Relative dopant concentration levels in solar cells
By lowering P-type dopant concentration and using hydrogen passivation, the recombination issue at the butt PN junction is addressed, achieving higher efficiency and cost-effectiveness in solar cell production.
Patent Information
- Application Number
- JP2020069400
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2014-05-30
- Filing Date
- 2020-04-07
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2035-05-21
AI Technical Summary
Existing solar cells face high recombination rates at the butt PN junction, limiting their efficiency to below 20%, particularly due to high dopant concentrations at grain boundaries in the polysilicon layer.
Reducing the P-type dopant concentration level in the polysilicon layer to ~5E17/cm3 and using hydrogen passivation to minimize recombination at the butt PN junction, thereby forming highly efficient solar cells without the need for physical trenches.
This approach enhances solar cell efficiency beyond 20% by reducing recombination and extending the service life of the material, while also lowering manufacturing costs by eliminating the need for additional processing steps.
Smart Images

Figure 0007580933000001 
Figure 0007580933000002 
Figure 0007580933000003
Abstract
Description
[Background technology]
[0001] Photovoltaic cells, known as solar cells, are well known devices for directly converting solar radiation into electrical energy. Typically, solar cells are fabricated on semiconductor wafers or substrates using semiconductor processing techniques to form a PN junction between a P-type diffusion region and an N-type diffusion region. Solar radiation impinges on the surface of the solar cell's substrate and penetrates into the substrate, generating electron-hole pairs in the bulk of the substrate. The electron-hole pairs migrate to P-type and N-type diffusion regions in the substrate, creating a voltage difference between the diffusion regions. The diffusion regions are connected to conductive regions on the solar cell to direct current from the solar cell to an external circuit. In a backside contact solar cell, for example, the diffusion regions and interdigitated metal contact fingers coupled to the diffusion regions are both on the backside of the solar cell. The contact fingers allow an external electrical circuit to be coupled to and powered by the solar cell.
[0002] Efficiency is an important property of solar cells since it is directly related to the solar cell's ability to generate electricity. Similarly, the efficiency in producing solar cells is directly related to the cost-effectiveness of such solar cells. Therefore, techniques for improving the efficiency of solar cells or for improving the efficiency in the manufacture of solar cells are generally desirable. Some embodiments of the present disclosure enable improved efficiency of solar cell manufacturing by providing novel processes for manufacturing solar cell structures. Some embodiments of the present disclosure enable improved efficiency of solar cells by providing novel solar cell structures. [Brief description of the drawings]
[0003] [Figure 1] 1 illustrates a cross-sectional view of a portion of an example solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed above a substrate, according to some embodiments.
[0004] [Diagram 2] 4 is a flow chart illustrating an exemplary method of forming a backside contact solar cell having a lower P-type dopant concentration level, according to one embodiment.
[0005] [Diagram 3] 4 is a flow chart illustrating an exemplary method of forming a backside contact solar cell having a lower P-type dopant concentration level, according to one embodiment.
[0006] [Figure 4] 1A-1D illustrate cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed on a substrate according to some embodiments. [Diagram 5] 1A-1D illustrate cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed on a substrate according to some embodiments. [Figure 6] 1A-1D illustrate cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed on a substrate according to some embodiments. [Figure 7] 1A-1D illustrate cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed on a substrate according to some embodiments. [Figure 8] 1A-1D illustrate cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed on a substrate according to some embodiments. [Figure 9] 1A-1D illustrate cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed on a substrate according to some embodiments.
[0007] [Figure 10]4 is a flow chart illustrating an exemplary method of forming a backside contact solar cell having a lower P-type dopant concentration level, according to one embodiment.
[0008] [Figure 11] 1A-1D show cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between P-type and N-type diffusion regions formed using counter-doping on a substrate, according to some embodiments. [Figure 12] 1A-1D show cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between P-type and N-type diffusion regions formed using counter-doping on a substrate, according to some embodiments. [Figure 13] 1A-1D show cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between P-type and N-type diffusion regions formed using counter-doping on a substrate, according to some embodiments. [Figure 14] 1A-1D show cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between P-type and N-type diffusion regions formed using counter-doping on a substrate, according to some embodiments. [Figure 15] 1A-1D show cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between P-type and N-type diffusion regions formed using counter-doping on a substrate, according to some embodiments. [Figure 16] 1A-1D show cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between P-type and N-type diffusion regions formed using counter-doping on a substrate, according to some embodiments.
[0009] [Figure 17]1 is a flow chart illustrating an exemplary method of forming a backside contact solar cell having a lower P-type dopant concentration level by printing P-type and N-type dopant sources according to one embodiment.
[0010] [Figure 18] 1A-1D show cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed by printing on a substrate, according to some embodiments. [Figure 19] 1A-1D show cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed by printing on a substrate, according to some embodiments. [Figure 20] 1A-1D show cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed by printing on a substrate, according to some embodiments. [Figure 21] 1A-1D show cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed by printing on a substrate, according to some embodiments. [Figure 22] 1A-1D show cross-sectional views of a process for forming a backside contact solar cell having a butted PN junction formed between a P-type diffusion region and an N-type diffusion region formed by printing on a substrate, according to some embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The following detailed description is merely exemplary in nature and is not intended to limit the embodiments of the subject matter of the present application or the uses of such embodiments. As used herein, the word "exemplary" means "serving as an example, instance, or illustration." Any implementation described herein as exemplary is not necessarily to be construed as preferred or advantageous over other implementations. Furthermore, there is no intention to be bound by any expressed or implied theory presented in the preceding technical field, background, brief summary, or the following detailed description.
[0012] The present specification includes references to "one embodiment" or "an embodiment." The appearances of the phrases "in one embodiment" or "in an embodiment" do not necessarily refer to the same embodiment. Particular features, structures, or characteristics may be combined in any suitable manner consistent with the present disclosure.
[0013] Terminology. The following paragraphs provide definitions and / or context for terms found in this disclosure (including the appended claims).
[0014] "Comprises." The term is open-ended. When used in the claims, the term does not exclude further structures or steps.
