Manufacturing apparatus and method for producing silicon nanowires on carbon-based powders for use in batteries

The CVD process using a tumbler reactor system efficiently produces silicon nanowires on carbon-based substrates, overcoming scalability and cost issues, enabling high-quality anode materials for lithium-ion batteries with enhanced energy density and durability.

JP7581296B2Active Publication Date: 2024-11-12ONED MATERIAL INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022160349
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-07-15
Filing Date
2022-10-04
Publication Date
2024-11-12
Estimated Expiration
2037-07-14

AI Technical Summary

Technical Problem

The production of silicon nanowires suitable for use as anode materials in lithium-ion batteries is constrained by low yields and high costs, limiting their availability and scalability to meet the growing demand in the industry.

Method used

A chemical vapor deposition (CVD) process using a tumbler reactor system is employed to grow silicon nanowires on carbon-based substrates like graphite particles, achieving high conversion rates and large-scale production of silicon-carbon composites, with configurations for efficient heating, cooling, and gas distribution to produce batches of up to hundreds or thousands of metric tons per year.

Benefits of technology

The method enables the production of high-quality silicon nanowires at industrial scales, addressing the limitations of previous methods and providing anode materials with superior energy density and cyclic durability, reducing costs and expanding their adoption in lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581296000001
    Figure 0007581296000001
  • Figure 0007581296000002
    Figure 0007581296000002
  • Figure 0007581296000003
    Figure 0007581296000003
Patent Text Reader

Abstract

There is a great need for methods to produce high-quality Si nanowire material for use in LIB components and devices in much larger annual volumes, within narrow manufacturing specifications, and at a cost suitable to address the fast-growing demand on the order of tens to thousands of metric tons per year per manufacturing facility. The present invention provides a manufacturing apparatus, system, and method for producing silicon (Si) nanowires on carbon-based powders, such as graphite, that can be used as anodes in lithium-ion batteries. In some embodiments, the present invention describes a tumbler reactor, a chemical vapor deposition (CVD) system, and a method for growing silicon nanowires on carbon-based powders in large quantities to provide production-scale anodes for the battery industry.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to and the benefit of U.S. Provisional Patent Application No. 62 / 363,087, filed July 15, 2016, entitled “Manufacturing Apparatus And Method For Making Silicon Nanowires On Carbon Based Powders For Use As Anodes In The Battery Industry,” the disclosure of which is incorporated herein by reference in its entirety.

[0002] Embodiments of the present application generally relate to manufacturing apparatus, systems, and methods for growing silicon (Si) nanowires on carbon-based substrates, such as particles of graphite powder, to economically produce silicon-carbon composite active materials for use in, for example, lithium-ion batteries. More specifically, embodiments of the present application relate to the inventive tumbler reactor and chemical vapor deposition (CVD) systems and methods for growing silicon nanowires on carbon-based substrates in large scale to meet the increasing demand for active materials for the battery industry. [Background technology]

[0003] The development of improved battery technologies continues to attract considerable effort and support. Lithium-ion batteries (LIBs) are one of the most promising areas for further advancement. LIBs generally consist of an anode, a cathode, a separation material separating the cathode and anode, and an electrolyte. The anodes of most commercially available LIBs generally include a copper foil current collector coated with a mixture of graphite powder, binder material, and / or conductive additives. The cathodes of most commercially available LIBs generally include an aluminum foil current collector coated with a lithium transition metal oxide-based cathode material. Conventional LIB anodes include intercalation-based active materials such as natural or synthetic graphite that have limited charge capacity and fall short of ever-increasing market demands for higher energy density (by volume or weight), higher power density, better cycling durability, longer battery life, faster charge rate, larger temperature charge or operating range, smaller expansion, and other important performance metrics.

[0004] Various anode materials with improved storage capacity and thermal stability have been proposed for lithium-ion batteries (LIBs) during the last decade. Silicon (Si) has been widely investigated as an active material for the anode in LIBs due to its attractive properties. The theoretical specific capacity of carbon-based active materials is 372 mAh / g, based on an intercalation ratio of one lithium atom (Li) per six carbon atoms (C). Alloys of Si and Li can be formed with a Li to Si ratio higher than the 1 / 6 ratio between Li and C atoms in fully lithiated carbon-based materials. In these alloys, the Li / Si ratio is such that the alloy phase Li 12 S 7 1.71 (with a theoretical capacity of 1636 mAh / g) for the alloy phase Li 15 S 4 The range is from 3.75 for Li (with a theoretical capacity of 3579 mAh / g). 22 S 5has a specific capacitance of 4.4 and a theoretical capacity of 4,200 mAh / g, but has not generally been reached in practical applications. In addition to the higher specific capacity, Si has a voltage plateau slightly higher than that of graphite, and therefore has attractive safety properties. Furthermore, Si is an abundant and inexpensive material, and lithiated Si is more stable than lithiated graphite in typical lithium-ion battery electrolytes.

[0005] Despite silicon's attractive properties, commercial attempts to utilize Si as an active material for LIBs have failed. Several factors contribute to this failure, including the lack of practical solutions to address the detrimental consequences of the large volume expansion and contraction of Si during lithiation and delithiation, the lack of solutions to address the short cycling durability of cells with Si-based anodes, and the lack of suitable methods to mass-produce high-quality Si-based anode materials at reasonable cost compared to existing commercial carbon-based active materials, even when cost comparisons take into account the improved specific capacity of anodes containing silicon.

[0006] According to the present invention, active materials based on Si nanowires grown and / or deposited on carbon-based substrates such as graphite particles can be produced in large quantities at attractive costs and address previous limitations of other silicon containing active anode materials for LIBs. Nanowires are commonly described as "one-dimensional nanostructures" due to their very small radius and large length / radius aspect ratio. For example, nanowires can have an average diameter of less than about 200 nm, e.g., between about 5 nm and about 100 nm, e.g., between about 20 nm and about 50 nm. Si nanowires exhibit aspect ratios (ratio of length to width) of 5, 10, 15 or more, 25 or more, 50 or more, or even greater than 100. Si nanowires offer unique physical, chemical, and electrical properties that make them suitable for overcoming many of the side effects caused by other forms of silicon-containing materials when used as anode active materials in LIBs. Specifically, during lithiation (charging) and delithiation (discharging), the large surface curvature (i.e., small diameter) of the Si nanowires provides a smaller energy barrier to lithium insertion, allowing for easier release of mechanical stress as the lithium ions disrupt the silicon structure. After the first cycle, the crystalline structure of the nanowires typically becomes amorphous, making the nanowires more flexible and able to accommodate volume changes without exhibiting cracks.

[0007] When silicon nanowires are grown directly on the surface of graphite particles, each nanowire is free to expand and contract while remaining attached at one end, at which point the nanowire attaches to and makes electrical contact with the surface of the graphite particle. When lithiated, the alloy formed by the combination of lithium and silicon atoms greatly increases the conductivity, allowing efficient exchange of electrons with the graphite matrix along each nanowire. Many nanowires attached to the surface of each graphite particle can expand and contract within the pores between the graphite particles while remaining electrically connected to the carbon-based matrix at their respective attachment points. As in conventional anodes, the graphite particles are in electrical contact with each other in a pore structure that includes a binder and conductive additives. Thus, the porous anode layer consists of adjacent graphite particles (each particle connected to many Si nanowires) that allow both the flow of lithium ions to and from the nanowires through the electrolyte, and the flow of electrons to and from the nanowires through the graphite particles and ultimately to the current collector foil of the anode electrode. Because each nanowire is attached at one end to the graphite substrate, the nanowires do not need to make direct electrical contact with each other, and electrons follow an electrical path from each nanowire, through its attachment at the surface of the graphite particle, through the graphite particle, and to the electrode current collector. Thus, each nanowire is free to bend and change shape during cycling without affecting the electrical connectivity or mechanical integrity of the anode composite layer.

