Copolymer, molding, injection molding and coated electric wire

A copolymer of TFE and PPVE units addresses the challenges of ozone-resistant materials by providing a uniform, thick coating with excellent abrasion resistance and low permeability, while preventing mold corrosion and fluorine ion elution, suitable for large-diameter core wires and high-temperature applications.

JP7580418B2Active Publication Date: 2024-11-11DAIKIN INDUSTRIES LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022012562
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-30
Filing Date
2022-01-31
Publication Date
2024-11-11
Estimated Expiration
2042-01-31

AI Technical Summary

Technical Problem

Existing molding materials for ozone-resistant articles face challenges in achieving a balance between ozone resistance, chemical resistance, heat resistance, mechanical properties, and the formation of uniform, thick coating layers on large-diameter core wires, while also maintaining low permeability to nitrogen, chemicals, and water vapor, and resisting fluorine ion elution into electrolytes.

Method used

A copolymer composed of tetrafluoroethylene (TFE) and perfluoro(propyl vinyl ether) (PPVE) units, with specific content ratios and melt flow rates, is used to create a copolymer with controlled functional groups, allowing for injection molding and extrusion molding of thick, uniform coatings with excellent abrasion resistance, low permeability, and resistance to fluorine ion elution.

Benefits of technology

The copolymer achieves a beautiful injection molded article with excellent ozone resistance, high-temperature sealing properties, and non-adhesiveness, while preventing mold corrosion and maintaining low permeability to nitrogen, chemicals, and water vapor, even under repeated loads.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580418000001
    Figure 0007580418000001
  • Figure 0007580418000002
    Figure 0007580418000002
  • Figure 0007580418000003
    Figure 0007580418000003
Patent Text Reader

Abstract

To provide a copolymer capable of obtaining a beautiful injection molded article by molding by an injection molding method, forming an extremely thick coating layer having a uniform thickness on a core wire having a very large diameter by an injection molding method which is less likely to corrode a mold used for molding or a coating core wire and obtaining a molded article which is excellent in wear resistance, low nitrogen permeability, low chemical liquid permeability, low water vapor permeability, rigidity at a high temperature of 110°C, high temperature tensile creep characteristics, degradation resistance against a repeated load, very long-term ozone resistance, sealability at a high temperature and non-adhesiveness and is less likely to elute fluorine ions in an electrolytic solution.SOLUTION: There is provided a copolymer which contains a tetrafluoroethylene unit and a perfluoro(propyl vinyl ether) unit, wherein the content of the perfluoro(propyl vinyl ether) unit is 3.9 to 4.9 mass% based on the total monomer units and the melt flow rate at 372°C is 4.0 to 9.0 g / 10 min and the number of functional groups is 40 or less per main-chain carbon number of 106.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a copolymer, a molded article, an injection molded article, and a coated electric wire. [Background technology]

[0002] Patent Document 1 describes a molding material for ozone-resistant articles, which is made of a copolymer (A) and has a melt flow rate of 0.1 to 50 g / 10 min. The copolymer (A) is a copolymer made of tetrafluoroethylene and perfluorovinyl ether, contains 3.5 mass % or more of perfluorovinyl ether units, has a melting point of 295° C. or higher, and has an unstable terminal group of 1×10 carbon atoms in the copolymer (A). 6 An ozone-resistant molding material for articles is described, characterized in that the number of particles per particle is 50 or less.

[0003] In Patent Document 2, a compound having 10 carbon atoms is described. 6 Disclosed are melt extruded cubes of a melt processable TFE copolymer having about 80 or less unstable end groups per cube, characterized in that at least about 80% by weight of the cubes are in the size range of about 200 to about 1200 μm. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2003 / 048214 [Patent Document 2] Special Publication No. 2003-534940 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present disclosure is to provide a copolymer that can be molded by injection molding to give a beautiful injection-molded article, that is resistant to corrosion of the mold used in molding and the core wire to be coated, that can be used by extrusion molding to form a very thick coating layer of uniform thickness on a core wire with a very large diameter, and that can give a molded article that has excellent abrasion resistance, low nitrogen permeability, low chemical permeability, low water vapor permeability, rigidity at a high temperature of 110°C, high-temperature tensile creep properties, resistance to deterioration under repeated loads, extremely long-term ozone resistance, sealing properties and non-stickiness at high temperatures, and that is also resistant to elution of fluoride ions into the electrolyte. [Means for solving the problem]

[0006] According to the present disclosure, a fluoropolymer containing tetrafluoroethylene units and perfluoro(propyl vinyl ether) units is provided, the content of the perfluoro(propyl vinyl ether) units being 3.9 to 4.9% by mass relative to the total amount of monomer units, the melt flow rate at 372°C being 4.0 to 9.0 g / 10 min, and the number of functional groups being 10 carbon atoms in the main chain. 6 Copolymers are provided in which the number of units per unit is 40 or less.

[0007] The copolymer of the present disclosure preferably has a melt flow rate at 372° C. of 5.0 to 9.0 g / 10 min.

[0008] The present disclosure also provides an injection-molded article containing the above-mentioned copolymer.

[0009] The present disclosure also provides a covered electric wire including a covering layer containing the above-mentioned copolymer.

[0010] The present disclosure also provides a molded article containing the above-described copolymer, the molded article being a joint, a film, a bottle, a gasket, a wire coating, or a tube. Effect of the Invention

[0011] According to the present disclosure, it is possible to provide a copolymer that can be molded by injection molding to obtain a beautiful injection-molded article, that is resistant to corrosion of the mold used in molding and the core wire to be coated, and that can be used by extrusion molding to form a very thick coating layer of uniform thickness on a core wire with a very large diameter, and that can obtain a molded article that has excellent abrasion resistance, low nitrogen permeability, low chemical permeability, low water vapor permeability, rigidity at a high temperature of 110°C, high-temperature tensile creep properties, resistance to deterioration under repeated loads, extremely long-term ozone resistance, sealing properties and non-stickiness at high temperatures, and that is resistant to elution of fluoride ions into the electrolyte. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Specific embodiments of the present disclosure will be described in detail below, but the present disclosure is not limited to the following embodiments.

[0013] The copolymers of the present disclosure contain tetrafluoroethylene (TFE) units and perfluoro(propyl vinyl ether) (PPVE) units.

[0014] Copolymers containing TFE units and PPVE units (PFA) are used as materials for forming piping components used to transport fluids, such as pipes, joints, gaskets, and packings. Piping components made of PFA are used, for example, to transport fluids that exceed 100°C, or to transport chemicals that do not tolerate the inclusion of moisture such as water vapor in the outside air. For this reason, there is a demand for materials that can provide molded products that are excellent in low permeability to chemicals, rigidity at high temperatures, tensile creep properties at high temperatures, sealing properties at high temperatures, and low water vapor permeability. Furthermore, when joints are repeatedly attached and detached, the joints are easily damaged by wear, so there is a demand for materials that can provide molded products that are excellent in resistance to deterioration and wear resistance against repeated loads.

[0015] Patent Document 1 describes that the molding material for ozone-resistant articles having the above-mentioned characteristics is a molding material that has excellent ozone resistance while maintaining the chemical resistance, heat resistance, and mechanical properties of fluororesin. In recent years, there has been a demand for molding materials with improved properties compared to the molding material for ozone-resistant articles described in Patent Document 1, and in particular, there has been a demand for materials that can obtain molded articles with excellent abrasion resistance, low nitrogen permeability, low chemical permeability, rigidity at high temperatures, high-temperature tensile creep properties, resistance to deterioration against repeated loads, extremely long-term ozone resistance, sealing properties at high temperatures, and low water vapor permeability. On the other hand, when trying to improve sealing properties and low water vapor permeability at high temperatures, there is a problem that abrasion resistance and ozone resistance are deteriorated.

[0016] It was found that by appropriately adjusting the content of PPVE units, melt flow rate (MFR) and number of functional groups of a copolymer containing TFE units and PPVE units, the moldability of the copolymer is significantly improved and the mold used for molding is not easily corroded. Furthermore, it was also found that by using such a copolymer, a molded product can be obtained that has excellent abrasion resistance, low nitrogen permeability, low chemical permeability, low water vapor permeability, rigidity at high temperatures of 110°C, high-temperature tensile creep properties, resistance to deterioration under repeated loads, extremely long-term ozone resistance, sealing properties and non-adhesiveness at high temperatures, and is also less likely to dissolve fluorine ions into the electrolyte.

[0017] Moreover, by molding the copolymer of the present disclosure by extrusion molding, a very thick coating layer can be formed with a uniform thickness on a core wire having a very large diameter. Furthermore, the obtained coating layer is less likely to corrode the core wire. Thus, the copolymer of the present disclosure can be used not only as a material for piping components, but also in a wide range of applications such as electric wire coating.

[0018] The copolymers of the present disclosure are melt-processable fluoroplastics, meaning that the polymers can be melted and processed using conventional processing equipment such as extruders and injection molding machines.

[0019] The content of the PPVE unit in the copolymer is 3.9 to 4.9% by mass based on the total monomer units. The content of the PPVE unit in the copolymer is preferably 4.0% by mass or more, more preferably 4.1% by mass or more, preferably 4.8% by mass or less, more preferably 4.7% by mass or less, even more preferably 4.6% by mass or less, even more preferably 4.5% by mass or less, particularly preferably 4.4% by mass or less, and most preferably 4.3% by mass or less. If the content of the PPVE unit in the copolymer is too high, the sealability at high temperatures is poor, and the low water vapor permeability, low nitrogen permeability, low chemical permeability, and rigidity at high temperatures of 110°C are poor. If the content of the PPVE unit in the copolymer is too low, it becomes difficult to obtain a molded product that is excellent in resistance to deterioration against repeated loads and has extremely excellent ozone resistance for a long period of time.

[0020] The content of TFE units in the copolymer is preferably 95.1 to 96.1% by mass, more preferably 95.2% by mass or more, even more preferably 95.3% by mass or more, still more preferably 95.4% by mass or more, particularly more preferably 95.5% by mass or more, particularly preferably 95.6% by mass or more, most preferably 95.7% by mass or more, more preferably 96.0% by mass or less, and even more preferably 95.9% by mass or less, based on the total monomer units. If the content of TFE units in the copolymer is too low, the sealability at high temperatures may be poor, or the low water vapor permeability, low nitrogen permeability, low chemical permeability, and rigidity at high temperatures of 110°C may be poor. If the content of TFE units in the copolymer is too high, it tends to be difficult to obtain a molded product that is excellent in resistance to deterioration against repeated loads and has extremely excellent long-term ozone resistance.

[0021] In the present disclosure, the content of each monomer unit in the copolymer is 19 Measured by F-NMR.