[0015] "Configured to." Various units or components may be described or claimed as being "configured to" perform a task. In such a context, "configured to" is used to imply structure by indicating that the units / components include structure that performs those tasks during operation. Thus, the units / components can be said to be configured to perform a task even if the specified unit / component is not currently operational (e.g., not on / active). Describing a unit / circuit / component as being "configured to" perform one or more tasks expressly intends that 35 U.S.C. § 112, paragraph 6 does not apply with respect to that unit / component.
[0016] "first," "second," etc. As used herein, these terms are used as indicators with respect to the noun they precede and do not imply any type of ordering (e.g., spatial, temporal, logical, etc.). For example, a reference to a "first" dopant source does not necessarily imply that this dopant source is the first dopant source in a sequence; instead, the term "first" is used to distinguish this dopant source from another dopant source (e.g., a "second" dopant source).
[0017] "Based on." As used herein, this term is used to describe one or more factors that influence the decision. This term does not exclude additional factors that may influence the decision. That is, the decision may be based solely on those factors or may be based at least in part on those factors. Consider the phrase "determining A based on B." Although B may be a factor that influences the decision of A, such a phrase does not exclude that the decision of A is also based on C. In other cases, A may be determined solely based on B.
[0018] "Coupled" - The following description refers to elements or nodes or features being "coupled" together. As used herein, unless expressly stated otherwise, "coupled" means that one element / node / feature is directly or indirectly connected to (or in direct or indirect communication with) another element / node / feature, not necessarily mechanically.
[0019] "Inhibit" - As used herein, inhibit is used to describe reducing or minimizing an effect. When components or mechanisms are described as inhibiting an action, operation, or condition, these components or mechanisms may completely prevent that result or outcome, or a future condition. Furthermore, "inhibit" may also refer to reducing or diminishing an outcome, performance, and / or effect that would normally occur. Thus, when components, elements, or mechanisms are described as inhibiting an outcome or condition, these components, elements, or mechanisms do not necessarily completely prevent or eliminate the outcome or condition.
[0020] Moreover, certain terminology may also be used in the following description for reference purposes only, and therefore, such terminology is not intended to be limiting. For example, terms such as "upper," "lower," "upper," and "lower" refer to directions within the drawings to which reference is made. Terms such as "front," "rear," "rear," "side," "outer," and "inner" describe the orientation and / or location of parts of a component within a consistent, but arbitrary, frame of reference that is made clear by reference to the text and associated drawings that describe the component under discussion. Such terminology may include the words specifically mentioned above, their derivatives, and synonyms.
[0021] For ease of understanding, much of this disclosure will be described with respect to solar cells, however, the techniques and structures disclosed apply equally to other semiconductor structures (eg, silicon wafers in general).
[0022] In the following description, numerous specific details are set forth, such as specific process flow operations, to provide a thorough understanding of the embodiments of the present disclosure. It will be apparent to those skilled in the art that the embodiments of the present disclosure may be practiced without these specific details. In other instances, well-known manufacturing techniques, such as lithography techniques, are not described in detail so as not to unnecessarily obscure the embodiments of the present disclosure. Furthermore, it should be understood that the various embodiments shown in the figures are illustrative representations and are not necessarily drawn to scale.
[0023] This specification will first describe an exemplary solar cell that may include the disclosed dopant levels, followed by a more detailed description of various embodiments for forming a dual dopant level solar cell structure. Various examples are provided throughout.
[0024] Referring to FIG. 1, a cross-sectional view of a solar cell 100 is shown having a front side 100A that faces the sun to receive solar radiation during normal operation, and a back side 100B opposite the front side. The back side 100B of the solar cell 100 includes a P-type diffused polysilicon region 102 and an N-type diffused polysilicon region 104 that, in one embodiment, are disposed above a dielectric layer 106 and form a butted PN junction 109 on a portion of a substrate 110. One example of the substrate 110 includes N-type silicon. Generally speaking, the P-type diffused polysilicon region 102 and the N-type diffused polysilicon region 104 form a diode at the butted junction 109. The P-type diffused polysilicon region 102 and the N-type diffused polysilicon region 104 may be formed in a single polysilicon layer. These diffusion regions can be formed, for example, by depositing a doped silicon dioxide layer on an undoped polysilicon layer and performing a diffusion step, or by depositing an undoped polysilicon layer followed by a dopant implantation step. In a particular embodiment, the P-type diffused polysilicon region 102 and the N-type diffused polysilicon region 104 are formed above the surface of the substrate 110 or external to the solar cell substrate.
[0025] The solar cell 100 may further include conductive contacts formed on an emitter region formed above the substrate 110, according to one embodiment. A first conductive contact, such as a first metal contact finger 114, may be disposed in a first contact opening disposed in the silicon nitride layer 112 and may be coupled to the P-type diffused polysilicon region 102. A second conductive contact, such as a second metal contact finger 116, may be disposed in a second contact opening disposed in the silicon nitride layer 112 and may be coupled to the N-type diffused polysilicon region 104. These "fingers" may be fabricated using a mask and etch or according to other techniques.
[0026] In one embodiment, the P-type diffused polysilicon region 102 and the N-type diffused polysilicon region 104 can provide an emitter region for the solar cell 100. Thus, in one embodiment, the first metal contact finger 114 and the second metal contact finger 116 are disposed on the corresponding emitter regions. In one embodiment, the first metal contact finger 114 and the second metal contact finger 116 are back contacts for a back-contact solar cell and are located on a surface of the solar cell opposite the light receiving surface (face 100A) of the solar cell 100. Furthermore, in one embodiment, the emitter region is formed on a thin dielectric layer or tunnel dielectric layer, such as the dielectric layer 106.
[0027] According to some embodiments, as shown in FIG. 1, fabricating a back contact solar cell may include forming a thin dielectric layer 106 on a substrate 110. In one embodiment, the thin dielectric layer is composed of silicon dioxide and has a thickness in the range of about 5-50 angstroms. In one embodiment, the thin dielectric layer functions as a tunnel oxide layer. In one embodiment, the substrate 110 is a bulk single crystal silicon substrate, such as an N-type doped single crystal silicon substrate. However, in another embodiment, the substrate comprises a polycrystalline silicon layer disposed on a global solar cell substrate.
