Method for manufacturing a joint of SiC-coated graphite members
The method for manufacturing SiC-coated graphite members addresses the challenge of achieving high bonding strength and airtightness by using a dual CVD-SiC layer strategy, ensuring both properties are maintained through strategic joint formation.
Patent Information
- Application Number
- JP2020046661
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-03-17
AI Technical Summary
Existing methods for manufacturing SiC-coated graphite materials face challenges in achieving high bonding strength, dimensional accuracy, and airtightness simultaneously due to the thickness requirements of the CVD-SiC layer, which can compromise one or more of these properties.
A method involving a first CVD-SiC layer on the surface of graphite members, with a second CVD-SiC layer forming convex and concave portions to ensure bonding strength and airtightness, where the second layer penetrates into recesses and forms joints on the outer surface, distributing the roles of maintaining airtightness and bonding strength differently across the bonded body.
The method achieves a bonded body of SiC-coated graphite members with high bonding strength and airtightness, despite using a thin CVD-SiC layer, by strategically forming joints to maintain both properties effectively.
Smart Images

Figure 0007580926000001 
Figure 0007580926000002 
Figure 0007580926000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a joined body of SiC-coated graphite members in which a composite material having a CVD-SiC layer on the surface of a graphite substrate is combined. [Background technology]
[0002] In order to supply high-quality products in semiconductor manufacturing, thereby improving the yield of semiconductor products and ensuring stable operation, composite materials in which a CVD-SiC layer is coated on the surface of a graphite base material are widely used for semiconductor device parts such as susceptors, jigs, furnace components, etc., used in the heat treatment process of silicon wafers, etc. Materials such as graphite and SiC do not dope silicon even when mixed with silicon, and do not change the electrical conductivity, so they have little effect on the quality of the obtained wafers, and both SiC and graphite are stable at high temperatures and wear little.
[0003] Graphite is easy to process and can easily be made into complex shapes, but it has the disadvantage of being easily worn away by contact with oxygen, water, hydrogen, etc. On the other hand, SiC is characterized by being easy to form a thin oxide film on its surface and being resistant to wear from oxygen, water, hydrogen, etc., but it has the disadvantage of being hard and difficult to process. A composite material in which a CVD-SiC layer is formed on the surface of a graphite substrate makes good use of these characteristics and disadvantages. With such a composite material, the substrate itself is very easy to process, so complex shapes can be easily obtained, and the surface is covered with a CVD-SiC layer, making it a durable composite material that can be used in a variety of atmospheres.
[0004] Patent Document 1 describes a component for semiconductor manufacturing equipment, which is a tube for a semiconductor diffusion furnace having a shape in which one end side of a long cylindrical portion is tapered, and which is characterized in that a tapered portion made of silicon carbide or graphite is joined to one end of a long cylinder made of silicon carbide or graphite by a silicon carbide CVD film, and at least the entire inner circumferential surface of the tube is coated with a CVD film. It is described that such semiconductor manufacturing equipment parts are covered with a high-purity, dense SiC coating, and that the gaps between the parts where they fit together are filled with CVD precipitates and are bonded together, eliminating any rattling of the parts. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 62-200722 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the above-mentioned invention, the gap is filled with a CVD-SiC layer, so in order to create a sufficient gap in advance and completely fill the gap, a CVD-SiC layer of sufficient thickness is required. However, there is a problem that the dimensional accuracy deteriorates when the CVD-SiC layer is made thick. On the other hand, when a thin CVD-SiC layer is used, the gaps cannot be filled sufficiently, resulting in a trade-off that reduces airtightness. This poses the challenge of making a bonded body of SiC-coated graphite material that simultaneously satisfies the bonding strength, dimensional accuracy, and airtightness requirements.
[0007] In view of the above problems, the present invention has an object to provide a method for producing a joined body of SiC-coated graphite materials having high joining strength, excellent dimensional accuracy, and high airtightness. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention provides a method for producing a joined body of SiC-coated graphite members, the CVD-SiC layer comprising a first CVD-SiC layer covering a surface of a substrate made of graphite, and a second CVD-SiC layer joining a plurality of the substrates, the method comprising the steps of: The above-mentioned joined body includes a combining step of combining a plurality of SiC-coated graphite members each having a first CVD-SiC layer on a combining surface, and a joining step of further covering the combined plurality of SiC-coated graphite members with a second CVD-SiC layer from the outside, wherein at least one of the SiC-coated graphite members has a convex portion higher than the surrounding area on one end side of the combining surface, and a concave portion on the other end side that opens to the outside when combined with another SiC-coated graphite member, and the second CVD-SiC layer has a first joining portion that joins the plurality of SiC-coated graphite members along the outer surface of the joined body outside the convex portion of the combining surface, and a second joining portion that penetrates into the concave portion of the combining surface from the outside and joins opposing surfaces of the SiC-coated graphite members. The above-mentioned joining surfaces include the surfaces where the SiC-coated graphite members come into contact when they are joined together, and refer to the surfaces where the two members face each other, and include convex portions and concave portions.
