Glass Composite

The glass composite addresses electromagnetic wave blocking and night reflections by incorporating a light reflective layer with specific metal thickness ratios and a protective resin layer, enhancing communication and lighting performance while maintaining radiative cooling.

JP7580645B1Active Publication Date: 2024-11-11OSAKA GAS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024048429
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-25
Publication Date
2024-11-11
Estimated Expiration
2044-03-25

AI Technical Summary

Technical Problem

The glass composite with a metal shielding layer, as described in Patent Document 1, faces issues with electromagnetic wave blocking, poor lighting performance, and reflections at night, particularly in vehicle windows, which affect communication and visibility.

Method used

A glass composite design with a light reflective layer having thick and thin metal portions, a protective layer, and an infrared emitting layer, optimized for electromagnetic wave permeability, lighting performance, and reduced night reflections, using materials like silver, silver alloy, and a protective resin layer.

Benefits of technology

The design enhances electromagnetic wave transmission, improves lighting performance, and reduces night reflections, ensuring effective communication and visibility while maintaining radiative cooling functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580645000001_ABST
    Figure 0007580645000001_ABST
Patent Text Reader

Abstract

It is possible to improve electromagnetic wave transparency and daylighting properties, and also to reduce glare at night, etc. [Solution] A glass composite W includes an infrared-emitting glass layer G1 that emits infrared light from a first radiation surface H1, which is a radiation surface H, and a light-reflecting layer B located on the infrared-emitting glass layer G1 on the side opposite to the side on which the first radiation surface H1 exists, laminated in the order described above. The light-reflecting layer B has a thick portion B3 in the stacking direction Z and a thin portion B2 whose thickness in the stacking direction is 2 / 3 or less of the thickness of the thick portion B3, and the thin portion B2 is provided continuously and integrally in a plan view perpendicular to the first radiation surface H1 and has an area of ​​5 cm in plan view. 2 and a second thin metal portion B2 that is provided integrally and continuously in a plan view and has an area in a plan view less than the area of ​​the first thin metal portion.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a glass composite having an infrared radiative glass layer and exhibiting a radiative cooling function. [Background technology]

[0002] Radiative cooling is known as a function for cooling objects. Radiative cooling is a phenomenon in which a substance's temperature drops when it radiates electromagnetic waves such as infrared rays to its surroundings. By utilizing this phenomenon, for example, it is possible to realize a composite cooling device that cools objects without consuming energy such as electricity.

[0003] Patent Document 1 discloses a glass composite in which a high-emissivity coating layer that emits infrared light from its radiation surface and a low-emissivity coating layer that reflects light are laminated on a glass substrate. Here, it is disclosed that the low-emissivity coating layer includes a shielding layer that blocks infrared and ultraviolet rays, and that the shielding layer is made of a metal material such as silver. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2022-543529 Summary of the Invention [Problem to be solved by the invention]

[0005] When the glass composite shown in Patent Document 1 has a shielding layer made of a metal material such as silver, for example in a structure such as a vehicle having a window that separates an external area from an internal area with the glass composite, there are problems such as the blocking of electromagnetic waves used for communication between the external area and the internal area, poor lighting from the external area to the internal area, and increased reflections when viewing the external area from the internal area through the glass composite at night. However, the technology disclosed in Patent Document 1 does not recognize such a problem, and there is room for improvement.

[0006] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a glass composite that can improve electromagnetic wave transmittance and daylighting properties and can reduce glare at night, etc. [Means for solving the problem]

[0007] The characteristic configuration of the glass composite for achieving the above object is as follows: a glass composite comprising: an infrared emitting glass layer that emits infrared light from a first emitting surface that is an emitting surface; and a light reflecting layer that is located on an opposite side of the infrared emitting glass layer to a side on which the first emitting surface is present, laminated in the order described above; the light reflecting layer has a thick portion in a stacking direction and a thin portion whose thickness in the stacking direction is 2 / 3 or less of the thickness of the thick portion, The thin portion is provided continuously and integrally in a plan view perpendicular to the first radiation surface, and has an area of ​​5 cm 2 a first metal thin portion having an area equal to or greater than the area of ​​the first metal thin portion, and a second metal thin portion provided integrally and continuously in the plan view and having an area in the plan view less than the area of ​​the first metal thin portion, The second thin metal portion is provided in a plurality of portions in a dispersed manner in the plan view, The overall surface average solar reflectance is 40% or more, and the surface average emissivity, which is the wavelength average of the emissivity of infrared light of 8 μm or more and 13 μm or less, is 80% or more.

[0008] According to the above characteristic configuration, the light reflecting layer has a thick portion having a large thickness in the stacking direction and a thin portion having a thickness in the stacking direction that is 2 / 3 or less of the thickness of the thick portion, and the thin portion is provided continuously and integrally in a plan view perpendicular to the first radiation surface and has an area of ​​5 cm in a plan view. 2Since the glass composite has a first thin metal portion having an area of ​​the above size, by setting the thickness of the first thin metal portion to an appropriate thickness that allows electromagnetic waves for communication to pass through, for example, it becomes possible to communicate by electromagnetic waves through the glass composite. Furthermore, as the thin portions of the light-reflecting layer, a plurality of second thin metal portions which are provided as a continuous, integral part in a planar view and whose area in a planar view is less than the area of ​​the first thin metal portion are provided in a dispersed and distributed form in a planar view, so that a predetermined amount of light can be obtained through the glass composite in a dispersed manner in the planar direction along the radiating surface. Furthermore, the second thin metal portions, which are provided in a dispersed manner in a plan view, have a smaller area in a plan view than the first thin metal portions, so that a certain degree of reflectance can be ensured as a light reflective layer. With the above configuration, a glass composite can be realized which has an overall surface average solar reflectance of 40% or more and a surface average average emissivity, which is the wavelength average of the emissivity of infrared light of 8 μm or more and 13 μm or less, of 80% or more, thereby improving electromagnetic wave transmittance and daylighting properties and reducing glare at night, etc.

[0009] Further characteristic features of the glass composite include: In the stacking direction, the thickness of each of the first thin metal portion and the second thin metal portion is 0 nm or more and 50 nm or less, and more preferably 0 nm or more and 10 nm or less.

[0010] The inventors set the thickness of the first metal thin portion in the product direction to 50 nm or less, and, as described above, set the area in plan view to 5 cm 2 It has been confirmed that by doing the above, electromagnetic waves for communication can be transmitted satisfactorily for communication. In addition, it has been confirmed that by having a certain area ratio of thick portions while keeping the thickness in the product direction of the second metal thin portion to 50 nm or less, it is possible to obtain appropriate light transmission while ensuring an average surface solar reflectance of 40% or more for the entire glass laminate.

[0011] Further characteristic features of the glass composite include: In the plan view, the area of ​​the second metal thin portion is 0.03 cm 2 That is all there is to it.

[0012] The inventors determined that the area of ​​the second metal thin section was 0.03 cm 2 It has been confirmed that if the thickness is less than this, it is difficult to obtain sufficient lighting for the entire glass laminate, even if the number of second thin metal portions is increased to the extent that the light reflective layer can be maintained as a thin metal film.

[0013] Further characteristic features of the glass composite include: a protective layer for protecting the light reflecting layer on the side of the light reflecting layer opposite to the side where the infrared radiation glass layer is present; The protective layer is an auxiliary infrared emitting layer that emits infrared light from a second emitting surface, which is the emitting surface on the opposite side to the side on which the light reflecting layer is present.

[0014] According to the above-described characteristic configuration, a protective layer for protecting the light reflecting layer is provided on the side of the light reflecting layer opposite to the side on which the infrared radiation glass layer is present. Therefore, even if the light reflecting layer is made of a metal vapor deposition film or the like that is vulnerable to external forces, the protective layer prevents the light reflecting layer from being exposed to external forces, and therefore the light reflecting layer can be effectively prevented from being peeled off due to external forces. Furthermore, by appropriately selecting the resin material for forming the above-mentioned protective layer, the protective layer can be made to function as an auxiliary infrared radiation layer capable of emitting infrared light, thereby realizing a glass composite that can also emit infrared light from a second radiation surface opposite to the first radiation surface.

[0015] Further characteristic features of the glass composite include: a back glass layer is provided on the side of the auxiliary infrared radiation layer opposite to the side on which the light reflecting layer is present; the rear surface glass layer is an infrared emission rear surface glass layer that emits infrared light from a third emission surface, which is an emission surface on the opposite side to the side on which the auxiliary infrared emission layer is present, The intermediate resin that bonds the auxiliary infrared radiation layer and the infrared radiation rear glass layer is made of at least one of polyvinyl butyral, polyethylene vinyl acetate, and polyurethane.

[0016] In the glass composite described thus far, a back surface glass layer may be provided on the side opposite to the side on which the auxiliary infrared emission layer is present, and the back surface glass layer may be an infrared emission back surface glass layer that emits infrared light from a third emission surface, which is the emission surface on the side opposite to the side on which the auxiliary infrared emission layer is present, thereby making it possible to obtain a glass composite having laminated glass. Here, by using one or more of polyvinyl butyral, polyethylene vinyl acetate, and polyurethane as the intermediate resin that bonds between the auxiliary infrared radiation layer and the infrared radiation back surface glass layer, it is possible to achieve good adhesion between the auxiliary infrared radiation layer and the infrared radiation back surface glass layer while appropriately maintaining the radiative cooling function.