[0028] In a back-contact solar cell, such as solar cell 100, that has interdigitated N-type and P-type diffusions in a polysilicon layer, there is a butted PN junction 109 that may be formed within the polysilicon layer at the interface between the two diffusions. The butted PN junction 109 is the area between boron doped (P-type) polysilicon and phosphorus doped (N-type) polysilicon. The butted PN junction 109 may extend into both sides of the physical interface between the P-type and N-type diffusion regions. The width of this physical junction and how far it extends into each side of the physical junction depends on the doping concentration levels and concentration gradients on each side of the butted PN junction 109.
[0029] Typically, space charge recombination occurs at the polycrystalline grain boundaries of the PN junction 109. Space charge recombination is the process by which mobile charge carriers (electrons and electron holes) are eliminated. This is the process by which conduction band electrons lose energy and reoccupy the energy state of electron holes in the valence band. The polycrystalline silicon of the polysilicon layer consists of grains. Each grain has a perfect crystal lattice with all the Si atoms aligned. However, different grains may have different orientations and there are boundaries between them where the crystallinity of the material is broken. This interface is called a grain boundary. In certain areas of the material, such as the grain boundaries, the probability of electron hole recombination is increased. For example, defects in metals increase recombination. The inventors have found that boron at grain boundaries is one such area where there is higher recombination. If such areas are reduced, the life of the material will be longer and the possibility of collecting carriers will increase.
[0030] Butt PN junctions 109 in most cases have high recombination, which prevents them from reaching high device efficiencies above 20%. However, the inventors have found that space charge recombination can vary with the P-type dopant concentration level. By lowering the dopant concentration level to ∼5E17 / cm3 in the polysilicon layer, there are enough boron atoms at the grain boundaries that recombination is suppressed to a level where a highly efficient device can be fabricated.
[0031] Consistent with one embodiment, the P-type diffused polysilicon region 102 can be formed by a P-type dopant source 120 having a first dopant concentration level, and the N-type diffused polysilicon region 104 can be formed by an N-type dopant source 122 having a second dopant concentration level, such that the first dopant concentration level is lower than the second dopant concentration level. For example, the P-type diffused polysilicon region 102 can be formed in the polysilicon layer by a P-type dopant source including boron having a dopant concentration level lower than the range of 1E17 / cm3 to 1E18 / cm3, resulting in the P-type diffused polysilicon region 102 having a dopant concentration level lower than the range of ∼5E19 / cm3 to ∼5E17 / cm3. Similarly, an N-type dopant source including phosphorus can be used to form the N-type diffused polysilicon region 104. The dopant source is a source of charge carrier impurity atoms for a substrate, such as boron for a silicon-based substrate. For example, in one embodiment, the charge carrier impurity atoms are N-type dopants, such as, but not limited to, phosphorus dopants, while in another embodiment, the charge carrier impurity atoms are P-type dopants, such as, but not limited to, boron dopants.
[0032] In one embodiment, the P-type diffused polysilicon region 102 and the N-type diffused polysilicon region 104 are active regions. Conductive contacts may be coupled to the active regions and separated from one another by isolation regions, which may be composed of a dielectric material. In one embodiment, the solar cell is a back-contact solar cell and further includes an anti-reflective coating layer (e.g., dielectric layer 106) disposed on a light-receiving surface, such as on the irregularly textured surface of the solar cell.
[0033] By having a first dopant concentration level of the P-type dopant source 120 less than a second dopant concentration level of the N-type dopant source 122, recombination at the butted PN junction 109 can be reduced to such an extent that the resulting device efficiency is greater than 20%. For example, an N-type dopant source including phosphorus having a dopant concentration level greater than about 1E19 / cm3 to 1E20 / cm3 can be used to form an N-type diffused polysilicon region 104 in a polysilicon layer, as compared to a P-type dopant source of boron having a dopant concentration level less than about 1E17 / cm3 to 1E18 / cm3.
[0034] By reducing the P-type dopant concentration level to a lower concentration level, recombination is reduced, thereby forming a highly efficient solar cell. In some embodiments, it is not necessary to physically separate the N-type and P-type diffusions using a trench to reduce recombination. By reducing recombination at the butted PN junction 109 without the need for a physical trench, at least two steps can be eliminated in the manufacturing process of the solar cell 100, thereby reducing costs.
[0035] Further increases in lifetime can be achieved by passivation of grain boundaries using hydrogen (H), i.e., further improvements in recombination can be achieved by passivating the now vacant grain boundary sites using hydrogen (H). This can be done during a forming gas anneal ("FGA"), which drives H from the nearby silicon nitride layer, or by plasma enhanced chemical vapor deposition (PECVD) of H (e.g., prior to nitride deposition).
[0036] Lowering the boron doping concentration level can help the effect of H passivation. For example, at lower boron levels, hydrogenation (e.g., H passivation of any dangling Si bonds at the surface) can result in longer battery life. In contrast, at higher boron concentrations, boron atoms can present a large number of dangling bonds. However, at lower concentrations, H can then reach those bonds and passivate them.
[0037] For example, in one embodiment, H passivation can be performed by forming gas annealing (FGA) using a mixture of N2 and H2. Traditionally, H in the forming gas is the source of H, but an alternative source of H is from a silicon nitride PECVD layer or film that can be deposited on top of the polysilicon layer. This silicon nitride PECVD layer or film itself can have a lot of H and can be used to diffuse into the interface region of the butted PN junction 109 to improve passivation during the anneal that creates the passivated region 124. The reduced boron level at this interface or at the butted PN junction 109 allows H to reach the dangling Si bonds and passivate them.
[0038] 1, a dielectric in the form of a silicon nitride layer 112 may extend over the P-type diffused polysilicon region 102 and the N-type diffused polysilicon region 104. In one embodiment, the silicon nitride layer 112 is formed by plasma enhanced chemical vapor deposition (PECVD) to a thickness of approximately 400 Angstroms.
