Anti-sulfuration coating material, cured product thereof, and electronic device

The anti-sulfuration coating material, composed of specific silicone components without metal powders, addresses durability and sulfidation issues in high-temperature environments, ensuring reliable protection for electronic devices.

JP7581352B2Active Publication Date: 2024-11-12SHIN ETSU CHEMICAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022538658
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-22
Filing Date
2021-06-28
Publication Date
2024-11-12
Estimated Expiration
2041-06-28

AI Technical Summary

Technical Problem

Conventional addition-curing silicone compositions containing metal powders or metal plating powders suffer from reduced durability in high-temperature environments due to cracking and poor curing, leading to insufficient heat resistance and sulfidation resistance.

Method used

An anti-sulfuration coating material comprising linear organopolysiloxane, organohydrogenpolysiloxane, crystalline silica or talc, a hydrosilylation catalyst, and cerium oxide, which does not contain metal powder or metal plating powder, to provide a cured product with excellent heat resistance and sulfidation resistance.

Benefits of technology

The coating material achieves high durability and sulfidation resistance in high-temperature environments, making it suitable for protecting electronic devices, particularly semiconductor elements for optical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581352000001
    Figure 0007581352000001
  • Figure 0007581352000002
    Figure 0007581352000002
  • Figure 0007581352000003
    Figure 0007581352000003
Patent Text Reader

Abstract

The present invention is an anti-sulfurization coating material, the anti-sulfurization coating material being characterized by: containing (A) a straight-chain organopolysiloxane represented by the following general formula (1), (B) an organohydrogen polysiloxane having two or more silicon-atom-bonded hydrogen atoms in a molecule, (C) one or more substances selected from crystalline silica and talc, (D) a straight-chain organopolysiloxane that has one or more phenyl groups and does not have an alkenyl group and a silicon-atom-bonded hydrogen atom in a molecule, (E) a hydrosilylation catalyst containing a platinum group metal, and (F) cerium oxide; and not containing a metal powder or a metal plating powder. It is thereby possible to provide an anti-sulfurization coating material comprising an addition-curable silicone composition that yields a cured product that does not contain a metal powder or a metal plating powder, that has exceptional durability in a high-temperature environment, and that has anti-sulfurization properties.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an anti-sulfuration coating material, a cured product of the anti-sulfuration coating material, and an electronic device encapsulated with the cured product. [Background technology]

[0002] 2. Description of the Related Art Addition-curable silicone rubber compositions containing metal powders such as copper or silver or metal-plated powders have been used as sealing and adhesive materials for preventing corrosion of electronic parts.

[0003] A known method for improving the dispersibility of metal powder is to compound metal powder or metal-plated powder that has been treated with fatty acids or fatty acid derivatives such as fatty acid esters (Patent Documents 1 and 2). However, there are problems with this method, such as a decrease in the catalytic ability of the curing catalyst due to the presence of fatty acids, which act as catalyst poisons, and the reaction of excess fatty acids with organohydrogenpolysiloxane, which is the crosslinking agent in addition-curing silicone rubber compositions, resulting in poor curing or foaming due to a dehydrogenation reaction.

[0004] Furthermore, increased heat generation accompanying improved output from electronic components causes metal powder to accelerate cracking of silicone rubber in high-temperature environments, resulting in a decrease in the strength of the rubber and insufficient durability of the silicone rubber. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2003-096301 A [Patent Document 2] JP 2011-201934 A Summary of the Invention [Problem to be solved by the invention]

[0006] As described above, addition-curable silicone compositions using conventional metal powders or metal-plated powders have been unable to maintain durability in high-temperature environments.

[0007] The present invention has been made in view of the above circumstances, and has an object to provide an anti-sulfuration coating material comprising an addition-curable silicone composition that does not contain metal powder or metal-plated powder, that has excellent durability in high-temperature environments, and that gives a cured product that is resistant to sulfuration. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention provides an anti-sulfuration coating material, (A) A linear organopolysiloxane represented by the following general formula (1): [ka] (In the formula, R 1 are the same or different, each of which is a substituted or unsubstituted monovalent hydrocarbon group that does not contain an alkenyl group, and R 2 is a methyl group or a phenyl group, h is a number from 0 to 50, and i is a number from 0 to 100. However, when h is 0, R 2 is a phenyl group, and i is a number from 1 to 100. The siloxane units in the parentheses to which h is added and the siloxane units in the parentheses to which i is added may be arranged randomly, in blocks, or alternately. (B) an organohydrogenpolysiloxane having two or more silicon-bonded hydrogen atoms per molecule; (C) one or more selected from crystalline silica and talc, (D) a linear organopolysiloxane having one or more phenyl groups and having no alkenyl groups or silicon-bonded hydrogen atoms in each molecule; (E) a hydrosilylation catalyst comprising a platinum group metal; and, (F) Cerium oxide and is free of metal powder and metal plating powder.