[0017] A further characteristic feature of the glass composite is that the infrared emitting glass layer is The glass is made of at least one of non-alkali glass, soda lime glass, alkali borosilicate glass, and acrylic resin glass.

[0018] Further characteristic features of the glass composite include: The infrared radiation glass layer and the infrared radiation back surface glass layer are The glass is made of at least one of non-alkali glass, soda lime glass, alkali borosilicate glass, and acrylic resin glass.

[0019] By selecting the material in this way, the infrared-emitting glass layer or the infrared-emitting back surface glass layer can function well as an infrared-emitting layer that radiates infrared rays. In addition, when connecting with the above-mentioned intermediate resin, the hydroxyl groups of the infrared-emitting glass layer or the infrared-emitting back surface glass layer and the hydroxyl groups of the intermediate resin can be bonded to each other to achieve good adhesion.

[0020] Further characteristic features of the glass composite include: In the plan view, The ratio of the area of ​​the thin portion to the entire area of ​​the light reflecting layer is 1% or more and 50% or less.

[0021] According to the above-mentioned characteristic configuration, a glass composite having an overall surface average solar reflectance of 40% or more can be satisfactorily realized.

[0022] Further characteristic features of the glass composite include: the light reflecting layer is a metal vapor-deposited layer formed by vapor-depositing a metal on a side of the infrared radiation glass layer opposite to a side on which the first radiation surface is present, The metal is at least one of silver, a silver alloy, aluminum, an aluminum alloy, and a copper alloy.

[0023] As described above, by making the light reflecting layer at least one of silver, a silver alloy, aluminum, an aluminum alloy, and a copper alloy vapor-deposited on the side opposite to the side where the first radiation surface of the infrared radiation glass layer is present, there is no need to bond the light reflecting layer and the infrared radiation glass layer with a resin material or the like, so that the glass laminate can be realized by a relatively simple manufacturing process.

[0024] Further characteristic features of the glass composite include: The feature is that a light control layer having a light control function is provided on the side of the auxiliary infrared radiation layer opposite to the side where the light reflection layer is present.

[0025] Further characteristic features of the glass composite include: The infrared radiation rear glass layer has a light control layer having a light control function on the side opposite to the side on which the auxiliary infrared radiation layer is present.

[0026] As explained above, the glass composite of the present invention has an overall surface average solar reflectance of 40% or more by providing thin sections in the light-reflecting layer, so it is anticipated that in some cases, too much light may pass through the gas composite. As described above, by having a dimming layer with a dimming function, it is possible to adjust the light transmission by increasing the amount of light attenuation by the dimming layer, for example, when the amount of light passing through the glass composite is too large. [Brief description of the drawings]

[0027] [Figure 1]FIG. 1 is a schematic cross-sectional view of a glass composite, and a vehicle as a structure including the glass composite. [Diagram 2] FIG. 13 is a diagram for explaining the process of sequentially sputtering a material for a light reflecting layer and a material for an infrared emitting layer onto an infrared emitting glass. [Diagram 3] FIG. 2 is a plan view of an example of a glass composite (or a light reflecting layer). [Figure 4] FIG. 13 is a schematic cross-sectional view of another embodiment of a glass composite. [Diagram 5] FIG. 13 is a schematic cross-sectional view of another embodiment of a glass composite. [Figure 6] FIG. 13 is a schematic cross-sectional view of another embodiment of a glass composite. [Figure 7] FIG. 13 is a schematic cross-sectional view of another embodiment of a glass composite. [Figure 8] FIG. 2 is a schematic cross-sectional view of a glass composite according to a comparative example. [Figure 9] FIG. 4 is a diagram showing the relationship between the absorption coefficient of a resin material and a wavelength band. [Figure 10] FIG. 4 is a diagram showing the relationship between the light absorptance of a resin material and the wavelength. [Figure 11] FIG. 1 is a diagram showing the emissivity spectrum of silicone rubber. [Figure 12] FIG. 1 shows the emissivity spectrum of PFA. [Figure 13] FIG. 1 is a diagram showing the emissivity spectrum of polyvinyl chloride resin. [Figure 14] FIG. 2 is a diagram showing the emissivity spectrum of ethylene terephthalate resin. [Figure 15] FIG. 1 is a diagram showing the emissivity spectrum of an olefin modified material. [Figure 16] FIG. 4 is a diagram showing the relationship between the temperature of the radiation surface and the temperature of the light reflecting layer. [Figure 17] FIG. 2 is a diagram showing the light absorptance spectra of silicone rubber and perfluoroalkoxy fluororesin. [Figure 18] FIG. 2 is a diagram showing the light absorptance spectrum of ethylene terephthalate resin. [Figure 19] FIG. 2 shows the light reflectance spectrum of a silver-based light reflective layer. [Figure 20] FIG. 2 shows the emissivity spectrum of fluoroethylene vinyl ether. [Figure 21] FIG. 2 is a diagram showing the emissivity spectrum of vinylidene chloride resin. [Figure 22] 13 is a table showing experimental results. [Figure 23] FIG. 4 is a diagram showing the relationship between the light absorptance of a resin material and the wavelength. [Figure 24] FIG. 1 is a graph showing the relationship between light transmittance and wavelength of polyethylene. [Diagram 25] FIG. 1 is a diagram illustrating a test configuration. [Figure 26] FIG. 13 is a diagram showing test results when the protective layer is made of polyethylene. [Figure 27] FIG. 13 is a diagram showing test results when the protective layer is made of ultraviolet absorbing acrylic. [Figure 28] FIG. 2 is a diagram showing the emissivity spectrum of polyethylene. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] The glass composite W according to the embodiment of the present invention can improve electromagnetic wave transparency and daylighting properties, and can also reduce glare at night or other times. Hereinafter, an embodiment of the glass composite W will be described with reference to the drawings.

[0029] As shown in Fig. 1, the glass composite W is preferably provided, for example, as window glass to be fitted into a frame C1 of a vehicle C as a structure that divides an internal area IS from an external environment OS. The window is a front window, rear window, side window, sunroof, etc. of the vehicle C. Other examples of the structure include commercial buildings and residential buildings, and the glass composite W can be suitably used as window glass for these. In this embodiment, the side of the atmosphere from which infrared rays are radiated is the side indicated by the arrow in the stacking direction Z.

[0030] As shown in FIG. 1 , the glass composite W comprises an infrared emitting glass layer G1 that emits infrared light from a first emitting surface H1, which is an emitting surface H, and a light reflecting layer B located on the opposite side of the infrared emitting glass layer G1 to the side where the first emitting surface H1 is present, laminated in the order described below. The light reflecting layer B has a thick portion B3 in the stacking direction Z and a thin portion B2 whose thickness L1 in the stacking direction Z is 2 / 3 or less of the thickness L2 of the thick portion B3. In the thin portion B2, the proportion of transmitted light Lt in the incident light L from the first radiation surface H1 side is relatively high and the proportion of reflected light Lr is relatively low compared to the thick portion B3.

[0031] Regarding the thin portion of the light reflecting layer B, as shown in the plan view of the light reflecting layer B (or the glass composite W) in FIG. 3, the thin portion is provided continuously and integrally in a plan view perpendicular to the first radiation surface H1 and has an area of ​​5 cm2 in plan view. 2 and a second thin metal portion B2 which is provided integrally and continuously in a plan view and has an area in a plan view less than the area of ​​the first thin metal portion B1. Here, the second thin metal portion B2 is provided in a plurality of locations so as to be dispersed in a plan view, and the area of ​​one second thin metal portion B2 is 0.03 cm 2 That's all.

[0032] The light reflecting layer B is preferably a metal vapor-deposited layer in which a metal is vapor-deposited on the side opposite to the side where the first radiation surface H1 of the infrared radiation glass layer G1 exists. The vapor-deposited metal is preferably at least one of silver, a silver alloy, aluminum, an aluminum alloy, and a copper alloy.

[0033] Furthermore, in the light reflecting layer B, the thickness of each of the first thin metal portion B1 and the second thin metal portion B2 in the stacking direction Z is preferably 0 nm or more and 50 nm or less, more preferably 0 nm or more and 10 nm or less. Incidentally, the thickness of the thick portion B3 is preferably 50 nm or more and 500 nm or less, more preferably 70 nm or more and 200 nm or less. With the above configuration, the first thin metal portion B1 can transmit electromagnetic waves for communication (for example, electromagnetic waves with frequencies of about 300 MHz or more and 300 GHz or less) well, and the second thin metal portion B2 can transmit visible light for daylighting well. In addition, it is possible to reduce glare at night, etc.

[0034] In plan view, the ratio of the area of ​​the thin portion to the entire area of ​​the light reflecting layer B is preferably 1% or more and 50% or less. From the viewpoint of light collection, the ratio of the area of ​​the second metal thin portion B2 to the entire area of ​​the light reflecting layer B is preferably 1% or more. In the plan view of FIG. 3, the first thin metal portion B1 is rectangular and the second thin metal portion B2 is circular, but they are not limited to this and may be various shapes such as elliptical or polygonal.

