Non-aqueous electrolyte secondary battery
The non-aqueous electrolyte secondary battery addresses the issue of negative electrode material falling off and low-temperature performance by optimizing the negative electrode composite layer composition, ensuring improved adhesion and flexibility, thus enhancing battery reliability and low-temperature regeneration.
Patent Information
- Application Number
- JP2021553413
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-31
- Filing Date
- 2020-10-19
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2040-10-19
AI Technical Summary
Existing non-aqueous electrolyte secondary batteries face issues with negative electrode composite material falling off during assembly, leading to internal short circuits and inadequate low-temperature regeneration characteristics, particularly when used in electric vehicles.
The battery design incorporates a negative electrode composite material layer with a tap density of 1.00 g/cm³ to 1.20 g/cm³, a CMC content of 0.6% to 0.8% by mass, and SBR content of 0.4% to 0.8% by mass, with a mass ratio of CMC to SBR less than 2, to enhance adhesion and flexibility, thereby reducing material loss and improving low-temperature performance.
This configuration enhances battery reliability by minimizing material loss and improves low-temperature regeneration characteristics without increasing electrical resistance.
Smart Images

Figure 0007580384000003 
Figure 0007580384000001 
Figure 0007580384000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery. [Background technology]
[0002] The negative electrode mixture layer constituting the negative electrode of the nonaqueous electrolyte secondary battery contains a negative electrode active material, a thickener, and a binder, and carbon materials such as graphite are widely used as the negative electrode active material. By adjusting the properties and contents of each of the negative electrode active material, the thickener, and the binder, various properties of the secondary battery can be changed.
[0003] For example, Patent Document 1 discloses a secondary battery having improved cycle characteristics by containing in the negative electrode composite layer natural graphite as a negative electrode active material having a degree of amorphousness of 0.3 to 0.5 as measured by Raman measurement, 1 mass % to 2 mass % of CMC as a thickener, and 1 mass % to 2 mass % of SBR as a binder.
[0004] In addition, Patent Document 2 describes a negative electrode mixture layer having a tap density of 0.7 g / cm 3 A secondary battery is disclosed that contains the above natural graphite, 1 mass % or more of CMC, and 1 mass % or more of SBR, thereby improving cycle characteristics.
[0005] In addition, Patent Document 3 describes a negative electrode composite layer having a specific surface area of 1 m 2 / g or more of graphite, 0.3 mass % to 3 mass % of CMC, 0.3 mass % to 5 mass % of SBR, and carbon fibers with a fiber diameter of 1 nm to 1000 nm as a conductive material, thereby improving high-speed charge / discharge characteristics. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2014-528631 [Patent Document 2] JP 2011-238622 A [Patent Document 3] JP 2005-222933 A Summary of the Invention
[0007] In the battery assembly process, when the negative electrode is cut to a certain size, the composite material of the negative electrode composite layer may fall off. If the fallen composite material is wound up in the battery, an internal short circuit may occur during charging and discharging of the battery. In addition, since the portion of the negative electrode composite layer from which the composite material has fallen off becomes brittle, the composite material may further fall off due to expansion and contraction of the composite layer during charging and discharging of the battery, causing an internal short circuit. Therefore, it is necessary to suppress the falling off of the negative electrode composite material in order to improve the reliability of the battery. In addition, when a secondary battery is used as a power source for an electric vehicle (EV) or the like, excellent low-temperature regeneration characteristics are required. However, Patent Documents 1 to 3 do not take into consideration the amount of the negative electrode composite material that falls off when the negative electrode is cut, and the low-temperature regeneration characteristics.
[0008] A nonaqueous electrolyte secondary battery according to an embodiment of the present disclosure includes an electrode assembly having a positive electrode and a negative electrode, and an exterior body that houses the electrode assembly. The negative electrode includes a negative electrode core and a negative electrode mixture layer formed on the surface of the negative electrode core. The negative electrode mixture layer has a tap density of 1.00 g / cm. 3 ~1.20g / cm 3 the negative electrode mixture layer contains 0.6 mass% to 0.8 mass% CMC and the negative electrode mixture layer contains 0.4 mass% to 0.8 mass% SBR, wherein in the negative electrode mixture layer, a mass ratio of the CMC content to the SBR content is smaller than 2, and the total content of the CMC and the SBR in the negative electrode mixture layer is smaller than 1.5 mass%.
