Light control film

The light control film with a raised portion on the electrode layer surface enhances heat shielding by increasing free electron density, addressing the inefficiency of existing films in managing sunlight heat reflection.

JP7581396B2Active Publication Date: 2024-11-12NITTO DENKO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023017382
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-02-08
Publication Date
2024-11-12
Estimated Expiration
2043-02-08

AI Technical Summary

Technical Problem

Existing light control films do not effectively address the need for improved heat shielding properties against sunlight, as the electrode layer, which contains free electrons, has a significant reflectivity to heat rays but occupies a large area, limiting the film's efficiency.

Method used

The light control film incorporates a surface on the light control layer side with a raised portion of 3 nm or more, enhancing the number of free electrons per unit area in the electrode layer, thereby increasing its reflectivity to heat rays and improving heat shielding properties.

Benefits of technology

The film achieves enhanced heat shielding by increasing the number of free electrons in the electrode layer, leading to higher reflectivity against sunlight, thus providing better thermal insulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581396000002
    Figure 0007581396000002
  • Figure 0007581396000003
    Figure 0007581396000003
  • Figure 0007581396000004
    Figure 0007581396000004
Patent Text Reader

Abstract

To provide a lighting control film suitable for achieving good sunlight heat blocking properties.SOLUTION: A lighting control film X of the present invention comprises a base material film 10, an electrode layer 20, a lighting control layer 30. and an electrode layer 40 in this order in a thickness direction H. A surface 20a of the electrode layer 20 on the lighting control layer 30 side has raised parts 21 with a height of 3 nm or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a light management film. [Background technology]

[0002] A light control film that is attached to window glass of a building, a vehicle, etc. is known. The light control film includes a light control section and a transparent substrate film that supports the light control section. The light control section includes, for example, a transparent conductive layer, a light control layer, and a transparent conductive layer in this order in the thickness direction. The light control layer is sandwiched between two transparent conductive layers. The light control layer is formed from an electrochromic (EC) material. The EC material is a material that can be reversibly changed between a colored non-transparent state and a transparent state, for example, by electrochemical oxidation-reduction. Each transparent conductive layer is an electrode. By turning on and off the voltage between the transparent conductive layers, the light control layer is switched, for example, between a non-transparent state (light blocking state) and a transparent state (non-light blocking state). In a window glass to which such a light control film is attached, the transmittance of light such as visible light through the window glass with the light control film is switched by turning on and off the voltage between the transparent conductive layers (switching control of light transmittance). Technology related to such light control films is described, for example, in Patent Document 1 below. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-101206 A Summary of the Invention [Problem to be solved by the invention]

[0004] From the viewpoint of improving comfort in buildings and vehicles and reducing the cooling load, etc., light control films are required to have heat shielding properties against sunlight.

[0005] Meanwhile, the present inventors have discovered the following about light-control films. The electrode layer (transparent conductive layer) contains free electrons as carriers that have significant reflectivity to heat rays in sunlight (electromagnetic waves such as near-infrared rays that transmit heat by radiation). In light-control films, such an electrode layer is provided over the entire surface of the light-control layer. That is, the area ratio of the electrode layer in a planar view of the light-control film is large. In such light-control films, the heat-shielding properties of the film against sunlight can be efficiently controlled by adjusting the number of carriers in the electrode layer. The present invention is based on such findings.

[0006] The present invention provides a light control film suitable for achieving good heat shielding properties against sunlight. [Means for solving the problem]

[0007] The present invention [1] includes a light-control film comprising a base film, a first electrode layer, a light-control layer, and a second electrode layer, in that order in the thickness direction, in which the surface of the first electrode layer facing the light-control layer has a protrusion having a height of 3 nm or more.

[0008] The present invention [2] includes the light-control film according to the above [1], in which the surface of the second electrode layer facing the light-control layer has a protrusion having a height of 3 nm or more.

[0009] The present invention [3] includes the light control film according to the above [1] or [2], in which the base film has a near-infrared absorbing layer and / or a near-infrared reflective layer.

[0010] The present invention [4] includes the light control film according to any one of the above [1] to [3], which has an average transmittance of 50% or less at wavelengths of 800 nm to 1300 nm. Effect of the Invention

[0011] As described above, the light-controlling film of the present invention comprises a base film, a first electrode layer, a light-controlling layer, and a second electrode layer in this order in the thickness direction, and the surface of the first electrode layer on the side of the light-controlling layer has a raised portion with a height of 3 nm or more. The first electrode layer having a significant raised portion with a height of 3 nm or more is suitable for ensuring the average thickness of the entire first electrode layer (when the first electrode layer has such a raised portion, the average thickness of the entire layer is larger than when the first electrode layer does not have the raised portion). Such a light-controlling film is suitable for ensuring the number of free electrons (the number of carriers) per unit area in a planar view in the first electrode layer. The more free electrons per unit area in the first electrode layer, the higher the reflectivity of the first electrode layer against heat rays in sunlight. The higher the reflectivity of the first electrode layer against heat rays, the higher the shielding property (heat shielding property) of the light-controlling film comprising such a first electrode layer against heat rays. Therefore, the light-controlling film of the present invention is suitable for realizing good heat shielding property against sunlight. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view of one embodiment of a light control film of the present invention. [Diagram 2] FIG. 2 is a partially enlarged cross-sectional view of the light control film shown in FIG. [Diagram 3] 2 is an enlarged cross-sectional view of another portion of the light control film shown in FIG. 1. [Figure 4] 4A and 4B show some steps in an example of a method for producing the light control film shown in Fig. 1. Fig. 4A shows a base film preparation step, Fig. 4B shows a transparent conductive layer formation step, Fig. 4C shows a crystallization step, and Fig. 4D shows a light control layer formation step. [Diagram 5] This shows a lamination step subsequent to the step shown in FIG. 4D. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The light control film X according to one embodiment of the present invention includes a base film 10 (first base film), an electrode layer 20 (first electrode layer), a light control layer 30, an electrode layer 40 (second electrode layer), and a base film 50 (second base film) in this order in the thickness direction H. The base film 10 has a first surface 10a and a second surface 10b opposite to the first surface 10a. The electrode layer 20 is disposed on the first surface 10a. The electrode layer 20 and the first surface 10a are in contact with each other. The electrode layer 20 has a surface 20a on the light control layer 30 side (the side opposite to the base film 10). The light control layer 30 is disposed on the surface 20a. The light control layer 30 and the surface 20a are in contact with each other. The electrode layer 40 is disposed on the light control layer 30. The electrode layer 40 has a surface 40a on the light control layer 30 side (the side opposite to the base film 50). The surface 40a and the light-controlling layer 30 are in contact with each other. The base film 50 is disposed on the electrode layer 40. The base film 50 has a first surface 50a on the electrode layer 40 side and a second surface 50b opposite to the first surface 50a. The electrode layer 40 and the first surface 50a are in contact with each other. The light-controlling film X has a sheet shape that spreads in a direction (plane direction) perpendicular to the thickness direction H. Such a light-controlling film X is, for example, a light-controlling film that is attached to window glass of a building, a vehicle, etc.