[0008] Producing well-controlled Si nanowires in large quantities has proven to be complex and difficult, and currently no large-scale manufacturing process or equipment is available for commercial production. A CVD batch of 1 kg Si nanowires grown on graphite particles with a 10% Si / C ratio would yield roughly 100 grams or 10 5 Contains milligrams of silicon nanowires, typically exceeding 100 billion per milligram (i.e., 10 11The nanowires contain more than 100,000 metric tons of anode active material for LIBs. Thus, the meaningful benefits of Si nanowires as anode active material for LIBs have not yet been fully realized. This is of significant concern, especially since the global demand for anode active material for LIBs is expected to exceed 100,000 metric tons in 2019, up from 60,000 metric tons in 2015 (Estimate from Avicenne ENERGY - "The worldwide rechargeable battery market" - July 2015). Today, such demand is mostly satisfied by various kinds of natural or synthetic graphite materials. In some commercial LIBs, the anode is made of silicon oxide (SiO x ) and other silicon additives in small proportions. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] US Patent Application Publication No. 2015 / 0086871 [Patent Document 2] US Patent Application Publication No. 2010 / 0297502 Summary of the Invention [Problem to be solved by the invention]

[0010] The availability and cost of Si nanowire composites suitable as anode materials for LIBs are limited by production methods capable of producing less than one metric ton per year, with small yields and high unit costs. Thus, there is a great need for methods to produce high-quality Si nanowire materials for use in LIB components and devices in much larger annual quantities, within narrow manufacturing specifications, and at costs suitable to address the fast-growing demand on the order of tens to thousands of metric tons per year per manufacturing facility. The present invention provides for the fabrication of industrial quantities of materials comprising silicon nanowires attached at one end to the surface of graphite particles, according to an efficient, automated process, within precise specifications, and at an acceptable cost. [Means for solving the problem]

[0011] Embodiments of the present invention generally relate to manufacturing apparatus, systems, and methods for making silicon (Si) nanowires suitable for use as anode active materials in lithium-ion batteries. In some embodiments, manufacturing apparatus, systems, and methods are provided for growing Si nanowires on graphite or carbon powders using a chemical vapor deposition (CVD) process for industrial-scale production.

[0012] In one aspect, embodiments of the present application provide a tumbler reactor and chemical vapor deposition (CVD) system of the present invention configured to grow silicon nanowires on carbon-based substrates, such as graphite particles or powder, in large-scale quantities. The apparatus and methods of the present application can be used to provide industrial-scale anode materials to the LIB industry. For purposes of this application, the terms tumbler reactor and tumbler are used interchangeably.

[0013] In one aspect, a method for producing silicon nanowires is provided, in which silicon nanowires are grown on a carbon-based substrate by chemical vapor deposition of a silicon-containing precursor to form a carbon-based silicon nanowire composite, the conversion of the silicon-containing precursor to silicon nanowires being at least 30%. In other embodiments, the conversion is at least 50%, preferably at least 70%, preferably at least 90%, or even greater than 98%, and at least 1 kg of composite of silicon nanowires and carbon-based substrate can be produced per batch, preferably in batches of more than 10 kg each, or even in batches of more than 20 kg each, with the mass of silicon being at least 4% by weight of such composite (wherein weight percentage is the ratio of the weight of silicon to the carbon substrate), and preferably with a weight ratio of silicon to carbon of more than 8% by weight, or even greater than 16%. It should be noted that the term "carbon-based silicon nanowire composite" may also be referred to as "carbon-based silicon nanowire composite powder" or simply "carbon-silicon composite", and these terms are used interchangeably.

[0014] In another aspect, the carbon-based silicon nanowire composite is further processed to form an anode by coating an electrode foil by techniques known in the art, hi another embodiment, the anode is further combined with a cathode, a separator, and an electrolyte to form a lithium ion battery.

[0015] As described in more detail in the description provided below, embodiments of the apparatus and system of the present invention include one or more of the following features: A low pressure CVD system (LPCVD) is configured, modified, and / or adapted to enable faster cooling and heating of the CVD chamber. The LPCVD system may be configured to move the furnace heating / cooling unit that heats and cools the process tube and tumbler reactor away from the chamber to increase furnace utilization efficiency. In some embodiments, wheeled dolly rails are provided and configured to move the tumbler reactor in and out of the metal or quartz process tube. The dolly rails may be configured to support the tumbler reactor when it is heavy for large inputs of carbon-based silicon nanowire composites. In another embodiment, the tumbler reactor may be maintained in a fixed position relative to the furnace assembly and the cooling and heating elements may be moved along the same axis as the axis of the tumbler. In some embodiments, a metal process tube is used, thereby replacing the quartz process tube, to enable heavier powder material input to the tumbler reactor, which allows for larger Si nanowire production yields. In some embodiments, the apparatus of the present application is configured to provide carbon-based silicon nanowire composites at production rates of up to hundreds or even thousands of metric tons per year. The ability to produce at such a scale is a significant advantage over previous manufacturing techniques, and the greater production rates provided by the apparatus and systems of the present invention will enable the widespread adoption of carbon-based silicon nanowire composites as anode materials for the battery industry.

[0016] In some embodiments, the LPCVD system of the present application incorporates a tumbler reactor with a rotation and mixing mechanism. In some embodiments, the rotation and mixing mechanism is coupled to a gas manifold, and optionally coupled to one or more scrapers. The gas manifold can be of several configurations to manage gas distribution through the tumbler reactor. For example, the gas manifold can be a single elongated member, a U-shaped, or a frame manifold. Optionally, the gas manifold can be combined with one or more scrapers. Optionally, the tumbler can be cylindrical, and its cross section can be circular or polygonal. The tumbler can be one of multiple batch chambers of similar length, or a series of chambers arranged in a spiral. In the case of a spiral configuration, a rotating spiral can push the substrate material forward through a series of one or more heating, reaction, and cooling zones, with the injection of reaction gases being directed toward the reaction zone, where silane is converted into silicon nanowires. The tumbler may be positioned horizontally, vertically, or at any angle relative to the floor on which the furnace is located.

[0017] In some embodiments, the tumbler further comprises one or more fins mounted on one or more inner walls of the tumbler reactor. The fins may be of any suitable size, shape, or distribution and are configured to provide control and / or distribution of powder movement in the tumbler, particularly during injection of process gases. For example, the fins may be configured to prevent graphite or carbon-based powder from sliding along the walls during rotation of the tumbler reactor. The fins may help lift the loaded graphite powder as the tumbler reactor rotates and may optionally optimize the precursor gas and heat distribution within the reactor.

[0018] In another aspect, embodiments of the present application provide systems and methods adapted to produce silicon nanowires in a variety of different types of natural or synthetic graphite particles to provide versatile and stable manufacturing. For example, the graphite particles may have low BET (less than 5 m2 / g) or high BET (greater than 15 m2 / g), can be coated or uncoated, can be spherical or flake-like, or any combination thereof.

[0019] Additional features and advantages of the present invention, as well as the structure and operation of various embodiments of the present invention, are described in more detail below with reference to the accompanying drawings. It is noted that the present invention is not limited to the specific embodiments described herein. Such embodiments are presented herein for illustrative purposes only. Additional embodiments will be apparent to those skilled in the art based on the teachings contained herein.

