a sum of a solid content weight of the thiophene compound and the polyanion is 2 parts by mass or more when a weight of the aqueous solvent is 100 parts by mass.
4. 4. The method for producing a conductive polymer dispersion according to claim 1, wherein in the polymerization step, an added amount of the hydrogen persulfate compound is 10 parts by mass or more and 100 parts by mass or less when a weight of the thiophene-based compound is 10 parts by mass.
5. 5. The method for producing a conductive polymer dispersion according to claim 1, wherein the polythiophene-based conductive polymer is poly(3,4-ethylenedioxythiophene), or the polyanion is polystyrenesulfonic acid.
6. The method for producing the conductive polymer dispersion according to any one of claims 1 to 5, further comprising an ion exchange step of contacting the conductive polymer dispersion obtained in the polymerization step with at least one of a cation exchange resin and an anion exchange resin.
7. A conductive polymer dispersion liquid containing a conductive complex containing a polythiophene-based conductive polymer and a polyanion, and water, A conductive polymer dispersion having a viscosity of 20 mPa·s or less at 23° C. when the content of the conductive complex with respect to the total mass of the conductive polymer dispersion is 1 mass %, when a dispersion medium of the conductive polymer dispersion is only ion-exchanged water, and when the conductive polymer dispersion does not contain any additives other than the conductive complex. (However, this does not include the case where the conductive complex contains a dopant polymer consisting of a copolymer containing a repeating unit a represented by the following general formula (1) and one or more repeating units b selected from the repeating units represented by the following general formulas (2-1) to (2-7). 【Chemistry 1】 [In the formula, R 1 is a hydrogen atom or a methyl group, Z is a phenylene group, a naphthylene group, or an ester group, if Z is a phenylene group or a naphthylene group, R 2 is a straight-chain, branched or cyclic hydrocarbon group having 1 to 12 carbon atoms which may have a single bond, an ester group, or an ether group, or both, and if Z is an ester group, R 2 is a single bond, or a straight-chain, branched or cyclic hydrocarbon group having 1 to 12 carbon atoms which may have an ether group, or both, and m is 1 to 3. R 3 , R 5 , R 7 , R 10 , R 12 , R 13 and R 15 are each independently a hydrogen atom or a methyl group, and R 4 , R 6 , R 8 , R 11 and R 14 are each independently a straight-chain, branched or cyclic hydrocarbon group having 1 to 12 carbon atoms which may have either a single bond, an ether group or an ester group or both. R 9 is a straight-chain or branched alkylene group having 1 to 4 carbon atoms, and one or two of the hydrogen atoms in R 9 may be substituted with a fluorine atom. X 1 , X 2 , X 3 , X 4 , X 6 and X 7 are each independently a single bond, a phenylene group, a naphthylene group, an ether group, an ester group or an amide group, and X 5 is a single bond, an ether group or an ester group. Y represents an ether group, an ester group, an amino group, or an amide group, and the amino group and the amide group may contain a hydrogen atom, or a linear, branched, or cyclic hydrocarbon group having 1 to 12 carbon atoms which may contain a heteroatom. Rf 1 is a fluorine atom or a trifluoromethyl group, Rf 2 and Rf 3 are a linear or branched alkyl group having 1 to 4 carbon atoms and at least one fluorine atom, or a phenyl group substituted with a fluorine atom or a trifluoromethyl group, and n is an integer from 1 to 4. a, b1, b2, b3, b4, b5, b6, and b7 are 0<a<1.0, 0≦b1<1.0, 0≦b2<1.0, 0≦b3<1.0, 0≦b4<1.0, 0≦b5<1.0, 0≦b6<1.0, 0≦b7<1.0, and 0<b1+b2+b3+b4+b5+b6+b7<1.
0.
8. A coating composition comprising the conductive polymer dispersion according to claim 7 and a water-soluble organic solvent.
9. A method for producing a conductive laminate, comprising applying the conductive polymer dispersion according to claim 7 or the coating composition according to claim 8 to at least a part of a surface of a substrate.
10. 9. A conductive laminate comprising: a substrate; and a conductive layer formed on at least a part of a surface of the substrate, the conductive layer being a cured layer of the conductive polymer dispersion according to claim 7 or the coating composition according to claim 8.
Citation Information
Patent Citations
New conductive high polymer and conductive material thereof
JP1992032104A
Method for producing conductive polymer dispersion, and method for producing conductive film
JP2020031013A
Conductive polymer composite and conductive polymer composition
JP2020128472A
Compositions useful for forming antistatic layers or electromagnetic radiation shielding
JP2020506986A
Conductive polymer dispersion, conductive film, electrode and method for producing the same
JP2021054929A