[0009] According to the manufacturing method of the joined body of SiC-coated graphite members of the present invention, at least one of the SiC-coated graphite members has a convex part higher than the surroundings on one end side of the joining surface, and has a joining part (second CVD-SiC layer) that joins the multiple SiC-coated graphite members along the outer surface of the joined body outside the convex part of the joining surface. Therefore, gaps are unlikely to form in the part where the convex parts of the joining surfaces contact, and the second CVD-SiC layer joins the above-mentioned base materials along the outer surface of the joined body on the outside, so that a thin, highly airtight CVD-SiC layer is obtained on one end side of the joining surfaces. In addition, the other end has a second joining portion (second CVD-SiC layer) that penetrates into the recess from the outside of the recess that opens to the outside and joins the opposing surfaces of the SiC-coated graphite members together by combining it with another SiC-coated member, thereby allowing for a firm bond at the joining portion and resulting in a strong bond.
[0010] In other words, according to the manufacturing method of the present invention for manufacturing a joint of SiC-coated graphite members, a second CVD-SiC layer, which is a thin CVD-SiC layer but has the role of maintaining airtightness at one end and ensuring bonding strength at the other end, can be formed on a combination of SiC-coated graphite members having a first CVD-SiC layer, and a joint of SiC-coated graphite members having high bonding strength and airtightness can be obtained.
[0011] In the method for producing a joined body of SiC-coated graphite members of the present invention, it is preferable that a first CVD-SiC layer be provided on the surfaces of both of the substrates made of graphite at the joining surfaces.
[0012] In the obtained bonded body of SiC-coated graphite members, the coating layer of the second CVD-SiC layer is formed thicker toward the inlet side and thinner toward the inside in the recess formed in the SiC-coated graphite member on the other end side. Therefore, if the first CVD-SiC layer is not formed on the surface of both graphite-made substrates, a portion where the graphite is exposed is likely to be formed. However, in the manufacturing method of the bonded body of SiC-coated graphite members of the present invention, if the first CVD-SiC layer is formed on the surface of both graphite-made substrates at the above-mentioned combined surface, the coating layer made of the first CVD-SiC layer is formed around the substrates before combining them, so that the portion where the graphite is exposed can be eliminated, and a second bonding portion (second CVD-SiC layer) that penetrates into the recess and bonds the opposing surfaces of the SiC-coated graphite members can be formed.
[0013] In the method for producing a bonded body of SiC-coated graphite members of the present invention, it is preferable that the first CVD-SiC layer on the surface of the top of the protrusion is a polished surface. When a CVD-SiC layer is formed on a substrate, the surface is rough and difficult to process. Therefore, unless a polished surface is formed on the CVD-SiC layer on the surface of the top of the convex portion, it is difficult to obtain a highly airtight joint even when the convex portion is pressed against another mating surface. However, in the method for manufacturing a joint of SiC-coated graphite members of the present invention, if the first CVD-SiC layer on the surface of the top of the convex portion is a polished surface, a highly accurate, flat top can be easily obtained, and the top of the convex portion can easily adhere to other SiC-coated graphite members with which it comes into contact, making it easy to obtain a highly airtight SiC-coated graphite member.
[0014] In the method for producing a joined body of SiC-coated graphite members of the present invention, it is preferable that the tops of the protrusions are on the same plane. In the method for manufacturing a joint of SiC-coated graphite members of the present invention, when the tops of the protrusions are on the same plane, the tops of the mating surface become one plane. Therefore, processing after film formation can be handled by simply flattening, and the part where the protrusions are formed becomes a highly accurate mating surface without gaps through simple processing. Therefore, a SiC-coated graphite member with high airtightness can be obtained.