[0020] The accompanying drawings, which are incorporated herein and form a part of this specification, illustrate the invention and, together with the description, serve to further explain the principles of the invention and to enable a person skilled in the art to make and use the invention. Embodiments of the invention are described, by way of example only, with reference to the accompanying drawings, in which: [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a cross-sectional partial view of a tumbler reactor and LPCVD system according to some embodiments of the present application. [Figure 2A] 1 is a cross-sectional partial view of a tumbler reactor and LPCVD system configuration according to some embodiments of the present application. FIG. [Figure 2B] 1 is a cross-sectional partial view of a tumbler reactor and LPCVD system configuration according to some embodiments of the present application. FIG. [Figure 3A] FIG. 1 is a partial cross-sectional view of a tumbler reactor according to some embodiments of the present application. [Figure 3B] FIG. 2 is an end view of a tumbler reactor according to some embodiments of the present application. [Figure 3C]FIG. 2 is an end view of a tumbler reactor according to some embodiments of the present application. [Figure 3D] FIG. 2 is a bottom cutaway view of a tumbler reactor according to some embodiments of the present application. [Figure 4A] 1A-1D are end views of a tumbler reactor illustrating various configurations of fins on the inner wall of the tumbler reactor according to some embodiments of the present application. [Figure 4B] 1A-1D are end views of a tumbler reactor illustrating various configurations of fins on the inner wall of the tumbler reactor according to some embodiments of the present application. [Figure 4C] 1A-1D are end views of a tumbler reactor illustrating various configurations of fins on the inner wall of the tumbler reactor according to some embodiments of the present application. [Diagram 5] FIG. 1 is a cross-sectional partial view of a LPCVD system with two tumbler reactors according to some embodiments of the present application. [Figure 6] 1 is a process flow diagram illustrating a method for making Si nanowires according to some embodiments of the present application. [Figure 7] FIG. 2 is a cross-sectional partial view of an alternative embodiment of an LPCVD system configured for semi-continuous manufacturing processes, according to some embodiments of the present application. [Figure 8] 1 is a cross-sectional partial view of an alternative embodiment of an LPCVD system having a spiral chamber configured for continuous manufacturing processes, in accordance with some embodiments of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The features and advantages of the present invention will become more apparent from the detailed description set forth below when taken in conjunction with the drawings, in which like reference numbers identify corresponding elements throughout and in which like reference numbers generally indicate identical, functionally similar, and / or structurally similar elements.

[0023] Embodiments of the present application generally relate to manufacturing apparatus, systems, and methods for making silicon (Si) nanowires suitable for use as an active material of anodes in lithium-ion batteries (LIBs). In some embodiments, manufacturing apparatus, systems, and methods configured to grow Si nanowires by chemical vapor deposition on carbon-based substrates, such as graphite particles or any carbon-containing powder, are provided to generate increased production yields.

[0024] For context, we would like to point out that as silicon (Si) has attracted more attention as a potential replacement for graphite (C) in the anodes of LIBs, some limitations have persisted. An atom of Si can combine with a much larger number of lithium ions than an atom of C. Replacing C with Si can substantially increase the energy density of the battery (theoretical capacity for graphite C is 372 mAh / g, while the alloy phase Li 22 S 5 The theoretical capacity for Si is 4,200 mAh / g when combined with Li in LIBs. However, using conventional bulk silicon (e.g., Si powder or Si particles) in LIBs has side effects that prevent it from being an ideal anode material. First, poor cycling durability of silicon material occurs as a result of pulverization during the large volume fluctuations (>300%) that accompany lithium ion insertion and extraction into and from the silicon host material. Second, significant irreversible capacity loss and low Coulombic efficiency occurs due to mechanical destruction of the Si anode during the alloying / dealloying process. Finally, the solid electrolyte interphase (SEI) breaks during cycling, exposing the electrolyte to the highly electrochemically active silicon surface. This leads to re-exposure of the silicon surface to the electrolyte and further reformation of the SEI, which causes the SEI layer to grow thicker through many charge / discharge cycles.

[0025] The inventors have found that the use of Si nanowires grown and / or deposited on graphite as the anode active material in LIBs preserves the superior energy density of Si compared to C while avoiding the side effects of conventional bulk Si. The Si nanowires grown and deposited on graphite can have an average diameter of less than about 200 nm, e.g., between about 5 nm and about 100 nm, e.g., between 30 nm and about 50 nm. The size of the Si nanowires is determined by the size of the catalyst nanoparticles, e.g., Cu. 2The size of the O nanoparticles ranges from 5 nm to 200 nm, and the Si nanowires exhibit aspect ratios (ratio of length to width) of 5, 10, 15 or more, 25 or more, 50 or more, and greater than 100. The length of the Si nanowires is determined by the growth time, temperature, pressure, gas flow rate, catalyst activity, and density at the graphite powder surface. When the temperature, pressure, gas flow rate, and catalyst / density of the growth process are selected, the growth time mainly controls the Si nanowire length. In this way, Si nanowires can be said to be one-dimensional (1-D) materials because their length is much larger than the radial dimension. The shape and geometry of the Si nanowires facilitate the rapid diffusion of lithium ions and mitigate side reactions between the Si nanowires and the electrolyte when used in LIBs. When Si is lithiated, the structure of the Si nanowires is transformed from a substantially crystalline to a substantially amorphous structure, and thus the Si nanowires become more flexible and can self-organize to better fill the available space between the graphite particles more efficiently. During the first few iterations of an electrochemical cell with Si nanowires attached to graphite particles as the anode active material, the battery manufacturer typically sets the voltage range to a value less than the full operating range of the battery and the current to a value less than the maximum rated current specified in the cell data sheet. This approach, typically called the "formation protocol," allows for careful construction of the SEI layer on each silicon nanowire during the first few lithiation iterations performed by the battery manufacturer. After the SEI layer is formed, the nanowires are protected from bonding and / or fusing with neighboring nanowires and can therefore bend and change shape more easily while remaining attached at one end to the surface of the graphite substrate. Furthermore, the inventors have found that after the first SEI formation iteration, the silicon nanowires progressively adjust their shape and position along neighboring silicon nanowires attached to the same graphite particle or adjacent graphite particles by remaining flexible and free to expand and contract during each iteration. This gradual self-arrangement of the SEI-coated silicon nanowires results in efficient and optimal use of the volume provided by the pores between the graphite particles to which the nanowires are attached.Typically, the silicon nanowires occupy a small portion of the surface of the carbon-based substrate, for example, the area where the silicon nanowires are attached corresponds to less than 5% or even less than 1% of the surface of the graphite particle. Therefore, it is not necessary to form or secure direct electrical contacts between adjacent nanowires along their length, since each nanowire is electrically connected to the carbon-based substrate at the attachment point. In fact, it is preferable to avoid fusing adjacent nanowires together, in order to allow each nanowire to flexibly change shape during the repetition. In essence, the Si nanowires attached to the graphite particles become like a sponge-like material that occupies the pore space of the graphite substrate while significantly restricting the expansion of the electrode. The mechanical and electrical integrity of the anode layer is provided by the interconnected network of graphite particles, held together with a binder and optional conductive additives as in conventional graphite-only anodes, and the sponge-like collection of silicon nanowires located within the pores of the graphite particles allows the flow of electrons through the graphite particles to the current collector foil while absorbing and releasing lithium ions. Also, when the silicon is substantially amorphous and the nanowires remain intact, the conduction of electrons along the nanowires is excellent. We have found that the nanowires remain attached to the graphite particles at one end and remain free to bend along their axis over hundreds and even thousands of cycles. Electrons can travel very quickly in and out of the layer of carbon-based pores that are typically attached to a copper current collector for a binder. This composite Si / C material, SEI formation process, and anode layer configuration can allow LIBs to have higher energy density and handle higher power with better capacity retention through charge-discharge cycles compared to conventional LIBs with graphite-only active anode materials or other silicon-containing anode materials.