[0009] According to the nonaqueous electrolyte secondary battery according to the present disclosure, the reliability and low-temperature regeneration characteristics of the battery can be improved. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a perspective view of a secondary battery according to an embodiment of the present invention, showing the internal structure of a battery case with the front side of an exterior body removed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] By increasing the tap density of the negative electrode active material contained in the negative electrode mixture layer, the electrolyte absorption path from the surface of the negative electrode mixture layer to the negative electrode core is shortened, improving the low-temperature regeneration characteristics. However, since a negative electrode active material with a high tap density has a high circularity, when a negative electrode active material with a high tap density is contained in the negative electrode mixture layer, the gap between the active materials becomes larger than when a negative electrode active material with a low tap density is contained, and there is a lot of free CMC that is not adsorbed on the surface of the negative electrode active material, making the negative electrode hard. If the negative electrode becomes hard, the negative electrode mixture containing the negative electrode active material is likely to fall off when the negative electrode is cut to a certain size in the battery assembly process, so the CMC content is preferably low, but if the CMC content is too low, the dispersibility of the negative electrode mixture slurry becomes poor and the negative electrode mixture layer cannot be formed. In addition, since SBR has flexibility, increasing the content in the negative electrode mixture layer can soften the negative electrode. If the total content of CMC and SBR in the negative electrode mixture layer is increased, the negative electrode can be softened to suppress the falling off of the negative electrode mixture containing the negative electrode active material, but the resistance of the battery increases and the low-temperature regeneration characteristics deteriorate. 3 ~1.20g / cm 3 The researchers discovered that by mixing CMC and SBR in a specified ratio with the high-temperature anode active material, it is possible to improve the low-temperature regeneration characteristics of the battery while reducing the amount of anode composite that falls off when the anode is cut during the battery assembly process (hereinafter referred to as "cut-off amount").
[0012] An example of an embodiment of the present disclosure will be described in detail below. In this embodiment, a secondary battery 100 including a rectangular metal exterior body 1 is illustrated, but the exterior body is not limited to a rectangular shape and may be, for example, cylindrical. In addition, a wound electrode body 3 in which a positive electrode and a negative electrode are wound with a separator interposed therebetween is illustrated, but a laminated electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately laminated one by one with a separator interposed therebetween may also be used. The electrode body 3 is preferably wound. In addition, in both the positive electrode and the negative electrode, a case in which each composite layer is formed on both sides of each core body is illustrated, but each composite layer is not limited to being formed on both sides of each core body, and may be formed on at least one surface.
[0013] 1, the secondary battery 100 includes a wound electrode assembly 3 formed in a flat shape having a flat portion and a pair of curved portions by winding a positive electrode and a negative electrode with a separator interposed therebetween, an electrolyte, and an exterior body 1 that contains the electrode assembly 3 and the electrolyte. Both the exterior body 1 and the sealing plate 2 are made of metal, and are preferably made of aluminum or an aluminum alloy.
[0014] The exterior body 1 has a bottom part that is generally rectangular in bottom view, and side walls that stand on the periphery of the bottom part. The side walls are formed perpendicular to the bottom part. The dimensions of the exterior body 1 are not particularly limited, but an example is a lateral length of 60 to 160 mm, a height of 60 to 100 mm, and a thickness of 10 to 40 mm.
[0015] The positive electrode is a long body having a metallic positive electrode core and a positive electrode composite layer formed on both sides of the core, and a strip-shaped positive electrode core exposed portion 4 is formed at one end in the short direction, where the positive electrode core is exposed along the longitudinal direction. Similarly, the negative electrode is a long body having a metallic negative electrode core and a negative electrode composite layer formed on both sides of the core, and a strip-shaped negative electrode core exposed portion 5 is formed at one end in the short direction, where the negative electrode core is exposed along the longitudinal direction. The electrode body 3 has a structure in which the positive electrode and negative electrode are wound with a separator interposed between them, with the positive electrode core exposed portion 4 of the positive electrode arranged at one axial end and the negative electrode core exposed portion 5 of the negative electrode arranged at the other axial end.
[0016] A positive electrode current collector 6 is connected to the lamination portion of the positive electrode core exposed portion 4 of the positive electrode, and a negative electrode current collector 8 is connected to the lamination portion of the negative electrode core exposed portion 5 of the negative electrode. The positive electrode current collector 6 is preferably made of aluminum or an aluminum alloy. The negative electrode current collector 8 is preferably made of copper or a copper alloy. The positive electrode terminal 7 has a positive electrode external conductive portion 13 arranged on the battery exterior side of the sealing plate 2, a positive electrode bolt portion 14 connected to the positive electrode external conductive portion 13, and a positive electrode insertion portion 15 inserted into a through hole provided in the sealing plate 2, and is electrically connected to the positive electrode current collector 6. The negative electrode terminal 9 has a negative electrode external conductive portion 16 arranged on the battery exterior side of the sealing plate 2, a negative electrode bolt portion 17 connected to the negative electrode external conductive portion 16, and a negative electrode insertion portion 18 inserted into a through hole provided in the sealing plate 2, and is electrically connected to the negative electrode current collector 8.