[0015] In the method for manufacturing a joined body of SiC-coated graphite members of the present invention, the difference in distance between the ends of the opposing base members on the convex portion side and the ends on the other side at the joining surfaces is desirably 40 to 100 μm. In the method for manufacturing a joint of SiC-coated graphite members of the present invention, when the difference in distance between the ends of the base members on the convex side and the ends of the base members on the other side at the joining surfaces is 40 μm or more, a CVD-SiC layer penetrating into the recesses is easily obtained, and a joint of high strength is obtained. When the difference in distance is 100 μm or less, the recesses are easily filled with a thin CVD-SiC layer, and a joint of SiC-coated graphite members with high dimensional accuracy is obtained.
[0016] In the method for producing a joined body of SiC-coated graphite members of the present invention, the ratio of the area of the tops of the protrusions to the area of the joining surfaces is desirably 5 to 60%. In the method for producing a joint of SiC-coated graphite members of the present invention, when the ratio of the area of the top of the protrusion to the area of the mating surfaces is 5% or more, the number of cavities formed is small and stress concentration is unlikely to occur around the protrusion, so that it is possible to make it difficult for distortion to be applied to the CVD-SiC layer on one end side. Also, when the ratio of the area of the top of the protrusion to the area of the mating surfaces is 60% or less, the joining surface can be made large, and a high-strength joint can be obtained. Effect of the Invention
[0017] According to the manufacturing method of the present invention for manufacturing a joint of SiC-coated graphite members, a second CVD-SiC layer, which is a thin CVD-SiC layer that maintains airtightness at one end and ensures bonding strength at the other end, can be formed on a combination of SiC-coated graphite members having a first CVD-SiC layer, and a joint of SiC-coated graphite members having high bonding strength and airtightness can be obtained. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1(a) is a perspective view showing an example of a substrate for producing a bonded body of SiC-coated graphite members, and FIG. 1(b) is a cross-sectional view taken along line AA of the substrate shown in FIG. 1(a). [Diagram 2] FIG. 2 is a cross-sectional view that typically shows a SiC-coated graphite member on which a first CVD-SiC layer is formed. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates a combination of two SiC-coated graphite members each having a first CVD-SiC layer formed thereon. [Figure 4] FIG. 4(a) is a perspective view showing a schematic diagram of a joined body of SiC-coated graphite members having a second CVD-SiC layer formed thereon, and FIG. 4(b) is a cross-sectional view along line BB of the joined body of SiC-coated graphite members shown in FIG. 4(a). [Diagram 5] 5(a) to (d) are cross-sectional views each showing a schematic diagram of each step of a method for producing a joined body of SiC-coated graphite members according to another embodiment of the present invention. [Figure 6]FIG. 6(a) is a perspective view showing a schematic diagram of a joined body of SiC-coated graphite members of the present invention according to another embodiment, and FIG. 6(b) is a cross-sectional view taken along line CC of the joined body of SiC-coated graphite members shown in FIG. 6(a). [Figure 7] FIG. 7(a) is a perspective view showing a schematic diagram of a joined body of SiC-coated graphite members of the present invention according to another embodiment, and FIG. 7(b) is a cross-sectional view taken along line DD of the joined body of SiC-coated graphite members shown in FIG. 7(a). [Figure 8] FIG. 8(a) is a polarizing microscope photograph showing a cross-section of a joined body of SiC-coated graphite members of the present invention, and FIG. 8(b) is a cross-sectional view showing a schematic configuration of the joined body of SiC-coated graphite members shown in FIG. 8(a). [Figure 9] 9(a) to 9(d) are cross-sectional views showing examples of combinations of SiC-coated graphite members other than the combinations of SiC-coated graphite members shown in FIGS. 1 to 7, respectively. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, the manufacturing method of a joined body of SiC-coated graphite members of the present invention will be described in detail with respect to each embodiment. However, the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope that does not change the gist of the present invention.
[0020] The method for producing a joined body of SiC-coated graphite members of the present invention is a method for producing a joined body of SiC-coated graphite members, the CVD-SiC layer comprising a first CVD-SiC layer covering a surface of a substrate made of graphite, and a second CVD-SiC layer joining a plurality of the substrates, The method includes a combining step of combining a plurality of SiC-coated graphite members each having a first CVD-SiC layer on a combining surface, and a joining step of covering the combined plurality of SiC-coated graphite members with a second CVD-SiC layer from the outside, wherein at least one of the SiC-coated graphite members has a convex portion higher than the surrounding area on one end side of the combining surface, and a concave portion on the other end side that opens to the outside when combined with another SiC-coated graphite member, and the second CVD-SiC layer has a first joining portion that joins the plurality of SiC-coated graphite members along the outer surface of the joined body outside the convex portion of the combining surface, and a second joining portion that penetrates into the concave portion of the combining surface from the outside and joins opposing surfaces of the SiC-coated graphite members.