[0026] The Si nanowires grown on the graphite particles can be sieved using existing roll-to-roll battery electrode coating manufacturing equipment into powders that can be used in slurries. The Si nanowires exhibit aspect ratios (ratio of length to width) of 5, 10, 15 or more, 25 or more, 50 or more, and greater than 100. Thus, Si nanowires can be described as one-dimensional (1-D) materials because their length is much larger than their lateral dimensions. Carbon nanotubes (CNTs) with Si nanoparticles on their surfaces are also 1-D materials and have been described as a potential replacement for Si nanowires as the active material of anodes in LIBs. However, the Si nanoparticles in CNTs have a specific surface area that is much larger than that of Si nanowires. This feature makes the physical structure and unique chemical and electrical properties of Si nanowires substantially different (and better) from those of CNTs with Si nanoparticles when used as the active anode material of anodes in LIBs.

[0027] For example, while the elements are the same (silicon and carbon) for the Si nanoparticles in CNTs and for the Si nanowires grown on carbon (graphite) powder, the two structures exhibit very different properties and performance. In the case of Si nanowires, the carbon (graphite) is simply the substrate to which the nanowires are attached. Unlike CNTs with Si particles on the surface, Si nanowires have a specific surface area that remains roughly constant as their length is increased (i.e., as more silicon atoms are attached), whereas increasing the number of silicon nanoparticles increases the specific surface area. This unique shape / physical property produces several benefits, as described below.

[0028] In LIBs, lithium ions migrate from the cathode to the anode and back through the electrolyte during each charge and discharge cycle. When Si nanowires are used as the active anode material in LIBs, silicon can be very active electrochemically when in direct contact with the electrolyte, producing side reactions (and by-products) that result in an SEI layer around the Si nanowires. The formation of the SEI layer around the Si nanowires during the first few cycles provides more electrochemically passive protection, preventing further silicon-electrolyte reactions, while still allowing lithium ions to diffuse through the SEI. Unlike the larger specific surface area of ​​Si nanoparticles, Si nanowires have a smaller specific surface area for an equivalent Si mass. Thus, a smaller SEI needs to be formed to passivate the surface of the Si nanowires than that of silicon nanoparticles in CNTs. Thus, the electrolyte-silicon side reaction in silicon nanowires consumes less electrolyte during SEI formation and produces a more stable SEI layer around the Si nanowires, helping to retain the reversible capacity through more cycles.

[0029] The inventors have found that while lithium ions can be rapidly lithiated and diffused in the Si nanowires, they also intercalate into the graphite particles. Thus, both the silicon in the nanowires and the carbon in the matrix participate in the lithium storage and electron flow. When fully lithiated, the percentage of lithium stored in the nanowires relative to that stored in the graphite particles is related to the weight ratio Si / C in the composite active material. At higher Si / C ratios, a smaller amount of lithium is stored in the carbon structure and a larger amount of lithium is stored in the silicon nanostructures. Thus, at higher Si / C ratios, cheaper graphite with a larger BET can be used to accommodate a larger number of Si nanowires, since the main function of graphite is not to store lithium but to provide a path for electrons to flow from the nanowires to the current collector. The larger the surface area of ​​each particle, the more nanowires can be accommodated without increasing the nanowire surface density on the surface of each particle. The hybrid solution, combining silicon nanowires grown on graphite particles, uniquely exploits the energy storage properties of silicon and the mechanical and electrical characteristics of carbon-based active materials.

[0030] All these properties, shape, electrochemical activity, electronic conductivity, and mechanical strength are unique to one-dimensional arrangements of Si nanowires attached to carbon-based particles at their bases and not along their lengths. The inventors have discovered that the combination of these properties makes Si nanowires grown on carbon-based particles a unique material for batteries, including LIBs, and have invented the CVD equipment designs and processes required to economically manufacture this novel material on a large scale.

[0031] Although the inventors have found that Si nanowires in carbon substrates are particularly valuable as a material for batteries, the production of Si nanowires on an industrial scale has proven very difficult and has not yet been achieved. Accordingly, this application describes novel manufacturing apparatus, systems, and methods for making silicon (Si) nanowires on an industrial scale suitable for use as the active material of the anode in lithium-ion batteries.

[0032] According to some embodiments, the powder of carbon-based substrate used in the tumbler reactor and system of the present application may be composed of any one or more of natural graphite, artificial graphite, soft carbon, hard carbon, and amorphous carbon. Such powder of carbon-based substrate may have a diameter of approximately 1 to 30 mm. 2 / g range, and more preferably, for larger Si weight percent nanowire growth, approximately 5-30 m 2 / g and has a tap density of 0.01 to 1.5 g / cc. It is important to note that the BET values ​​mentioned above are the opposite, typically with a BET surface area of ​​2 m 2 The present invention does not teach current conventional high performance graphite anode materials that require less than 1 / g / g. The carbon-based substrate powders of the present application can be modified by their surface coatings, such as carbon coatings, by decomposing organic compounds such as acetylene, methane, carbon monoxide, sugars, and polymers such as CMC, PVDF, PAA, PVA, polymer blends, and the like.

[0033] Au, Cu, or Cu 2 Catalyst nanoparticles such as O are deposited on the surface of the powder of carbon-based substrate to catalyze the decomposition of silane for Si nanowire growth. The Au catalyst has a gas-liquid-solid (VLS) nanowire growth mechanism, whereas Cu or Cu 2O has a gas-solid-solid (VSS) nanowire growth mechanism, which allows for the growth of much larger Si wt % nanowires on carbon-based substrates, as described in more detail in U.S. Patent Application Publication No. 2015 / 0086871 and U.S. Patent Application Publication No. 2010 / 0297502, the disclosures of which are incorporated herein by reference in their entireties.

[0034] The fabrication of Si nanowire anode materials is based on the inventive industrial-scale combined fixed-bed and fluidized-bed reactor design and system as described herein, which can be loaded with graphite powder in each batch at large scale, e.g., 0.5 kg, 1 kg, 1.5 kg, 2 kg, and 2.5 kg to 5 kg, 10 kg, 100 kg, or 500 kg, to fabricate Si nanowire-graphite composites with more than 4 wt.% Si. The size of a "batch" is understood to mean the weight of silicon-carbon composite powder produced in a single reaction chamber during the "growth step" of the process. In a continuous process, the size of a "batch" is the weight of silicon-carbon composite powder produced per hour in a single processing device. An important advantage is that the tumbler reactor and CVD system of the present application are highly scalable. In some embodiments, the tumbler reactor can produce at least 1 kg of Si nanowires on graphite powder per batch (1 kg / batch). In some embodiments, the tumbler reactor produces at least 10 kg of Si nanowires on graphite powder per batch (10 kg / batch), or at least 100 kg of Si nanowires on graphite powder per batch (100 kg / batch).