[0017] The positive electrode terminal 7 and the positive electrode current collector 6 are fixed to the sealing plate 2 via an internal insulating member and an external insulating member, respectively. The internal insulating member is disposed between the sealing plate 2 and the positive electrode current collector 6, and the external insulating member is disposed between the sealing plate 2 and the positive electrode terminal 7. Similarly, the negative electrode terminal 9 and the negative electrode current collector 8 are fixed to the sealing plate 2 via an internal insulating member and an external insulating member, respectively. The internal insulating member is disposed between the sealing plate 2 and the negative electrode current collector 8, and the external insulating member is disposed between the sealing plate 2 and the negative electrode terminal 9.
[0018] The electrode body 3 is housed in the exterior body 1. The sealing plate 2 is connected to the opening edge of the exterior body 1 by laser welding or the like. The sealing plate 2 has an electrolyte injection hole 10, which is sealed with a sealing plug after the electrolyte is injected into the exterior body 1. The sealing plate 2 is formed with a gas exhaust valve 11 for exhausting gas when the pressure inside the battery reaches or exceeds a predetermined value.
[0019] The electrolyte is a non-aqueous electrolyte containing a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. For example, carbonates, lactones, ethers, ketones, esters, etc. can be used as the non-aqueous solvent, and two or more of these solvents can be mixed and used. When two or more solvents are mixed and used, it is preferable to use a mixed solvent containing a cyclic carbonate and a chain carbonate. For example, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used as the cyclic carbonate, and dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), etc. can be used as the chain carbonate. The non-aqueous solvent may contain a halogen-substituted product in which at least a part of the hydrogen of the above-mentioned solvent is replaced with a halogen atom such as fluorine. For the electrolyte salt, LiPF6, LiBF4, LiCF3SO3, etc., and mixtures thereof can be used. The amount of electrolyte salt dissolved in the non-aqueous solvent can be, for example, 0.5 to 2.0 mol / L. In addition, additives such as vinylene carbonate (VC) can be added as appropriate. The electrolyte is not limited to a liquid electrolyte, and may be a solid electrolyte using a gel polymer or the like.
[0020] The positive electrode, negative electrode, and separator that constitute the electrode assembly 3 will be described in detail below, and in particular the negative electrode mixture layer that constitutes the negative electrode.
[0021] [Positive electrode] The positive electrode includes a positive electrode core and a positive electrode composite layer formed on the surface of the positive electrode core. For the positive electrode core, for example, a foil of a metal such as aluminum that is stable in the potential range of the positive electrode, or a film with the metal disposed on the surface layer, can be used. The positive electrode composite layer includes, for example, a positive electrode active material, a binder, a conductive material, etc. The positive electrode can be produced, for example, by applying a positive electrode composite slurry including a positive electrode active material, a binder, a conductive material, etc., onto the positive electrode core, drying the slurry to form a positive electrode composite layer, and then rolling the positive electrode composite layer.
[0022] Examples of the positive electrode active material include lithium transition metal oxides containing transition metal elements such as Co, Mn, and Ni. The lithium transition metal oxide is, for example, Li x CoO2, Li x NiO2, Li x MnO2, Li x Co y Ni 1-y O2, Li x Co y M 1-y O z , Li x Ni 1-y M y O z , Li x Mn2O4, Li x Mn 2-y M y O4, LiMPO4, Li2MPO4F (M; at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0 < x ≤ 1.2, 0 < y ≤ 0.9, 2.0 ≤ z ≤ 2.3). These may be used alone or in combination of two or more. In terms of achieving a higher capacity of the secondary battery 100, the positive electrode active material preferably contains lithium nickel composite oxides such as Li x NiO2, Li x Co y Ni 1-y O2, Li x Ni 1-y M y O z (M; at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0 < x ≤ 1.2, 0 < y ≤ 0.9, 2.0 ≤ z ≤ 2.3) etc.
[0023] Examples of the conductive material include carbon-based particles such as carbon black (CB), acetylene black (AB), ketjen black, and graphite. These may be used alone or in combination of two or more.
[0024] Examples of the binder include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, polyolefin-based resins, etc. These may be used alone or in combination of two or more kinds.
