SiC-coated graphite component joint

The bonded body of SiC-coated graphite members addresses the challenge of achieving high bonding strength and airtightness by employing a dual-joint structure with a convex and recessed design, ensuring thin CVD-SiC layers maintain airtightness and bonding strength effectively.

JP7580925B2Active Publication Date: 2024-11-12IBIDEN CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020046660
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-17
Publication Date
2024-11-12
Estimated Expiration
2040-03-17

AI Technical Summary

Technical Problem

Existing bonded bodies of SiC-coated graphite materials face challenges in achieving high bonding strength, dimensional accuracy, and airtightness simultaneously due to the trade-off between CVD-SiC layer thickness, where insufficient thickness leads to inadequate gap filling and decreased airtightness, while excessive thickness compromises dimensional accuracy.

Method used

A bonded body of SiC-coated graphite members with a convex portion and a recessed portion on the combination surface, utilizing a first joint along the outer surface and a second joint penetrating into the recess, where the CVD-SiC layer is applied to ensure thin layers maintain airtightness and bonding strength by dividing roles between the two joints.

Benefits of technology

The solution provides a bonded body with high bonding strength and airtightness, ensuring a thin CVD-SiC layer maintains airtightness at one end and bonding strength at the other, overcoming the limitations of traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580925000001
    Figure 0007580925000001
  • Figure 0007580925000002
    Figure 0007580925000002
  • Figure 0007580925000003
    Figure 0007580925000003
Patent Text Reader

Abstract

To provide a joined body of a SiC clad graphite material high in bond strength, excellent in dimensional accuracy, and high in air-tightness.SOLUTION: A joint body of SiC-clad graphite members in which a CVD-SiC layer covers a surface of a substrate made of graphite and a plurality of the substrates are joined by the CVD-SiC layer via a mating surface, in which at least one of the substrates has a convex part higher than the surrounding on one side of the combination surface and a concave part opened toward the outside on the other side when combined with the other substrate. The CVD-SiC layer has a first joint part joining the substrate along an outer surface of the joint body, on the outside of the convex part of the combination surface, and has the second joint part penetrated into the concave part outside of the convex part of the combination surface and joining opposite surfaces of the substrates.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a joined body of SiC-coated graphite members in which a composite material having a CVD-SiC layer on the surface of a substrate is joined with a CVD-SiC layer. [Background technology]

[0002] In order to supply high-quality products in semiconductor manufacturing, thereby improving the yield of semiconductor products and ensuring stable operation, composite materials in which a CVD-SiC layer is coated on the surface of a graphite base material are widely used for semiconductor device parts such as susceptors, jigs, furnace components, etc., used in the heat treatment process of silicon wafers, etc. Materials such as graphite and SiC are suitable for semiconductor device parts because they do not dope silicon even when mixed with silicon and do not change the electrical conductivity, so they have little effect on the quality of the obtained wafer, and both SiC and graphite are stable at high temperatures and therefore wear out little.

[0003] Graphite is easy to process and can easily be made into complex shapes, but it has the disadvantage of being easily worn away by contact with oxygen, water, hydrogen, etc. On the other hand, SiC is characterized by being easy to form a thin oxide film on its surface and being resistant to wear from oxygen, water, hydrogen, etc., but it has the disadvantage of being hard and difficult to process. A composite material in which a CVD-SiC layer is formed on the surface of a graphite substrate makes good use of these characteristics and disadvantages. In such composite materials, the substrate itself is very easy to process, so complex shapes can be easily obtained, and the surface is covered with a CVD-SiC layer, making it a durable composite material that can be used in a variety of atmospheres.

[0004] Patent Document 1 describes a component for semiconductor manufacturing equipment, which is a tube for a semiconductor diffusion furnace having a shape in which one end side of a long cylindrical portion is tapered, and which is characterized in that a tapered portion made of silicon carbide or graphite is joined to one end of a long cylinder made of silicon carbide or graphite by a silicon carbide CVD film, and at least the entire inner circumferential surface of the tube is coated with a CVD film. It is described that such semiconductor manufacturing equipment parts are covered with a high-purity, dense SiC coating, and that the gaps between the assembled parts are filled with CVD precipitates and joined together, eliminating any rattling of the parts. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 62-200722 Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the above-mentioned invention, the gap is filled with a CVD-SiC layer, so in order to create a sufficient gap in advance and completely fill the gap, a CVD-SiC layer of sufficient thickness is required. However, there is a problem that the dimensional accuracy deteriorates when the CVD-SiC layer is made thick. In addition, if a thin CVD-SiC layer is used, the gaps cannot be filled sufficiently, resulting in a trade-off in reduced airtightness. This posed the challenge of making it difficult to obtain a bonded SiC-coated graphite material that simultaneously satisfied the requirements for bonding strength, dimensional accuracy, and airtightness.