[0035] 1 , the glass composite W according to this embodiment further includes a protective layer for protecting the light reflecting layer B on the side of the light reflecting layer B opposite to the side on which the infrared emitting glass layer G1 is present, and the protective layer is an auxiliary infrared emitting layer J (hereinafter sometimes referred to as infrared emitting layer J) that emits infrared light from a second emitting surface H2, which is the emitting surface H on the side opposite to the side on which the light reflecting layer B is present. Details of the light reflecting layer B and the auxiliary infrared emitting layer J will be described later.

[0036] As shown in FIG. 2, the light reflecting layer B and the infrared emitting layer J are formed on the surface of the infrared emitting glass layer G1 opposite to the first emitting surface H1 by sputtering (deposition by physical vapor deposition (PVD)) a metal material as the light reflecting layer B and sputtering a resin material as the infrared emitting layer J via a punching metal PM. As the punched metal PM, as shown in Fig. 2, a first flat plate portion PM1 shaped to overlap the first metal thin portion B1 (shown in Fig. 3) in a plan view and a second flat plate portion PM2 shaped to overlap the second metal thin portion B2 (shown in Fig. 3) are preferably connected integrally to a metal frame body PM4. Note that, although a plurality of second flat plate portions PM2 are present dispersedly in a plan view, the plurality of second flat plate portions PM2 are connected to the metal frame body PM4 by, for example, connection lines PM3 that are sufficiently thin in a plan view.

[0037] The method for forming the light reflecting layer B is not particularly limited, and may be a chemical vapor deposition (CVD) method, a plasma enhanced chemical vapor deposition (PECVD) method, magnetron sputtering, an ion beam assisted deposition method, or the like. The deposition method of the infrared emitting layer J may be the same as or different from that of the light reflecting layer B, and may be spray coating, dip coating, or a plasma enhanced chemical vapor deposition (PECVD) method.

[0038] As shown in FIG. 4, the glass composite W may be a structure obtained by inverting the glass composite W shown in FIG. 1 in the lamination direction Z, that is, a structure obtained by laminating an auxiliary infrared-emitting layer J as a protective layer, a light-reflecting layer B, and an infrared-emitting glass layer G1 in this order from the air side.

[0039] 5, the glass composite W may have a laminated glass structure in which the light reflecting layer B and the auxiliary infrared emitting layer J are sandwiched between an infrared emitting glass layer G1 and a back surface glass layer G2. In other words, the glass composite W shown in FIG. 1 may have a configuration in which the back surface glass layer G2 is provided on the side opposite to the side where the light reflecting layer B of the auxiliary infrared emitting layer J is present (the side where the second emitting surface H2 is present). The back surface glass layer G2 may be an infrared emitting back surface glass layer that emits infrared light from the third emitting surface H3, which is the emitting surface H on the side opposite to the side where the auxiliary infrared emitting layer J is present. Here, the auxiliary infrared radiation layer J and the rear glass layer G2 (infrared radiation rear glass layer) are bonded together by an intermediate resin Tu. The intermediate resin Tu is made of one or more of polyvinyl butyral, polyethylene vinyl acetate, and polyurethane. With this configuration, the infrared radiation glass layer G1 and the rear surface glass layer G2 (infrared radiation rear surface glass layer) can maintain the glass fragments when they are broken due to an impact.

[0040] The infrared radiation glass layer G1 and the back surface glass layer G2 (infrared radiation back surface glass layer) are preferably glass for vehicles, and more preferably made of at least one of alkali-free glass, soda-lime glass, alkali borosilicate glass, and acrylic resin glass. The infrared radiation glass layer G1 and the back surface glass layer G2 (infrared radiation back surface glass layer) may be made of the same material or different materials. The infrared radiation glass layer G1 and the back surface glass layer G2 (infrared radiation back surface glass layer) may be configured as tempered glass, and a single layer glass treated by heat treatment or chemical treatment can be suitably used, and the strength can be increased compared to that of ordinary glass (i.e., untempered glass such as soda-lime silica glass or annealed glass). Furthermore, the infrared-emitting glass layer G1 and the back glass layer G2 (infrared-emitting back glass layer) may be reinforced with fillers and / or fibers. The infrared radiation glass layer G1 and the rear surface glass layer G2 (infrared radiation rear surface glass layer), and the intermediate resin Tu are preferably transparent to visible light.

[0041] As an example of a method for producing a glass composite W as shown in FIG. 5, a laminate in which an infrared emitting glass layer G1, a light reflecting layer B, and an auxiliary infrared emitting layer J are laminated as shown in FIG. 1, and a back surface glass layer G2 are laminated with an intermediate resin Tu interposed between them. Next, the glass composite W is temporarily bonded by a method such as a nipper roll method in which the laminated glass composite W is heated to about 70 to 100°C, then sandwiched between rollers and temporarily bonded while removing the air, a rubber channel method in which the ends (four sides) of the glass composite W in a planar view are tied with rubber tubes, the air is removed, and temporarily bonded, or a rubber bag method in which the glass composite W is placed in a rubber bag and the inside of the rubber bag is vacuumed to temporarily bond the glass composite W. Finally, the components are permanently bonded by autoclaving at about 100 to 130° C. for about 1 to 2 hours under pressure to remove all air and bond the components together. Furthermore, when the intermediate resin Tu is heated during the bonding process, it flows into the portion of the light-reflecting layer B where the thin portion B2 exists, and when the thickness of the thin portion B2 is 0 μm, it directly connects the infrared radiation glass layer G1 and the back surface glass layer G2.

[0042] As another example, as shown in FIG. 6, the glass composite W may be a structure obtained by inverting the glass composite W shown in FIG. 5 in the stacking direction Z, that is, a back surface glass layer G2, an intermediate resin Tu, an auxiliary infrared emitting layer J as a protective layer, a light reflecting layer B, and an infrared emitting glass layer G1, which are stacked in this order from the air side.

[0043] As another example, the glass composite W may have a structure in which the auxiliary infrared emitting layer J in the glass composite W shown in FIG. 5 is omitted, as shown in FIG.

[0044] From the viewpoint of exerting the above-mentioned infrared radiation performance, in the glass composite W shown in FIG. 1 , the thickness of the infrared-emitting glass layer G1 is preferably 200 μm or more and 10,000 μm or less, in the glass composite W shown in FIG. 5 , the thickness of the infrared-emitting glass layer G1 is preferably 200 μm or more and 10,000 μm or less, in the glass composite W shown in FIG. 1 , the thickness of the infrared-emitting glass layer G1 is preferably 200 μm or more and 10,000 μm or less, in the glass composite W shown in FIG. 6 , the thickness of the back surface glass layer G2 (infrared-emitting back surface glass layer) is preferably 200 μm or more and 10,000 μm or less, and in the glass composite W shown in FIG. 7 , the thickness of the infrared-emitting glass layer G1 is preferably 200 μm or more and 10,000 μm or less.

[0045] Incidentally, the auxiliary infrared emission layer J of the glass composite W according to Figs. 1 to 6 described above is illustrated as not being present in the portions corresponding to the thin portions B1 and B2 of the light reflecting layer B in plan view. However, from the viewpoints of improving electromagnetic wave transparency and daylighting properties and reducing glare at night, etc., such a configuration is not necessarily required. Specifically, the auxiliary infrared emission layer J may have a thickness in the portions corresponding to the thin portions B1 and B2 of the light reflecting layer B in plan view.

[0046] The glass composite W described thus far has an overall surface average solar reflectance of 40% or more, and a surface average average emissivity, which is the wavelength average of the emissivity of infrared light of 8 μm or more and 13 μm or less, of 80% or more. It is more preferable that the overall surface average solar reflectance is 60% or more, and the surface average average emissivity, which is the wavelength average of the emissivity of infrared light of 8 μm or more and 13 μm or less, is 85% or more.

[0047] [Details of the resin material constituting the infrared radiation layer] In the following description, the description regarding the film thickness of the infrared emitting layer J is based on a configuration in which the infrared emitting layer J has a substantially uniform thickness in a planar view and is directed toward the atmosphere. The resin material can be a colorless resin material that contains a carbon-fluorine bond (CF), a siloxane bond (Si-O-Si), a carbon-chlorine bond (C-Cl), a carbon-oxygen bond (CO), an ester bond (R-COO-R), an ether bond (COC bond), or a benzene ring. For each resin material (excluding carbon-oxygen bonds), the wavelength ranges with absorption coefficients in the atmospheric window wavelength band are shown in FIG.

[0048] According to Kirchhoff's law, emissivity (ε) and light absorptance (A) are equal. Light absorptance can be calculated from the absorption coefficient (α) using the relation A=1-exp(-αt) (hereafter referred to as the light absorptance relation). Here, t is the film thickness. In other words, by adjusting the film thickness of the infrared radiative layer J, a large thermal radiation can be obtained in a wavelength band with a large absorption coefficient. When performing radiative cooling outdoors, it is recommended to use a material with a large absorption coefficient in the wavelength band of the atmospheric window, that is, from 8 μm to 14 μm. In addition, to suppress the absorption of sunlight, it is advisable to use a material that has no or has a small absorption coefficient in the wavelength range of 0.3 μm to 4 μm, especially in the range of 0.4 μm to 2.5 μm. As can be seen from the relational equation between the absorption coefficient and the absorptance, the light absorptance (emissivity) changes depending on the film thickness of the resin material.