[0021] The method for manufacturing a joint of SiC-coated graphite members of the present invention includes an assembling step of assembling multiple SiC-coated graphite members having a first CVD-SiC layer on their joining surfaces, and a joining step of further covering the assembled multiple SiC-coated graphite members from the outside with a second CVD-SiC layer.
[0022] In the method for producing a joined body of SiC-coated graphite members of the present invention, a first CVD-SiC layer forming step is first carried out before the assembling step, in which a first CVD-SiC layer is formed so as to cover the surface of the graphite member, which is the base material.
[0023] The type of graphite constituting the substrate is not particularly limited, but is preferably an isotropic graphite material with low anisotropy. When such an isotropic graphite material with low anisotropy is used as the substrate, the mechanical properties are less biased depending on the direction, so that the substrate is less likely to break and can be used stably for a long period of time.
[0024] The isotropic graphite material is a graphite material having an isotropic structure and characteristics, and can be produced, for example, by CIP (Cold Isostatic Press). Specifically, for example, the raw powder of the isotropic graphite material is packed into a rubber bag in a pressure vessel, and molded by applying pressure with water or the like, and then sintered and graphitized to produce the isotropic graphite material. In the above-mentioned isotropic graphite material, the average particle size of the raw material powder is, for example, 10 to 50 μm, and the isotropic graphite material is characterized by having a fine structure.
[0025] When the substrate is made of graphite, the porosity is 5 to 20% and the bulk density is 1.70 to 1.90 g / cm 3 It is preferable that the material is When the porosity of the substrate is 5% or more, the substrate contains open pores, so that the first CVD-SiC layer is easily impregnated into the open pores, and the first CVD-SiC layer is firmly attached to the substrate due to the anchor effect. On the other hand, when the porosity of the substrate is 20% or less, the pore content is not too high, so that the substrate itself has high mechanical strength.
[0026] In addition, the bulk density of the base material is 1.70 g / cm 3 When the bulk density of the substrate is 1.90 g / cm or more, the substrate has excellent mechanical properties even if it has pores. 3 If it is equal to or less, the open pores are contained within an appropriate range, the first CVD-SiC layer is easily filled into the open pores, and the coating layer made of the first CVD-SiC layer has excellent adhesion.
[0027] The substrate may be a C / C composite material reinforced by filling gaps between carbon fiber aggregates with a carbon matrix. The type of carbon fiber aggregate is not particularly limited, and may be PAN-based carbon fiber or pitch-based carbon fiber. C / C composites can be obtained, for example, by depositing pyrolytic carbon on a carbon fiber substrate, or by impregnating a carbon fiber substrate with resin and then carbonizing it, etc. Since C / C composites are reinforced with high-strength carbon fibers, they have fracture toughness even at high temperatures and can maintain their mechanical strength.
[0028] In the manufacturing method of the bonded body of SiC-coated graphite members of the present invention, the first CVD-SiC layer is formed on the surface of the substrate with a substantially uniform thickness, but the basic shape of the SiC-coated graphite member on which the first CVD-SiC layer is formed is the same as that of the substrate. Therefore, the parts of the substrate that correspond to the SiC-coated graphite member (protrusions, recesses, etc.) are given the same names as the members that constitute the SiC-coated graphite member.
[0029] The shape of the substrate is not particularly limited, but at least one of the substrates (hereinafter referred to as the first substrate) has a convex portion higher than the surrounding area and a concave portion relatively lower than the convex portion on one end side of the mating surface. The top of the convex portion is preferably a flat surface. The concave portion may be a flat surface that is one step lower than the convex portion, and the convex portion and the concave portion may be stepped, or an inclined surface may be formed so as to gradually decrease in height from the convex portion. The combination surface of another substrate to be combined with the substrate may be a simple flat surface, and may have the same shape as the substrate, but the two do not necessarily have to have the same shape.