[0009] Such an anti-sulfurization coating material can give a cured product that has excellent heat resistance and sulfurization resistance.

[0010] In addition, the R 1 is preferably a phenyl group or a methyl group.

[0011] Such an anti-sulfuration coating material can improve heat resistance and sulfuration resistance.

[0012] It is also preferable that the number of phenyl groups of the total number of organic groups bonded to silicon atoms in component (A) be 20% or more.

[0013] Such an anti-sulfuration coating material can reliably improve the sulfuration resistance.

[0014] Furthermore, the present invention provides a silicone cured product which is a cured product of the above-mentioned anti-sulfuration coating material.

[0015] Such a silicone cured product has excellent heat resistance and sulfurization resistance and can therefore be used as a protective coating material or sealing material for electronic devices, particularly semiconductor elements for optical applications.

[0016] The present invention further provides an electronic device that is encapsulated with the above-described cured silicone product.

[0017] The silicone cured product of the present invention has excellent heat resistance and sulfidation resistance, and therefore electronic devices sealed with such a silicone cured product will be highly reliable. Effect of the Invention

[0018] As described above, the sulfuration prevention coating material of the present invention does not contain metal powder or metal plating powder, and can provide a cured product that is excellent in durability in high-temperature environments and excellent in sulfuration resistance. Therefore, the cured product obtained from such a sulfuration prevention coating material can be suitably used for protecting electronic devices, such as optical element sealing materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] As described above, there has been a demand for the development of a coating material that does not contain metal powder or metal plating powder, has excellent durability in high-temperature environments, and has excellent sulfidation resistance, and a highly reliable electronic device encapsulated with the cured product thereof.

[0020] As a result of extensive research into achieving the above-mentioned object, the present inventors have found that the above-mentioned problems can be solved by an anti-sulfurization coating composition that contains the components (A), (B), (C), (D), (E) and (F) described below and does not contain metal powder or metal plating powder, and have thus completed the present invention.

[0021] That is, the present invention provides an anti-sulfuration coating material, (A) A linear organopolysiloxane represented by the following general formula (1): [ka] (In the formula, R 1 are the same or different, each of which is a substituted or unsubstituted monovalent hydrocarbon group that does not contain an alkenyl group, and R 2 is a methyl group or a phenyl group, h is a number from 0 to 50, and i is a number from 0 to 100. However, when h is 0, R 2 is a phenyl group, and i is a number from 1 to 100. The siloxane units in the parentheses to which h is added and the siloxane units in the parentheses to which i is added may be arranged randomly, in blocks, or alternately. (B) an organohydrogenpolysiloxane having two or more silicon-bonded hydrogen atoms per molecule; (C) one or more selected from crystalline silica and talc, (D) a linear organopolysiloxane having one or more phenyl groups and having no alkenyl groups or silicon-bonded hydrogen atoms in each molecule; (E) a hydrosilylation catalyst comprising a platinum group metal; and, (F) Cerium oxide and is free of metal powder and metal plating powder.

[0022] The present invention will be described in detail below, but the present invention is not limited thereto.

[0023] [Anti-sulfuration coating material] The anti-sulfuration coating material of the present invention comprises an addition-curable silicone composition containing the following components (A), (B), (C), (D), (E) and (F). Each component will be described in detail below.

[0024] <Component (A)> The component (A) in the sulfuration preventing coating material of the present invention is a linear organopolysiloxane represented by the following general formula (1). [ka] (In the formula, R 1 are the same or different, each of which is a substituted or unsubstituted monovalent hydrocarbon group that does not contain an alkenyl group, and R 2 is a methyl group or a phenyl group, h is a number from 0 to 50, and i is a number from 0 to 100. However, when h is 0, R 2 is a phenyl group, and i is a number from 1 to 100. The siloxane units in the parentheses to which h is added and the siloxane units in the parentheses to which i is added may be arranged randomly, in blocks, or alternately.