[0025] [Negative electrode] The negative electrode includes a negative electrode core and a negative electrode composite layer formed on the surface of the negative electrode core. For the negative electrode core, for example, a foil of a metal such as copper that is stable in the potential range of the negative electrode, or a film having such a metal disposed on the surface layer can be used. The negative electrode composite layer has a tap density of 1.00 g / cm 3 ~1.20g / cm 3 The negative electrode active material includes the negative electrode active material, CMC whose content in the negative electrode mixture layer is 0.6% by mass to 0.8% by mass, and SBR whose content in the negative electrode mixture layer is 0.4% by mass to 0.8% by mass. In the negative electrode mixture layer, the mass ratio of the CMC content to the SBR content is less than 2, and the total content of the CMC and SBR in the negative electrode mixture layer is less than 1.5% by mass. This can improve the low-temperature regeneration characteristics of the battery while reducing the amount of cut-off. The negative electrode can be produced by applying a negative electrode mixture slurry containing at least the negative electrode active material, CMC, and SBR onto a negative electrode core, drying the slurry to form a negative electrode mixture layer, and then rolling the negative electrode mixture layer.
[0026] The negative electrode active material is not particularly limited as long as it can reversibly absorb and release lithium ions, and for example, carbon materials such as natural graphite and artificial graphite, metals that can be alloyed with lithium such as silicon (Si) and tin (Sn), or alloys containing metal elements such as Si and Sn, complex oxides, etc. can be used. As the negative electrode active material, carbon materials are preferable, and natural graphite is more preferable. The negative electrode active material may be used alone or in combination of two or more kinds.
[0027] The negative electrode active material may be substantially spherical with an average circularity of 0.8 or more. This shortens the liquid absorption path of the electrolyte from the surface of the negative electrode mixture layer to the negative electrode core, improving low-temperature regeneration characteristics. In this specification, the average circularity is defined as 4πS / L, where S is the projected area of the negative electrode active material and L is the perimeter. 2 It is defined as follows: The circularity of a circle is 1, and the longer and thinner the shape, the smaller the circularity becomes. The average circularity is the average value of the circularity calculated by observing 100 negative electrode active materials with a scanning electron microscope and measuring the area S and perimeter L of the active materials using image analysis software (for example, ImageJ, manufactured by the National Institutes of Health, USA).
[0028] The negative electrode active material may have an average particle size of 8 μm to 13 μm. By having the average particle size and average circularity of the negative electrode active material fall within the specified ranges, the tap density of the negative electrode active material can be made to be 1.00 g / cm 3 ~1.20g / cm 3 In this specification, the average particle size of the negative electrode active material refers to the volume-based median size (D50). D50 means the particle size at which the cumulative frequency is 50% from the smallest particle size in the volume-based particle size distribution, and is also called the median size. The particle size distribution of the negative electrode active material can be measured using a laser diffraction type particle size distribution measuring device (e.g., SALD-2200 manufactured by Shimadzu Corporation) with an aqueous solution of a surfactant as a dispersion medium.
[0029] The tap density of the negative electrode active material is 1.00 g / cm 3 ~1.20g / cm 3 and 1.03 g / cm 3 ~1.18g / cm 3 is preferred, and 1.05 g / cm 3 ~1.15g / cm 3is more preferable. The higher the tap density of the negative electrode active material, the better the low-temperature regeneration characteristics are, but the greater the amount of cut-off. By setting the tap density of the negative electrode active material within the above range, it is possible to achieve both improved low-temperature regeneration characteristics and reduced amount of cut-off. The tap density can be calculated by placing a connecting filling frame (about 50 mL) on a graduated cylinder of a fixed volume (for example, 50 mL), introducing 60 g of the negative electrode active material, tapping 300 times, removing the filling frame, and then calculating from the mass of the negative electrode active material in the graduated cylinder volume. The tap density of the negative electrode active material can be measured, for example, using TVP-1A (fixed volume type) manufactured by Tsutsui Rikagaku Kikai Co., Ltd.
[0030] The oil absorption of the negative electrode active material may be 43 ml / 100 g to 52 ml / 100 g. The oil absorption can be determined according to DBP (dibutyl phthalate) absorption method A (mechanical method) specified in JIS K-6217-4 "Basic properties of carbon black for rubber, Part 4: Determination of DBP absorption." Here, linseed oil is used instead of DBP. Specifically, 4 cm of linseed oil is added to 30 g of negative electrode active material particles that are being stirred by two blades. 3 Linseed oil is added at a rate of 1000g / min. The change in viscosity characteristics at this time is detected by a torque detector, and the output is converted into torque by a microcomputer. The amount of linseed oil corresponding to the torque at 100% of the maximum torque generated is converted per 100g of negative electrode active material particles, and the oil absorption can be calculated. The oil absorption of the negative electrode active material can be measured, for example, using an absorption tester (manufactured by Asahi Research Institute Co., Ltd., model name "S-500") or the like.