[0014] In the light control film X, the base film 10 and the electrode layer 20 form an electrode-attached base film Y1.

[0015] In this embodiment, the base film 10 includes a resin film 11 and a cured resin layer 12, which are arranged in this order in the thickness direction H. The cured resin layer 12 is in contact with the resin film 11. The cured resin layer 12 forms a first surface 10a of the base film 10.

[0016] The resin film 11 is a base material that ensures the strength of the light control film X. The resin film 11 is a transparent resin film having flexibility. Examples of the material of the resin film 11 include polyester resin, polyolefin resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin, and polystyrene resin. Examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. Examples of the polyolefin resin include polyethylene, polypropylene, and cycloolefin polymer. Examples of the acrylic resin include polymethacrylate. As the material of the resin film 11, for example, from the viewpoint of transparency and strength, polyester resin is preferably used, and more preferably PET is used.

[0017] The surface of the resin film 11 on the side of the cured resin layer 12 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment (the same applies to the surface modification treatment of the resin film 51 described below).

[0018] The thickness of the resin film 11 is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more, from the viewpoint of ensuring the strength of the light control film X. The thickness of the resin film 11 is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 150 μm or less, from the viewpoint of ensuring the handleability of the resin film 11 in the roll-to-roll system.

[0019] The visible light transmittance of the resin film 11 is preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency required for the light control film in the transparent state in the light control film X. The visible light transmittance of the resin film 11 is, for example, 100% or less. The visible light transmittance is the transmittance in the wavelength range of 380 nm to 780 nm.

[0020] In this embodiment, the cured resin layer 12 is an optical adjustment layer (refractive index adjustment layer) for improving the optical characteristics of the light control film X. The cured resin layer 12 may have a function of blocking moisture and organic gases generated from the resin film 11 in the transparent conductive layer forming step (FIG. 4B) described later. In this embodiment, the cured resin layer 12 is a cured product of a first curing type resin composition. The first curing type resin composition contains a resin. Examples of the resin include melamine resin, alkyd resin, organic silane condensate, polyester resin, acrylic urethane resin, acrylic resin (excluding acrylic urethane resin), urethane resin (excluding acrylic urethane resin), amide resin, silicone resin, and epoxy resin. These resins may be used alone or in combination of two or more kinds. From the viewpoint of ensuring the adhesion of the electrode layer 20 to the base film 10, the resin is preferably at least one selected from the group consisting of melamine resin, alkyd resin, and organic silane condensate. The first curable resin composition may be an ultraviolet curable resin composition or a thermosetting resin composition.

[0021] The surface (first surface 10a) of the cured resin layer 12 opposite to the resin film 11 preferably does not have any raised portion having a height of 3 nm or more, more preferably does not have any raised portion having a height of 2 nm or more, and even more preferably does not have any raised portion having a height of 1 nm or more, from the viewpoint of ensuring the average thickness of the electrode layer 20 formed on the cured resin layer 12. From the viewpoint of forming a cured resin layer 12 without any raised portion, it is preferable that the first curable resin composition does not contain particles.

[0022] The thickness of the cured resin layer 12 is preferably 5 nm or more, more preferably 10 nm or more, even more preferably 20 nm or more, and particularly preferably 30 nm or more, from the viewpoint of improving the transmission characteristics of the light control film X. The thickness of the cured resin layer 12 is preferably 1000 nm or less, more preferably 50 nm or less, and even more preferably 40 nm or less, from the viewpoint of making the light control film X thinner.

[0023] The base film 10 may have another cured resin layer on the opposite side of the resin film 11 to the cured resin layer 12. Examples of the other cured resin layer include a hard coat layer and an anti-blocking layer.

[0024] The other cured resin layer is, for example, a cured product of a second curable resin composition. The second curable resin composition contains a resin. Examples of the resin include polyester resin, acrylic urethane resin, acrylic resin (excluding acrylic urethane resin), urethane resin (excluding acrylic urethane resin), amide resin, silicone resin, epoxy resin, and melamine resin. These resins may be used alone or in combination of two or more kinds. The second curable resin composition may be an ultraviolet-curable resin composition or a thermosetting resin composition.

[0025] The second curable resin composition may contain particles. Examples of the particles include inorganic oxide particles and organic particles. Examples of the inorganic oxide particle material include silica, alumina, titania, zirconia, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide. Examples of the organic particle material include polymethyl methacrylate, polystyrene, polyurethane, acrylic-styrene copolymer, benzoguanamine, melamine, and polycarbonate. As the particles, inorganic oxide particles are preferably used, and more preferably silica particles and / or zirconia particles are used.

[0026] The thickness of the other cured resin layer is preferably 0.5 μm or more, more preferably 1 μm or more, and even more preferably 2 μm or more, from the viewpoint of ensuring the function of the cured resin layer. The thickness of the cured resin layer 12 is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less, from the viewpoint of making the light control film X thinner.

[0027] The thickness of the base film 10 is preferably 10 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more, from the viewpoint of ensuring the handleability of the light control film X. The thickness of the base film 10 is preferably 500 μm or less, more preferably 300 μm or less, even more preferably 200 μm or less, and even more preferably 150 μm or less, from the viewpoint of making the light control film X thinner.

[0028] The visible light transmittance of the base film 10 is preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency required for the light control film in the transparent state in the light control film X. The visible light transmittance of the base film 10 is, for example, 100% or less.