[0049] In order to lower the temperature below the surrounding atmosphere by radiative cooling in a solar radiation environment, if a material is selected that has a large absorption coefficient in the wavelength band of the atmospheric window and almost no absorption coefficient in the wavelength band of sunlight, then by adjusting the film thickness, it will absorb almost no sunlight but emit a lot of thermal radiation from the atmospheric window, meaning it is possible to create a state in which the output from radiative cooling is greater than the input of sunlight.

[0050] Regarding carbon-fluorine bonds (CF), the absorption coefficients due to CHF and CF2 are widely distributed over a wide band from 8 μm to 14 μm, which is the atmospheric window, with the absorption coefficient being particularly large at 8.6 μm. In addition, regarding the solar wavelength band, there is no noticeable absorption coefficient in the wavelength range from 0.3 μm to 2.5 μm, where the energy intensity is high.

[0051] Resin materials having carbon-fluorine bonds (CF) include: Polytetrafluoroethylene (PTFE), a fully fluorinated resin; Partially fluorinated resins polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF) and polyvinyl fluoride (PVF), Perfluoroalkoxy fluororesin (PFA), a fluorinated resin copolymer; Tetrafluoroethylene-hexafluoropropylene copolymer (FEP), Ethylene-tetrafluoroethylene copolymer (ETFE), Examples include ethylene-chlorotrifluoroethylene copolymer (ECTFE).

[0052] Resin materials having a siloxane bond (Si-O-Si) include silicone rubber and silicone resin. In this resin, a large absorption coefficient caused by the expansion and contraction of C-Si bonds appears broadly around a wavelength of 13.3 μm, an absorption coefficient caused by the out-of-plane bending angle (vertical rocking) of CSiH2 appears broadly around a wavelength of 10 μm, and a small absorption coefficient caused by the in-plane bending angle (scissors) of CSiH2 appears around a wavelength of 8 μm.

[0053] For carbon-chlorine bonds (C-Cl), the absorption coefficient due to the C-Cl stretching vibration appears in a broad band with a half-width of 1 μm or more centered at a wavelength of 12 μm. Resin materials include polyvinyl chloride resin (PVC) and polyvinylidene chloride resin (PVDC). In the case of polyvinyl chloride resin, due to the electron-withdrawing effect of chlorine, an absorption coefficient originating from the bending vibration of CH of the alkene contained in the main chain appears at a wavelength of around 10 μm.

[0054] Ester bonds (R-COO-R) and ether bonds (COC bonds) have absorption coefficients in the wavelength range of 7.8 μm to 9.9 μm. In addition, the carbon-oxygen bonds contained in ester bonds and ether bonds have strong absorption coefficients in the wavelength range of 8 μm to 10 μm. When a benzene ring is introduced into the side chain of a hydrocarbon resin, absorption appears over a wide wavelength range from 8.1 μm to 18 μm due to the vibration of the benzene ring itself and the vibration of surrounding elements caused by the influence of the benzene ring.

[0055] Resins having these bonds include methyl methacrylate resin, ethylene terephthalate resin, trimethylene terephthalate resin, butylene terephthalate resin, ethylene naphthalate resin, and butylene naphthalate resin.

[0056] [Optical absorption considerations] Let us consider the light absorption in the ultraviolet-visible region of resin materials with the bonds and functional groups described above, that is, sunlight absorption. The origin of the absorption of ultraviolet to visible light is the transition of electrons that contribute to the bonds. Absorption in this wavelength range can be understood by calculating the bond energy. First, let us consider the wavelengths at which resin materials with carbon-fluorine bonds (CF) have absorption coefficients in the ultraviolet to visible range. The bond energies of the CC, CH, and CF bonds in the basic structure of polyvinylidene fluoride (PVDF) are 4.50 eV, 4.46 eV, and 5.05 eV. These correspond to wavelengths of 0.275 μm, 0.278 μm, and 0.246 μm, respectively, and absorb light of these wavelengths.

[0057] Since the solar spectrum only contains wavelengths longer than 0.300μm, when fluororesin is used, it hardly absorbs the ultraviolet, visible, or near-infrared rays of sunlight. Note that ultraviolet rays are defined as wavelengths shorter than 0.400μm, visible light as wavelengths from 0.400μm to 0.800μm, near-infrared rays as wavelengths from 0.800μm to 3μm, mid-infrared rays as wavelengths from 3μm to 8μm, and far-infrared rays as wavelengths longer than 8μm.

[0058] The absorptance spectrum of 50 μm thick PFA (perfluoroalkoxy fluororesin) in the ultraviolet to visible range is shown in Figure 10, which shows that it has almost no absorptance. Note that a slight increase in the absorptance spectrum is observed on the shorter wavelength side than 0.4 μm, but this increase is merely due to the effect of scattering in the sample used for measurement, and there is no actual increase in absorptance.

[0059] In the ultraviolet region of siloxane bonds (Si-O-Si), the bond energy of the Si-O-Si in the main chain is 4.60 eV, which corresponds to a wavelength of 269 nm. Since the solar spectrum only contains wavelengths longer than 0.300 μm, in the majority of cases, siloxane bonds hardly absorb any ultraviolet, visible, or near-infrared light in sunlight.

[0060] The absorptance spectrum of 100μm thick silicone rubber in the ultraviolet to visible range is shown in Figure 10, which shows that it has almost no absorptance. Note that a slight increase in the absorptance spectrum can be seen on the shorter wavelength side than 0.4μm, but this increase is merely due to the effect of scattering in the sample used for measurement, and there is no actual increase in absorptance.

[0061] Regarding the carbon-chlorine bond (C-Cl), the bond energy between the carbon and chlorine in an alkene is 3.28 eV, and the wavelength is 0.378 μm, so it absorbs a lot of ultraviolet light in sunlight, but has almost no absorption in the visible range. FIG. 10 shows the absorption spectrum of a 100 μm thick polyvinyl chloride resin in the ultraviolet to visible range, and indicates that optical absorption is high at wavelengths shorter than 0.38 μm. FIG. 10 shows the absorptance spectrum of a 100 μm thick vinylidene chloride resin in the ultraviolet to visible range, and a slight increase in the absorptance spectrum is observed on the shorter wavelength side than 0.4 μm.

[0062] Resins with ester bonds (R-COO-R), ether bonds (COC bonds), and benzene rings include methyl methacrylate resin, ethylene terephthalate resin, trimethylene terephthalate resin, butylene terephthalate resin, ethylene naphthalate resin, and butylene naphthalate resin. For example, the bond energy of the C-C bond in acrylic is 3.93 eV, and it absorbs sunlight with wavelengths shorter than 0.315 μm, but has almost no absorption in the visible range.

[0063] As an example of a resin material having these bonds and functional groups, the absorption spectrum from ultraviolet to visible light of a 5 mm-thick methyl methacrylate resin is shown in Figure 10. The methyl methacrylate resin shown is a commonly available product on the market, and contains a benzotriazole-based ultraviolet absorber. Because the plate is 5 mm thick, the wavelengths with small absorption coefficients are also large, and light absorption is greater on the shorter wavelength side than 0.38 μm, which is longer than the wavelength of 0.315.

[0064] As an example of a resin material having these bonds and functional groups, the absorption spectrum from ultraviolet to visible light of a 40 μm-thick ethylene terephthalate resin is shown in FIG. As shown in the figure, the absorptance increases as the wavelength approaches 0.315 μm, and the absorptance increases sharply at a wavelength of 0.315 μm. Note that with ethylene terephthalate resin, as the thickness is increased, the absorptance due to the absorption edge derived from the C-C bond increases slightly longer than the wavelength of 0.315 μm, and the absorptance in ultraviolet light increases in the same way as with commercially available methyl methacrylate resin.

[0065] As long as the infrared radiation layer J uses a resin material having the above-mentioned emissivity (light emissivity) and light absorptivity characteristics, it may be a single layer film of one type of resin material, a multilayer film of multiple types of resin materials, a single layer film of a resin material in which multiple types of resin materials are blended, or a multilayer film of a resin material in which multiple types of resin materials are blended. The blends include copolymers such as alternating copolymers, random copolymers, block copolymers and graft copolymers, as well as modified products with substituted side chains.

[0066] [Emissivity of silicone rubber] FIG. 11 shows the emissivity spectrum of the air window of silicone rubber having siloxane bonds. Silicone rubber exhibits a large broad absorption coefficient due to the stretching of C-Si bonds, centered around a wavelength of 13.3 μm. CSiH2 exhibits a broad absorption coefficient due to the out-of-plane bending angle (vertical rocking) of the target object, centered around a wavelength of 10 μm. CSiH2 exhibits a small absorption coefficient due to the in-plane bending angle (scissors) of the target object, centered around a wavelength of 8 μm. Due to this effect, the wavelength average of the emissivity of a 1 μm thick film is 80% at wavelengths from 8 μm to 14 μm, which falls within the regulation of a wavelength average of 40% or more. As shown in the figure, the emissivity in the atmospheric window region increases as the film thickness increases.