[0025] Above R 1is not particularly limited as long as it does not contain an alkenyl group, and examples thereof include unsubstituted or halogen-substituted monovalent hydrocarbon groups usually having 1 to 12, preferably 1 to 10, and more preferably 1 to 8 carbon atoms, such as alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, and heptyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl and phenethyl; and halogenated alkyl groups such as chloromethyl, 3-chloropropyl, and 3,3,3-trifluoropropyl. In particular, a methyl group and a phenyl group are preferred.

[0026] In the general formula (1), h is an integer of 0 to 50, i is an integer of 0 to 100, and when h is 0, R 2 is a phenyl group, and i is 1 to 100. If h and i are outside the above ranges, it will be impossible to impart high hardness and sulfurization resistance to the cured product of the silicone composition of the present invention.

[0027] In addition, the number of phenyl groups among the total number of organic groups bonded to silicon atoms in component (A) is preferably 20% or more, and although there is no particular upper limit, 80% or less is sufficient. Within this range, sufficient corrosion resistance can be obtained.

[0028] The viscosity of component (A) at 25°C is preferably 10 to 100,000 mPa·s, and more preferably in the range of 10 to 10,000 mPa·s. If the viscosity is within the above range, there is no risk of the composition becoming extremely viscous and causing problems such as poor workability. Unless otherwise specified below, the viscosity is a value measured using a rotational viscometer at 25°C. The rotational viscometer is not particularly limited, and for example, a BL type, BH type, BS type, or cone-plate type can be used.

[0029] Specific examples of component (A) include diphenylpolysiloxane capped at both ends with methylphenylvinylsiloxy groups, diphenylpolysiloxane capped at both ends with diphenylvinylsiloxy groups, diphenylsiloxane-methylphenylsiloxane copolymer capped at both ends with diphenylvinylsiloxy groups, diphenylpolysiloxane capped at both ends with dimethylvinylsiloxy groups, methylphenylpolysiloxane capped at both ends with dimethylvinylsiloxy groups, etc. The component (A) may be used alone or in combination of two or more types.

[0030] <(B) component> Component (B) is an organohydrogenpolysiloxane that contains two or more silicon-bonded hydrogen atoms in each molecule, and undergoes a hydrosilylation reaction with component (A) and acts as a crosslinking agent.

[0031] There are no particular limitations on the molecular structure of component (B), and various conventionally produced organohydrogenpolysiloxanes can be used, such as linear, cyclic, branched, three-dimensional network structures, etc. Furthermore, component (B) may be liquid, waxy, or solid at 25°C.

[0032] From the viewpoint of compatibility with component (A), component (B) preferably has at least one aryl group or arylene group. Examples of the aryl group include the same ones as those exemplified for component (A), and examples of the arylene group include a phenylene group, a naphthylene group, etc.

[0033] The organohydrogenpolysiloxane of component (B) has at least 2, preferably 3 to 300, and particularly preferably 3 to 100 hydrogen atoms bonded to silicon atoms (i.e., hydrosilyl groups (SiH groups)) per molecule. When the organohydrogenpolysiloxane has a linear structure, these SiH groups may be located either at the molecular chain terminals or in the middle of the molecular chain (non-terminals), or may be located at both.

[0034] The number of silicon atoms (degree of polymerization) in one molecule of the organohydrogenpolysiloxane of component (B) is preferably 2-300, more preferably 3-200, and even more preferably 4-150.

[0035] As the component (B), for example, an organohydrogenpolysiloxane represented by the following average composition formula (2) can be used. R 1 j H k SiO (4-j-k) / 2 (2) (In the formula, R 1 is the same as above, and j and k are positive numbers that preferably satisfy 0.7≦j≦2.1, 0.001≦k≦1.0, and 0.8≦j+k≦3.0, and more preferably satisfy 1.0≦j≦2.0, 0.01≦k≦1.0, and 1.55≦j+k≦2.5.