[0007] In view of the above problems, an object of the present invention is to provide a joined body of SiC-coated graphite materials having high joining strength, excellent dimensional accuracy, and high airtightness. [Means for solving the problem]

[0008] In order to solve the above problems, a joined body of SiC-coated graphite members of the present invention is a joined body of SiC-coated graphite members in which a CVD-SiC layer covers a surface of a base material made of graphite, and a plurality of the base materials are joined by the CVD-SiC layer via a mating surface, At least one of the substrates has a convex portion higher than the surrounding area on one end side of the combination surface, and a concave portion on the other end side that opens to the outside when combined with the other substrate, and the CVD-SiC layer has a first bonding portion that bonds the substrate along the outer surface of the bonded body outside the convex portion of the combination surface, and a second bonding portion that penetrates into the concave portion outside the concave portion of the combination surface and bonds the substrates to each other with their opposing surfaces. The above-mentioned joining surfaces refer to the surfaces that face each other when joining together substrates having CVD-SiC layers, and include convex and concave portions.

[0009] According to the bonded body of SiC-coated graphite members of the present invention, one end of the combination surface has a convex part higher than the surrounding area, and the CVD-SiC layer bonds the substrates along the outer surface of the bonded body outside the convex part of the combination surface, so that the part sandwiched between the convex parts of the substrates is less likely to have a gap, and the CVD-SiC layer bonds the substrates along the outer surface of the bonded body on the outside, so that a first bonded part of the thin and highly airtight CVD-SiC layer is obtained on one end of the combination surface. Also, on the other end side, when combined with another substrate, the CVD-SiC layer penetrates into the recessed part opening to the outside, and a second bonded part is provided that bonds the opposing surfaces of the substrates, so that the bonded part can be firmly bonded, and a strong bond can be obtained. In other words, according to the joined SiC-coated graphite members of the present invention, despite the thin CVD-SiC layer, by dividing the roles of maintaining airtightness at the first joint on one end and ensuring bonding strength at the second joint on the other end, it is possible to provide a joined SiC-coated graphite member having high bonding strength and airtightness.

[0010] In the joined body of SiC-coated graphite members of the present invention, it is desirable that the above-mentioned combined surfaces have a CVD-SiC layer on the surfaces of the above-mentioned base materials made of both graphite.

[0011] The CVD-SiC layer of the bonded body of SiC-coated graphite members of the present invention is composed of an outer CVD-SiC layer and an inner CVD-SiC layer. Specifically, the surface of each graphite substrate is covered with a coating layer of the inner CVD-SiC layer to form a SiC-coated member, and the outer CVD-SiC layer is obtained by bonding each SiC-coated member. Note that in the areas other than the combined surfaces, the inner CVD-SiC layer and the outer CVD-SiC layer are simply laminated and integrated.

[0012] In the joined body of SiC-coated graphite members, the coating layer of the outer CVD-SiC layer is formed thicker toward the entrance side and thinner toward the inside in the recess having the CVD-SiC layer on the other end side, so that cavities are likely to be formed in the back. Therefore, if the inner CVD-SiC layer is not formed on the surface of the substrates made of both graphite, a portion where the graphite is exposed is likely to be formed. However, in the joined body of SiC-coated graphite members of the present invention, if the inner CVD-SiC layer is formed on the surface of both substrates made of graphite at the above-mentioned combined surface, the coating layer made of the inner CVD-SiC layer is formed around the substrates before combining, so that the portion where the graphite is exposed can be eliminated, and a second joint can be formed by the outer CVD-SiC layer that penetrates into the recess and joins the opposing surfaces of the SiC-coated graphite members.

[0013] In the bonded body of SiC-coated graphite members of the present invention, it is preferable that the CVD-SiC layer on the surface of the top of the protrusion is a polished surface. The surface of the CVD-SiC layer formed on the substrate is rough and hard, and has poor workability. Therefore, unless a polished surface is formed on the inner CVD-SiC layer on the surface of the top of the convex portion, it is difficult to obtain a highly airtight joint even when the CVD-SiC layers formed on the surfaces of the convex portions are pressed together. However, in the joined SiC-coated graphite members of the present invention, if the CVD-SiC layer on the surface of the top of the above-mentioned convex portion is a polished surface, the surface of the CVD-SiC layer becomes flat with high precision, and a highly airtight SiC-coated graphite member can be easily obtained.

[0014] In the joined SiC-coated graphite members of the present invention, it is desirable that the surface of the CVD-SiC layer formed on the top of the convex portion be on the same plane as the surface of the CVD-SiC layer formed on the surface of the other substrate. In the bonded body of SiC-coated graphite members of the present invention, when the surface of the CVD-SiC layer formed on the top of the convex portion is on the same plane as the surface of the CVD-SiC layer formed on the surface of the other substrate, the surfaces of the CVD-SiC layers formed on the convex portions are in a single plane. Therefore, processing after film formation can be handled by simply flattening, and the portion where the convex portion is formed becomes a highly accurate combination surface without gaps by simple processing. Therefore, a SiC-coated graphite member with high airtightness is obtained.