[0067] Incidentally, the emission spectrum when quartz, an inorganic material, with a thickness of 1 μm is present on silver is also shown in Figure 11. When quartz is 1 μm thick, it has only a narrow-band emission peak between wavelengths of 8 μm and 14 μm. When this thermal radiation is averaged over the wavelength range from 8 μm to 14 μm, the emissivity in the wavelength range from 8 μm to 14 μm is 32%, making it difficult to demonstrate radiative cooling performance.

[0068] [Emissivity of PFA] Figure 12 shows the emissivity in the atmospheric window of perfluoroalkoxy fluororesin (PFA), a representative example of resins with carbon-fluorine bonds. The absorption coefficients due to CHF and CF2 are widely distributed over a wide band from 8 μm to 14 μm, which is the atmospheric window, and the absorption coefficient is particularly large at 8.6 μm. Due to this effect, the wavelength average of the emissivity of a 10 μm thick film is 45% at wavelengths from 8 μm to 14 μm, which falls within the regulation of a wavelength average of 40% or more. As shown in the figure, the emissivity in the atmospheric window region increases as the film thickness increases.

[0069] [Emissivity of polyvinyl chloride resin and vinylidene chloride resin] Figure 13 shows the emissivity of polyvinyl chloride resin (PVC) at the atmospheric window as a representative example of resins having carbon-chlorine bonds, and Figure 21 shows the emissivity of polyvinylidene chloride resin (PVDC) at the atmospheric window. For carbon-chlorine bonds, the absorption coefficient due to the C-Cl stretching vibration appears in a broad band with a half-width of 1 μm or more centered at a wavelength of 12 μm. In the case of polyvinyl chloride resin, the absorption coefficient due to the bending vibration of CH of the alkene contained in the main chain appears at a wavelength of around 10 μm due to the electron-withdrawing effect of chlorine. The same is true for vinylidene chloride resin. Due to these effects, the wavelength average of the emissivity of a 10 μm thick film is 43% at wavelengths from 8 μm to 14 μm, which falls within the regulation of a wavelength average of 40% or more. As shown in the figure, the emissivity in the atmospheric window region increases as the film thickness increases.

[0070] [Ethylene terephthalate resin] FIG. 14 shows the emissivity of ethylene terephthalate resin in the atmospheric window as a representative example of a resin having an ester bond or a benzene ring. Ester bonds have an absorption coefficient in the wavelength range from 7.8 μm to 9.9 μm. Furthermore, the carbon-oxygen bonds contained in ester bonds have a strong absorption coefficient in the wavelength range from 8 μm to 10 μm. When a benzene ring is introduced into the side chain of a hydrocarbon resin, absorption appears in a wide range from 8.1 μm to 18 μm due to the vibration of the benzene ring itself and the vibration of surrounding elements caused by the influence of the benzene ring. Due to these effects, the wavelength average of the emissivity of a 10 μm thick film is 71% at wavelengths from 8 μm to 14 μm, which falls within the regulation of a wavelength average of 40% or more. As shown in the figure, the emissivity in the atmospheric window region increases as the film thickness increases.

[0071] [Emissivity of olefin modified materials] Figure 15 shows the emissivity spectrum of an olefin-modified material that does not contain carbon-fluorine bonds (CF), carbon-chlorine bonds (C-Cl), ester bonds (R-COO-R), ether bonds (COC bonds), or benzene rings, and whose main component is olefin. The sample was prepared by applying olefin resin onto evaporated silver with a bar coater and drying it. As shown in the figure, the emissivity in the atmospheric window region is small, and as a result, the wavelength average of the emissivity for a thickness of 10 μm is 27% at wavelengths from 8 μm to 14 μm, which does not fall within the regulation that the wavelength average is 40% or more.

[0072] The emissivity shown is that of an olefin resin modified for application with a bar coater, and in the case of a pure olefin resin, the emissivity in the atmospheric window region is even smaller. Thus, radiative cooling is not possible unless the molecule contains a carbon-fluorine bond (CF), a carbon-chlorine bond (C-Cl), an ester bond (R-COO-R), an ether bond (COC bond), or a benzene ring.

[0073] [Surface Temperature of Light Reflecting Layer and Resin Material Layer] Thermal radiation from the atmospheric window of the infrared radiation layer J occurs near the surface of the resin material. As shown in Fig. 11, in the case of silicone rubber, if the thickness is greater than 10 μm, the thermal radiation in the air window region does not increase. In other words, in the case of silicone rubber, most of the thermal radiation in the air window occurs within a depth of about 10 μm from the surface, and radiation from deeper parts does not escape.

[0074] From Figure 12, in the case of fluororesin, even if the thickness exceeds 100 μm, there is almost no increase in thermal radiation in the atmospheric window region. In other words, in the case of fluororesin, thermal radiation in the atmospheric window occurs within a depth of about 100 μm from the surface, and radiation from deeper parts does not escape to the outside. From Figure 13, in the case of polyvinyl chloride resin, even if the thickness exceeds 100 μm, there is almost no increase in thermal radiation in the atmospheric window region. In other words, in the case of polyvinyl chloride resin, thermal radiation in the atmospheric window occurs within a depth of about 100 μm from the surface, and radiation from deeper parts does not escape to the outside. From FIG. 21, it can be seen that vinylidene chloride resin is similar to vinyl chloride resin.

[0075] 14, in the case of ethylene terephthalate resin, even if the thickness exceeds 125 μm, there is almost no increase in thermal radiation in the air window region. In other words, in the case of ethylene terephthalate resin, thermal radiation in the air window occurs at a depth of about 100 μm from the surface, and radiation from deeper parts does not escape to the outside.

[0076] As described above, the thermal radiation from the atmospheric window region generated from the surface of the resin material occurs within a depth of approximately 100 μm from the surface. If the resin thickness increases beyond this, the cold generated by the radiative cooling of the glass composite W is insulated by the resin material that does not contribute to thermal radiation. Consider an infrared emitting layer J, which ideally does not absorb any sunlight, formed on a light reflecting layer B. In this case, sunlight is absorbed only by the light reflecting layer B of the glass composite W. The thermal conductivity of resin materials is generally about 0.2 W / m / K. When calculations are made taking this thermal conductivity into consideration, if the thickness of the infrared emitting layer J exceeds 20 mm, the temperature of the cooling surface (the surface of the light reflecting layer B opposite the side where the infrared emitting layer J is present) will rise.

[0077] Even if an ideal resin material that does not absorb any sunlight exists, the thermal conductivity of resin materials is generally about 0.2 W / m / K, so if the thickness exceeds 20 mm as shown in Figure 16, the light reflecting layer B will be heated by sunlight and the object to be cooled (not shown) placed on the light reflecting layer side will be heated. In other words, the thickness of the resin material as the auxiliary infrared radiation layer J of the glass composite W needs to be 20 mm or less.

[0078] FIG. 16 is a plot of the surface temperature of the radiating surface H of the glass composite W and the temperature of the light reflecting layer B, calculated assuming a clear day in the meridian at midsummer in western Japan. The sunlight is AM1.5 and 1000W / m 2 The outside temperature is 30°C, and the radiant energy varies depending on the temperature, but is 100W at 30°C. This calculation assumes that the resin material layer does not absorb sunlight. It is assumed that there is no wind, and the convection heat transfer coefficient is 5W / m 2 / K.

[0079] [Light absorptivity of silicone rubber, etc.] Figure 17 shows the light absorptance of silicone rubber with CH3 side chains at a thickness of 100 μm against the sunlight spectrum, and the light absorptance spectrum of perfluoroalkoxy fluororesin at a thickness of 100 μm against the sunlight spectrum. As mentioned above, it can be seen that both resins have almost no light absorptance in the ultraviolet region.

[0080] For silicone rubber, in the near infrared region, the light absorptance increases in the region longer than 2.35 μm. However, because the intensity of the solar spectrum in this wavelength region is weak, even if the light absorptance on the longer wavelength side than 2.35 μm is 100%, the solar energy absorbed is only 20 W / m 2 It is.

[0081] Perfluoroalkoxy fluororesin has almost no light absorption in the wavelength range of 0.3 μm to 2.5 μm, but has light absorption on the longer wavelength side than 2.5 μm. However, even if the film thickness of the resin is increased and the light absorption on the longer wavelength side than 2.5 μm becomes 100%, the solar energy absorbed is about 7 W.

[0082] In addition, if the thickness (film thickness) of the infrared radiation layer J is increased, the emissivity of the atmospheric window region becomes almost 1. In other words, in the case of a thick film, the thermal radiation radiated to space in the atmospheric window region when used at low altitudes is 160 W / m at 30°C. 2 from 125 W / m 2 The light absorption in the light reflecting layer B is about 50 W / m 2 Even if the light absorption of the light reflective layer B and the sunlight absorption when the silicone rubber or perfluoroalkoxy fluororesin is made into a thick film are added together, the total amount is smaller than the thermal radiation radiated into space. From the above, the maximum film thickness of silicone rubber and perfluoroalkoxy fluororesin is 20 mm from the viewpoint of thermal conductivity.

[0083] [Light absorption of hydrocarbon resins] When the resin material forming the infrared radiation layer J is a resin having a main chain made of a hydrocarbon having one or more carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, ether bonds, or benzene rings, or when the resin material is a silicone resin having two or more carbon atoms in the hydrocarbon side chain, absorption due to vibrations such as bond bending and stretching is observed in the near-infrared region in addition to the ultraviolet absorption due to the covalent bond electrons described above.