[0036] Specific examples of component (B) include 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, tris(hydrogendimethylsiloxy)methylsilane, tris(hydrogendimethylsiloxy)phenylsilane, tris(hydrogenmethylphenylsiloxy)methylsilane, tris(hydrogenmethylphenylsiloxy)phenylsilane, methylhydrogencyclopolysiloxane, methylhydrogensiloxane-dimethylsiloxane cyclic copolymer, and both-terminal trimethylsiloxy Endblocked methylhydrogenpolysiloxane, endblocked dimethylsiloxane-methylhydrogensiloxane copolymer with trimethylsiloxy groups at both ends, endblocked methylhydrogensiloxane-diphenylsiloxane copolymer with trimethylsiloxy groups at both ends, endblocked methylhydrogensiloxane-diphenylsiloxane-dimethylsiloxane copolymer with trimethylsiloxy groups at both ends, endblocked methylhydrogensiloxane-methylphenylsiloxane-dimethylsiloxane copolymer with trimethylsiloxy groups at both ends, endblocked dimethylhydrogensiloxane Dimethylpolysiloxane, diphenylpolysiloxane capped at both ends with dimethylhydrogensiloxy groups, methylhydrogenpolysiloxane capped at both ends with dimethylhydrogensiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer capped at both ends with dimethylhydrogensiloxy groups, methylhydrogensiloxane-dimethylsiloxane-diphenylsiloxane copolymer capped at both ends with dimethylhydrogensiloxy groups, methylhydrogensiloxane-dimethylsiloxane-methyl methylphenylsiloxane copolymer, dimethylpolysiloxane capped at both ends with hydrogenmethylphenylsiloxy groups, diphenylpolysiloxane capped at both ends with dimethylhydrogensiloxy groups, methylhydrogenpolysiloxane capped at both ends with hydrogenmethylphenylsiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer capped at both ends with hydrogenmethylphenylsiloxy groups, methylhydrogensiloxane-dimethylsiloxane-diphenylsiloxane copolymer capped at both ends with hydrogenmethylphenylsiloxy groups,Methylhydrogensiloxane-dimethylsiloxane-methylphenylsiloxane copolymer terminated at both ends with hydrogenmethylphenylsiloxy groups, (CH3)2HSiO, 1 / 2 Units and (CH3)3SiO 1 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and SiO 4 / 2 Units and (C6H5)3SiO 1 / 2 and copolymers consisting of units.

[0037] The amount of component (B) blended is such that the number of silicon-bonded hydrogen atoms in component (B) per silicon-bonded alkenyl group in component (A) is preferably within the range of 0.1 to 5.0, more preferably 0.5 to 3.0, and even more preferably 0.5 to 2.0. Within such ranges, it is possible to impart high strength to the silicone cured product, making it suitable for use as a coating material or a sealing material. The organohydrogenpolysiloxane of component (B) may use either a single compound, or a combination of two or more different compounds.

[0038] <(C) component> Component (C) is at least one member selected from crystalline silica and talc, and is capable of imparting suitable mechanical strength and thixotropy to the cured product of the anti-sulfurization coating material of the present invention.

[0039] Examples of crystalline silica include the Crystallite (registered trademark) series (manufactured by Tatsumori Co., Ltd.) and the MIN-U-SIL (registered trademark) series (manufactured by US Silica Co., Ltd.), and examples of talc include the Microace series (manufactured by Nippon Talc Co., Ltd.) and MS-P (manufactured by Nippon Talc Co., Ltd.) The average particle size (median size in volume-based particle size distribution) of component (C) is preferably 0.1 to 50 μm, and more preferably 1 to 20 μm.

[0040] The blend amount of the component (C) is preferably within a range from 10 to 300 parts by mass, and more preferably within a range from 10 to 100 parts by mass, per 100 parts by mass of the combined total of the components (A) and (B). The component (C) may use either a single compound, or a combination of two or more different compounds.

[0041] <(D) component> Component (D) is a linear organopolysiloxane containing one or more phenyl groups in each molecule and containing no alkenyl groups or silicon-bonded hydrogen atoms. This component is not involved in the crosslinking of components (A) and (B) and contributes to improving the workability of the anti-sulfurization coating material of the present invention and reducing the stress of the cured product.

[0042] The viscosity of component (D) is preferably in the range of 10 to 3,000 mPa s, and more preferably in the range of 10 to 1,000 mPa s. If the viscosity is within this range, bleeding and separation from components (A) and (B) can be suppressed, and the anti-sulfuration coating material of the present invention has excellent workability.

[0043] Specific examples of component (D) include diphenylpolysiloxane capped at both ends with trimethylsiloxy groups, methylphenylpolysiloxane capped at both ends with trimethylsiloxy groups, and diphenylsiloxane-methylphenylsiloxane copolymer capped at both ends with trimethylsiloxy groups. The component (D) may be used alone or in combination of two or more types.