[0015] In the bonded body of SiC-coated graphite members of the present invention, the difference in distance between the ends of the opposing base members on the convex portion side and the ends on the other side at the combined surfaces is desirably 40 to 100 μm. In the joined body of SiC-coated graphite members of the present invention, if the difference in distance between the ends of the opposing base members on the convex side and the ends of the opposing base members on the other side at the joining surfaces is 40 μm or more, a CVD-SiC layer penetrating into the recesses is easily obtained, and a joined body of high strength is obtained. If the difference in distance is 100 μm or less, the recesses are easily filled with a thin CVD-SiC layer, and a joined body of SiC-coated graphite members with high dimensional accuracy can be obtained.

[0016] In the method for producing a joined body of SiC-coated graphite members of the present invention, the ratio of the area of ​​the tops of the protrusions to the area of ​​the joining surfaces is desirably 5 to 60%. In the method for producing a joint of SiC-coated graphite members of the present invention, when the ratio of the area of ​​the top of the protrusion to the area of ​​the mating surfaces is 5% or more, the number of cavities formed is small and stress concentration is unlikely to occur around the protrusion, so that it is possible to make it difficult for distortion to be applied to the CVD-SiC layer on one end side. Also, when the ratio of the area of ​​the top of the protrusion to the area of ​​the mating surfaces is 60% or less, the joining surface can be made large, and a high-strength joint can be obtained. Effect of the Invention

[0017] According to the joined body of SiC-coated graphite members of the present invention, a joined body of SiC-coated graphite members having high bonding strength and airtightness can be provided by dividing the roles of maintaining airtightness at the first bonding part at one end and ensuring bonding strength at the second bonding part at the other end, despite the thin CVD-SiC layer. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1(a) is a perspective view showing an example of a substrate for a bonded body of SiC-coated graphite members, and FIG. 1(b) is a cross-sectional view taken along line AA of the substrate shown in FIG. 1(a). [Diagram 2] FIG. 2 is a cross-sectional view that typically shows a SiC-coated graphite member on which a CVD-SiC layer is formed. [Diagram 3] FIG. 3(a) is a perspective view showing a schematic diagram of a joined body of SiC-coated graphite members of the present invention, FIG. 3(b) is a cross-sectional view taken along line BB of the joined body of SiC-coated graphite members shown in FIG. 3(a), and FIG. 3(c) is a cross-sectional view in which the distinction between the inner CVD-SiC layer and the outer CVD-SiC layer in the cross-sectional view shown in FIG. 3(b) has been eliminated. [Figure 4] FIG. 4 is a cross-sectional view that shows a schematic view of a combination of two SiC-coated graphite members each having an inner CVD-SiC layer formed thereon. [Diagram 5] 5(a) to (d) are cross-sectional views each showing a schematic diagram of each step of a method for producing a joined body of SiC-coated graphite members according to another embodiment of the present invention. [Figure 6] FIG. 6(a) is a perspective view showing a schematic diagram of a joined body of SiC-coated graphite members of the present invention according to another embodiment, and FIG. 6(b) is a cross-sectional view taken along line CC of the joined body of SiC-coated graphite members shown in FIG. 6(a). [Figure 7] FIG. 7(a) is a perspective view showing a schematic diagram of a joined body of SiC-coated graphite members of the present invention according to another embodiment, and FIG. 7(b) is a cross-sectional view taken along line DD of the joined body of SiC-coated graphite members shown in FIG. 7(a). [Figure 8]FIG. 8(a) is a polarizing microscope photograph showing a cross-section of a joined body of SiC-coated graphite members of the present invention, and FIG. 8(b) is a cross-sectional view showing a schematic configuration of the joined body of SiC-coated graphite members shown in FIG. 8(a). [Figure 9] 9(a) to 9(d) are cross-sectional views showing examples of combinations of SiC-coated graphite members other than the combinations of SiC-coated graphite members shown in FIGS. 1 to 7, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, the bonded body of SiC-coated graphite members of the present invention will be described in detail with respect to each embodiment. However, the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope that does not change the gist of the present invention.

[0020] The joined body of SiC-coated graphite members of the present invention is a joined body of SiC-coated graphite members in which a CVD-SiC layer covers a surface of a base material made of graphite, and a plurality of the base materials are joined by the CVD-SiC layer via a mating surface, At least one of the substrates has a convex portion higher than the surrounding area on one end of the combination surface, and a concave portion on the other end that opens to the outside when combined with the other substrate, and the CVD-SiC layer has a first bonding portion that bonds the substrate along the outer surface of the bonded body outside the convex portion of the combination surface, and a second bonding portion that penetrates into the concave portion outside the concave portion of the combination surface and bonds the substrates to each other with their opposing surfaces.