[0035] Among other advantages, the systems and methods of manufacture of the present application achieve utilization or conversion of Si feedstock (e.g., silane) to Si nanowires approaching 100%. In some embodiments, utilization of Si feedstock ranges from about 30-100%, or from 30-99.5%, and more typically from about 70-99.5%. In one exemplary embodiment, Si nanowires can be fabricated under the following conditions: temperature of about 300-900° C., about 5-100% by weight of SiH 4 , about 0 to 50% by weight of He (or Ar or N 2 ), and about 0-50 wt.% H 2 Silane is grown in the system described herein using a silane concentration of about 5-100% in the process gas mixture, and growth times in the range of 10-500 minutes. The aforementioned conditions and tumbler rotation are preferably controlled by a computer with production automation software.

[0036] In another aspect, embodiments of the tumbler reactor, system, and method provide surface density control that allows selective formation of varying weight percent Si in carbon powder. 2 The larger BET surface area graphite powder combined with the use of O increases the Si nanowire surface density (simply, Si% / m 2 ) is about 1 to 30 m 2 The growth of uniform Si nanowires can be controlled on suitable graphite substrates with BET surface areas in the range of 5 m / g, allowing for uniform Si nanowire growth of 35 wt. % or more of Si. For example, if one gram of powder is taken, the growth of Si nanowires can be controlled on suitable graphite substrates with BET surface areas in the range of 5 m / g. 2 8 wt % Si nanowires in 5m graphite (e.g., graphite is available from Hitachi) yields 8 wt % Si / 5m 2 =1.6wt%Si / m 2 This has a nanowire surface density of 20m 2 32 wt. % Si nanowires in KS6 type graphite with a surface area of ​​32 wt. % Si / 20 m 2 =1.6wt%Si / m 2 The length and diameter of the Si nanowire are equal to 5 m.2 8 wt% Si nanowires in graphite at 20 m / g 2 % Si nanowires in 1000 / g graphite, the number of Si nanowires per square meter of substrate surface will be similar. The inventors first discovered such surface density control, which allows 32% Si anode material to be repeated in a cell, and 8% Si anode material to be repeated in a cell, because the volume expansion of the Si nanowires during lithiation can be accommodated by more void space between the graphite particles in the anode composite layer.

[0037] Turning now to the figures, there is shown an embodiment of the present application illustrating a tumbler reactor and chemical vapor deposition (CVD) system of the present invention configured to grow silicon nanowires on graphite or carbon-based powders in large quantities.

[0038] Referring to FIG. 1, a low pressure CVD (LPCVD) system 100 is shown, which generally consists of an elongated CVD chamber 102, a process tube 104, and a tumbler reactor 106. The CVD chamber 102 includes heating elements 108 and 110, which are typically controlled by a processing unit 128, to heat and cool the process tube 104 and the tumbler reactor 106 according to a particular process recipe. In this embodiment, the process tube 104 is an elongated cylindrical tube formed from quartz and is positioned inside the CVD chamber 102. During operation, the process tube 104 is kept under vacuum. A purge gas, typically nitrogen, is injected into the process tube by a vacuum port 112, and an exhaust port 114, connected to a vacuum pump and cyclone (not shown), is provided at the output end of the process tube 104 to provide a low pressure environment.

[0039] The tumbler reactor 106 consists of an elongated cylindrical metal chamber and is positioned inside the process tube 104. The tumbler reactor 106 is configured to rotate inside the process tube. An electric motor 120 drives the rotation of the tumbler 106 via a rotating gear 115.

[0040] The tumbler reactor 106 includes a gas manifold 116 for injecting process gas into the reactor. Any suitable silicon-containing process gas may be injected through the gas manifold 116. In some embodiments, silane combined with one or more inert gases, such as nitrogen, helium, argon, and / or hydrogen, is injected into the tumbler reactor 106 through the gas manifold 116. In some embodiments, the gas manifold 116 consists of a single elongated gas injection member 117 that extends through at least a portion or a substantial length of the tumbler reactor 106. In some embodiments, a plurality of injection ports 119 are positioned along the gas injection member 117 for injecting process gas into the tumbler reactor 106. Preferably, the injection ports are substantially evenly distributed along the gas injection member to provide a substantially uniform distribution of the process gas within the tumbler reactor. In some embodiments, the gas injection member 117 is stationary. Alternatively, the gas injection member 117 may rotate. A portion of the process gas is injected into the tumbler reactor 106 through gas purge piping 112 .

[0041] Optionally, the tumbler reactor 106 further comprises one or more scrapers 113. The scrapers 113 are configured to scrape at least a portion of the inner wall of the tumbler reactor 106 to prevent accumulation of powder on the inner wall. In some embodiments, the scrapers 113 are positioned at one or more of the ends of the tumbler reactor to scrape powder from the outer periphery of the tumbler reactor. In another embodiment, the scrapers 113 may consist of elongated blades that extend over at least a portion or a substantial length of the tumbler reactor 106 to scrape powder accumulated along the inner wall. In yet another embodiment, the scrapers 113 may be integrated with the gas manifold 116.

[0042] In the exemplary embodiment shown in FIG. 1, scraper 113 is attached to gas injection member 117 by mounting members 121a and 121b, which are fixed to feedthroughs in flanges 122a and 122b located at either end of gas injection member 117. The flanges can be fixed and vacuum sealed, so scraper 113 is also stationary. In this embodiment, the scraper remains stationary while tumbler reactor 106 rotates. Alternatively, scraper 113 may be configured to rotate. In the exemplary embodiment, scraper 113 comprises an elongated blade 124, the outer side of which scrapes powder from the inner wall of tumbler reactor 106 during tumbler rotation. Alternatively, the elongated blade 124 may comprise a brush-like member 125 positioned along a portion or substantial length of the exterior of the blade 124 such that the brush-like member 125 scrapes powder off the interior walls of the tumbler reactor 106 during tumbler rotation.

[0043] Referring to FIG. 2A, another embodiment of a low pressure CVD (LPCVD) system 200 is shown, generally consisting of an elongated CVD chamber 202, a process tube 204, and a tumbler reactor 206. The CVD chamber 202 includes heating elements 208 and 210 controlled by a processing unit 228 to heat the CVD chamber according to a particular process recipe. In this embodiment, the process tube 204 is an elongated cylindrical tube formed from metal. The process tube 204 is exhausted by a purge gas through a port 212 to provide a low pressure environment. The process tube 204 is exhausted by an exhaust port 214 positioned at the output end of the process tube 204 and connected to a vacuum pump and cyclone (not shown). The tumbler reactor 206 is configured to rotate inside the process tube 204. An electric motor 220 drives the rotation of the tumbler reactor 206 through a rotating gear 215.

[0044] To increase throughput and reduce processing time between cycles, the LPCVD system 200 is adapted to allow for more rapid cooling and heating of the process tube 204 and tumbler reactor 206. In this embodiment, the tumbler reactor 206 is configured to be removed from the CVD chamber 202. In this manner, the tumbler reactor 206 and process tube 204 can be removed from the CVD chamber 202 and cooled upon completion of processing while another tumbler reactor and process tube is placed in the CVD chamber. This configuration allows for more rapid processing since the CVD chamber does not need to be cooled and then heated for each batch, thereby increasing system utilization.

[0045] In this embodiment, the CVD system 200 further comprises a carriage rail 221 with wheels 222 configured to slide the tumbler reactor 206 in and out of the process tube 204 and to support the tumbler reactor 206. The carriage rail allows the tumbler reactor 206 to slide in and out of the metal process tube 204. The carriage rail also supports the tumbler reactor 206 when it is heavy with powder. In some embodiments, a metal process tube 204 is used, thereby replacing a quartz process tube, allowing heavier powder material to be loaded into the tumbler reactor 206, which provides increased production of Si nanowires. In an alternative embodiment, the tumbler reactor 206 and process tube 204 are configured to slide in and out of the CVD chamber 202.