[0044] <(E) component> The hydrosilylation catalyst containing a platinum group metal of component (E) may be any catalyst that promotes the addition reaction between the alkenyl groups in component (A) and the silicon-bonded hydrogen atoms in component (B). Specific examples include platinum group metals such as platinum, palladium, and rhodium, and platinum group metal compounds such as chloroplatinic acid, alcohol-modified chloroplatinic acid, coordination compounds of chloroplatinic acid with olefins, vinylsiloxanes, or acetylene compounds, tetrakis(triphenylphosphine)palladium, chlorotris(triphenylphosphine)rhodium, etc., with platinum compounds being particularly preferred. The component (E) may use either a single compound, or a combination of two or more different compounds.

[0045] The amount of component (E) to be blended may be an effective amount as a catalyst, but is preferably within the range of 1 to 500 ppm, more preferably 1 to 100 ppm, by mass, calculated as catalytic metal element relative to the total amount of components (A) and (B).Within such a range, the reaction rate of the addition reaction becomes appropriate, and a cured product having high strength can be obtained.

[0046] <(F) Component> Component (F) is cerium oxide, which is a component that improves the heat resistance of the anti-sulfurization coating material of the present invention.

[0047] From the viewpoint of hardness and heat resistance of the obtained cured product, the amount of component (F) added is preferably 0.1 to 20 parts by mass, and more preferably 1 to 10 parts by mass, per 100 parts by mass of components (A) and (B) combined. The particle size of component (F) is preferably such that the volume median diameter (D50) measured by a laser diffraction / scattering method is in the range of 0.5 to 5.0 μm.

[0048] It is preferable to mix the (F) component with the (A) or (B) component beforehand and then blend the component. This improves the dispersibility of the (F) component in the anti-sulfuration coating material of the present invention and suppresses separation. To further improve the dispersibility, the (F) component may be mixed with the (C) component beforehand.

[0049] Furthermore, the sulfuration preventing coating material of the present invention does not contain metal powder or metal plating powder, which makes it superior in durability in high temperature environments.

[0050] <Other ingredients> (Reinforcing ingredients) The sulfuration preventing coating material of the present invention may contain a crosslinkable organopolysiloxane other than component (A) as a reinforcing component in order to improve the mechanical properties of the cured product. Examples of the crosslinkable organopolysiloxane include organopolysiloxanes represented by the following average formula (3). (R 1 3SiO 1 / 2 ) a (R 3 R 1 2SiO 1 / 2 ) b (R 3 R 1 SiO) c (R 1 2SiO) d (R 3 SiO 3 / 2 ) e (R 1 SiO 3 / 2 ) f (SiO 4 / 2 ) g (3) (In the formula, R 1 is the same as above, and R 3 is an alkenyl group. a, b, c, d, e, f, and g are numbers that satisfy a ≧ 0, b ≧ 0, c ≧ 0, d ≧ 0, e ≧ 0, f ≧ 0, and g ≧ 0, and b + c + e > 0 and a + b + c + d + e + f + g = 1, with the proviso that when e + f + g = 0, c > 0.

[0051] The reinforcing component is a branched organopolysiloxane having an alkenyl group, or a linear organopolysiloxane having an alkenyl group in the side chain (or both the side chain and the molecular end), which can increase the crosslink density.

[0052] R 3Examples of the alkyl group include alkenyl groups having 2 to 10 carbon atoms, such as vinyl, allyl, and ethynyl groups, with alkenyl groups having 2 to 6 carbon atoms being preferred, and vinyl groups being particularly preferred. The reinforcing components may be used alone or in combination of two or more.

[0053] (Adhesion improver) An adhesion improver may be added to the sulfuration preventing coating material of the present invention in order to improve adhesion to resins, etc. As the adhesion improver, from the viewpoint of imparting self-adhesiveness to the composition of the present invention, which is an addition reaction curing type, organic silicon compounds such as silane and siloxane, which contain a functional group that imparts adhesiveness, and non-silicone organic compounds are used.

[0054] Specific examples of functional groups that impart adhesiveness include alkenyl groups such as vinyl groups and allyl groups bonded to silicon atoms, and hydrogen atoms; epoxy groups (e.g., γ-glycidoxypropyl group, β-(3,4-epoxycyclohexyl)ethyl group, etc.), acryloxy groups (e.g., γ-acryloxypropyl group, etc.) or methacryloxy groups (e.g., γ-methacryloxypropyl group, etc.) bonded to silicon atoms via carbon atoms; alkoxysilyl groups (e.g., trimethoxysilyl group, triethoxysilyl group, methyldimethoxysilyl group, etc. alkoxysilyl groups bonded to silicon atoms via alkylene groups which may contain 1 to 2 ester structures, urethane structures, or ether structures); and the like.