[0022] The copolymer may also contain monomer units derived from a monomer copolymerizable with TFE and PPVE. In this case, the content of the monomer units copolymerizable with TFE and PPVE is preferably 0 to 1.2 mass%, more preferably 0.05 to 1.0 mass%, and further preferably 0.1 to 0.7 mass%, based on the total monomer units of the copolymer.

[0023] Monomers that can be copolymerized with TFE and PPVE include hexafluoropropylene (HFP), CZ 1 Z 2 =CZ 3 (CF2) n Z 4 (In the formula, Z 1 , Z 2 and Z 3 are the same or different and represent H or F; Z 4 represents H, F or Cl, and n represents an integer of 2 to 10. 1 (In the formula, Rf 1 Perfluoro(alkyl vinyl ether) [PAVE] (excluding PPVE) represented by CF2=CF-OCH2-Rf 1 (In the formula, Rf 1 represents a perfluoroalkyl group having 1 to 5 carbon atoms.) Among these, HFP is preferred.

[0024] The copolymer is preferably at least one selected from the group consisting of copolymers consisting of only TFE units and PPVE units, and TFE / HFP / PPVE copolymers, and more preferably a copolymer consisting of only TFE units and PPVE units.

[0025] The melt flow rate (MFR) of the copolymer is 4.0 to 9.0 g / 10 min. The MFR of the copolymer is preferably 4.1 g / 10 min or more, more preferably 4.5 g / 10 min or more, even more preferably 5.0 g / 10 min or more, particularly preferably 6.0 g / 10 min or more, most preferably 7.0 g / 10 min or more, preferably 8.0 g / 10 min or less, more preferably 7.5 g / 10 min or less, and even more preferably 7.4 g / 10 min or less. By having the MFR of the copolymer within the above range, the moldability of the copolymer is improved, and a molded product excellent in abrasion resistance, low nitrogen permeability, low chemical permeability, low water vapor permeability, rigidity at high temperature of 110°C, high temperature tensile creep property, deterioration resistance against repeated load, extremely long-term ozone resistance, sealability and non-stickiness at high temperature can be obtained. If the MFR is too high, it becomes difficult to obtain a molded product excellent in abrasion resistance and extremely long-term ozone resistance. If the MFR is too low, the molded article tends to have poor nitrogen permeability, poor chemical permeability and low rigidity at a high temperature of 110°C.

[0026] The copolymer of the present disclosure can be molded by injection molding or by wire coating extrusion molding, since the content of PPVE units, melt flow rate (MFR), and functionality of the copolymer containing TFE units and PPVE units are appropriately adjusted. A copolymer that flows sufficiently when heated is suitable for injection molding, while a copolymer with too high flowability at high temperatures can be used to form a coating layer for an electric wire by extrusion molding, resulting in large fluctuations in the outer diameter. The copolymer of the present disclosure can be molded by injection molding to obtain a beautiful injection molded product, and can be molded by extrusion molding to obtain a coated electric wire with small fluctuations in the outer diameter.

[0027] In this disclosure, the MFR is a value obtained in accordance with ASTM D1238 using a melt indexer, as the mass of polymer flowing out per 10 minutes from a nozzle having an inner diameter of 2.1 mm and a length of 8 mm under a load of 5 kg at 372°C (g / 10 minutes).

[0028] The MFR can be adjusted by adjusting the type and amount of a polymerization initiator used when polymerizing the monomers, the type and amount of a chain transfer agent, and the like.

[0029] In the present disclosure, the copolymer has a main chain carbon number of 10 6 The number of functional groups per unit is 40 or less. The main chain carbon number of the copolymer is 10 6 The number of functional groups per unit is preferably 30 or less, more preferably 20 or less, even more preferably 15 or less, even more preferably 10 or less, and particularly preferably less than 6. When the number of functional groups of the copolymer is within the above range, the copolymer is less likely to corrode a mold during molding using a mold, and is less likely to corrode a core wire even when used as a wire coating. Furthermore, a molded product can be obtained that has extremely long-term ozone resistance, low nitrogen permeability, low chemical permeability, excellent rigidity and non-stickiness at a high temperature of 110°C, and is less likely to elute fluorine ions into an electrolyte. In particular, by appropriately adjusting the content of PPVE units, melt flow rate (MFR), and number of functional groups of the copolymer containing TFE units and PPVE units, a molded product that exhibits excellent low permeability to various chemicals such as dimethyl carbonate and ethyl acetate can be obtained.

[0030] The type of functional group and the number of functional groups can be identified by infrared spectroscopy.

[0031] Specifically, the number of functional groups is measured by the following method. First, the copolymer is molded by cold pressing to prepare a film having a thickness of 0.25 to 0.30 mm. This film is analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum of the copolymer, and a difference spectrum with a base spectrum that is completely fluorinated and has no functional groups is obtained. From the absorption peaks of specific functional groups that appear in this difference spectrum, the number of carbon atoms in the copolymer is calculated according to the following formula (A): 6 Calculate the number of functional groups per unit, N.

[0032] N=I×K / t (A) I: Absorbance K: Correction coefficient t: film thickness (mm)

[0033] For reference, the absorption frequencies, molar absorption coefficients, and correction coefficients for several functional groups are shown in Table 1. The molar absorption coefficients were determined from the FT-IR measurement data of low-molecular-weight model compounds. [Table 1]

[0034] The absorption frequencies of -CH2CF2H, -CH2COF, -CH2COOH, -CH2COOCH3, and -CH2CONH2 are shown in the table. The absorption frequencies of -CF2H, -COF, -COOH free, -COOH bonded, -COOCH3, and -CONH2 are several tens of Kaiser (cm -1 ) lower.

[0035] For example, the functional group number of -COF is the absorption frequency of 1883 cm due to -CF2COF. -1 The number of functional groups determined from the absorption peak of -CH2COF and the absorption frequency of 1840 cm -1 The number of functional groups is the sum of the number of functional groups determined from the absorption peaks of

[0036] The functional groups are those present at the ends of the main chain or side chains of the copolymer, and those present in the main chain or side chains. The number of functional groups may be the total number of -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH.

[0037] The functional group is introduced into the copolymer by, for example, a chain transfer agent or a polymerization initiator used in producing the copolymer. For example, when an alcohol is used as a chain transfer agent or a peroxide having a -CH2OH structure is used as a polymerization initiator, -CH2OH is introduced into the main chain end of the copolymer. In addition, the functional group is introduced into the side chain end of the copolymer by polymerizing a monomer having a functional group.

[0038] By subjecting the copolymer having such a functional group to a fluorination treatment, a copolymer having a number of functional groups within the above range can be obtained. That is, the copolymer of the present disclosure is preferably a fluorination-treated copolymer. It is also preferable that the copolymer of the present disclosure has a -CF3 end group.

[0039] The melting point of the copolymer is preferably 295 to 315° C., more preferably 298° C. or higher, even more preferably 300° C. or higher, particularly preferably 301° C. or higher, most preferably 302° C. or higher, and more preferably 310° C. or lower. When the melting point is within the above range, it is possible to obtain a copolymer that gives a molded article having even more excellent sealability, especially at high temperatures.

[0040] In this disclosure, melting points can be measured using a differential scanning calorimeter (DSC).

[0041] The water vapor permeability of the copolymer is preferably 14.0 g cm / m 2 less than or equal to 13.5 g cm / m 2 or less, and more preferably 13.0 g cm / m 2 The copolymer of the present disclosure has excellent low water vapor permeability because the content of PPVE units, melt flow rate (MFR) and number of functional groups of the copolymer containing TFE units and PPVE units are appropriately adjusted. Therefore, when a molded body containing the copolymer of the present disclosure is used as a piping member (for example, piping, joints, gaskets, packing) for supplying a chemical solution that should not be contaminated with water, the penetration of water vapor into the inside of the piping member can be suppressed, and the infiltration of water into the chemical solution can be suppressed. In addition, by using a molded body containing the copolymer of the present disclosure as a compressed member of a secondary battery, for example, the infiltration of water can be effectively prevented even under high temperature and high humidity conditions.

[0042] In the present disclosure, the water vapor permeability can be measured under conditions of a temperature of 95° C. for 30 days. The water vapor permeability can be specifically measured by the method described in the Examples.

[0043] The electrolyte permeability of the copolymer is preferably 7.9 g cm / m 2 More preferably, it is 7.7 g cm / m or less. 2 The copolymer of the present disclosure has excellent low electrolyte permeability because the content of PPVE units, melt flow rate (MFR) and number of functional groups of the copolymer containing TFE units and PPVE units are appropriately adjusted. That is, by using the copolymer of the present disclosure, a molded body that is difficult to permeate chemicals such as electrolytes can be obtained, so that, for example, piping members and flowmeter members obtained by using the copolymer of the present disclosure can be suitably used for transporting chemicals such as electrolytes.

[0044] In the present disclosure, the electrolyte permeability can be measured under conditions of a temperature of 60° C. for 30 days. The electrolyte permeability can be specifically measured by the method described in the Examples.

[0045] The ethyl acetate permeability of the copolymer is preferably 7.0 g cm / m 2 The copolymer of the present disclosure has excellent low ethyl acetate permeability because the content of the PPVE unit, the melt flow rate (MFR) and the number of functional groups of the copolymer containing the TFE unit and the PPVE unit are appropriately adjusted. That is, by using the copolymer of the present disclosure, a molded product that is difficult to permeate chemicals such as ethyl acetate can be obtained.

[0046] In the present disclosure, the ethyl acetate permeability can be measured under conditions of a temperature of 60° C. for 45 days. The specific measurement of the ethyl acetate permeability can be performed by the method described in the Examples.

[0047] The nitrogen permeability coefficient of the copolymer is preferably 330 cm 3 mm / (m 2The copolymer of the present disclosure has excellent low nitrogen permeability because the PPVE unit content, melt flow rate (MFR), and number of functional groups of the copolymer containing TFE units and PPVE units are appropriately adjusted. Therefore, by using the copolymer of the present disclosure, a molded article with excellent gas barrier properties can be obtained.

[0048] In the present disclosure, the nitrogen permeability coefficient can be measured under the conditions of a test temperature of 70° C. and a test humidity of 0% RH. The nitrogen permeability coefficient can be specifically measured by the method described in the Examples.

[0049] The copolymer of the present disclosure has an amount of eluted fluorine ions detected in an electrolyte immersion test of preferably 1.0 ppm or less, more preferably 0.8 ppm or less, and even more preferably 0.7 ppm or less, by mass. When the amount of eluted fluorine ions is within the above range, the generation of gases such as HF in the nonaqueous electrolyte battery can be further suppressed, and the deterioration of the battery performance and the shortening of the battery life of the nonaqueous electrolyte battery can be further suppressed.