[0021] In the bonded body of SiC-coated graphite members of the present invention, the CVD-SiC layer is composed of an outer CVD-SiC layer and an inner CVD-SiC layer. Specifically, the surface of each graphite substrate is covered with a coating layer of the inner CVD-SiC layer to form a SiC-coated member, and the outer CVD-SiC layer is obtained by bonding each SiC-coated member. Note that in the areas other than the joining surfaces, the inner CVD-SiC layer and the outer CVD-SiC layer are simply laminated and integrated.

[0022] In terms of the assembled surface, the inner CVD-SiC layers are not joined because they are manufactured separately, but are joined by the outer CVD-SiC layer to obtain a joined body. For the sake of explanation below, the CVD-SiC layer may be explained as being divided into an inner CVD-SiC layer and an outer CVD-SiC layer, but the outer CVD-SiC layer is likely to be formed continuously even if it is coated on the inner CVD-SiC layer, and the boundary between them is not necessarily clearly identifiable.

[0023] First, the substrate constituting the bonded body of SiC-coated graphite members will be described. FIG. 1(a) is a perspective view showing an example of a substrate for a bonded body of SiC-coated graphite members, and FIG. 1(b) is a cross-sectional view taken along line AA of the substrate shown in FIG. 1(a).

[0024] The substrate 10 is a substrate constituting a joint of tubular SiC-coated graphite members according to one embodiment of the present invention, and has a groove 15 formed in the center as a through hole, and walls 12 for forming a mating surface on both sides of the groove. The walls 12 on both sides are composed of a protrusion 13 and a recess 14, and the top 13a of the protrusion 13 is flat. The protrusion 13 and the recess 14 are stepped, and the protrusion 13 is formed one step higher than the recess 14.

[0025] The type of graphite constituting the substrate is not particularly limited, but is preferably an isotropic graphite material with low anisotropy. When such an isotropic graphite material with low anisotropy is used as the substrate, the mechanical properties are less likely to be biased depending on the direction, so that the substrate is less likely to break and can be used stably for a long period of time.

[0026] The isotropic graphite material is a graphite material having an isotropic structure and characteristics, and can be produced, for example, by CIP (Cold Isostatic Press). Specifically, for example, the raw powder of the isotropic graphite material is packed into a rubber bag in a pressure vessel, and molded by applying pressure with water or the like, and then sintered and graphitized to produce the isotropic graphite material. In the above-mentioned isotropic graphite material, the average particle size of the raw material powder is, for example, 10 to 50 μm, and the isotropic graphite material is characterized by having a fine structure.

[0027] When the substrate is made of graphite, the porosity is 5 to 20% and the bulk density is 1.70 to 1.90 g / cm 3 It is preferable that the material be: When the porosity of the substrate is 5% or more, the substrate contains open pores, so that the inner CVD-SiC layer can easily penetrate into the open pores, and the inner CVD-SiC layer can be firmly attached to the substrate due to the anchor effect. On the other hand, when the porosity of the substrate is 20% or less, the pore content is not too high, so that the substrate itself has high mechanical strength.

[0028] In addition, the bulk density of the base material is 1.70 g / cm 3 When the bulk density of the substrate is 1.90 g / cm or more, the substrate has excellent mechanical properties even if it has pores. 3 If it is equal to or less, the open pores are contained within an appropriate range, the inner CVD-SiC layer is easily filled into the open pores, and the coating layer made of the inner CVD-SiC layer has excellent adhesion.

[0029] The substrate may be a C / C composite material reinforced by filling gaps between carbon fiber aggregates with a carbon matrix. The type of carbon fiber aggregate is not particularly limited, and may be PAN-based carbon fiber or pitch-based carbon fiber. C / C composites can be obtained, for example, by depositing pyrolytic carbon on a carbon fiber substrate, or by impregnating a carbon fiber substrate with resin and then carbonizing it, etc. Since C / C composites are reinforced with high-strength carbon fibers, they have fracture toughness even at high temperatures and can maintain their mechanical strength.

[0030] The shape of the substrate is not particularly limited, but as described above, at least one of the substrates (hereinafter referred to as the one substrate) has a convex portion that is higher than the surrounding area and a concave portion that is relatively lower than the convex portion on one end side of the mating surface. The top of the convex portion is preferably a flat surface. The concave portion may be a flat surface that is one step lower than the convex portion, and the convex portion and the concave portion may be stepped, or an inclined surface may be formed so as to gradually decrease in height from the convex portion. The combination surface of another substrate to be combined with the substrate may be a simple flat surface, and may have the same shape as the substrate, but the two do not necessarily have to have the same shape.