[0046] The tumbler reactor 206 includes a gas manifold 216 for injecting process gas into the reactor. In some embodiments, the gas manifold 216 consists of a single elongated gas injection member that extends across a substantial length of the tumbler reactor 206. In an exemplary embodiment, the gas manifold consists of a U-shaped gas injection member 217. In some embodiments, a plurality of injection ports 219 are positioned along the U-shaped gas injection member 217 for injecting process gas into the tumbler reactor 206. Preferably, the injection ports are substantially evenly distributed along the gas injection member to provide a substantially uniform distribution of process gas within the tumbler reactor. In some embodiments, the U-shaped gas injection member 217 is stationary. Alternatively, the U-shaped gas injection member 217 may rotate.

[0047] The tumbler reactor 206 further comprises one or more scrapers 213 as described above in relation to FIG. 1. The scrapers 213 are configured to scrape at least a portion of the inner wall of the tumbler reactor 206 to prevent accumulation of powder on the inner wall. In some embodiments, the scrapers 213 are positioned at one or both ends of the tumbler reactor to scrape powder from the outer periphery. Alternatively, the scrapers 213 may consist of elongated blades that extend over a substantial length of the tumbler reactor 206 to scrape powder accumulated along the inner wall. In yet another embodiment, the scrapers 213 may be integrated with the U-shaped gas manifold 216.

[0048] In the exemplary embodiment shown in FIG. 2A, the scraper 213 is attached to the gas injection member 217 by mounting members 223a and 223b fixed to either end of the U-shaped gas injection member 217. In this embodiment, the U-shaped gas injection member 217 and scraper 213 remain fixed while the tumbler reactor 206 rotates. Alternatively, the U-shaped gas injection member and scraper may be configured to rotate. In the exemplary embodiment, the scraper 213 consists of an elongated blade 224 with a brush-like member 225 positioned along an outer portion or substantial length of the blade 224 such that the brush-like member 225 scrapes powder off the inner wall of the tumbler reactor 206 during rotation.

[0049] An alternative embodiment is shown in FIG. 2B, in which the CVD chamber 202 is moved away from the process tube 204 and the tumbler reactor 206, generally as indicated by the direction of the arrow in FIG. 2B, to increase throughput and reduce processing time between cycles. In this manner, the CVD chamber 202 with the heating elements 108, 110 is pulled away from the tumbler reactor 206 and the process tube 204 when processing is completed, so that another tumbler reactor and process tube can be received for further processing. This configuration allows for faster processing since the CVD chamber does not need to be cooled and then heated for each batch, thereby increasing the utilization efficiency of the system. To move the CVD chamber 202, a dolly rail 226 with wheels 227 is positioned to carry and slide the CVD chamber 202 away from the process tube 204 and the tumbler reactor 206.

[0050] 3A-3D depict various views of one embodiment of a tumbler reactor 300. More specifically, FIG. 3A shows a partial cross-sectional view of an exemplary tumbler reactor 300, FIGS. 3B and 3C show partial end views of the tumbler reactor 300, and FIG. 3D shows a partial bottom cutaway view of the tumbler reactor 300. In this embodiment, the tumbler reactor 300 comprises an elongated cylindrical tube 303 having a first end 301 and a second end 302. Both ends 301 and 302 are generally comprised of a mesh end cap 304 and an end plate 306. The end plate 306 has a toothed outer edge 305 that extends around the entire circumference of the end plate 306 (for simplicity, only a portion of the toothed outer edge is shown in the figures) that acts as a gear to rotate the tumbler reactor 300. The external gear 305 engages with smaller rotating gears 115, 215 (FIGS. 1, 2A, and 2B) coupled to a motor 120 to drive rotation of the tumbler reactor 300. A frame 308 (FIG. 3B) may be provided to secure the mesh end caps and end plates via mounting bolts 307. The frame 308 includes openings configured to receive various components, such as, for example, the injection manifolds 116, 216.

[0051] A particular advantage is that the mesh end cap 304 comprises a mesh having a plurality of openings 309 sized to contain the graphite powder inside the tumbler reactor and prevent the flow of graphite powder into the process tube while permitting the flow of process gases, purge gases, and other gases between the tumbler reactor and the process tube. The size of the mesh openings 309 in the mesh end cap 304 may vary depending on the size and / or shape of the graphite powder being fed into the tumbler reactor 300. The mesh end cap 304 allows for uniform gas distribution from the gas manifold to the graphite powder inside the tumbler reactor.

[0052] One embodiment of a tumbler reactor 400 is shown in more detail with reference to Figures 4A-4C. The tumbler reactor 400 comprises one or more fins 402 mounted or formed on one or more interior walls 404 of the tumbler reactor 400. The fins 402 can be of any suitable size, shape, or distribution and are configured to provide control and / or distribution of powder movement in the tumbler reactor, particularly during injection of process gases. The fins 402 are configured to prevent the graphite or carbon-based powder from sliding along or clinging to the walls during rotation of the tumbler reactor. The fins can also assist in lifting the loaded graphite powder as the tumbler reactor rotates. In some embodiments, the fins 402 are elongated lips protruding from the surface of the interior wall. The height of the fins 402 can vary depending on the type of graphite powder used, among other factors. In some embodiments, the height of the fins 402 ranges from about 0.05 to 50 mm. The height of each of the fins 402 may be uniform, or alternatively, the height of one or more of the fins 402 may vary.

[0053] The fins 402 may have a rectangular shape as shown in Figure 4A or a triangular shape as shown in Figure 4B, among other shapes. In Figure 4C, the fins 402 have a curved shape that helps lift the graphite powder as the tumbler reactor rotates. One skilled in the art will recognize that many different shapes can be used, all within the spirit and scope of the present invention.

[0054] To further increase the yield of Si nanowires, a CVD system 500 is disclosed that consists of two or more tumbler reactors 503a and 503b as shown in Figure 5. In this embodiment, the tumbler reactors 503a and 503b are coupled via a flange 504 and rotated together by a rotating gear 506 that is coupled to a rotating electric motor 508. Alternatively, the tumbler reactors 503a and 503b can be independent. The process gas (in this example, silane or N 2 , Ar, H 2, or silane with mixtures with other gases such as He) is injected independently into each of the tumbler reactors through ports 501.

[0055] The process of operation will now be described with reference to Figure 6. In operation, the tumbler reactor rotates inside the process tube and CVD chamber to mix the pre-treated graphite powder fed into the tumbler reactor while silane (SiH) is added to ensure proper conditions to grow Si nanowires on the graphite powder. 4 A process gas such as toluene is injected into the tumbler reactor under controlled pressure and temperature.

[0056] FIG. 6 shows a flow diagram 600 of the outline of the manufacturing process for Si nanowires according to an embodiment of the present application. In step 602, a tumbler reactor is loaded with graphite or carbon powder that has been previously treated by deposition of catalytic particles (Au, Cu, or Cu oxide) and weighted. In step 604, the tumbler reactor is inserted into a process tube and a CVD chamber, and the tumbler reactor and the process tube are heated to a certain temperature. In step 606, Si nanowires are grown by chemical vapor deposition. After the growth of silicon nanowires, in step 608, the tumbler is removed from the CVD chamber and cooled. In step 610, the formed graphite powder with Si nanowires is removed.