[0050] In the present disclosure, the electrolyte immersion test can be performed by preparing a test piece having a weight equivalent to 10 pieces of molded bodies (15 mm × 15 mm × 0.2 mm) using the copolymer, placing the test piece and 2 g of dimethyl carbonate (DMC) in a glass sample bottle in a constant temperature bath at 80°C, and leaving it for 144 hours.

[0051] The storage modulus (E') of the copolymer at 150°C is preferably 70 MPa or more, more preferably 75 MPa or more, and preferably 1000 MPa or less, more preferably 500 MPa or less, and even more preferably 300 MPa or less. When the storage modulus (E') of the copolymer at 150°C is within the above range, it is possible to obtain a copolymer that can continue to exhibit sufficient rebound resilience even at high temperatures for a long period of time and that can give a molded product with even more excellent sealability at high temperatures.

[0052] The storage modulus (E') can be measured by dynamic viscoelasticity measurement in the range of 30 to 250°C under conditions of a temperature increase rate of 2°C / min and a frequency of 10 Hz. The storage modulus (E') at 150°C can be increased by adjusting the PPVE unit content and melt flow rate (MFR) of the copolymer.

[0053] The seal pressure of the copolymer at 150° C. is preferably 0.45 MPa or more, more preferably 0.50 MPa or more, and even more preferably 0.55 MPa or more, and although there is no particular upper limit, it may be 3.00 MPa or less. The seal pressure at 150° C. can be increased by adjusting the PPVE unit content, melt flow rate (MFR) and number of functional groups of the copolymer.

[0054] The seal pressure can be calculated by the following formula from the height of the test piece obtained from the copolymer after it has been deformed by 50% compression deformation rate, left at 150°C for 18 hours, released from the compression state, and left at room temperature for 30 minutes, and then measuring the height of the test piece (the height of the test piece after compression deformation). 150℃ sealing pressure (MPa) = (t2-t1) / t1×E' t1: original height of test piece before compressive deformation (mm) x 50% t2: Height of the test piece after compressive deformation (mm) E': Storage modulus at 150℃ (MPa)

[0055] The copolymer of the present disclosure can be produced by a polymerization method such as suspension polymerization, solution polymerization, emulsion polymerization, bulk polymerization, etc. As the polymerization method, emulsion polymerization or suspension polymerization is preferable. In these polymerizations, each condition such as temperature and pressure, polymerization initiator and other additives can be appropriately set according to the composition and amount of the copolymer.

[0056] As the polymerization initiator, an oil-soluble radical polymerization initiator or a water-soluble radical polymerization initiator can be used.

[0057] The oil-soluble radical polymerization initiator may be a known oil-soluble peroxide, for example: dialkyl peroxycarbonates such as di-normal propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, and di-2-ethoxyethyl peroxydicarbonate; Peroxyesters such as t-butyl peroxyisobutyrate and t-butyl peroxypivalate; Dialkyl peroxides such as di-t-butyl peroxide; Di[fluoro(or fluorochloro)acyl]peroxides; The following are some representative examples.

[0058] The di[fluoro(or fluorochloro)acyl]peroxides include diacyl peroxides represented by [(RfCOO)-]2 (Rf is a perfluoroalkyl group, a ω-hydroperfluoroalkyl group, or a fluorochloroalkyl group).

[0059] Examples of di[fluoro(or fluorochloro)acyl]peroxides include di(ω-hydro-dodecafluorohexanoyl)peroxide, di(ω-hydro-tetradecafluoroheptanoyl)peroxide, di(ω-hydro-hexadecafluorononanoyl)peroxide, di(perfluoropropionyl)peroxide, di(perfluorobutyryl)peroxide, di(perfluoroparyl)peroxide, di(perfluorohexanoyl)peroxide, di(perfluoroheptanoyl)peroxide, di(perfluorooctanoyl)peroxide, di(perfluorononanoyl)peroxide, di(ω-chloro-hexafluorobutyryl)peroxide, and di(ω-chloro-decafluorohexa di(ω-chloro-tetradecafluorooctanoyl) peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexadecafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydrododecafluoroheptanoyl-perfluorobutyryl-peroxide, di(dichloropentafluorobutanoyl) peroxide, di(trichlorooctafluorohexanoyl) peroxide, di(tetrachloroundecafluorooctanoyl) peroxide, di(pentachlorotetradecafluorodecanoyl) peroxide, di(undecachlorotriacontafluorodocosanoyl) peroxide, and the like.

[0060] The water-soluble radical polymerization initiator may be a known water-soluble peroxide, for example, ammonium salts, potassium salts, sodium salts of persulfuric acid, perboric acid, perchloric acid, perphosphoric acid, percarbonic acid, etc., organic peroxides such as disuccinic acid peroxide, diglutaric acid peroxide, t-butyl permalate, t-butyl hydroperoxide, etc. A reducing agent such as a sulfite may be used in combination with the peroxide, and the amount used may be 0.1 to 20 times the amount of the peroxide.

[0061] In the polymerization, a surfactant, a chain transfer agent, and a solvent can be used, and conventionally known surfactants, chain transfer agents, and solvents can be used.

[0062] As the surfactant, a known surfactant can be used, for example, a nonionic surfactant, an anionic surfactant, a cationic surfactant, etc. Among them, a fluorine-containing anionic surfactant is preferable, and a linear or branched fluorine-containing anionic surfactant having 4 to 20 carbon atoms, which may contain ether-bonded oxygen (i.e., an oxygen atom may be inserted between carbon atoms), is more preferable. The amount of the surfactant added (relative to the polymerization water) is preferably 50 to 5000 ppm.

[0063] Examples of the chain transfer agent include hydrocarbons such as ethane, isopentane, n-hexane, and cyclohexane; aromatics such as toluene and xylene; ketones such as acetone; acetates such as ethyl acetate and butyl acetate; alcohols such as methanol and ethanol; mercaptans such as methyl mercaptan; and halogenated hydrocarbons such as carbon tetrachloride, chloroform, methylene chloride, and methyl chloride. The amount of the chain transfer agent to be added may vary depending on the magnitude of the chain transfer constant of the compound used, but is usually used in the range of 0.01 to 20% by mass based on the polymerization solvent.

[0064] The solvent may be water or a mixed solvent of water and alcohol.

[0065] In the suspension polymerization, in addition to water, a fluorine-based solvent may be used. Examples of the fluorine-based solvent include hydrochlorofluoroalkanes such as CH3CClF2, CH3CCl2F, CF3CF2CCl2H, and CF2ClCF2CFHCl; chlorofluoroalkanes such as CF2ClCFClCF2CF3 and CF3CFClCFClCF3; hydrofluoroalkanes such as CF3CFHCFHCF2CF2CF3, CF2HCF2CF2CF2CF2H, and CF3CF2CF2CF2CF2CF2CF2H; CH3OC2F5, CH3OC3F5 Examples of the fluorine-based solvent include hydrofluoroethers such as CF3CF2CH2OCHF2, CF3CHFCF2OCH3, CHF2CF2OCH2F, (CF3)2CHCF2OCH3, CF3CF2CH2OCH2CHF2, and CF3CHFCF2OCH2CF3; and perfluoroalkanes such as perfluorocyclobutane, CF3CF2CF2CF3, CF3CF2CF2CF2CF3, and CF3CF2CF2CF2CF2CF3, among which perfluoroalkanes are preferred. The amount of the fluorine-based solvent used is preferably 10 to 100% by mass relative to the aqueous medium from the standpoints of suspension and economy.

[0066] The polymerization temperature is not particularly limited and may be 0 to 100° C. The polymerization pressure is appropriately determined depending on the type, amount, and vapor pressure of the solvent used, as well as other polymerization conditions such as polymerization temperature, and may usually be 0 to 9.8 MPaG.

[0067] When an aqueous dispersion containing the copolymer is obtained by the polymerization reaction, the copolymer contained in the aqueous dispersion is coagulated, washed, and dried to recover the copolymer. When a slurry is obtained by the polymerization reaction, the copolymer is recovered by removing the slurry from the reaction vessel, washing, and drying. By drying, the copolymer can be recovered in the form of a powder.

[0068] The copolymer obtained by polymerization may be molded into pellets. The molding method for molding into pellets is not particularly limited, and conventionally known methods can be used. For example, a method of melt-extruding the copolymer using a single-screw extruder, a twin-screw extruder, or a tandem extruder, cutting the copolymer to a predetermined length, and molding the copolymer into pellets can be mentioned. The extrusion temperature during melt extrusion needs to be changed depending on the melt viscosity of the copolymer and the manufacturing method, and is preferably from the melting point of the copolymer +20°C to the melting point of the copolymer +140°C. The method of cutting the copolymer is not particularly limited, and conventionally known methods such as a strand cut method, a hot cut method, an underwater cut method, and a sheet cut method can be adopted. The obtained pellets may be heated to remove volatiles in the pellets (degassing treatment). The obtained pellets may be treated by contacting them with hot water at 30 to 200°C, steam at 100 to 200°C, or hot air at 40 to 200°C.

[0069] The copolymer obtained by polymerization may be fluorinated. The fluorination treatment can be carried out by contacting the unfluorinated copolymer with a fluorine-containing compound. The fluorination treatment can convert thermally unstable functional groups of the copolymer, such as -COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, -CONH2, and relatively thermally stable functional groups, such as -CF2H, to extremely thermally stable -CF3. As a result, the total number (functional group number) of -COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, -CONH2, and -CF2H of the copolymer can be easily adjusted to the above-mentioned range.

[0070] The fluorine-containing compound is not particularly limited, but may be a fluorine radical source that generates fluorine radicals under fluorination treatment conditions, such as F2 gas, CoF3, AgF2, UF6, OF2, N2F2, CF3OF, or halogen fluorides (e.g., IF5, ClF3).

[0071] A fluorine radical source such as F2 gas may be of 100% concentration, but from the viewpoint of safety, it is preferable to mix it with an inert gas and dilute it to 5 to 50 mass%, more preferably to dilute it to 15 to 30 mass%. Examples of the inert gas include nitrogen gas, helium gas, and argon gas, and nitrogen gas is preferable from the viewpoint of economy.

[0072] The conditions for the fluorination treatment are not particularly limited, and the copolymer in a molten state may be contacted with a fluorine-containing compound, but the treatment is usually carried out at a temperature below the melting point of the copolymer, preferably 20 to 240°C, more preferably 100 to 220°C. The fluorination treatment is generally carried out for 1 to 30 hours, preferably 5 to 25 hours. The fluorination treatment is preferably carried out by contacting a non-fluorinated copolymer with fluorine gas (F2 gas).