[0055] Examples of organosilicon compounds containing a functional group that imparts adhesiveness include silane coupling agents, siloxanes having an alkoxysilyl group and an organic functional group, and compounds in which an alkoxysilyl group has been introduced into an organic compound having a reactive organic group.

[0056] Examples of non-silicone organic compounds include organic acid allyl esters, epoxy group ring-opening catalysts, organic titanium compounds, organic zirconium compounds, and organic aluminum compounds.

[0057] (Reaction inhibitor) A reaction inhibitor may be added to the sulfuration preventing coating material of the present invention in order to adjust the curing rate.

[0058] Examples of reaction inhibitors include phosphorus-containing compounds such as triphenylphosphine; nitrogen-containing compounds such as tributylamine, tetramethylethylenediamine, and benzotriazole; sulfur-containing compounds; acetylene compounds; hydroperoxy compounds; maleic acid derivatives; 1-ethynylcyclohexanol, 3,5-dimethyl-1-hexyn-3-ol, and ethynylmethyldecylcarbinol.

[0059] Since the degree of the curing inhibition effect of the reaction inhibitor varies depending on the chemical structure of the reaction inhibitor, it is desirable to adjust the amount of the reaction inhibitor to an optimal amount for each reaction inhibitor used. Preferably, the amount is 0.001 to 5 parts by mass per 100 parts by mass of the total of the (A) component and the (B) component. If the amount is 0.001 part by mass or more, the long-term storage stability of the composition at room temperature can be sufficiently obtained. If the amount is 5 parts by mass or less, there is no risk of the curing of the composition being inhibited.

[0060] (Coupling Agent) A coupling agent may be added to the anti-sulfuration coating material of the present invention.

[0061] Examples of the coupling agent include triallyl isocyanurate and a silane coupling agent represented by the following structural formula. [ka]

[0062] (Fumed Silica) Fumed silica may be added to the anti-sulfuration coating material of the present invention.

[0063] The fumed silica has a specific surface area (BET method) of 50 m from the viewpoint of imparting thixotropy to the anti-sulfuration coating material of the present invention and reinforcing properties to the cured product. 2 / g or more, and more preferably 50 to 400m 2 / g, particularly preferably 100 to 300m 2 / g.

[0064] In addition, it is preferable to use fumed silica that has been treated with an organosilicon compound, such as methylchlorosilanes, such as trimethylchlorosilane, dimethyldichlorosilane, and methyltrichlorosilane, or hexaorganodisilazanes, such as dimethylpolysiloxane, hexamethyldisilazane, divinyltetramethyldisilazane, and dimethyltetravinyldisilazane.

[0065] Examples of such fumed silica include Reolosil DM30 (manufactured by Tokuyama Corp.), Aerosil NSX-200 (manufactured by Nippon Aerosil Co., Ltd.), and Musil 120A (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0066] When fumed silica is used, the blending amount is preferably 0.1 to 20 parts by mass, more preferably 1 to 10 parts by mass, based on 100 parts by mass of the total of the (A) component and the (B) component. In such a range, the precipitation of the fumed silica in the coating material can be suppressed, and sufficient reinforcing properties can be obtained. In addition, there is no risk of excessive thixotropy being imparted, resulting in a decrease in workability.

[0067] [Silicone cured product] Furthermore, the present invention provides a cured product (silicone cured product) obtained by curing the above-mentioned anti-sulfuration coating material.

[0068] [Electronic Devices] The present invention further provides an electronic device that is encapsulated with the above-described cured silicone product.

[0069] The curing method and conditions for the anti-sulfuration coating material of the present invention can be any known curing method and conditions, for example, curing can be performed at 100 to 180° C. for 10 minutes to 5 hours. EXAMPLES

[0070] The present invention will be specifically described below using synthesis examples, examples, and comparative examples, but the present invention is not limited thereto. The molecular weight is the number average molecular weight calculated as standard polystyrene by gel permeation chromatography (GPC), and the viscosity is the value measured at 25°C using a rotational viscometer. The average particle size is the median size in the volume-based particle size distribution measured by the laser diffraction / scattering method.