[0030] In the following, the manufacturing method of the joined body of SiC-coated graphite members of the present invention will be explained using the substrates shown in Figures 1(a) and (b) as an example, but later, the manufacturing method of the joined body of SiC-coated graphite members of other substrates (SiC-coated graphite members) will also be explained as an example.
[0031] FIG. 1(a) is a perspective view showing an example of a substrate for producing a bonded body of SiC-coated graphite members, and FIG. 1(b) is a cross-sectional view taken along line AA of the substrate shown in FIG. 1(a). The substrate 10 is a substrate for manufacturing a joint of tubular SiC-coated graphite members having a through hole for passing a fluid therethrough, and has a groove 15 formed in the center as a through hole, and walls 12 for forming a mating surface formed on both sides of the groove. The walls 12 on both sides are composed of a protrusion 13 and a recess 14, and the top 13a of the protrusion 13 is flat. The protrusion 13 and the recess 14 are stepped, and the protrusion 13 is formed one step higher than the recess 14. In the manufacturing method of a joined body of SiC-coated graphite members described below, since it is difficult to see the state of the coating from a perspective view, the method will be described based only on the above-mentioned AA line cross-sectional view.
[0032] (First CVD-SiC layer formation process) A first CVD-SiC layer is formed on the surface of the substrate having the above-mentioned shape. The method for forming the first CVD-SiC layer by CVD is not particularly limited, and examples thereof include thermal CVD, plasma organic CVD, photo-CVD, low pressure CVD, metal organic CVD, and CVI (chemical vapor impregnation).
[0033] When the CVI method is used, the graphite substrate is heated to about 800 to 1400°C, and a source gas consisting of an organic silane gas such as methyltrichlorosilane is circulated around the substrate or sprayed onto the substrate to form a first CVD-SiC layer on the surface or in the open pores of the substrate. The source gas may be diluted with an inert gas such as argon or hydrogen. By setting conditions that facilitate impregnation into the open pores and using the CVI method, the first CVD-SiC layer can penetrate into the open pores of the substrate, forming a CVD-SiC layer that is not easily peeled off.
[0034] The thickness of the first CVD-SiC layer to be formed is preferably 20 to 100 μm. The first CVD-SiC layer may be formed on the entire surface of a substrate made of graphite, or may be formed on the other surfaces except for the bottom surface 10a that is in contact with the support by being placed on the support of a CVD apparatus.
[0035] FIG. 2 is a cross-sectional view that typically shows a SiC-coated graphite member on which a first CVD-SiC layer is formed. 2, a first CVD-SiC layer 26 is formed with a substantially uniform thickness over the entire surface including the bottom surface 10a of the substrate 10. That is, this SiC-coated graphite member 20 also has a groove 25 serving as a through hole in the center, and walls 22 for forming a combination surface are formed on both sides of the groove 25. The walls 22 on both sides have a protrusion 23 higher than the surrounding area on one end side, and a recess 24 on the other end side that is combined with another SiC-coated graphite member and opens to the outside.
[0036] In the present invention, since graphite is used as the substrate, processing can be easily carried out before forming the first CVD-SiC layer, and a SiC-coated graphite component having a substrate of any shape can be obtained. In the present invention, a first CVD-SiC layer is also formed on a plurality of other substrates to be joined, thereby producing a plurality of SiC-coated graphite members each having a first CVD-SiC layer formed thereon.
[0037] (Combination process) In the combining step, a plurality of SiC-coated graphite members having a first CVD-SiC layer on a combining surface are combined. FIG. 3 is a cross-sectional view that illustrates a state in which two SiC-coated graphite members, each having a first CVD-SiC layer formed on the surface of a base material, are combined together. 3, two SiC-coated graphite members 20 are combined such that the tops 23a of the protrusions 23 constituting the combining surface abut against each other. The combining surface refers to both the protrusions 23 and the recesses 24. The protrusions 23 and the recesses 24 form a second CVD-SiC layer and play an important role in joining the two SiC-coated graphite members.
[0038] In Figure 3, two SiC-coated graphite members 20 (substrates 10) of exactly the same shape and configuration are combined, but as mentioned above, the other SiC-coated graphite member may have a surface that can abut against the convex portion of one SiC-coated graphite member, and the shapes may be different as long as the combination of the two members forms a concave portion that is open to the outside. In addition, three or more SiC-coated graphite members, including one SiC-coated graphite member, may be combined, so long as the structure is such that the members are joined by combining multiple SiC-coated graphite members and then forming a second CVD-SiC layer.