[0039] Turning now to Figure 2, a flow chart illustrating a method for forming a solar cell is shown, according to one embodiment. As shown at 202, a layer of polysilicon can be deposited, printed, or implanted over the semiconductor region. Alternatively, in some embodiments, the polysilicon can be formed from amorphous silicon that has been converted to polysilicon. As described herein, in Figure 1, a pre-doped polysilicon layer is shown.
[0040] As shown at 204, a P-type diffused polysilicon region 102 as shown in Figure 1 may be formed from a P-type doped region. The P-type diffused polysilicon region 102 may be formed by a P-type dopant source having a dopant concentration level A present in the P-type doped region. As shown at 206, an N-type diffused polysilicon region 104 as shown in Figure 1 may be formed from an N-type doped region by an N-type dopant source having a dopant concentration level B present in the N-type doped region. The dopant concentration level A of the P-type dopant source is less than the dopant concentration level B of the N-type dopant source. For example, the boron dopant concentration level A can be 1E17 / cm3 to 1E18 / cm3, and the phosphorus dopant concentration level B can be 1E19 / cm3 to 1E20 / cm3 in the N-type dopant source, such that the resulting doping concentration level in the P-type diffused polysilicon region 102 can be 5E19 / cm3 to 5E17 / cm3. In one embodiment, the boron doping can be kept .about.2 orders of magnitude different from the phosphorus doping, such that the P-type to N-type concentration ratio is 1:100. Hydrogen H can be used to passivate at least a portion of the dangling Si bonds at the butted PN junction 109, as shown at 208.
[0041] Referring to FIG. 3, a flow chart 300 is shown depicting operations in a method for forming P-type and N-type diffusion regions for a back-contact solar cell, according to one embodiment. FIGS. 4-9 show cross-sectional views of various stages in the fabrication of a back-contact solar cell, corresponding to operations of flow chart 300, according to one embodiment of the present invention. In this example, the process steps mentioned are performed in the order shown. In other examples, these process steps can be performed in other orders. It should be noted that other process steps not necessary for understanding have been omitted for clarity. Other process steps, such as, for example, forming metal contacts to the P-type and N-type diffusion regions, follow the passivation step to complete the fabrication of the solar cell. Furthermore, in some embodiments, the process may include less than all of the steps shown.
[0042] With reference to operation 302 of Flowchart 300 and corresponding Figure 4, a method of forming a butted PN junction 411 (see Figure 8) for a back-contact solar cell includes forming a thin dielectric layer 402 on a backside surface of a substrate 400. As shown, Figure 4 shows a solar cell substrate 400 having a backside 405 and a frontside 406. Within the solar cell, there are multiple P-type and N-type diffusion regions, although for clarity of illustration, only one of each is shown to be fabricated in the following examples.
[0043] In one embodiment, the thin dielectric layer 402 is comprised of silicon dioxide and has a thickness in the range of about 5-50 angstroms (e.g., 20 angstroms). In one embodiment, the dielectric layer 402 comprises silicon dioxide thermally grown on the surface of the substrate 400. The dielectric layer 402 may also comprise, for example, silicon nitride. The thin dielectric layer 402 functions as a tunneling oxide layer. In a particular embodiment, the dielectric layer 402 is an anti-reflective coating (ARC) layer. In one embodiment, the substrate 400 is a bulk single crystal substrate, such as an N-type doped single crystal silicon substrate or an N-type silicon wafer. However, in an alternative embodiment, the substrate 400 may comprise a polycrystalline silicon layer disposed on a global solar cell substrate.
[0044] 4, there is shown the formation of an undoped polycrystalline silicon (polysilicon) layer 404 on the thin dielectric layer 402. It should be understood that the use of the term polysilicon layer is intended to encompass materials that may also be described as amorphous silicon or alpha silicon. The polysilicon layer 404 may be formed, for example, by low pressure chemical vapor deposition (LPCVD) to a thickness of approximately 2000 Angstroms.
[0045] Referring to operation 306 of Flowchart 300 and corresponding Figures 5 and 6, there is shown the steps of forming a first doped silicon dioxide layer 407 of Figure 5 on polysilicon layer 404 and patterning a first dopant source 408 of a first conductivity type, such as P-type (e.g., boron) (operation 308 of Flowchart 300). The first doped silicon dioxide layer 407 serves as a dopant source for a subsequently formed diffusion region, which in this example is P-type diffusion region 414 (see Figure 8). The first doped silicon dioxide layer 407 may therefore be doped with a P-type dopant, such as boron. The first doped silicon dioxide layer 407 is patterned (Figure 6) such that it remains over an area of polysilicon layer 404 where P-type diffusion region 414 is to be formed. The first doped silicon dioxide layer 407 may be formed by atmospheric pressure chemical vapor deposition (APCVD) to a thickness of approximately 1000 Angstroms.
[0046] In one embodiment, this patterning step exposes areas of the polysilicon layer 404 adjacent to the areas of the first dopant source 408, as shown in FIG. 6. In one embodiment, forming and patterning the first dopant source 408 includes forming and patterning a layer of borosilicate glass (BSG). In a particular embodiment, this BSG layer is formed by chemical vapor deposition as a uniform blanket layer and then patterned by lithography and etching processes. In one such embodiment, the BSG layer is formed by a chemical vapor deposition technique, such as, but not limited to, atmospheric pressure chemical vapor deposition (APCVD), plasma enhanced chemical vapor deposition (PECVD), low pressure chemical vapor deposition (LPCVD), or ultra-high vacuum chemical vapor deposition (UHVCVD). In an alternative embodiment, the BSG layer is deposited in a pre-patterned state, so that the forming and patterning steps are performed simultaneously. In one such embodiment, the patterned BSG layer is formed by a screen printing technique. In one embodiment, the first dopant source 408 is a layer of film containing P-type dopant impurity atoms and may be deposited above the substrate. In an alternative embodiment, an ion implantation technique may be used.