[0073] A composition may be obtained by mixing the copolymer of the present disclosure with other components as necessary, such as fillers, plasticizers, processing aids, release agents, pigments, flame retardants, lubricants, light stabilizers, weather stabilizers, conductive agents, antistatic agents, UV absorbers, antioxidants, foaming agents, fragrances, oils, softeners, and dehydrofluorination agents.

[0074] Examples of the filler include silica, kaolin, clay, organo clay, talc, mica, alumina, calcium carbonate, calcium terephthalate, titanium oxide, calcium phosphate, calcium fluoride, lithium fluoride, cross-linked polystyrene, potassium titanate, carbon, boron nitride, carbon nanotubes, and glass fibers. Examples of the conductive agent include carbon black. Examples of the plasticizer include dioctyl phthalate and pentaerythritol. Examples of the processing aid include carnauba wax, sulfone compounds, low molecular weight polyethylene, and fluorine-based aids. Examples of the dehydrofluorination agent include organic oniums and amidines.

[0075] As the other component, a polymer other than the above-mentioned copolymer may be used. Examples of the other polymer include a fluororesin, a fluororubber, and a non-fluorinated polymer other than the above-mentioned copolymer.

[0076] Examples of a method for producing the above composition include a method of dry mixing the copolymer and other components, and a method of previously mixing the copolymer and other components in a mixer and then melt-kneading them in a kneader, melt extruder, or the like.

[0077] The copolymer of the present disclosure or the above composition can be used as a processing aid, molding material, etc., but is preferably used as a molding material. Aqueous dispersions, solutions, suspensions, and copolymer / solvent systems of the copolymer of the present disclosure are also available, which can be applied as paints, or used for encapsulation, impregnation, and film casting. However, since the copolymer of the present disclosure has the above-mentioned properties, it is preferable to use it as the above-mentioned molding material.

[0078] The copolymer of the present disclosure or the above composition may be molded to obtain a molded body.

[0079] The method for molding the copolymer or the composition is not particularly limited, and examples thereof include injection molding, extrusion, compression, blow, transfer, roto-molding, and roto-lining. As the molding method, among others, extrusion, compression, injection, or transfer molding is preferred, and injection, extrusion, or transfer molding is more preferred, and injection molding is even more preferred, because the molded body can be produced with high productivity. That is, the molded body is preferably an extrusion molded body, a compression molded body, an injection molded body, or a transfer molded body, and more preferably an injection molded body, an extrusion molded body, or a transfer molded body, because the molded body can be produced with high productivity, and injection molding is even more preferred. By molding the copolymer of the present disclosure by injection molding, an injection molded body with a beautiful appearance can be obtained without corroding the mold used for molding.

[0080] Examples of molded articles containing the copolymer of the present disclosure may be nuts, bolts, joints, films, bottles, gaskets, wire coatings, tubes, hoses, pipes, valves, sheets, seals, packing, tanks, rollers, containers, cocks, connectors, filter housings, filter cages, flow meters, pumps, wafer carriers, wafer boxes, and the like.

[0081] The copolymer of the present disclosure, the above-mentioned composition, or the above-mentioned molded article can be used, for example, in the following applications. Food packaging films, lining materials for fluid transfer lines used in food manufacturing processes, packings, sealing materials, sheets and other fluid transfer components for food manufacturing equipment; Chemical stoppers, packaging films, lining materials for fluid transfer lines used in pharmaceutical manufacturing processes, packings, sealing materials, sheets and other chemical transfer components; Inner lining materials for chemical tanks and pipes in chemical plants and semiconductor factories; O-rings, tubes, packing, valve core materials, hoses, seals, etc. used in automobile fuel systems and peripheral devices; hoses, seals, and other fuel transfer materials used in automobile automatic transmission devices; Carburetor flange gaskets, shaft seals, valve stem seals, sealing materials, hoses, etc. used in automobile engines and peripheral devices, automobile brake hoses, air conditioner hoses, radiator hoses, wire covering materials, and other automobile parts; Semiconductor manufacturing equipment O-rings, tubes, packing, valve core materials, hoses, seal materials, rolls, gaskets, diaphragms, joints, and other chemical liquid transfer components for semiconductor equipment; Paint rolls for painting equipment, hoses, tubes, ink containers and other paint and ink components; Food and beverage tubes and food and beverage hoses and other food and beverage transport components such as tubes, hoses, belts, packings, and joints, food packaging materials, and glass cooking equipment; Waste liquid transport components such as tubes and hoses for transporting waste liquid; Components for transporting high-temperature liquids, such as tubes and hoses for transporting high-temperature liquids; Steam piping components such as steam piping tubes and hoses; Anticorrosive tapes for piping, such as tapes wrapped around piping on ship decks, etc.; Various coating materials such as electric wire coating materials, optical fiber coating materials, transparent front coating materials and back coating materials to be applied to the light incident surface of photovoltaic elements of solar cells; Sliding parts such as diaphragms in diaphragm pumps and various packings; Agricultural films, weather-resistant covers for various roofing materials and side walls; Interior materials used in the construction industry, and glass covering materials such as non-flammable fire-resistant safety glass; Lining materials such as laminated steel sheets used in the home appliance sector, etc.;

[0082] Further examples of the fuel transfer members used in the fuel systems of the above-mentioned automobiles include fuel hoses, filler hoses, evaporative hoses, etc. The above-mentioned fuel transfer members can also be used as fuel transfer members for sour gasoline, alcohol-resistant fuels, and fuels containing gasoline additives such as methyl tertiary butyl ether and amine-resistant fuels.

[0083] The above-mentioned chemical stoppers and packaging films for chemicals have excellent chemical resistance against acids, etc. Another example of the above-mentioned chemical liquid transfer member is anticorrosive tape wrapped around piping in chemical plants.

[0084] Examples of the molded article include radiator tanks for automobiles, chemical tanks, bellows, spacers, rollers, gasoline tanks, containers for transporting waste liquids, containers for transporting high-temperature liquids, and fishery / fish farming tanks.

[0085] Further examples of the molded article include parts used for automobile bumpers, door trims, instrument panels, food processing equipment, cooking appliances, water- and oil-repellent glass, lighting-related equipment, display panels and housings for office automation equipment, illuminated signs, displays, liquid crystal displays, mobile phones, printed circuit boards, electric and electronic components, miscellaneous goods, trash cans, bathtubs, unit baths, ventilation fans, lighting frames, etc.

[0086] Molded articles containing the copolymer of the present disclosure have excellent abrasion resistance, low nitrogen permeability, low chemical permeability, low water vapor permeability, rigidity at high temperatures of 110°C, high-temperature tensile creep properties, resistance to deterioration under repeated loads, extremely long-term ozone resistance, and sealing properties and non-stick properties at high temperatures, and therefore can be suitably used for nuts, bolts, joints, packings, valves, cocks, connectors, filter housings, filter cages, flow meters, pumps, and the like.

[0087] The molded article containing the copolymer of the present disclosure can be easily manufactured by injection molding without corroding the mold, and has excellent abrasion resistance, low nitrogen permeability, low chemical permeability, low water vapor permeability, rigidity at a high temperature of 110°C, high temperature tensile creep properties, resistance to deterioration against repeated loads, extremely long-term ozone resistance, sealing properties and non-adhesiveness at high temperatures, and is not likely to elute fluorine ions into the electrolyte, so it can be suitably used as a compressed member such as a gasket or packing. The compressed member of the present disclosure may be a gasket or packing. The gasket or packing of the present disclosure can be manufactured at low cost by injection molding without corroding the mold, is not likely to be damaged even when installed in a location where frequent opening and closing is repeated, and has excellent sealing properties at high temperatures, low nitrogen permeability, low chemical permeability, and low water vapor permeability. The compressed member of the present disclosure has excellent abrasion resistance, low chemical permeability, extremely long-term ozone resistance, sealing properties at high temperatures, low chemical permeability, and low water vapor permeability, and can therefore be suitably used as a piping member for transporting chemicals that do not tolerate the inclusion of moisture such as water vapor in the outside air.

[0088] The compressed member of the present disclosure exhibits high sealing pressure even when deformed at a high compression deformation rate. The compressed member of the present disclosure can be used in a state compressed and deformed at a compression deformation rate of 10% or more, and can be used in a state compressed and deformed at a compression deformation rate of 20% or more or 25% or more. By using the compressed member of the present disclosure after being deformed at such a high compression deformation rate, a certain level of resilience can be maintained for a long period of time, and sealing and insulating properties can be maintained for a long period of time.

[0089] The compressed member of the present disclosure exhibits a high storage modulus, a high recovery amount, and a high sealing pressure even when deformed at a high compression deformation rate at high temperatures. The compressed member of the present disclosure can be used in a state where it is compressed and deformed at 150°C or higher and a compression deformation rate of 10% or more, and can be used in a state where it is compressed and deformed at 150°C or higher and a compression deformation rate of 20% or more or 25% or more. By using the compressed member of the present disclosure after being deformed at such a high temperature and high compression deformation rate, a certain rebound resilience can be maintained for a long period of time even at high temperatures, and the sealing properties and insulating properties at high temperatures can be maintained for a long period of time.

[0090] The above compression deformation ratio is the compression deformation ratio of the part with the largest compression deformation ratio when the compressed member is used in a compressed state. For example, when a flat compressed member is used in a state compressed in its thickness direction, it is the compression deformation ratio in the thickness direction. Also, for example, when the compressed member is used in a state where only a part of it is compressed, it is the compression deformation ratio of the part with the largest compression deformation ratio among the compressed parts.

[0091] The size and shape of the compressed member of the present disclosure may be appropriately set depending on the application, and are not particularly limited. The shape of the compressed member of the present disclosure may be, for example, annular. In addition, the compressed member of the present disclosure may have a shape such as a circle, an oval, or a rectangle with rounded corners in a plan view, and may have a through hole in the center.

[0092] The compressed member of the present disclosure is preferably used as a piping member for passing a chemical liquid such as ozone water. The compressed member of the present disclosure is particularly suitable as a member used in contact with ozone water, since it has excellent long-term ozone resistance, sealing property at high temperatures, abrasion resistance, low chemical liquid permeability, and low water vapor permeability. That is, the compressed member of the present disclosure may have a surface in contact with ozone water.