[0071] [Synthesis Example 1] 29 parts by mass of cerium oxide powder (CeO2, average particle size 2.7 μm, SN-2 manufactured by Nikki Co., Ltd.), (CH2=CH(CH3)2SiO 1 / 2 )2((CH3)2SiO) 420 A paste (F) was obtained by mixing 71 parts by mass of a linear organopolysiloxane (viscosity 5,000 mPa·s) represented by the following formula (1):

[0072] [Synthesis Example 2] The reaction product of hexachloroplatinic acid and 1,3-divinyltetramethyldisiloxane was diluted with methylphenylorganopolysiloxane containing 30 mol % phenyl groups and having a viscosity of 700 mPa s so that the platinum content was 1.0 mass %, to prepare platinum catalyst (E-1).

[0073] [Synthesis Example 3] The reaction product of hexachloroplatinic acid and 1,3-divinyltetramethyldisiloxane was diluted with dimethylorganopolysiloxane with a viscosity of 600 mPa·s to give a platinum content of 1.0 mass%, to prepare platinum catalyst (E-2).

[0074] [Examples 1 to 6, Comparative Examples 1 to 5] A coating material was prepared by mixing the following components in the amounts shown in Table 1. The numerical values ​​for each component in Table 1 represent parts by mass. The [Si-H] / [Si-Vi] value represents the molar ratio of hydrogen atoms bonded to silicon atoms in component (B) to all silicon-bonded alkenyl groups in the coating material.

[0075] (A-1): (CH2=CH(CH3)2SiO 1 / 2 )2((C6H5)2SiO) 30 ((CH3)2SiO) 68 A linear organopolysiloxane with a viscosity of 4,000 mPa·s. (A-2): (CH2=CH(CH3)(C6H5)SiO 1 / 2 )2((C6H5)2SiO)3, a linear organopolysiloxane with a viscosity of 2,000 mPa s (A-3):(CH2=CH(CH3)2)((CH3)2SiO) 205 A linear organopolysiloxane with a viscosity of 1,000 mPa·s, represented by the formula

[0076] (B-1): ((CH3)3SiO 1 / 2 )2(H(CH3)SiO)8 (B-2): Organohydrogenpolysiloxane represented by the following formula: [ka] (In the formula, the order of the siloxane units in parentheses is not specified.) (B-3): (H(CH3)2SiO 1 / 2 )2((C6H5)2SiO) (B-4): (H(CH3)2SiO 1 / 2 )2(H(CH3)SiO)2((C6H5)2SiO)2 (B-5): (H(CH3)2SiO 1 / 2 )2(H(CH3)SiO)2((CH3)2SiO) 14 Organohydrogenpolysiloxane represented by the formula: (B-6): ((CH3)3SiO 1 / 2 )2(H(CH3)SiO)6((CH3)2SiO) 17 Organohydrogenpolysiloxane represented by the formula:

[0077] (C-1): Crystalline silica KAIDA SP5 (manufactured by CBC Co., Ltd., average particle size 5 μm) (C-2): Crystalline silica Crystallite VX-S (Tatsumori Co., Ltd., average particle size 4 μm) (C-3): Crystalline silica MIN-U-SIL 15 (manufactured by US Silica, average particle size 5μm) (C-4): Talc powder MS-P (manufactured by Nippon Talc Co., Ltd., average particle size 15 μm) (C-5): Calcium carbonate MC Coat S20 (manufactured by Maruo Calcium Co., Ltd.) (C-6): Copper powder FCC-SP-99 (manufactured by Fukuda Metal Foil and Powder Co., Ltd., treated with stearic acid)

[0078] (D): ((CH3)3SiO 1 / 2 )2((CH3)2SiO)9((C6H5)2SiO)4, a viscosity of 400 mPa s.

[0079] (E-1): Platinum catalyst obtained in Synthesis Example 2 (E-2): Platinum catalyst obtained in Synthesis Example 3

[0080] (F): Cerium oxide-containing paste obtained in Synthesis Example 1

[0081] (G): ((CH3)3SiO 1 / 2 )2((CH=CH2)(CH3)2SiO)6((CH3)2SiO)3((C6H5)2SiO)9

[0082] (H): 1-ethynylcyclohexanol

[0083] (I-1): Triallyl isocyanurate (I-2): A silane coupling agent represented by the following structural formula: [ka]

[0084] (J): Fumed silica Musil 120A (Shin-Etsu Chemical Co., Ltd., specific surface area by BET adsorption method: 200 m 2 / g)

[0085] The coating materials obtained in Examples 1 to 6 and Comparative Examples 1 to 5 were subjected to the following evaluations. The results are shown in Table 2.

[0086] (Tensile strength) Each coating material was poured into a mold to a thickness of 2 mm and cured at 150°C for 1 hour to obtain a sheet-like cured product. The tensile strength of the cured product was measured using dumbbell-shaped test pieces based on JIS K6251:2017.