[0047] In one embodiment, lower P-type doping in the polysilicon layer is achieved by lowering the amount of dopant in the BSG oxide layer (P-type dopant source). The concentration of boron (B) in the BSG oxide layer is reduced from a typical level of ~4% to ~1-2%. This results in a reduction in the amount of P-type dopant concentration level in the polysilicon layer from ~5E19 / cm3 to ~5E17 / cm3.
[0048] Referring to operation 310 of Flowchart 300 and corresponding FIG. 7, there is shown the step of forming a second doped silicon dioxide layer 410 of FIG. 7 on the polysilicon layer 404 and above the first dopant source 408 of P type to provide a second dopant source 412 of a second conductivity type, such as N type (e.g., phosphorus). The second doped silicon dioxide layer 410 serves as a dopant source for a subsequently formed diffusion region, which in this embodiment is an N type diffusion region 416 (see FIG. 8). The second doped silicon dioxide layer 410 may therefore be doped with an N type dopant, such as phosphorus. The second doped silicon dioxide layer 410 may be formed by APCVD to a thickness of about 2000 angstroms.
[0049] In one embodiment, forming the second dopant source 412 includes forming a layer of phosphosilicate glass (PSG). In a particular embodiment, the PSG layer is formed by chemical vapor deposition as a uniform blanket layer and then patterned by lithography and etching processes. In one such embodiment, the PSG layer is formed by a chemical vapor deposition technique, such as, but not limited to, atmospheric pressure chemical vapor deposition (APCVD), plasma enhanced chemical vapor deposition (PECVD), low pressure chemical vapor deposition (LPCVD), or ultra-high vacuum chemical vapor deposition (UHVCVD). In one embodiment, the second dopant source 412 is a layer of a film containing N-type dopant impurity atoms and may be deposited above the substrate. In an alternative embodiment, ion implantation techniques may be used.
[0050] By using a PSG layer, in one embodiment, the N-type doping concentration level in the N-type diffusion region 416 of the polysilicon layer 404 can range from about 10% of the dopant concentration level of the N-type dopant source, e.g., 1E19 / cm3 to 1E20 / cm3.
[0051] Referring now to operation 312 of Flowchart 300 and corresponding FIG. 8, a step of heating substrate 400 is illustrated. In one embodiment, this heating drives dopants from first dopant source 408 and second dopant source 412. For example, in one embodiment, heating substrate 400 drives dopants from first dopant source 408 and second dopant source 412, respectively, into polysilicon layer 404. However, in another embodiment, first dopant source 408 and second dopant source 412 may be formed directly on substrate 400 or on a thin oxide on substrate 400, and heating substrate 400 drives dopants from first dopant source 408 and second dopant source 412, respectively, into substrate 400. In one particular such embodiment, the substrate 400 is a bulk crystalline silicon substrate on which a first dopant source 408 and a second dopant source 412 are formed. The bulk crystalline silicon substrate is then heated to drive dopants from the first dopant source 408 and the second dopant source 412 into the bulk crystalline silicon substrate.
[0052] In operation 312, a thermal drive-in step diffuses dopants from the first doped silicon dioxide layer 407 and the second doped silicon dioxide layer 410 into the underlying polysilicon layer 404 to form P-type and N-type diffusion regions in the polysilicon layer 404, appropriately labeled as P-type and N-type diffused polysilicon regions 414 and 416. This thermal drive-in step may be performed by heating the sample of FIG. 7. In one embodiment, the drive conditions result in a highly doped polysilicon layer that is uniform throughout the thickness of the film, e.g., greater than 1E20 / cm3, with very little doping beneath the polysilicon, e.g., 1E18 / cm3 or less. This thermal drive-in process results in the polysilicon layer 404 underneath the first doped silicon dioxide layer 407 forming a P-type diffused polysilicon region 414 and the polysilicon layer 404 underneath the second doped silicon dioxide layer 410 forming an N-type diffused polysilicon region 416. The dopant concentration level of the P-type diffused polysilicon region 414 may be less than the dopant concentration level of the N-type diffused polysilicon region 416. For example, the P-type dopant concentration level may be 1E17-1E18 / cm3 and the N-type dopant concentration level may be 1E19-1E20 / cm3.
[0053] 9, a step of forming a silicon nitride layer 420 (e.g., similar to FIG. 7) on the second doped silicon dioxide layer 410 is shown. Hydrogen (H), as indicated by arrow 425, generated in operation 314 can be used to passivate the butted PN junction 411 of FIG.
[0054] Forming contact openings can provide exposure to N-type diffused polysilicon region 416 and P-type diffused polysilicon region 414. In one embodiment, the contact openings are formed by laser ablation. Forming contacts for a back-contact solar cell can include forming conductive contacts in the contact openings to couple N-type diffused polysilicon region 416 and P-type diffused polysilicon region 414. Thus, in one embodiment, the conductive contacts are formed on or above a surface of a bulk N-type silicon substrate, such as substrate 400, opposite the light-receiving surface of substrate 400.
[0055] Referring to FIG. 10, a flow chart 1000 is shown depicting operations in an exemplary method of forming P-type and N-type diffusion regions by counterdoping for a back-contact solar cell. FIGS. 11-16 show cross-sectional views of various stages in the fabrication of a back-contact solar cell, corresponding to operations of flow chart 1000, according to one embodiment. In this example, the process steps mentioned are performed in the order shown, but in other embodiments, different orders can be used. It should be noted that other process steps not necessary for understanding have been omitted for clarity. Other process steps, such as, for example, forming metal contacts to the P-type and N-type diffusion regions, follow the passivation step to complete the fabrication of the solar cell. Furthermore, in some embodiments, fewer than all of the steps shown in FIG. 10 can be used. In various embodiments, the description of the method of FIG. 3 applies equally to the description of the method of FIG. 10. Therefore, for clarity of explanation, some of the descriptions will not be repeated.