[0039] (Joining process) In the bonding process, the periphery of the assembled multiple SiC-coated graphite members is covered with a second CVD-SiC layer.
[0040] Figure 4(a) is a perspective view showing a schematic diagram of a joint of SiC-coated graphite members having a second CVD-SiC layer formed on the surface of a base material, and Figure 4(b) is a cross-sectional view along line BB of the joint of SiC-coated graphite members shown in Figure 4(a).
[0041] As shown in Figures 4(a) and (b), in the joined body 200 of SiC-coated graphite members, two SiC-coated graphite members 20 each having a first CVD-SiC layer 26 are combined, and the entire portions of the combined two SiC-coated graphite members 20, including the outer surfaces and internal recesses, are covered with a second CVD-SiC layer 28 to form the joined body 200 of SiC-coated graphite members.
[0042] That is, in this joined body 200 of SiC-coated graphite members, the second CVD-SiC layer 28 has a first joining portion 28a that joins the two SiC-coated graphite members 20 outside the convex portion 23 of the combining surface along the outer surface of the joined body, and has a second joining portion 28b that penetrates into the concave portion 24 of the combining surface from outside and joins the opposing surfaces of the SiC-coated graphite members to each other. Therefore, a joined body of SiC-coated graphite members having high joining strength and airtightness can be obtained. In the drawing, the region where the first bonded portion 28a is formed is shown as region A, and the region where the second bonded portion 28b is formed is shown as region B.
[0043] The method for forming the second CVD-SiC layer is the same as the method for forming the first CVD-SiC layer, and involves heating the graphite substrate to approximately 800 to 1400°C, and either circulating a raw material gas consisting of an organosilane gas such as methyltrichlorosilane around the SiC-coated graphite member or spraying it onto the SiC-coated graphite member to form a second CVD-SiC layer on the surface of the SiC-coated graphite member. The thickness of the second CVD-SiC layer to be formed is preferably 20 to 100 μm.
[0044] 5(a) to (d) are cross-sectional views each showing a schematic diagram of each step of a method for producing a joined body of SiC-coated graphite members according to another embodiment of the present invention. In Figure 5(a), it is intended to combine two identically shaped SiC-coated graphite members 30 each having a first CVD-SiC layer 36 formed thereon; however, the surface of the tops 33a of the convex portions 33 of the first CVD-SiC layer 36 tends to become rough, and even when the tops 33a are brought into contact with each other, gaps tend to form, making it difficult to maintain airtightness of the combined portion even when a second CVD-SiC layer is formed.
[0045] Therefore, as shown in Fig. 5(b), the top 33a is polished to form a flat top 330a having a flat surface. Thereafter, as shown in Fig. 5(c), two SiC-coated graphite members 30 are combined so that the flat tops 330a abut against each other, and a second CVD-SiC layer 38 is formed as shown in Fig. 5(d). By forming the second CVD-SiC layer 38 in this manner, a joint 300 of SiC-coated graphite members can be formed.
[0046] In this embodiment, the second CVD-SiC layer 38 is not formed throughout the entire inside of the recess 34, but is formed only at the entrance of the recess 34, and a cavity 39 is formed inside. However, a first bonding portion 38a is formed in region A outside convex portion 33, and a second bonding portion 38b is formed in region B, penetrating into concave portion 34 and bonding the two SiC-coated graphite members together, resulting in a bonded body 300 of SiC-coated graphite members in which the two SiC-coated graphite members are firmly bonded together, which also has excellent airtightness.
[0047] FIG. 6(a) is a perspective view showing a schematic diagram of a joined body of SiC-coated graphite members of the present invention according to another embodiment, and FIG. 6(b) is a cross-sectional view taken along line CC of the joined body of SiC-coated graphite members shown in FIG. 6(a).
[0048] In the SiC-coated graphite member joint 400 of this embodiment, the SiC-coated graphite member 40 having the substrate 41 and the first CVD-SiC layer 46 is cylindrical in shape, with the convex portion 43 forming one end being formed on the central axis side and the concave portion 44 forming the other end being formed on the outer periphery side. The top of the projection 43 is polished to remove any protrusions that may have formed on the surface of the CVD-SiC layer, and to provide a flat surface.