[0087] (hardness) Six sheets of the above cured product were stacked together, and the hardness at a thickness of 12 mm was measured using an Asker C hardness tester. If the hardness is within the range of 5 to 50 on the Asker C hardness scale, the material has excellent stress relaxation properties and can impart high durability to electronic devices when coated or sealed therewith.

[0088] (Change in hardness after heat resistance test) The cured product was then exposed to a 200°C environment for 500 hours, cooled to 25°C, and the hardness after the heat resistance test was measured using an Asker C hardness tester in the same manner as above. The smaller the change in hardness, the more durable the material is.

[0089] (mass reduction rate) The mass of the cured product was measured before and after exposure to an environment of 200° C. for 500 hours, and the weight loss rate was calculated. A weight loss rate of less than 5% is preferable, and the smaller the weight loss rate, the more durable the material is.

[0090] (Sulfidation resistance) Silicone gel KE-1057 (Shin-Etsu Chemical Co., Ltd.) was poured into a 100 g wide-mouth glass bottle with a silver substrate placed at the bottom inside, and cured at 150°C for 30 minutes. Next, 10 g of each coating material was poured into the bottle, cured at 150°C for 1 hour, and then a container containing 0.1 g of sulfur was placed on the cured product. After sealing the glass bottle, it was left to stand at 70°C for 10 days, and the discoloration of the silver substrate was visually confirmed. The evaluation was performed as follows: if the silver substrate turned black, it was marked with ×; if no discoloration was observed, it was marked with ○.

[0091] [Table 1]

[0092] [Table 2]

[0093] As shown in Table 2, the cured products made of the anti-sulfurization coating materials of Examples 1 to 6 showed little change in hardness and mass before and after the heat resistance test at 200° C. for 500 hours, and were excellent in sulfurization resistance.

[0094] On the other hand, in Comparative Example 1, in which a coating material not containing crystalline silica or talc was used, the tensile strength of the cured product was significantly reduced, and in Comparative Example 2, in which a coating material containing calcium carbonate instead of crystalline silica or talc was used, the hardness changed significantly after the heat resistance test and the durability was poor.

[0095] In addition, Comparative Example 3, which used a dimethylpolysiloxane-based coating material as component (A), was excellent in heat resistance but poor in sulfurization resistance. On the other hand, Comparative Examples 4 and 5, in which copper powder was added to the dimethylpolysiloxane-based coating material, obtained sulfurization resistance, but the mass loss rate during the heat resistance test increased due to cracking.

[0096] From the above, it has been demonstrated that the anti-sulfuration coating material of the present invention does not contain metal powder, gives a cured product that is excellent in durability in high-temperature environments and has sulfuration resistance, and is suitable for protecting electronic devices.

[0097] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. 1. An anti-sulfidation coating material comprising: (A) A linear organopolysiloxane represented by the following general formula (1): 【Chemistry 1】 (In the formula, R 1 is a methyl group, R 2 is a methyl group, h is a number from 1 to 50, and i is a number from 1 to 100. The siloxane units in the brackets marked with h and the siloxane units in the brackets marked with i may be arranged randomly, in blocks, or alternatingly with respect to each other. (B) an organohydrogenpolysiloxane having two or more silicon-bonded hydrogen atoms in each molecule; (C) one or more selected from crystalline silica and talc, (D) a linear organopolysiloxane having one or more phenyl groups and having no alkenyl groups or silicon-bonded hydrogen atoms in each molecule; (E) a hydrosilylation catalyst comprising a platinum group metal; and, (F) Cerium oxide and is free of metal powder and metal-plated powder, and the number of phenyl groups among the total number of organic groups bonded to silicon atoms in component (A) is 20% or more.

2. A silicone cured product, which is a cured product of the anti-sulfuration coating material according to claim 1.

3. An electronic device, which is sealed with the silicone cured product according to claim 2.

Citation Information

Patent Citations

  • Silicone rubber composition for encapsulating / Sealing electric / Electronic parts

    JP2003096301A

  • Addition reaction-curable type silicone rubber composition and method for producing the same

    JP2011201934A

  • Curable silicone resin composition and light-emitting diode device using the same

    JP2012041496A

  • Silicone gel composition, and electronic circuit sealed with cured material of the same

    JP2012251116A

  • Optical semiconductor device using curable composition containing inorganic filler as sealing agent

    JP2018044067A