[0056] If the P-type dopant level is dramatically reduced, counterdoping techniques can be used to create N-type and P-type diffused regions. A very low P-type diffusion using boron can be used in the counterdoping process for areas where an N-type diffusion using phosphorus is required. For this purpose, an in-situ doped P-type film can be formed and then a patterned deposition using high levels of phosphorus can be performed. This will cause the original P-type material to be counterdoped to N-type. The non-N-type doped areas will remain P-type. One possible patterned deposition technique that can be deployed is implantation, but other techniques can work as well.
[0057] 11 shows a solar cell substrate 1100 having a backside 1105 and a frontside 1106. Within the solar cell, there are multiple P-type and N-type diffusion regions, but for clarity of explanation, only one of each is shown to be fabricated in the following examples.
[0058] Referring to operation 1002 of Flowchart 1000, and corresponding FIG. 11, a process is shown for forming a thin dielectric layer 1102 on a backside surface of a substrate 1100. In one embodiment, the substrate 1100 is a bulk single crystal substrate, such as an N-type doped single crystal silicon substrate or an N-type silicon wafer. The illustrated thin dielectric layer 1102 of FIG. 11 includes the same features as the thin dielectric layer 402 of FIG. 4. The illustrated substrate 1100 of FIG. 11 includes the same features as the substrate 400 of FIG. 4.
[0059] 11, there is shown a process for forming an undoped polycrystalline silicon (polysilicon) layer 1104 on a thin dielectric layer 1102. The illustrated polysilicon layer 1104 in FIG. 11 includes the same features as polysilicon layer 404 in FIG.
[0060] Referring to operation 1006 of Flowchart 1000 and corresponding FIG. 12, a step of forming a first doped silicon dioxide layer 1107 to provide a first dopant source 1108 of a first conductivity type, such as P-type (e.g., boron), on the polysilicon layer 1104 is shown. The first doped silicon dioxide layer 1107 serves as a dopant source for a subsequently formed diffusion region, which in this example is a P-type diffused polysilicon region 1114 (see FIG. 15), formed from the first dopant source or P-type dopant source 1108. In one embodiment, forming the first dopant source 1108 includes forming a layer of borosilicate glass (BSG). The illustrated first doped silicon dioxide layer 1107 of FIG. 12 includes the same features as the first doped silicon dioxide layer 407 of FIG. 5.
[0061] Referring to operation 1008 of Flowchart 1000 and corresponding FIG. 13, a step of forming a second doped silicon dioxide layer 1110 on the first doped silicon dioxide layer 1107 to provide a second dopant source 1112 of a second conductivity type, such as N-type (e.g., phosphorus). The second doped silicon dioxide layer 1110 serves as a dopant source for a subsequently formed diffusion region, which in this example is an N-type diffused polysilicon region 1116 (see FIG. 15). In one embodiment, forming the second dopant source 1112 includes forming a layer of phosphosilicate glass (PSG). The illustrated second doped silicon dioxide layer 1110 of FIG. 13 includes the same features as the second doped silicon dioxide layer 410 of FIG. 7.
[0062] Referring to operation 1010 of flowchart 1000 and corresponding Figures 14 and 15, a step is shown of patterning a second dopant source 1112 of a second conductivity type, such as N-type (e.g., phosphorus), on the first doped silicon dioxide layer 1107. The second doped silicon dioxide layer 1110 serves as a dopant source for a subsequently formed diffusion region, which in this example is an N-type diffused polysilicon region 1116 (see Figure 15). The second doped silicon dioxide layer 1110 can therefore be doped with an N-type dopant, such as phosphorus. The second doped silicon dioxide layer 1110 is patterned such that it remains over an area of the first doped silicon dioxide layer 1107 where the N-type diffused polysilicon region 1116 will be formed (Figure 15).
[0063] Referring to operation 1012 of Flowchart 1000 and corresponding FIG. 15, a step of heating the substrate 1100 is performed. In one embodiment, heating the substrate 1100 drives dopants from the first dopant source 1108 and the second dopant source 1112, respectively, into the polysilicon layer 1104. In operation 1012, a thermal drive-in step diffuses dopants from the first doped silicon dioxide layer 1107 and the second doped silicon dioxide layer 1110 into the underlying polysilicon layer 1104 to form P-type and N-type diffusion regions in the polysilicon layer 1104, appropriately labeled as P-type and N-type diffused polysilicon regions 1114 and 1116. The dopant concentration level of the P-type diffused polysilicon region 1114 may be less than the dopant concentration level of the N-type diffused polysilicon region 1116. For example, the P-type dopant concentration level may be between 1E17 and 1E18 / cm3, and the N-type dopant concentration level may be between 1E19 and 1E20 / cm3.
[0064] With reference to operation 1014 of Flowchart 1000 and corresponding Figure 16, there is shown the formation of a silicon nitride layer 1120 over the second doped silicon dioxide layer 1110 and the exposed first doped silicon dioxide layer 1107 of Figure 15. Hydrogen (H), as indicated by arrow 1125, generated in operation 1014 can be used to passivate the butted PN junction 1111 of Figure 15.
[0065] Forming contact openings can provide exposure to N-type diffused polysilicon region 1116 and the plurality of P-type diffused polysilicon regions 1114. In one embodiment, the contact openings are formed by laser ablation. Forming contacts for a back-contact solar cell can include forming conductive contacts in the contact openings to couple N-type diffused polysilicon region 1116 and P-type diffused polysilicon region 1114. Thus, in one embodiment, the conductive contacts are formed on or above a surface of a bulk N-type silicon substrate, such as substrate 1100, opposite the light-receiving surface of substrate 1100.
[0066] Referring to Figure 17, a flowchart 1700 is shown depicting operations in a method for printing P-type and N-type dopant sources for a back-contact solar cell according to one embodiment of the disclosure. Figures 18-22 show cross-sectional views of various stages in the fabrication of a back-contact solar cell corresponding to operations of flowchart 1700, according to one embodiment. Figure 18 shows a solar cell substrate 1800 having a backside 1805 and a frontside 1806. There are multiple P-type and N-type diffusion regions within the solar cell, but for clarity of illustration, only one of each is shown to be fabricated in the following examples.