[0093] The compressed member of the present disclosure is preferably used as a member for constituting a nonaqueous electrolyte battery. The compressed member of the present disclosure has excellent abrasion resistance, low permeability to chemicals, and low permeability to water vapor, excellent sealing properties at high temperatures, rigidity at high temperatures of 110°C, high-temperature tensile creep properties, and resistance to deterioration against repeated loads, and is not prone to dissolving fluorine ions into the electrolyte, and is therefore particularly suitable as a member used in contact with the nonaqueous electrolyte in a nonaqueous electrolyte battery. That is, the compressed member of the present disclosure may have a surface in contact with the nonaqueous electrolyte in a nonaqueous electrolyte battery.

[0094] The compressed member of the present disclosure is unlikely to dissolve fluorine ions into the non-aqueous electrolyte. Therefore, by using the compressed member of the present disclosure, it is possible to suppress an increase in the fluorine ion concentration in the non-aqueous electrolyte. As a result, by using the compressed member of the present disclosure, it is possible to suppress the generation of gases such as HF in the non-aqueous electrolyte battery, and to suppress the deterioration of the battery performance and the shortening of the life of the non-aqueous electrolyte battery.

[0095] Since the compressed member of the present disclosure can further suppress the generation of gases such as HF in a nonaqueous electrolyte battery and can further suppress the deterioration of battery performance and shortening of life of the nonaqueous electrolyte battery, the amount of eluted fluorine ions detected in an electrolyte immersion test is preferably 1.0 ppm or less, more preferably 0.8 ppm or less, and more preferably 0.7 ppm or less, based on mass. The electrolyte immersion test can be performed by preparing a test piece having a weight equivalent to 10 molded bodies (15 mm x 15 mm x 0.2 mm) using the compressed member, placing the test piece and 2 g of dimethyl carbonate (DMC) in a glass sample bottle in a thermostatic chamber at 80°C, and leaving it for 144 hours.

[0096] The compressed member of the present disclosure is difficult to transmit water vapor. Therefore, by using the compressed member of the present disclosure, it is possible to suppress the transmission of water vapor from the outside to the secondary battery. As a result, by using the compressed member of the present disclosure, it is possible to suppress the deterioration of the battery performance and the shortening of the life of the nonaqueous electrolyte battery.

[0097] The water vapor permeability of the compressed member of the present disclosure is preferably 14.0 g cm / m because this can further suppress deterioration of the battery performance and shortening of the life of the nonaqueous electrolyte battery. 2 less than or equal to 13.5 g cm / m 2 or less, and more preferably 13.0 g cm / m 2 The water vapor permeability of the compressed member can be measured at a temperature of 95°C for 30 days. The copolymer of the present disclosure has excellent low water vapor permeability because the content of PPVE units, melt flow rate (MFR), and number of functional groups of the copolymer containing TFE units and PPVE units are appropriately adjusted. Therefore, when a molded article containing the copolymer of the present disclosure is used as a piping member (e.g., packing, gasket) for supplying ozone water, the penetration of water vapor into the piping member can be suppressed, and therefore the amount of ozone that penetrates into the piping member together with water vapor can be reduced, so that the excellent ozone resistance of the piping member can be maintained for a long period of time.

[0098] The nonaqueous electrolyte battery is not particularly limited as long as it is a battery containing a nonaqueous electrolyte, and examples thereof include a lithium ion secondary battery, a lithium ion capacitor, etc. Examples of members constituting the nonaqueous electrolyte battery include a sealing member, an insulating member, etc.

[0099] The non-aqueous electrolyte is not particularly limited, but one or more of known solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate can be used. The non-aqueous electrolyte battery may further include an electrolyte. The electrolyte is not particularly limited, but LiClO4, LiAsF6, LiPF6, LiBF4, LiCl, LiBr, CH3SO3Li, CF3SO3Li, cesium carbonate, and the like can be used.

[0100] The compressed member of the present disclosure can be suitably used as, for example, a sealing member such as a sealing gasket or sealing packing, or an insulating member such as an insulating gasket or insulating packing. A sealing member is a member used to prevent leakage of liquid or gas or intrusion of liquid or gas from the outside. An insulating member is a member used to insulate electricity. The compressed member of the present disclosure may be a member used for both sealing and insulating purposes.

[0101] The compressed member of the present disclosure has excellent heat resistance and excellent sealing properties at high temperatures, and therefore can be suitably used in high-temperature environments. For example, the compressed member of the present disclosure is suitably used in an environment where the maximum temperature is 40° C. or higher. For example, the compressed member of the present disclosure is suitably used in an environment where the maximum temperature is 150° C. or higher. Examples of cases in which the compressed member of the present disclosure may reach such high temperatures include a case in which the compressed member is attached to a battery in a compressed state and then other battery components are attached to the battery by welding, and a case in which a nonaqueous electrolyte battery generates heat.

[0102] The compressed member of the present disclosure has excellent low water vapor permeability, excellent sealing properties at high temperatures, and is unlikely to dissolve fluorine ions into the electrolyte, and therefore can be suitably used as a sealing member for a nonaqueous electrolyte battery or an insulating member for a nonaqueous electrolyte battery. For example, when a battery such as a nonaqueous electrolyte secondary battery is charged, the temperature of the battery may temporarily reach 40°C or higher, particularly temporarily reach 150°C or higher. The compressed member of the present disclosure does not lose its high resilience even when it is used in a battery such as a nonaqueous electrolyte secondary battery after being deformed at a high compression deformation rate at high temperatures, and even when it comes into contact with a nonaqueous electrolyte at high temperatures. Therefore, when the compressed member of the present disclosure is used as a sealing member, it has excellent sealing properties and the sealing properties are maintained for a long period of time even at high temperatures. In addition, the compressed member of the present disclosure has excellent insulating properties because it contains the above-mentioned copolymer. Therefore, when the compressed member of the present disclosure is used as an insulating member, it firmly adheres to two or more conductive members to prevent short circuits for a long period of time.

[0103] The copolymer of the present disclosure is unlikely to corrode the core wire to be covered. Furthermore, by molding the copolymer of the present disclosure by extrusion molding, a very thick coating layer can be formed with a uniform thickness on a core wire with a very large diameter, and therefore the copolymer can be suitably used as a material for forming an electric wire coating. Therefore, a coated electric wire having a coating layer containing the copolymer of the present disclosure has excellent electrical properties because the core wire is unlikely to corrode and there is almost no change in the outer diameter.

[0104] When attempting to form a very thick coating layer of uniform thickness on a core wire with a very large diameter, it takes time for the molten coating layer to solidify, and the coating layer is also heavy, so when using conventional copolymers, the coating layer deforms under its own weight before solidifying, making it difficult to form a coating layer of uniform thickness. By using the copolymer of the present disclosure, it is possible to form a very thick coating layer of uniform thickness.

[0105] The coated electric wire comprises a core wire and a coating layer that is provided around the core wire and contains the copolymer of the present disclosure. For example, the coating layer can be an extrusion molded body obtained by melt-extrusion molding the copolymer of the present disclosure onto the core wire. The coated electric wire is suitable for use as a high-frequency transmission cable, a flat cable, a heat-resistant cable, etc., and is particularly suitable for use as a high-frequency transmission cable.

[0106] The core wire may be made of a metal conductor material such as copper or aluminum. The core wire preferably has a diameter of 0.02 to 3 mm. The core wire preferably has a diameter of 0.04 mm or more, more preferably 0.05 mm or more, and particularly preferably 0.1 mm or more. The core wire preferably has a diameter of 2 mm or less.

[0107] Specific examples of the core wire include AWG (American Wire Gauge)-46 (solid copper wire with a diameter of 40 micrometers), AWG-26 (solid copper wire with a diameter of 404 micrometers), AWG-24 (solid copper wire with a diameter of 510 micrometers), and AWG-22 (solid copper wire with a diameter of 635 micrometers).

[0108] The thickness of the coating layer is preferably 0.1 to 3.0 mm. It is also preferable that the thickness of the coating layer is 2.0 mm or less.

[0109] An example of a high-frequency transmission cable is a coaxial cable. A coaxial cable generally has a structure in which an internal conductor, an insulating coating layer, an external conductor layer, and a protective coating layer are laminated in this order from the core to the outer periphery. A molded article containing the copolymer of the present disclosure can be suitably used as an insulating coating layer containing a copolymer. The thickness of each layer in the above structure is not particularly limited, but usually, the internal conductor has a diameter of about 0.1 to 3 mm, the insulating coating layer has a thickness of about 0.3 to 3 mm, the external conductor layer has a thickness of about 0.5 to 10 mm, and the protective coating layer has a thickness of about 0.5 to 2 mm.

[0110] The coating layer may contain bubbles, and it is preferable that the bubbles are uniformly distributed in the coating layer.

[0111] The average bubble diameter of the bubbles is not limited, but is preferably 60 μm or less, more preferably 45 μm or less, even more preferably 35 μm or less, even more preferably 30 μm or less, particularly preferably 25 μm or less, and even more preferably 23 μm or less. The average bubble diameter is preferably 0.1 μm or more, and more preferably 1 μm or more. The average bubble diameter can be determined by taking an electron microscope image of the cross section of the electric wire, calculating the diameter of each bubble by image processing, and averaging the results.

[0112] The coating layer may have an expansion rate of 20% or more. More preferably, it is 30% or more, even more preferably, it is 33% or more, and even more preferably, it is 35% or more. There is no particular upper limit, but it is, for example, 80%. The upper limit of the expansion rate may be 60%. The expansion rate is a value calculated by ((specific gravity of electric wire coating material-specific gravity of coating layer) / specific gravity of electric wire coating material)×100. The expansion rate can be appropriately adjusted according to the application, for example, by adjusting the amount of gas inserted in the extruder described later, or by selecting the type of gas to be dissolved.

[0113] The coated electric wire may have another layer between the core wire and the coating layer, or may have another layer (outer layer) around the coating layer. When the coating layer contains bubbles, the electric wire of the present disclosure may have a two-layer structure (skin-foam) in which a non-foamed layer is inserted between the core wire and the coating layer, a two-layer structure (foam-skin) in which the outer layer is coated with a non-foamed layer, or even a three-layer structure (skin-foam-skin) in which the outer layer of skin-foam is coated with a non-foamed layer. The non-foamed layer is not particularly limited, and may be a resin layer made of a resin such as a TFE / HFP copolymer, a TFE / PAVE copolymer, a TFE / ethylene copolymer, a vinylidene fluoride polymer, a polyolefin resin such as polyethylene (PE), or polyvinyl chloride (PVC).

[0114] The coated electric wire can be produced, for example, by using an extruder to heat the copolymer and extrude the copolymer in a molten state onto a core wire to form a coating layer.