[0084] Specifically, the absorption due to the reference tones of the transitions to the first excited state of CH3, CH2, and CH appears at wavelengths of 1.6 μm to 1.7 μm, 1.65 μm to 1.75 μm, and 1.7 μm, respectively. Furthermore, the absorption due to the reference tones of the combination tones of CH3, CH2, and CH appears at wavelengths of 1.35 μm, 1.38 μm, and 1.43 μm, respectively. Furthermore, the overtones of the transitions to the second excited state of CH2 and CH appear at around 1.24 μm. The reference tones of the bending and stretching of the CH bond are distributed over a wide band from 2 μm to 2.5 μm.

[0085] Furthermore, when an ester bond (R-COO-R) or an ether bond (COC) is present, a large optical absorption occurs at a wavelength of around 1.9 μm. According to the above-mentioned light absorptance relational expression, the light absorptance caused by these factors becomes smaller and less noticeable when the resin material film is thin, but becomes larger when the film is thick.

[0086] FIG. 18 shows the relationship between the light absorptance and the spectrum of sunlight when the film thickness of an ethylene terephthalate resin having an ester bond and a benzene ring is changed. As shown in the figure, as the film thickness increases from 25 μm to 125 μm to 500 μm, the optical absorption in the wavelength range longer than 1.5 μm caused by the respective vibrations increases. In addition, the light absorption increases not only on the long wavelength side but also from the ultraviolet region to the visible region. This is due to the broadening of the light absorption edge caused by chemical bonds.

[0087] When the film thickness is thin, the light absorption rate is high at the wavelength with the largest absorption coefficient, but when the film thickness is thick, the weak absorption coefficient at the absorption edge with a broader spread appears as the absorption rate according to the above-mentioned light absorption rate relational expression. As a result, the light absorption increases from the ultraviolet region to the visible region as the film thickness increases. When the thickness is 25 μm, the absorption of the solar spectrum is 15 W / m 2 When the thickness is 125 μm, the absorption of the solar spectrum is 41 W / m 2 , the solar spectrum absorption at a thickness of 500 μm is 88 W / m 2 It is.

[0088] The light absorption of the light reflecting layer B is 50 W / m 2 Therefore, when the film thickness is 500 μm, the sum of the solar light absorption of the ethylene terephthalate resin and the solar light absorption of the light reflective layer B is 138 W / m 2 As mentioned above, the maximum value of infrared radiation in the wavelength band of the atmospheric window in the summer in lowlands of Japan is about 160 W at 30°C on a day with good atmospheric conditions, and usually about 125 W. From the above, it is found that if the thickness of the ethylene terephthalate resin film is 500 μm or more, the radiative cooling performance is not exhibited.

[0089] The origin of the absorption spectrum in the wavelength band from 1.5 μm to 4 μm is the vibration of the hydrocarbon main chain, not the functional group, and if it is a hydrocarbon-based resin, it will show the same behavior as ethylene terephthalate resin. In addition, hydrocarbon-based resins have light absorption due to chemical bonds in the ultraviolet range, and they show the same behavior as ethylene terephthalate resin from ultraviolet to visible light. In other words, hydrocarbon resins behave similarly to ethylene terephthalate resins from wavelengths of 0.3 μm to 4 μm. For this reason, the film thickness of hydrocarbon resins must be thinner than 500 μm.

[0090] [Light absorption of blended resins] When the resin material is a blend of a resin having a main chain of a carbon-fluorine bond or a siloxane bond and a resin having a main chain of a hydrocarbon, light absorption in the near-infrared region caused by CH, CH2, CH3, etc. appears according to the ratio of the blended resin having a main chain of a hydrocarbon. When the main component is carbon-fluorine bond or siloxane bond, the light absorption in the near infrared region caused by hydrocarbon is small, so the thickness can be increased up to the upper limit of 20 mm from the viewpoint of thermal conductivity. However, when the main component is a blended hydrocarbon resin, the thickness must be 500 μm or less.

[0091] Blends of fluororesin or silicone rubber with hydrocarbons include those in which the side chains of fluororesin or silicone rubber are replaced with hydrocarbons, and alternating copolymers, random copolymers, block copolymers, and graft copolymers of fluoromonomers, silicone monomers, and hydrocarbon monomers. Examples of alternating copolymers of fluoromonomers and hydrocarbon monomers include fluoroethylene-vinyl ester (FEVE), fluoroolefin-acrylic acid ester copolymer, ethylene-tetrafluoroethylene copolymer (ETFE), and ethylene-chlorotrifluoroethylene copolymer (ECTFE).

[0092] Depending on the molecular weight and ratio of the substituted hydrocarbon side chains, optical absorption in the near infrared region caused by CH, CH2, CH3, etc. appears. When the monomers introduced as side chains or copolymers are low molecular weight, or when the density of the monomers introduced is low, optical absorption in the near infrared region caused by hydrocarbons becomes small, so the thickness can be increased up to 20 mm, which is the limit from the viewpoint of thermal conductivity. When a high molecular weight hydrocarbon is introduced as a side chain of a fluororesin or silicone rubber or as a copolymerizable monomer, the thickness of the resin must be 500 μm or less.

[0093] [Thickness of resin material layer] From the viewpoint of practical use of the glass composite W, it is preferable that the thickness of the infrared emitting layer J is thin. The thermal conductivity of a resin material is generally lower than that of metal or glass. To effectively cool an object to be cooled (not shown), it is preferable that the thickness of the infrared emitting layer J is the minimum necessary. The thicker the thickness of the infrared emitting layer J, the greater the thermal radiation of the atmospheric window becomes, and when a certain thickness is exceeded, the thermal radiation energy at the atmospheric window becomes saturated.

[0094] The thickness at which the film saturates depends on the resin material, but in the case of fluororesin, 300 μm is generally sufficient for saturation. Therefore, from the perspective of thermal conductivity, it is preferable to keep the film thickness at 300 μm or less rather than 500 μm. Furthermore, although thermal radiation is not saturated, sufficient thermal radiation can be obtained in the atmospheric window region even with a thickness of about 100 μm. The thinner the thickness, the higher the thermal conductivity and the more effectively the temperature of the object to be cooled can be lowered, so in the case of fluororesin, it is best to keep the thickness at about 100 μm or less.

[0095] The absorption coefficients due to carbon-silicon bonds, carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, and ether bonds are greater than the absorption coefficient due to C-F bonds. Naturally, from the viewpoint of thermal conductivity, it is preferable to keep the film thickness to 300 μm or less rather than 500 μm, but an even greater radiative cooling effect can be expected if the film thickness is made even thinner to increase thermal conductivity. In the case of resins containing carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, ether bonds, and benzene rings, even a thickness of 100 μm is saturated, and even a thickness of 50 μm provides sufficient thermal radiation in the atmospheric window region. The thinner the resin material, the higher the thermal transmittance and the more effectively the temperature of the object to be cooled can be lowered, so in the case of resins containing carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, ether bonds, and benzene rings, a thickness of 50 μm or less reduces the insulation and allows the object to be cooled effectively. In the case of carbon-chlorine bonds, a thickness of 100 μm or less allows the object to be cooled effectively.

[0096] The benefit of making the glass thinner is not just that it reduces heat insulation and makes it easier to transfer heat. It also reduces the absorption of near-infrared light originating from CH, CH2, and CH3 in the near-infrared region, which is exhibited by resins that contain carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, and ether bonds. By making the glass thinner, it is possible to reduce the amount of sunlight absorbed by these bonds, which increases the cooling capacity of the glass composite W. From the above perspective, in the case of resins containing carbon-chlorine bonds, carbon-oxygen bonds, ester bonds, ether bonds, and benzene rings, a thickness of 50 μm or less can more effectively produce a radiative cooling effect under sunlight.

[0097] In the case of carbon-silicon bonds, even with a thickness of 50 μm, thermal radiation is saturated in the atmospheric window region, and even with a thickness of 10 μm, sufficient thermal radiation can be obtained in the atmospheric window region. The thinner the infrared radiation layer J, the higher the thermal transmittance and the more effectively the temperature of the object to be cooled can be lowered, so in the case of resins containing carbon-silicon bonds, a thickness of 10 μm or less reduces the thermal insulation and allows the object to be cooled to be cooled effectively. The thinner the layer, the less sunlight absorption it can be, and the greater the cooling capacity of the glass composite W. From the above perspective, in the case of resins containing carbon-silicon bonds, a thickness of 10 μm or less can more effectively produce a radiative cooling effect under sunlight.

[0098] [Details of the light reflecting layer] As shown in FIG. 19, if the light reflecting layer B is formed based on silver, the reflectance required for the light reflecting layer B can be satisfactorily obtained.

[0099] Incidentally, the "silver alloy" may be an alloy in which, for example, 0.4% to 4.5% by mass of any of copper, palladium, gold, zinc, tin, magnesium, nickel, and titanium is added to silver. A specific example is "APC-TR (made by Furuya Metal)," a silver alloy made by adding copper and palladium to silver.