[0029] The base film 10 preferably has a near-infrared absorbing layer and / or a near-infrared reflective layer. The near-infrared absorbing layer is a layer that exhibits significant absorption ability for near-infrared rays (wavelength 700 nm to 2500 nm). The near-infrared reflective layer is a layer that exhibits significant reflection ability for near-infrared rays (wavelength 700 nm to 2500 nm).

[0030] The near-infrared absorbing layer may be disposed between the resin film 11 and the cured resin layer 12, or may be disposed on the opposite side of the resin film 11 to the cured resin layer 12. The resin film 11 may be a near-infrared absorbing layer, or may have a multi-layer structure including a near-infrared absorbing layer. The near-infrared absorbing layer includes, for example, a near-infrared absorbing agent and a binder resin. Examples of the near-infrared absorbing agent include inorganic near-infrared absorbing agents and organic near-infrared absorbing agents. Examples of the inorganic near-infrared absorbing agent include CFM complex oxide particles and tungsten oxide particles. The CFM complex oxide is a complex oxide of copper, iron, and manganese. Examples of the material of the binder resin include the materials described above with respect to the resin film 11.

[0031] The near-infrared reflective layer may be disposed between the resin film 11 and the cured resin layer 12, or may be disposed on the opposite side of the resin film 11 to the cured resin layer 12. The resin film 11 may be a near-infrared reflective layer, or may have a multilayer structure including a near-infrared reflective layer. The near-infrared reflective layer has, for example, a multilayer structure including a plurality of resin thin layers having different optical properties, and preferably has a multilayer structure in which a first resin thin layer and a second resin thin layer having different optical properties are alternately arranged in the thickness direction H. Examples of the optical properties include an in-plane average refractive index. The difference in the in-plane average refractive index between the first resin thin layer and the second resin thin layer is preferably 0.01 or more, more preferably 0.03 or more, and is preferably 0.15 or less, more preferably 0.12 or less. The number of laminated resin thin layers forming the multilayer structure is, for example, 20 or more, and, for example, 700 or less. Examples of the material of the resin thin layer include the materials described above for the resin film 11.

[0032] The electrode layer 20 is a layer that has both optical transparency and electrical conductivity. Such an electrode layer 20 is formed from a transparent conductive material. That is, the electrode layer 20 is a transparent conductive layer. Examples of the transparent conductive material include transparent conductive oxides.

[0033] Examples of the conductive oxide include indium-containing conductive oxide and antimony-containing conductive oxide. Examples of the indium-containing conductive oxide include indium tin composite oxide (ITO), indium zinc composite oxide (IZO), indium gallium composite oxide (IGO), and indium gallium zinc composite oxide (IGZO). Examples of the antimony-containing conductive oxide include antimony tin composite oxide (ATO). From the viewpoint of realizing high transparency and good electrical conductivity, the conductive oxide is preferably an indium-containing conductive oxide, and more preferably ITO. This ITO may contain a metal or semimetal other than In and Sn in an amount less than the respective contents of In and Sn.

[0034] The ratio of the content of tin oxide to the total content of indium oxide (In2O3) and tin oxide (SnO2) in ITO is preferably 4 mass% or more, more preferably 6 mass% or more, even more preferably 8 mass% or more, and particularly preferably 9 mass% or more. Such a configuration is preferable for growing crystal grains of the transparent conductive layer to form the protuberances 21 in the crystallization step (FIG. 4C) described later. Moreover, from the viewpoint of reducing the resistance of the electrode layer 20, the ratio of the content of tin oxide to the total content of indium oxide and tin oxide in ITO is preferably 15 mass% or less, more preferably 13 mass% or less, and even more preferably 12 mass% or less.

[0035] The tin oxide ratio in ITO can be identified, for example, as follows. First, the abundance ratio of indium atoms (In) and tin atoms (Sn) in ITO, which is the object to be measured, is determined by X-ray photoelectron spectroscopy. From the abundance ratios of In and Sn in ITO, the ratio of the number of Sn atoms to the number of In atoms in ITO is determined. This gives the tin oxide ratio in ITO. The tin oxide ratio in ITO can also be determined from the tin oxide (SnO2) content of the ITO target used during sputtering film formation.

[0036] The electrode layer 20 is preferably a crystalline film. The electrode layer 20 is preferably a crystalline film from the viewpoint of reducing the resistance of the electrode layer 20, and is also preferable for realizing good infrared reflection characteristics in the electrode layer 20 and the light control film X.

[0037] Whether an electrode layer (electrode layers 20 and 40 in the light control film X) made of a conductive oxide is a crystalline film can be determined, for example, by the following method. First, the electrode layer is immersed in hydrochloric acid with a concentration of 5% by mass at 20°C for 15 minutes. Next, the electrode layer is washed with water and then dried. Next, the resistance between a pair of terminals separated by a distance of 15 mm (inter-terminal resistance) is measured on the exposed surface of the electrode layer. In this measurement, if the inter-terminal resistance is 10 kΩ or less, the electrode layer can be determined to be a crystalline film.

[0038] As shown in FIG. 2, the surface 20a of the electrode layer 20 has a raised portion 21 with a height d of 3 nm or more. The height d of the raised portion 21 is the distance from the flat surface 22 of the surface 20a to the top of the raised portion 21 in the thickness direction H. The electrode layer 20 has a raised portion 21 with a significant height of 3 nm or more, which is suitable for ensuring the average thickness of the entire electrode layer 20 (when the electrode layer 20 has such a raised portion 21, the average thickness of the entire layer is larger than when the electrode layer 20 does not have the raised portion 21). This is suitable for ensuring the number of free electrons (the number of carriers) per unit area in the planar view of the electrode layer 20. The greater the number of free electrons in the electrode layer 20, the higher the reflectivity of the electrode layer 20 against heat rays (mainly near-infrared rays) in sunlight, and therefore the higher the shielding property (heat shielding property) of the light control film X against heat rays. From the viewpoint of ensuring good heat shielding properties in the light control film X, the height d of the raised portion 21 is preferably 4 nm or more, and more preferably 5 nm or more. From the viewpoint of suppressing an increase in the resistance value of the electrode layer 20, the height d of the raised portion 21 is preferably 20 nm or less, more preferably 10 nm or less, and even more preferably 8 nm or less. The method for measuring the height of the raised portion is as described later in the examples.