[0031] In the case of a joined body of SiC-coated graphite members of the present invention, a joined body of SiC-coated graphite members of the present invention is produced using a SiC-coated graphite member having a CVD-SiC layer formed on the surface of the above-mentioned base material.

[0032] 2 is a cross-sectional view showing a SiC-coated graphite member on which a CVD-SiC layer is formed. Since it is difficult to understand the state of the coating in a perspective view of a SiC-coated graphite member, the following description will be based on the cross-sectional view.

[0033] 2, the inner CVD-SiC layer 26 is formed with a substantially uniform thickness over the entire surface including the bottom surface 10a, so that the basic shape is the same as that of the substrate. Therefore, the corresponding parts of the SiC-coated graphite member 20 having the inner CVD-SiC layer will also be referred to as the groove 25, the wall 22, the protrusion 23, and the recess 24.

[0034] That is, in this SiC coated graphite member 20 as well, a groove 25 serving as a through hole is formed in the center, and walls 22 for forming a mating surface are formed on both sides of the groove 25. The wall portions 22 on both sides have a protrusion 23 that is higher than the surrounding area and a recess 24 that is lower than the protrusion 23 on one end side.

[0035] FIG. 3(a) is a perspective view showing a schematic diagram of a joint of SiC-coated graphite members of the present invention using the above-mentioned SiC-coated graphite members, FIG. 3(b) is a cross-sectional view taken along line BB of the joint of SiC-coated graphite members shown in FIG. 3(a), and FIG. 3(c) is a cross-sectional view in which the distinction between the inner CVD-SiC layer and the outer CVD-SiC layer in the cross-sectional view shown in FIG. 3(b) has been eliminated.

[0036] In the SiC-coated graphite member joint 200 of the present invention, as shown in Figures 3(a) and (b), the joint is formed by combining SiC-coated graphite members 20 of the same shape via their joining surfaces and forming a CVD-SiC layer around them.

[0037] The SiC coated graphite member 20 has a convex portion 23 that is higher than the surrounding area on one end side of the combination surface, and a concave portion 24 that opens to the outside on the other end side, and the joined body 200 of the SiC coated graphite members has a first joining portion 28a that joins along the outer surface of the joined body 200 of the SiC coated graphite members in region A outside the convex portion 23 of the combination surface, and has a second joining portion 28b in region B that penetrates into the concave portion 24 of the combination surface from the outside and joins the opposing surfaces of the above-mentioned substrates together. In the drawing, the region where the first bonded portion 28a is formed is shown as region A, and the region where the second bonded portion 28b is formed is shown as region B.

[0038] The first bond 28a and the second bond 28b are formed in the outer CVD-SiC layer 28, but in the manufactured SiC-coated graphite member bond 200, the two CVD-SiC layers are integrated, and it is difficult to identify the boundary between the two CVD-SiC layers. Therefore, the produced joint of SiC-coated graphite members has substrates of the above-mentioned shape embedded inside with their protrusions facing each other, a CVD-SiC layer formed on the surface, a through hole with a rectangular cross-section perpendicular to the length direction, and a tubular body with a constant tube thickness.

[0039] 3(c), in the joined body 200 of SiC-coated graphite members of the present invention, when viewed from the center of the substrates 10 constituting the joined body 200 of SiC-coated graphite members, the substrates 10 have a convex portion 13 higher than the surroundings at one end of the mating surface and a concave portion 14 opening to the outside at the other end, and the CVD-SiC layer 27 has a first bonding portion that bonds along the outer surface of the outer side of the convex portion 13, and a second bonding portion that penetrates into the concave portion of the mating surface from the outside and bonds the opposing surfaces of the substrates to each other. Note that the portion where the top 23a of the convex portion 23 abuts is not bonded even after production because the raw material gas is unlikely to penetrate into the inside.

[0040] Next, a method for producing a bonded body of SiC-coated graphite members according to the present invention will be described. The bonded body of SiC-coated graphite members of the present invention is manufactured through an inner CVD-SiC layer forming step, an assembling step, and a bonding step. Each step will be described below.

[0041] (Inner CVD-SiC layer formation process) In the inner CVD-SiC layer forming step, an inner CVD-SiC layer is formed on the surface of the base material shown in FIG. The method for forming the inner CVD-SiC layer by CVD is not particularly limited, and examples thereof include thermal CVD, plasma organic CVD, photo-CVD, low pressure CVD, metal organic CVD, and CVI (chemical vapor impregnation).

[0042] When the CVI method is used, the graphite substrate is heated to about 800 to 1400°C, and a source gas consisting of an organic silane gas such as methyltrichlorosilane is circulated around the substrate or sprayed onto the substrate to form an inner CVD-SiC layer on the surface or in the open pores of the substrate. The source gas may be diluted with an inert gas such as argon or hydrogen. By setting conditions that facilitate impregnation into the open pores and using the CVI method, the inner CVD-SiC layer can penetrate into the open pores of the substrate, forming a CVD-SiC layer that is difficult to peel off.