[0115] When forming the coating layer, the copolymer is heated and in the molten state, a gas is introduced into the copolymer to form the coating layer containing bubbles. As the gas, for example, chlorodifluoromethane, nitrogen, carbon dioxide, or a mixture of the above gases can be used. The gas may be introduced into the heated copolymer as a pressurized gas, or may be generated by mixing a chemical foaming agent into the copolymer. The gas dissolves in the molten copolymer.

[0116] Moreover, the copolymer of the present disclosure can be suitably used as a material for high-frequency signal transmission products.

[0117] The above-mentioned high-frequency signal transmission products are not particularly limited as long as they are products used for transmitting high-frequency signals, and examples thereof include (1) insulating plates for high-frequency circuits, insulators for connecting parts, molded plates such as printed wiring boards, (2) molded bodies such as bases for high-frequency vacuum tubes and antenna covers, and (3) coated electric wires such as coaxial cables and LAN cables. The above-mentioned high-frequency signal transmission products can be suitably used in devices that utilize microwaves, particularly microwaves of 3 to 30 GHz, such as satellite communication devices and mobile phone base stations.

[0118] In the above-mentioned high-frequency signal transmission product, the copolymer of the present disclosure can be suitably used as an insulator because of its low dielectric tangent.

[0119] The above (1) molded plate is preferably a printed wiring board in that it can obtain good electrical properties. The above printed wiring board is not particularly limited, but examples thereof include printed wiring boards for electronic circuits of mobile phones, various computers, communication devices, etc. The above (2) molded body is preferably an antenna cover in that it has low dielectric loss.

[0120] The copolymer of the present disclosure can be molded by injection molding to obtain a beautiful sheet. In addition, the molded article containing the copolymer of the present disclosure has low nitrogen permeability, low chemical permeability, low water vapor permeability, and excellent non-adhesiveness. Therefore, the molded article containing the copolymer of the present disclosure can be suitably used as a film or sheet.

[0121] The film of the present disclosure has particularly excellent non-adhesive properties, and therefore, even when the film of the present disclosure is heat-pressed with a resin such as an epoxy resin, a toner, or the like, the two do not adhere to each other, and the resin, toner, or the like can be peeled off from the film.

[0122] The film of the present disclosure is useful as a release film. The release film can be produced by molding the copolymer of the present disclosure by melt extrusion molding, calendar molding, press molding, casting molding, etc. From the viewpoint of obtaining a uniform thin film, the release film can be produced by melt extrusion molding.

[0123] The film of the present disclosure can be applied to the surface of rolls used in OA equipment. The copolymer of the present disclosure can also be molded into a required shape by extrusion molding, compression molding, press molding, or the like to form a sheet, film, or tube, and used as a surface material for OA equipment rolls or OA equipment belts, etc. In particular, thin-walled tubes and films can be produced by the melt extrusion molding method.

[0124] A molded article containing the copolymer of the present disclosure has excellent abrasion resistance, low nitrogen permeability, low chemical permeability, low water vapor permeability, rigidity at a high temperature of 110°C, high-temperature tensile creep characteristics, resistance to deterioration under repeated load, extremely long-term ozone resistance, sealing properties and non-stickiness at high temperatures, and is also unlikely to elute fluoride ions into an electrolyte, and therefore can be suitably used as a bottle or tube.

[0125] Although the embodiments have been described above, it will be understood that various changes in form and details are possible without departing from the spirit and scope of the claims. EXAMPLES

[0126] Next, embodiments of the present disclosure will be described with reference to examples, but the present disclosure is not limited to these examples.

[0127] The values ​​in the examples were measured by the following methods.

[0128] (Monomer unit content) The content of each monomer unit was measured by an NMR analyzer (for example, AVANCE300 high temperature probe manufactured by Bruker Biospin).

[0129] (Melt Flow Rate (MFR)) According to ASTM D1238, the mass of polymer flowing out per 10 minutes (g / 10 minutes) from a nozzle with an inner diameter of 2.1 mm and a length of 8 mm under a load of 5 kg at 372°C was determined using a Melt Indexer G-01 (manufactured by Toyo Seiki Seisakusho).

[0130] (Number of functional groups) The copolymer pellets were molded by cold pressing to prepare a film with a thickness of 0.25 to 0.30 mm. This film was scanned 40 times using a Fourier transform infrared spectrometer [FT-IR (Spectrum One, manufactured by PerkinElmer)] to obtain an infrared absorption spectrum, and a difference spectrum was obtained from the base spectrum, which was completely fluorinated and had no functional groups. From the absorption peaks of specific functional groups that appeared in this difference spectrum, the ratio of carbon atoms in the sample to carbon atoms in the sample was calculated according to the following formula (A): 6 The number of functional groups per unit, N, was calculated. N=I×K / t (A) I: Absorbance K: Correction coefficient t: film thickness (mm) For reference, the absorption frequencies, molar extinction coefficients, and correction coefficients for the functional groups in this disclosure are shown in Table 2. The molar extinction coefficients were determined from FT-IR measurement data of low molecular weight model compounds.

[0131] [Table 2]

[0132] (Melting Point) Using a differential scanning calorimeter (product name: X-DSC7000, manufactured by Hitachi High-Tech Science Corporation), the sample was heated a first time from 200°C to 350°C at a heating rate of 10°C / min, then cooled from 350°C to 200°C at a cooling rate of 10°C / min, and then heated a second time from 200°C to 350°C at a heating rate of 10°C / min. The melting point was determined from the melting curve peak occurring during the second heating process.

[0133] Example 1 26.6L of pure water was put into a 174L autoclave, and after sufficient nitrogen replacement, 30.4kg of perfluorocyclobutane, 1.21kg of perfluoro(propyl vinyl ether) (PPVE), and 0.26kg of methanol were charged, and the temperature in the system was kept at 35°C and the stirring speed at 200 rpm. Next, tetrafluoroethylene (TFE) was pumped in up to 0.58MPa, and then 0.010kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added to start polymerization. As the polymerization proceeded, the pressure in the system decreased, so TFE was continuously fed to keep the pressure constant, and 0.043kg of PPVE was added for every 1kg of TFE fed, and polymerization was continued for 6 hours. After releasing TFE and returning the autoclave to atmospheric pressure, the reaction product obtained was washed with water and dried to obtain 15kg of powder.

[0134] The obtained powder was melt-extruded at 360°C using a screw extruder (product name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of a TFE / PPVE copolymer. The PPVE content of the obtained pellets was measured by the method described above. The results are shown in Table 3.

[0135] The obtained pellets were placed in a vacuum vibration reactor VVD-30 (manufactured by Okawara Manufacturing Co., Ltd.) and heated to 210°C. After evacuation, F2 gas diluted to 20% by volume with N2 gas was introduced up to atmospheric pressure. 0.5 hours after the introduction of F2 gas, evacuation was performed once and F2 gas was introduced again. Another 0.5 hours later, evacuation was performed again and F2 gas was introduced again. Thereafter, the above-mentioned F2 gas introduction and evacuation operation was performed once every hour, and the reaction was carried out at a temperature of 210°C for 10 hours. After the reaction was completed, the inside of the reactor was sufficiently replaced with N2 gas to complete the fluorination reaction. Various physical properties were measured using the fluorinated pellets by the above-mentioned methods. The results are shown in Table 3.

[0136] Example 2 Fluorinated pellets were obtained in the same manner as in Example 1, except that 1.32 kg of PPVE, 0.31 kg of methanol, 0.046 kg of PPVE was added for every 1 kg of TFE fed, the polymerization time was 6.5 hours, the temperature rise temperature of the vacuum vibrating reactor was 170° C., and the reaction was carried out at a temperature of 170° C. for 5 hours. The results are shown in Table 3.

[0137] Example 3 Fluorinated pellets were obtained in the same manner as in Example 1, except that 1.40 kg of PPVE, 0.31 kg of methanol, 0.048 kg of PPVE per kg of TFE fed, and the polymerization time were changed to 6.5 hours. The results are shown in Table 3.

[0138] Example 4 Fluorinated pellets were obtained in the same manner as in Example 1, except that 1.48 kg of PPVE, 0.35 kg of methanol, 0.050 kg of PPVE per kg of TFE fed, and the polymerization time were changed to 6.5 hours. The results are shown in Table 3.

[0139] Comparative Example 1 Fluorinated pellets were obtained in the same manner as in Example 1, except that the amounts of PPVE and methanol were changed to 0.97 kg and 0.37 kg, respectively, and 0.036 kg of PPVE was added for every 1 kg of TFE fed. The results are shown in Table 3.

[0140] Comparative Example 2 Fluorinated pellets were obtained in the same manner as in Example 1, except that 1.05 kg of PPVE, 0.29 kg of methanol, 0.038 kg of PPVE per kg of TFE fed, and the polymerization time were changed to 5.5 hours. The results are shown in Table 3.

[0141] Comparative Example 3 Fluorinated pellets were obtained in the same manner as in Example 1, except that the amounts of PPVE and methanol were changed to 1.32 kg and 0.10 kg, respectively, and 0.046 kg of PPVE was added for every 1 kg of TFE fed. The results are shown in Table 3.

[0142] Comparative Example 4 51.8L of pure water was put into a 174L autoclave, and after sufficient nitrogen replacement, 40.9kg of perfluorocyclobutane, 2.24kg of perfluoro(propyl vinyl ether) (PPVE), and 1.85kg of methanol were charged, and the temperature in the system was kept at 35°C and the stirring speed at 200 rpm. Next, tetrafluoroethylene (TFE) was pumped in up to 0.64MPa, and then 0.051kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was pumped in to start polymerization. As the polymerization proceeded, the pressure in the system decreased, so TFE was continuously fed in to keep the pressure constant, and 0.049kg of PPVE was added for every 1kg of TFE fed. The polymerization was terminated when the amount of TFE added reached 40.9kg. After releasing the unreacted TFE and returning the autoclave to atmospheric pressure, the reaction product obtained was washed with water and dried to obtain 41.0kg of powder.

[0143] The obtained powder was melt extruded to obtain non-fluorinated pellets in the same manner as in Example 1. The results are shown in Table 3.

[0144] Comparative Example 5 51.8L of pure water was put into a 174L autoclave, and after sufficient nitrogen replacement, 40.9kg of perfluorocyclobutane, 1.85kg of perfluoro(propyl vinyl ether) (PPVE), and 3.36kg of methanol were charged, and the temperature in the system was kept at 35°C and the stirring speed at 200 rpm. Next, tetrafluoroethylene (TFE) was pumped in up to 0.64MPa, and then 0.051kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was pumped in to start polymerization. As the polymerization proceeded, the pressure in the system decreased, so TFE was continuously fed in to keep the pressure constant, and 0.043kg of PPVE was added for every 1kg of TFE fed. The polymerization was terminated when the amount of TFE added reached 40.9kg. After releasing the unreacted TFE and returning the autoclave to atmospheric pressure, the reaction product obtained was washed with water and dried to obtain 41.0kg of powder.