[0031] The BET specific surface area of the negative electrode active material is 3.5m 2 / g~4.8m 2 / g. By setting the BET specific surface area of the negative electrode active material in the above range, the initial discharge capacity of the battery can be improved, and a high capacity retention rate can be obtained even after high-temperature storage. The BET specific surface area can be measured using nitrogen gas with a commercially available measuring device such as Macsorb's HM model-1201.
[0032] The CMC content in the negative electrode mixture layer (hereinafter, C CMCThe content of CMC in the negative electrode mixture is 0.6% by mass to 0.8% by mass. In the present specification, CMC refers to carboxymethylcellulose or a salt thereof. Examples of the salt of carboxymethylcellulose include sodium carboxymethylcellulose and ammonium carboxymethylcellulose. Examples of suitable CMC include carboxymethylcellulose and sodium carboxymethylcellulose (CMC-Na). CMC may function as a binder, or may have a function of adjusting the viscosity of the negative electrode mixture slurry as a thickener.
[0033] The mass average molecular weight of CMC is 3.7 x 10 5 ~4.3×10 5 By setting the mass average molecular weight of CMC in this range, the thixotropy of the negative electrode slurry is improved, and the coating property of the composite slurry on the core body can be improved. In addition, the hardness of the composite layer of the electrode plate becomes more appropriate, and the amount of cut-off can be suppressed.
[0034] The content of SBR in the negative electrode mixture layer (hereinafter, C SBR The content of SBR (referred to as "straight rubber") is 0.4% by mass to 0.8% by mass. In this specification, SBR means styrene-butadiene rubber or a modified product thereof. The average primary particle size of SBR is preferably 120 to 250 nm, more preferably 150 to 230 nm.
[0035] The Tg of the SBR may be equal to or lower than 5° C. This makes the SBR soft, thereby improving the flexibility of the negative electrode.
[0036] In the negative electrode mixture layer, the mass ratio of the CMC content to the SBR content (hereinafter, C CMC / C SBR The sum of CMC, SBR and content (hereafter referred to as C CMC +C SBR This makes it possible to reduce the amount of cut and fallen particles while improving the low-temperature regeneration characteristics of the battery.
[0037] The negative electrode mixture layer may contain, in addition to CMC and SBR, fluorine-containing resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), binders such as polyacrylonitrile (PAN), polyimide, acrylic resins, and polyolefins, as well as polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), and the like, as long as the effects of the present embodiment are not hindered.
[0038] The negative electrode mixture layer has a packing density of 1.05 g / cm 3 ~1.25g / cm 3 and the thickness may be 65 μm to 75 μm. The packing density and thickness of the negative electrode mixture layer can be determined by the following method. (1) 10cm negative electrode 2 The mass A (g) and thickness C (cm) of the cut negative electrode are measured. (2) The negative electrode mixture layer is peeled off from the cut negative electrode, and the mass B (g) of the negative electrode core and the thickness D (cm) of the core are measured. (3) Thickness (μm) = (CD) × 10 4 The thickness of the negative electrode mixture layer is calculated from the formula. (4) Packing density (g / cm 3 The packing density of the negative electrode mixture layer is calculated from the formula:
[0039] [Separator] For example, a porous sheet having ion permeability and insulation is used as the separator. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. The separator is preferably made of an olefin resin such as polyethylene or polypropylene, or cellulose. The separator may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. The separator may also be a multilayer separator including a polyethylene layer and a polypropylene layer, and may have a material such as an aramid resin or ceramic applied to the surface of the separator.
[0040] <Example> The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0041] [Negative electrode active material] Natural graphite was used as the negative electrode active material. Five types of natural graphite, A to E, were used, and Table 1 shows the tap density, average circularity, average particle size (D50), oil absorption, and BET specific surface area of each.
[0042] [Table 1]
[0043] <Example 1> [Preparation of positive electrode] As the positive electrode active material, LiNi 0.35 Co 0.35 Mn 0.30 A composite oxide represented by O2 was used. The positive electrode active material, PVdF, and carbon black were mixed in a mass ratio of 90:3:7, and kneaded while adding N-methyl-2-pyrrolidone to prepare a positive electrode composite slurry. Next, the positive electrode composite slurry was applied to both sides of a long positive electrode core made of aluminum foil with a thickness of 13 μm, and the coating was dried. The dried coating was applied to a 1000-molecular positive electrode core having a packing density of 2.5 g / cm. 3 The positive electrode was then cut into a predetermined electrode size to produce a positive electrode having a positive electrode composite layer formed on both sides of the positive electrode core. The positive electrode had a positive electrode core exposed portion for connecting a positive electrode current collector at one end in the width direction along the longitudinal direction of the positive electrode.