[0039] The thickness of the electrode layer 20 is preferably 30 nm or more, more preferably 50 nm or more, even more preferably 70 nm or more, even more preferably 90 nm or more, and particularly preferably 100 nm or more, from the viewpoint of forming the raised portion 21. The thickness of the electrode layer 20 is the distance from the surface of the electrode layer 20 on the substrate film 10 side to the flat surface 22 in the thickness direction H. The thicker the electrode layer 20 is, the easier it is for the crystal grains of the transparent conductive layer to grow larger in the crystallization step described below, and therefore the easier it is to form the raised portion 21 on the surface 20a of the electrode layer 20. In addition, a thick electrode layer 20 is also preferable from the viewpoint of reducing the resistance of the electrode layer 20. The thickness of the electrode layer 20 is preferably 300 nm or less, more preferably 200 nm or less, even more preferably 150 nm or less, and even more preferably 120 nm or less, from the viewpoint of ensuring the bending resistance of the light control film X (such as suppressing cracking of the electrode layer 20 when bent).

[0040] The number of free electrons (the number of carriers) in the plan view of the electrode layer 20 is preferably 5×10 15 / cm 2 More preferably, 8×10 15 / cm 2 More preferably, 10×10 15 / cm 2 More preferably, 11×10 15 / cm 2 The number of free electrons (the number of carriers) in the plan view of the electrode layer 20 is preferably 100×10 15 / cm 2 Less than or equal to 60×10 15 / cm 2 Less than 40×10, more preferably 15 / cm 2 The method for measuring the number of carriers in the electrode layer is as described below in the examples.

[0041] The visible light transmittance of the electrode layer 20 is, for example, 50% or more, preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency required for the light control film in the transparent state in the light control film X. The visible light transmittance of the electrode layer 20 is, for example, 100% or less.

[0042] The light-adjusting layer 30 is a material that can be reversibly changed between a colored non-transparent state (light-shielding state) and a transparent state (light-non-shielding state) by the action of, for example, an electric current or an electric field. Examples of the light-adjusting layer 30 include an electrochromic (EC) light-adjusting layer, a light-adjusting layer containing a polymer dispersed liquid crystal (PDLC), a light-adjusting layer containing a polymer network liquid crystal (PNLC), and a suspended particle device (SPD) light-adjusting layer.

[0043] The EC light control layer is formed from an EC material. The EC material is a material that can be reversibly changed between a colored non-transparent state (light-shielding state) and a transparent state (light-non-shielding state) by electrochemical oxidation and reduction. The EC material includes inorganic EC materials and organic EC materials. The inorganic EC materials include, for example, tungsten oxide, vanadium oxide, molybdenum oxide, iridium oxide, rhodium oxide, and indium nitride. The organic EC materials include, for example, polyaniline, viologen, and polyoxotungstate.

[0044] Polymer-dispersed liquid crystal has a structure in which liquid crystal is phase-separated in a polymer. Polymer-network liquid crystal has a structure in which liquid crystal is dispersed in a polymer network, and the liquid crystal in the polymer network forms a continuous phase. In these, examples of liquid crystal compounds include nematic liquid crystal compounds, smectic liquid crystal compounds, and cholesteric liquid crystal compounds. Examples of nematic liquid crystal compounds include biphenyl-based compounds, phenylbenzoate-based compounds, cyclohexylbenzene-based compounds, azoxybenzene-based compounds, azobenzene-based compounds, azomethine-based compounds, terphenyl-based compounds, biphenylbenzoate-based compounds, cyclohexylbiphenyl-based compounds, phenylpyridine-based compounds, cyclohexylpyrimidine-based compounds, and cholesterol-based compounds.

[0045] The thickness of the light-controlling layer 30 is preferably 1 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more, from the viewpoint of ensuring a large difference in visible light transmittance between the non-transparent state and the transparent state in the light-controlling film X. The thickness of the light-controlling layer 30 is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less, from the viewpoint of making the light-controlling film X thin and ensuring high transmittance in the transparent state.

[0046] In the light control film X, the base film 50 and the electrode layer 40 form an electrode-attached base film Y2.

[0047] In this embodiment, the base film 50 includes a resin film 51 and a cured resin layer 52, which are arranged in this order in the thickness direction H. The cured resin layer 52 is in contact with the resin film 51. The cured resin layer 52 forms a first surface 50a of the base film 50.

[0048] The resin film 51 is a base material that ensures the strength of the light control film X. The resin film 51 is a flexible and transparent resin film. Examples of materials for the resin film 51 include the materials described above as the materials for the resin film 11. The surface of the resin film 51 on the side of the cured resin layer 52 may be subjected to a surface modification treatment. The preferred thickness and the preferred visible light transmittance of the resin film 51 are the same as those described above for the resin film 11.

[0049] In this embodiment, the cured resin layer 52 is an optical adjustment layer (refractive index adjustment layer) for improving the optical properties of the light control film X. The cured resin layer 52 may have a function of blocking moisture and organic gases generated from the resin film 51 in the transparent conductive layer forming step. In this embodiment, the cured resin layer 52 is a cured product of a third curing type resin composition. The third curing type resin composition contains a resin. Examples of the resin of the third curing type resin composition include the resins described above with respect to the first curing type resin composition. In addition, the third curing type resin composition may be an ultraviolet curing type resin composition or a thermosetting type resin composition.

[0050] The surface (first surface 50a) of the cured resin layer 52 opposite to the resin film 51 preferably does not have any raised portion having a height of 3 nm or more, more preferably does not have any raised portion having a height of 2 nm or more, and even more preferably does not have any raised portion having a height of 1 nm or more, from the viewpoint of ensuring the average thickness of the electrode layer 40 formed on the cured resin layer 52. From the viewpoint of forming a cured resin layer 52 without any raised portion, it is preferable that the third curable resin composition does not contain particles.

[0051] The thickness of the cured resin layer 52 is preferably 5 nm or more, more preferably 10 nm or more, even more preferably 20 nm or more, and particularly preferably 30 nm or more, from the viewpoint of ensuring the adhesion of the electrode layer 40 to the base film 50. The thickness of the cured resin layer 52 is preferably 50 nm or less, more preferably 40 nm or less, from the viewpoint of making the light control film X thinner.

[0052] Similar to the above-mentioned regarding the base film 10, the base film 50 may have another cured resin layer (for example, a hard coat layer and an anti-blocking layer) on the opposite side of the resin film 51 to the cured resin layer 52.