[0057] FIG. 7 shows a cross-sectional partial view of an alternative embodiment of an LPCVD system 700 in which three tumblers 706a, 706b, and 706c are processed in a semi-continuous manufacturing process. Each tumbler reactor is loaded with graphite powder with catalyst deposited on the graphite, inserted at one end of the LPCVD system, processed through a sequence of three active zones consisting of a heating zone 701, a reaction zone 703, and a cooling zone 705, and then withdrawn from the opposite end of the LPCVD system. The three active zones are separated from each other by two buffer zones 702 and 704 that allow the transition of each tumbler from the active zone to the next controlled conditions of pressure and temperature. In the pre-heat zone 701, tumbler 706a is heated to reach specific temperature and pressure conditions before moving through the buffer zone 702 to the reaction zone 703. In the reaction zone 703, graphite powder contained in tumbler reactor 706b mixes with silicon-containing process gas to grow silicon nanowires on the graphite powder before transitioning to the cooling zone 705. In the cooling zone 705, the carbon-based silicon nanowire composite powder contained in tumbler 706c is cooled before the tumbler is withdrawn to remove the powder. Each time the tumbler moves from one active zone to the next, a new tumbler loaded with catalyst-containing carbon-based powder is inserted into the preheat zone to start the process again, with fully formed nanowires growing on the carbon-based powder and the attached tumbler withdrawn from the cooling zone ready to be removed. This configuration ensures a semi-continuous manufacturing process where at any one time three tumblers are always present in each of the three active zones 701, 703, and 705. An advantage of this configuration is that the reaction region 703 grows nanowires continuously in the tumbler without interruption, except for the intermittent transition of the tumbler from one active region to the next. This configuration may be expanded to include N active regions separated from each other by N-1 buffer regions, where N is greater than 3.

[0058] 8 shows a cross-sectional partial view of an alternative embodiment of an LPCVD system 800 in which the tumbler reactor comprises a spiral chamber 802 configured for a continuous manufacturing process. In the spiral configuration, a rotating spiral or auger pushes the substrate powder material forward through a series of one or more heating, reaction, and cooling zones, with an injection of process gases directed toward the reaction zone where silane is converted into silicon nanowires.

[0059] In the illustrated embodiment, the LPCVD system 800 comprises an elongated CVD chamber 802 consisting of at least one preheat region 804, a reaction region 806, and a cooling region 808, and a gas manifold 801 for injecting process gases (and optionally other gases) into the CVD chamber 802. During operation, the chamber 802 is kept under vacuum. A purge gas, typically nitrogen, is injected into the chamber through a vacuum port 810, and an exhaust port 812 connected to a cyclone (not shown) is provided at the output end of the chamber 802 to provide a low pressure environment.

[0060] In some embodiments, the gas manifold 801 consists of an elongated gas injection member 814 that extends through a substantial or full length of the chamber 802. To deliver process gas to the reaction region, the gas injection member 814 includes a plurality of injection ports 815 along the section of the gas injection member 814 positioned in the reaction region 806. Injection of process gas (typically silane, optionally mixed with one or more inert gases such as nitrogen, argon, helium, and / or hydrogen) in the reaction region 806 converts the silane into silicon nanowires grown on the graphite powder. The sections of the gas injection member 814 positioned in the preheat region 804 and the cooling region 808 do not include ports, so process gas is not injected into these regions.

[0061] Graphite powder is fed into the chamber 802 by a graphite injector 816. The graphite powder is preheated to deposit a catalyst on the graphite powder. A rotating helix or auger 803 pushes the graphite powder forward through a preheating region 804, a reaction region 806, and a cooling region 808. The auger 803 may be integral with the gas injection member 814 or, alternatively, may be separate from the gas injection member 814. If the auger 803 and gas injection member 814 are an integral assembly, a gas conduit is formed through the center of the auger to distribute the gas radially. Optionally, scrapers as previously described may be included in one or more of the regions 804, 806, 808 to minimize powder buildup on the interior walls of the chamber 802.

[0062] In one embodiment, when the graphite powder enters the chamber 802, it is dried under vacuum and preheated in a preheating area 804. As the graphite powder travels through the preheating area, the graphite is heated to a certain temperature. The heated graphite powder then exits the preheating area and enters the reaction area. Optionally, the preheating area and the reaction area may be separated by a purge curtain or a separation curtain (not shown) or other suitable means to partially or fully isolate the areas. As the heated graphite powder enters and travels through the reaction area 806, the graphite powder mixes with a silicon-containing process gas to grow silicon nanowires on the graphite powder, forming a carbon-based silicon nanowire composite powder. This silicon nanowire-graphite powder then travels through a cooling area 808 where the powder is cooled. As the powder (now the formed product) passes through the cooling area 808, the powder is continuously removed from the chamber 802 via a product output 818.

[0063] As previously mentioned, the graphite powder moves through the multiple regions by a helical movement driven by the auger 803. Each of the regions 804, 806, 808 may require a different dwell or progression time depending on the processing step being performed in each region. For example, in some embodiments, preheating the graphite powder in the preheating region 804 may require more time than is required to grow silicon nanowires in the reaction region 806. In such an example, control of the dwell or progression time through a particular region is achieved by varying the pitch of the auger 803 in that region, as depicted in FIG. 8, which shows three auger sections 1, 2, and 3. For example, the pitch of the auger may be adjusted to be narrower or wider as needed. Thus, the rate of progression of the graphite powder through each region may be selectively adjusted. Although the three auger sections shown in FIG. 8 are similar in length, this is for simplicity only, and it is understood that the length of the various auger sections can be varied according to the teachings of the present invention. In another embodiment, a semi-continuous batch system and process is provided that can process multiple tumbler reactors in a semi-continuous manner. In one exemplary embodiment, the process tube is elongated and configured to accommodate, for example, four tumbler reactors, with a heating zone, a reaction (growth) zone, and a cooling zone, such that multiple tumbler reactors can undergo processing and can be moved through the process tube from zone to zone, whereby tumblers can be loaded and unloaded at each end of the process tube in a semi-continuous manner.

[0064] In some embodiments, the use of the methods, systems, and reactors for producing carbon-based silicon nanowire composite powders described above are further processed to form an anode. In some embodiments, the anode is formed by coating an electrode foil with the carbon-based silicon nanowire composite powder by coating techniques known in the art. In other embodiments, the anode is further combined with a cathode, a separator, and an electrolyte to form a lithium ion battery.

[0065] Disclosed herein is the combination of lower cost catalyst nanoparticles that enable the growth of silicon nanowires with statistically controlled radial and length dimensions with very high conversion and yield, with lower cost graphite substrate powder in a large CVD volume process, enabling the production of high performance and high energy density active anode materials in large quantities at attractive manufacturing costs.

[0066] The apparatus and methods described herein offer significant advantages over previous manufacturing techniques, and the increased yields provided by the apparatus and systems of the present application will help enable and promote the widespread adoption of Si nanowires grown on graphite or other carbon powders as anode materials in the battery industry.