[0049] In this SiC-coated graphite member joint 400, as shown in FIG. 6(b), two SiC-coated graphite members 40 are combined so that their flattened tops abut against each other, and a second CVD-SiC layer 48 is formed on the inside and outer periphery of the cylinder. In this embodiment, the second CVD-SiC layer 48 is not formed throughout the entire inside of the recess 44, but is formed only at the entrance of the recess 44, and a cavity 49 is formed inside. However, a first bonding portion 48a is formed in region A outside the convex portion 43, and a second bonding portion 48b is formed in region B, penetrating into the concave portion 44 and bonding the two SiC-coated graphite members together, resulting in a bonded body 400 of SiC-coated graphite members in which two SiC-coated graphite members 40 are firmly bonded together.
[0050] FIG. 7(a) is a perspective view showing a schematic diagram of a joined body of SiC-coated graphite members of the present invention according to another embodiment, and FIG. 7(b) is a cross-sectional view taken along line DD of the joined body of SiC-coated graphite members shown in FIG. 7(a).
[0051] In the SiC-coated graphite member joint 500 of this embodiment, a pipe-shaped SiC-coated graphite member 50 having a tapered lower portion is combined with a flange-shaped SiC-coated graphite member 60 having an inclined surface formed so as to approximately fit into the tapered portion of the SiC-coated graphite member 50, and the two are joined together by forming a second CVD-SiC layer. The SiC-coated graphite member 50 has a base material 51 coated with a first CVD-SiC layer 56, and the SiC-coated graphite member 60 has a base material 61 coated with a first CVD-SiC layer 66.
[0052] A convex portion 53 that serves as one end is formed on the central axis side of the tapered portion of the pipe-shaped SiC-coated graphite member 50, and a concave portion 54 that serves as the other end is formed on the outer periphery side. Also, on the inclined surface of the flange-shaped SiC-coated graphite member 60, a convex portion 63 which becomes one end is formed on the central axis side, and a concave portion 64 which becomes the other end is formed on the outer periphery side. These tops are flattened by a method such as co-milling.
[0053] The SiC-coated graphite member 50 and the SiC-coated graphite member 60 having such a configuration are combined so that the convex portions 53 and 63 of the SiC-coated graphite member 50 and the SiC-coated graphite member 60 abut against each other, and a second CVD-SiC layer 58 is formed on the outside of the convex portions 53 and 63 and on the entire inside of the recesses formed by the recesses 54 and 64, so that the SiC-coated graphite member 50 and the SiC-coated graphite member 60 are joined to form a joined body 500 of SiC-coated graphite members.
[0054] FIG. 8(a) is a polarizing microscope photograph showing a cross-section of a joined body of SiC-coated graphite members of the present invention, and FIG. 8(b) is a cross-sectional view showing a schematic configuration of the joined body of SiC-coated graphite members shown in FIG. 8(a). According to Figure 8 (b), SiC-coated graphite members 70 each having a first CVD-SiC layer 76 formed on the surface of a base material 71 are combined at their mating surfaces, a second CVD-SiC layer 78 is formed in the recess 74, and the two SiC-coated graphite members 70 are joined by this second CVD-SiC layer 78. When forming the second CVD-SiC layer 78 on the SiC-coated graphite member 70, the source gas is supplied to the recess 74 from the right side (outside) of the drawing, but since the concentration of the source gas usually decreases the deeper into the recess 74, depending on the source gas conditions, after the second bonding portion 78b is formed in the surface layer, no bonding portion is formed in the recess 74, leaving a cavity. However, the first bonding portion is formed on the convex side of the second bonding portion 78b and the photograph (not shown), resulting in a bonded body of SiC-coated graphite members with high bonding strength and airtightness.
[0055] 9(a) to (d) are cross-sectional views showing examples of combinations of SiC-coated graphite members other than those shown in FIGS. 1 to 7 when producing a joined body of SiC-coated graphite members. 9(a) to (d), d1 indicates the distance between the substrates at the convex portions when the SiC-coated graphite members are assembled, and d2 indicates the longest distance between the substrates at the concave portions. A short d1 means that the first CVD-SiC layer sandwiched between them is thin. In addition, (d2-d1) is the difference in distance between the ends on the convex portion side and the ends on the other end side (concave portion side) on the assembled surfaces.
[0056] Figure 9(a) shows an example of a combination in which substrates 81 (SiC-coated graphite members 80) of the same shape, on which convex portions and concave portions are formed, are combined. In this example of combination, the distance d2 is large and concave portions with large capacity are formed, making it easy to form a second CVD-SiC layer inside the concave portions.