[0053] The visible light transmittance of the base film 50 is preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency required for the light control film in the transparent state in the light control film X. The visible light transmittance of the base film 50 is, for example, 100% or less.

[0054] The substrate film 50 preferably has a near-infrared absorbing layer and / or a near-infrared reflective layer.

[0055] In the base film 50, the near-infrared absorbing layer may be disposed between the resin film 51 and the cured resin layer 52, or may be disposed on the opposite side of the resin film 51 to the cured resin layer 52. The resin film 51 may be a near-infrared absorbing layer, or may have a multi-layer structure including a near-infrared absorbing layer. The near-infrared absorbing layer includes, for example, a near-infrared absorbing agent and a binder resin. Examples of the near-infrared absorbing agent include the near-infrared absorbing agents described above for the base film 10. Examples of the material for the binder resin include the materials described above for the resin film 11.

[0056] In the base film 50, the near-infrared reflective layer may be disposed between the resin film 51 and the cured resin layer 52, or may be disposed on the opposite side of the resin film 51 to the cured resin layer 52. The resin film 51 may be a near-infrared reflective layer, or may have a multilayer structure including a near-infrared reflective layer. Examples of the near-infrared reflective layer include the near-infrared reflective layers described above with respect to the base film 10.

[0057] The electrode layer 40 is a layer having both optical transparency and electrical conductivity. The electrode layer 40 is formed from a transparent conductive material. That is, the electrode layer 40 is a transparent conductive layer. Examples of the transparent conductive material include the transparent conductive materials described above with respect to the electrode layer 20. When the electrode layer 40 is formed from ITO, the ratio of the content of tin oxide to the total content of indium oxide (In2O3) and tin oxide (SnO2) in ITO is preferably 4 mass% or more, more preferably 6 mass% or more, even more preferably 8 mass% or more, and particularly preferably 9 mass% or more. Such a configuration is preferable for growing crystal grains of the transparent conductive layer to form the protuberance 41 in the crystallization step described later. In addition, the ratio of the content of tin oxide to the total content of indium oxide and tin oxide in ITO is preferably 15 mass% or less, more preferably 13 mass% or less, and even more preferably 12 mass% or less, from the viewpoint of reducing the resistance of the electrode layer 40.

[0058] The electrode layer 40 is preferably a crystalline film. The electrode layer 40 is preferably a crystalline film from the viewpoint of reducing the resistance of the electrode layer 40, and is also preferable for realizing good infrared reflection characteristics in the electrode layer 40 and the light control film X.

[0059] As shown in FIG. 3, the surface 40a of the electrode layer 40 preferably has a raised portion 41 with a height d of 3 nm or more. The height d of the raised portion 41 is the distance from the flat surface 42 of the surface 40a to the top of the raised portion 41 in the thickness direction H. The electrode layer 40 has a raised portion 41 with a significant height of 3 nm or more, which is suitable for ensuring the average thickness of the entire electrode layer 40 and for ensuring the number of free electrons (the number of carriers) per unit area in the planar view of the electrode layer 40. The greater the number of free electrons per unit area of ​​the electrode layer 40, the higher the reflectivity of the electrode layer 40 against heat rays in sunlight, and therefore the higher the heat shielding property of the light control film X against heat rays. From the viewpoint of ensuring good heat shielding property in the light control film X, the height d of the raised portion 41 is preferably 4 nm or more, more preferably 5 nm or more. From the viewpoint of suppressing an increase in the resistance value of the electrode layer 40, the height d of the protrusion 41 is preferably 20 nm or less, more preferably 10 nm or less, and further preferably 8 nm or less.

[0060] The thickness of the electrode layer 40 is preferably 30 nm or more, more preferably 50 nm or more, even more preferably 70 nm or more, even more preferably 90 nm or more, and particularly preferably 100 nm or more, from the viewpoint of forming the raised portion 41. The thickness of the electrode layer 40 is the distance from the surface of the electrode layer 40 on the substrate film 50 side to the flat surface 42 in the thickness direction H. The thicker the electrode layer 40 is, the easier it is for the crystal grains of the transparent conductive layer to grow larger in the crystallization process described below, and therefore the easier it is to form the raised portion 41 on the surface 40a of the electrode layer 40. In addition, a thick electrode layer 40 is also preferable from the viewpoint of reducing the resistance of the electrode layer 40. The thickness of the electrode layer 40 is preferably 300 nm or less, more preferably 200 nm or less, even more preferably 150 nm or less, and even more preferably 120 nm or less, from the viewpoint of ensuring the bending resistance of the light control film X (such as suppressing cracking of the electrode layer 40 when bent).

[0061] The number of free electrons (the number of carriers) in the electrode layer 40 in a plan view is preferably 5×10 15 / cm 2 More preferably, 8×10 15 / cm 2 More preferably, 10×10 15 / cm 2 More preferably, 11×10 15 / cm 2 The number of free electrons (the number of carriers) in the plan view of the electrode layer 40 is preferably 100×10 15 / cm 2 Less than or equal to 60×10 15 / cm 2 Less than 40×10, more preferably 15 / cm 2 The following is the result.

[0062] The visible light transmittance of the electrode layer 40 is, for example, 50% or more, preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency required for the transparent state of the light control film in the light control film X. The visible light transmittance of the electrode layer 40 is, for example, 100% or less.

[0063] The visible light transmittance (in a transparent state) of the light control film X is preferably 70% or more, more preferably 80% or more, and even more preferably 85% or more, from the viewpoint of ensuring the transparency of the light control film X. The visible light transmittance of the base film 10 is, for example, 100% or less.

[0064] The average transmittance of the light control film X at wavelengths of 800 nm to 1300 nm is preferably 50% or less, more preferably 40% or less, and even more preferably 30% or less, from the viewpoint of ensuring good heat shielding properties against sunlight in the light control film X. The average transmittance of the light control film X is, for example, 0% or more, and preferably 10% or less. The light control film X preferably has such an average transmittance (wavelength 800 nm to 1300 nm) in a colored state or a transparent state, and more preferably has such an average transmittance (wavelength 800 nm to 1300 nm) in both a colored state and a transparent state.

[0065] The light control film X is produced, for example, as follows.