[0044] [Preparation of negative electrode] Natural graphite A was used as the negative electrode active material. The negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed so that the mass ratio was 98.8:0.6:0.6, and an appropriate amount of water was added to prepare a negative electrode mixture slurry. C calculated from the above mixing ratio CMC / C SBR is 1, and C CMC +C SBR The mass average molecular weight of CMC is 4.0×105 and the Tg of SBR was 1.0°C.
[0045] The negative electrode composite slurry was applied to both sides of a negative electrode core made of copper foil by a die coating method, and after drying the coating, a negative electrode was produced in which a negative electrode composite layer was formed on both sides of the negative electrode core. The negative electrode composite layer of the negative electrode was rolled to a packing density of 1.2 g / cm. 3 The negative electrode was rolled to a thickness of 67 μm by rolling at a rolling mill, and then cut to a predetermined electrode size. In addition, a negative electrode core exposed portion for connecting a negative electrode current collector was provided at one end in the width direction along the longitudinal direction of the negative electrode.
[0046] [Preparation of electrode body] The positive electrode and the negative electrode were wound with a strip-shaped separator having a width of 120 mm interposed therebetween, and then the wound body was pressed in the radial direction to form a flat shape, thereby producing a wound-type electrode body. The wound body was formed by stacking the separator / positive electrode / separator / negative electrode in this order and winding it around a cylindrical winding core (the same separator was used for the two sheets). The positive electrode and the negative electrode were wound so that the exposed parts of the core were located on opposite sides of the wound body in the axial direction. The pressing conditions for the wound body were a pressing temperature of 75° C., a pressing pressure of 100 kN, and a pressing time of 3 minutes.
[0047] [Preparation of electrolyte] An electrolyte solution was prepared by adding LiPF6 to a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a volume ratio of 3:3:4 (25°C, 1 atm) to a concentration of 1 mol / L, and further adding vinylene carbonate to a concentration of 0.3 mass%.
[0048] [Preparation of secondary battery] A secondary battery (prismatic battery) was produced using the electrode body, the electrolyte, and a rectangular battery case. A positive electrode terminal was attached to the sealing plate constituting the battery case, and a positive electrode current collector was connected to the positive electrode terminal. A negative electrode terminal was attached to the sealing plate, and a negative electrode current collector was connected to the negative electrode terminal. Then, the positive electrode current collector was welded to the core exposed part of the positive electrode, and the negative electrode current collector was welded to the core exposed part of the negative electrode. The electrode body integrated with the sealing plate was placed in an insulating sheet formed into a box shape, and was housed in a rectangular, bottomed, cylindrical exterior body (lateral length 148.0 mm (inner dimension 146.8 mm), thickness 17.5 mm (inner dimension 16.5 mm), height 65.0 mm (inner dimension 64.0 mm)) constituting the battery case, and the opening of the exterior body was closed with a sealing plate. After 65 g of electrolyte was injected through the electrolyte injection hole in the sealing plate, the electrode body was thoroughly immersed in the electrolyte and then a temporary charge was performed. A sealing plug was then attached to the injection hole to obtain a secondary battery (battery capacity: 8 Ah).
[0049] <Example 2> A negative electrode and a secondary battery were obtained in the same manner as in Example 1, except that natural graphite B was used as the negative electrode active material. The obtained negative electrode and secondary battery were designated as Example 2.
[0050] <Example 3> Except for using natural graphite C as the negative electrode active material, a negative electrode and a secondary battery were obtained in the same manner as in Example 1. The obtained negative electrode and secondary battery were designated as Example 3.
[0051] <Example 4> A negative electrode and a secondary battery were obtained in the same manner as in Example 1, except that the negative electrode active material: carboxymethyl cellulose (CMC): styrene butadiene rubber (SBR) were mixed so that the mass ratio of these was 99.0:0.6:0.4 to prepare a negative electrode mixture slurry. The obtained negative electrode and secondary battery were designated as Example 4.
[0052] <Example 5> A negative electrode and a secondary battery were obtained in the same manner as in Example 1, except that the negative electrode active material, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) were mixed so that the mass ratio of these was 98.6:0.6:0.8 to prepare a negative electrode mixture slurry. The obtained negative electrode and secondary battery were designated as Example 5.
[0053] <Example 6> A negative electrode and a secondary battery were obtained in the same manner as in Example 1, except that the negative electrode active material, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) were mixed so that the mass ratio of these was 98.6:0.8:0.6 to prepare a negative electrode mixture slurry. The obtained negative electrode and secondary battery were designated as Example 6.
[0054] <Comparative Example 1> Except for using natural graphite D as the negative electrode active material, a negative electrode and a secondary battery were obtained in the same manner as in Example 1. The obtained negative electrode and secondary battery were designated as Comparative Example 1.