[0145] Using the obtained powder, a fluorination reaction was carried out in the same manner as in Example 1 to obtain fluorinated pellets. The results are shown in Table 3.

[0146] Comparative Example 6 Fluorinated pellets were obtained in the same manner as in Comparative Example 5, except that 2.53 kg of PPVE, 3.42 kg of methanol, 0.026 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate, and 0.055 kg of PPVE were added for every 1 kg of TFE fed, to obtain 41.0 kg of dry powder. The results are shown in Table 3.

[0147] [Table 3]

[0148] In Table 3, "<6" means that the number of functional groups is less than 6.

[0149] The pellets thus obtained were then evaluated for the following properties, the results of which are shown in Table 4.

[0150] (Storage modulus (E')) Dynamic viscoelasticity was measured using a DVA-220 (manufactured by IT Measurement & Control Co., Ltd.) A heat press molded sheet measuring 25 mm in length, 5 mm in width, and 0.2 mm in thickness was used as a sample test piece, and measurements were performed in the range of 30°C to 250°C under conditions of a heating rate of 2°C / min and a frequency of 10 Hz, and the storage modulus (MPa) at 150°C was read.

[0151] (Restored amount) The amount of recovery was measured according to the method described in ASTM D395 or JIS K6262:2013.

[0152] About 2 g of the pellets were put into a mold (inner diameter 13 mm, height 38 mm), and the pellets were melted at 370 ° C for 30 minutes using a hot plate press, and then water-cooled while being pressurized at a pressure of 0.2 MPa (resin pressure) to produce a molded body with a height of about 8 mm. The molded body obtained was then cut to produce a test piece with an outer diameter of 13 mm and a height of 6 mm. The test piece thus produced was compressed at room temperature to a compression deformation rate of 50% using a compression device (i.e., a test piece with a height of 6 mm was compressed to a height of 3 mm). The compressed test piece was fixed to the compression device and placed in an electric furnace and left at 150 ° C for 18 hours. The compression device was removed from the electric furnace, cooled to room temperature, and the test piece was removed. The collected test piece was left at room temperature for 30 minutes, and then the height of the collected test piece was measured, and the recovery amount was calculated using the following formula. Recovery amount (mm) = t2-t1 t1: Spacer height (mm) t2: Height of the test piece removed from the compression device (mm) In the above test, t1=3 mm.

[0153] (Seal pressure at 150℃) From the results of the compression set test at 150°C and the results of the storage modulus measurement at 150°C, the 150°C seal pressure was calculated according to the following formula. 150℃ sealing pressure (MPa) = (t2-t1) / t1×E' t1: Spacer height (mm) t2: Height of the test piece removed from the compression device (mm) E': Storage modulus at 150℃ (MPa)

[0154] (Water vapor permeability) Using the pellets and a heat press molding machine, a sheet-like test piece with a thickness of about 0.2 mm was prepared. The test cup (permeation area 12.56 cm2) was 2 The sheet test piece was placed in a container containing 18 g of water, covered with a sheet test piece, and then clamped with a PTFE gasket to seal. The sheet test piece was placed in contact with the water and held at 95°C for 30 days, then removed and left at room temperature for 2 hours before measuring the amount of mass loss. The water vapor permeability (g cm / m 2 ) was measured. Water vapor permeability (g cm / m 2 ) = mass loss (g) × thickness of sheet specimen (cm) / permeation area (m 2 )

[0155] (Injection moldability) The copolymer was injection molded using an injection molding machine (SE50EV-A, manufactured by Sumitomo Heavy Industries, Ltd.) with a cylinder temperature of 395°C, a mold temperature of 220°C, and an injection speed of 3 mm / s. The mold used was a Cr-plated HPM38 mold (100 mm x 100 mm x 3 mmt, film gate, flow length from the gate was 100 mm). The obtained injection molded body was observed and evaluated according to the following criteria. The presence or absence of cloudiness was confirmed visually. The presence or absence of surface roughness was confirmed by touching the surface of the injection molded body. 3: The entire injection molded product is transparent and the entire surface is smooth. 2: White turbidity is observed within 1 cm of the mold gate, and the entire surface is smooth. 1: White turbidity is observed within 1 cm of where the mold gate was located, and surface roughness is confirmed within 1 cm of where the mold gate was located. 0: The copolymer is not filled entirely into the mold, and a molded product with the desired shape cannot be obtained.

[0156] (Electrolyte immersion test) Approximately 5 g of pellets were placed in a mold (inner diameter 120 mm, height 38 mm) and melted for 20 minutes at 370°C using a hot plate press, then water-cooled while being pressurized at 1 MPa (resin pressure) to produce a molded body with a thickness of approximately 0.2 mm. Test pieces measuring 15 mm square were then made using the molded body obtained.

[0157] Ten of the obtained test pieces and 2 g of dimethyl carbonate (DMC) were placed in a 20 mL glass sample bottle, and the lid of the sample bottle was closed. The sample bottle was placed in a thermostatic chamber at 80 ° C. and left for 144 hours to immerse the test pieces in DMC. The sample bottle was then removed from the thermostatic chamber and cooled to room temperature, after which the test pieces were removed from the sample bottle. The DMC remaining after the test pieces were removed was air-dried in a room controlled at 25 ° C. for 24 hours while still in the sample bottle, and 2 g of ultrapure water was added. The obtained aqueous solution was transferred to the measurement cell of an ion chromatography system, and the amount of fluorine ions in this aqueous solution was measured by an ion chromatography system (Dionex ICS-2100 manufactured by Thermo Fisher Scientific).

[0158] (Mold corrosion test) 20 g of pellets were placed in a glass container (50 ml screw tube), and a metal pillar (5 mm square, 30 mm long) made of HPM38 (Cr plating) or HPM38 (Ni plating) was hung from the glass container so as not to touch the pellets. The glass container was then covered with aluminum foil. The glass container was placed in an oven in this state and heated at 380°C for 3 hours. The heated glass container was then removed from the oven and cooled to room temperature, and the degree of corrosion on the surface of the metal pillar was visually observed. The degree of corrosion was judged according to the following criteria. ○: No corrosion observed △: Slight corrosion observed ×: Corrosion is observed

[0159] (Wire coating test) Using a 30 mmφ electric wire coating molding machine (manufactured by Tanabe Plastic Machinery Co., Ltd.), the copolymer was extruded onto a copper conductor having a conductor diameter of 1.00 mm to the following coating thickness to obtain a coated electric wire. The electric wire coating extrusion molding conditions were as follows. a) Core conductor: Conductor diameter 1.00 mm b) Coating thickness: 0.50 mm c) Insulated wire diameter: 2.00 mm d) Wire withdrawal speed: 7m / min e) Extrusion conditions: Single-screw extruder with cylinder diameter of 20 mm and L / D of 22 Die (inner diameter) / chip (outer diameter) = 30.0mm / 10.0mm Extruder temperature settings: Barrel C-1 (330°C), Barrel C-2 (360°C), Barrel C-3 (375°C), Head H (390°C), Die D-1 (405°C), Die D-2 (395°C). Core wire preheating was set at 80°C.

[0160] (Outer diameter variation) The outer diameter of the obtained coated electric wire was measured continuously for one hour using an outer diameter measuring device (ODAC18XY manufactured by Zumbach). The outer diameter fluctuation value was obtained by rounding off the third decimal place of the outer diameter value that was the largest deviation from the specified outer diameter value (2.00 mm) among the measured outer diameter values. The ratio of the absolute value of the difference between the specified outer diameter and the outer diameter fluctuation value relative to the specified outer diameter (2.00 mm) (the outer diameter fluctuation rate) was calculated and evaluated according to the following criteria. (Outer diameter fluctuation rate (%)) = | (Outer diameter fluctuation value) - (Predetermined outer diameter) | / (Predetermined outer diameter) x 100 ±1%: The variation rate of the outer diameter is 1% or less. ±2%: The fluctuation rate of the outer diameter is more than 1% and less than 2%. ×: The fluctuation rate of the outer diameter is more than 2%.

[0161] (Core Corrosion Test) The obtained coated wire was cut into a length of 20 cm and left to stand for two weeks in a thermo-hygrostat (Junior SD-01, manufactured by FATC) at 60°C and humidity of 95%. After that, the coating layer was peeled off to expose the conductor, and the surface of the conductor was visually observed and evaluated according to the following criteria. ○: No corrosion observed ×: Corrosion is observed

[0162] (Toner release test) A film was produced using a φ14 mm extruder (manufactured by Imoto Manufacturing Co., Ltd.) and a T-die. The extrusion molding conditions were as follows: a) Winding speed: 1m / min b) Roll temperature: 120℃ c) Film width: 70mm d) Thickness: 0.10mm e) Extrusion conditions: Single-screw extruder with cylinder diameter of 14 mm and L / D of 20 Extruder temperature settings: Barrel section C-1 (330°C), Barrel section C-2 (350°C), Barrel section C-3 (370°C), T-die section (380°C)

[0163] A 50 mm x 50 mm test piece was cut out from the obtained 0.10 mm thick film, the obtained test piece was placed on a SUS tray, 3 g of black toner powder was spread on top of it in a circular shape with a diameter of about 30 mm, the tray's lid was closed, and the tray was placed in a thermostatic chamber heated to 160°C with the inside being a closed space. After 10 minutes, the tray was removed and allowed to cool to room temperature, and then the test piece was removed from the tray. The molten and solidified black toner was peeled off from the test piece, and the peeled surface of the test piece was visually observed and evaluated according to the following criteria. ○: No black deposits were observed on the peeled surface of the test piece. ×: Black deposits were observed on the peeled surface of the test piece.