[0066] First, as shown in FIG. 4A, a substrate film 10 is prepared. The substrate film 10 can be produced by forming a cured resin layer 12 on a resin film 11. The cured resin layer 12 can be formed by applying the above-mentioned first curable resin composition on the resin film 11 to form a coating film, and then curing the coating film. When the first curable resin composition contains a thermosetting resin, the coating film is cured by heating. When the first curable resin composition contains an ultraviolet-curable resin, the coating film is cured by ultraviolet irradiation. The exposed surface of the cured resin layer 12 formed on the resin film 11 is subjected to a surface modification treatment as necessary. When a plasma treatment is performed as the surface modification treatment, argon gas, for example, is used as an inert gas. The discharge power in the plasma treatment is, for example, 10 W or more, and, for example, 5000 W or less.

[0067] 4B, an amorphous transparent conductive layer 20' is formed on the base film 10 (transparent conductive layer forming step). Specifically, a transparent conductive material is deposited on the cured resin layer 12 of the base film 10 by a sputtering method to form the transparent conductive layer 20'.

[0068] In the sputtering method, it is preferable to use a sputtering deposition apparatus capable of performing a film formation process by a roll-to-roll method. When using a sputtering deposition apparatus of the roll-to-roll method in the manufacture of the light control film X, a material is deposited on the long substrate film 10 while the substrate film 10 is running from a pay-out roll to a take-up roll provided in the apparatus, to form the transparent conductive layer 20'. In addition, in the sputtering method, a sputtering deposition apparatus having one deposition chamber may be used, or a sputtering deposition apparatus having multiple deposition chambers arranged in order along the running path of the substrate film 10 may be used.

[0069] Specifically, in the sputtering method, a sputtering gas (inert gas) is introduced under vacuum conditions into a deposition chamber of a sputter deposition apparatus, while a negative voltage is applied to a target placed on a cathode in the deposition chamber. This generates a glow discharge to ionize gas atoms, and the gas ions collide with the target surface at high speed to eject target material from the target surface, which is then deposited on the substrate film 10. As the target material, for example, a sintered body of the conductive oxide described above with respect to the electrode layer 20 is used.

[0070] The sputtering method is preferably a reactive sputtering method. In the reactive sputtering method, for example, a sputtering gas (inert gas) and oxygen as a reactive gas are introduced into a film formation chamber. In the reactive sputtering method, the ratio of the amount of oxygen introduced to the total amount of the sputtering gas and oxygen introduced into the film formation chamber is, for example, 0.01 flow % or more, and, for example, 15 flow % or less.

[0071] The air pressure in the film formation chamber during film formation by sputtering (sputter film formation) is, for example, 0.02 Pa or more and, for example, 1 Pa or less.

[0072] The film formation temperature in the sputtering method (the temperature of the substrate film 10 during sputtering film formation) is preferably 50° C. or less, more preferably 30° C. or less, even more preferably 10° C. or less, still more preferably 0° C. or less, and even more preferably −5° C. or less, from the viewpoint of properly forming an amorphous transparent conductive layer capable of crystal growth in the subsequent crystallization step. The film formation temperature is, for example, −30° C. or more or −20° C. or more.

[0073] Examples of power sources for applying voltage to the target include DC power sources, AC power sources, MF power sources, and RF power sources. A DC power source and an RF power source may be used in combination as the power source. The absolute value of the discharge voltage during sputtering deposition is, for example, 50 V or more, and, for example, 500 V or less. The horizontal magnetic field strength on the target is, for example, 10 mT or more, and, for example, 100 mT or less.

[0074] Next, as shown in FIG. 4C, the transparent conductive layer 20' (FIG. 4B) on the base film 10 is crystallized by heating to form an electrode layer 20 (crystalline transparent conductive layer) (crystallization step). In this way, the electrode-attached base film Y1 is produced. Examples of heating means include an infrared heater and an oven (heat medium heating oven, hot air heating oven). The heating temperature is preferably 100° C. or higher, more preferably 120° C. or higher, from the viewpoint of ensuring a high crystallization rate. The heating temperature is preferably 200° C. or lower, more preferably 170° C. or lower, and even more preferably 150° C. or lower, from the viewpoint of suppressing the influence of heating on the base film 10. The heating time is, for example, less than 600 minutes, preferably less than 120 minutes, more preferably 90 minutes or lower, and even more preferably 60 minutes or lower, and is, for example, 1 minute or more, preferably 5 minutes or more.

[0075] Next, as shown in Fig. 4D, the light-controlling layer 30 is formed on the electrode layer 20. When an inorganic EC material is used as the material for forming the light-controlling layer 30, the inorganic EC material is formed into a film on the electrode layer 20 by, for example, a dry coating method. As the dry coating method, a sputtering method is preferable. When an organic EC material is used as the material for forming the light-controlling layer 30, the organic EC material is formed into a film on the electrode layer 20 by, for example, a wet coating method.

[0076] On the other hand, an electrode-attached base film Y2 (base film 50, electrode layer 40) is prepared. Specifically, the method is the same as that for preparing the electrode-attached base film Y1 (FIGS. 4A to 4C).

[0077] Next, as shown in Figures 5A and 5B, the electrode-attached base film Y1 with the light-adjusting layer 30 and the electrode-attached base film Y2 were integrated. Specifically, the electrode-attached base film Y1, Y2 and the light-adjusting layer 30 were integrated so that the light-adjusting layer 30 was sandwiched between the electrode-attached base films Y1, Y2.

[0078] In this manner, the light control film X can be manufactured. In the light control film X, the light control layer 30 is switched between a non-transparent state (light blocking state) and a transparent state (light non-blocking state) by turning on and off the voltage between the electrode layers 20 and 40. In a window glass to which such a light control film X is attached, the transmittance of light, such as visible light, through the window glass with the light control film X attached thereto can be switched by turning on and off the voltage between the electrode layers 20 and 40.

[0079] As described above, the light-control film X has a raised portion 21 with a height of 3 nm or more on the surface 20a of the electrode layer 20 facing the light-control layer 30. The electrode layer 20 having the raised portion 21 with a significant height of 3 nm or more is suitable for ensuring the average thickness of the entire electrode layer 20. As described above, the light-control film X having such an electrode layer 20 is suitable for ensuring the number of free electrons (the number of carriers) per unit area in the planar view of the electrode layer 20. The greater the number of free electrons in the electrode layer 20, the higher the reflectivity of the electrode layer 20 against heat rays in sunlight, and therefore the higher the heat-blocking property of the light-control film X. Therefore, the light-control film X is suitable for achieving good heat-blocking property against sunlight. Such a light-control film X is suitable as a light-control film for outdoor use. Examples of light-control films for outdoor use include light-control films for sunroofs of cars such as private cars, and light-control films for windows of buildings such as houses and buildings.