[0043] The thickness of the inner CVD-SiC layer to be formed is preferably 20 to 200 μm. The inner CVD-SiC layer does not have to be formed on the entire surface of the substrate made of graphite, but it is preferable that the inner CVD-SiC layer is formed on the entire surface. Through this inner CVD-SiC layer forming step, the SiC-coated graphite member 20 shown in FIG. 2 is manufactured.

[0044] In the present invention, since graphite is used as the substrate, processing can be easily carried out before forming the inner CVD-SiC layer, and a SiC-coated graphite component having a substrate of any shape can be obtained. In the present invention, inner CVD-SiC layers are also formed on a plurality of other substrates to be joined, thereby producing a plurality of SiC-coated graphite members each having an inner CVD-SiC layer formed thereon.

[0045] (Combination process) In the combining step, a plurality of SiC-coated graphite members each having an inner CVD-SiC layer on a combining surface are combined. FIG. 4 is a cross-sectional view that shows a schematic view of a combination of two SiC-coated graphite members each having an inner CVD-SiC layer formed thereon. As shown in Fig. 4, two SiC-coated graphite members 20 are combined so that the tops 23a of the protrusions 23 constituting the combining surface abut against each other. The combining surface refers to both the protrusions 23 and the recesses 24. This is because the recesses 24 form an outer CVD-SiC layer and play an important role in joining the two SiC-coated graphite members.

[0046] In Figure 4, two SiC-coated graphite members 20 (substrates 10) of exactly the same shape and configuration are combined, but the other SiC-coated graphite member may have a different shape as long as it has a surface that can abut against the convex portion of one SiC-coated graphite member and a concave portion that is open to the outside is formed by combining the two. In addition, three or more SiC-coated graphite members, including one SiC-coated graphite member, may be combined, so long as the structure is such that the members are joined by combining multiple SiC-coated graphite members and then forming an outer CVD-SiC layer.

[0047] (Joining process) In the joining process, the assembled multiple SiC-coated graphite members are further covered from the outside with an outer CVD-SiC layer.

[0048] The method for forming the outer CVD-SiC layer is the same as the method for forming the inner CVD-SiC layer, and involves heating the graphite substrate to approximately 800 to 1400°C, and either circulating a raw material gas consisting of an organosilane gas such as methyltrichlorosilane around the SiC-coated graphite member or spraying it onto the SiC-coated graphite member to form an outer CVD-SiC layer on the surface of the SiC-coated graphite member. In this manner, a bonded body 200 of SiC-coated graphite members shown in FIGS. 3(a) and 3(b) is manufactured.

[0049] 5(a) to (d) are cross-sectional views that typically show the steps of producing a joined body of SiC-coated graphite members according to another embodiment of the present invention. In Figure 5(a), two identically shaped SiC-coated graphite members 30 each having an inner CVD-SiC layer 36 are being combined, but the surface of the tops 33a of the convex portions 33 of the inner CVD-SiC layer 36 tends to become rough, and even when the tops 33a are brought into contact with each other, gaps tend to form, making it difficult to maintain airtightness of the combined portion even when an outer CVD-SiC layer is formed.

[0050] Therefore, as shown in Fig. 5(b), the top 33a is polished to form a flat top 330a having a flat surface. Thereafter, as shown in Fig. 5(c), two SiC-coated graphite members 30 are combined so that the flat tops 330a abut against each other, and an outer CVD-SiC layer 38 is formed as shown in Fig. 5(d). By forming the outer CVD-SiC layer 38 in this manner, a joint 300 of SiC-coated graphite members can be formed.

[0051] In this embodiment, the outer CVD-SiC layer 38 is not formed over the entire inside of the recess 34, but is formed only at the entrance of the recess 34, and a cavity 39 is formed inside. However, a first bonding portion 38a is formed in region A, and a second bonding portion 38b is formed in region B, penetrating into recess 34 and bonding the two SiC-coated graphite members, resulting in a bonded body 300 of SiC-coated graphite members in which the two SiC-coated graphite members are firmly bonded together.

[0052] The manufactured bonded body of SiC-coated graphite members has a CVD-SiC layer of a predetermined thickness formed on the surface of the base material having a convex portion and a concave portion, and the CVD-SiC layer has a first bonding portion that bonds the base material along the outer surface of the bonded body outside the convex portion of the combined surface, and a second bonding portion that penetrates into the concave portion outside the concave portion of the combined surface and bonds the opposing surfaces of the base material to each other, and is a bonded body of SiC-coated graphite members with a cavity formed inside. Note that the flattened top portion 330a is not bonded even after it is manufactured because it is difficult for the raw material gas to penetrate into the inside.