[0100] In order to provide the light-reflecting layer B with appropriate reflectance characteristics, a laminated structure may be used in which silver or a silver alloy is located adjacent to the protective layer and aluminum or an aluminum alloy is located away from the protective layer. Even in this case, the reflective material on the side where the radiation surface H exists (the side where the infrared radiation layer J exists) must be silver or a silver alloy. When it is composed of two layers of silver (silver alloy) and aluminum (aluminum alloy), the thickness of the silver needs to be 10 nm or more, and the thickness of the aluminum needs to be 30 nm or more.

[0101] Incidentally, examples of "aluminum alloys" that can be used include alloys in which aluminum has been doped with copper, manganese, silicon, magnesium, zinc, carbon steel for mechanical structures, yttrium, lanthanum, gadolinium, and terbium.

[0102] Silver and silver alloys are vulnerable to rain and humidity and need to be protected from them, and also need to be prevented from tarnishing. For this reason, it is preferable to provide a protective layer for protecting the silver adjacent to the silver or silver alloy.

[0103] [About the experimental results] Silver was formed to a thickness of 300 nm on a glass substrate, and silicone rubber with siloxane bonds, fluoroethylene vinyl ether with carbon-fluorine bonds, olefin modified material (olefin modified material), and polyvinyl chloride resin were applied on top of it while controlling the film thickness with a bar coater, and the radiative cooling performance was measured. The evaluation of radiative cooling performance was carried out three hours after sundown outdoors in late June when the outside temperature was 35°C, and the temperature (°C) of the backside of the board was measured while the board was kept highly insulated. However, for polyvinyl chloride resin, the evaluation was carried out when the outside temperature was 29°C. The presence or absence of a radiative cooling effect was evaluated based on whether the temperature five minutes after placement on the jig was lower or higher than the outside temperature. The results of the radiative cooling test are shown in Figure 22.

[0104] Incidentally, the emissivity of the atmospheric window region of fluoroethylene vinyl ether is as shown in Figure 20. The emissivity of silicone rubber is as shown in Figure 11, the emissivity of an olefin modified body (olefin modified material) is as shown in Figure 15, and the emissivity of polyvinyl chloride resin is as shown in Figure 13.

[0105] In the case of silicone rubber containing siloxane bonds, it was found that a thickness of 1 μm or more exhibits radiative cooling capabilities, as predicted by theory. It was found that fluoroethylene vinyl ether, which has a carbon-fluorine bond, exhibits radiative cooling ability at a film thickness of 5 μm, which is thinner than the theoretically predicted thickness of 10 μm. This is because the optical absorption rate of the atmospheric window is increased by not only the optical absorption of the carbon-fluorine bond but also the optical absorption of the ether bond of the vinyl ether, compared to when each is used alone. Olefin modified materials (olefin modified materials) have no radiative cooling ability because they hardly radiate heat in the atmospheric window region.

[0106] [Details of protective layer] The protective layer (auxiliary infrared emitting layer J) is preferably made of a polyolefin resin having a thickness of 300 nm or more and 40 μm or less, or polyethylene terephthalate having a thickness of 17 μm or more and 40 μm or less. Polyolefin resins include polyethylene and polypropylene.

[0107] FIG. 23 shows the ultraviolet light absorptance of polyethylene, vinylidene chloride resin, ethylene terephthalate resin, and vinyl chloride resin. FIG. 24 shows the light transmittance of polyethylene, which is a suitable synthetic resin for forming the protective layer.

[0108] Since the glass composite W exerts a radiative cooling effect not only at night but also in a solar radiation environment, in order to maintain the light-reflecting layer B in a state in which it exerts its light-reflecting function, it is necessary to protect the light-reflecting layer B with a protective layer so that the silver of the light-reflecting layer B does not discolor in a solar radiation environment.

[0109] When the protective layer is made of polyolefin resin and has a thickness of 300 nm or more and 40 μm or less, the polyolefin resin is a synthetic resin that has an ultraviolet light absorptance of 10% or less over the entire ultraviolet wavelength range of 0.3 μm to 0.4 μm, so that the protective layer is less likely to deteriorate due to absorption of ultraviolet light.

[0110] Furthermore, since the thickness of the polyolefin resin forming the protective layer is 300 nm or more, it effectively exhibits a blocking function of blocking radicals generated in the infrared emitting layer J from reaching the silver or silver alloy forming the light reflective layer B, and also blocks moisture passing through the infrared emitting layer J from reaching the silver or silver alloy forming the light reflective layer B, thereby making it possible to suppress discoloration of the silver or silver alloy forming the light reflective layer B.

[0111] Incidentally, the protective layer made of polyolefin resin deteriorates as it absorbs ultraviolet rays, forming radicals on the surface side away from the light-reflecting layer B. However, since the thickness is 300 nm or more, the formed radicals will not reach the light-reflecting layer B. Even if the protective layer deteriorates as radicals are formed, the rate of deterioration is slow due to the low absorption of ultraviolet rays, so the above-mentioned blocking function will be maintained for a long period of time.

[0112] When the protective layer is formed from ethylene terephthalate resin to a thickness of 17 μm or more and 40 μm or less, ethylene terephthalate resin is a resin material that has a higher ultraviolet light absorptance in the ultraviolet wavelength range of 0.3 μm to 0.4 μm than polyolefin resin. However, since the thickness is 17 μm or more, the protective layer can effectively exhibit blocking functions for a long period of time, such as blocking radicals generated in the infrared emitting layer J from reaching the silver or silver alloy that forms the light reflecting layer B and blocking moisture that penetrates the infrared emitting layer J from reaching the silver or silver alloy that forms the light reflecting layer B, and can suppress discoloration of the silver or silver alloy that forms the light reflecting layer B.

[0113] In other words, the protective layer made of ethylene terephthalate resin will deteriorate as it absorbs ultraviolet rays, forming radicals on the surface side away from the light-reflecting layer B. However, since the thickness is 17 μm or more, the formed radicals will not reach the light-reflecting layer B. Furthermore, even if the protective layer deteriorates while forming radicals, the thickness is 17 μm or more, so the above-mentioned blocking function will be maintained for a long period of time.

[0114] To explain further, the deterioration of ethylene terephthalate resin (PET) is caused by ultraviolet light cleaving the ester bonds between ethylene glycol and terephthalic acid to form radicals. This deterioration progresses from the surface of the ethylene terephthalate resin (PET) that is irradiated with ultraviolet light.

[0115] For example, when ethylene terephthalate resin (PET) is irradiated with ultraviolet rays with the strength in Osaka, the ester bonds of the ethylene terephthalate resin (PET) are cleaved by about 9 nm per day, starting from the irradiated surface. Because the ethylene terephthalate resin (PET) is sufficiently polymerized, the cleaved ethylene terephthalate resin (PET) on the surface does not attack the silver (silver alloy) of the light-reflecting layer B. However, when the cleaved end of the ethylene terephthalate resin (PET) reaches the silver (silver alloy) of the light-reflecting layer B, the silver (silver alloy) will discolor.

[0116] Therefore, for a protective layer to last for more than one year when used outdoors, a thickness of about 3μm is required, calculated by multiplying 9nm / day by 365 days. For the ethylene terephthalate resin (PET) protective layer to last for more than three years, a thickness of 10μm or more is required. For it to last for more than five years, a thickness of 17μm or more is required.

[0117] In addition, when the protective layer is formed of a polyolefin resin and an ethylene terephthalate resin, the reason for determining the upper limit of the thickness is to prevent the protective layer from exhibiting heat insulating properties that do not contribute to radiative cooling. In other words, the thicker the protective layer is, the more heat insulating properties it exhibits that do not contribute to radiative cooling. Therefore, the upper limit of the thickness is determined to prevent the protective layer from exhibiting heat insulating properties that do not contribute to radiative cooling while still exerting the function of protecting the light reflecting layer B.

[0118] In other words, if the protective layer becomes thicker, there will be no disadvantage in terms of preventing coloring of the silver (silver alloy) in the light-reflecting layer B, but it will cause problems in terms of radiative cooling. In other words, making the protective layer thicker will increase the thermal insulation properties of the radiative cooling material. For example, a resin whose main component is polyethylene, which is an excellent synthetic resin for forming a protective layer, has a low emissivity at the atmospheric window, as shown in Figure 28, so even if it is formed thickly, it does not contribute to radiative cooling. On the contrary, making it thicker increases the thermal insulation of the radiative cooling material. Next, as the thickness increases, absorption of near-infrared light originating from the vibration of the main chain increases, increasing the effect of increasing solar absorption. Due to these factors, a thick protective layer is disadvantageous for radiative cooling. From this viewpoint, the thickness of the protective layer made of a polyolefin resin is preferably 5 μm or less, and more preferably 1 μm.

[0119] [Considerations on protective layer] In order to examine the difference in the way the protective layer colored the silver, a sample in which the protective layer was exposed and did not include the infrared emitting layer J was prepared as shown in Figure 25, and the coloring of the silver after being irradiated with simulated sunlight was examined. That is, as a protective layer, samples were formed by applying two types of materials, a general acrylic resin that absorbs ultraviolet rays (for example, methyl methacrylate resin mixed with a benzotriazole-based ultraviolet absorber) and polyethylene, to a film layer F (corresponding to the substrate) containing silver as a light-reflecting layer B using a bar coater, and their function as a protective layer was examined. The thicknesses of the applied protective layers were 10 μm and 1 μm, respectively. The film layer F (corresponding to the substrate) is formed into a film shape using PET (ethylene terephthalate resin) or the like.