[0067] 18-22 show a schematic of the process including the following process steps: a) damage etching, b) polysilicon deposition, c) printing of dopant source, d) curing, and e) passivation. In this example, the process steps are performed in the order shown. Note that other process steps not necessary for understanding are omitted for clarity. Other process steps, such as forming metal contacts to the P-type and N-type diffusion regions, follow the passivation step to complete the fabrication of the solar cell.
[0068] Referring to operation 1702 of Flowchart 1700, and corresponding FIG. 18, a step of preparing a substrate 1800 for processing into a solar cell is shown by performing a damage etch step.
[0069] The substrate 1800, in this example, may comprise an N-type silicon wafer, and is typically obtained with a damaged surface from a sawing process used by a wafer supplier to slice the substrate 1800 from its ingot. The substrate 1800 may be approximately 100-200 micrometers thick when obtained from the wafer supplier. In one embodiment, the damage etching step involves removing approximately 10-20 μm from each side of the substrate 1800 using a wet etching process including potassium hydroxide. The damage etching step may also include cleaning the substrate 1800 to remove metal contamination. Thin dielectric layers (not labeled) may be formed on the front and back surfaces of the substrate 1800. These thin dielectric layers may comprise silicon dioxide, thermally grown to a thickness of 20 angstroms or less (e.g., 16 angstroms) on both surfaces of the substrate 1800. The front surface of substrate 1800, and materials formed thereon, are also referred to as being on the front side of the solar cell, since they face the sun to receive solar radiation during normal operation. Similarly, the back surface of substrate 1800, and materials formed thereon, are also referred to as being on the back side of the solar cell, which is opposite the front side.
[0070] 19, there is illustrated a process for forming a polysilicon layer 1804 on a thin dielectric layer (not shown) over a substrate 1800. The polysilicon layer 1804 is formed on the thin dielectric layer on the backside 1805 of the substrate 1800. The polysilicon layer 1804, which is undoped at this stage of the fabrication process, may be formed by LPCVD to a thickness of approximately 2200 Angstroms.
[0071] Referring to operation 1706 of Flowchart 1700, and corresponding FIG. 20, there is shown a step of printing a first dopant source 1808 and a second dopant source 1812 onto a polysilicon layer 1804 on a substrate 1800. As will become more apparent below, the first dopant source 1808 and the second dopant source 1812 provide dopants for forming diffusion regions in the polysilicon layer 1804 on the backside of the solar cell. For any given solar cell, several first dopant sources 1808 and second dopant sources 1812 are formed, although only one of each is shown in FIG. 20 for clarity of illustration. The first dopant source 1808 and the second dopant source 1812, which comprise printable inks, have different conductivity types. In the embodiment of Fig. 20, the first dopant source 1808 is a P-type dopant source and the second dopant source 1812 is an N-type dopant source. The first dopant source 1808 and the second dopant source 1812 are formed by printing, such as inkjet printing or screen printing. Inkjet printing may advantageously allow printing both the first dopant source 1808 and the second dopant source 1812 in a single pass of an inkjet printer nozzle over the substrate 1800. The first dopant source 1808 and the second dopant source 1812 may also be printed in separate passes, depending on the process.
[0072] Referring to operation 1708 of Flowchart 1700 and corresponding FIG. 21, a step is shown of forming a P-type diffused polysilicon region 1814 and an N-type diffused polysilicon region 1816 on a polysilicon layer 1804 over a substrate 1800 by diffusing dopants from a first dopant source 1808 and a second dopant source 1812. To diffuse the dopants, a curing step is performed to diffuse dopants from the first dopant source 1808 into the polysilicon layer 1804 to form a P-type diffused polysilicon region 1814 in the polysilicon layer 1804 and from the second dopant source 1812 into the polysilicon layer 1804 to form an N-type diffused polysilicon region 1816 in the polysilicon layer 1804. This curing step may be performed at a temperature range between 600° C. and 1100° C. (e.g., 950° C.) for approximately 30 minutes.
[0073] 22, there is shown a step of forming a silicon nitride layer 1820 over the printed first dopant source 1808 and second dopant source 1812. Hydrogen (H), as shown by arrow 1825, generated in operation 1710 can be used to passivate the butted PN junction 1811 of FIG.
[0074] Forming contact openings can provide exposure to N-type diffused polysilicon region 1816 and the plurality of P-type diffused polysilicon regions 1814. In one embodiment, the contact openings are formed by laser ablation. Forming contacts for a back-contact solar cell can include forming conductive contacts in the contact openings to couple N-type diffused polysilicon region 1816 and P-type diffused polysilicon region 1814. Thus, in one embodiment, the conductive contacts are formed on or above a surface of a bulk N-type silicon substrate, such as substrate 1800, opposite the light-receiving surface of substrate 1800.
[0075] Although specific embodiments have been described above, these embodiments are not intended to limit the scope of the present disclosure, even if only a single embodiment is described for a particular mechanism. The mechanism examples provided in this disclosure are intended to be illustrative rather than restrictive, unless otherwise specified. The above description is intended to cover alternatives, modifications, and equivalents as will be apparent to those skilled in the art having the benefit of this disclosure.
[0076] The scope of the present disclosure includes any feature or combination of features disclosed herein (explicitly or implicitly), or any generalization thereof, whether or not they alleviate any or all of the problems addressed herein. Accordingly, new claims may be formulated for any such combination of features during prosecution of this application (or an application claiming priority to this application). In particular, with reference to the appended claims, features from the dependent claims may be combined with features of the independent claims, and features from each independent claim may be combined in any suitable manner, and not just in the specific combinations recited in the appended claims.
[0077] In one embodiment, a solar cell includes a substrate having a front side facing the sun for receiving solar radiation during normal operation and a back side opposite the front side, on which a butt PN junction is formed between a P-type diffusion region and an N-type diffusion region, the P-type diffusion region being formed from a P-type doped region including a first dopant source having a first dopant concentration level, and the N-type diffusion region being formed from an N-type doped region including a second dopant source having a second dopant concentration level higher than the first dopant concentration level.