[0055] <Comparative Example 2> Except for using natural graphite E as the negative electrode active material, a negative electrode and a secondary battery were obtained in the same manner as in Example 1. The obtained negative electrode and secondary battery were designated as Comparative Example 2.
[0056] <Comparative Example 3> A negative electrode and a secondary battery were obtained in the same manner as in Example 1, except that the negative electrode active material, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) were mixed so that the mass ratio of these was 99.2:0.6:0.2 to prepare a negative electrode mixture slurry. The obtained negative electrode and secondary battery were designated as Comparative Example 3.
[0057] <Comparative Example 4> A negative electrode and a secondary battery were obtained in the same manner as in Example 1, except that the negative electrode active material, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) were mixed so that the mass ratio of these was 98.4:0.6:1.0 to prepare a negative electrode mixture slurry. The obtained negative electrode and secondary battery were designated as Comparative Example 4.
[0058] <Comparative Example 5> A negative electrode and a secondary battery were obtained in the same manner as in Example 1, except that the negative electrode active material, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) were mixed so that the mass ratio of these was 99.0:0.8:0.2 to prepare a negative electrode mixture slurry. The obtained negative electrode and secondary battery were designated as Comparative Example 5.
[0059] <Comparative Example 6> A negative electrode and a secondary battery were obtained in the same manner as in Example 1, except that the negative electrode active material, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) were mixed so that the mass ratio of these was 98.8:0.8:0.4 to prepare a negative electrode mixture slurry. The obtained negative electrode and secondary battery were designated as Comparative Example 6.
[0060] <Comparative Example 7> A negative electrode and a secondary battery were obtained in the same manner as in Example 1, except that the negative electrode active material, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) were mixed so that the mass ratio of these was 98.4:0.8:0.8 to prepare a negative electrode mixture slurry. The obtained negative electrode and secondary battery were designated as Comparative Example 7.
[0061] <Comparative Example 8> A negative electrode and a secondary battery were obtained in the same manner as in Example 1, except that the negative electrode active material, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) were mixed so that the mass ratio of these was 98.6:1.0:0.4 to prepare a negative electrode mixture slurry. The obtained negative electrode and secondary battery were designated as Comparative Example 8.
[0062] <Comparative Example 9> A negative electrode and a secondary battery were obtained in the same manner as in Example 1, except that the negative electrode active material, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) were mixed so that the mass ratio of these was 98.4:1.0:0.6 to prepare a negative electrode mixture slurry. The obtained negative electrode and secondary battery were designated as Comparative Example 9.
[0063] <Comparative Example 10> An attempt was made to obtain a negative electrode in the same manner as in Example 1, except that the negative electrode active material, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) were mixed so that the mass ratio of these was 98.9:0.5:0.6 to prepare a negative electrode mixture slurry, but the dispersibility of the negative electrode mixture slurry was poor, and a negative electrode mixture layer could not be formed, and a negative electrode and a secondary battery could not be obtained. This result was designated Comparative Example 10.
[0064] [Measurement of absorption time] Each negative electrode of the examples and comparative examples was dried for 10 hours in a thermostatic chamber heated to 200°C under a nitrogen atmosphere, and each negative electrode was cut into a size of 5 cm x 5 cm to prepare a sample. 3.0 μL of polypropylene carbonate (PC) was dropped vertically onto the surface of each sample, and the time until the PC was absorbed into the inside of the sample was measured visually. Measurements were performed six times for each sample, and the average value was taken as the liquid absorption time. The shorter the liquid absorption time, the smoother the electrolyte replacement from the surface of the negative electrode mixture layer to the core side, so that the electrolyte discharged from the negative electrode mixture layer during discharge is quickly absorbed into the negative electrode mixture layer during charge. Therefore, the shorter the liquid absorption time, the better the low-temperature regeneration characteristics are, and the more suppressed the deterioration of the rapid charge / discharge cycle characteristics are.
[0065] [Measurement of cut-off amount] Each of the negative electrodes of the Examples and Comparative Examples was cut under the conditions described below, and the amount of cut and fallen off was determined from the area of the powder of the negative electrode mixture that fell off during cutting. (1) The negative electrode was cut into a sample piece measuring 100 mm x 100 mm. (2) The test piece was placed on a piece of white paper, and 100 mm was cut from one end of the test piece with a cutter, causing the negative electrode mixture to fall onto the white paper. (3) An image of the fallen negative electrode composite material was taken using a stereomicroscope. The magnification of the stereomicroscope was 10 times. (4) The image obtained by the above process was imported into a computer and binarized using image analysis software (e.g., ImageJ, manufactured by the National Institutes of Health, USA) to obtain a binarized image in which the fallen negative electrode composite was colored black and the white paper was colored white. (5) The area of the fallen negative electrode mixture was calculated from the binarized image. (6) The above steps (1) to (5) were repeated 10 times, and the average area of the fallen negative electrode mixture was taken as the amount of cut and fallen material.