[0120] As shown in Figure 27, if the protective layer is made of acrylic resin, which absorbs ultraviolet rays well, the protective layer is decomposed by ultraviolet rays to form radicals, and the silver immediately turns yellow and no longer functions as the glass composite W (it absorbs sunlight and rises in temperature when exposed to sunlight, like general materials). The 600h line in the figure indicates the time when the product was subjected to a xenon weather test under the conditions of JIS standard 5600-7-7 (ultraviolet light energy is 60W / m 2 The reflectance spectrum after 600h (hours) of exposure to xenon weathering is shown in Fig. 1. The 0h line is the reflectance spectrum before the xenon weathering test.

[0121] As shown in Figure 26, when the protective layer is made of polyethylene, which has a low ultraviolet light absorption rate, no decrease in reflectance is observed from the near infrared region to the visible region. In other words, resins whose main component is polyethylene (polyolefin resins) hardly absorb the ultraviolet light contained in sunlight that reaches the ground, and so radicals are unlikely to form even when exposed to sunlight, so coloring of the silver serving as the light-reflecting layer B does not occur even when exposed to sunlight. The 600h line in the figure indicates the time when the product was subjected to a xenon weather test under the conditions of JIS standard 5600-7-7 (ultraviolet light energy is 60W / m 2 The reflectance spectrum after 600h (hours) of exposure to xenon weathering is shown in Fig. 1. The 0h line is the reflectance spectrum before the xenon weathering test.

[0122] The reason why the reflectance spectrum in this wavelength band is wavy is due to the Fabry-Perot resonance of the polyethylene layer. It can be seen that the resonance position is slightly different between the 0h line and the 600h line due to the change in the thickness of the polyethylene layer caused by the heat of the xenon weather test, but no significant decrease in reflectance in the ultraviolet-visible range due to the yellowing of silver is observed.

[0123] From the viewpoint of ultraviolet light absorption, fluororesin-based materials can also be used as materials for forming protective layers. However, when actually formed into a protective layer, they become discolored and deteriorate during the formation stage, and therefore cannot be used as materials for forming protective layers. Silicone can also be used as a material for forming a protective layer from the viewpoint of ultraviolet light absorption, but it has extremely poor adhesion to silver (silver alloys) and cannot be used as a material for forming a protective layer.

[0124] [Test Results] Regarding the glass composite W described above, those having the structure shown in Fig. 1 were designated as Examples 1, 5, and 6, those having the structure shown in Fig. 4 were designated as Example 2, those having the structure shown in Fig. 5 were designated as Examples 3 and 7, and those having the structure shown in Fig. 6 were designated as Example 4. In addition, as shown in Fig. 8, a structure in which an infrared emitting glass layer G, a light reflective layer B, and an infrared emitting layer J were laminated in the listed order from the atmospheric side was designated as Comparative Example 1, and an infrared emitting glass layer alone was designated as Comparative Example 2.

[0125] The conditions for the glass composite W tested in the examples and comparative examples are as shown in the following [Table 2]. The test results are shown in [Table 1].

[0126] [Table 1]

[0127] [Table 2]

[0128] The above test results show that the glass composites W according to Examples 1 to 7 provide good results in terms of emissivity, visible light reflectance, radio wave transmittance, daylighting properties, and glare resistance. On the other hand, in the glass composite W of Comparative Example 1, since the light-reflecting layer B does not have a thin portion, it is presumed that the test conditions for radio wave transmittance, lighting, and anti-reflection properties are not satisfied. Moreover, in the glass composite W according to Comparative Example 2, since the light reflecting layer B is not provided, it is presumed that the test conditions for visible light reflectance are not satisfied.

[0129] [Another embodiment] (1) The glass composite W described above may have a light control layer (not shown) having a light control function on the side of the auxiliary infrared emitting layer J opposite to the side on which the light reflecting layer B is present. Alternatively, a light control layer (not shown) having a light control function may be provided on the side of the infrared emitting back glass layer G2 opposite to the side on which the auxiliary infrared emitting layer J is present.

[0130] (2) The glass composite W described above may have a configuration in which an ultraviolet reflective layer that reflects ultraviolet rays is provided along the emitting surface H. In the case of the glass composite W, the ultraviolet reflective layer can be suitably made of a material such as an aluminum alloy.

[0131] Furthermore, the configurations disclosed in the above embodiments (including other embodiments, the same applies below) can be applied in combination with configurations disclosed in other embodiments, provided that no contradiction arises. Furthermore, the embodiments disclosed in this specification are merely examples, and the embodiments of the present invention are not limited thereto, and can be appropriately modified within the scope that does not deviate from the purpose of the present invention. [Industrial Applicability]

[0132] INDUSTRIAL APPLICABILITY The glass composite of the present invention can be effectively used as a glass composite that can improve electromagnetic wave transmittance and daylighting properties and can reduce glare at night, etc. [Explanation of symbols]

[0133] A: Infrared radiation layer B: Light reflective layer B1: 1st metal thin section B2: 2nd metal thin section B3:Thick part G1: Infrared radiation glass layer G2: Rear glass layer H: Radiation surface H1: 1st radiation surface H2: Second radiation surface H3: 3rd radiation surface J:Supplementary infrared radiation layer L1: Thickness of thin section L2: Thickness of thick part Tu: Intermediate resin W: Glass composite Z:Lamination direction

Claims

1. a glass composite comprising: an infrared emitting glass layer that emits infrared light from a first emitting surface that is a emitting surface; and a light reflecting layer that is located on an opposite side of the infrared emitting glass layer to a side on which the first emitting surface is present, laminated in the order described above; the light reflecting layer has a thick portion in a stacking direction and a thin portion whose thickness in the stacking direction is 2 / 3 or less of the thickness of the thick portion, The thin portion is provided continuously and integrally in a plan view perpendicular to the first radiation surface and has an area of ​​5 cm 2 a first metal thin portion having an area equal to or greater than the area of ​​the first metal thin portion, and a second metal thin portion provided integrally and continuously in the plan view and having an area in the plan view less than the area of ​​the first metal thin portion, The second thin metal portion is provided in a plurality of portions in a dispersed manner in the plan view, A glass composite having an overall surface average solar reflectance of 40% or more and a surface average average emissivity, which is the wavelength average of the emissivity of infrared light of 8 μm or more and 13 μm or less, of 80% or more.

2. The glass composite according to claim 1 , wherein the first thin metal portion and the second thin metal portion each have a thickness in the stacking direction of 0 nm or more and 50 nm or less.

3. The glass composite according to claim 1 , wherein the first thin metal portion and the second thin metal portion each have a thickness in the stacking direction of 0 nm or more and 10 nm or less.

4. In the plan view, the area of ​​the second metal thin portion is 0.03 cm 2 The glass composite according to claim 1 or 2.

5. a protective layer for protecting the light reflecting layer on the side of the light reflecting layer opposite to the side where the infrared radiation glass layer is present; 3. The glass composite according to claim 1, wherein the protective layer is an auxiliary infrared emitting layer that emits infrared light from a second emitting surface that is an emitting surface on the opposite side to the side on which the light reflecting layer is present.

6. a back glass layer is provided on the side of the auxiliary infrared radiation layer opposite to the side on which the light reflecting layer is present; the rear surface glass layer is an infrared radiation rear surface glass layer that emits infrared light from a third radiation surface that is an radiation surface on the opposite side to the side on which the auxiliary infrared radiation layer is present, 6. The glass composite of claim 5, wherein the intermediate resin that bonds the auxiliary infrared-emitting layer and the infrared-emitting back glass layer comprises at least one of polyvinyl butyral, polyethylene vinyl acetate, and polyurethane.

7. The infrared emitting glass layer is 2. The glass composite according to claim 1, which is made of at least one of alkali-free glass, soda-lime glass, alkali borosilicate glass, and acrylic resin glass.

8. The infrared radiation glass layer and the infrared radiation back surface glass layer are 7. The glass composite according to claim 6, which is made of at least one of alkali-free glass, soda-lime glass, alkali borosilicate glass, and acrylic resin glass.

9. In the plan view, 3. The glass composite according to claim 1, wherein a ratio of an area of ​​the thin portion to an entire area of ​​the light reflective layer is 1% or more and 50% or less.

10. the light reflecting layer is a metal vapor-deposited layer formed by vapor-depositing a metal on a side of the infrared radiation glass layer opposite to a side on which the first radiation surface is present, 3. The glass composite according to claim 1, wherein the metal is at least one of silver, a silver alloy, aluminum, an aluminum alloy, and a copper alloy.

11. The glass composite according to claim 5 , further comprising a light control layer having a light control function on the side of the auxiliary infrared radiation layer opposite to the side on which the light reflecting layer is present.

12. The glass composite according to claim 6 , further comprising a light control layer having a light control function on the side of the infrared radiation back glass layer opposite to the side on which the auxiliary infrared radiation layer is present.

Citation Information

Patent Citations

  • Windshield for vehicle and method for manufacturing the same

    JP2002020142A

  • Highly heat insulating dimming glass and method of manufacturing the same

    JP2006206398A

  • Laminate and vehicle roof window

    JP2014034486A

  • Substantially transparent substrate with high-emissivity and low-emissivity coating layers - Patent Application 20070122997