[0053] FIG. 6(a) is a perspective view showing a schematic diagram of a joined body of SiC-coated graphite members of the present invention according to another embodiment, and FIG. 6(b) is a cross-sectional view taken along line CC of the joined body of SiC-coated graphite members shown in FIG. 6(a).

[0054] In the SiC-coated graphite member joint 400 of this embodiment, the SiC-coated graphite member 40 having the substrate 41 and the inner CVD-SiC layer 46 is cylindrical in shape, with the convex portion 43 forming one end being formed on the central axis side and the concave portion 44 forming the other end being formed on the outer periphery side. The top of the projection 43 is polished to remove any protrusions that may have formed on the surface of the CVD-SiC layer, and to provide a flat surface.

[0055] In this SiC-coated graphite member joint 400, as shown in FIG. 6(b), two SiC-coated graphite members 40 are combined so that the tops of the convex portions 43 abut against each other, and an outer CVD-SiC layer 48 is formed on the inside and outer peripheral portions of the cylinder. In this embodiment, the outer CVD-SiC layer 48 is not formed over the entire inside of the recess 44, but is formed only at the entrance of the recess 44, and a cavity 49 is formed inside. However, a first bonding portion 48a is formed in region A, and a second bonding portion 48b is formed in region B, penetrating into recess 44 and bonding the two SiC-coated graphite members, resulting in a bonded body 400 of SiC-coated graphite members in which two SiC-coated graphite members 40 are firmly bonded together.

[0056] FIG. 7(a) is a perspective view showing a schematic diagram of a joined body of SiC-coated graphite members of the present invention according to another embodiment, and FIG. 7(b) is a cross-sectional view taken along line DD of the joined body of SiC-coated graphite members shown in FIG. 7(a).

[0057] In the SiC-coated graphite member joint 500 of this embodiment, a pipe-shaped SiC-coated graphite member 50 having a tapered lower portion is combined with a flange-shaped SiC-coated graphite member 60 having an inclined surface formed so as to approximately fit into the tapered portion of the SiC-coated graphite member 50, and the two are joined together by forming an outer CVD-SiC layer.

[0058] A convex portion 53 that serves as one end is formed on the central axis side of the tapered portion of the pipe-shaped SiC-coated graphite member 50, and a concave portion 54 that serves as the other end is formed on the outer periphery side. Also, on the inclined surface of the flange-shaped SiC-coated graphite member 60, a convex portion 63 which becomes one end is formed on the central axis side, and a concave portion 64 which becomes the other end is formed on the outer periphery side. These tops are flattened by a method such as co-milling.

[0059] The SiC-coated graphite member 50 and the SiC-coated graphite member 60 of this configuration are combined so that the convex portions 53 and 63 abut against each other, an outer CVD-SiC layer 58 is formed on the outside of the convex portions 53 and 63 and over the entire inside of the concave portions 54 and 64, and the SiC-coated graphite member 50 and the SiC-coated graphite member 60 are joined to form a joined body 500 of SiC-coated graphite members.

[0060] FIG. 8(a) is a polarizing microscope photograph showing a cross-section of a joined body of SiC-coated graphite members of the present invention, and FIG. 8(b) is a cross-sectional view showing a schematic configuration of the joined body of SiC-coated graphite members shown in FIG. 8(a). According to FIG. 8(b), SiC-coated graphite members 70 each having an inner CVD-SiC layer 76 formed on the surface of a base material 71 are combined at their mating surfaces, and an outer CVD-SiC layer 78 is formed in a recess 74, with the two SiC-coated graphite members 70 being joined by this outer CVD-SiC layer 78. When forming the outer CVD-SiC layer 78 on the SiC-coated graphite member 70, the source gas is supplied to the recess 74 from the right side (outside) of the drawing, but since the concentration of the source gas usually decreases the deeper into the recess 74, depending on the source gas conditions, after the second bonding portion 78b is formed in the surface layer, no bonding portion is formed in the recess 74, and a cavity may result. However, the second bonding portion 78b and the first bonding portion, not shown in the photograph, are formed on the convex side, resulting in a bonded body of SiC-coated graphite members with high bonding strength and airtightness.

[0061] 9(a) to (d) are cross-sectional views showing examples of combinations of SiC-coated graphite members other than those shown in FIGS. 1 to 7 when producing a joined body of SiC-coated graphite members. 9(a) to (d), d1 indicates the distance between the substrates at the convex portions when the SiC-coated graphite members are assembled, and d2 indicates the longest distance between the substrates at the concave portions. A short d1 means that the thickness of the sandwiched inner CVD-SiC layer is thin. In addition, (d2-d1) is the difference in distance between the ends on the convex portion side and the ends on the other end side (concave portion side) on the assembled surface.