[0078] In one embodiment, the solar cell further includes polysilicon formed on the backside of the substrate, with P-type and N-type diffusion regions formed in the polysilicon.
[0079] In one embodiment, the solar cell further comprises a passivation region at the boundary region of the butted PN junction.
[0080] In one embodiment, the P-type diffusion region includes boron having a dopant concentration level of less than about 5E17 / cm3.
[0081] In one embodiment, the P-type diffusion region is doped with a dopant concentration level that reduces recombination at the butted PN junction to such an extent that the resulting device efficiency is greater than 20%.
[0082] In one embodiment, the N-type diffusion region includes phosphorous having a dopant concentration level greater than about 10% of 1E20 / cm3.
[0083] In one embodiment, the solar cell further includes a first metal contact finger coupled to a P-type diffusion region formed from a P-type doped region on the backside of the substrate, and a second metal contact finger coupled to an N-type diffusion region formed from an N-type doped region on the backside of the substrate.
[0084] In one embodiment, the P-type doped region and the N-type doped region are disposed on a dielectric layer over a substrate.
[0085] In one embodiment, a method of manufacturing a solar cell includes forming a P-type diffusion region over a substrate from a P-type doped region including a first dopant source having a first dopant concentration level, and forming an N-type diffusion region over the substrate and adjacent to the P-type diffusion region from an N-type doped region including a second dopant source having a second dopant concentration level, such that the first dopant concentration level is lower than the second dopant concentration level, thereby providing a butt PN junction between the P-type diffusion region and the N-type diffusion region.
[0086] In one embodiment, forming the butt PN junction further includes forming a layer of polysilicon on a backside of a substrate opposite a front side of the substrate that faces the sun for receiving solar radiation during normal operation, forming a P-type doped region on the layer of polysilicon, and forming an N-type doped region on the layer of polysilicon.
[0087] In one embodiment, the method further includes diffusing dopants from the P-type doped region to form a P-type diffusion region on the substrate, diffusing dopants from the N-type doped region to form an N-type diffusion region on the substrate, and forming the P-type diffusion region and the N-type diffusion region outside the substrate and over the dielectric layer.
[0088] In one embodiment, the method further comprises passivating the boundary region of the butted PN junction using hydrogen.
[0089] In one embodiment, diffusing dopants from the P-type doped region further comprises using boron as the P-type dopant source at a dopant concentration level of less than 1E17 / cm3.
[0090] In one embodiment, diffusing dopants from the N-type doped region further comprises using phosphorus as the N-type dopant source at a dopant concentration level greater than 1E20 / cm3.
[0091] In one embodiment, the method further comprises printing the P-type doped regions and the N-type doped regions using a printable ink.
[0092] In one embodiment, the method further includes electrically coupling a first metal contact finger to a P-type diffusion region on the backside of the substrate and electrically coupling a second metal contact finger to an N-type diffusion region on the backside of the substrate.
[0093] In one embodiment, the method further includes depositing in situ doped P-type polysilicon to form a P-type diffusion region, and forming an N-type diffusion region by counterdoping with dopants from a second dopant source using a masked N-type diffusion.
[0094] In one embodiment, a solar cell includes a substrate having a front side facing the sun for receiving solar radiation during normal operation and a back side opposite the front side, a polysilicon layer formed on the back side of the substrate, a P-type diffusion region and an N-type diffusion region formed in the polysilicon layer, a butt PN junction formed between the P-type diffusion region and the N-type diffusion region, the P-type diffusion region having a first dopant concentration level and the N-type diffusion region having a second dopant concentration level higher than the first dopant concentration level.
[0095] In one embodiment, the first dopant concentration level of the P-type diffusion region is less than about 5E17 / cm3.
[0096] In one embodiment, the concentration ratio of the P-type dopant source used to form the P-type diffusion region to the N-type dopant source used to form the N-type diffusion region is about 1:100.
Claims
1. a substrate including a front side facing the sun for receiving solar radiation during normal operation and a back side opposite the front side; a dielectric layer on the backside of the substrate; a P-type diffusion region and an N-type diffusion region in a polysilicon layer formed on the dielectric layer, the P-type diffusion region having a first dopant concentration level and the N-type diffusion region having a second dopant concentration level higher than the first dopant concentration level, with a passivation region disposed at a physical interface of the P-type diffusion region and the N-type diffusion region; a first metal contact finger coupled to the P-type diffusion region on the backside of the substrate; a second metal contact finger coupled to the N-type diffusion region on the backside of the substrate; The first dopant concentration level of the P-type diffusion region is 5E17 / cm 3 and the second dopant concentration level of the N-type diffusion region is less than 1E19 to 1E20 / cm 3 and The P-type diffusion region comprises boron having the first dopant concentration level.
2. 10. The solar cell of claim 1 further comprising a butted PN junction formed on the backside of the substrate extending on either side of the physical interface between the P-type diffusion region and the N-type diffusion region.
3. The solar cell of claim 2 , wherein the butted PN junction extends above a surface of the substrate.
4. The solar cell of claim 1 , wherein the P-type diffusion region comprises hydrogen-passivated silicon.
5. 5. The solar cell of claim 1 , wherein the surface of the polysilicon layer, the grain boundaries within the polysilicon layer, and the physical interface between the P-type diffusion region and the N-type diffusion region are hydrogen passivated.
6. The solar cell of claim 1 , wherein the P-type diffusion region is laterally adjacent to the N-type diffusion region.
7. The solar cell of claim 1 , wherein the N-type diffusion region comprises phosphorus having the second dopant concentration level.
Citation Information
Patent Citations
Single-sided electrode polycrystalline silicon thin film solar cell and manufacturing method thereof
CN102738253A
Method for introducing dopant element into silicon layer, manufacturing method for polysilicon solar battery, manufacturing method for polysilicon thin-film transistor, and apparatus for introducing dopant element into silicon layer
JP2008282921A
Back contact solar cell element, and method of manufacturing the same
JP2011061020A
Anti-reflective coating with a high light-absorbing layer for back-side contact solar cells
JP2011518422A
Solar cell module and its manufacturing method
JP2012500490A