[0164] (Wear test) Using pellets and a heat press molding machine, a sheet-like test piece with a thickness of about 0.2 mm was prepared, and a test piece of 10 cm x 10 cm was cut out from it. The prepared test piece was fixed on the test stand of a Taber abrasion tester (No. 101 special type Taber abrasion tester, manufactured by Yasuda Seiki Seisakusho Co., Ltd.), and an abrasion test was performed using the Taber abrasion tester under the conditions of a load of 500 g, an abrasion wheel CS-10 (polished 20 times with abrasive paper #240), and a rotation speed of 60 rpm. The weight of the test piece after 1000 rotations was measured, and the weight of the test piece was measured after another 10,000 rotations of the same test piece. The amount of abrasion was calculated using the following formula. Wear amount (mg)=M1-M2 M1: Test piece weight after 1000 rotations (mg) M2: Test piece weight after 10,000 rotations (mg)

[0165] (Nitrogen permeability coefficient) Using the pellets and a heat press molding machine, a sheet-like test piece with a thickness of about 0.1 mm was produced. The obtained test piece was used to measure the nitrogen permeability using a differential pressure gas permeability meter (L100-5000 gas permeability meter, manufactured by Systech Illinois) according to the method described in JIS K7126-1:2006. Permeability area: 50.24 cm 2 The nitrogen permeability was measured at a test temperature of 70°C and a test humidity of 0%RH. The nitrogen permeability coefficient was calculated from the obtained nitrogen permeability and the thickness of the test piece according to the following formula. Nitrogen permeability coefficient (cm 3 mm / (m 2 ·24h·atm))=GTR×d GTR: Nitrogen permeability (cm 3 / (m 2 24h atm) d: test piece thickness (mm)

[0166] (Electrolyte permeability) Using the pellets and a heat press molding machine, a sheet-like test piece with a thickness of about 0.2 mm was prepared. The test cup (permeation area 12.56 cm2) was 2 10 g of dimethyl carbonate (DMC) was placed in a test piece, which was then covered with a sheet specimen and a PTFE gasket was placed between the test pieces and tightened to seal. The test piece was placed in contact with the DMC and held at 60°C for 30 days, then removed and left at room temperature for 1 hour before measuring the amount of mass loss. The DMC permeability (g cm / m 2 ) was sought. Electrolyte permeability (g cm / m 2 ) = mass loss (g) × thickness of sheet specimen (cm) / permeation area (m 2 )

[0167] (Ethyl acetate permeability) Using the pellets and a heat press molding machine, a sheet-like test piece with a thickness of about 0.1 mm was prepared. The test cup (permeation area 12.56 cm2) was 2The sheet test piece was placed in a container containing 10 g of ethyl acetate, covered with a sheet test piece, and then a PTFE gasket was placed between the test piece and the container, which was then tightened and sealed. The sheet test piece was placed in contact with the ethyl acetate and kept at 60°C for 45 days, after which it was removed and left at room temperature for 1 hour, after which the amount of mass loss was measured. The ethyl acetate permeability (g cm / m 2 ) was sought. Ethyl acetate (g cm / m 2 ) = mass loss (g) × thickness of sheet specimen (cm) / permeation area (m 2 )

[0168] (110℃ load deflection rate) Using pellets and a heat press molding machine, a sheet-like test piece with a thickness of about 4.2 mm was prepared, from which a test piece of 80 x 10 mm was cut out and heated in an electric furnace at 100 ° C for 20 hours. Except for using the obtained test piece, a test was performed in accordance with the method described in JIS KK 7191-1 using a heat distortion tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd.) under the conditions of a test temperature of 30 to 150 ° C, a heating rate of 120 ° C / hour, a bending stress of 1.8 MPa, and a flatwise method. The deflection rate under load was calculated using the following formula. A sheet with a small deflection rate under load at 110 ° C has excellent rigidity at a high temperature of 110 ° C. Load deflection rate (%) = a2 / a1 x 100 a1: thickness of test piece before test (mm) a2: Deflection at 110℃ (mm)

[0169] (Tensile creep test) Tensile creep strain was measured using a Hitachi High-Tech Science TMA-7100. A sheet with a thickness of approximately 0.1 mm was produced using pellets and a heat press molding machine, and a sample with a width of 2 mm and a length of 22 mm was produced from the sheet. The sample was attached to a measuring jig with a jig distance of 10 mm. The cross-sectional load on the sample was 2.41 N / mm 2A load was applied so that the sample would not stretch even when a tensile load was applied, and the sample was left at 240°C. The sample's length displacement (mm) was measured from 90 minutes after the start of the test until 300 minutes after the start of the test, and the ratio of the length displacement (mm) to the initial sample length (10 mm) (tensile creep strain (%)) was calculated. Sheets with a small tensile creep strain (%) measured under conditions of 240°C and 300 minutes are less likely to stretch even when a tensile load is applied in an extremely high-temperature environment, and have excellent high-temperature tensile creep properties.

[0170] (60,000 times tensile strength retention rate) The tensile strength retention rate after 60,000 cycles was measured using a fatigue testing machine MMT-250NV-10 manufactured by Shimadzu Corporation. A sheet with a thickness of approximately 2.4 mm was produced using pellets and a heat press molding machine, and a dumbbell-shaped sample (thickness 2.4 mm, width 5.0 mm, measurement section length 22 mm) was produced using an ASTM D1708 micro dumbbell. The sample was attached to a measuring jig, and the measuring jig was placed in a thermostatic chamber at 150°C with the sample attached. The tensile strength after each stretch (tensile strength when the stroke was +0.2 mm) was measured by repeating uniaxial tension with a stroke of 0.2 mm and a frequency of 100 Hz. The tensile strength retention rate after 60,000 cycles was calculated from the measured values ​​according to the following formula. Tensile strength retention rate at 60,000 cycles (%) = Tensile strength (60,000 cycles) (mN) / Tensile strength (5,000 cycles) (mN) x 100

[0171] The 60,000-cycle tensile strength retention rate is the ratio of the tensile strength when a repeated load is applied 60,000 times to the tensile strength when a repeated load is applied 5,000 times. A sheet with a high 60,000-cycle tensile strength retention rate maintains its initial tensile strength even after being subjected to a repeated load 60,000 times, and has excellent resistance to deterioration due to repeated loads.

[0172] (Ozone exposure test) The copolymer was compression molded at 350°C under a pressure of 0.5 MPa to prepare a sheet with a thickness of 1 mm, which was then cut into a size of 10 x 20 mm to prepare a sample for ozone exposure testing. Ozone gas (ozone / oxygen = 10 / 90% by volume) generated by an ozone generator (product name: SGX-A11MN (modified), manufactured by Sumitomo Seiki Kogyo Co., Ltd.) was connected to a PFA container containing ion-exchanged water, and water vapor was added to the ozone gas by bubbling it into the ion-exchanged water, and the sample was exposed to the wet ozone gas by passing it through a PFA cell containing the sample at room temperature at a rate of 0.7 liters / min. 150 days after the start of exposure, the sample was removed, the surface was lightly rinsed with ion-exchanged water, and the area 5 to 200 μm deep from the sample surface was observed at a magnification of 100 times using a transmission optical microscope, photographed with a standard scale, and measured from 1 mm deep from the sample surface. 2 The number of cracks having a length of 10 μm or more per unit area was counted and evaluated according to the following criteria. ○: 10 or less cracks ×: More than 10 cracks

[0173] (Tube formability) The pellets obtained in the examples were extruded in a φ30 mm extrusion molding machine (manufactured by Tanabe Plastics Machinery Co., Ltd.) to form a tube having an outer diameter of 10.0 mm and a wall thickness of 1.0 mm. The extrusion molding conditions are as follows. a) Die inner diameter: 20mm b) Mandrel outer diameter: 13mm c) Sizing die inner diameter: 10.5mm d) Take-off speed: 0.4m / min e)Outer diameter: 10.0mm f) Wall thickness: 1.0mm g) Extrusion conditions: · Single-screw extruder with cylinder diameter = 30 mm, L / D = 22 Extruder temperature settings: Barrel section C-1 (330°C), Barrel section C-2 (365°C), Barrel section C-3 (380°C), Head section H-1 (380°C), Die section D-1 (390°C), Die section D-2 (390°C) The obtained tube was observed and evaluated according to the following criteria: The appearance of the tube was confirmed by visual inspection. ○: Appearance is good ×: The cross section is not circular, but is flat or has uneven thickness, and the appearance is poor.

[0174] (Dielectric tangent) The pellets were melt-molded to produce cylindrical test pieces with a diameter of 2 mm. The test pieces were set in a 6 GHz cavity resonator manufactured by Kanto Electronics Application Development Co., Ltd., and measured with a network analyzer manufactured by Agilent Technologies, Inc. The measurement results were analyzed with the analysis software "CPMA" manufactured by Kanto Electronics Application Development Co., Ltd. on a PC connected to the network analyzer, and the dielectric loss tangent (tan δ) at 20°C and 6 GHz was obtained.

[0175] [Table 4]

Claims

1. Contains tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, The content of perfluoro(propyl vinyl ether) units is 4.1 to 4.9 mass% based on the total monomer units; The content of tetrafluoroethylene units is 95.1 to 95.9% by mass based on the total monomer units, the content of monomer units derived from monomers copolymerizable with tetrafluoroethylene and perfluoro(propyl vinyl ether) is 0 to 0.7% by mass based on the total monomer units; The melt flow rate at 372°C is 4.0 to 9.0 g / 10 min. The number of functional groups of -CF=CF 2 , -CF 2 H, -COF, -COOH, -COOCH 3 , -CONH 2 and -CH 2 OH is 10 or less. 6 Each piece is 40 or less. A copolymer (containing tetrafluoroethylene units, perfluoro(propyl vinyl ether) units, and monomer units derived from monomers copolymerizable with tetrafluoroethylene and perfluoro(propyl vinyl ether), the content of perfluoro(propyl vinyl ether) units is 4.4 to 6.0 mass% based on the total monomer units, the content of tetrafluoroethylene units is 94.0 to 95.6 mass% based on the total monomer units, the content of monomer units derived from monomers copolymerizable with tetrafluoroethylene and perfluoro(propyl vinyl ether) is 0 to 1.0 mass% based on the total monomer units, the melt flow rate at 372°C is 7.5 to 11.0 g / 10 min, the number of functional groups, -CF=CF 2 , -CF 2 H, -COF, -COOH, -COOCH 3 , -CONH 2 and -CH 2 OH, is greater than or equal to 10 carbon atoms in the main chain, and (Excluding copolymers having 40 or less units per unit).

2. 2. The copolymer according to claim 1, which has a melt flow rate at 372° C. of 5.0 to 9.0 g / 10 min.

3. An injection molded article comprising the copolymer according to claim 1 or 2.

4. A coated electric wire comprising a coating layer containing the copolymer according to claim 1 or 2.

5. 3. A molded article comprising the copolymer according to claim 1 or 2, the molded article being a joint, a film, a bottle, a gasket, a wire coating or a tube.

Citation Information

Patent Citations

  • Low dielectric tangential fluorocarbon resin and cable produced therefrom

    JP1991184209A

  • Granulated tetrafluoroethylene copolymer and its production

    JP1998087746A

  • Rotomolding method using melt extruded tfe / pave copolymer

    JP2003534940A

  • Molding material for ozone-resistant articles and ozone-resistant injection-molded articles

    WO2003048214A1

  • Fluororesin composition, process for producing the same, semiconductor producing apparatus and coated wire

    WO2004052987A1