[0062] Figure 9(a) shows an example of a combination in which substrates 81 (SiC-coated graphite members 80) of the same shape, on which convex portions and concave portions are formed, are combined. In this example of combination, the distance d2 is large and a concave portion with a large capacity is formed, making it easy to form an outer CVD-SiC layer inside the concave portion.

[0063] 9(b) shows an example of a combination of a substrate 81 (SiC-coated graphite member 80) having convex and concave portions formed thereon and a substrate 91 (SiC-coated graphite member 90) having a flat mating surface, in which the distance d2 is about half that of the combination example shown in FIG. 9(a), and the outer CVD-SiC layer that closes the concave portions is easy to form, but the second outer CVD-SiC layer is easy to form only at the entrance of the concave portions. In addition, the substrate 91 having a flat mating surface is easy to process because of its simple shape.

[0064] 9(c) is an example of a combination of a substrate 81 (SiC-coated graphite member 80) having a convex portion and a substrate 101 (SiC-coated graphite member 100) having a slightly different shape but also having a convex portion. However, the convex portion of one SiC-coated graphite member is combined with a lower surface of the other SiC-coated graphite member on which no convex portion is formed, and the volume of the concave portion is small and the distance d2 between the two members is shorter. Therefore, when the outer CVD-SiC layer is formed, a second joint can be easily formed in the concave portion, but a cavity is likely to be formed. In addition, in this combination example, since the shapes are fitted together, misalignment of the setting is unlikely to occur when the outer CVD-SiC layer is formed, and handling during manufacturing is easy.

[0065] Figure 9(d) shows an example of a combination of a substrate 111 (SiC-coated graphite member 110) having an inclined surface in which the recess becomes gradually lower from the top of the protrusion, and a substrate 91 (SiC-coated graphite member 90) having a flat mating surface. Since the cross-sectional area of ​​the recess becomes gradually smaller, the raw material gas can easily penetrate deep into the recess, and an outer CVD-SiC layer can easily be formed over the entire recess.

[0066] As shown in Figs. 9(a) to (d), two SiC-coated graphite members are combined and an outer CVD-SiC layer is formed to obtain a joint of SiC-coated graphite members of the present invention. [Explanation of symbols]

[0067] 10, 31, 41, 51, 61, 71, 81, 91, 101, 111 Base material 10a Bottom 12, 22 Wall section 13, 23, 33, 43, 53, 63 Convex 13a, 23a, 33a top 14, 24, 34, 44, 54, 64, 74 recess 15, 25 Groove 20, 30, 40, 50, 60, 70 SiC coated graphite components 80, 90, 100, 110 SiC coated graphite components 27 CVD-SiC layer 26, 36, 46, 56, 76 Inner CVD-SiC layer 28, 38, 48, 58, 78 Outer CVD-SiC layer 28a, 38a, 48a, 58a First joint 28b, 38b, 48b, 58b, 78b Second joint 39, 49 hollow 200, 300, 400, 500, 700 SiC-coated graphite member joint 330a flattened top

Claims

1. A joint of SiC-coated graphite members, in which a CVD-SiC layer covers a surface of a substrate made of graphite, and a plurality of the substrates are joined by the CVD-SiC layer via a combination surface, The combination surface of the at least one base material has a convex portion on one end side of the combination surface that is higher than the surrounding area, and a concave portion on the other end side that opens to the outside of the combination surface when combined with another base material, The CVD-SiC layer is a first bonding portion that bonds the base material along an outer surface of the bonded body outside the convex portion of the mating surface; a second joining portion that penetrates the recess of the mating surface outside the recess and joins the opposing surfaces of the substrates; A joined body of SiC-coated graphite members, characterized in that the tops of the protrusions are on the same plane, and the ratio of the area of ​​the tops of the protrusions to the area of ​​the joining surfaces is 5 to 60%.

2. 2. The joined body of SiC-coated graphite members according to claim 1, characterized in that, at the joining surface, a CVD-SiC layer is provided on the surface of each of the substrates made of graphite.

3. 3. The joined body of SiC-coated graphite members according to claim 2, wherein the CVD-SiC layer formed on the top of the protrusion has a polished surface.

4. The joined body of SiC-coated graphite members as described in claim 3, characterized in that the surface of the CVD-SiC layer formed on the top of the convex portion is on the same plane as the surface of the CVD-SiC layer formed on the surface of the other substrate.

Citation Information

Patent Citations

  • Manufacture of tubular member

    JP1987128974A

  • Member for semiconductor diffusion furnace

    JP1987200722A

  • SiC COATED CARBON MEMBER, AND MANUFACTURING METHOD THEREOF

    JP2010070797A

  • Carbon component and method of manufacturing the same

    JP2011225949A

  • Production method of silicon carbide member

    JP2019055897A