[0057] 9(b) shows an example of a combination of a substrate 81 (SiC-coated graphite member 80) having a convex portion and a concave portion formed thereon and a substrate 91 (SiC-coated graphite member 90) having a flat mating surface, in which the distance d2 is about half that of the combination example shown in FIG. 9(a), and the second CVD-SiC layer that closes the concave portion is easy to form, but the second CVD-SiC layer is easy to form only at the entrance of the concave portion. In addition, the substrate 91 having a flat mating surface is easy to process because of its simple shape.
[0058] 9(c) shows a combination example in which a base material 81 (SiC-coated graphite member 80) having a convex portion is combined with a base material 101 (SiC-coated graphite member 100) having a convex portion of a slightly different shape, but the convex portion of one SiC-coated graphite member is combined with a lower surface of the other SiC-coated graphite member on which no convex portion is formed, and since the volume of the concave portion is small and the distance d2 between the two members is closer, when the second CVD-SiC layer is formed, the second joint can be easily formed in the concave portion, but a cavity is likely to be formed. Also, in this combination example, since the shapes are fitted together, the setting is unlikely to shift when the second CVD-SiC layer is formed, and handling during manufacturing is easy.
[0059] Figure 9(d) shows an example of a combination of a substrate 111 (SiC-coated graphite member 110) having an inclined surface in which the recess becomes gradually lower from the top of the protrusion, and a substrate 91 (SiC-coated graphite member 90) having a flat mating surface. Since the cross-sectional area of the recess becomes gradually smaller, the raw material gas can easily penetrate deep into the recess, and a second CVD-SiC layer can easily be formed over the entire recess. [Explanation of symbols]
[0060] 10, 31, 41, 51, 61, 71, 81, 91, 101, 111 Base material 10a Bottom 12, 22 Wall section 13, 23, 33, 43, 53, 63 Convex 13a, 23a, 33a top 14, 24, 34, 44, 54, 64, 74 recess 15, 25 Groove 20, 30, 40, 50, 60, 70 SiC coated graphite components 80, 90, 100, 110 SiC coated graphite components 26, 36, 46, 56, 66 First CVD-SiC layer 28, 38, 48, 58, 78 Second CVD-SiC layer 28a, 38a, 48a, 58a First joint 28b, 38b, 48b, 58b, 78b Second joint 39, 49 hollow 200, 300, 400, 500, 700 SiC-coated graphite member joint 330a flattened top
Claims
1. A method for producing a joined body of SiC-coated graphite members, the CVD-SiC layer comprising a first CVD-SiC layer covering a surface of a substrate made of graphite, and a second CVD-SiC layer joining a plurality of the substrates, comprising: a combining step of combining a plurality of SiC-coated graphite members each having a first CVD-SiC layer on a combining surface; and a bonding step of covering the combined SiC-coated graphite members from the outside with a second CVD-SiC layer; a combination surface of at least one of the SiC-coated graphite members includes a convex portion on one end side of the combination surface that is higher than the surrounding area, and a concave portion on the other end side that opens to the outside of the combination surface by being combined with another SiC-coated graphite member; The second CVD-SiC layer is a first bonding portion that bonds the plurality of SiC-coated graphite members along an outer surface of the bonded body outside the convex portion of the combination surface; a second joining portion that penetrates into the recess from the outside of the recess of the mating surface and joins the opposing surfaces of the SiC-coated graphite members; having a top of each of the protrusions being on the same plane, and a ratio of an area of the top of each of the protrusions to an area of the joining surfaces being 5 to 60%.
2. 2. The method for manufacturing a joined body of SiC-coated graphite members according to claim 1, wherein at the joining surface, a first CVD-SiC layer is provided on the surface of each of the substrates made of graphite.
3. 3. The method for producing a joined body of SiC-coated graphite members according to claim 2, wherein the first CVD-SiC layer on the top surface of the protrusion is a polished surface.
4. 4. The method for manufacturing a joined body of SiC-coated graphite members according to claim 3, wherein the tops of the protrusions are on the same plane.
Citation Information
Patent Citations
Manufacture of tubular member
JP1987128974A
Member for semiconductor diffusion furnace
JP1987200722A
SiC COATED CARBON MEMBER, AND MANUFACTURING METHOD THEREOF
JP2010070797A
Carbon component and method of manufacturing the same
JP2011225949A
Production method of silicon carbide member
JP2019055897A