[0066] [Evaluation of low-temperature regeneration characteristics] Each of the batteries of the examples and comparative examples was charged under the following conditions, and the low-temperature regeneration value was determined. (1) The battery was charged at 25°C until the SOC reached 50%. (2) Batteries with SOC 50% were charged at currents of 3.7 It, 12.5 It, 17.5 It, 22.5 It, 31.2 It, and 37.5 It for 5 seconds each at -10°C (It (A) = rated capacity (Ah) / 1 (h)). (3) The battery voltage was measured immediately after charging for 5 seconds, and the battery voltage was plotted against each current value to determine the current value IP (A) that corresponds to the battery voltage (V) equivalent to SOC 100%. The low-temperature regeneration value (W) was calculated by multiplying the current value IP by the battery voltage (V) equivalent to SOC 100%.
[0067] Table 2 summarizes the results of the liquid absorption time, the cut-off amount, and the low-temperature regeneration characteristics of the examples and the comparative examples. Table 2 also shows the quantitative relationship (C CMC , C SBR , C CMC / C SBR , C CMC +C SBR ) was also stated.
[0068] [Table 2]
[0069] As can be seen from Table 2, in comparison with Comparative Examples 1 to 9, all of Examples 1 to 5 were able to maintain high low-temperature regeneration characteristics while suppressing the amount of cut falling off to a certain level or less. [Explanation of symbols]
[0070] 1 Exterior body 2 Sealing plate 3 Electrode body 4 Positive electrode core exposed part 5 Negative electrode core exposed part 6 Positive electrode current collector 7 Positive terminal 8 Negative electrode current collector 9 Negative terminal 10 Electrolyte injection hole 11 Gas exhaust valve 13 Positive electrode outer conductive part 14 Positive Bolt Part 15 Positive electrode insertion part 16 Negative electrode outer conductive part 17 Negative Bolt Part 18 Negative electrode insertion part 100 Secondary battery
Claims
1. A non-aqueous electrolyte secondary battery comprising an electrode assembly having a positive electrode and a negative electrode, and an exterior body that houses the electrode assembly, The negative electrode includes a negative electrode core and a negative electrode mixture layer formed on a surface of the negative electrode core, The negative electrode mixture layer has a tap density of 1.00 g / cm 3 ~1.20g / cm 3 a CMC content in the negative electrode mixture layer of 0.6% by mass to 0.8% by mass, and an SBR content in the negative electrode mixture layer of 0.4% by mass to 0.8% by mass, In the negative electrode mixture layer, a mass ratio of the CMC content to the SBR content is less than 2; the total content of CMC and SBR in the negative electrode mixture layer is 1.2 mass % or less.
2. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the negative electrode active material has an oil absorption of 43 ml / 100 g to 52 ml / 100 g.
3. The BET specific surface area of the negative electrode active material is 3.5 m 2 / g to 4.8m 2 3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the capacitance is 0.1 to 0.5 μm.
4. 4. The nonaqueous electrolyte secondary battery according to claim 1, wherein the negative electrode active material has a substantially spherical shape with an average circularity of 0.8 or more.
5. 5. The nonaqueous electrolyte secondary battery according to claim 1, wherein the negative electrode active material has an average particle size of 8 μm to 13 μm.
6. 6. The nonaqueous electrolyte secondary battery according to claim 1, wherein the negative electrode active material is natural graphite.
7. 7. The nonaqueous electrolyte secondary battery according to claim 1, wherein the SBR has a Tg of 5° C. or lower.
8. The mass average molecular weight of CMC is 3.7 × 10 5 ~4.3 x 10 5 The nonaqueous electrolyte secondary battery according to any one of claims 1 to 7,
9. The electrode body is a wound type in which the positive electrode and the negative electrode are wound with a separator interposed therebetween, The negative electrode mixture layer has a packing density of 1.05 g / cm 3 ~1.25g / cm 3 and a thickness of 65 μm to 75 μm.
Citation Information
Patent Citations
Negative pole material for lithium battery, and lithium battery
JP2005222933A
Negative electrode material for nonaqueous secondary battery, negative electrode for nonaqueous secondary battery, and nonaqueous secondary battery
JP2011238622A
Lithium secondary battery containing spheroidized natural graphite as the negative electrode active material
JP2014528631A
Secondary battery
JP2015220173A