[0067] Although specific embodiments of the invention have been described above, it will be understood that the invention can be practiced otherwise than as described. The above description is intended to be illustrative and not limiting. Thus, it will be apparent to one skilled in the art that modifications can be made to the invention as described without departing from the scope of the claims set forth hereinafter. [Explanation of symbols]

[0068] 100, 200 Low Pressure CVD (LPCVD) System 102, 202 CVD room 104 Process Tube 106 Tumbler Reactor 108, 110 heating elements 112 Vacuum port, gas purge piping 113 Scraper 114 Exhaust port 115 Rotating Gear 116 Gas manifold 117 Gas injection parts 119 Injection Port 120 Electric Motor 121a, 121b Mounting members 122a, 122b flanges 124 Long and thin blade 125 Brush-like member 200 Low Pressure CVD (LPCVD) System 202 CVD room 204 Process Tube 206 Tumbler Reactor 208, 210 heating elements 212 Port 213 Scraper 214 Exhaust port 215 Rotating Gear 216 Gas manifold 217 U-shaped gas injection member 219 Injection Port 220 Electric Motor 221 Cart Rail 222 Wheels 223a, 223b Mounting members 224 Long and thin blade 225 Brush-like member 226 Cart Rail 227 Wheels 300 Tumbler Reactor 301 First End 302 Second End 303 Long, thin cylindrical tube 304 Mesh end cap 305 Toothed outer edge, external gear 306 End Plate 307 Mounting bolt 308 Frames 400 Tumbler Reactor 402 Fin 404 Interior wall 500 CVD System 503a, 503b Tumbler reactor 504 flange 506 Rotating Gear 508 Electric Motor 700 LPCVD System 701 Heating area, preheating area 702, 704 buffer area 703 Reaction Area 705 Cooling area 706a, 706b, 706c Tumblers 800 LPCVD System 801 Gas Manifold 802 Spiral chamber, CVD chamber 803 Spiral, Ogre 804 Preheating area 806 Reaction Area 808 Cooling area 810 Vacuum Port 812 Exhaust port 814 Gas injection parts 815 Injection port 816 Graphite Injection Equipment 818 Product Output Section

Claims

1. 1. A method for producing a carbon-based silicon nanowire composite, comprising: providing a carbon-based substrate having catalytic nanoparticles deposited thereon; dosing the carbon-based substrate in a plurality of tumbler reactors; inserting the plurality of tumbler reactors into at least one heating zone located at one end of a low pressure CVD system for heating the carbon-based substrate in the plurality of tumbler reactors until the carbon-based substrate reaches a specific temperature, the CVD system including N consecutive active zones separated from each other by N-1 buffer zones, the N active zones comprising the at least one heating zone, at least one reaction zone, and at least one cooling zone, each zone comprising at least one of the plurality of tumbler reactors; growing silicon-containing nanowires from the catalyst nanoparticles deposited on the carbon-based substrate in one or more of the plurality of tumbler reactors located within the at least one reaction zone by a gas-solid-solid synthesis technique; cooling the carbon-based silicon nanowire composite in one or more of the plurality of tumbler reactors located within the at least one cooling zone; intermittently varying the positions of the plurality of tumbler reactors in the low pressure CVD system from the at least one heating zone to the at least one reaction zone and from the at least one reaction zone to the at least one cooling zone, such that, except for the intermittent transitions of the plurality of tumbler reactors from one active zone to the next active zone, one or more of the plurality of tumbler reactors located in at least one reaction zone continuously grows silicon-containing nanowires on the carbon-based substrate; The method, wherein the growing step comprises injecting one or more process gases comprising silane into one or more of the plurality of tumbler reactors located within the at least one reaction zone.

2. The method of claim 1 , wherein the carbon-based substrate comprises at least one of natural graphite particles or synthetic graphite particles.

3. The method of claim 1 , wherein the catalytic nanoparticles comprise copper or copper oxide.

4. 10. The method of claim 1, wherein the growing step further comprises mixing the carbon-based substrate while uniformly injecting one or more process gases into one or more of the plurality of tumbler reactors via injection ports located along an injection member.

5. 4. The method of claim 3, wherein the growing step further comprises controlling the temperature and pressure of one or more process gases by a computer with production automation software.

6. The method of claim 3 , wherein mixing further comprises rotating one or more of the multiple tumbler reactors during the nanowire growth process.

7. 10. The method of claim 1, wherein the carbon-based silicon nanowire composite has a silicon nanowire density with a weight ratio of silicon to carbon of at least 12%.

8. 10. The method of claim 1, wherein the carbon-based silicon nanowire composite has a silicon nanowire density with a weight ratio of silicon to carbon between 16% and 32%.

9. 10. The method of claim 1, wherein one or more process gases comprise a silicon-containing precursor, and wherein the conversion of the silicon-containing precursor to silicon nanowires is greater than 90%.

10. The method of claim 1, further comprising a step of scraping one or more inner walls of the plurality of tumbler reactors located in at least one reaction zone to minimize accumulation of carbon-based substrates on the one or more inner walls of the plurality of tumbler reactors.

11. 1. A method for producing a carbon-based silicon nanowire composite, comprising: providing a carbon-based substrate having catalytic nanoparticles deposited thereon; continuously feeding the carbon-based substrate through a graphite injector into an elongated chamber comprising an auger and a gas injection member, the auger and the gas injection member extending over at least a portion of the length of the elongated chamber, the elongated chamber comprising a plurality of active regions comprising at least one preheating region, at least one reaction region, and at least one cooling region; heating the carbon-based substrate in the one or more preheating zones to a particular temperature; growing silicon-containing nanowires on the carbon-based substrate from the catalyst nanoparticles deposited on the carbon-based substrate in the one or more reaction zones to form a carbon-based silicon nanowire composite by a gas-solid-solid synthesis technique; cooling the carbon-based silicon nanowire composite in one or more cooling zones; and pushing the carbon-based substrate through a series of one or more preheating zones, reaction zones, and cooling zones by rotating the auger; The method, wherein the growing step comprises mixing the carbon-based substrate while injecting one or more process gases including silane through injection ports located along a section of a gas injection member extending through the one or more reaction zones.

12. The method of claim 11 , wherein the carbon-based substrate comprises at least one of natural graphite particles or synthetic graphite particles.

13. The method of claim 11 , wherein the catalytic nanoparticles comprise copper or copper oxide.

14. 12. The method of claim 11 , wherein the growing step further comprises mixing the carbon-based substrate while uniformly injecting one or more process gases through injection ports located along an area of ​​a gas injection member that extends through the one or more reaction zones.

15. 12. The method of claim 11, wherein the carbon-based silicon nanowire composite has a silicon nanowire density with a weight ratio of silicon to carbon of at least 12%.

16. 12. The method of claim 11, wherein the carbon-based silicon nanowire composite has a silicon nanowire density with a weight ratio of silicon to carbon between 16% and 32%.

17. 15. The method of claim 14, wherein one or more process gases comprise a silicon-containing precursor, and the conversion of the silicon-containing precursor to silicon nanowires is greater than 90%.

18. The method of claim 11, further comprising the step of scraping the inner walls of the elongated chamber in one or more of the multiple active regions to minimize accumulation of carbon-based substrates on the inner walls of the elongated chamber.

19. The method of claim 11 , further comprising controlling a travel time of the carbon-based substrate through the plurality of active regions by varying a pitch of a section of an auger extending through the regions.

20. 12. The method of claim 11, wherein the at least one preheat zone and the at least one reaction zone are separated by a separation curtain such that the zones are at least partially separated.

Citation Information

Patent Citations

  • Surface treatment method of powder

    JP1977068886A

  • Rotary kiln

    JP1985053775A

  • Method and apparatus for manufacturing spherical semiconductor element

    JP2004349368A

  • Nanostructured battery active material and method for producing the same

    JP2014532023A

  • Anode material for lithium secondary batteries, method for manufacturing the same, and lithium secondary battery containing the same

    JP2015524149A