[0080] As described above, in the light control film X, the surface 40a of the electrode layer 40 facing the light control layer 30 preferably has raised portions 41 with a height of 3 nm or more. The electrode layer 40 having raised portions 41 with a significant height of 3 nm or more helps the light control film X to achieve good heat shielding properties against sunlight. EXAMPLES

[0081] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the examples. In addition, the specific numerical values ​​of the blending amounts (contents), physical property values, parameters, etc. described below can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the blending amounts (contents), physical property values, parameters, etc. corresponding to those described in the above-mentioned "Form for carrying out the invention".

[0082] Example 1 First, a roll of polyethylene terephthalate (PET) film (thickness 100 μm, manufactured by Mitsubishi Chemical Corporation) was prepared as a long resin film. Next, a thermosetting resin composition C1 was applied to one side (first side) of the PET film to form a coating film. The resin composition C1 contains 100 parts by mass of melamine resin, 100 parts by mass of alkyd resin, and 50 parts by mass of an organic silane condensate. Next, the coating film on the PET film was heated and thermally cured. The heating temperature was 185° C. The heating time was 1 minute. As a result, a first cured resin layer was formed as an optical adjustment layer having a thickness of 35 nm. Next, a UV-curable resin composition C2 was applied to the other side (second side) of the PET film to form a coating film. Next, the coating film was cured by UV irradiation. As a result, a second cured resin layer was formed as a hard coat (HC) layer having a thickness of 2 nm. In this manner, a substrate film (first cured resin layer / substrate film / second cured resin layer) was produced.

[0083] Next, a 105 nm thick amorphous transparent conductive layer was formed on the first cured resin layer of the base film by reactive sputtering (transparent conductive layer formation process). In this process, a roll-to-roll sputter deposition device (DC magnetron sputter deposition device) was used. The device is equipped with a deposition chamber that can perform the deposition process while running the work film by the roll-to-roll method. The conditions for sputter deposition in this process are as follows:

[0084] In sputtering, the ultimate vacuum in the deposition chamber is 0.6×10 -4After the sputtering deposition apparatus was evacuated to a pressure of 0.4 Pa, argon (Ar) as a sputtering gas (inert gas) and oxygen as a reactive gas were introduced into the deposition chamber, and the pressure in the deposition chamber was set to 0.4 Pa. The ratio of the amount of oxygen introduced to the total amount of argon and oxygen introduced into the deposition chamber was set to about 2.6 flow rate %. In addition, a sintered body of indium oxide and tin oxide (ITO with a tin oxide concentration of 10 mass %) was used as the target (first target). A DC power supply was used as the power source for applying a voltage to the target. The horizontal magnetic field strength above the target was 90 mT. The deposition temperature (the temperature of the substrate film on which the transparent conductive layer is laminated) was set to -8°C.

[0085] Next, the amorphous transparent conductive layer was crystallized by heating in a hot air oven (crystallization step). The heating temperature was 140° C. and the heating time was 1 hour. As a result, a crystalline transparent conductive layer having a thickness of 105 nm was formed as an electrode layer.

[0086] In this manner, a roll of the electrode layer-attached film was produced. This electrode layer-attached film included a base film (second cured resin layer / resin film / first cured resin layer) and an electrode layer on the base film.

[0087] Next, two sheets of electrode layer-attached film were cut out from the roll of electrode layer-attached film. Next, an adhesive (product name "LUCIACS CS9861UA", manufactured by Nitto Denko Corporation) was applied onto the electrode layer of one of the electrode layer-attached films (first electrode layer-attached film) to form an adhesive layer having a thickness of 25 μm as a pseudo-light control layer. Next, the electrode layer side of the other electrode layer-attached film (second electrode layer-attached film) was attached to the adhesive layer. That is, the two electrode layer-attached films were joined via the adhesive layer.

[0088] In this manner, the laminated film of Example 1 was produced. This laminated film is a pseudo-light control film having a laminated structure similar to that of a light control film (this film has a pseudo shape and does not have a light control function). Specifically, the laminated film of Example 1 has a first base film, a first electrode layer having a thickness of 105 nm, a pseudo-light control layer, a second electrode layer having a thickness of 105 nm, and a second base film in this order in the thickness direction.

[0089] Comparative Example 1 A laminated film of Comparative Example 1 was produced in the same manner as the laminated film of Example 1, except for the transparent conductive layer formation step.

[0090] In the transparent conductive layer process in this comparative example, a first layer (thickness 11 nm) of an amorphous transparent conductive layer was formed on the first cured resin layer of the base film by reactive sputtering, and then a second layer (thickness 11 nm) of an amorphous transparent conductive layer was formed on the first layer. In this process, a roll-to-roll sputtering deposition device (DC magnetron sputtering deposition device) was used. The device is equipped with a first deposition chamber and a second deposition chamber that can perform a deposition process while running a work film by a roll-to-roll method.

[0091] The conditions for sputter deposition in the first deposition chamber were the same as those for sputter deposition in Example 1, except that the deposition temperature was 80°C instead of -8°C.

[0092] The conditions for sputtering deposition in the second deposition chamber were the same as those for sputtering deposition in Example 1, except for the following: The deposition temperature was 80°C instead of -8°C. As the target, a second target was used instead of the first target. The second target was ITO, a sintered body of indium oxide and tin oxide, with a tin oxide concentration of 3 mass%.

[0093] The laminated film of Comparative Example 1 has, in this order in the thickness direction, a first base film, a first electrode layer having a thickness of 22 nm, a pseudo-dimming layer, a second electrode layer having a thickness of 22 nm, and a second base film.

[0094] <Electrode layer thickness> The thickness of the electrode layer of the electrode layer-attached film obtained in the process of producing each laminated film in Example 1 and Comparative Example 1 was measured by observation with a field emission transmission electron microscope (FE-TEM). Specifically, first, a sample for cross-sectional observation of each electrode layer in Example 1 and Comparative Example 1 (first sample) was produced by FIB (Focused Ion Beam) processing (FIB microsampling method). In the FIB microsampling method, a FIB device (product name "FB2200", manufactured by Hitachi) was used, and the acceleration voltage was set to 10 kV. Next, the cross section of the electrode layer in the first sample was observed by FE-TEM, and the thickness of the electrode layer was measured in the observed image. In the observation, a FE-TEM device (product name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV.

[0095] The thickness of the first layer of the electrode layer in Comparative Example 1 was measured by preparing a cross-sectional observation sample from an intermediate product before forming the second layer on the first layer, and observing the sample by FE-TEM. The thickness of the second layer of the electrode layer in Comparative Example 1 was determined by subtracting the thickness of the first layer from the total thickness of the electrode layer in Comparative Example 1.

[0096] Observation of the protuberance For the electrode layer of the electrode layer-attached film obtained in the process of producing each of the laminated films of Example 1 and Comparative Example 1, the presence or absence of a protrusion on the surface (the surface opposite to the base film) was confirmed.

[0097] First, a cross-sectional observation sample (second sample) capable of observing the cross-sectional shape of the electrode layer surface was prepared by FIB (Focused Ion Beam) processing. The method for preparing the second sample was the same as that for the first sample described above. Next, the cross-section of the electrode layer in the second sample was observed by FE-TEM, and the presence or absence of protuberances on the surface of the electrode layer was confirmed in the observed image. In the observation, a FE-TEM device (product name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV. In the electrode layer-attached film in Example 1, protuberances could be confirmed on the electrode layer surface. In the electrode layer-attached film in Comparative Example 1, protuberances could not be confirmed on the electrode layer surface. In the observation image of the electrode layer-attached film in Example 1, the height of each protuberance (protuberance having a shape protruding from the surrounding flat surface) included in the observation field was measured. The height of the protuberance is the distance from the flat surface to the top of the protuberance in the thickness direction of the electrode layer. Then, the average height of 10 arbitrarily selected protuberances having a height of 3 nm or more was calculated. The value is shown as the protrusion height in Table 1. The electrode layers of the laminated film of Comparative Example 1 are each configured by stacking relatively thin transparent conductive layers (first layer and second layer) and are formed at a relatively high temperature, and therefore are considered to have no protrusions with a height of 3 nm or more.

[0098] <Transmittance, reflectance> For each laminate film of Example 1 and Comparative Example 1, the solar transmittance (Te) and solar reflectance (Re) in the wavelength range of 300 nm to 2500 nm were measured using a spectrophotometer U-4100 (manufactured by HITACHI). In this measurement, the measurement interval was 5 nm. The measurement results are shown in Table 1. Solar radiation refers to radiation in the wavelength range of 300 to 2500 nm. The solar transmittance (Te) is calculated by the spectrophotometer from a predetermined product-sum calculation including the spectral transmittance and the spectral solar irradiance in the formula. The solar reflectance (Re) is calculated by the spectrophotometer from a predetermined product-sum calculation including the spectral reflectance and the spectral solar irradiance in the formula.

[0099] <Solar heat gain rate> The solar heat gain coefficient was determined for each of the laminate films of Example 1 and Comparative Example 1. Specifically, the solar heat gain coefficient of the laminate film was determined by the following formulas (1) to (3) based on ISO 13837:2021. In formula (1), Tts represents the solar heat gain coefficient and is an index of heat shielding properties.

[0100] Tts = Te + Qi (1) Qi = Ae × {hi / (hi + he)} (2) Ae = 100- Te - Re (3)

[0101] For each laminated film of Example 1 and Comparative Example 1, formulas (1) to (3) are as follows. Tts indicates the ratio (%) of the total energy passing through the sample when the total energy of the light (irradiated light) irradiated to the sample (laminated film) is taken as 100%. Te indicates the energy of the light (transmitted light) that passes through the sample out of the light irradiated to the sample, expressed as a ratio. The solar transmittance obtained in the above measurement was used as Te. Qi represents the secondary heat flux passing through the sample, and is calculated by formula (2). The smaller this value, the less the sample transmits heat, meaning that the sample has higher heat insulation. In formula (2), Ae indicates the ratio of the energy absorbed by the sample out of the energy of the light irradiated to the sample, and is calculated by formula (3). hi is a parameter indicating the ease of heat transmission in the sample in the same direction as the light passing direction. When hi is 8 W / (m 2 ·K) was used. he is a parameter that indicates the ease of heat transfer in the opposite direction to the light transmission direction in the sample. he is 21 W / (m 2 ·K) was used. In formula (3), Re indicates the ratio of the energy of the light reflected by the sample (reflected light) to the light irradiated to the sample. The solar reflectance obtained in the above measurement was used as Re.

[0102] Number of careers The number of carriers in each electrode layer in Example 1 and Comparative Example 1 was measured using a Hall effect measuring device (product name "HL5500PC", manufactured by Bio-Rad Laboratories). The measurement results are shown in Table 1.

[0103] [Table 1] [Explanation of symbols]

[0104] X-light control film Y1, Y2 Substrate film with electrodes 10. Base film 11 Resin film 20 Electrode layer (first electrode layer) 20a,40a surface 21,41 Ridge 30 Photochromic Layer 40 Electrode layer (second electrode layer)

Claims

1. A light-controlling film including a base film, a first electrode layer, a light-controlling layer, and a second electrode layer in this order in a thickness direction, the surface of the first electrode layer on the side of the light-controlling layer has a protrusion having a height of 3 nm or more and 8 nm or less; A light-controlling film, wherein the first electrode layer has a thickness of 30 nm or more.

2. The light-controlling film according to claim 1 , wherein the surface of the second electrode layer on the side of the light-controlling layer has a protrusion having a height of 3 nm or more.

3. The light control film according to claim 1 , wherein the substrate film has a near-infrared absorbing layer and / or a near-infrared reflective layer.

4. The light control film according to any one of claims 1 to 3, having an average transmittance of 50% or less at wavelengths of 800 nm to 1300 nm.

Citation Information

Patent Citations

  • Electrochromic display element

    JP2019003060A

  • Lighting control film

    JP2019101206A

  • Light control body

    JP2020134575A

  • Transmittance variable element and manufacturing method thereof

    JP2021173825A

  • Dimming sheet

    JP2024034702A